Process for structuring glass elements by etching processes and glass element produced according to the process

A combined sodium-potassium hydroxide etching process for glass substrates addresses high roughness and corrosion issues, achieving efficient etching with low roughness and extended equipment life.

WO2026233690A1PCT designated stage Publication Date: 2026-11-12SCHOTT AG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/061392
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-04-21
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing etching processes for glass substrates face challenges such as high surface roughness, contamination from silicate precipitates, and equipment corrosion, particularly when using sodium hydroxide, while potassium hydroxide-based processes are slow.

Method used

A wet-chemical etching process using a mixture of sodium hydroxide and potassium hydroxide with controlled proportions to achieve high etching rates and low surface roughness, reducing equipment corrosion and precipitate formation.

Benefits of technology

The method achieves etching rates of over 2 pm/h with low surface roughness (Ra < 0.5 nm) and extends equipment life by using a diluted alkali hydroxide solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026061392_12112026_PF_FP_ABST
    Figure EP2026061392_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a process for producing an etched glass element, wherein at least regions of a glass element are etched through the influence of an aqueous, basic etching medium. The provided etching medium contains sodium hydroxide and potassium hydroxide having a total content in the range of 15% to 40% by weight, wherein the weight fractions of sodium hydroxide and potassium hydroxide in the etching medium are subject to the following condition: 0 < m(NaOH) / m(KOH) < 1. The invention further relates to an etched glass element produced by the process according to the invention and having a roughness Ra < 0.4 nm and / or a roughness Rq < 0.5 in the etched regions.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Method for structuring glass elements by etching processes and glass element produced according to the method

[0002] Description

[0003] The invention relates generally to a method for producing structured glass elements and to a glass element produced accordingly. In particular, the invention relates to a method for producing structured glass elements by basic etching.

[0004] State of the art

[0005] The precise structuring of glass is of great interest in many application areas. Among others, glass substrates are used in camera imaging, especially 3D camera imaging, in electro-optics such as LEDs, microfluidics, optical diagnostics, sensor technology (e.g., pressure sensors), and diagnostic technology. Such application areas include, for example, light sensors, camera sensors, pressure sensors, LEDs, and laser diodes. Here, glass substrates are mostly used as components in the form of thin wafers or glass membranes. Furthermore, glass substrates can be used as covers or cover glasses in displays, such as LED displays.

[0006] To enable the glass substrates to be used in a wide range of applications, the processing should not leave any damage, residues (such as separated, abraded, or detached material), or stresses in the edge area or volume of the substrate. Furthermore, the production process for these substrates should allow for the most efficient manufacturing process possible.

[0007] Structuring processes often involve basic etching processes used to remove material from the glass substrate or modify surfaces. Sodium hydroxide (NaOH) in an aqueous etching medium is typically used as the base in this type of etching. Sodium hydroxide is particularly favored because it allows for high etch rates, meaning high material removal per unit of time. However, the use of sodium hydroxide has some drawbacks. While high etch rates and thus high material removal per unit of time can be achieved in etching processes with sodium hydroxide, the resulting surfaces exhibit relatively high roughness. High roughness can negatively impact subsequent processes, such as surface bonding.

[0008] Another disadvantage of using etching solutions with sodium hydroxide as the sole base is the poor solubility of the components dissolved during the process in the etching solution. This can lead to the formation of silicate precipitates, which in turn can contaminate the etched substrates in the form of streaks or deposits.

[0009] Furthermore, etching media based on sodium hydroxide exhibit a high corrosive effect on the equipment, containers, and their components used, for example, on stainless steel components. Therefore, etching devices with stainless steel tanks and equipment have relatively short service lives when used in etching processes with sodium hydroxide as the base.

[0010] Other basic etching media, such as aqueous potassium hydroxide (KOH) solutions, do not exhibit these disadvantages or only to a lesser degree. However, a disadvantage here is the low etching rate, making corresponding etching processes time-consuming.

[0011] WO 2020 / 243211 A1 discloses a process for etching glass substrates using a eutectic mixture of sodium hydroxide and potassium hydroxide. The etching medium is formed by a mixed melt of sodium hydroxide and potassium hydroxide. The etching process therefore takes place at high process temperatures of 170 to 300°C. Furthermore, it is not a wet chemical process.

[0012] Object of the invention

[0013] Therefore, there is a need to provide a method for structuring glass substrates through etching processes that enables high etching rates without the disadvantages known from the prior art. In particular, the method should make it possible to produce etched glass surfaces with low roughness. The method should also enable improved service life of the equipment used. A further objective is to provide a glass substrate with at least partially etched areas, the etched areas of which exhibit low roughness.

[0014] Disclosure of the invention

[0015] The object of the invention is already solved by the subject matter of the independent claim. Advantageous embodiments and further developments are the subject matter of the dependent claims.

[0016] The invention relates to a method for producing glass elements with at least partially etched surfaces, or to a method for etching glass elements in which material is removed from the glass element at least partially or in certain areas by an etching process. In particular, the etching process is a wet-chemical, basic etching process.

[0017] According to one embodiment of the disclosed method, a structured glass element can be obtained. For the purposes of this disclosure, a structured glass element is understood to be a glass element that has at least one etched area. The disclosed etching method can also be part of a structuring process, for example, in laser structuring or lithography processes.

[0018] The process for producing a glass element that is at least partially etched comprises at least the following steps:

[0019] Providing a glass element

[0020] Providing an aqueous, basic etching medium,

[0021] The etching medium acts on the areas of the glass element to be etched for a duration t and

[0022] Removal of the etching medium from the etched glass element, wherein the provided aqueous etching medium contains sodium hydroxide and potassium hydroxide with a total content of sodium hydroxide and potassium hydroxide in the range of 15 to 52 wt% and wherein the proportion p of sodium hydroxide to the total alkali content

[0023] m NaOH

[0024] p = - m NaOH + m KOH

[0025] In the etching medium, the following applies: 0 < p < 1, in particular 0.1 < p < 0.8, preferably 0.09 < p < 0.8.

[0026] The glass element, with the areas to be etched, is brought into contact with the aqueous, alkaline etching medium for a duration t. The etching medium has a liquid phase. The liquid phase acts as a solvent in which alkali metal hydroxides are dissolved. For the purposes of this disclosure, an aqueous etching medium is understood to be, in particular, an etching medium whose liquid phase contains at least 48 wt.%, preferably at least 70 wt.%, and most preferably at least 85 wt.% water as a solvent. One embodiment provides that the liquid phase of the etching medium consists of water. The liquid phase of the etching medium may contain other liquid compounds, in particular solvents such as low molecular weight alcohols.

[0027] The etching medium contains sodium hydroxide and potassium hydroxide. The total content of alkali metal hydroxides, particularly the sodium hydroxide and potassium hydroxide content in the etching medium, is in the range of 15 to 52 wt.%. According to one embodiment, the etching solution contains 48 to 85 wt.% water, preferably 60 to 75 wt.% water. This ensures a sufficiently high concentration of hydroxide ions for the etching process, while simultaneously guaranteeing that the sodium hydroxide and potassium hydroxide are present in dissolved form in the etching medium and that the solubility product of the glass components released during the etching process is not reached, thus reducing or preventing precipitate formation. Preferably, the etching medium has a temperature below 135°C during the process, particularly in the range of 80 to 130°C, and more preferably in the range of 90 to 100°C.

[0028] For application and action, the etching medium can be applied to the glass element or areas of the glass element. Another embodiment provides that the glass element, at least with the areas to be etched, is immersed in the etching medium. Preferably, the glass element is immersed in the etching medium, at least with the areas to be etched.

[0029] In a general embodiment, p: 0.01 < p < 0.99, preferably 0.05 < p < 0.95. The relative proportion of sodium hydroxide to the sum of sodium hydroxide and potassium hydroxide can therefore lie within a very wide range, with interesting advantages being achieved for both low and high p-values, as will be shown below.

[0030] According to one embodiment, potassium hydroxide predominates in the etching medium. The following applies to the proportion of sodium hydroxide in the total alkali content of the etching medium:

[0031] 0.01 < p < 0.50, preferred; 0.05 < p < 0.5, more preferred; 0.1 < p < 0.5; and most preferred; 0.15 < p < 0.30

[0032] Surprisingly, the etching rate can be increased by adding even a small amount of sodium hydroxide compared to a process using an etching medium containing only potassium hydroxide. Therefore, in the disclosed process, the etching medium contains sodium hydroxide in addition to potassium hydroxide. The proportion of sodium hydroxide in the etching medium is preferably kept so low that it has no effect, or at least no significant effect, on the solubility of the dissolved glass components. Furthermore, the surfaces etched using the disclosed process exhibit a roughness that is significantly lower than that achievable with comparable structuring processes using sodium hydroxide as the sole base in the etching medium.

[0033] Another embodiment provides that the proportion of sodium hydroxide in the etching medium is greater than the proportion of potassium hydroxide. Here, p > 0.5. In particular, in this embodiment, 0.5 < p < 0.99, preferably 0.5 < p < 0.9, more preferably 0.7 < p < 0.9, and most preferably 0.7 < p < 0.85. With these embodiments, low surface roughness can still be achieved despite higher etching rates. However, the higher sodium hydroxide content can lead to greater stress on the equipment. The addition of sodium hydroxide to the etching medium results in a significant increase in the etching rate. The inventors have discovered that there is no linear relationship between the mixing ratio of potassium hydroxide and sodium hydroxide and the etching rate.While the etching rate initially increases upon the addition of small amounts of sodium hydroxide, beyond a certain sodium hydroxide-potassium hydroxide ratio, the rate increases significantly more slowly with increasing sodium hydroxide content, approaching a limit. Simultaneously, the solubility of the silicates released by the etching process decreases with increasing sodium hydroxide content, causing them to precipitate and deposit as impurities in the etched areas. The roughness of the etched glass, or in the etched areas, remains low up to a NaOH concentration corresponding to p = 0.8, which is particularly advantageous for subsequent applications. This allows for increasing etching removal with low or only slightly increased roughness of the etched areas.

[0034] The disclosed proportion of sodium hydroxide in the total alkali content of the etching medium is therefore selected to enable an etching process that combines the advantages of a potassium hydroxide-based etching process with those of a sodium hydroxide-based etching process.

[0035] Preferably, the etching medium contains 3 to 15 wt.%, more preferably 3 to 12 wt.%, and particularly preferably 3 to 9 wt.% sodium hydroxide. The potassium hydroxide content in the etching medium is preferably in the range of 12 to 30 wt.%, more preferably 12 to 25 wt.%, and particularly preferably 15 to 20 wt.%. According to one embodiment, the etching medium has a sodium hydroxide content in the range of 3 to 9 wt.% and a potassium hydroxide content in the range of 15 to 20 wt.%. The specified contents apply in particular to an etching medium that is provided at the beginning of the structuring process. These values ​​can change during the process, especially during the etching time t, as the glass components are released.

[0036] Surprisingly, by using an etching medium comprising both sodium hydroxide and potassium hydroxide, the total alkali hydroxide content in the etching medium can be reduced without significantly reducing the etching rate. One embodiment provides that the alkali hydroxide content, particularly sodium hydroxide and potassium hydroxide, in the etching medium is in the range of 15 to 25 wt.%, preferably 15 to 20 wt.%, or even below 20 wt.%. In etching processes where only sodium hydroxide is used as the base, etching media with a sodium hydroxide content of 25 to 30 wt.% are typically employed. In this embodiment, the etching medium thus has a lower alkali hydroxide concentration. This has a beneficial effect on both the service life of the equipment used in the process and the solubility of the dissolved silicates in the etching medium.

[0037] In the disclosed process, etching rates of more than 2 pm / h, preferably more than 3 pm / h or even more than 4 pm / h can be achieved at an etching temperature in the range of 90 to 135 °C, particularly at an etching temperature of 95 °C. According to one embodiment, the glass has the following composition in mol%:

[0038] SiO265 - 75

[0039] B2O3 5 - 10

[0040] AI2O3 1 - 4

[0041] Na2O 3 - 8

[0042] K2O 2 - 6

[0043] ZnO 2 - 6

[0044] TiO22 - 5

[0045] When etching this glass at a temperature of 95°C, etch rates of more than 2 pm / h or even more than 3 pm / h can be achieved. During the structuring or etching process, the glass components are dissolved from the glass of the element to be structured by hydroxide ions. This reduces the concentration of free hydroxide ions in the etching medium, while simultaneously introducing the dissolved components, such as silicates, into the etching medium. As a result, the etch rate may not remain constant throughout the structuring process, but rather decrease with increasing silicate input.

[0046] One embodiment provides that the etching rate is in the range of 2 to 7 pm / h, preferably in the range of 3 to 7 pm / h. In comparison, similar processes, in which the etching medium contains only potassium hydroxide as the base, achieve etching rates of less than 2 pm / h. The disclosed process is particularly suitable for multi-component glasses, especially borosilicate glasses.

[0047] According to one embodiment, the provided glass has the following oxide-based composition in mol%: SiO275 - 85

[0048] B2O3 9 - 12

[0049] AI2O3 0.5 - 3

[0050] Na2O 2 - 5

[0051] K2O 0.1 - 1

[0052] The areas of the glass element etched using the disclosed method exhibit low roughness in the nm range. According to one embodiment, the root mean square (Rq) roughness of a surface structured using the disclosed method is at most 0.6 nm, preferably at most 0.5 nm. The roughness value Rq was determined using a white light interferometer. In particular, the root mean square (Rq) is in the range of 0.05 to 0.6 nm, preferably in the range of 0.05 to 0.5 nm.

[0053] Alternatively or additionally, an area etched using the disclosed method has an arithmetic mean roughness Ra of at most 0.5 nm, preferably at most 0.4 nm. The roughness value Rq was determined using a white light interferometer. In particular, the arithmetic mean roughness Ra is in the range of 0.05 to 0.5 nm, preferably in the range of 0.05 to 0.4 nm.

[0054] The inventors surprisingly discovered that even the addition of small amounts of KOH to a NaOH-containing etching solution leads to low surface roughness while maintaining good etching rates. For example, etching with pure 30% KOH at an etching temperature of 95 °C results in a target roughness of Rq in the range of 0.3–0.45 nm. Etching with pure NaOH, on the other hand, leads to an undesirable increase in roughness Rq > 0.7 nm. However, by adding small amounts of KOH to the etching solution, etched areas with low roughness can be obtained. Even with a NaOH ratio of p = m(NaOH) / m(NaOH) + m(KOH) of 0.8, roughness Ra of less than 0.5 nm can be achieved after the etching process.

[0055] The invention will be described in more detail below with reference to the figures and exemplary embodiments, without limitation thereto. Identical reference numerals denote identical or similar elements. The figures show:

[0056] Fig. 1 shows a schematic representation of a glass element before the etching process according to a first embodiment.

[0057] Fig. 2: a schematic representation of the etching process using the first embodiment shown in Fig. 1,

[0058] Fig. 3: a schematic representation of an etched glass element,

[0059] Fig. 4: a graphical representation of the relationship between sodium hydroxide content in the etching medium p and the etching rate

[0060] Fig. 5 is a graphical representation of the relationship between the proportion of NaOH in the etching medium p and the roughness of the structured areas.

[0061] Fig. 6 shows a schematic representation of a glass element before the etching process according to a second embodiment.

[0062] Figs. 7 and 8: a schematic representation of the etching process using the second embodiment shown in Fig. 6, and

[0063] Fig. 9 shows a schematic representation of an etched glass element according to the second embodiment.

[0064] Fig. 1 schematically shows a plate-shaped glass element 1 according to a first embodiment, which is etched using the disclosed method. The glass element 1 has a first surface 2 and a second surface 3 arranged opposite the first. The distance between the first surface 2 and the second surface 3 corresponds to the glass thickness d1.

[0065] Fig. 2 schematically illustrates the step of the disclosed method in which the glass element 1 is brought into contact with the etching medium 7 in certain areas. In the embodiment shown in Fig. 2, the glass element 1 is immersed with its first surface 2 in an etching bath 6 comprising the etching medium 7.

[0066] In the embodiment shown in Fig. 2, the etching medium 7 is an aqueous solution of sodium hydroxide and potassium hydroxide, with the proportion of sodium hydroxide being 15 wt.% and the proportion of potassium hydroxide 5 wt.%. The total alkali metal oxide content is thus 20 wt.%. In addition to the alkali metal oxides, other compounds may be present in the liquid phase of the etching medium 7. These may include, in particular, auxiliary substances such as complexing agents. These can be used, for example, to increase the solubility of the dissolved glass components in the etching medium 7. This is particularly advantageous if the glass of the glass element 1 to be structured has a high proportion of alkaline earth oxides, especially calcium oxide, which form sparingly soluble silicates during the etching process.

[0067] The etching medium 7 has a temperature in the range of 90 to 100 °C during the etching process. This accelerates the etching reaction. The reaction temperature is limited by the boiling point of the etching medium 7.

[0068] The glass element 1 in the present case has the following oxide-based composition in mol%:

[0069] SiO283.3

[0070] B2O3 11 ,3

[0071] AI2O3 1 ,5

[0072] Na2O 3.5

[0073] K2O 0.4

[0074] The surface 2 of the glass element 1 is exposed to the etching medium, so that material is removed from the glass element starting from surface 2. In the case shown in Fig.

[0075] In the embodiment shown in Figure 3, the thickness of the glass element 1 is reduced. Thus, the etched glass element 10 has a thickness d2 after the etching process. The difference between the glass thicknesses d1 and d2 is the material removal rate 70. The rate at which the material is removed can be specified by the etching rate, also called the removal rate. The glass element 1 remains in the etching medium 7 for a period of time t until the desired material removal rate 70 is reached and the etched glass element 10 is obtained. After the etching time t, the etched glass element 10 is removed from the etching bath 6 and, if necessary, cleaned. In the embodiment shown, the etching time t is in the range of 5 to 6 hours. This is comparable to the etching time of etching processes using an etching medium with sodium hydroxide as the sole base.

[0076] The etched surface 20 exhibits a mean roughness Ra of less than 0.4 nm. Furthermore, the root mean square roughness Rq is less than 0.6 nm. These low roughness values ​​are advantageous for subsequent processes such as metallization.

[0077] Table 1 shows the composition of various etching media as well as the determined etching rates of various embodiments 1 to 3 and the comparative examples 4 to 6.

[0078] c(NaOH) c(KOH) C(NaOH+KOH) Etching rate

[0079] Example Rq [nm] Ra [nm] wt.% wt.% wt.% P [pm / h]

[0080] 1 6 24 30 0.2 1.7 0.42 0.33 2 7.2 18 25.2 0.25 2.8 0.43 0.33 3 7.2 18 25.2 0.25 3.3 0.40 0.32 4 14.9 13.5 28.4 0.5 4 0.41 0.32 5 24 6 30 0.8 7.1 0.42 0.33 6 0 30 30 0 1.8 0.43 0.34

[0081]

[0082] 7 30 0 30 1 6.8 0.72 0.55

[0083] Table 1

[0084] In all examples, a glass element was etched at 95°C for 6 hours. The etching loss was then determined. The individual examples differ in terms of the sodium hydroxide and potassium hydroxide contents in the etching medium. The glass element in these embodiments has the following oxide-based composition in mol%:

[0085] SiO269.60

[0086] B2O3 7.90

[0087] AI2O3 2.70

[0088] Na2O 6.70

[0089] K2O 4.80

[0090] ZnO 4.73

[0091] TiO23.35

[0092] In examples 1 to 5, both sodium hydroxide and potassium hydroxide were used in the etching medium. The etching media in examples 4 and 5 have a higher sodium hydroxide content than potassium hydroxide content. In comparative example 6, only potassium hydroxide was used in the etching medium, and in comparative example 7, only sodium hydroxide was used as the alkali metal oxide.

[0093] Table 1 clearly shows that the etching rate of an etching solution with sodium hydroxide as the sole base (Comparison Example 7) is increased by a factor of 3 to 4 compared to an etching solution with potassium hydroxide as the sole base (Comparison Example 6). Surprisingly, even relatively small amounts of sodium hydroxide in an etching solution containing both sodium hydroxide and potassium hydroxide lead to a significant increase in the etching rate. The etching solution in Example 2 contains only 7.2 wt% sodium hydroxide at a ratio p = m(NaOH) / (m(KOH) + m(NaOH)) of 0.25. Despite this, the etching rate has increased significantly compared to an etching solution with potassium hydroxide as the sole base, while the roughness Ra and Rq of the structured areas are not increased compared to an etching process with pure KOH (Example 6).

[0094] Table 1 shows that with etching solutions containing both sodium hydroxide and potassium hydroxide, the total alkali metal hydroxide content can be reduced without significantly affecting the etching rate. For example, Example 2 has an alkali metal hydroxide content of only 25 wt%, yet exhibits a higher etching rate than a pure potassium hydroxide etching solution with 30 wt% alkali metal hydroxides. Example 2 thus demonstrates that, with the disclosed process, the alkali metal hydroxide content can be significantly reduced by adding sodium hydroxide to the potassium hydroxide etching solution without adversely affecting the etching rate. This is advantageous from a process engineering perspective for several reasons. Firstly, the use of a more dilute etching solution leads to less corrosion of the corresponding equipment, thereby extending its service life.The lower concentration of alkali hydroxides also leads to an increase in the solubility of the dissolved glass components, especially the silicates. Furthermore, the etching solution has a lower viscosity, which has a beneficial effect on process control.

[0095] Table 1 also clearly shows that adding sodium hydroxide to the potassium hydroxide etching solution increases the etching rate, but the increase in the etching rate is not linear with the sodium hydroxide concentration in the etching solution. The relationship between the sodium hydroxide content of the etching solution and the etching rate is shown in Fig. 4.

[0096] Figure 4 clearly shows that the etching rate is not linearly correlated with the sodium hydroxide content in the etching medium. Rather, the etching rate initially increases sharply and then asymptotically approaches a limiting value, which corresponds to the etching rate in a pure sodium hydroxide etching medium. Figure 4 illustrates this relationship for Examples 1 to 6 listed in Table 1. Surprisingly, even etching media in which the potassium hydroxide content significantly exceeds the sodium hydroxide content exhibit high etching rates.

[0097] Figure 5 shows the relationship between the roughness Ra and Rq of the structured areas and the sodium hydroxide content in the etching medium. It is evident that even with high proportions of NaOH in the total alkali hydroxide concentration of the etching medium, roughness values ​​can be achieved that are essentially comparable to those obtained from etching processes using pure KOH as the etching medium. For example, even the etched areas of Example 5, with a ratio p = m(NaOH) / (m(NaOH)+m(KOH)) of 0.8, exhibit a roughness Ra of only 0.33 nm and a roughness Rq of only 0.42 nm. In contrast, the roughness Rq in comparative example 7, where the etching medium contains only NaOH and thus has a proportion of NaOH in the etching medium p of 1, is 0.77 nm. The surfaces etched with NaOH as the sole alkali hydroxide therefore exhibit significantly higher roughness than surfaces etched with the disclosed etching solutions containing both KaOH and NaOH.

[0098] Adding NaOH to a KOH-containing etching medium increases the etch rate without significantly increasing the roughness in the structured areas. Surprisingly, this is true even when the NaOH content in the etching medium is higher than the KOH content. Thus, even with etching media containing a ratio of p = m(NaOH) / (m(NaOH)+m(KOH)) of 0.8, roughness values ​​in the structured areas can be achieved that are essentially indistinguishable from those achieved with pure KOH etching media.

[0099] Fig. 6 schematically shows a plate-shaped glass element 1 with a first surface 2 and a second surface 3 arranged opposite the first, according to a further embodiment. The glass of the glass element 1 has the same composition as the glass of the first embodiment.

[0100] In the embodiment shown in Fig. 6, the glass element also has a plurality of defects 4, which are formed as filament-shaped channels. The channels run transversely to the first and second surfaces 2, 3 of the glass element 1 in their longitudinal direction and penetrate both surfaces 2, 3. The channels 4 are arranged side by side on the glass element 1 such that a plurality of channels 4 forms a perforation, and this perforation, or rather this plurality of channels, forms the outline of a structure 40. In the illustrated embodiment, the channels 4 in the glass element 1 were generated using an ultrashort pulse laser. Thus, in the embodiment shown in Fig. 6, the glass element was structured by a laser structuring process prior to the etching process.

[0101] Fig. 7 schematically illustrates the step of the disclosed etching process in which the glass element 1 is brought into contact with the etching medium 7. The glass element 1 is detachably arranged on supports 5. The glass element 1 can either simply rest on the supports 5 or be fixed to them. The glass element 1 is held in the etching medium 7 by means of the supports 5 and, in particular, immersed in it. The etching medium 7 is arranged in the etching bath 6. The etching bath 6 can, for example, be a stainless steel tank. The etching medium 7 has the same composition as in the first embodiment. By exposing the glass element 1 to the etching medium 7, material is removed from the glass element 1, resulting in a material removal rate 70. The rate at which the material is removed can be specified by the etching rate, also referred to as the removal rate. In the illustrated embodiment, the channels 4 are enlarged by the material removal.The glass element 1 remains in the etching medium 7 for a period of time t until the desired material removal is achieved and the structured glass element 10 is obtained. After the etching time t, the structured glass element 10 is removed from the etching bath 6 and, if necessary, cleaned. In the illustrated embodiment, the etching time t is in the range of 5 to 6 hours. This is comparable to the etching time of etching processes using an etching medium with sodium hydroxide as the sole base.

[0102] Fig. 8 schematically shows the etching process from Fig. 7 at an advanced stage. In the areas of the glass element 1 that are not shielded by the retaining elements 5, material has been removed. This mainly affects the channels 4, but can also affect certain areas of the first 2 and / or second 3 surface. Preferably, the channel walls of several channels 4 were removed to such an extent that several channels 4 were merged, thereby creating a recess 41 as a structure.

[0103] Fig. 9 schematically shows the etched glass article 10 obtained in this way. The etching process also gave the glass article 1 a structure. The etched glass article 10 now has a recess 41, which was created by the etching process.

[0104] Although the present invention has been described with reference to preferred embodiments, it is not limited to these and can be modified in many ways. Reference numerals

[0105] 1 glass element

[0106] 2, 3 side surfaces of the glass element 1

[0107] 4 channels

[0108] 5 Holding device

[0109] 6 Etching bath

[0110] 7 Etching medium

[0111] 10 etched glass elements

[0112] 20, 30 etched side surfaces of the etched glass element 10 40 arrangement of the channels 4

[0113] 41 Exclusion

[0114] 42 Wall of the recess 41

[0115] 70 removal

Claims

Patent claims 1. Method for producing a glass element that is at least partially etched (10) comprising at least the following steps: Providing a glass element (1) Providing an aqueous, basic etching medium (7), The etching medium (7) is applied to the areas of the glass element (1) to be etched for a period of time t. Removing the etching medium (7) from the etched glass element (10), wherein the provided aqueous etching medium (7) contains sodium hydroxide and potassium hydroxide with a total content of sodium hydroxide and potassium hydroxide in the range of 15 to 52 wt% and for the weight fraction of sodium hydroxide in the etching medium p: 0 < p < 1, with p = m(NaOH) / (m(NaOH)+m(KOH)).

2. Method according to the preceding claim, wherein the etching medium (7) has a temperature in the range of 80 to 135°C, preferably in the range of 90 to 100°C.

3. Method according to one of the preceding claims, wherein the total content of sodium hydroxide and potassium hydroxide in the etching medium (7) is in the range of 15 to 25 wt.%, preferably in the range of 15 to 20 wt.%.

4. Method according to one of the preceding claims, wherein the sodium hydroxide content in the etching medium (7) is 3 to 15 wt.%, preferably 3 to 12 wt.% and particularly preferably 3 to 9 wt.%.

5. Method according to one of the preceding claims, wherein the potassium hydroxide content in the etching medium (7) is 12 to 30 wt.%, preferably 15 to 25 wt.% and particularly preferably 20 to 25 wt.%.

6. Method according to one of the preceding claims, wherein the etching medium (7) contains at least 60 wt.% water, preferably at least 70 wt.%, particularly preferably at least 80 wt.% water.

7. Method according to one of the preceding claims, wherein p is: 0.01 < p < 0.99, preferably 0.05 < p < 0.

95.

8. Method according to any one of the preceding claims, wherein p is: 0.01 < p < 0.50, preferred 0.05 < p < 0.50, more preferred 0.1 < p < 0.5 and most preferred 0.15 < p < 0.

30.

9. Method according to any one of the preceding claims 1 to 7, wherein p is: 0.5 < p < 0.99, preferably 0.5 < p < 0.9, or more preferably 0.7 < p < 0.9 and most preferred 0.7 < p < 0.

85.

10. Method according to one of the preceding claims, wherein the glass element (1) is etched in the areas which are brought into contact with the etching medium (7) at an etching rate of at least 2 pm / h, preferably at least 3 pm / h, particularly preferably at least 4 pm / h and / or the etching rate is in the range of 2 to 7 pm / h, preferably 2.5 to 7 pm / h.

11. Etched glass element (10) comprising a surface (2, 3) that is at least partially etched, produced by a method according to one of the preceding claims, wherein the etched glass element (10) has a roughness Ra < 0.5 nm and / or a roughness Rq < 0.6 nm in the etched areas (41).

12. Etched glass element (10) according to the preceding claim, wherein the etched glass element (10) has a roughness Ra < 0.4 nm, preferably in the range of 0.05 to 0.4 nm and / or a roughness Rq < 0.5 nm, preferably in the range of 0.05 to 0.5 nm in the etched areas (41).

13. Etched glass element (10) according to one of the two preceding claims, wherein the glass of the glass element (10) has the following composition in mol-%: SiO275 - 85 B2O3 9 - 12 AI2O3 0.5 - 3 Na2O 2 - 5 K2O 0.1 - 114. Etched glass element (10) according to claim 12 or 13, wherein the glass of the glass element (10) has the following composition in mol-%: SiO265 - 75 B2O3 5 - 10 AI2O3 1 - 4 Na2O 3 - 8 K2O 2 - 6 ZnO 2 - 6