Two-component acrylate compositions, and articles and assemblies and using method thereof

A two-component acrylate adhesive with a gradient of properties effectively bonds neodymium magnet steel and metallic substrates, addressing thermal expansion and corrosion issues, ensuring durable and heat-resistant bonding.

WO2026232287A1PCT designated stage Publication Date: 2026-11-12HENKEL KGAA +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/092951
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing adhesives struggle to provide strong, durable, and heat-resistant bonding between neodymium magnet steel and metallic substrates, particularly due to differences in thermal expansion coefficients and susceptibility to corrosion, leading to internal stress and failure of the adhesive bond.

Method used

A two-component acrylate adhesive composition is formulated with specific monomers, adhesion promoters, rubber toughening agents, and initiators, applied in a bead-on-bead method to create a gradient of properties suitable for bonding neodymium magnet steel and metallic substrates, ensuring flexibility and adhesion.

Benefits of technology

The composition achieves excellent thermal resistance, moisture resistance, and heat aging performance, maintaining bond integrity under stress and temperature variations, preventing shift and crack formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025092951-FTAPPB-I100001
    Figure PCTCN2025092951-FTAPPB-I100001
  • Figure PCTCN2025092951-FTAPPB-I100002
    Figure PCTCN2025092951-FTAPPB-I100002
  • Figure PCTCN2025092951-FTAPPB-I100003
    Figure PCTCN2025092951-FTAPPB-I100003
Patent Text Reader

Abstract

A two-component acrylate composition comprises a component A and a component B, the component A comprising a first (meth) acrylate monomer, a second (meth) acrylate monomer which being reactive with metal, an adhesion promoter, a rubber toughening agent, a peroxide initiator; the component B comprising a first (meth) acrylate monomer, a rubber toughening agent, a soft (meth) acrylate monomer, a catalyst, a reductant, wherein the two-component acrylate composition being used to bond a neodymium magnet substrate and a metallic substrate, the component A being used on the metallic substrate and the component B being used on the neodymium magnet substrate. The two-component acrylate composition could be used as structural adhesive, for example, in magnet bonding of two different substrates, such as bonding of metallic substrate and neodymium magnet substrate.
Need to check novelty before this filing date? Find Prior Art

Description

TWO-COMPONENT ACRYLATE COMPOSITIONS, AND ARTICLES AND ASSEMBLIES AND USING METHOD THEREOFTechnical field

[0001] The present disclosure relates to two-component acrylate compositions suitable for structural adhesive applications, articles, and assemblies therefrom, using method thereof. The two-component acrylate compositions can be used for bonding of two different substrates, for example, for bonding of neodymium magnet substrate and metallic substrate.Background of the invention

[0002] Magnets are everywhere and so is magnet bonding. It is an application used in a wide range of industries, including electrical machinery, power tools, the automotive industry, audio and video equipment, household appliances and other fields. Innovative magnet bonding goes beyond traditional methods, offering a reliable way to harness the power of magnetism while ensuring strong and durable adhesion. Whatever in manufacturing, electronics, automotive, or even creative projects, magnet bonding adhesives provide a unique way to create versatile connections that combine the strength of magnets with the versatility of adhesives.

[0003] To meet our customers' manufacturing and application needs, choosing a suitable adhesive is crucial. For example, the magnet bonding adhesive used in a speaker must be strong, durable, and heat-resistant, as speakers operate at high temperatures and are subject to significant internal stress during use. Speaker adhesive typically has a high-temperature resistance, which means it can withstand elevated temperatures without losing its adhesive properties. Vibration resistance is also essential to ensure the speaker remains in one piece and maintains sound quality over time. A speaker structural adhesive glue with good vibration resistance will keep the bond intact even under the most strenuous conditions.

[0004] Ferrite magnets are the most common type of magnet used in loudspeakers. They are made from iron oxide and other metallic oxide such as strontium oxide or barium oxide. Ferrite magnets are relatively low cost, have good magnetic properties, and provides excellent performance in most loudspeaker application. But, under the action of external force, adhesives with high modulus will generate internal stress, and excessive internal stress will cause the ferrite magnetic steel bonded to the structural adhesive to break / crack.

[0005] Neodymium magnets are the strongest permanent magnets at present. They are made of neodymium, iron and boron (NdFeB) alloys. Neodymium magnets have a much stronger magnetic force than ferrite magnets and have the characteristics of high efficiency and small size in loudspeaker design. NdFeB magnet steel has better anti-crack property than ferrite magnetic steel during thermal shock test. But the NdFeB magnet steel, withstand several cycles of high temperature and low temperature exposure will generate internal stress, and excessive internal stress will cause the failure mode between adhesive bond line, which leads to the shift between assembled parts.

[0006] NdFeB magnet steel is brittle and flat with very low coefficient of thermal expansion (CTE) , while metallic substrate, such as galvanized steel normally has a polar and rough surface with relative higher CTE. To bond metallic substrate, a polar structural adhesive with some corrosiveness is usually desired to achieve high adhesion. But to bond NdFeB magnet steel, corrosion is completely prohibited.

[0007] In working condition, magnets will generate lots of heat. To maintain significant adhesion between adhesive and metallic substrates, the structural adhesive is usually designed to be tough enough with high heat resistance. But to avoid the shift between assembled parts, adhesive need to be flexible enough to minimize the internal stress between NdFeB and adhesive. It is hard to find a structural adhesive has these desired properties for bonding NdFeB magnet and other metallic substrate. Thus, development of an acrylic structural adhesive composition for bonding NdFeB magnet steel and metallic substrate is demanding.Summary of the invention

[0008] It is therefore the object of the present invention to overcome the above-mentioned drawbacks by providing a two-component acrylic adhesive composition with excellent thermal resistance for bonding NdFeB magnet steel substrate and metallic substrate. In addition, the acrylate composition has good resistance to moisture and heat aging.

[0009] In the present invention, it is surprisingly found that based on proper formulation design, two-component bead-on-bead adhesives could show better performance when bonding two different substrates, especially NdFeB steel and galvanized steel, compared to pre-mix two-component adhesives. The two-component acrylic adhesive of present invention forms a good transition layer between NdFeB and galvanized steel, and two components have good compatible property. Adhesives close to the galvanized steel side are polar and tough while adhesives close to the NdFeB side are flexible. The performance of such bead-on-bead adhesive is even better when fixture time and film thickness is better controlled.

[0010] According to one aspect, the present invention relates to a two-component acrylate composition comprises a component A and a component B, the component A comprising a first (meth) acrylate monomer, a second (meth) acrylate monomer which being reactive with metal, an adhesion promoter, a rubber toughening agent, a peroxide initiator; the component B comprising a first (meth) acrylate monomer, a rubber toughening agent, a soft (meth) acrylate monomer, a catalyst, a reductant, wherein the two-component acrylate composition being used to bond a neodymium magnet substrate and a metallic substrate, the component A being used on the metallic substrate and the component B being used on the neodymium magnet substrate.

[0011] According to one aspect, the present invention is directed to a structural adhesive comprising a cured product of the two-component acrylate composition according to present invention.

[0012] According to still another aspect, the present invention also relates to an article comprising a neodymium magnet substrate, a metallic substrate and a structural adhesive bonded the neodymium magnet substrate and the metallic substrate, wherein the structural adhesive is the cured product of the two-component acrylate composition according to present invention.

[0013] According to still another aspect, the present invention is also directed to a speaker, a motor or a metal component comprises an article of present invention.

[0014] According to still another aspect, the present invention also relates to a method of bonding two substrates comprising steps:

[0015] 1) applying a component A of a two-component acrylate composition according to any one of claims 1-18 to a metallic substrate to be bonded,

[0016] 2) applying a component B of a two-component acrylate composition according to any one of claims 1-16 to a neodymium magnet substrate to be bonded,

[0017] 3) overlaying the metallic substrate on the neodymium magnet substrate or overlaying the neodymium magnet substrate on the metallic substrate; and

[0018] 4) bonding the metallic substrate to the neodymium magnet substrate by mixing the component A and the component B of the two-component acrylate composition and curing the composition.

[0019] According to still another aspect, the present invention is also directed to an article comprising a bonding product made according to present invention, wherein

[0020] 1) the content of the adhesion promoter in the acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate,

[0021] 2) the content of the second (meth) acrylate monomer which being reactive with metal in acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate,

[0022] 3) the content of the soft (meth) acrylate monomer in acrylate composition showing a concentration gradient, with an increasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate.Detailed description of the invention

[0023] In the following passages the present invention is described in more detail. Each aspect so described may be combined with any other aspect or aspects unless clearly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature or features indicated as being preferred or advantageous.

[0024] In the context of the present invention, the terms used are to be construed in accordance with the following definitions, unless a context dictates otherwise.

[0025] As used herein, the singular forms “a” , “an” and “the” include both singular and plural referents unless the context clearly dictates otherwise. For example, reference to "afiller" encompasses embodiments having one, two or more fillers. As used in this specification and the appended claims, the term "or" is generally employed in its sense including "and / or" unless the content clearly dictates otherwise.

[0026] The terms “comprising” , “comprises” and “comprised of” as used herein are synonymous with “including” , “includes” or “containing” , “contains” , and are inclusive or open-ended and do not exclude additional, non-recited members, elements or process steps.

[0027] The term “ambient temperature” refers to a temperature in the range of 21-25℃, inclusive.

[0028] The recitation of numerical end points includes all numbers and fractions subsumed within the respective ranges, as well as the recited end points.

[0029] Unless otherwise defined, all terms used in the disclosing the invention, including technical and scientific terms, have the meaning as commonly understood by one of the ordinary skills in the art to which this invention belongs to. By means of further guidance, term definitions are included to better appreciate the teaching of the present invention.

[0030] In the context of this disclosure, several terms shall be utilized.

[0031] The terms “polymer” is used herein consistent with its common usage in chemistry. Polymers are composed of many repeated subunits. The term “polymer” is used to describe the resultant material formed from a polymerization reaction.

[0032] The term “acrylic” refers to both or any one of “acrylic” and “methacrylic” .

[0033] The term “acrylate” refers to both or any one of “acrylate” and “methacrylate” .

[0034] The terms “curing” is used herein means a process of hardening of a material. The term is intended to encompass the cross-linking of components within the material which possess reactive groups.

[0035] As used herein, the term “one component (1 K) composition" refers to a composition where, during storage of the composition, the composition components are all admixed together but the properties of the composition, including viscosity, remain consistent enough over the time of storage to permit successful utility of the composition later.

[0036] The term “two-component (2K) compositions" are understood to be compositions in which a first component / component and a second component / part must be stored in separate vessels because of their (high) reactivity. The two components / parts are mixed only shortly before application and then react, typically without additional activation, with bond formation and thereby formation of a polymeric network.

[0037] The term “fixture time” refers to the amount of time it takes for the adhesive to not only bond but also reach handling strength, e.g., reach 0.1 MPa shear strength within 1 minute.

[0038] The term “bead-on-bead” describes a unique chemistry for a two-component acrylic adhesive. Rather than premixing components A and B, each component is applied to the substrate and the mixing occurs when the two substrates to be bonded are joined.

[0039] For purposes of this invention, number average molecular weight (Mn) is determined by gel permeation chromatography (GPC, also known as SEC) at 23℃ using a styrene standard according to DIN EN ISO 16014-5: 2012-10.

[0040] Viscosities of the composition compositions may be determined using the Brookfield Viscometer, Model RVT at standard conditions of 25℃ and 50%Relative Humidity (RH) . The viscometer is calibrated using silicone oils of known viscosities, which vary from 5,000 cps to 300,000 cps. A set of RV spindles that attach to the viscometer are used for the calibration. Measurements of the damping composition are done at 25℃ using the No. 7 spindle at a speed of 20 revolutions per minute for 1 minute until the viscometer equilibrates.

[0041] As used herein, the glass transition temperature (Tg) is determined by differential scanning calorimetry (DSC) employing a 20 K / min ramp rate and midpoint measurement in accordance with DIN 53 765.

[0042] It is known to all that two-component structural adhesive should be mixed as homogeneous as possible before curing, so that it could reach the best performance. However, for bonding between two different substrates, such as NdFeB magnet and galvanized steel, a normal pre-mix adhesive can hardly balance all required properties. Therefore, we provided a two-component acrylate composition and using method thereof to solve the problem.

[0043] As discussed previously, embodiments of the present disclosure are directed to a two-component acrylate composition comprising a component A (part A) and a component B (part B) . The component A comprises a first (meth) acrylate monomer, a second (meth) acrylate monomer which being reactive with metal, an adhesion promoter, a rubber toughening agent, and a peroxide initiator. The component B comprises a first (meth) acrylate monomer, a rubber toughening agent, a soft (meth) acrylate monomer, a catalyst, and a reductant. The two-component acrylate composition being used to bond a neodymium magnet substrate and a metallic substrate, the component A being used on the metallic substrate and the component B being used on the neodymium magnet substrate.

[0044] First (meth) acrylate monomer (a)

[0045] The composition according to the present invention comprises at least one first (meth) acrylate monomer. The first (meth) acrylate monomer in component A is the same or different from the first (meth) acrylate monomer in component B.

[0046] Suitable first (meth) acrylate monomer comprises mono-functional (meth) acrylate monomer and multi-functional (meth) acrylate monomer. Herein the mono-functional monomer means (meth) acrylate monomer with one polymerizable unsaturated bond per molecular, multi-functional monomer means (meth) acrylate monomer with more than one polymerizable unsaturated bond per molecular.

[0047] The first (meth) acrylate monomer comprises aromatic acrylate monomer, heterocyclic acrylate monomer and aliphatic acrylate monomer.

[0048] In some embodiments, the first (meth) acrylate monomer is a heterocyclic acrylate monomer or a aromatic acrylate monomer comprising a cyclic moiety. Although the cyclic moiety may be cycloaliphatic, in preferred embodiments, the cyclic moiety is an aromatic.

[0049] Suitable first (meth) acrylate monomers comprising an aromatic moiety include for instance and without limitation, benzyl (meth) acrylate, 2-phenoxyethyl (meth) acrylate, ethoxylated nonyl-phenol (meth) acrylate, propoxylated (2.5) nonyl phenyl (meth) acrylate, o-phenylphenoxyethyl (meth) acrylate, 2- (phenylthiol) ethyl (meth) acrylate, cumyl phenoxyl ethyl (meth) acrylate, and 2-hydroxy-3-phenoxypropyl (meth) acrylate.

[0050] Suitable first (meth) acrylate monomers comprising a cycloaliphatic moiety include for instance and without limitation, 3, 3, 5-trimethylcyclohexyl (meth) acrylate, butyl-cyclohexyl (meth) acrylate, 2-decahydronapthyl (meth) acrylate, 1-adamantyl (meth) acrylate, dicyclopentadienyl (meth) acrylate, bornyl (meth) acrylate including isobornyl (meth) acrylate, dimethyl-1-adamantyl (meth) acrylate, and 3-tetracyclo [4.4.0.1.1] dodecyl methacrylate.

[0051] In some embodiments, the first (meth) acrylate monomers are aliphatic acrylate monomer comprising alkyl acrylates or methacrylates, i.e., compounds containing one acrylate or methacrylate group and an alkyl moiety. For instance, alkyl acrylate monomers have the structure CH2═CH-C (═O) -O-R, where R is alkyl; and alkyl methacrylate monomers have the structure CH2 ═C (CH3) -C (═O) -O-R, wherein R is alkyl. In some embodiments, the alkyl moiety comprises between 1 and 11 carbon atoms. In some embodiments, the alkyl moiety comprises between 1 and 8 carbon atoms (i.e., 1, 2, 3, 4, 5, 6, 7 or 8 carbon atoms) . In some embodiments, the alkyl moiety comprises between 1 and 6 carbon atoms. The alkyl group can be either straight chain or branched.

[0052] The suitable alkyl acrylate monomer is preferably selected from the group consisting of methyl (meth) acrylate, ethyl (meth) acrylate, n-propyl (meth) acrylate, isobutyl (meth) acrylate and the mixture thereof.

[0053] (Meth) acrylate monomers comprising an aromatic moiety such as benzyl (meth) acrylate, 2-phenoxyethyl (meth) acrylate, since they have relatively high Tg and / or good adhesion to magnet substances.

[0054] Suitable commercially available first (meth) acrylate monomers for use in the present invention include but is not limited to BNMA (benzyl methacrylate from Evonik and SR340NS (2-phenoxyethyl methacrylate) from Sartoma.

[0055] The first (meth) acrylate monomer may be present from 30 wt. %to 80 wt. %, or from 40 wt. %to 70 wt. %, or from 42 wt. %to 65 wt. %, or from 45 wt. %to 55 wt. %, based on the total weight of the component A. And / or the (meth) acrylate monomer may be present in the component B according to the present invention from 30 wt. %to 80 wt. %, or from 40 wt. %to 70 wt. %, or from 42 wt. %to 65 wt. %, or from 45 wt. %to 55 wt. %, based on the total weight of the component B.

[0056] In the component B, based on the total weight of the component B, the first (meth) acrylate monomer comprises at least 20 wt. %, or at least 25 wt. %, or at least 30 wt. %, or at least 35 wt. %, or at least 40 wt. %, or at least 45 wt. %, or at least 50 wt. %of (meth) acrylate monomers comprising an aromatic moiety. If in the component B, the aromatic moiety is less than 20 wt. %based on the total weight of the component B, the adhesion to NdFeB would be poor and the adhesive can’ t pass the thermal shock test due to the shift between assembled parts.

[0057] The upper limit of the first (meth) acrylate monomer is 80 wt. %, or 75 wt. %, or 70 wt. %, or 65 wt. %, or 60 wt. %based on the total weight of the composition. The lower limit of the first (meth) acrylate monomer is 30 wt. %, or 35 wt. %, or 40 wt. %, or 42 wt. %, or 48 wt. %, or 50 wt. %, based on the total weight of the composition.

[0058] Second (meth) acrylate monomer (b)

[0059] The composition according to the present invention comprises at least one second (meth) acrylate monomer only in component A. The second (meth) acrylate monomer in component A is reactive with metallic material.

[0060] Suitable second (meth) acrylate monomer is one or more being selected from methacrylic acid (MAA) , acrylic acid (MA) , tetrahydrofurfuryl (meth) acrylate (THF (M) A) , β-carboxyethylacrylate (β-ECA) , crotonic acid, maleic acid, fumaric acid, itaconic acid.

[0061] In some preferably embodiments of present invention, the second (meth) acrylate monomer comprises methyl methacrylate (MAA) , methyl acrylate (MA) , tetrahydrofurfuryl (meth) acrylate (THF (M) A) and β-carboxyethylacrylate (β-ECA) .

[0062] Suitable commercially available second (meth) acrylate monomers for use in the present invention include but is not limited to Visiomer MAA (methacrylic acid) from Evonik and SR 203NS (tetrahydrofurfuryl methacrylate) from Sartoma.

[0063] The second (meth) acrylate monomer may be present from 5 wt. %to 30 wt. %, or from 10 wt. %to 20 wt. %, or from 12 wt. %to 20 wt. %, based on the total weight of the component A.

[0064] The component B of present invention doesn’ t comprise the second (meth) acrylate monomer, such monomers that are reactive to metallic materials could corrode the surface of neodymium magnet material.

[0065] Soft (meth) acrylate monomer (f)

[0066] The composition according to the present invention comprises at least one soft (meth) acrylate monomer only in the component B.

[0067] The soft (meth) acrylate monomer can’ t exist in the component A, otherwise the thermal stability of the composition will decrease.

[0068] In some embodiments, the soft (meth) acrylate monomers are alkyl acrylates or methacrylates, i.e., compounds containing one acrylate or methacrylate group and an alkyl moiety. For instance, alkyl acrylate monomers have the structure CH2═CH-C (═O) -O-R, where R is alkyl; and alkyl methacrylate monomers have the structure CH2═C (CH3) -C (═O) -O-R, wherein R is alkyl. In some embodiments, the alkyl moiety comprises at least 12 carbon atoms. In some embodiments, the alkyl moiety comprises between 12 and 22 carbon atoms, or 12 to 20 carbon atoms (i.e., 12, 12 14, 15, 16, 17, 18, 19, or 20 carbon atoms) . In some embodiments, the alkyl moiety comprises between 12 and 18 carbon atoms. The alkyl group can be either straight chain or branched, and straight chain is preferred.

[0069] Examples of the soft (meth) acrylate monomer include lauryl (meth) acrylate, tetradecyl (meth) acrylate, hexadecyl (meth) acrylate, stearyl (meth) acrylate, behenyl (meth) acrylate and the mixtures thereof.

[0070] Suitable commercially available soft (meth) acrylate monomers for use in the present invention include but is not limited to Bisomer LMA (lauryl methacrylate) from Geo and SMA (stearyl methacrylate) from BASF.

[0071] The soft (meth) acrylate monomer may be present in the component B of the composition according to the present invention from 15 wt. %to 40 wt. %, or from 18 wt. %to 30 wt. %, or from 20 wt. %to 25 wt. %, based on the total weight of the component B. The thermal stability of the composition will be reduced if the soft (meth) acrylate monomer content in component B is too high.

[0072] Adhesion promoter (c)

[0073] To achieve a better adhesion property, an adhesion promoter can be introduced in the component A of present invention.

[0074] Examples of the adhesion promoter (c) include a phosphoric acid (meth) acrylate, which is preferably selected from the group consisting of phosphoric acid 2-hydroxymethyl methacrylate ester, 2-methacryloyloxyethyl acid phosphate, mono- (2-hydroxyethylmethacrylate) phosphate, 2-hydroxyethylmethylacrylate acid phosphate, bis (2-methacryloxyethyl) phosphate and mixtures thereof, preferably the adhesion promoter is 2-hydroxyethylmethylacrylate acid phosphate.

[0075] Suitable commercially available adhesion promoter for use in the present invention include but is not limited to JPA 514 from Johoku Chemical Co., Ltd.

[0076] The phosphoric acid (meth) acrylate adhesion promoter can’ t exist in the component B, otherwise the surface of the neodymium magnet substrate will be corroded.

[0077] The adhesion promoter may be present in the component A according to the present invention of less than 2 wt. %based on the component A, such concentration is good for controlling the cure rate greater than the mixing rate of the component A and component B.

[0078] The adhesion promoter may be present in the composition according to the present invention from 0.01 wt. %to 2 wt. %based on the total weight of the component A, preferably from 0.1 wt. %to 2 wt. %and more preferably from 0.2 wt. %to 2 wt. %. If the quantity of the adhesion promoter is less than 0.01 wt. %, it may not have an adhesion promoting effect, whereas higher quantity than 2 wt. %, may lead to a slow adhesion speed, and increased fixture time.

[0079] Rubber toughening agent (d)

[0080] The composition according to the present invention comprises a rubber. The rubber is present in part A and part B of the composition, the rubber in the part A is the same or different than the rubber in part B.

[0081] The rubber may be liquid or solid natural or synthetic rubber elastomeric polymer. Preferably the rubber is selected from the group consisting of polybutadienes, functionalized polybutadienes, polyisobutylenes, functionalized polyisobutylenes, butadiene-acrylonitrile copolymers, functionalized butadiene-acrylonitrile copolymers, functionalized styrene-butadiene copolymers, styrene butadiene copolymers, styrene-isoprene copolymers, functionalized styrene-isoprene copolymers, polyisoprenes, methyl methacrylate-butadiene-styrene copolymers, and mixtures thereof, wherein said polybutadienes, polyisobutylenes, butadiene-acrylonitrile copolymers and styrene-butadiene copolymers are functionalized with a functional group selected from the group consisting of a hydroxyl, a carboxyl, a carboxylic acid anhydride, an epoxy, and mixtures thereof, more preferably the rubber is selected from the group consisting of , styrene-butadiene copolymers, butadiene-acrylonitrile copolymers, styrene-isoprene copolymers, methyl methacrylate-butadiene-styrene copolymers and mixtures thereof.

[0082] Above listed rubbers are preferred because they provide good impact resistant properties while hydrophobic properties of the selected rubbers ensure that they do not impact high temperature, high humidity performance.

[0083] Suitable commercially available rubber for use in the present invention include but is not limited to Kraton D 1155ES from Kraton.

[0084] The rubber may be present in the part A and / or Part B of the composition according to the present invention from 10 wt. %to 40 wt. %, preferably from 15 wt. %to 30 wt. %, and more preferably from 18 wt. %to 25 wt. %, based on the total composition.

[0085] In some embodiments, the rubber is 10 wt. %, or 15 wt. %, or 18 wt. %, or 20 wt. %, or 25 wt. %, or 30 wt. %, or 35 wt. %, or 40 wt. %, based on the total composition.

[0086] Peroxide initiator (e)

[0087] The composition according to the present invention comprises a peroxide initiator. The suitable peroxide initiator for use in the present invention is an organic peroxide.

[0088] The radical initiator is preferably selected from the group consisting of cyclic peroxides, diacyl peroxides, dialkyl peroxides, hydroperoxides, peroxycarbonates, peroxydicarbonates, peroxyesters, and peroxyketals, more preferably selected from the group consisting cumene hydroperoxide (CHP) , para-menthane hydroperoxide, t-butyl hydroperoxide (TBH) , t-butyl peroxybenzoate, t-butyl peroxy pivalate, di-t-butyl peroxide, t-butyl peroxy acetate, t-butyl peroxy-2-hexanoate, t-amyl hydroperoxide, 1 ,2, 3, 4-tetramethylbutyl hydroperoxide, benzoyl peroxide, dibenzoyl peroxide, 1 , 3-bis (t-butylperoxyisopropyl) benzene, diacetyl peroxide, butyl 4, 4-bis (t-butylperoxy) valerate, p-chlorobenzoyl peroxide, t-butyl cumyl peroxide, di-t-butyl peroxide, dicumyl peroxide, di (dodecanoyl) peroxide, 2, 5-dimethyl-2, 5-di-t-butylperoxyhexane, 2, 5-dimethyl-2, 5-di-t-butyl-peroxyhex-3-yne, 4-methyl-2, 2-di-t-butylperoxypentane and mixtures thereof.

[0089] Suitable commercially available radical initiators for use in the present invention include but are not limited to Trigonox C (t-butyl peroxybenzoate) and Trigonox K 90 (cumene hydroperoxide) from Akzo Nobel.

[0090] The peroxide initiator may be present in the composition according to the present invention from 2.5 wt. %to 7 wt. %, or from 3 wt. %to 6 wt. %, or from 3 wt. %to 5 wt. %, based on the total weight of the component A.

[0091] If the quantity of the peroxide initiator is less than 2.3 wt. %in component A, it may not have desired and required cure speed, whereas higher quantity than 7 wt. %may lead to instability of the adhesive and too high quantity may also result in low molecular weight polymer formation and a brittle cured polymer.

[0092] Catalyst (g)

[0093] The composition according to the present invention comprises a catalyst. The suitable catalyst for use in the present invention is an organic metal salt.

[0094] Preferably catalyst is selected from the group consisting of cobalt (II) naphthenate, copper carbonate, copper (II) acetylacetonate, copper naphtenate, silver nitrate, vanadium (III) acetylacetonate, iron (II) naphthenate, copper disodium ethylenediamine tetra acetic acid (EDTA. 2Na. Cu (ll) ) , copper naphthenate, vanadium acetylacetonate, vanadyl acetylacetonate, iron (II) acetate, and mixtures thereof, preferably the catalyst is selected from copper naphtenate, vanadium (III) acetylacetonate and mixtures thereof.

[0095] Suitable commercially available catalyst for use in the present invention include but is not limited to copper naphthenate 8%from OMG Americas Inc.

[0096] The catalyst may be present in the composition according to the present invention from 0.06 wt. %to 3 wt. %based on the total weight of the component B, or from 0.06 wt. %to 1 wt. %, or from 0.08 wt. %to 0.5 wt. %.

[0097] If the quantity of the catalyst is less than 0.06 parts by weight, it may not have desired and required cure speed, whereas higher quantity than 3 parts by weight, may lead to instability of the adhesive.

[0098] Reductant (h)

[0099] The composition according to the present invention comprises a reductant (h) .

[0100] The suitable reductant for use in the present invention may be an aromatic amine, an aliphatic amine or a pyridine.

[0101] Preferably, the reductant is selected from the group consisting of tributylamine, toluidine, acetylpenyl hydrazine, N, N-dimethyl-p-toluidine, N, N-diethyl-p-toluidine, pyridine, 3, 5-diethyl-1, 2-dihydro-1-phenyl-2-propylpyridine and mixtures thereof.

[0102] Suitable commercially available reducing agent for use in the present invention include but is not limited to Reilly PDHP (3, 5-diethyl-1, 2-dihydro-1-phenyl-2-propylpyridine) from Vertellus.

[0103] The reductant may be present in the composition according to the present invention from 0.1 wt. %to 5 wt. %, based on the total weight of the component B, preferably from 0.5 wt. %to 5 wt. %and more preferably from 1 wt. %to 3 wt. %.

[0104] If the quantity of the reductant is less than 0.01 wt. %, it may not have desired and required cure speed, whereas higher quantity than 5 wt. %, may lead to instability of the adhesive.

[0105] Additives

[0106] The two-component acrylate composition according to present invention may further comprise optional additives in a component A and / or in the component B of the composition.

[0107] Non-limiting examples of optional additives are anti-shrinking agents, stabilizers, such as metal chelators; free radical stabilizers, such as dibutyl hydroxytoluene, ethylenediamine tetra acetic acid (EDTA) , p-benzoquinone; thickeners; fluorescent additives; dyes and mixtures thereof.

[0108] The component A and the component B of the composition according to the present invention may be mixed in a weight ratio of from 0.5 to 2.0: 1, or from 0.8: 1 to 1.2: 1, or from 0.9: 1 to 1.1: 1, preferably at 1: 1.

[0109] Preparing Method of the two-component acrylate composition

[0110] The two-component acrylate compositions are formulated by simple mixing of the various components of component A and component B separately. Whilst the order of mixing of the components is not intended to be limited, it may be prudent to keep the initiator and catalyst / reducing agent in different components.

[0111] The present invention also relates to the use of the two-component acrylate structural adhesive composition according to the present invention as a structural adhesive in speaker magnet bonding, e-motor structural bonding and metal component bonding. The two-component acrylate composition being used to bond a neodymium iron boron (NdFeB) substrate and a metallic substrate, the component A being used on the metallic substrate and the component B being used on the neodymium iron boron (NdFeB) substrate.

[0112] The present invention relates to a method of bonding two substrates comprising the following steps:

[0113] 1) applying component A of a two-component acrylate composition according to the present invention to a metallic substrate;

[0114] 2) applying component B of a two-component acrylate composition according to the present invention to a neodymium iron boron (NdFeB) substrate;

[0115] 3) overlaying the metallic substrate on the neodymium iron boron (NdFeB) substrate or overlaying the neodymium iron boron (NdFeB) substrate on the metallic substrate; and

[0116] 4) bonding the metallic substrate to the neodymium iron boron (NdFeB) substrate by mixing the component A and the component B of the two-component acrylate composition and curing the composition.

[0117] The compositions according to the present invention may be applied to a variety of metallic substrates to perform with the desired benefits and advantages described herein. For instance, appropriate metallic substrates may be constructed from steel, zinc dichromate coated steel, zinc chromate coated steel, nickel, nickel coated steel, galvanized steel, zinc phosphate coated steel, zinc-flake coated steel, and mixtures thereof.

[0118] Prior to applying the compositions, the relevant surfaces don’ t need any pre-treatments.

[0119] After applying the compositions, controlling the gap between the metallic substrate and the neodymium magnet substrate in a range of 0.01 mm to 0.5 mm and preferable in a range of 0.1 mm to 0.2 mm during the above step 3) overlaying and step 4) bonding.

[0120] It was found surprisingly that the controlled gap between the metallic substrate and the neodymium magnet substrate help to control the cure rate greater than the mixing rate of the component A and component B. In some embodiments, the gap between the metallic substrate and the neodymium magnet substrate in from 0.01 mm to 0.5 mm, or from 0.02 mm to 0.4 mm, or from 0.05 mm to 0.35 mm, or from 0.07 mm to 0.3 mm, or 0.09 mm to 0.35 mm, or 0.1 mm to 0.2 mm.

[0121] In the article comprising a bonding product made according to the method of present invention, the content of the adhesion promoter in the acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate. The content of the second (meth) acrylate monomer which being reactive with metal in acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate. The content of the soft (meth) acrylate monomer in acrylate composition showing a concentration gradient, with an increasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate.

[0122] The curing of the compositions of the invention typically occurs at temperatures in the range of from 10℃ to 40℃, from 20℃ to 30℃, preferably from 23℃ to 27℃. The temperature that is suitable depends on the specific compounds present and the desired curing rate and can be determined in the individual case by the skilled artisan, using simple preliminary tests if necessary.

[0123] Listing of Embodiments

[0124] 1. A two-component acrylate composition comprises a component A and a component B,

[0125] the component A comprising:

[0126] a) a first (meth) acrylate monomer,

[0127] b) a second (meth) acrylate monomer which being reactive with metal,

[0128] c) an adhesion promoter,

[0129] d) a rubber toughening agent,

[0130] e) a peroxide initiator,

[0131] the component B comprising:

[0132] a) a first (meth) acrylate monomer,

[0133] d) a rubber toughening agent,

[0134] f) a soft (meth) acrylate monomer,

[0135] g) a catalyst,

[0136] h) a reductant,

[0137] wherein the two-component acrylate composition being used to bond a neodymium magnet substrate and a metallic substrate, the component A being used on the metallic substrate and the component B being used on the neodymium magnet substrate.

[0138] 2. The two-component acrylate composition of embodiment 1, wherein the first (meth) acrylate monomer comprises aromatic acrylate monomer, heterocyclic acrylate monomer and aliphatic acrylate monomer.

[0139] 3. The two-component acrylate composition of any one of preceding embodiments, wherein the first (meth) acrylate monomers in component A and component B are the same or different.

[0140] 4. The two-component acrylate composition of any one of preceding embodiments, wherein the first (meth) acrylate monomer is present from 30 wt. %to 80 wt. %, or from 42 wt. %to 65 wt. %, based on the total weight of the two-component acrylate composition.

[0141] 5. The two-component acrylate composition of any one of preceding embodiments, wherein the second (meth) acrylate monomer which being reactive with metal comprises one or more selected from methyl methacrylate (MAA) , methyl acrylate (MA) , tetrahydrofurfuryl (meth) acrylate (THF (M) A) and β-carboxyethylacrylate (β-ECA) .

[0142] 6. The two-component acrylate composition of any one of preceding embodiments, wherein the second (meth) acrylate monomer is present from 5 wt. %to 30 wt. %, or from 12 wt. %to 20 wt. %, based on the total weight of the component A.

[0143] 7. The two-component acrylate composition of any one of preceding embodiments, wherein the rubber toughening agent is liquid or solid natural or synthetic rubber elastomeric polymer, preferably selected from the group consisting of polybutadienes, functionalized polybutadienes, polyisobutylenes, functionalized polyisobutylenes, butadiene-acrylonitrile copolymers, functionalized butadiene-acrylonitrile copolymers, functionalized styrenebutadiene copolymers, styrene butadiene copolymers, polyisoprenes, ethylenepropylene copolymers, and mixtures thereof.

[0144] 8. The two-component acrylate composition of any one of preceding embodiments, wherein the rubber toughening agent in component A and component B are the same or different.

[0145] 9. The two-component acrylate composition of any one of preceding embodiments, wherein the rubber toughening agent is present from 10 wt. %to 40 wt. %, or from 15 wt. %to 30 wt. %, based on the total weight of the composition.

[0146] 10. The two-component acrylate composition of any one of preceding embodiments, wherein the adhesion promoter is a phosphoric acid (meth) acrylate, preferably selected from the group consisting of phosphoric acid 2-hydroxymethyl methacrylate ester, 2-methacryloyloxyethyl acid phosphate, mono- (2-hydroxyethylmethacrylate) phosphate, 2-hydroxyethylmethylacrylate acid phosphate, bis (2-methacryloxyethyl) phosphate and mixtures thereof, preferably the adhesion promoter is 2-hydroxyethylmethylacrylate acid phosphate.

[0147] 11. The two-component acrylate composition of any one of preceding embodiments, wherein the adhesion promoter is present from 0.01 wt. %to 2 wt. %, or from 0.1 wt. %to 2 wt. %, or from 0.2 wt. %to 2 wt. %, based on the total weight of the component A.

[0148] 12. The two-component acrylate composition of any one of preceding embodiments, wherein the peroxide initiator comprises one or more selected from cyclic peroxides, diacyl peroxides, dialkyl peroxides, hydroperoxides, peroxycarbo nates, peroxydicarbonates, peroxyesters, and peroxyketals, more preferably selected from the group consisting cumene hydroperoxide (CHP) , para-menthane hydroperoxide, t-butyl hydroperoxide (TBH) , t-butyl peroxybenzoate, t-butyl peroxy pivalate, di-t-butyl peroxide, t-butyl peroxy acetate, t-butyl peroxy-2-hexanoate, t-amyl hydroperoxide, 1 , 2, 3, 4-tetramethylbutyl hydroperoxide, benzoyl peroxide, dibenzoyl peroxide, 1 , 3-bis (t-butylperoxyisopropyl) benzene, diacetyl peroxide, butyl 4, 4-bis (t-butylperoxy) valerate, p-chlorobenzoyl peroxide, t-butyl cumyl peroxide, di-t-butyl peroxide, dicumyl peroxide, di (dodecanoyl) peroxide, 2, 5-dimethyl-2, 5-di-t-butylperoxyhexane, 2, 5-dimethyl-2, 5-di-t-butyl-peroxyhex-3-yne, 4-methyl-2, 2-di-t-butylperoxypentane.

[0149] 13. The two-component acrylate composition of any one of preceding embodiments, wherein the peroxide initiator is present from 2.5 wt. %to 7 wt. %, or from 2.5 wt. %to 6 wt. %, or from 3 wt. %to 5 wt. %, based on the total weight of the component A.

[0150] 14. The two-component acrylate composition of any one of preceding embodiments, wherein the soft (meth) acrylate monomer comprises aliphatic acrylic monomer comprising straight or branched alkyl group having from 12 to 22, or from 12 to 18 carbon atoms.

[0151] 15. The two-component acrylate composition of any one of preceding embodiments, wherein the soft (meth) acrylate monomer is present from 15 wt. %to 40 wt. %, or from 20 wt. %to 25 wt. %, based on the total weight of the component B.

[0152] 16. The two-component acrylic structural adhesive composition of any one of preceding embodiments, wherein the catalyst is organic metal salts.

[0153] 17. The two-component acrylate composition of any one of preceding embodiments, wherein the catalyst is present from 0.06 wt. %to 3 wt. %, or from 0.08 wt. %to 2 wt. %, based on the total weight of the component B.

[0154] 18. The two-component acrylic structural adhesive composition of any one of preceding embodiments, wherein the reductant is an amine compound.

[0155] 19. A structural adhesive comprising a cured product of the two-component acrylate composition according to any one of embodiments 1-18.

[0156] 20. An article comprising a neodymium magnet substrate, a metallic substrate and a structural adhesive bonded the neodymium magnet substrate and the metallic substrate, wherein the structural adhesive is the cured product of the two-component acrylate composition according to any one of embodiments 1-18.

[0157] 21. A speaker, a motor or a metal component comprises an article of embodiment 20.

[0158] 22. A method of bonding two substrates comprising steps:

[0159] 1) applying a component A of a two-component acrylate composition according to any one of embodiments 1-18 to a metallic substrate to be bonded,

[0160] 2) applying a component B of a two-component acrylate composition according to any one of claims 1-16 to a neodymium magnet substrate to be bonded,

[0161] 3) overlaying the metallic substrate on the neodymium magnet substrate or overlaying the neodymium magnet substrate on the metallic substrate; and

[0162] 4) bonding the metallic substrate to the neodymium magnet substrate by mixing the component A and the component B of the two-component acrylate composition and curing the composition.

[0163] 23. The method of embodiment 22, wherein, controlling the gap between the metallic substrate and the neodymium magnet substrate in a range of 0.01 mm to 0.5 mm, or in a range of 0.1 mm to 0.2 mm during the step 3) overlaying and step 4) bonding.

[0164] 24. An article comprising a bonding product made according to any one of embodiments 22-23, wherein

[0165] 1) the content of the adhesion promoter in the acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate,

[0166] 2) the content of the second (meth) acrylate monomer which being reactive with metal in acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate,

[0167] 3) the content of the soft (meth) acrylate monomer in acrylate composition showing a concentration gradient, with an increasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate.

[0168] Examples:

[0169] The present invention will be further described and illustrated in detail with reference to the following examples. The examples are intended to assist one skilled in the art to better understand and practice the present invention, however, are not intended to restrict the scope of the present invention. All numbers in the examples are based on weight unless otherwise stated.

[0170] Raw Materials *All raw materials are directly used without any special treatment.

[0171] Example 1

[0172] <Preparation of two-component acrylate composition>i

[0173] Compositions of the invention comprise the following raw materials at the indicated levels. The component A was obtained by first adding the acrylate monomers to a vessel and mixing at 5℃-25℃ for 5-20 minutes. The toughening agent and additive were then added and mixed at 30-50℃ until a smooth homogeneous liquid was obtained. The adhesion promoter and initiator were then added at 5-25℃ for 5-10 minutes.

[0174] The component B was obtained by first adding the acrylate monomers to a vessel and mixing at 5℃-25℃ for 5-20 minutes. The toughening agent and glass beads were then added and mixed at 30-50℃ until a smooth homogeneous liquid was obtained. The catalyst and reductant were then added at 5-25℃ for 15-30 minutes. Vacuum is preferred during mixing to reduce the trapped air bubbles.

[0175] <Curing of two-component acrylate composition>

[0176] The compositions were applied to the substrate by Dispensing. The thickness was controlled from about 0.01 mm to about 0.5 mm under ambient temperature. After application on the substrate, the composition was typically cured at ambient temperature for at least about 0.25 minutes, more typically from about 0.75 to about 1.75 minutes.

[0177] Example 2-8, and CE1-CE8

[0178] The compositions of E2 to E8, CE1 to CE8 were prepared in reference to Example 1. The composition of E2 to E8 and CE1 to CE8 were cured in reference to Example 1. More details are listed in the result part. For E2 to E8, CE1 to CE8, the full curing of the compositions was performed at ambient temperature for 24 hours.

[0179] Test Methods

[0180] <Push out force>

[0181] The push out force test was carried out to determine the bonding strength of the structural adhesive. The adhesive was used to bond galvanized steel with NdFeB and then cured for 24hrs. The size of galvanized was Φ35mm × 5mm and the NdFeB was Φ50mm × 15mm with a hollow of Φ15mm ×15mm. The push force test was carried out to determine the force required to separate galvanized steel and NdFeB by Instron universal testing machine.

[0182] Push out force results are recorded and ranked as follows (initial push out force) :

[0183] - Not pass: the push out force is less than 1000N.

[0184] - Pass: the push out force is equal to or greater than 1000N.

[0185] <High temperature aging / heat aging>

[0186] The test specimens were put into an oven with a setting temperature of 150℃. After 336 hrs., the aging was over. Then test the push out force of the specimens.

[0187] High temperature aging results are recorded and ranked as follows:

[0188] - Not pass: the push out force is less than 1000N.

[0189] - Pass: the push out force is equal to or greater than 1000N.

[0190] <Thermal shock>

[0191] The test specimens were put into a thermal shock environmental test chamber. The temperature of the upper chamber was set to 95℃ and the temperature of the lower chamber was set to -40℃ relatively. The specimens stayed in the upper chamber for 60 minutes, and then in the lower chamber for another 60 minutes. This was recorded as one cycle. The specimen must be transferred from one chamber to another within 15 seconds. After 200 cycles, the aging test was finished. Then test the push out force of the specimens.

[0192] If there is a shift of more than 0.5 mm between two assembled parts, mark it as a magnet shift.

[0193] Thermal shock results are recorded and ranked as follows:

[0194] - Not pass: the push out force is less than 200N or magnet shift.

[0195] - Pass: the push out force is equal to or greater than 200N.

[0196] - Good: the push out force is equal to or greater than 300N.

[0197] <HTHH (High Temperature High Humidity) aging>

[0198] The test specimens were put into an environmental testing chamber with a setting temperature of 85℃ and humidity of 85%. After 336 hrs., the aging was over. In stricter test, the aging test would last for 500 hrs.

[0199] If red rust was observed on the surface of magnets after HTHH test, mark the test specimen as Y. If not, mark the test specimen as N.

[0200] <Fixture time test>

[0201] The fixture time test was to determine the time at which an adhesive bond developed handling strength. In this test, a sufficient quantity of adhesive was applied to the prepared surface of each lap-shear specimen such that when the mating lap-shear specimen was placed on top of the adhesive a 322.6 mm2 (0.5 in. 2) area would be completely covered. Then clamped the assembly on each side of the bond area approximately 6.4mm and let the adhesive cure for some certain periods. After that, a 3kg object was hung on the lap shear specimen and lifted the lap shear specimen up for 5 seconds. If the mating lap shear specimen did not separate, recorded the result as “Pass” . Recorded the minimum time to pass such test as the ultimate “fixture time” of the adhesive.

[0202] If the fixture time is equal to or less than 100 seconds, mark the result as “Pass” ; if the fixture time is equal to or less than 60 seconds, mark the result as “Good” .

[0203] Table 1.

[0204] Table 1 shows the 2-component acrylate compositions of E1-E8.

[0205] Table 2.

[0206] Table 2 shows testing results of the two-component acrylate compositions E1-E8.

[0207] *The magnetic steel basin frame breaks when the push out force is greater than 1500N.

[0208] Table 3.

[0209] Table 3 shows the two-component acrylate compositions of CE1-CE8.

[0210] Table 4.

[0211] Table 4 shows testing results of the two-component acrylate compositions of CE1-CE8.

[0212] Table 5.

[0213] Table 5 shows testing results of composition E1 under different operating parameters.

[0214] *Gap control: N means no gap control / 0 gap control, 0.127mm means the gap between two substrates is controlled by 0.127mm aluminum spacer.

[0215] *Pre-mix A and B means: Mixed component A and component B well and then apply mixed composition on one substrate. The open time is approximately 1 minute. To avoid gelation after the open time, a 2K dispensing nozzle is usually used.

[0216] In comparative examples CE1 and CE2, the soft (meth) acrylate monomer is partially or completely in component A, resulting in an unqualified push out force after thermal shock test. The content of the soft (meth) acrylate monomer in the acrylate composition shows a concentration gradient, with an increasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate. It was found in present invention that such trend doesn’ t impact on the overall thermal strength of structural adhesive, but the internal stress between the structural adhesive and NdFeB is greatly decreased by this design which provides good anti-thermal shock property.

[0217] CE3, CE4, CE5 and E5 comprise different first (meth) acrylate monomers in the component B. It can be seen from the push out force after thermal shock result, without the (meth) acrylate monomers comprising an aromatic moiety in the component B, the structural adhesives can’t pass the thermal shock test.

[0218] Compared the High Temperature High Humidity aging result of E1 and CE6, the phosphoric acid (meth) acrylate adhesion promoter in component B cause corrosion on NdFeB Magnet substrate but adding phosphoric acid (meth) acrylate adhesion promoter in component A can avoid corrosion. Of course, the unique bead-on-bead applying method also contributed to the good anti-corrosion result.

[0219] From the result of CE8, insufficient amount of peroxide initiator and catalyst reduce the curing speed. When the mixing speed of component A and component B is higher than the curing speed, it is hard to produce a structural adhesive with concentration gradient. The results are similar to pre-mixed two-component adhesive.

Claims

1.A two-component acrylate composition comprises a component A and a component B,the component A comprising:a) a first (meth) acrylate monomer,b) a second (meth) acrylate monomer which being reactive with metal,c) an adhesion promoter,d) a rubber toughening agent,e) a peroxide initiator,the component B comprising:a) a first (meth) acrylate monomer,d) a rubber toughening agent,f) a soft (meth) acrylate monomer,g) a catalyst,h) a reductant,wherein the two-component acrylate composition being used to bond a neodymium magnet substrate and a metallic substrate, the component A being used on the metallic substrate and the component B being used on the neodymium magnet substrate.2.The two-component acrylate composition of claim 1, wherein the first (meth) acrylate monomer comprises aromatic acrylate monomer, heterocyclic acrylate monomer and aliphatic acrylate monomer.3.The two-component acrylate composition of claim 1, wherein the first (meth) acrylate monomers in component A and component B are the same or different.4.The two-component acrylate composition of claim 1, wherein the first (meth) acrylate monomer is present from 30 wt. %to 80 wt. %, or from 42 wt. %to 65 wt. %, based on the total weight of the two-component acrylate composition.5.The two-component acrylate composition of claim 1, wherein the second (meth) acrylate monomer which being reactive with metal comprises one or more selected from methyl methacrylate (MAA) , methyl acrylate (MA) , tetrahydrofurfuryl (meth) acrylate (THF (M) A) and β-carboxyethylacrylate (β-ECA) .6.The two-component acrylate composition of claim 1, wherein the second (meth) acrylate monomer is present from 5 wt. %to 30 wt. %, or from 12 wt. %to 20 wt. %, based on the total weight of the component A.7.The two-component acrylate composition of claim 1, wherein the rubber toughening agent is liquid or solid natural or synthetic rubber elastomeric polymer, preferably selected from the group consisting of polybutadienes, functionalized polybutadienes, polyisobutylenes, functionalized polyisobutylenes, butadiene-acrylonitrile copolymers, functionalized butadiene-acrylonitrile copolymers, functionalized styrenebutadiene copolymers, styrene butadiene copolymers, polyisoprenes, ethylenepropylene copolymers, and mixtures thereof.8.The two-component acrylate composition of claim 1, wherein the rubber toughening agent in component A and component B are the same or different.9.The two-component acrylate composition of claim 1, wherein the rubber toughening agent is present from 10 wt. %to 40 wt. %, or from 15 wt. %to 30 wt. %, based on the total weight of the composition.10.The two-component acrylate composition of claim 1, wherein the adhesion promoter is a phosphoric acid (meth) acrylate, preferably selected from the group consisting of phosphoric acid 2-hydroxymethyl methacrylate ester, 2-methacryloyloxyethyl acid phosphate, mono- (2-hydroxyethylmethacrylate) phosphate, 2-hydroxyethylmethylacrylate acid phosphate, bis (2-methacryloxyethyl) phosphate and mixtures thereof, preferably the adhesion promoter is 2-hydroxyethylmethylacrylate acid phosphate.11.The two-component acrylate composition of claim 1, wherein the adhesion promoter is present from 0.01 wt. %to 2 wt. %, or from 0.1 wt. %to 2 wt. %, or from 0.2 wt. %to 2 wt. %, based on the total weight of the component A.12.The two-component acrylate composition of claim 1, wherein the peroxide initiator comprises one or more selected from cyclic peroxides, diacyl peroxides, dialkyl peroxides, hydroperoxides, peroxycarbo nates, peroxydicarbonates, peroxyesters, and peroxyketals, more preferably selected from the group consisting cumene hydroperoxide (CHP) , para-menthane hydroperoxide, t-butyl hydroperoxide (TBH) , t-butyl peroxybenzoate, t-butyl peroxy pivalate, di-t-butyl peroxide, t-butyl peroxy acetate, t-butyl peroxy-2-hexanoate, t-amyl hydroperoxide, 1 , 2, 3, 4-tetramethylbutyl hydroperoxide, benzoyl peroxide, dibenzoyl peroxide, 1 , 3-bis (t-butylperoxyisopropyl) benzene, diacetyl peroxide, butyl 4, 4-bis (t-butylperoxy) valerate, p-chlorobenzoyl peroxide, t-butyl cumyl peroxide, di-t-butyl peroxide, dicumyl peroxide, di (dodecanoyl) peroxide, 2, 5-dimethyl-2, 5-di-t-butylperoxyhexane, 2, 5-dimethyl-2, 5-di-t-butyl-peroxyhex-3-yne, 4-methyl-2, 2-di-t-butylperoxypentane.13.The two-component acrylate composition of claim 1, wherein the peroxide initiator is present from 2.5 wt. %to 7 wt. %, or from 2.5 wt. %to 6 wt. %, or from 3 wt. %to 5 wt. %, based on the total weight of the component A.14.The two-component acrylate composition of claim 1, wherein the soft (meth) acrylate monomer comprises aliphatic acrylic monomer comprising straight or branched alkyl group having from 12 to 22, or from 12 to 18 carbon atoms.15.The two-component acrylate composition of claim 1, wherein the soft (meth) acrylate monomer is present from 15 wt. %to 40 wt. %, or from 20 wt. %to 25 wt. %, based on the total weight of the component B.16.The two-component acrylic structural adhesive composition of claim 1, wherein the catalyst is organic metal salts.17.The two-component acrylate composition of claim 1, wherein the catalyst is present from 0.06 wt. %to 3 wt. %, or from 0.08 wt. %to 2 wt. %, based on the total weight of the component B.18.The two-component acrylic structural adhesive composition of claim 1, wherein the reductant is an amine compound.19.A structural adhesive comprising a cured product of the two-component acrylate composition according to any one of claims 1-18.20.An article comprising a neodymium magnet substrate, a metallic substrate and a structural adhesive bonded the neodymium magnet substrate and the metallic substrate, wherein the structural adhesive is the cured product of the two-component acrylate composition according to any one of claims 1-18.21.A speaker, a motor or a metal component comprises an article of claim 20.22.A method of bonding two substrates comprising steps:1) applying a component A of a two-component acrylate composition according to any one of claims 1-18 to a metallic substrate to be bonded,2) applying a component B of a two-component acrylate composition according to any one of claims 1-16 to a neodymium magnet substrate to be bonded,3) overlaying the metallic substrate on the neodymium magnet substrate or overlaying the neodymium magnet substrate on the metallic substrate; and4) bonding the metallic substrate to the neodymium magnet substrate by mixing the component A and the component B of the two-component acrylate composition and curing the composition.23.The method of claim 22, wherein controlling the gap between the metallic substrate and the neodymium magnet substrate in a range of 0.01 mm to 0.5 mm, or in a range of 0.1 mm to 0.2 mm during the step 3) overlaying and step 4) bonding.24.An article comprising a bonding product made according to any one of claims 22-23, wherein1) the content of the adhesion promoter in the acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate,2) the content of the second (meth) acrylate monomer which being reactive with metal in acrylate composition showing a concentration gradient, with a decreasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate,3) the content of the soft (meth) acrylate monomer in acrylate composition showing a concentration gradient, with an increasing trend in the direction of the modified concentration gradient from the metallic substrate to the neodymium magnet substrate.