Oxygen candle ignition composition, and preparation method therefor

By employing a combined dry-mixing and pressing technique involving oxidizer powder, fuel powder, and inert inorganic filler, the problems of unstable low-temperature ignition, high sensitivity, significant safety risks, and poor formability of oxygen candle igniters have been solved, enabling the efficient and safe preparation of oxygen candle igniters.

WO2026232737A1PCT designated stage Publication Date: 2026-11-12HUBEI INST OF AEROSPACE CHEMOTECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/122660
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2025-09-19
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing oxygen candle igniters suffer from problems such as unstable low-temperature ignition performance, high sensitivity, significant safety risks, poor formability, and low production efficiency.

Method used

An oxygen candle igniter with low mechanical sensitivity, high safety, and good formability is prepared by using a combination of oxidant powder, fuel powder, and inert inorganic filler, which are dry-mixed and then pressed into shape.

Benefits of technology

Stable ignition performance was achieved in environments ranging from -40℃ to 70℃, improving safety and production efficiency, reducing mechanical sensitivity, and ensuring the impact and vibration resistance of the propellant charge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025122660-FTAPPB-I100001
    Figure PCTCN2025122660-FTAPPB-I100001
  • Figure PCTCN2025122660-FTAPPB-I100002
    Figure PCTCN2025122660-FTAPPB-I100002
  • Figure PCTCN2025122660-FTAPPB-I100003
    Figure PCTCN2025122660-FTAPPB-I100003
Patent Text Reader

Abstract

An oxygen candle ignition composition, consisting of the following components in percentages by mass: 20-46% of an oxidant powder, 15-32% of a fuel powder, and 28-56% of an inert inorganic filler, wherein the fuel powder consists of a primary fuel powder and an auxiliary fuel powder in a weight ratio of (1-8):1. A preparation method therefor comprises: dry-mixing the above raw materials until uniform, and loading same into a mold press for compression molding. The present disclosure is suitable for rapidly igniting an oxygen-generating prill column to generate oxygen upon percussion ignition in a solid chemical oxygen generator. The present oxygen candle ignition composition has low mechanical sensitivity, high safety in terms of use, and good moldability, and the prill column has strong impact and vibration resistance effects; and the composition has good ignition performance, and thus can achieve ignition and flame propagation in an environment of -40°C to 70°C. The preparation method is simple and has a high modular production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

An oxygen candle igniter and its preparation method

[0001] Cross-references to related applications

[0002] This disclosure claims priority to Chinese Patent Application No. 2025105842112, filed on May 7, 2025, entitled "An Oxygen Candle Ignition Agent and a Method for Preparing the Same", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure pertains to the field of manufacturing compositions of explosives or thermal agents, and specifically relates to an oxygen candle igniter. Background Technology

[0004] An oxygen candle (solid chemical oxygen generator) is an oxygen supply device that generates oxygen through a chemical reaction. It is widely used in confined spaces such as aerospace, aviation, maritime, and mining, and is an important piece of equipment for oxygen deficiency protection and emergency escape. An oxygen candle mainly consists of an ignition system, an oxygen production system, a heat insulation system, and a filtration system. The ignition system includes an igniter and a igniter. The igniter is located at the head of the oxygen-producing propellant column and is ignited by the energy released from an electric igniter or an impact primer. It utilizes the large amount of high-temperature gas or incandescent solid particles generated during combustion to provide sufficient energy and temperature to ignite the oxygen-producing propellant column, thus providing follow-up ignition. The igniter plays a crucial role in the working performance of the oxygen candle, affecting its reliability and mission safety under various environmental conditions.

[0005] At present, the igniters for oxygen candles have been studied in considerable depth, and they can basically achieve the goal of ignition. However, most oxygen candle igniters in China currently suffer from problems such as unstable low-temperature ignition performance, high sensitivity, high safety risks, poor formability, and low production efficiency due to immature technology.

[0006] For example, the igniters disclosed in Chinese patents CN1817824A and CN103204755A all use a method of coating or pressing a layer of titanium powder onto the surface of the igniter. This indicates that the igniters in these patents have poor ignition capabilities and suffer from drawbacks such as easy detachment of the titanium powder and poor process consistency. Furthermore, the igniters in these patents require molding within the grooves of the oxygen-generating propellant column, indicating poor formability and the inability to be molded independently.

[0007] Chinese patents CN108083235A, CN114890853A, and CN114804987A use barium chromate as an oxidant and magnesium powder, zirconium powder, etc. as fuels. These patents have drawbacks such as high formulation sensitivity, poor safety, insufficient calorific value, and poor low-temperature ignition performance. In addition, the chemical precipitation method and acid-base intervention processes are complex and have low production efficiency.

[0008] Chinese patent CN107619021A describes a method of wet-mixing the igniter and oxygen-generating propellant of an oxygen candle with water, then placing the igniter on top of the oxygen-generating propellant and pressing them together. This wet-pressing process requires uniform wet mixing before pressing and high-temperature drying after pressing. These steps increase process costs and extend the product production cycle. Pressing the igniter and oxygen-generating propellant together before demolding can easily cause deflagration or explosion, resulting in poor safety. Furthermore, a large amount of igniter is required to ensure a single, integrated molding process.

[0009] Public content

[0010] The purpose of this disclosure is to overcome the above-mentioned shortcomings of the prior art and provide an oxygen candle igniter that has low mechanical sensitivity, high safety in use, good formability, strong resistance to impact and vibration of the propellant, and good low-temperature ignition performance.

[0011] The technical solution provided in this disclosure is: an oxygen candle igniter, suitable for rapidly igniting an oxygen-producing column to generate oxygen when a solid chemical oxygen generator is ignited, which is composed of the following components by mass percentage: 20%-46% oxidant powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler.

[0012] The fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):1.

[0013] Optionally, the oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

[0014] Optionally, the main fuel powder is selected from one or more of Mg, Al, and Ti powders.

[0015] Optionally, the auxiliary fuel powder is selected from one or more of Si, Fe, Sn, and Mn powders.

[0016] Optionally, the inert inorganic filler is selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride.

[0017] Optionally, the inert inorganic filler is selected from one or more of zinc oxide, nickel oxide, titanium oxide, chromium oxide, aluminum oxide, silicon dioxide, magnesium sulfate, calcium sulfate, calcium silicate, and boron nitride.

[0018] Optionally, the particle size of the oxidant powder is 60-200 mesh.

[0019] Optionally, the fuel powder particle size is 100-400 mesh.

[0020] Optionally, the particle size of the inert inorganic filler is not less than 800 mesh.

[0021] In another aspect, this disclosure provides an oxygen candle ignition block, which is composed of 20%-46% oxidant powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler by mass percentage, which are dry-mixed evenly and then pressed into shape.

[0022] The fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):1.

[0023] Optionally, the oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

[0024] Optionally, the particle size of the oxidant powder is 60-200 mesh.

[0025] Optionally, the main fuel powder is selected from one or more of Mg, Al, and Ti powders.

[0026] Optionally, the particle size of the main fuel powder is 100-400 mesh.

[0027] Optionally, the auxiliary fuel powder is selected from one or more of Si, Fe, Sn, and Mn powders.

[0028] Optionally, the particle size of the auxiliary fuel powder is 100-400 mesh.

[0029] Optionally, the inert inorganic filler is selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride.

[0030] Optionally, the particle size of the inert inorganic filler is not less than 800 mesh.

[0031] This disclosure also provides a method for preparing an oxygen candle igniter, comprising the following steps:

[0032] S1. Weigh out 20%-46% oxidant powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler by mass percentage, mix and sieve to break up the powder; the fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):1.

[0033] S2. Pour the sieved mixture into the mixer, mix until homogeneous, then pour out to complete the dry mixing of the ignition charge;

[0034] S3. Load the dry-mixed ignition charge into the mold and press it into shape.

[0035] Optionally, in step S1, the oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

[0036] Optionally, the particle size of the oxidant powder is 60-200 mesh.

[0037] Optionally, the main fuel powder is selected from one or more of Mg, Al, and Ti powders.

[0038] Optionally, the particle size of the main fuel powder is 100-400 mesh.

[0039] Optionally, the auxiliary fuel powder is selected from one or more of Si, Fe, Sn, and Mn powders.

[0040] Optionally, the particle size of the auxiliary fuel powder is 100-400 mesh.

[0041] Optionally, the inert inorganic filler is selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride.

[0042] Optionally, the particle size of the inert inorganic filler is not less than 800 mesh.

[0043] Optionally, in step S2, the mixing time is 5-10 minutes.

[0044] Optionally, in step S3, an automatic press is used to press the material at a pressure of 30-50 T / cm. 2 After being compressed and molded, the density of the ignition charge is 1.7-2.3 g / cm³. 3 .

[0045] Compared with the prior art, the advantages of this disclosure include:

[0046] 1) Low mechanical sensitivity and high safety of the igniter. Inert inorganic fillers can neutralize the mechanical sensitivity of the igniter, forming a high-performance protective layer between the oxidizer and fuel. This layer can prevent and extinguish the explosive propagation of hot spots under mechanical action, acting as an endothermic filling agent and a friction buffer between the oxidizer and metal particles, thereby reducing its sensitivity under mechanical action and improving the safety of transportation and use. Simultaneously, inorganic fillers facilitate crack-free propellant grain formation and stabilize residues, improving ignition performance and further enhancing ignition safety.

[0047] 2) The preparation method is simple, and modular production is highly efficient. The molding process does not require wet mixing and drying; the dry powder is directly pressed, significantly improving production efficiency. Simultaneously, the igniter is molded separately in modular form, and the pressing and demolding processes are not affected or limited by the oxygen-generating propellant column, resulting in good process consistency.

[0048] 3) The igniter has good formability and can be pressed into various shapes according to the design of the propellant column. It has high density and strong resistance to impact and vibration.

[0049] 4) The ignition performance of the igniter is good. The particle size of the inorganic filler is significantly smaller than that of the oxidizer and fuel powder, so it does not affect the ignition and combustion performance of the igniter and can achieve ignition and ignition in environments ranging from -40℃ to 70℃.

[0050] 5) The low gas production rate of the igniter is conducive to the qualified gas composition indicators of the oxygen candle product; the formula contains no catalyst and has a high decomposition temperature, thus having a high calorific value, which is beneficial to the ignition performance of the igniter at low temperatures. Detailed Implementation

[0051] To facilitate understanding of this disclosure, the following description will be more comprehensive and detailed in conjunction with preferred embodiments, but the scope of protection of this disclosure is not limited to the following specific embodiments.

[0052] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of this disclosure.

[0053] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this disclosure are available on the market or can be prepared by existing methods.

[0054] This disclosure provides an oxygen candle igniter, which is suitable for rapidly igniting an oxygen-producing propellant column to generate oxygen when a solid chemical oxygen generator is ignited.

[0055] The oxygen candle igniter is composed of the following components by mass percentage: 20%-46% oxidizer powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler.

[0056] In some alternative embodiments, the amount of oxidant powder can be 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 44%, or 46%, or other values ​​in the range of 20% to 46%.

[0057] The amount of fuel powder can be 15%, 18%, 20%, 22%, 25%, 28%, 30% or 32%, or other values ​​within the range of 15%-32%.

[0058] The amount of inert inorganic filler can be 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, or 56%, or other values ​​within the range of 28%-56%.

[0059] In some optional embodiments, the fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):1. Exemplarily, the weight ratio of main fuel powder to auxiliary fuel powder can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1, or other values ​​within the range of (1-8):1.

[0060] In some alternative embodiments, the oxidant powder may be selected, exemplarily, from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

[0061] In some alternative embodiments, the main fuel powder may be selected, for example, from one or more of Mg, Al, and Ti powders.

[0062] In some alternative embodiments, the auxiliary fuel powder is exemplary selected from one or more of Si, Fe, Sn, and Mn powders.

[0063] In some alternative embodiments, the inert inorganic filler may be selected, exemplarily, from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride. For example, the inert inorganic filler may be selected from one or more of zinc oxide, nickel oxide, titanium oxide, chromium oxide, aluminum oxide, silicon dioxide, magnesium sulfate, calcium sulfate, calcium silicate, and boron nitride.

[0064] In some alternative embodiments, the particle size of the oxidant powder can be 60-200 mesh, such as 60 mesh, 80 mesh, 100 mesh, 120 mesh, 150 mesh, 180 mesh or 200 mesh, or other values ​​within the range of 60-200 mesh.

[0065] In some alternative embodiments, the particle size of the main fuel powder and the auxiliary fuel powder can be independently 100-400 mesh, such as 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh, 350 mesh or 400 mesh, or other values ​​within the range of 100-400 mesh.

[0066] In some alternative embodiments, the particle size of the inert inorganic filler is not less than 800 mesh.

[0067] In addition, this disclosure also provides an oxygen candle ignition block, which is composed of 20%-46% oxidant powder, 15%-32% fuel powder and 28%-56% inert inorganic filler by mass percentage, which are dry-mixed evenly and then pressed into shape.

[0068] In some alternative embodiments, the amount of oxidant powder can be 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 44%, or 46%, or other values ​​in the range of 20% to 46%.

[0069] The amount of fuel powder can be 15%, 18%, 20%, 22%, 25%, 28%, 30% or 32%, or other values ​​within the range of 15%-32%.

[0070] The amount of inert inorganic filler can be 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, or 56%, or other values ​​within the range of 28%-56%.

[0071] In some optional embodiments, the fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):1. Exemplarily, the weight ratio of main fuel powder to auxiliary fuel powder can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1, or other values ​​within the range of (1-8):1.

[0072] In some optional embodiments, the oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate. The particle size of the oxidant powder can be 60-200 mesh, such as 60 mesh, 80 mesh, 100 mesh, 120 mesh, 150 mesh, 180 mesh, or 200 mesh, or other values ​​within the range of 60-200 mesh.

[0073] In some alternative embodiments, the main fuel powder is exemplary selected from one or more of Mg, Al, and Ti powders. The particle size of the main fuel powder can be 100-400 mesh, such as 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh, 350 mesh, or 400 mesh, or other values ​​within the range of 100-400 mesh.

[0074] In some alternative embodiments, the auxiliary fuel powder is exemplary selected from one or more of Si, Fe, Sn, and Mn powders. The particle size of the auxiliary fuel powder can be 100-400 mesh, such as 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh, 350 mesh, or 400 mesh, or other values ​​within the range of 100-400 mesh.

[0075] In some alternative embodiments, the inert inorganic filler may be exemplary selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride. The particle size of the inert inorganic filler is not less than 800 mesh.

[0076] In addition, this disclosure also provides a method for preparing an oxygen candle igniter, comprising the following steps:

[0077] S1. Weigh 20%-46% oxidant powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler by mass percentage, mix and sieve to break up the powder; the fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):1.

[0078] The oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate. The particle size of the oxidant powder can be 60-200 mesh, such as 60 mesh, 80 mesh, 100 mesh, 120 mesh, 150 mesh, 180 mesh, or 200 mesh, or other values ​​within the range of 60-200 mesh.

[0079] The main fuel powder can be selected, for example, from one or more of Mg, Al, and Ti powders. The particle size of the main fuel powder can be 100-400 mesh, such as 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh, 350 mesh, or 400 mesh, or other values ​​within the range of 100-400 mesh.

[0080] The auxiliary fuel powder can be selected, for example, from one or more of Si, Fe, Sn, and Mn powders. The particle size of the auxiliary fuel powder can be 100-400 mesh, such as 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh, 350 mesh, or 400 mesh, or other values ​​within the range of 100-400 mesh.

[0081] Inert inorganic fillers may be selected, for example, from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride. The particle size of the inert inorganic filler is not less than 800 mesh.

[0082] S2. Pour the sieved mixture into the mixer, mix until homogeneous, then pour out to complete the dry mixing of the ignition charge.

[0083] The mixing time can be 5-10 minutes, such as 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, or other values ​​within the range of 5-10 minutes.

[0084] S3. Load the dry-mixed ignition charge into the mold and press it into shape.

[0085] This process can be performed using an automatic press.

[0086] The press pressure can be 30-50T / cm 2 , such as 30T / cm 2 35T / cm 2 40T / cm 2 45T / cm 2 Or 50T / cm 2 etc., or 30-50T / cm 2 Other values ​​within the range.

[0087] The density of the ignition charge after compression molding can be 1.7-2.3 g / cm³. 3 .

[0088] Example 1

[0089] The particle size and proportion of the oxygen candle igniter formulation components in this embodiment are shown in Table 1.

[0090] Table 1

[0091] The preparation method of the oxygen candle igniter in this embodiment is as follows:

[0092] Weigh 28g of 80-mesh potassium perchlorate, 12g of 300-mesh aluminum powder, 12g of 400-mesh tin powder, 32g of 3000-mesh zinc oxide, and 16g of 7000-mesh calcium silicate, and pass them through an 80-mesh sieve to disperse the powders. Pour the sieved mixture into a mixer and mix it using a vortex mixer for 5 minutes until it is homogeneous. Then pour it out to complete the dry mixing of the ignition charge.

[0093] Weigh 15g of the dry-mixed ignition charge and fill it into a mold. Press it into shape using an automatic press at a pressure of 30T / cm. 2 The density of the ignition charge after compression molding is 1.9 g / cm³. 3 .

[0094] The igniter prepared in this embodiment has an impact sensitivity of 0%, a friction sensitivity of 8%, an electrostatic sensitivity of 3876V, a flame sensitivity of 75 / 90mm, a heat of explosion of 5.4kJ / g, and a yield of 0.03g. 2 The powder shedding rate was ≤0.6% during a 6-hour durability vibration test at / Hz. The oxygen generator, installed with a flame cap, was kept at -40℃, 23℃, and 70℃ for 4 hours respectively before ignition. Ignition was successful, and the oxygen-producing column burned continuously.

[0095] Example 2

[0096] The particle size and proportion of the oxygen candle igniter formulation components in this embodiment are shown in Table 2.

[0097] Table 2

[0098] The preparation method of the oxygen candle igniter in this embodiment is as follows:

[0099] Weigh 32g of 200-mesh sodium chlorate, 12g of 300-mesh magnesium powder, 5g of 400-mesh silicon powder, 30g of 4000-mesh nickel oxide, and 21g of 900-mesh magnesium sulfate, and pass them through a 200-mesh sieve to disperse the powders. Pour the sieved mixture into a mixer and mix it using a vortex mixer for 5 minutes until it is homogeneous. Then pour it out to complete the dry mixing of the ignition charge.

[0100] Weigh 15g of the dry-mixed ignition charge and fill it into a mold. Press it into shape using an automatic press at a pressure of 30T / cm. 2 The density of the ignition charge after compression molding is 1.8 g / cm³. 3 .

[0101] The igniter prepared in this embodiment has an impact sensitivity of 0%, a friction sensitivity of 0%, an electrostatic sensitivity of 3318V, a flame sensitivity of 45 / 90mm, a heat of explosion of 4.8kJ / g, and a yield of 0.03g. 2 The powder shedding rate was ≤0.8% during a 6-hour durability vibration test at / Hz. The oxygen generator, installed with a flame cap, was kept at -40℃, 23℃, and 70℃ for 4 hours before ignition. Ignition was successful, and the oxygen-producing column burned continuously.

[0102] Example 3

[0103] The particle size and proportion of the oxygen candle igniter formulation components in this embodiment are shown in Table 3.

[0104] Table 3

[0105] The preparation method of the oxygen candle igniter in this embodiment is as follows:

[0106] Weigh 20g of 200-mesh sodium chlorate, 22g of 60-mesh sodium perchlorate, 18g of 300-mesh magnesium powder, 4g of 400-mesh iron powder, 28g of 2000-mesh silicon dioxide, and 8g of 1200-mesh titanium dioxide, and pass them through a 60-mesh sieve to disperse the powders. Pour the sieved mixture into a mixer and mix it using a vortex mixer for 5 minutes until it is homogeneous. Then pour it out to complete the dry mixing of the ignition charge.

[0107] Weigh 20g of the dry-mixed ignition charge and fill it into a mold. Press it into shape using an automatic press at a pressure of 40T / cm. 2 The density of the ignition charge after compression molding is 2.1 g / cm³. 3 .

[0108] The igniter prepared in this embodiment has an impact sensitivity of 0%, a friction sensitivity of 4%, an electrostatic sensitivity of 2983V, a flame sensitivity of 65 / 90mm, a heat of explosion of 5.2kJ / g, and a yield of 0.03g. 2 The powder shedding rate was ≤0.4% during a 6-hour durability vibration test at / Hz. The oxygen generator, installed with a flame cap, was kept at -40℃, 23℃, and 70℃ for 4 hours before ignition. Ignition was successful, and the oxygen-producing column burned continuously.

[0109] Example 4

[0110] The particle size and proportion of the oxygen candle igniter formulation components in this embodiment are shown in Table 4.

[0111] Table 4

[0112] The preparation method of the oxygen candle igniter in this embodiment is as follows:

[0113] Weigh 36g of 100-mesh sodium chlorate, 14g of 100-mesh titanium powder, 7g of 400-mesh tin powder, and 43g of 8000-mesh boron nitride and pass them through a 100-mesh sieve to disperse the powders. Pour the sieved mixture into a mixer and mix it for 5 minutes using a vortex mixer until it is homogeneous. Then pour it out to complete the dry mixing of the ignition charge.

[0114] Weigh 15g of the dry-mixed ignition charge and fill it into a mold. Press it into shape using an automatic press at a pressure of 40T / cm. 2 The density of the ignition charge after compression molding is 1.9 g / cm³. 3 .

[0115] The igniter prepared in this embodiment has an impact sensitivity of 0%, a friction sensitivity of 0%, an electrostatic sensitivity of 3523V, a flame sensitivity of 50 / 90mm, a heat of explosion of 5.1kJ / g, and a yield of 0.03g. 2 The powder shedding rate was ≤0.2% during a 6-hour durability vibration test at / Hz. The oxygen generator, installed with a flame cap, was kept at -40℃, 23℃, and 70℃ for 4 hours respectively before ignition. Ignition was successful, and the oxygen-producing column burned continuously. Industrial applicability

[0116] The oxygen candle igniter provided in this disclosure has low mechanical sensitivity and high safety in use; it has good formability and strong resistance to impact and vibration of the propellant; it has good ignition performance, enabling ignition and ignition transmission in environments ranging from -40℃ to 70℃, and is suitable for rapidly igniting oxygen-producing propellant to generate oxygen when ignited in a solid chemical oxygen generator. The preparation method of this oxygen candle igniter is simple, and modular production has high efficiency; it is suitable for rapidly igniting oxygen-producing propellant to generate oxygen when ignited in a solid chemical oxygen generator.

Claims

1. An oxygen candle igniter, characterized in that: It is composed of the following components by mass percentage: 20%-46% oxidant powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler; The fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):

1.

2. The oxygen candle igniter according to claim 1, characterized in that: The oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

3. The oxygen candle igniter according to claim 1 or 2, characterized in that: The main fuel powder is selected from one or more of Mg, Al, and Ti powders.

4. The oxygen candle igniter according to any one of claims 1 to 3, characterized in that: The auxiliary fuel powder is selected from one or more of Si, Fe, Sn, and Mn powders.

5. The oxygen candle igniter according to any one of claims 1 to 4, characterized in that: The inert inorganic filler is selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride.

6. The oxygen candle igniter according to claim 5, characterized in that: The inert inorganic filler is selected from one or more of zinc oxide, nickel oxide, titanium oxide, chromium oxide, aluminum oxide, silicon dioxide, magnesium sulfate, calcium sulfate, calcium silicate, and boron nitride.

7. The oxygen candle igniter according to any one of claims 1 to 6, characterized in that: The oxidant powder has a particle size of 60-200 mesh.

8. The oxygen candle igniter according to any one of claims 1 to 7, characterized in that: The fuel powder has a particle size of 100-400 mesh.

9. The oxygen candle igniter according to any one of claims 1 to 8, characterized in that: The particle size of the inert inorganic filler is not less than 800 mesh.

10. An oxygen candle igniter for a propellant block, characterized in that: It is made by dry mixing 20%-46% oxidant powder, 15%-32% fuel powder and 28%-56% inert inorganic filler by mass percentage, and then pressing it into shape. The fuel powder consists of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):

1.

11. The oxygen candle ignition block according to claim 10, characterized in that: The oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

12. The oxygen candle ignition block according to claim 11, characterized in that: The particle size of the oxidant powder is 60-200 mesh.

13. The oxygen candle ignition block according to any one of claims 10 to 12, characterized in that: The main fuel powder is selected from one or more of Mg, Al, and Ti powders.

14. The oxygen candle ignition block according to any one of claims 10 to 13, characterized in that: The main fuel powder has a particle size of 100-400 mesh.

15. The oxygen candle ignition block according to any one of claims 10 to 14, characterized in that: The auxiliary fuel powder is selected from one or more of Si, Fe, Sn, and Mn powders.

16. The oxygen candle ignition block according to any one of claims 10 to 15, characterized in that: The auxiliary fuel powder has a particle size of 100-400 mesh.

17. The oxygen candle ignition block according to any one of claims 10 to 16, characterized in that: The inert inorganic filler is selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride.

18. The oxygen candle ignition block according to any one of claims 10 to 17, characterized in that: The particle size of the inert inorganic filler is not less than 800 mesh.

19. A method for preparing an oxygen candle igniter, characterized in that: Includes the following steps: S1. Weigh 20%-46% oxidant powder, 15%-32% fuel powder, and 28%-56% inert inorganic filler by mass percentage, mix and sieve to disperse the powder; the fuel powder is composed of main fuel powder and auxiliary fuel powder in a weight ratio of (1-8):

1. S2. Pour the sieved mixture into the mixer, mix until homogeneous, then pour out to complete the dry mixing of the ignition charge; S3. Load the dry-mixed ignition charge into the mold and press it into shape.

20. The method for preparing the oxygen candle igniter according to claim 19, characterized in that: In step S1, the oxidant powder is selected from one or more of sodium chlorate, sodium perchlorate, potassium chlorate, and potassium perchlorate.

21. The method for preparing the oxygen candle igniter according to claim 19 or 20, characterized in that: The particle size of the oxidant powder is 60-200 mesh.

22. The method for preparing the oxygen candle igniter according to any one of claims 19 to 21, characterized in that: The main fuel powder is selected from one or more of Mg, Al, and Ti powders.

23. The method for preparing the oxygen candle igniter according to any one of claims 19 to 22, characterized in that: The main fuel powder has a particle size of 100-400 mesh.

24. The method for preparing the oxygen candle igniter according to any one of claims 19 to 23, characterized in that: The auxiliary fuel powder is selected from one or more of Si, Fe, Sn, and Mn powders.

25. The method for preparing the oxygen candle igniter according to any one of claims 19 to 24, characterized in that: The particle size of the auxiliary fuel powder is 100-400 mesh.

26. The method for preparing the oxygen candle igniter according to any one of claims 19 to 25, characterized in that: The inert inorganic filler is selected from one or more of metal oxides, silicon dioxide, sulfate compounds, silicate compounds, and boron nitride.

27. The method for preparing the oxygen candle igniter according to any one of claims 19 to 26, characterized in that: The particle size of the inert inorganic filler is not less than 800 mesh.

28. The method for preparing the oxygen candle igniter according to any one of claims 19 to 27, characterized in that: In step S2, the mixing time is 5-10 minutes.

29. The method for preparing the oxygen candle igniter according to any one of claims 19 to 28, characterized in that: In step S3, an automatic press is used to compress the propellant at a pressure of 30-50 T / cm², resulting in a propellant charge density of 1.7-2.3 g / cm³ after compression. 3 .