Cross-linked sulfonated polybenzimidazole membrane, preparation method therefor and use thereof

By grafting sulfonic acid groups onto the PBI membrane and forming a crosslinking network using a crosslinking agent, the problems of high cost of Nafion membrane and low conductivity of PBI membrane in vanadium redox flow batteries were solved, achieving high proton conductivity, low vanadium permeation and excellent chemical stability.

WO2026232726A1PCT designated stage Publication Date: 2026-11-12EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/120266
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2025-09-10
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The Nafion membrane used in existing vanadium redox flow batteries is expensive and has high vanadium ion permeability, while the PBI membrane has low conductivity, making it difficult to simultaneously meet the requirements of high proton conductivity, low vanadium permeability, and excellent chemical stability.

Method used

By grafting sulfonic acid groups onto the PBI membrane and using glycerol triglycidyl ether as a crosslinking agent, a crosslinking network is formed, constructing a dynamic hydrogen bond network, which improves proton transport channels and restricts vanadium ion diffusion.

Benefits of technology

It significantly improved the proton conductivity and ion selectivity of the membrane, reduced the vanadium ion permeability, and enhanced the electrochemical performance and stability of the all-vanadium redox flow battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025120266_12112026_PF_FP_ABST
    Figure CN2025120266_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention is a method for preparing a cross-linked sulfonated polybenzimidazole membrane, comprising the following steps: under a nitrogen atmosphere, adding polybenzimidazole to a first solvent, adding anhydrous potassium carbonate powder after reaction, then slowly adding a sulfonating agent to react, and performing work-up to obtain sulfonated polybenzimidazole; dissolving the sulfonated polybenzimidazole in a second solvent, adding a cross-linking agent, heating the mixture to react, and performing work-up to obtain a cross-linked sulfonated polybenzimidazole; and dissolving the cross-linked sulfonated polybenzimidazole in a third solvent, drying the mixture to obtain a cross-linked sulfonated polybenzimidazole membrane, and activating the cross-linked sulfonated polybenzimidazole membrane to obtain an activated cross-linked sulfonated polybenzimidazole membrane. The cross-linked sulfonated polybenzimidazole membrane provided by the present invention has both excellent proton conductivity and ion selectivity, exhibits excellent Coulombic efficiency and voltage efficiency in an all-vanadium redox flow battery, and has optimal battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

A cross-linked sulfonated polybenzimidazole membrane, its preparation method and application Technical Field

[0001] This invention belongs to the field of membrane technology for flow batteries, specifically, it relates to a cross-linked sulfonated polybenzimidazole membrane, its preparation method and application. Background Technology

[0002] In energy storage technology, electrochemical energy storage technology has received widespread attention and has developed rapidly. In particular, redox flow batteries (RFBs) are considered an ideal choice for large-scale long-term energy storage due to their overall safety, flexible design, high conversion efficiency, and long cycle life. Currently, vanadium redox flow batteries (VRFBs) have achieved commercial application and have good development prospects.

[0003] The separator is a core component in VRFB (Vibration Flow Battery) and must meet the requirements of high proton conductivity, low vanadium permeation, good mechanical properties, and excellent chemical stability. Currently, DuPont's Nafion series membranes are the most widely used in vanadium redox flow batteries, exhibiting good mechanical stability and proton conductivity. However, the high water absorption rate of perfluorosulfonic acid (PFSA) membranes exacerbates vanadium ion permeation, resulting in low ion selectivity; furthermore, the cost of Nafion membranes accounts for more than 40% of the total cost of a 1 kW battery stack, and such high material costs hinder the widespread commercialization of VRFB. Therefore, there is an urgent need to develop new low-cost, high-performance flow battery separators.

[0004] Polybenzimidazole (PBI) membranes, as one of the most promising non-fluorinated ion-conducting membranes, possess excellent vanadium-blocking properties and chemical stability, and have been widely used in VRFB (Vibration-Reducing Fusion Membranes). However, PBI membranes lack ion-exchange groups, resulting in very low conductivity. Researchers have explored the effects of various ion groups on the conductivity of PBI over the past few years. Sulfonic acid groups exhibit a much higher proton dissociation capacity than other proton-conducting groups, making the introduction of sulfonic acid groups an effective way to improve the ionic conductivity of PBI membranes. However, this may potentially reduce the membrane's mechanical strength, chemical stability, and ion selectivity. To address these issues, other modification strategies can be used simultaneously to achieve optimal performance. Covalent cross-linking is a major means of improving the mechanical and chemical stability of membranes, effectively reducing excessive swelling and electrolyte cross-contamination in PBI membranes, thus balancing the mass transfer capacity and stability of sulfonated PBI membranes. Furthermore, using suitable cross-linking agents can form a broad cross-linked network within the membrane, widening ion transport channels and optimizing the pore structure, ensuring that the high ion selectivity and chemical stability of PBI membranes are maintained while improving their ionic conductivity. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing a cross-linked sulfonated polybenzimidazole membrane.

[0006] Another object of the present invention is to provide an application of the cross-linked sulfonated polybenzimidazole membrane prepared by the method in the preparation of flow batteries.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] In a first aspect, the present invention provides a method for preparing a cross-linked sulfonated polybenzimidazole membrane, comprising the following steps:

[0009] The first step involves adding polybenzimidazole to a first solvent under a nitrogen atmosphere and stirring at a temperature of 60–100°C (preferably 80°C) for 1–3 hours (preferably 2 hours). Anhydrous potassium carbonate powder is then added, with a molar ratio of polybenzimidazole to anhydrous potassium carbonate powder of 1:1–2 (preferably 1:1.5). A sulfonating agent is then slowly added, with a molar ratio of polybenzimidazole to sulfonating agent of 8–20:1 (preferably 10:1). The reaction is carried out at a temperature of 30–50°C (preferably 40°C) for 1–48 hours (preferably 24 hours). After post-treatment, sulfonated polybenzimidazole is obtained.

[0010] The sulfonating agent is selected from at least one of 1,3-propanesulfonate lactone, 1,3-propenesulfonate lactone, 1,4-butanesulfonate lactone, vinylsulfonate lactone, benzosulfonate lactone, ethylenesulfonate lactone, and functionalized sulfonate lactone derivatives.

[0011] The second step involves dissolving sulfonated polybenzimidazole in a second solvent to obtain a solution with a mass fraction of 1-10% (preferably 2%), adding a crosslinking agent, wherein the molar ratio of sulfonated polybenzimidazole to crosslinking agent is 1-20:1 (preferably 10:1 or 5:1), heating to 60-100℃ (preferably 80℃) and reacting for 1-48 hours (preferably 24 hours), and then undergoing post-treatment to obtain crosslinked sulfonated polybenzimidazole.

[0012] The crosslinking agent is selected from at least one of glycerol triglycidyl ether (GTE), ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and pentaerythritol diglycidyl ether.

[0013] The third step involves dissolving cross-linked sulfonated polybenzimidazole in a third solvent, drying it to obtain a cross-linked sulfonated polybenzimidazole membrane, activating it, and obtaining an activated cross-linked sulfonated polybenzimidazole membrane.

[0014] The first solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, and methanesulfonic acid.

[0015] The post-processing steps in the first step are as follows: pour the mixture into acetone to precipitate the polymer, wash it several times with water and ethanol until the solution becomes colorless, and then dry it.

[0016] In the first step, drying involves vacuum drying the precipitate at a temperature of 50–70°C (preferably 60°C) for 1–48 hours (preferably 24 hours).

[0017] The preparation method of the polybenzimidazole includes the following steps:

[0018] Under a nitrogen atmosphere, phosphorus pentoxide and methanesulfonic acid are mixed in a mass ratio of 1:1 to 20 (preferably 1:10), and 3,3'-diaminobenzidine (DAB) and 4,4'-dicarboxylic acid diphenyl ether (OBA) are added in a molar ratio of 1:1 to 2 (preferably 1:1). The mass ratio of phosphorus pentoxide to 3,3'-diaminobenzidine is 1 to 5:1 (preferably 3.1:1). Under stirring, the reaction system is heated to 90 to 110°C (preferably 100°C) and stirred for 1 to 3 hours (preferably 2 hours). Then, the temperature is raised to 130 to 150°C (preferably 140°C) and reacted for 1 to 5 hours (preferably 4 hours) to obtain the polybenzimidazole.

[0019] The number-average molecular weight (Mn) of the polybenzimidazole is 34175 g·mol⁻¹. -1 The weight-average molecular weight (Mw) is 57958 g·mol⁻¹. -1 The polydispersity index (PDI) is 1.69.

[0020] The second solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, and methanesulfonic acid.

[0021] The post-processing steps in the second step are as follows: pour the mixture into acetone to precipitate the polymer, and wash it several times with water and ethanol until the solution becomes colorless and then dry it.

[0022] In the second step, drying involves vacuum drying the precipitate at a temperature of 50–70°C (preferably 60°C) for 1–48 hours (preferably 24 hours).

[0023] The cross-linked sulfonated polybenzimidazole is dissolved in a third solvent to obtain a solution with a mass fraction of 1-10% (preferably 2%).

[0024] The drying step in the third step involves drying the above solution at a temperature of 60–100°C (preferably 80°C) for 1–48 hours (preferably 24 hours).

[0025] The third solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, and methanesulfonic acid.

[0026] The thickness of the cross-linked sulfonated polybenzimidazole film is 20-30 μm (preferably 25 μm).

[0027] The activation step in the third step involves placing the prepared membrane in an 85wt% phosphoric acid solution and allowing it to stand for 1–48 hours (preferably 24 hours) for activation pretreatment, followed by washing with deionized water multiple times.

[0028] In a second aspect, the present invention provides a cross-linked sulfonated polybenzimidazole membrane, wherein the cross-linked sulfonated polybenzimidazole membrane is prepared by the preparation method described above.

[0029] A third aspect of the present invention provides the application of the cross-linked sulfonated polybenzimidazole membrane in the preparation of a flow battery.

[0030] The flow battery is selected from at least one of the following: vanadium redox flow battery, lithium-ion flow battery, zinc-bromine flow battery, zinc-cerium flow battery, zinc-nickel flow battery, lead flow battery, iron-chromium flow battery, sodium polysulfide / bromine flow battery, or all-iron flow battery.

[0031] By adopting the above technical solution, the present invention has the following advantages and beneficial effects:

[0032] The cross-linked sulfonated polybenzimidazole membrane provided by this invention modifies the molecular structure of PBI through grafting and cross-linking reactions. The grafted hydrophilic sulfonic acid groups provide more proton transport sites for the membrane, and the cross-linking reaction constructs a dynamic hydrogen bond network that facilitates proton transport, providing excellent ion transport channels and significantly improving the membrane's proton conductivity. Simultaneously, the continuous cross-linked network formed by covalent bonds effectively restricts the diffusion of active materials, maintaining excellent ion selectivity. The cross-linked sulfonated polybenzimidazole membrane provided by this invention exhibits excellent performance in VRFB (Vibration-Reduced Fluid Absorption Fiber).

[0033] The present invention provides a method for preparing a cross-linked sulfonated polybenzimidazole membrane. This method involves grafting highly conductive sulfonic acid groups onto the PBI backbone as ion exchange groups, and using glycerol triglycidyl ether (GTE) as a covalent cross-linking agent. On one hand, the synergistic effect of the sulfonic acid groups and the protonated imidazole groups provides more ion exchange sites for protons. On the other hand, the dynamic hydrogen bond network formed by the ether bonds and hydroxyl groups between chain segments provides excellent ion transport channels for protons, significantly improving the membrane's proton conductivity. Simultaneously, the tight cross-linked network also maintains excellent ion selectivity and chemical stability. Vanadium redox flow batteries assembled with this membrane exhibit excellent electrochemical performance and stability. This invention provides an effective strategy for designing high-performance PBI membranes, thereby enhancing the competitiveness of PBI membranes in the field of vanadium redox flow batteries.

[0034] The cross-linked sulfonated polybenzimidazole membrane provided by this invention has both excellent proton conductivity and ion selectivity, and exhibits excellent coulombic efficiency and voltage efficiency in vanadium redox flow batteries, thus demonstrating optimal battery performance. Attached Figure Description

[0035] Figure 1 is a schematic diagram of a vanadium ion permeation test.

[0036] Figure 2 shows the XRD patterns of the OPBI-SO3H-GTE membrane and the pure OPBI membrane.

[0037] Figure 3 shows the physical image and SEM image of the OPBI-SO3H-GTE membrane.

[0038] Figure 4 is a schematic diagram of the water absorption and swelling rate test results of OPBI membrane, OPBI-SO3H membrane and OPBI-SO3H-GTE membrane.

[0039] Figure 5 shows the IEC schematic diagrams of Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane and OPBI-SO3H-GTE membrane.

[0040] Figure 6 is a schematic diagram of the water contact angles of the OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane.

[0041] Figure 7 shows the proton conductivity and sheet resistance of Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane and OPBI-SO3H-GTE membrane.

[0042] Figure 8 is a schematic diagram of the vanadium ion permeation of Nafion212 membrane, OPBI membrane, OPBI-SO3H membrane and OPBI-SO3H-GTE membrane.

[0043] Figure 9 shows the current-changing performance of Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane and OPBI-SO3H-GTE membrane.

[0044] Figure 10 shows the OPBI-SO3H-GTE membrane at 200 mA·cm⁻¹. -2 The following is a graph showing the long-term cycling performance.

[0045] Figure 11 is a schematic diagram of the self-discharge curves of Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane and OPBI-SO3H-GTE membrane. Detailed Implementation

[0046] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments, further clarifies the invention. Those skilled in the art should understand that the specific descriptions below are illustrative rather than restrictive, and should not be construed as limiting the scope of protection of the present invention.

[0047] This invention, through the rational selection of modification strategies and careful control of the structure and properties of polymer side chains, enables PBI membranes to maintain high chemical stability while improving proton conductivity. This invention uses inexpensive and highly reactive 1,3-propanesulfonic acid lactone as the sulfonating agent for PBI, and performs epoxy ring-opening at 40°C to attach sulfonic acid groups to the PBI side chains; the process is simple and stable. Furthermore, glycerol triglycidyl ether (GTE) is used as a covalent crosslinking agent, possessing abundant epoxy active sites to ensure effective crosslinking. The numerous ether bonds and hydroxyl groups between crosslinked segments not only broaden the membrane's free volume but also form a dynamic hydrogen bond network, providing more ion transport channels for protons and further enhancing the membrane's mass transfer capacity.

[0048] Example 1

[0049] Preparation of aryl ether-type polybenzimidazole (OPBI)

[0050] 10 g of phosphorus pentoxide and 100 g of methanesulfonic acid were added to a three-necked flask, with a mass ratio of phosphorus pentoxide to methanesulfonic acid of 1:10. Under a nitrogen atmosphere, 15 mmol (3.21 g) of 3,3'-diaminobenzidine (DAB) and 15 mmol (3.87 g) of 4,4'-dicarboxylic acid diphenyl ether (OBA) were added, with a molar ratio of 1:1 between 3,3'-diaminobenzidine (DAB) and 3,4'-dicarboxylic acid diphenyl ether (OBA). The mass ratio of phosphorus pentoxide to 3,3'-diaminobenzidine (OBA) was 3.1:1. Under stirring, the reaction system was heated to 100 °C and stirred for 2 h, and then the temperature was increased to 140 °C and reacted for 4 h. After the reaction was complete, the solution was slowly poured into saturated NaHCO3 under stirring to precipitate and neutralize the residual methanesulfonic acid in the product. The precipitated product was cut into small pieces and washed repeatedly with water and ethanol until the solution was neutral. Finally, the OPBI polymer was vacuum dried at 120°C for 24 hours to obtain 4.97 g of OPBI. The number average molecular weight (Mn) was 34175 g·mol⁻¹. -1 The weight-average molecular weight (Mw) is 57958 g·mol⁻¹. -1 The calculated polydispersity index (PDI) is 1.69.

[0051]

[0052] Preparation of sulfonated polybenzimidazole (OPBI-SO3H) membrane

[0053] Under a nitrogen atmosphere, OPBI (2.5 mmol, 1 g) was added to 50 g of dimethyl sulfoxide and stirred at 80 °C for 2 h. After complete dissolution, anhydrous K₂CO₃ powder (3.75 mmol, 0.52 g) was added as a catalyst, with a molar ratio of OPBI to anhydrous K₂CO₃ powder of 1:1.5. Then, 1,3-propanesulfonic acid lactone (0.25 mmol, 0.03 g) was slowly added, with a molar ratio of OPBI to 1,3-propanesulfonic acid lactone of 10:1. The reaction was carried out at 40 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.84 g of OPBI-SO₃H.

[0054] 0.5 g of OPBI-SO3H solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish (Flat-glass culture dish, FS-30, 32 mm in diameter, 15 mm in height, Japan) and dried in an oven at 80 °C for 24 h to obtain a 25 μm thick, uniformly surfaced OPBI-SO3H membrane. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI-SO3H membrane.

[0055] Preparation of cross-linked sulfonated polybenzimidazole (OPBI-SO3H-GTE) membrane

[0056] OPBI-SO3H (0.95 mmol, 0.5 g) solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. Glycerol triglycidyl ether (GTE) (0.095 mmol, 0.025 g) was added, with a molar ratio of OPBI-SO3H to GTE of 10:1. The reaction was carried out at 80 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and the precipitate was washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.42 g of OPBI-SO3H-GTE product.

[0057] 0.5 g of OPBI-SO3H-GTE solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish and dried in an oven at 80 °C for 24 h to obtain an OPBI-SO3H-GTE membrane with a thickness of 25 μm and a uniform surface. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI-SO3H-GTE membrane.

[0058]

[0059] Comparative Example 1

[0060] Preparation of OPBI pure membrane

[0061] 0.5 g of OPBI solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish and dried in an oven at 80 °C for 24 h to obtain a PBI membrane with a thickness of 25 μm and a uniform surface. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI membrane.

[0062] Comparative Example 2

[0063] Purchased Nafion 212 film.

[0064] Test methods for samples prepared in Example 1 and Comparative Examples 1-2

[0065] Swelling rate and water absorption rate

[0066] The membranes used in the preparation of the membrane samples below are all activated membranes.

[0067] The cut film sample was placed in a vacuum drying oven at 60℃ and dried for 24 hours. After removing the sample from the oven, the mass of the dried film was quickly weighed and recorded as M. dry And measure its diameter, denoted as D. dry Immerse the membrane in deionized water for 24 hours. After immersion, remove the water from the membrane surface with filter paper, and then immediately weigh the wet membrane (M). wet and diameter D wet To ensure data accuracy and minimize errors, each membrane sample was measured three times, and the average value was taken. The membrane's SR (swelling rate) and WU (water absorption rate) were obtained from the following two equations:

[0068]

[0069] Among them, M dry M is the dry weight of the membrane. wet D is the wet weight of the membrane after it absorbs water. dry D is the diameter of the membrane in its dry state. wet The diameter is the membrane in the wetted state.

[0070] Ion exchange capacity

[0071] The prepared membrane sample was dried in a vacuum drying oven at 60℃ for 24 hours. After removing the sample from the oven, the mass m of the dried membrane was accurately weighed. The membrane was then immersed in 10 mL of 1 mol / L sulfuric acid for 24 hours. After immersion, the membrane surface was rinsed with deionized water to remove free acid, and the surface was dried with filter paper. Using phenolphthalein as an indicator, the membrane was titrated with 0.01 mol / L NaOH standard solution. The volume of standard solution consumed was recorded. The formula for calculating the ion exchange capacity (IEC) is as follows:

[0072] Where m is the dry weight of the membrane, C NaOH V' represents the molar concentration of NaOH, and V' and V' represent the volume readings before and after titration, respectively.

[0073] proton conductivity

[0074] The proton conductivity (σ) and sheet resistivity (AR) of various membranes were measured using an electrochemical workstation via AC impedance spectroscopy. The frequency range was 10 Hz. -2 -10 6 Between Hz, the AC amplitude is 5mV. The formulas for calculating proton conductivity and surface resistivity are as follows:

[0075] AR = A × R

[0076] Where σ is the proton conductivity of the membrane (mS·cm) -1 L is the thickness of the membrane between the positive and negative electrode plates (cm), and A is the cross-sectional area of ​​the membrane sample (cm²). 2 R is the actual measured value of the membrane impedance (Ω), and AR is the sheet resistance of the membrane (Ω·cm). 2 ).

[0077] Vanadium ion penetration test

[0078] Vanadium ion permeation was tested by diffusion. First, a standard vanadium oxysulfate solution (VOSO4) was prepared by dissolving VOSO4 in 3.0 M H2SO4, with a concentration of 0.1 mol·L⁻¹. -1 0.075 mol·L -1 0.03 mol·L -1 0.015 mol·L -1 0.005 mol·L -1 and 0.0025 mol·L -1 Used to calibrate V in VOSO4 4+ The concentration-absorbance standard curve was obtained. Figure 1 shows a schematic diagram of the vanadium ion permeation test. The prepared membrane was sandwiched in a diffusion cell, with 50 mL of [1.5 M VOSO4 + 3.0 M H2SO4 solution] on the left and 50 mL of [1.5 M MgSO4 + 3.0 M H2SO4] on the right and left sides respectively. To avoid concentration polarization, both sides were magnetically stirred at the same rotation speed. Every 24 hours, 4 mL of sample was taken from the side containing MgSO4 solution, and 4 mL of [1.5 M MgSO4 + 3.0 M H2SO4] solution was added again to maintain ion balance. The absorbance of the solution was measured using a UV-Vis spectrophotometer, and the corresponding Vb was obtained according to the calibrated standard curve. 4+ Concentration. Finally, the permeability of vanadium ions was calculated using the following formula.

[0079]

[0080] Among them, V B Let t be the volume of the solution (mL), t be the time (min), and A be the membrane area being tested (cm²). 2L is the membrane thickness (cm), and P is the vanadium ion permeability of the membrane (cm). 2 ·min -1 ), C A V in VOSO4 solution 4+ Concentration (mol·L) -1 ), C B (t) represents the V in the MgSO4 solution. 4+ Concentration (mol·L) -1 ).

[0081] Basic characterization of membranes

[0082] Figure 2 shows the XRD patterns of the OPBI-SO3H-GTE film and the pure OPBI film. As can be seen from the figure, the pure OPBI film with its dense structure exhibits a single strong diffraction peak only at 2θ = 23.6° due to π-π stacking, and its intersegment spacing corresponds to... Compared to the OPBI film, the OPBI-SO3H-GTE film exhibits a new diffraction peak at 2θ = 16.9°, in addition to the diffraction peak at 2θ = 22.8°. This indicates that within the local space where grafting and cross-linking reactions occur, the distance between molecules is increased due to the presence of long side chains, leading to an increase in the free volume of the polymer chain.

[0083] Figure 3 shows the physical image and SEM image of the OPBI-SO3H-GTE membrane, where (a) is the SEM surface image; (b) is the SEM cross-sectional image; and (c) is the schematic diagram of the EDS elemental spectrum. As can be seen from the figure, the membrane is smooth, transparent and dense, with a thickness of approximately 25 μm, and the sulfur element is uniformly distributed in the membrane.

[0084] Figure 4 shows the test results of water absorption and swelling rate of OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. As can be seen from the figure, the water absorption rate of OPBI-SO3H-GTE membrane is 25.35%, which is 2.4 times that of pure OPBI membrane (10.52%), and its anti-swelling performance is enhanced compared to OPBI-SO3H membrane. This is because the grafted sulfonic acid groups have good hydrophilicity, and the grafting and cross-linking of long side chains expands the free volume of the chains, allowing more water molecules to be accommodated inside the membrane. This significantly enhances the proton transport process using water as a carrier. After the cross-linking reaction, a continuous cross-linked network is formed inside the membrane, thus enhancing the membrane's anti-swelling performance.

[0085] Figure 5 shows the IEC (Integrity, Electron, and Thermochemical) values ​​of the Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. As can be seen from the figure, the OPBI-SO3H-GTE membrane has the highest IEC value (1.57 mmol / g), significantly higher than the Nafion 212 membrane (0.84 mmol / g) and the OPBI membrane (0.45 mmol / g). The sulfonic acid groups in SO32-containing sulfonic acid molecules carry a negative charge. - The anion is H + The abundant ion exchange sites result in a high ion exchange capacity for the membrane. After crosslinking, the long side chains expand the ion conduction channels of the membrane, allowing it to absorb more water molecules and promoting ion transport.

[0086] Figure 6 shows the water contact angles of the OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. After grafting and crosslinking, the water contact angle of the membrane decreased from 80.69° to 28.6°, which further illustrates that the hydrophilic sulfonic acid groups, ether bonds, and hydroxyl groups in the membrane can adsorb more water molecules and significantly improve its ion transport capacity.

[0087] Figure 7 shows the proton conductivity and sheet resistance of Nafion 212 film, OPBI film, OPBI-SO3H film, and OPBI-SO3H-GTE film. As can be seen from the figure, the proton conductivity of the pure OPBI film is only 30.27 mS·cm. -1 This is lower than that of the Nafion 212 membrane (47.3 mS·cm). -1 After grafting and crosslinking reactions, the conductivity of the OPBI-SO3H-GTE membrane reached 74.86 mS·cm. -1 Furthermore, its surface resistivity is as low as 13.40 Ω·cm. 2 This is far lower than the sheet resistivity of the Nafion 212 film (21.18 Ω·cm). 2 This is because the introduction of sulfonic acid groups increases the hydrophilicity of the membrane and provides more proton transport sites, thereby promoting proton transport; after crosslinking, the content of hydroxyl and ether bonds in the membrane is increased, and these hydroxyl and ether bonds form a dynamic hydrogen bond network that is conducive to proton transport, providing a good ion transport channel for protons and greatly reducing the sheet resistance of the membrane.

[0088] Figure 8 shows the vanadium ion permeability of Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. As can be seen from the figure, the vanadium ion permeability of the OPBI, OPBI-SO3H, and OPBI-SO3H-GTE membranes is significantly lower than that of the Nafion 212 membrane. The crosslinked OPBI-SO3H-GTE membrane exhibits a particularly low vanadium ion permeability (12.63 × 10⁻⁶).-8 cm 2 ·min -1 This indicates that the cross-linked network formed by covalent bonds can effectively limit membrane swelling, reduce intermolecular gaps, and thus hinder the transmembrane transfer of vanadium ions.

[0089] Flow battery performance

[0090] The membrane performance was tested at room temperature using a flow battery device. The flow battery device mainly consists of the following components: an effective area of ​​4 cm². 2 The vanadium battery consists of a membrane, two activated carbon felt electrodes, two graphite conductive plates, several gaskets, several bolts and nuts, and two PTFE shells. From left to right, the structure of the vanadium battery is as follows: PTFE shell, gaskets, graphite conductive plates, gaskets, electrode frame, carbon felt electrodes, and membrane. The structure on the right side is identical to that on the left, symmetrically distributed. All components are secured by bolts and nuts running through both ends. The membrane sample is firmly clamped between the two electrodes inside the battery to isolate the positive and negative electrolytes. Both the positive and negative electrolytes are vanadium ion solutions dissolved in sulfuric acid.

[0091] After assembling the flow battery, variable current charge-discharge performance tests were conducted, with the variable current density ranging from 80 to 220 mA·cm⁻¹. -2 The interval is 20 mA·cm -2 The cutoff voltage is 0.8-1.7V. At 200mA·cm -2 Long-term cycling tests were conducted, with the cutoff voltage the same as in the variable current test. Self-discharge tests were performed at 50% state of charge (SOC), and the voltage variation with rest time during the test was recorded. The coulombic efficiency (CE), energy efficiency (EE), and voltage efficiency (VE) of the flow battery were calculated using the following formulas.

[0092]

[0093]

[0094]

[0095] Among them, I c Battery charging current (mA), I d V is the battery discharge current (mA). c Battery charging voltage (V), V d Let t be the battery discharge voltage (V) and t be the time (s).

[0096] Figure 9 shows the current-varying performance of the Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. In this figure, (a) is a schematic diagram of the coulombic efficiency (CE) of the Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane; (b) is a schematic diagram of the voltage efficiency (VE) of the Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane; and (c) is a schematic diagram of the energy efficiency (EE) of the Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. As shown in the figure, the OPBI-SO3H-GTE membrane exhibits the highest coulombic efficiency (98.49%-99.68%), indicating that the tightly cross-linked network formed within the membrane effectively enhances its ion selectivity. The voltage efficiency test results are consistent with the sheet resistivity results of various membranes. The voltage efficiency of the OPBI-SO3H-GTE membrane (91.98%-78-95%) is significantly better than other membranes. This is due to its highly efficient proton transport channels. On the one hand, the presence of sulfonic acid groups and protonated imidazole provides more transport sites for protons. On the other hand, the presence of flexible side chains not only expands the free volume of the membrane, but also the dynamic hydrogen bond network formed by the ether bonds and hydroxyl groups between the chain segments provides more ion transport channels for protons, thereby improving its voltage efficiency. Based on its excellent coulombic and voltage efficiencies, the OPBI-SO3H-GTE membrane exhibits the best overall performance, with an energy efficiency of 90.60%-78.34%. In contrast, the overall performance of the OPBI-SO3H membrane grafted with only sulfonic acid groups (87.48%-74.74%) is somewhat inferior to that of the OPBI-SO3H-GTE membrane, but it is still higher than that of the pure OPBI membrane (86.36%-72.45%) and the commercial Nafion 212 membrane (90.60%-78.34%). This also indicates that the cross-linked sulfonated polybenzimidazole membrane has a good application scenario in VRFB.

[0097] Figure 10 shows the OPBI-SO3H-GTE membrane at 200 mA·cm⁻¹. -2 The following is a graph showing the long-term cycling performance. The all-vanadium redox flow battery assembled using the OPBI-SO3H-GTE membrane completed approximately 1200 cycles with a cycle time of 720 hours. Its excellent ion selectivity resulted in a superior coulombic efficiency (>99%), and its energy efficiency remained almost constant at around 80% throughout the test. This indicates that the cross-linked sulfonated polybenzimidazole membrane with grafted and cross-linked structures not only efficiently conducts protons during the dynamic charge-discharge process of VRFB, but also exhibits excellent long-term chemical stability under the strongly acidic and oxidizing conditions of the electrolyte.

[0098] Figure 11 shows the self-discharge curves of the Nafion 212 membrane, OPBI membrane, OPBI-SO3H membrane, and OPBI-SO3H-GTE membrane. The self-discharge time of the OPBI-SO3H-GTE membrane can reach 54 hours, which is much longer than that of the OPBI membrane (34 hours) and the Nafion 212 membrane (24 hours). This is consistent with the self-discharge time of the VO2+ membrane. 2+ The ion permeation results are consistent with the coulombic efficiency of the battery, proving that the cross-linked sulfonated polybenzimidazole membrane prepared in this invention has excellent ion selectivity.

[0099] Example 2

[0100] Preparation of sulfonated polybenzimidazole (OPBI-SO3H) membrane

[0101] Under a nitrogen atmosphere, OPBI (2.5 mmol, 1 g) was added to 50 g of dimethyl sulfoxide and stirred at 80 °C for 2 h. After complete dissolution, anhydrous K₂CO₃ powder (3.75 mmol, 0.52 g) was added as a catalyst, with a molar ratio of OPBI to anhydrous K₂CO₃ powder of 1:1.5. Then, 1,4-butyryl lactone (0.25 mmol, 0.034 g) was slowly added, with a molar ratio of OPBI to 1,4-butyryl lactone of 10:1. The reaction was carried out at 40 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.86 g of OPBI-SO₃H.

[0102] Preparation of cross-linked sulfonated polybenzimidazole (OPBI-SO3H-GTE) membrane

[0103] OPBI-SO3H (0.93 mmol, 0.5 g) solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. Glycerol triglycidyl ether (GTE) (0.093 mmol, 0.024 g) was added, with a molar ratio of OPBI-SO3H to GTE of 10:1. The reaction was carried out at 80 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and the precipitate was washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was dried under vacuum at 60 °C for 24 h to obtain 0.43 g of OPBI-SO3H-GTE product.

[0104] 0.5 g of OPBI-SO3H-GTE solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish and dried in an oven at 80 °C for 24 h to obtain an OPBI-SO3H-GTE membrane with a thickness of 25 μm and a uniform surface. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI-SO3H-GTE membrane.

[0105] Example 3

[0106] Preparation of sulfonated polybenzimidazole (OPBI-SO3H) membrane

[0107] Under a nitrogen atmosphere, OPBI (2.5 mmol, 1 g) was added to 50 g of dimethyl sulfoxide and stirred at 80 °C for 2 h. After complete dissolution, anhydrous K₂CO₃ powder (3.75 mmol, 0.52 g) was added as a catalyst, with a molar ratio of OPBI to anhydrous K₂CO₃ powder of 1:1.5. Then, 1,3-propanesulfonic acid lactone (0.25 mmol, 0.03 g) was slowly added, with a molar ratio of OPBI to 1,3-propanesulfonic acid lactone of 10:1. The reaction was carried out at 40 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.84 g of OPBI-SO₃H.

[0108] Preparation of cross-linked sulfonated polybenzimidazole (OPBI-SO3H-GDE) membrane

[0109] OPBI-SO3H (0.95 mmol, 0.5 g) solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. Ethylene glycol diglycidyl ether (GDE) (0.095 mmol, 0.016 g) was added, with a molar ratio of OPBI-SO3H to GDE of 10:1. The reaction was carried out at 80 °C for 24 h. After the reaction was complete, the mixture was poured into acetone to precipitate the polymer, and the precipitate was washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.41 g of OPBI-SO3H-GDE product.

[0110] 0.5 g of OPBI-SO3H-GDE solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish and dried in an oven at 80 °C for 24 h to obtain an OPBI-SO3H-GDE membrane with a thickness of 25 μm and a uniform surface. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI-SO3H-GDE membrane.

[0111] Example 4

[0112] Preparation of sulfonated polybenzimidazole (OPBI-SO3H) membrane

[0113] Under a nitrogen atmosphere, OPBI (2.5 mmol, 1 g) was added to 50 g of dimethyl sulfoxide and stirred at 80 °C for 2 h. After complete dissolution, anhydrous K₂CO₃ powder (3.75 mmol, 0.52 g) was added as a catalyst, with a molar ratio of OPBI to anhydrous K₂CO₃ powder of 1:1.5. Then, 1,3-propanesulfonic acid lactone (0.5 mmol, 0.061 g) was slowly added, with a molar ratio of OPBI to 1,3-propanesulfonic acid lactone of 5:1. The reaction was carried out at 40 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.92 g of OPBI-SO₃H.

[0114] Preparation of cross-linked sulfonated polybenzimidazole (OPBI-SO3H-GTE) membrane

[0115] OPBI-SO3H (0.95 mmol, 0.5 g) solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. Glycerol triglycidyl ether (GTE) (0.095 mmol, 0.025 g) was added, with a molar ratio of OPBI-SO3H to GTE of 10:1. The reaction was carried out at 80 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and the precipitate was washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was dried under vacuum at 60 °C for 24 h to obtain 0.44 g of OPBI-SO3H-GTE product.

[0116] 0.5 g of OPBI-SO3H-GTE solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish and dried in an oven at 80 °C for 24 h to obtain an OPBI-SO3H-GTE membrane with a thickness of 25 μm and a uniform surface. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI-SO3H-GTE membrane.

[0117] Example 5

[0118] Preparation of sulfonated polybenzimidazole (OPBI-SO3H) membrane

[0119] Under a nitrogen atmosphere, OPBI (2.5 mmol, 1 g) was added to 50 g of dimethyl sulfoxide and stirred at 80 °C for 2 h. After complete dissolution, anhydrous K₂CO₃ powder (3.75 mmol, 0.52 g) was added as a catalyst, with a molar ratio of OPBI to anhydrous K₂CO₃ powder of 1:1.5. Then, 1,3-propanesulfonic acid lactone (0.25 mmol, 0.03 g) was slowly added, with a molar ratio of OPBI to 1,3-propanesulfonic acid lactone of 10:1. The reaction was carried out at 40 °C for 24 h. After the reaction was completed, the mixture was poured into acetone to precipitate the polymer, and washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.84 g of OPBI-SO₃H.

[0120] Preparation of cross-linked sulfonated polybenzimidazole (OPBI-SO3H-GTE) membrane

[0121] OPBI-SO3H (0.95 mmol, 0.5 g) solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. Glycerol triglycidyl ether (GTE) (0.19 mmol, 0.049 g) was added, with a molar ratio of OPBI-SO3H to GTE of 5:1. The mixture was heated to 80 °C and reacted for 24 h. After the reaction was complete, the mixture was poured into acetone to precipitate the polymer, and washed several times with water and ethanol until the solution became colorless. Finally, the precipitate was vacuum dried at 60 °C for 24 h to obtain 0.44 g of OPBI-SO3H-GTE product.

[0122] 0.5 g of OPBI-SO3H-GTE solid was dissolved in 25 g of dimethyl sulfoxide to obtain a 2% (w / w) solution. 2.0 mL of this solution was added to a petri dish and dried in an oven at 80 °C for 24 h to obtain an OPBI-SO3H-GTE membrane with a thickness of 25 μm and a uniform surface. The prepared membrane was then placed in 10 mL of 85 wt% phosphoric acid solution and allowed to stand for 24 h for activation pretreatment. After removal, the membrane was washed several times with deionized water to obtain the activated OPBI-SO3H-GTE membrane.

[0123] Table 1 shows the performance results of the membranes prepared in the embodiments and comparative examples of the present invention.

[0124] Table 1

[0125] As can be seen from the data in Table 1, Example 1 exhibits the best overall performance, thanks to the highly efficient proton transport channels and cross-linking network within the OPBI-SO3H-GTE membrane, with coulombic efficiency and voltage efficiency exceeding 200 mA·cm⁻¹. -2 The efficiency ratios were 99.40% and 80.73%, respectively, which are superior to the pure OPBI film (98.73%, 75.36%) in Comparative Example 1 and the Nafion 212 film (97.54%, 75.60%) in Comparative Example 2. Based on its excellent coulombic efficiency and voltage efficiency, its energy efficiency is above 80 mA·cm⁻¹. -2 and 200mA·cm -2 The membranes achieved 90% and 80% or higher respectively, exhibiting the highest performance across all embodiments. In contrast, the OPBI pure membrane of Comparative Example 1 and the Nafion 212 membrane of Comparative Example 2 showed performance at 200 mA·cm⁻¹. -2 The energy efficiency at high current densities is only 74.41% and 73.74%. This indicates that the cross-linked sulfonated polybenzimidazole membrane prepared in this invention maintains its excellent selectivity and stability while achieving higher ionic conductivity, demonstrating great application potential.

[0126] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for preparing a cross-linked sulfonated polybenzimidazole membrane, characterized in that, Includes the following steps: The first step involves adding polybenzimidazole to a first solvent under a nitrogen atmosphere and stirring at 60–100°C for 1–3 hours. Anhydrous potassium carbonate powder is then added, with a molar ratio of polybenzimidazole to anhydrous potassium carbonate powder of 1:1–2. A sulfonating agent is then slowly added, with a molar ratio of polybenzimidazole to sulfonating agent of 8–20:

1. The reaction is carried out at 30–50°C for 1–48 hours. After post-treatment, sulfonated polybenzimidazole is obtained. The polybenzimidazole is an aromatic ether type polybenzimidazole OPBI; The sulfonating agent is selected from at least one of 1,3-propanesulfonate lactone and 1,4-butanesulfonate lactone; The second step involves dissolving sulfonated polybenzimidazole in a second solvent to obtain a solution with a mass fraction of 1-10%, adding a crosslinking agent with a molar ratio of sulfonated polybenzimidazole to crosslinking agent of 1-20:1, heating to 60-100℃ and reacting for 1-48 hours, and then undergoing post-treatment to obtain crosslinked sulfonated polybenzimidazole. The crosslinking agent is selected from glycerol triglycidyl ether; The third step involves dissolving cross-linked sulfonated polybenzimidazole in a third solvent, drying it to obtain a cross-linked sulfonated polybenzimidazole membrane, activating it, and obtaining an activated cross-linked sulfonated polybenzimidazole membrane. The activation step in the third step involves placing the prepared membrane in an 85wt% phosphoric acid solution and allowing it to stand for 1–48 hours for activation pretreatment, followed by washing with deionized water multiple times.

2. The method for preparing the cross-linked sulfonated polybenzimidazole membrane according to claim 1, characterized in that, The first solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, and methanesulfonic acid; The post-processing steps in the first step are as follows: pour the mixture into acetone to precipitate the polymer, wash it several times with water and ethanol until the solution becomes colorless, and then dry it.

3. The method for preparing the cross-linked sulfonated polybenzimidazole membrane according to claim 1, characterized in that, The preparation method of the polybenzimidazole includes the following steps: Under a nitrogen atmosphere, phosphorus pentoxide and methanesulfonic acid were mixed in a mass ratio of 1:1 to 20, and 3,3'-diaminobenzidine and 4,4'-dicarboxylic acid diphenyl ether were added in a molar ratio of 1:1 to 2. The mass ratio of phosphorus pentoxide to 3,3'-diaminobenzidine was 1 to 5:

1. Under stirring, the reaction system was heated to 90 to 110°C and stirred for 1 to 3 hours. Then, the temperature was raised to 130 to 150°C and reacted for 1 to 5 hours to obtain the polybenzimidazole.

4. The method for preparing the cross-linked sulfonated polybenzimidazole membrane according to claim 1, characterized in that, The second solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, and methanesulfonic acid; The post-processing steps in the second step are as follows: pour the mixture into acetone to precipitate the polymer, and wash it several times with water and ethanol until the solution becomes colorless and then dry it.

5. The method for preparing the cross-linked sulfonated polybenzimidazole membrane according to claim 1, characterized in that, Cross-linked sulfonated polybenzimidazole is dissolved in a third solvent to obtain a solution with a mass fraction of 1-10%.

6. The method for preparing the cross-linked sulfonated polybenzimidazole membrane according to claim 1, characterized in that, The third solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, and methanesulfonic acid.

7. The method for preparing the cross-linked sulfonated polybenzimidazole membrane according to claim 1, characterized in that, The thickness of the cross-linked sulfonated polybenzimidazole membrane is 20–30 μm.

8. A cross-linked sulfonated polybenzimidazole membrane, characterized in that, The cross-linked sulfonated polybenzimidazole membrane is prepared by the preparation method according to any one of claims 1 to 7.

9. The application of the cross-linked sulfonated polybenzimidazole membrane according to claim 8 in the preparation of a flow battery.

10. The application according to claim 9, characterized in that, The flow battery is selected from at least one of the following: vanadium redox flow battery, lithium-ion flow battery, zinc-bromine flow battery, zinc-cerium flow battery, zinc-nickel flow battery, lead flow battery, iron-chromium flow battery, sodium polysulfide / bromine flow battery, or all-iron flow battery.