Method and device for producing an inorganic non-metal material in a melting process
A conical melting unit with screw-connected cooling fingers addresses the challenges of producing inorganic non-metallic materials with high thermal expansion, ensuring continuous and reversible processing while preventing corrosion and leakage, enhancing the production efficiency of these materials.
Patent Information
- Application Number
- PCT/EP2026/062873
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-05
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods and devices for producing inorganic non-metallic materials, particularly those with high thermal expansion and low viscosity, face challenges such as corrosion, leakage, and inability to handle continuous and reversible processes due to their aggressive nature and narrow processing ranges.
A melting unit with a conical design featuring a cooled wall, a base, and a rim area, allowing for the continuous production of inorganic non-metallic materials with high thermal expansion by controlling thermal expansion forces and preventing leakage through a conical shape and screw-connected cooling fingers, ensuring uniform heating and cooling.
Enables the continuous and reversible production of inorganic non-metallic materials with high thermal expansion, minimizing corrosion and leakage, and facilitating efficient handling of highly corrosive and low-viscosity melts.
Smart Images

Figure EP2026062873_12112026_PF_FP_ABST
Abstract
Description
[0001] SCHOTT AG 1
[0002] P06194 WO
[0003] Method and apparatus for producing an inorganic non-metallic material in a melting process
[0004] Description
[0005] Field of invention
[0006] The present invention relates generally to a method and an apparatus for producing an inorganic non-metallic material in a melting process. In particular, the present invention relates to a method and an apparatus for producing an inorganic non-metallic material in a melting process, each of which makes it possible to obtain materials from aggressive and / or low-viscosity melts and / or from melts with a very narrow processing range, yielding a solid with a predetermined shape. The method and apparatus each offer the possibility of obtaining the corresponding inorganic non-metallic material not only in a continuous process but also in a reversibly startable and interruptible process.This allows, for example, the melting of inorganic non-metallic materials which not only form aggressive and / or particularly low-viscosity melts, as mentioned above, but also, in particular, materials which have a high linear coefficient of thermal expansion.
[0007] Background of the invention
[0008] As the energy transition progresses and the associated increase in the use of electricity grows, so does the general demand for electrical energy storage. Such innovative energy storage systems require novel materials that, for example, allow for the safe storage of electrical energy and enable rapid charging and discharging. At the same time, charging losses should be minimized, and the storage system should also exhibit low self-discharge. SCHOTT AG 2
[0009] P06194 WO
[0010] Particularly interesting energy storage devices include lithium-ion batteries or lithium-ion accumulators, which are rechargeable electrical energy storage systems based on lithium ions as cationic charge carriers. The advantages of such lithium-ion batteries lie in the low mass of lithium ions and the associated potential high energy density of the storage device. However, a disadvantage is that the high reactivity of metallic (elemental) lithium poses particular challenges for the materials used in such batteries. For example, aqueous electrolytes are not possible in a lithium battery.
[0011] Therefore, there is a general need for materials, especially inorganic non-metallic materials, which can be used in a lithium-ion battery and / or in other storage devices for electrical energy.
[0012] For example, crystalline or semi-crystalline inorganic non-metallic materials with a garnet-like structure are known, such as lithium lanthanum zirconate (also known as lithium lanthanum zirconate oxide, abbreviated LLZO). These exhibit relatively high ionic conductivity even in the solid state and are therefore very attractive as solid-state electrolytes for solid-state ion batteries. Also of interest are lithium-containing crystalline materials with a so-called NASICON structure (NASICON stands for "sodium superion conductor," for example, lithium aluminum titanium phosphate, abbreviated LATP) or lithium nickel manganese cobalt oxide (Li-NMC), which can be used, for example, as cathode materials in lithium-ion batteries. Other materials used in the aforementioned energy storage devices, for example, as electrode materials, including lithium, may also be of interest for the subject matter disclosed herein.
[0013] Such inorganic non-metallic materials are generally very difficult to produce via a melting route (or synonymously a melting process). However, this approach offers the advantage that the shape of the solid can be determined from the inorganic non-metallic material to be melted, which, within the scope of this disclosure, includes the microstructure of the solid, i.e., for example, its SCHOTT AG 3
[0014] P06194 WO
[0015] The phase content can be reproducibly and precisely adjusted. Lithium-containing melts, such as those necessary in the melting process of an LLZO material, but also generally inorganic non-metallic materials used in energy storage devices, should ideally be free of metallic particles or impurities, especially if they are intended for use as solid-state ion conductors. Other impurities from common crucible materials are also undesirable. However, particularly attractive materials for use in electrical energy storage devices, such as the aforementioned LLZO, are highly corrosive to metallic crucible materials like platinum or platinum-containing alloys, or other crucible materials such as SiH₂.
[0016] One way to produce inorganic non-metallic materials that are not readily accessible to conventional melting processes for various reasons is, for example, melting in a so-called "skull" or "skull crucible." Such skull crucibles are described, for example, in US 2006 / 291528 A1, US 6817212 B1, US 2005 / 005646 A1, JP 2016 / 051701 A, US 2005 / 083989 A1, and DE 10202449 A1. These patents relate to corresponding melting units or describe processes for producing glasses and / or glass-ceramics in such melting units.
[0017] The skull process involves a melting unit, in this case the "skull" or "skull crucible," with cooled walls, and the melt is heated by coupling in high-frequency energy. In the context of glass and / or glass-ceramic production, high frequency is typically understood to be a frequency range of 10 kHz to 1 MHz, particularly 10 kHz to 100 kHz.
[0018] Such a method is also known in principle for so-called “LLZO” materials, for example for the material described in US 2016 / 329598 A1.
[0019] However, the aforementioned documents either concern melting units in which glass or glass-ceramics are melted, or they do involve the melting of an inorganic, non-metallic material such as LLZO, but then in a batch process. SCHOTT AG 4
[0020] P06194 WO
[0021] There is therefore a need for a device that enables the continuous melting of materials with a high tendency to crystallize, which are inaccessible to conventional melting processes due to the specific characteristics of the inorganic non-metallic melt (for example, because the melt is highly corrosive and / or has a very low melt viscosity). In particular, there is a need for a device that allows the melting of inorganic non-metallic materials with a high linear coefficient of thermal expansion a of at least 10 K'. 1 exhibit, can be melted, in particular in a continuous and preferably reversible stopable and startable process.
[0022]
[0023] The object of the invention is to at least partially eliminate the described disadvantages in the prior art and to provide a device and a method for melting inorganic non-metallic materials that enable improved handling of highly corrosive melts and / or melts with high coefficients of thermal expansion compared to known devices and methods.
[0024]
[0025] the
[0026] The problem is solved by the subject matter of the independent claims. Preferred and specific embodiments are found in the dependent claims, the description, and the drawings of the disclosure.
[0027] The present disclosure thus relates generally to a device for producing an inorganic non-metallic material in a melting process, obtaining a solidified melt and / or a solid with a predetermined shape, wherein the solidified melt or the solid has a substantially linear coefficient of thermal expansion a of at least 10 7 K 1 exhibits, comprehensive
[0028] - a melting unit with a cooled wall, a base and a rim area, - a device for supplying a mixture, SCHOTT AG 5
[0029] P06194 WO
[0030] - a device for heating the mixture to obtain a liquid or viscous melt and / or for heating the melt, wherein the melt has a viscosity of at most 1 Pa-s,
[0031] - preferably a device for homogenizing the melt,
[0032] - a device for extracting the melt,
[0033] - preferably a device for forming a solid body with a predetermined shape, wherein a first cross-sectional area of the melting unit is smaller than a second cross-sectional area of the melting unit, and wherein the distance of the first cross-sectional area to the bottom of the melting unit is smaller than the distance of the second cross-sectional area to the bottom. In other words, the melting unit according to the invention is essentially conical in such a way that the diameter of the melting unit decreases continuously towards the bottom of the melting unit. The skull-shaped crucible, preferably designed as a cone, thus tapers towards the bottom.
[0034] Such a design offers a number of advantages, particularly in the production of inorganic non-metallic materials that end up as a solidified melt or as a solid with high thermal expansion. High thermal expansion, as defined in this disclosure, is present in particular when the solidified melt or the resulting solid has a linear coefficient of thermal expansion a of at least 10 K. 1 , preferably of at least 10 6 K 1 and in particular of at least 10- 5 K 1The coefficient of thermal expansion can be determined using the dilatometer method, whereby a rod is prepared from the material to be analyzed and the change in length is measured as a function of temperature (e.g., in the range of 20 °C to 300 °C) (standard (ISO 7991:1987-12)). Alternatively, the change in crystal cell dimensions (volume of the unit cell) as a function of temperature can also be determined using XRD.
[0035] For the purposes of this disclosure, a distinction is made between the terms "solidified" or "solidifying melt" on the one hand and "solid" on the other, unless the context indicates otherwise. Solidified melt generally refers to the hardened melt contained in the melting unit. This typically includes the so-called residual melt that remains after the melting process and / or after SCHOTT AG 6
[0036] P06194 WO
[0037] Removal of the solid from the melting unit leaves residue on the walls of the melting unit. The term "solid," however, refers to solidified melt that has a predetermined and generally crystalline form—in a preferred embodiment, the solid is present as a powdery and / or platelet-shaped bulk material. Unless otherwise indicated by the context or specified in more detail, the term "melt" in this disclosure refers to a viscous, (yet) unsolidified melt.
[0038] Within the scope of the present disclosure, it is further understood that viscous melt, solidified melt, and solid "correspond to one another" insofar as they are in equilibrium with each other. It is possible that the viscous melt, solidified melt, and solid may have the same composition; however, this is not necessarily the case, as the system under consideration may also tend to form eutectics and / or mixed crystals, so that, for example, the melt and the corresponding solid (e.g., on the cooled wall of a melting unit according to one embodiment) may have different compositions.
[0039] The device described here for heating the mixture to obtain a melt or for heating the melt should preferably be designed for melts with a viscosity in the range of 0.001 to 1 Pa-s to 0.6 Pa-s, preferably for melts with a viscosity in the range of 0.01 Pa-s to 0.5 Pa-s and particularly preferably for melts with a viscosity in the range of 0.02 Pa-s to 0.3 Pa-s.
[0040] The melt can also be determined by its processing range, whereby the processing range of the melt preferably has a starting viscosity of < 10 4dPa s and a cooling rate Ki, which is between 3.3 K / s and 7,500 K / s, preferably between 500 K / s and 1,500 K / s. In the case of a rotating roller arranged under the melting unit, a cooling rate of 3.3 K / s would, for example, mean a cooling from 1,351 °C to 1,350 °C at 150 rpm of the continuously rotating roller and 75% "wrap-around". Similarly, a cooling rate of 7,500 K / s would, for example, mean a cooling from 1,600 °C to 1,350 °C at 450 rpm and 25% "wrap-around". The "wrap-around" describes what proportion of the circumference of the roller is covered with molten material. A wrap-around of 75% therefore means that the SCHOTT AG 7
[0041] P06194 WO
[0042] The material would have to be in contact with the roller over more than 270° of the roller circumference in order to achieve the stated cooling rate.
[0043] Known devices for producing inorganic non-metallic materials in a melting process using a melting unit with cooled walls (or a cooled shell) typically feature cylindrical geometries with a flat base and walls arranged perpendicular to this base. In other words, the melting unit has the basic shape of a cylinder, more precisely a right cylinder, meaning the base and the outer surface are parallel to each other. Generally, the base of this "cylinder" is round, but of course, the geometry of the base can also be elliptical or polygonal. This also generally includes a design as a right prism with an arbitrarily polygonal base.
[0044] Within the scope of this disclosure, the terms "wall" and "walls" of the melting unit are used synonymously. Geometrically speaking, the wall or walls can be described as the shell of the cylinder or prism, or, in the case of the melting unit, according to embodiments of a truncated cone or a truncated pyramid.
[0045] This cylindrical (or, as described above, also prismatic) basic shape of the melting unit with a cooled wall is, however, unsuitable for use in the melting processes described here, especially if the solid has a high thermal expansion (i.e., in particular a linear coefficient of thermal expansion a of at least 10 K). 1In this case, for example, it is not possible to interrupt the process, i.e., to cool the melt while it solidifies and then remelt it at a later time. When reheating cooled melt, its expansion during heating causes very high forces to act on the vertical walls. These forces can be so strong that the vertical walls of well-known so-called skull crucibles are pushed outwards, causing the crucible to leak or even be destroyed. SCHOTT AG 8
[0046] P06194 WO
[0047] This difficulty has been solved in the device according to the present disclosure in a surprisingly simple and elegant way by designing the melting unit with cooled walls such that its cross-sectional area varies along its height. In other words, the melting unit can be described, in simplified terms, as a truncated cone or truncated pyramid, with the base having a smaller area than the outer region, i.e., the upwardly open area of the melting unit or crucible into which the mixture can be added. The melting unit thus opens upwards. Consequently, the expanding material can also expand upwards, reducing the forces acting due to thermal expansion during remelting. As a result, the melting unit remains sealed even after remelting.
[0048] In this way it is possible to produce an inorganic non-metallic material while obtaining a solidified melt or a solid with high thermal expansion, in particular with a linear coefficient of thermal expansion a of at least 10 K. 1 , to melt continuously, which includes in particular the possibility of switching the device or the process carried out with the device on and off to heat the mixture / melt.
[0049] The materials for which the melting unit is primarily designed are generally those exhibiting a particularly strong tendency to crystallize, preferably forming crystals with a garnet structure (in the case of LLZO) or a NaSiCon structure (LATP). However, the decisive factor for categorizing the materials in question is primarily the thermal expansion of their respective solid state.
[0050] According to one embodiment, the cross-sectional area of the melting unit increases continuously in the direction of the second cross-sectional area Q2, at least between the first cross-sectional area Qi and the second cross-sectional area Q2. In other words, according to this embodiment, the cross-sectional area does not increase in steps, but rather continuously. In this case, the melting unit can also be geometrically described, at least between the first and second cross-sectional areas, by the geometric shape of a truncated pyramid or a truncated cone. SCHOTT AG 9
[0051] P06194 WO
[0052] Such an embodiment is particularly advantageous for embodiments of a method for producing an inorganic non-metallic material in a melting process, obtaining a solid with a preferably predetermined shape, wherein the solid has a linear coefficient of thermal expansion a of at least 10 K 1 This is advantageous because, in this case, if the melting process is stopped, at least part of the solid remains within the melting unit itself due to the solidification of the melt, restarting the melting unit is easily possible. In this case, the melt can expand as the melting unit is reheated and move along the wall in the larger cross-sectional area.
[0053] In a further embodiment, the melting unit can be provided with a wall opening angle of at least 2° and at most 30°. With a relatively small opening angle of only 2°, the difference in the size of the first and second cross-sectional areas is rather small; however, this can already be sufficient to heat the solid body in the melting unit with high thermal expansion without causing mechanical failure such as breakage and / or leakage of the melting unit. In this case, the opening angle is so small that the manufacture of the melting unit is still very simple. Depending on the material's specific characteristics, however, it can also be advantageous to have larger opening angles; for design reasons, the opening angle should preferably not exceed 30°.
[0054] In one embodiment, the base and wall are connected by a mechanical and / or force-fit connection. This is particularly advantageous for melts with very low viscosity. In this way, materials with such low viscosity can also be melted in the melting unit according to this embodiment. For known melting units with a cooled wall, in which primarily melts with higher viscosity are processed, this is not strictly necessary, since the highly viscous material cannot flow through gaps in the wall and / or between the base and the wall. SCHOTT AG 10
[0055] P06194 WO
[0056] However, for the materials with a high tendency to crystallize that are primarily addressed here, the situation is different, as these usually have a low viscosity and melt can therefore escape even through small cracks.
[0057] According to a further embodiment of the device, the wall comprises cooling fingers which are arranged one another in a direction perpendicular to the bottom of the melting unit and which are connected to each other by means of a screw connection, preferably in such a way that the cooling fingers are fixed to the bottom of the melting unit by means of a screw connection.
[0058] This design is highly advantageous, especially compared to previously known "skull" concepts. Conventional melting units with a cooled wall rely on components being joined by soldering and / or welding. However, these joining technologies have the disadvantage of making maintenance and / or repair of the melting unit very complex. When individual parts need cleaning or replacement, the corresponding joints must be opened while hot. Reassembling with a replacement part then requires the same hot joining process again, involving welding and / or soldering. This procedure is not only complex; the melting unit material can also be permanently damaged with each of these hot steps, thus reducing the unit's service life.
[0059] This is addressed here by the fact that the melting unit generally comprises components, but in particular the wall, cooling fingers, which are fixed against each other. Specifically, as described above, the cooling fingers of the wall can be fixed to the base of the melting unit by means of a screw connection. According to a further embodiment, the cooling fingers and the base can be connected to each other by a sealing plug connection. In this way, not only is the escape of a low-viscosity melt through gaps between the cooling fingers and / or between the wall and the base largely prevented, but the maintenance of the melting unit is also improved. SCHOTT AG 11
[0060] P06194 WO
[0061] It can also be provided that the cooling fingers are arranged at an angle between 1° and 89° to the base of the melting unit, with the cooling fingers preferably being arranged at an angle between 45° and 89° and particularly preferably at an angle between 60° and 87° to the base of the melting unit. Due to the essentially conical shape of the melting unit, a perpendicular arrangement (i.e., 90° to the base) is just as unsuitable as a parallel arrangement to the base (i.e., 0° or 180° to the base).
[0062] In particular, it can also be provided that the cooling elements of the cooling fingers and the base are interconnected. This ensures uniform cooling of the melting unit, thus preventing so-called "hot spots".
[0063] In a further embodiment, the cooling fingers and the base are electrically connected. This is also very advantageous for uniform heating of the melt. The electrically conductive connection also ensures that the electrical potentials generated by the electromagnetic field, which is necessary for the inductive heating of the material, remain as low as possible at the individual adjacent cooling fingers, since otherwise electrical arcing can occur in the melt. This, in turn, can lead to damage to the cooling fingers.
[0064] In a further embodiment, the cooling fingers are arranged in the wall of the melting unit at a lateral distance of at least 0.1 mm and at most 3 mm from each other, so that gaps and / or joints are formed between the cooling fingers. In this way, escape of the low-viscosity melt can be easily prevented. The cooling fingers can be manufactured, in particular, using an additive manufacturing process.
[0065] According to a further embodiment, at least one cooling finger can have a surface designed to fit together with a surface of at least one adjacent cooling finger, resulting in a positive-locking connection. Furthermore, the cooling fingers can each have a constant wall thickness. It can also be provided that at least one cooling finger has a curved, preferably convex, surface on an inner side of its wall. SCHOTT AG 12
[0066] P06194 WO
[0067] The cooling fingers can also be electrically connected to each other, and can have a coating, at least in some areas, which is preferably electrically insulating.
[0068] The wall and cooling finger designs described here improve the manufacturability of the melting unit and result in more uniform heating of its contents. Most importantly, they lead to safer and more durable operation of the crucible.
[0069] The aforementioned design of the device and the corresponding melting unit are therefore highly advantageous. This applies firstly to the longevity of the crucible, and secondly to the other challenges encountered when melting the solids addressed here, for example, those with high thermal expansion and / or a high tendency to crystallize. As already discussed in detail above, melts that tend to form a glass typically exhibit high viscosity. In melting units composed of different segments, it must be ensured that the melt, which often has a honey-like viscosity, cannot escape from the joints between individual segments of a melting unit.In a melting unit with a cooled wall, it must also be ensured that the width of any gaps between segments, such as cooling fingers, prevents the melt from escaping. However, conventional measures for melts with high viscosity and the described honey-like viscosity fail with melts of low viscosity, especially those with a strong tendency to crystallize. These often have an almost water-like, very low viscosity, where, unlike typical "glass melts," the viscosity is also only slightly dependent on the temperature of the melt. Furthermore, melts with high density can exert a very high hydrostatic pressure on the walls of a melting unit.
[0070] Difficulties arise when using a melting unit with a cooled wall, i.e., a so-called "skull," but especially because, as explained above, the heating is done using high frequency. This means that the electromagnetic fields... SCHOTT AG 13
[0071] P06194 WO
[0072] Since it can be coupled into the melt, a completely sealed metal construction cannot be used.
[0073] Another difficulty lies in the fact that, when using cooling fingers, the coupling of electromagnetic high-frequency fields can cause potentials to build up, which can result in arc discharges between the cooling fingers. Such voltage discharges damage the metal and can consequently lead to leaks at the cooling fingers. Advantageously, therefore, the melting unit or the wall of the melting unit comprises at least one dielectric material, which is preferably arranged at least partially in a gap and / or joint. Such a dielectric material can then be used to create a seal between the cooling fingers.
[0074] Alternatively or additionally, according to one embodiment, at least one cooling finger may have at least one surface, preferably a flat surface, which is designed to fit together with a flat surface of at least one adjacent cooling finger, resulting in a positive-locking connection. In this way, a sufficiently reliable seal of the gaps or joints between the individual segments / cooling fingers can be achieved even without the use of a dielectric material arranged in a gap.
[0075] The use of dielectric material can be disadvantageous if very high temperatures occur during the melting process. Although the dielectric material itself is also cooled by the cooling fingers, it may still leach components of the dielectric material and contaminate the melt. However, this risk is at least somewhat mitigated in this case because, according to one embodiment of the melting unit or device, the cooling system or cooling circuit is optimized.
[0076] Alternatively or additionally, according to one embodiment, at least one cooling finger, preferably several, and in particular all, may have a curved, preferably convex, surface on an inner side of the wall. This rounding of the cooling finger, ideally of all cooling fingers, helps to reduce field protrusions at edges. SCHOTT AG 14
[0077] P06194 WO
[0078] to avoid or at least reduce their formation and thus reduce the risk of arcing.
[0079] Alternatively or additionally, according to one embodiment, it can also be provided that at least one cooling finger has at least one coating in at least one area, wherein the coating is preferably electrically insulating.
[0080] Such a coating, preferably with a dielectric, electrically insulating material, can be advantageous in reducing the risk of arcing. For example, this coating can also be applied as a hard anodizing of the cooling finger. In particular, all cooling fingers can have such a coating.
[0081] According to another embodiment of the device, the wall and / or bottom of the melting unit comprise a material which includes the following:
[0082] - a thermal conductivity Ao at 20 °C of at least 15 W / (m-K), preferably at least 20 W / (mK), particularly preferably at least 70 W / (mK), in particular at least 145 W / (mK) and / or in the range of 15 W / (mK) to 450 W / (mK), and / or
[0083] - an electrical conductivity of at least 0.5 × 10 6 and at most 65 ■ 10 6 S / m, preferably of at least 1.3 ■ 10 6 and at most 60 ■ 10 6 S / m.
[0084] When selecting a material for the melting unit, attention must be paid to stability and the guarantee of critical emergency running properties; thermal conductivity and / or electrical conductivity are also critical components. The special design of the melting unit in embodiments with a conical structure also means that the material used must be suitable for corresponding manufacturing, preferably, for example, by 3D printing or an additive manufacturing process. The thermal conductivity Ao refers to the thermal conductivity at 0°C. Suitable materials include, for example, silver and stainless steel, with silver exhibiting high thermal conductivity and stainless steel having a thermal conductivity closer to the lower end of the range. SCHOTT AG 15
[0085] P06194 WO
[0086] It is possible that, according to a specific embodiment, the wall and base of the melting unit comprise different materials or are made of different materials. Of course, it is also possible for the wall and base to be made of the same material.
[0087] According to one embodiment, the material encompassing the wall and / or base of the melting unit may be aluminum, a steel, preferably stainless steel, aluminum nitride, copper, boron nitride, silver, and / or mixtures thereof. These materials exhibit high thermal conductivity, characterized as Ao as defined above within the corresponding limits, as well as high stability.
[0088] Furthermore, aluminium nitride has no electrical conductivity.
[0089] The precise geometric design of the melting unit is also important to ensure efficient energy input while maintaining low overall energy consumption, which is largely determined by the ratio of the melt's surface area to its volume. The flow conditions within the melt are also significant. Further practical aspects concern the loading and melting of the batch and the method of extracting the melt from the unit. Therefore, according to one embodiment, the melting unit preferably has a mean lateral dimension, for example, a mean diameter, in a direction perpendicular to the base, and a height defined as the distance from the base to the edge region, wherein the ratio of the mean lateral dimension perpendicular to the base to the height is between 1.5:1 and 0.8:1. A ratio of mean lateral dimension (for example, the diameter) to height of 1:1 is particularly preferred.The mean lateral dimension can be determined, regardless of the exact geometric design, as four times the mean cross-sectional area divided by its perimeter. The mean cross-sectional area is the arithmetic mean of the smallest and largest cross-sectional areas of the melting unit. These cross-sectional areas are generally determined parallel to the base of the melting unit. Typically, the base of the melting unit will have the smallest cross-sectional area, and its edge region the largest. SCHOTT AG 16.
[0090] P06194 WO
[0091] The present disclosure also relates generally to a process for producing an inorganic non-metallic material in a melting process, obtaining a solidified melt and / or a solid with a predetermined shape, wherein the solidified melt or solid has a substantially linear coefficient of thermal expansion a of at least 10 K 1 exhibit, encompassing the following steps:
[0092] - Providing a device for producing an inorganic non-metallic material in a melting process to obtain a solid with a preferably predetermined shape, in particular a device according to an embodiment of the disclosure,
[0093] - Providing a mixture,
[0094] - Heating the mixture to obtain a melt and / or heating the melt, wherein the melt has a viscosity of at most 1 Pa-s,
[0095] - Extracting at least part of the melt.
[0096] - The process is also characterized by the fact that the heating of the viscous melt and / or the melt solidified in the melting unit can be started and stopped reversibly.
[0097] The process may also include the following steps:
[0098] - Homogenizing the melt, whereby this step is carried out in particular before the step "removing at least part of the melt", and
[0099] - Forming a solid with a predetermined shape from the melt, wherein this step in particular follows directly after the removal of at least a part of the melt.
[0100] The solid produced using the method disclosed herein has a linear coefficient of thermal expansion a of at least 10 7 K 1 on.
[0101] The disclosed process is particularly suitable for heating a melt having a viscosity of less than 0.5 Pa·s, preferably a viscosity in the range of 0.07 to 1 mPa·s, and which in particular has a processing range comprising a processing temperature of at least 1,000 °C, preferably at least 1,300 °C, and most preferably 1,600 °C. The process may also include the following steps: SCHOTT AG 17
[0102] P06194 WO
[0103] - Forming a solid with a predetermined shape from the melt, wherein the production, in particular the heating of the mixture and / or the melt, is reversibly startable and stoppable, wherein after homogenization of the melt, the melt is cooled in a melting unit with a cooled wall such that the solidified melt or at least part of the solid is present in the melting unit, and wherein the melting unit with a cooled wall is designed such that a first cross-sectional area Qi of the melting unit is smaller than a second cross-sectional area Q2 of the melting unit, and a distance a1 of the first cross-sectional area to the bottom of the melting unit is smaller than a distance a2 of the second cross-sectional area Q2 to the bottom.
[0104] In a possible step of the process, in which the solid or solidified melt within the melting unit is reheated or melted, preferably in the form of the solid being melted in the melting unit, the solid or solidified melt can expand when heated and, due to the conical shape of the melting unit, move along the wall in the direction of the above edge region.
[0105]
[0106] the
[0107] The invention will be further explained below with the aid of figures. These show
[0108] Fig. 1 shows a schematic and not to scale device for producing an inorganic non-metallic material in a melting process, obtaining a solid with a preferably predetermined shape according to one embodiment, and
[0109] Fig. 2 is a schematic and not to scale representation of the melting unit of the device according to one embodiment.
[0110] Fig. 1 shows a schematic representation of a device 100 for producing an inorganic non-metallic material in a melting process while maintaining the SCHOTT AG 18
[0111] P06194 WO
[0112] solid 9, wherein the solid 9 preferably has a linear coefficient of thermal expansion a of at least 10 K 1The device 100 is one that enables the execution of a process for producing an inorganic non-metallic material in a melting process according to the embodiments described above. The device 100 comprises a melting unit 1 with a cooled wall (not specified herein), a bottom (also not specified herein), and a rim region (also not specified herein), a device 2 for providing a mixture 3, and a device 4 for heating the mixture 3 to obtain the melt 5 or for heating the melt 5. The melt 5 has a processing range that includes a processing temperature of at least 1,000 °C, preferably at least 1,300 °C, and particularly preferably 1,600 °C. The device 100 further comprises a device 6 for homogenizing the melt 5 and a device 7 for removing it.
[0113] The device 100 is generally, without limitation to a specific embodiment of the method and / or the device, constructed as a so-called "skull" or "sculp crucible". This generally means that the melting unit 1 comprises a cooled wall or walls, which are formed, for example, from cooled metal tubes.
[0114] In general, the device 100 also includes a device 4 for heating the mixture 3 to obtain a melt 5 or for heating the melt 5. In such a device 100, as described here in general terms, the heating of the crucible contents, i.e., mixture 3 and / or melt 5, is known to be carried out by high-frequency energy coupled into the crucible contents. For this to occur, the crucible contents should have a certain conductivity. This is the case, for example, with some glass melts or with melts that generally contain ions. However, this is usually not the case for the mixture 3, which is present in solid form as bulk material. For the sake of simplicity, the term "crucible" here refers to the melting unit 1 with a cooled wall.
[0115] To start the melting process, it may therefore be provided that no high-frequency energy is initially coupled into the crucible contents, but rather, for example, that the mixture 3 is heated by means of thermal energy so that it at least partially melts, SCHOTT AG 19
[0116] P06194 WO
[0117] so that the partially melted mixture becomes conductive enough to allow high-frequency energy to be coupled into the crucible contents. The supply of, for example, thermal energy can then be stopped, and the subsequent heating of the crucible contents is carried out solely by high-frequency energy. In this way, both the melt 5 and the mixture 3, which is continuously fed into the melting unit 1 (i.e., the crucible), can be heated.
[0118] The embodiment of the device 100 shown in Fig. 1 also includes a device 8 for forming the solid body 9 with a predetermined shape.
[0119] The device 2 for supplying the mixture 3 is shown in Fig. 1 as comprising, for example, a hopper 21 from which the mixture 3 flows onto a trough 22, from where it can be continuously fed to the melting unit 1. In the illustration of Fig. 1, the mixture 3 falls from the trough onto the melt 5 or is placed onto it. Of course, it is also possible to first transfer the mixture 3, which is initially in solid form, from the device 2 into the melting unit 1 and only then start the melting process. Generally, the melting unit 1 can also be filled differently than shown before the melting process is started. However, for carrying out a continuous process, it is advantageous to provide a device 2 for supplying the mixture 3 that allows for the continuous feeding of the mixture 3.
[0120] The device 4 for heating the mixture 3 to obtain a melt 5 and / or for heating the melt 5 is designed here such that it includes a generator 41 for providing high-frequency energy, which can be inductively coupled into the crucible contents, i.e., melt 5 and, if applicable, mixture 3, by means of the coils 42, not all of which are shown for the sake of simplicity. As explained, the device 100 can also include a further device for heating, in particular, the mixture 3, for example, by means of thermal energy, specifically for the initiation process of the melting process. This further device is not shown here for the sake of simplicity. SCHOTT AG 20
[0121] P06194 WO
[0122] The device 100 preferably further comprises a device 6 for homogenizing the melt 5, which is shown schematically here in the form of a stirring rod immersed in the melt 5. However, other devices 6 are also conceivable. In its simplest form, this device 6 is not strictly necessary, since the introduction of high-frequency energy into the melt 5 induces an electric current, which is then homogenized by convection currents. However, it can be advantageous if the device 100 also includes a special component, for example in the form of a device 6, which facilitates efficient homogenization of the melt 5.
[0123] The device 100 further comprises a device 7 for extracting the melt 5, which here is designed in the form of a feeder. However, other designs for the device 7 for extracting the melt are generally possible. For example, this device 7 can also be designed as a body immersed in the melt 5.
[0124] The device 100 also includes a device 8 for forming the solid 9 with a predetermined shape. Generally, without limiting it to the specific embodiment of the device 100 shown in Fig. 1, the device 7 for extracting the melt 5 and / or the device 8 for forming the solid 9 with a predetermined shape are designed such that the processing area of the melt 5 is at least partially traversed, or can be traversed, with at least a cooling rate Ki, which lies between 3.3 K / s and 7,500 K / s, preferably between 500 K / s and 1,500 K / s. In this way, the solid 9 is obtained from the melt 5 and is present in a predetermined shape, the predetermined shape containing a crystalline phase fraction, preferably determined by weight.-% in a Rietveld analysis of an X-ray diffractogram, and / or a mean crystallite size of a crystal phase, preferably determined from a Rietveld analysis of an X-ray diffractogram, and / or the presence of a crystal phase, and wherein the solid 9 is preferably obtained or is obtained in the form of a powdered and / or plate-shaped bulk material 10.
[0125] The device 100 shown in Fig. 1 depicts a particularly preferred embodiment in which the device 100 has a device 7 for extracting the melt 5 in the form of a feeder, which is arranged here by way of example in the base of the melting unit 100. Furthermore, the device 100 here comprises a device 8 for forming the solid 9 with SCHOTT AG 21
[0126] P06194 WO
[0127] of predetermined shape. This device 8 is designed here such that it comprises a cool, preferably a cooled, roller 81. The roller 81 is preferably rotatable, as also shown here. This is particularly advantageous because in this way the point of impact of the melt 5 on the roller 81 can be varied very easily without, for example, having to provide a lateral movement in addition to the rotational movement, as might be the case, for example, in a device 8 comprising a cool, preferably cooled, plate in order to heat the point of impact of the melt 5 as little as possible.
[0128] If, as here, the device 100 or the device 8 is designed such that the roller 81 is rotatable or rotates, the formed solid body 9 is separated from the roller 81 by centrifugal force and can then, as schematically shown here, also be flung away from it. The solid body 9 can then, for example, be directed towards a collecting device 83 or at least collected in such a device. At the same time, this procedure, as described, has the advantage that the point of impact of the melt 5 on the roller 81 varies over time.
[0129] In this further development of the method or device 100, the rotation of the roller 81 allows for the production of highly specific shapes (i.e., shaped bodies) of the solid 9. The molten droplets that strike the roller 81 are drawn long and thin on the roller surface by the rotation. Through contact with the cool surface and heat radiation, the melt 5 cools rapidly, then solidifies into flakes and is separated from the roller surface by centrifugal force.
[0130] In general, the advantages of the method, when using a roller 81, or correspondingly the device 100 comprising a roller 81 as part of the device 8 for forming the solid 9, in particular a rotating roller 81, lie in the achievable high cooling rate and the accuracy with which the cooling rate can be adjusted. Furthermore, the method and corresponding device 100 are suitable for continuous operation and high throughputs. By selecting suitable parameters, the flake geometry of the bulk material 10, as which the formed solid 9 is obtained, can also be precisely adjusted to minimize the grinding effort. SCHOTT AG 22
[0131] P06194 WO
[0132] In a further development of the method and / or device 100, it can be advantageously provided that the roller 81 comprises a thermally conductive, mechanically robust material such as copper, stainless steel, or aluminum. According to a preferred embodiment, the surface of the roller 81 can be coated to protect the surface and prevent metal abrasion. For example, such a coating can comprise or be made of a high-temperature-resistant material. An exemplary material could be Al₂O₃, but other materials, such as Si₂ and / or ZrC or mixtures thereof, are also suitable.
[0133] In general, it can be provided that the roller 81 comprises or is made of a metallic material with a thermal conductivity of at least 15 W / (mK), in particular copper, aluminium and / or stainless steel.
[0134] In a further preferred embodiment, it can be provided that the roller 81 is cooled, in particular by water.
[0135] In general, after the melt 5 impacts the material and immediately after the solid 9 forms from it, the temperature of the solid particles preferably obtained in this way, for example in the form of flakes, can still be high enough at the moment of being ejected from the rotating roller 81 to allow for a second, slower cooling step in the processing area. This second cooling step, with a cooling rate K2 and any subsequent cooling rates, can be used to further adjust the predetermined shape of the solid 9, in particular, for example, to adjust the desired crystal phase. The cooling rate(s) can be adjusted passively via the transport conditions themselves (e.g., height of the bulk material 10 in a transport container, insulation of the subsequent transport route, etc.), or by targeted active cooling or heating (e.g., cooled vibrating trough, cooling oven, etc.).
[0136] To protect persons, such as employees and plant operators, and the plant itself, generally, without limitation to a specific embodiment of the method and / or the device 100, but especially for an embodiment with a preferably SCHOTT AG 23
[0137] P06194 WO
[0138] Suitable protective plates 82 are attached to the rotating roller 81 to prevent uncontrolled splashing of material. Ideally, the protective plates 82 are water-cooled to protect them from overheating and to prevent adhesion of sintered material. They can also, if necessary, direct the splashing solid 9 into a collection device 83 for the bulk material 10, as schematically indicated in Fig. 1.
[0139] The device 100 can generally include further devices. The hood 11, which can at least partially cover the upper area of the melting unit 1, is shown schematically here. The hood 11 can be arranged at a distance from the upper edge of the melting unit 1, as shown here, or it can close it completely in the form of a lid. In this way, excessive heat loss can be avoided.
[0140] The special, conical shape of the melting unit 1 will now be further explained with reference to Fig. 2.
[0141] The melting unit 1 with a cooled wall is designed such that a first cross-sectional area Qi of the melting unit 1 is smaller than a second cross-sectional area (Q2) of the melting unit 1, and a distance ai of the first cross-sectional area to the base 102 of the melting unit 1 is smaller than a distance a2 of the second cross-sectional area Q2 to the base 102. In particular, it can be provided that at least between the first cross-sectional area Qi and the second cross-sectional area Q2, the cross-sectional area of the melting unit 1 increases continuously in the direction between the first cross-sectional area Qi and the second cross-sectional area Q2 (i.e., in a direction from the base to the wall region).
[0142] For example, in this case it can be provided that the melting unit 1 can be described as having an opening angle of the wall 101 of at least 2° and at most 30°.
[0143] As described above, this form of melting unit with a boundary region 103 of the melting unit (or crucible) has the advantage that it enables or particularly facilitates the production of such inorganic non-metallic materials in which the solid 9 exhibits high thermal expansion. SCHOTT AG 24
[0144] P06194 WO
[0145] In this way, it is also possible to easily interrupt and restart the melting process without causing mechanical failure of the melting unit 1. In particular, it can be provided that, after an initial melting of the solid 9 from the mixture in the melting unit 1, the remaining solid 9 expands during a heating step and moves along the wall 101 in the direction of the cross-sectional area Q2, preferably melting at least partially or even completely.
[0146] Also shown in Fig. 2 is the distance h from the edge region 103 to the base 102 of the melting unit 1. In general, according to one embodiment of the device 100, the melting unit 1 can be designed such that it has a mean lateral dimension, for example a mean diameter, in a direction perpendicular to the base 102 and a height h, determined as the distance from the base 102 to the edge region 103, wherein the ratio of the mean lateral dimension perpendicular to the base 102 and the height h is between 1.5:1 and 0.8:1. The mean lateral dimension is determined as four times the mean cross-sectional area divided by its circumference, as has already been described in detail above.
[0147] In general, without limiting it to a specific embodiment of the device 100, it can be provided that the bottom 102 and wall 101 of the melting unit 1 are connected to each other by a mechanical and / or force-fit connection.
[0148] In particular, it is possible that the wall 101 comprises cooling fingers, for example in such a way that the cooling fingers form the wall 101, wherein the cooling fingers are arranged one another in a direction perpendicular to the bottom 102 of the melting unit 1, wherein they can be connected to each other by means of a screw connection, for example and preferably in such a way that the cooling fingers are fixed to the bottom 102 of the melting unit 1 by means of a screw connection.
[0149] In general, for example, it can be provided that the cooling finger and base 102 are connected to each other by a sealing plug connection. SCHOTT AG 25
[0150] P06194 WO
[0151] Preferably, the cooling elements of the cooling fingers and the base 102 can be connected to each other.
[0152] In particular, it may also be provided that the cooling fingers and the base 102 are electrically connected to each other.
[0153] In general, without being limited to a specific described and / or illustrated embodiment, the device 100 can be designed such that the wall 101 comprises cooling fingers, wherein gaps and / or joints are formed between the cooling fingers, preferably having at least one of the following features:
[0154] - The wall 101 comprises at least one dielectric material, wherein the at least one dielectric material is preferably arranged at least partially in a gap and / or a joint;
[0155] - at least one cooling finger has at least one surface, preferably a flat surface, which is designed to fit together with a flat surface of at least one adjacent cooling finger in such a way that a positive locking connection results,
[0156] - at least one cooling finger has a curved, preferably convex, surface on an inner side 101 a of the wall;
[0157] - the gaps and / or joints have a lateral dimension of the gaps and / or joints in a direction perpendicular to the bottom 102 of the melting unit 1 between 0.1 mm and 3 mm,
[0158] - At least one cooling finger has at least one coating in at least one area, the coating preferably being electrically insulating.
[0159] - at least one cooling finger has a constant wall thickness,
[0160] - the cooling fingers are electrically connected to each other.
[0161] Furthermore, in general terms, as described above, the device 100 can be designed according to one embodiment such that the wall 101 and / or the base 102 comprise a material having
[0162] - a thermal conductivity Ao at 20 °C of at least 15 W / (m-K), preferably at least 20 W / (mK), particularly preferably at least 70 W / (mK), in particular at least 145 W / (mK) and / or in the range of 15 W / (mK) to 450 W / (mK), and / or SCHOTT AG 26
[0163] P06194 WO
[0164] - an electrical conductivity of at least 0.5 × 10 6 and at most 65 ■ 10 6 S / m, preferably of at least 1.3 ■ 10 6 and at most 60 ■ 10 6 S / m.
[0165] It may preferably be provided that the device 100 or, accordingly, the melting unit encompassed by it, is designed such that it has at least one of the following features:
[0166] - Wall 101 and base 102 are made of different materials;
[0167] - The material enclosed by wall 101 and / or base 102 is aluminum, a steel, preferably stainless steel, aluminum nitride, copper, boron nitride, silver and / or mixtures thereof. SCHOTT AG 27
[0168] P06194 WO
[0169] List of reference signs
[0170] 100 Device for producing an inorganic non-metallic material in a melting process
[0171] 1 melting unit
[0172] 101 Cooled wall
[0173] 101a Inside of the wall
[0174] 102 Floor
[0175] 103 Edge area
[0176] 2 Device for providing a mixture
[0177] 3 Mixture
[0178] 4. Heating device
[0179] 41 Generator for providing high-frequency energy
[0180] 42 coils
[0181] 5 Viscose Melt
[0182] 6 Device for homogenizing the melt
[0183] 7 Device for extracting the melt 8 Device for forming a solid with a predetermined shape
[0184] 81 roller
[0185] 82 mudguards
[0186] 83 Containment device
[0187] 9 Solids
[0188] 10 bulk goods
[0189] 11 Hood
[0190] Qi, Q2 cross-sectional areas
[0191]
[0192] SCHOTT AG 28
[0193] P06194 WO
[0194] ai, a2 Distance of the respective cross-sectional area from the ground 102
[0195] h Distance from floor 102 and edge area 103
[0196]
Claims
SCHOTT AG 29 P06194 WO 1. Device (100) for producing an inorganic non-metallic material in a melting process, obtaining a solidified melt and / or a solid (9) with a predetermined shape, wherein the solidified melt and / or the solid has a substantially linear coefficient of thermal expansion a of at least 10 K 1 exhibit, comprehensive - a melting unit (1) with a cooled wall (101), a bottom (102) and a rim area (103), - a device (2) for providing a mixture (3), - a device (4) for heating the mixture (3) to obtain a viscous melt (5) and / or for heating the melt (5), and - a device (7) for extracting the melt (5), characterized in that a first cross-sectional area (Qi) of the melting unit (1) is smaller than a second cross-sectional area (Q2) of the melting unit (1), and wherein a distance (ai) of the first cross-sectional area to the bottom (102) of the melting unit (1) is smaller than a distance (32) of the second cross-sectional area (Q2) to the bottom (102).
2. Device according to claim 1, characterized in that at least between the first cross-sectional area (Qi) and the second cross-sectional area (Q2) the cross-sectional area of the melting unit (1) increases continuously in the direction of the second cross-sectional area (Q2), so that the melting unit (1) is formed at least sectionally as a cone that tapers towards the bottom (103).
3. Device according to one of claims 1 or 2, characterized in that the melting unit has an opening angle of the wall (101) of at least 2° and at most 30°.
4. Device (100) according to one of claims 1 to 3, characterized in that the base (102) and the wall (101) are connected to each other by a mechanical and / or force-fit connection. SCHOTT AG 30 P06194 WO 5. Device (100) according to one of claims 1 to 4, characterized in that the wall (101) comprises a plurality of cooling fingers which are connected to the base (102).
6. Device (100) according to claim 5, characterized in that the cooling fingers are arranged at an angle between 1 and 89° to the bottom (102) of the melting unit (1), and wherein the cooling fingers are preferably arranged at an angle between 45 and 89° and particularly preferably at an angle between 60° and 87° to the bottom (102) of the melting unit (1).
7. Device (100) according to one of claims 5 or 6, characterized in that the cooling of the cooling fingers and the base (102) are connected to each other.
8. Device (100) according to one of claims 5 to 7, characterized in that the cooling fingers and the base (102) are electrically connected to each other.
9. Device (100) according to one of claims 5 to 8, characterized in that the cooling fingers are arranged along a plane parallel to the base (102) at a distance of at least 0.1 mm and at most 3 mm from each other, so that gaps and / or joints are formed between the cooling fingers in the wall (101).
10. Device (100) according to claim 9, characterized in that the wall (101) comprises at least one dielectric material which is arranged at least partially in one of the gaps and / or joints.
11. Device (100) according to one of claims 5 to 10, characterized in that at least one cooling finger has a curved, preferably convex, surface on an inner side (101a) of the wall (101).
12. Device (100) according to one of claims 5 to 11, characterized in that the cooling fingers are electrically connected to one another. SCHOTT AG 31 P06194 WO 13. Device (100) according to one of claims 5 to 10, characterized in that at least one cooling finger has a coating at least in one area which is preferably electrically insulating.
14. Device (100) according to one of the preceding claims, characterized in that the wall (101) and / or the base (102) each comprise a material having a thermal conductivity Ao at 20 °C of at least 15 W / (mK), preferably at least 20 W / (mK), particularly preferably at least 70 W / (mK), in particular at least 145 W / (mK) and / or in the range of 15 W / (mK) to 450 W / (mK) and / or having an electrical conductivity of at least 0.5 × 10⁶ and at most 65 - 10⁶ S / m, preferably at least 1.3 - 10⁶ and at most 60 - 10⁶ S / m.
15. Device (100) according to one of claims 1 to 13, characterized in that the material of the wall (101) and / or the material of the bottom (102) are selected from the group comprising aluminium, steel, stainless steel, aluminium nitride, copper, boron nitride, silver and mixtures of the aforementioned materials.
16. Method for producing an inorganic non-metallic material in a melting process, obtaining a solidified melt (5) and / or a solid (9) with a predetermined shape, wherein the solidified melt (5) and / or the solid (9) has a substantially linear coefficient of thermal expansion a of at least 10 K 1 exhibit, encompassing the following steps: - Providing the device (100) according to one of the preceding claims, - Providing a mixture (3), - Heating the mixture (3) to obtain a melt (5) and / or heating the melt (5) wherein the melt (5) has a viscosity of less than 1 Pa-s, - Extracting at least a part of the melt (5), characterized in that the heating of the viscous melt (5) and / or the melt (5) solidified in the melting unit (1) is or can be started and stopped reversibly. SCHOTT AG 32 P06194 WO 17. The method of claim 16, characterized in that the method further comprises the step of: - Homogenizing the melt (5), in particular taking place before taking at least part of the melt (5).
18. Method according to one of claims 16 or 17, characterized in that the method further comprises the step: - Forming a solid (9) with a predetermined shape from the melt (5), wherein this step in particular follows immediately after the removal of at least a part of the melt (5).