Cementitious mortar material and preparation method therefor, and composite marble formed therefrom

By improving the mortar material, using a mortar composed of hybrid silica emulsion, cement, quartz sand, etc., the problems of traditional composite marble being heavy, brittle, and costly have been solved, achieving high strength and low-cost construction of ultra-thin composite marble.

WO2026232664A1PCT designated stage Publication Date: 2026-11-12NATURE NEW MATERIAL TECHNOLOGY (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/100474
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2025-06-11
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Traditional composite marble is heavy and brittle, costly, and difficult to automate. The mortar has poor water resistance and low bonding strength. Ultra-thin composite marble has insufficient strength and is inconvenient to construct.

Method used

Hybridized silica emulsions are used to improve mortar materials, including cement, quartz sand, basalt fiber, etc. Organic-inorganic hybrid technology is used to improve the adhesion and water resistance of the mortar and the workability of cement to prepare ultra-thin composite marble.

Benefits of technology

The resulting composite marble is thin, lightweight, has high bonding strength and water resistance, high construction efficiency, low cost, and is suitable for automated production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025100474-FTAPPB-I100001
    Figure PCTCN2025100474-FTAPPB-I100001
Patent Text Reader

Abstract

A cementitious mortar material and a preparation method therefor, and composite marble formed therefrom. The cementitious mortar material comprises the following raw materials in percentages by mass: 5-45% of cement, 10-78% of quartz sand, 0.5-1% of calcium formate, 0.2-0.5% of basalt fibers, 5-25% of a hybrid silicon emulsion, 0.2-0.6% of hydroxypropyl methyl cellulose, 0.1-0.3% of a defoaming agent, 0.1-0.3% of potassium methyl siliconate, and 5-20% of water.
Need to check novelty before this filing date? Find Prior Art

Description

A putty material, its preparation method, and the composite marble thereof. Technical Field

[0001] This invention belongs to the field of composite marble preparation technology, and specifically relates to a putty material and its preparation method, and the composite marble formed therefrom. Background Technology

[0002] Traditional composite marble is typically 12-20mm thick, weighing 35kg-55kg per square meter, resulting in high costs, as well as significant expenses for transportation, handling, and installation. To overcome the drawbacks of traditional stone due to its excessive thickness and fragility, ultra-thin stone slabs often employ composite materials such as ceramic tiles, slabs, granite, aluminum honeycomb, plastic honeycomb, and fiberglass honeycomb. While composite ceramic tiles, slabs, and granite can reduce costs to some extent, the weight reduction effect is limited. Composite aluminum honeycomb, plastic honeycomb, and fiberglass honeycomb solutions can significantly reduce weight, but these are costly and only reduce costs for high-end stone; for mid- to low-end stone, they may even increase costs, and none of these methods allow for automated production. Furthermore, 1-8mm thick natural ultra-thin composite marble has poor strength, is prone to cracking, and lacks the properties suitable for installation and handling.

[0003] To achieve high performance in ultra-thin composite marble, a specialized high-performance cement-based polymer was developed as the substrate. Traditional cement polymer mortar mainly consists of quartz sand, cement, dry powder latex, early-strength agents, carboxymethyl cellulose, and crack-resistant fibers. The key component is the dry powder latex, which is a PVA (polyvinyl alcohol)-coated vinyl acetate polymer. PVA has poor water resistance, and vinyl acetate polymers readily hydrolyze into hydrophilic monomers in strongly alkaline environments, resulting in poor water resistance and low bonding strength in traditional mortars. Currently, some high-performance water-resistant emulsions on the market have good hydrophobic properties, but poor workability with cement and poor wet bonding performance. Summary of the Invention

[0004] To address the above problems, this invention provides a putty material, its preparation method, and a composite marble thereof.

[0005] The first objective of this invention is achieved through the following technical solution:

[0006] A putty material, by weight percentage, comprises the following raw materials: 5-45% cement, 10-78% quartz sand, 0.5-1% calcium formate, 0.2-0.5% basalt fiber, 5-25% hybrid silica emulsion, 0.2-0.6% hydroxypropyl methylcellulose, 0.1-0.3% defoamer, 0.1-0.3% potassium methylsilicate, and 5-20% water.

[0007] Preferably, the putty material, by weight percentage, comprises the following raw materials: 5-45% cement, 5-65% 80-90 mesh quartz sand, 5-25% 100-120 mesh quartz sand, 0.5-1% calcium formate, 0.2-0.5% basalt fiber, 5-25% hybrid silicone emulsion, 0.2-0.6% hydroxypropyl methylcellulose, 0.1-0.3% defoamer, 0.1-0.3% potassium methylsilicate, and 5-20% water.

[0008] Further, the hybrid silicone emulsion comprises the following raw materials in parts by weight: 75-85 parts of inorganic-organic hybrid styrene-acrylate polymer emulsion, 10-30 parts of ethylene glycol butyl ether, 1-5 parts of polysiloxane coupling agent, 3-8 parts of cyclodimethylsilane, 5-15 parts of vinyltrimethoxysilane, and 0.25-0.8 parts of benzoyl peroxide.

[0009] Furthermore, the inorganic-organic hybrid styrene-acrylate polymer emulsion is preferably BASF Ancouli Plus 7602.

[0010] Furthermore, the preparation of the hybrid silicon emulsion includes:

[0011] The inorganic-organic hybrid styrene-acrylate polymer emulsion was heated to 80-90℃, and ethylene glycol butyl ether was added while maintaining the temperature. After stirring evenly, polysiloxane coupling agent, cyclodimethylsilane, vinyltrimethoxysilane and benzoyl peroxide were added in sequence. The mixture was kept warm and stirred for 3-6 hours, and then cooled to obtain the hybrid silicone emulsion.

[0012] Furthermore, the cement has a particle size of 400-450 mesh, preferably 425 mesh;

[0013] Preferably, the cement is white cement, which has a weaker alkalinity during hydration, thus preventing efflorescence from contaminating the stone during curing.

[0014] Furthermore, the length of the basalt fiber is 2.5-3.5 mm, preferably 3 mm. The basalt fiber can increase the overall shear strength of the composite marble by more than 30%.

[0015] The second objective of this invention is achieved through the following technical solution:

[0016] A method for preparing a putty material includes:

[0017] After mixing water, hybrid silica emulsion, carboxymethyl cellulose, defoamer and potassium methylsilicate evenly, cement, calcium formate and quartz sand are added in sequence and mixed evenly to obtain the putty material.

[0018] Furthermore, the quartz sand is composed of quartz sand with different particle sizes, and the quartz sand is added in order of decreasing particle size.

[0019] The third objective of this invention is achieved through the following technical solution:

[0020] A composite marble comprising a surface layer and a base layer bonded to the back of the surface layer;

[0021] The base layer is obtained by pouring the aforementioned putty material into a mesh cloth and then curing it.

[0022] Furthermore, the surface layer is a natural stone with a thickness of 1-8 mm.

[0023] Furthermore, the thickness of the base layer is 1-2 mm.

[0024] Furthermore, the preparation of the composite marble includes:

[0025] A mesh fabric is laid on the back of the surface layer, and then the above-mentioned putty material is poured into the mesh fabric and cured at room temperature to obtain composite marble.

[0026] Furthermore, the curing time is more than 7 days.

[0027] Furthermore, the mesh fabric is made of fiberglass mesh, carbon fiber mesh, or aramid mesh.

[0028] The beneficial effects of this invention are:

[0029] The present invention discloses a putty material, its preparation method, and a composite marble thereof, wherein a hybrid silicon emulsion is introduced into the putty material, and the hybrid silicon emulsion has the following advantages:

[0030] First, it is synthesized using organic and inorganic silicon hybrid technology. The organic silicon segments can be hydrolyzed to form silanol groups, which condense with the hydroxyl groups on the stone surface to form bonds. Therefore, it gives the putty material excellent adhesion to the stone surface, making the bonding strength between the base layer and the surface layer in this invention reach more than 1.0 MPa.

[0031] Secondly, because organosilicon has low surface tension and a large water contact angle, it gives the composite marble base layer excellent water resistance.

[0032] Third, the inorganic silicon segments are similar in composition to cement, and they have excellent workability with cement.

[0033] The composite marble obtained by this invention is an ultra-thin marble slab with a thickness of less than 10mm. At this thickness, the composite marble can withstand the impact of a falling ball of more than 10J without breaking. The weight per square meter is only about 15kg. This makes the composite marble slab not only cheaper in terms of material cost than traditional thick solid marble, but also easier to transport and handle. Wall installation does not require dry hanging. After the substrate is leveled, a hard-bottom thin-laying process is used. The ground does not require a very thick semi-dry mortar construction. A hard-bottom thin-laying process is also used. The construction efficiency is high and the overall cost is low.

[0034] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures pointed out in the description and claims. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preparation of putty materials:

[0038] A1. Prepare the following raw materials in parts by weight: 75 parts BASF Ancouli Plus 7602, 30 parts ethylene glycol butyl ether, 2 parts Dow Corning 11-100, 3 parts cyclodimethylsilane, 5 parts vinyltrimethoxysilane, and 0.25 parts benzoyl peroxide; heat BASF Ancouli Plus 7602 to 80°C, keep warm and add ethylene glycol butyl ether, stir evenly, then add Dow Corning 11-100, cyclodimethylsilane, vinyltrimethoxysilane and benzoyl peroxide in sequence, keep warm and stir for 5 hours, cool to obtain hybrid silicone emulsion.

[0039] A2. Prepare the following raw materials by weight: 30% 425-mesh white cement, 30% 80-90-mesh quartz sand, 15% 100-120-mesh quartz sand, 0.6% calcium formate, 0.2% basalt fiber (3mm in length), 15% hybrid silica emulsion obtained in step A1, 0.2% hydroxypropyl methylcellulose, 0.2% defoamer (PD-1 defoamer in this example), 0.2% potassium methylsilicate, and the remainder is water. After mixing the water, hybrid silica emulsion, carboxymethyl cellulose, defoamer, and potassium methylsilicate evenly, add the cement, calcium formate, 80-90-mesh quartz sand, and 100-120-mesh quartz sand in sequence, and mix evenly to obtain the putty material.

[0040] Example 2

[0041] Preparation of putty materials:

[0042] A1. Prepare the following raw materials in parts by weight: 80 parts BASF Ancouli Plus 7602, 20 parts ethylene glycol butyl ether, 2 parts Dow Corning 11-100, 4 parts cyclodimethylsilane, 10 parts vinyltrimethoxysilane, and 0.5 parts benzoyl peroxide; heat BASF Ancouli Plus 7602 to 85°C, keep warm and add ethylene glycol butyl ether, stir evenly, then add Dow Corning 11-100, cyclodimethylsilane, vinyltrimethoxysilane and benzoyl peroxide in sequence, keep warm and stir for 5 hours, cool to obtain hybrid silicone emulsion.

[0043] A2. Prepare the following raw materials by weight: 15% 425-mesh white cement, 50% 80-90-mesh quartz sand, 10% 100-120-mesh quartz sand, 0.5% calcium formate, 0.2% basalt fiber (3mm in length), 12% hybrid silica emulsion obtained in step A1, 0.2% hydroxypropyl methylcellulose, 0.1% defoamer (PD-1 defoamer in this example), 0.2% potassium methylsilicate, and the remainder is water. After mixing the water, hybrid silica emulsion, carboxymethyl cellulose, defoamer, and potassium methylsilicate evenly, add the cement, calcium formate, 80-90-mesh quartz sand, and 100-120-mesh quartz sand in sequence, and mix evenly to obtain the putty material.

[0044] Example 3

[0045] Preparation of putty materials:

[0046] A1. Prepare the following raw materials in parts by weight: 85 parts BASF Ancouli Plus 7602, 10 parts ethylene glycol butyl ether, 5 parts Dow Corning 11-100, 8 parts cyclodimethylsilane, 15 parts vinyltrimethoxysilane, and 0.8 parts benzoyl peroxide; heat BASF Ancouli Plus 7602 to 90°C, keep warm and add ethylene glycol butyl ether, stir evenly, then add Dow Corning 11-100, cyclodimethylsilane, vinyltrimethoxysilane and benzoyl peroxide in sequence, keep warm and stir for 6 hours, cool to obtain a hybrid silicone emulsion.

[0047] A2. Prepare the following raw materials by weight: 45% 425-mesh white cement, 10% 80-90-mesh quartz sand, 20% 100-120-mesh quartz sand, 1% calcium formate, 0.3% basalt fiber (3mm in length), 7.5% hybrid silica emulsion obtained in step A1, 0.6% hydroxypropyl methylcellulose, 0.3% defoamer (PD-1 defoamer in this example), 0.3% potassium methylsilicate, and the remainder is water. After mixing the water, hybrid silica emulsion, carboxymethyl cellulose, defoamer, and potassium methylsilicate evenly, add the cement, calcium formate, 80-90-mesh quartz sand, and 100-120-mesh quartz sand in sequence, and mix evenly to obtain the putty material.

[0048] Example 4

[0049] Preparation of composite marble slabs:

[0050] A mesh cloth was placed on the back of a 2mm thick natural stone (marble in this example), and the putty material prepared in Example 1 was poured into the mesh cloth (carbon fiber mesh cloth) (the putty layer thickness was 2mm). After curing at room temperature for 7 days, composite marble was obtained.

[0051] Example 5

[0052] Preparation of composite marble slabs:

[0053] A mesh cloth was placed on the back of a 5mm thick natural stone (marble in this example), and the putty material prepared in Example 2 was poured into the mesh cloth (carbon fiber mesh cloth) (the putty layer thickness was 2mm). After curing at room temperature for 7 days, composite marble was obtained.

[0054] Example 6

[0055] Preparation of composite marble slabs:

[0056] A mesh cloth was placed on the back of a natural stone with a thickness of 8 mm (marble is used as an example in this embodiment), and then the putty material prepared in Example 3 was poured into the mesh cloth (carbon fiber mesh cloth) (the putty layer thickness is 1 mm). After curing at room temperature for 7 days, composite marble was obtained.

[0057] Comparative Example 1

[0058] Preparation of composite marble slabs: Compared with Example 4, the putty material was replaced with traditional cement polymer putty (brand name: TTBII), and the rest remained the same.

[0059] Comparative Example 2

[0060] Preparation of composite marble slabs: Compared with Example 5, the putty material was replaced with traditional cement polymer putty (brand name: DAG TTBII), and the rest remained the same.

[0061] Comparative Example 3

[0062] Preparation of composite marble slabs: Compared with Example 6, the putty material was replaced with traditional cement polymer putty (brand name: TTBII), and everything else remained the same.

[0063] The physical properties of the composite marble slabs of Examples 4-6 and Comparative Examples 1-3 were tested, and the test results are shown in Table 1.

[0064] Table 1

[0065] As can be seen from Table 1, the composite marbles obtained in Examples 4-6 of the present invention have better resistance to the maximum height of a 1kg ball drop and better shear strength than those in Comparative Examples 1-3, and the bonding strength between the base layer and the surface layer is also better than that of the composite marbles in Comparative Examples 1-3.

[0066] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A putty material, characterized in that, By weight percentage, it includes the following raw materials: cement 5-45%, quartz sand 10-78%, calcium formate 0.5-1%, basalt fiber 0.2-0.5%, hybrid silicone emulsion 5-25%, hydroxypropyl methylcellulose 0.2-0.6%, defoamer 0.1-0.3%, potassium methylsilicate 0.1-0.3%, and water 5-20%.

2. The putty material according to claim 1, characterized in that, By weight percentage, it includes the following raw materials: cement 5-45%, 80-90 mesh quartz sand 5-65%, 100-120 mesh quartz sand 5-25%, calcium formate 0.5-1%, basalt fiber 0.2-0.5%, hybrid silicone emulsion 5-25%, hydroxypropyl methylcellulose 0.2-0.6%, defoamer 0.1-0.3%, potassium methylsilicate 0.1-0.3%, and water 5-20%.

3. The putty material according to claim 1, characterized in that, The hybrid silicone emulsion comprises the following raw materials in parts by weight: 75-85 parts of inorganic-organic hybrid styrene-acrylate polymer emulsion, 10-30 parts of ethylene glycol butyl ether, 1-5 parts of polysiloxane coupling agent, 3-8 parts of cyclodimethylsilane, 5-15 parts of vinyltrimethoxysilane, and 0.25-0.8 parts of benzoyl peroxide.

4. The putty material according to claim 1, characterized in that, The preparation of the hybrid silicon emulsion includes: The inorganic-organic hybrid styrene-acrylate polymer emulsion was heated to 80-90℃, and ethylene glycol butyl ether was added while maintaining the temperature. After stirring evenly, polysiloxane coupling agent, cyclodimethylsilane, vinyltrimethoxysilane and benzoyl peroxide were added in sequence. The mixture was kept warm and stirred for 3-6 hours, and then cooled to obtain the hybrid silicone emulsion.

5. The putty material according to claim 1, characterized in that, The cement has a particle size of 400-450 mesh.

6. A putty material according to any one of claims 1-5, characterized in that, The basalt fibers are 2.5-3.5 mm in length.

7. A method for preparing a putty material according to claims 1-6, characterized in that, include: After mixing water, hybrid silica emulsion, carboxymethyl cellulose, defoamer and potassium methylsilicate evenly, cement, calcium formate and quartz sand are added in sequence and mixed evenly to obtain the putty material.

8. A composite marble, characterized in that, Includes the top layer and the base layer bonded to the back of the top layer; The base layer is obtained by pouring the putty material described in claims 1-6 into the mesh fabric and then curing it.

9. A composite marble according to claim 8, characterized in that, The surface layer is made of natural stone with a thickness of 1-8mm.

10. A composite marble according to claim 8 or 9, characterized in that, The thickness of the base layer is 1-2 mm.