Method and device for producing an inorganic non-metal material in a melting process

The method and apparatus address the challenge of producing inorganic non-metallic materials by using a cooled wall melting unit to achieve rapid cooling and controlled crystallization, enabling continuous production of materials with desired shapes and microstructures for energy storage.

WO2026234074A1PCT designated stage Publication Date: 2026-11-12SCHOTT AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063062
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods struggle to produce inorganic non-metallic materials, particularly those with high lithium content, from aggressive and low-viscosity melts, as they corrode conventional crucible materials and result in uncontrollable crystallization, making large-scale continuous production challenging and economically unviable.

Method used

A method and apparatus using a melting unit with a cooled wall to form a solid layer, allowing the melt to cool rapidly on the wall, achieving a cooling rate of 3.3 K/s to 7,500 K/s, thereby producing a solid with a predetermined shape and microstructure, including amorphous or crystalline phases, in a continuous process.

Benefits of technology

Enables reproducible production of inorganic non-metallic materials in a predetermined shape, suitable for energy storage applications, with controlled microstructure and high throughput, overcoming corrosion and crystallization issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026063062_12112026_PF_FP_ABST
    Figure EP2026063062_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention generally relates to a method and a device for producing an inorganic non-metal material in a melting process so as to obtain a solid body in a specified form in a melting unit having a cooled wall, wherein the melt is removed from the melting unit such that the melt at least partly passes through a processing range, characterized by a starting viscosity of <109 dPa-s, at at least a cooling rate K1 ranging from 3.3 K / s to 7,500K / s. The solid body obtained from the melt is present in a specified form, the specified form being a crystal phase fraction, preferably determined in wt.% in a Rietveld analysis of an X-ray diffractogram, and / or an average crystallite size of a crystal phase, preferably determined from a Rietveld analysis of an X-ray diffractogram, and / or the presence of a crystal phase. Preferably, the solid body is obtained in the form of a pulverulent and / or a platelet-shaped bulk material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] SCHOTT AG 1 May 6, 2026 P06193 WHERE

[0002] Method and apparatus for producing an inorganic non-metallic material in a melting process

[0003]

[0004] area of

[0005]

[0006] The present invention relates generally to a method and an apparatus for producing an inorganic non-metallic material in a melting process. In particular, the present invention relates to a method and an apparatus for producing an inorganic non-metallic material in a melting process, each of which makes it possible to obtain materials from aggressive and / or low-viscosity melts and / or from melts that have only a very narrow processing range, whereby a solid with a predetermined shape is obtained. In particular, according to embodiments, the method and the apparatus can be used to produce materials in a melting process in which, for example, a melt with a very high lithium content is present, and which would otherwise be very difficult to access via a melting route.

[0007]

[0008] the

[0009] In the course of the energy transition and the increased use of electrical energy, for example in electromobility, there is a need for materials that can be used in energy storage systems, whether as solid-state ion conductors or as electrode materials. In particular, there is a need for inorganic non-metallic materials that can be used in such processes. However, suitable materials for such applications, such as lithium-containing materials with a garnet-like structure and / or lithium-containing glasses, exhibit a number of special characteristics that make their production difficult. For example, lithium-containing sulfide glasses are known to have high ionic conductivity, but cannot be melted using conventional melting methods and are very susceptible to corrosion.Other inorganic non-metallic materials, which are suitable as solid-state ion conductors, for example lithium-containing crystalline materials with a garnet-like structure (e.g., Lithium-SCHOTT AG 2 06.05.2026 P06193 WO.

[0010] While materials such as lanthanum zirconate (or LLZO for lithium lanthanum zirconium oxide), or those with a so-called NASICON structure (NASICON for "sodium superion conductor," for example, lithium aluminum titanium phosphate, or LATP), or cathode materials for lithium-ion batteries made of lithium nickel manganese cobalt oxide (Li-NMC), are less susceptible to corrosion, they strongly attack common crucible materials in known melting processes. For example, a melt of an "LLZO"-type material strongly corrodes a precious metal like platinum, which is frequently used in high-temperature applications, and leads to the contamination of the resulting material with metallic particles. This is significant for the resulting electrical properties of such a melted material, since a solid-state ion conductor in a solid-state battery should simultaneously be an insulator against electron conduction.Metallic impurities in the solid-state ion conductor are therefore undesirable. Regardless, severe corrosion of the refractory materials used in a melting process, such as platinum or other precious metals commonly used in melting units, or even other ceramic refractory materials, is generally undesirable, as it is associated with considerable costs and is therefore not economically viable. While the above explanations were given specifically with regard to crystallizing materials, they naturally also apply to non-crystalline materials, such as glasses, which are also highly corrosive to common crucible or tank materials, for example, due to a high fluorine content in the melt.

[0011] Such generally "problematic" materials, as explained above, cannot be melted using conventional methods, or only with great difficulty, and therefore ultimately only uneconomically. However, melting some of these materials in a so-called "skull" crucible has proven suitable. Here, the material to be melted itself effectively forms the crucible wall; that is, the aggressive melt is only in contact with the corresponding solid in equilibrium with the melt. In this way, even materials that, like the aforementioned "LLZO," could not otherwise be produced using a melting process due to their highly corrosive nature can be melted. SCHOTT AG 3 06.05.2026 P06193 WO

[0012] Such skull crucibles, i.e., melting units with cooled walls, are described, for example, in US 2006 / 291528 A1, US 6 817212 B1, US 2005 / 005646 A1, JP 2016 / 051701 A, US 2005 / 083989 A1, and DE 10202449 A1. These patents concern general designs for such melting units, particularly with regard to the production of glasses and / or glass-ceramics in such melting units.

[0013] Such a melting process for an LLZO material can be found, for example, in US 2016 / 329598 A1.

[0014] The skull process is often not continuous. Rather, after melting, homogenization, and cooling, a batch of the molten material is obtained. If this solid is to be in bulk form, i.e., as a particulate solid (for example, as a powder), one or even several post-processing steps may be necessary. Particularly with materials prone to crystallization, zoning of the material can occur within the skull itself, so that only certain areas may exhibit the desired properties.

[0015] Despite the possibility, in principle, of melting certain materials that are “critical” with regard to their melting properties as described above – for example, those with very aggressive or corrosive melts, melts with very low viscosity and / or melts that have a very “short” processing range – challenges arise when such materials are to be provided on a larger scale, preferably in a continuous process.

[0016] Difficulties remain in that the resulting solid should not only be obtained as a bulk material, but also have to be given a specific, predetermined shape. Within the scope of this disclosure, such a "predetermined shape" is defined in particular as a crystal phase fraction, preferably determined as a percentage of the volume of crystals (VoL) in a Rietveld analysis of an X-ray diffractogram, and / or a mean crystallite size of a crystal phase, preferably determined from a Rietveld analysis of a sample. SCHOTT AG 4 06.05.2026 P06193 WO

[0017] X-ray diffractogram, and / or the presence of a crystalline phase. In other words, the form in this sense refers specifically to the microstructure of the solid.

[0018] This creates a need for a device and a process by which a solid made of an inorganic non-metallic material can be continuously obtained in a predetermined shape from a skull melting process.

[0019] Object of the invention

[0020] The object of the invention is therefore to provide a device and a method which at least partially reduces or overcomes the aforementioned weaknesses of the prior art.

[0021] Summary of the invention

[0022] The object of the invention is achieved by the subject matter of the independent claims. Preferred and / or specific embodiments are found in the dependent claims, the description, and the drawings of the disclosure.

[0023] The disclosure thus relates to a process for producing an inorganic, non-metallic material in a melting process while obtaining a solid with a predetermined shape, comprising the steps

[0024] - Providing a mixture in a melting unit, preferably in a melting unit with a cooled wall,

[0025] - Heating the mixture to obtain a melt, whereby a solid layer resulting from the melt forms on the cooled wall of the melting unit, which prevents direct physical contact between the melt and the wall of the melting unit,

[0026] - preferably homogenizing the melt,

[0027] - Removal of the melt, SCHOTT AG 5 06.05.2026 P06193 WO

[0028] so that a solid is obtained from the melt, which is present in a predetermined shape, wherein the predetermined shape has a defined crystal phase fraction and / or comprises an average crystallite size. The process is characterized in that, during the extraction of the melt, the initial viscosity of the melt is < 10 9 dPa s is at least partially crossed with a cooling rate Ki, where Ki is at least 3.3 K / s and at most 7,500 K / s. The initial viscosity of the melt is preferably < 10 6 dPa-s, especially preferred < 10 4 dPa s and in particular < 10 dPa s.

[0029] A cooling rate of 3.3 K / s, for example, would mean that a melt hitting a continuously rotating roller would cool from 1,351 °C to 1,350 °C at 150 rpm of the wheel and 75% "wrap". Similarly, a cooling rate of 7,500 K / s would mean, for example, a cooling from 1,600 °C to 1,350 °C at 450 rpm and 25% "wrap".

[0030] "Coverage" describes what percentage of the roller's circumference is covered with molten material. A coverage of 75% therefore means that the material would have to be in contact with the roller over 270° of its circumference in order to achieve the stated cooling rate.

[0031] Within the scope of this disclosure, the following definitions apply:

[0032] An inorganic non-metallic material is understood to be a material that exists inorganically and exhibits no metallic bonding or metal bonding. The inorganic non-metallic material of the disclosure may, for example, exist in a crystalline state, be amorphous (which includes X-ray amorphous), or contain both crystalline and amorphous components, i.e., be partially crystalline. A partially crystalline inorganic non-metallic material may also be referred to as a glass-ceramic; an amorphous, especially X-ray amorphous, material as a glass; and a completely crystalline material as a ceramic.

[0033] Even if the inorganic non-metallic material of the disclosure is non-metallic in the sense that it in particular does not exhibit any electronic conductivity (i.e., conductivity with electrons as the charge carriers) or preferably has such conductivity at most 10 SCHOTT AG 6 06.05.2026 P06193 WO

[0034] If the S / cm (at room temperature) is high, it is possible and may even be preferred that the material acts as a solid-state ion conductor or at least exhibits some ion conductivity.

[0035] Unless otherwise indicated by the context, for the purposes of this disclosure a mixture shall be understood to mean a mixture of different starting materials which is in particulate form, i.e. as a powder, and which is generally known, for example, from the glass and / or ceramics industry as a starting material for the production of an inorganic, non-metallic material.

[0036] In the context of this disclosure, a predetermined shape of a solid is understood to refer in particular to its microstructure. The microstructure of the solid, in the context of this disclosure, refers in particular to the crystallographic composition of the solid, specifically the formation of a particular crystal phase or, if applicable, several particular crystal phases, and / or the absence of a particular crystal phase or, if applicable, several particular crystal phases, and / or a crystal phase fraction, preferably determined as a percentage by volume or as a percentage by weight in a Rietveld analysis of an X-ray diffractogram, and / or a mean crystallite size of a crystal phase, preferably determined from a Rietveld analysis of an X-ray diffractogram.

[0037] It is generally understood that the solid body with a predetermined shape, which is formed from the inorganic non-metallic material in the process and / or by means of the device described in this disclosure, is formed. The inorganic non-metallic material thus relates to a general composition, and the solid body is its specifically obtained embodiment, which has the composition of the inorganic non-metallic material and is in the form of a shaped body. The solid body (which can also be referred to synonymously as the formed or resulting solid body) has a specific shape, which here generally refers to the microstructure of the solid body.

[0038] The process described above has a number of advantages. SCHOTT AG 7 06.05.2026 P06193 WO

[0039] This process makes it possible for the first time to reproducibly produce a predetermined shape of an inorganic non-metallic material from a melting unit with a cooled wall (this melting unit with a cooled wall can also be referred to as a skull crucible or simply skull within the scope of this disclosure), and in particular in a continuous process in which the solid is obtained from the melt and preferably directly from the process in the form of a bulk material, i.e., in the form of a mixture comprising particles. The particles can be shaped such that they are directly available as a very fine powder, or obtained as flakes or platelets.

[0040] Within the scope of the present disclosure, the wall is referred to as the entirety of the walls of the melting unit, whereby, for example, the term "wall" is preferred, particularly for embodiments with round base surfaces of the bottom of the melting unit.

[0041] The production of the inorganic non-metallic material, such that a solid with a predetermined shape is obtained, is achieved by extracting the melt from the melting unit into a processing range of the melt, which is characterized by a starting viscosity of < 10 9 dPa-s, with at least a cooling rate Ki in the range of 3.3 K / s to 7,500 K / s, is at least partially crossed. Alternatively or additionally, the quotient of dissipated heat power (dQ / dt) and mass flow rate (dm / dt) can also be used. Then: (dQ / dt) / (dm / dt) = k 2The speed k lies in a range of 100 m / s to 2,000 m / s, preferably in a range of 300 m / s to 1,000 m / s, and particularly preferably in a range of 600 m / s to 900 m / s. This takes into account the crystalline nature of the material and ensures that the heat of fusion is dissipated on the wheel.

[0042] The cooling rate Ki can preferably be in the range of 500 K / s to 1,500 K / s. Alternatively, the cooling rate Ki can be in the range of 3.3 K / s to 50 K / s.

[0043] The processing range of the melt is the temperature range in which the inorganic non-metallic material transitions from the liquid state to the solid state, or, in the case of amorphous materials, when a defined viscosity range is crossed. SCHOTT AG 8 06.05.2026 P06193 WO

[0044] Since the inorganic non-metallic material according to the present disclosure can also be at least partially amorphous, in particular glassy, ​​and in particular even completely amorphous and thus as a glass, the processing range can best be determined via the corresponding viscosity.

[0045] The cooling rate Ki, at which the processing range is at least partially traversed, is very high, meaning that the processing range is traversed very quickly, at least partially. Accordingly, the method according to the present disclosure provides that the melt of the inorganic non-metallic material is at least partially quenched. In this way, it is possible to reproducibly establish a predetermined shape for inorganic non-metallic materials, and in particular, the microstructure of the resulting material. This is especially relevant for materials with a high tendency to crystallize. For these materials, this is particularly important with regard to the resulting properties, such as the desired ionic conductivity, should they, for example, be solid-state ion conductors.Here it can be important to preserve certain crystal phases and / or to suppress the occurrence of certain other crystal phases.

[0046] However, it has also been shown that it can be advantageous for processing such materials if they are not fully crystalline, i.e., not ceramic, but at least partially crystalline or glass-ceramic. It has been shown that such materials can exhibit particularly advantageous properties, for example, with regard to further processing in the manufacture of energy storage devices for electrical energy. These processes typically use powdered solids, which often need to be ground to a specific particle size. Significant advantages can arise here if a glass-ceramic material is used.

[0047] As previously stated, it was already common knowledge to melt materials with a garnet-like structure in a melting unit with a cooled wall. However, in this process, no molten material was extracted, specifically no continuous extraction; rather, the solid was only obtained after the melting unit had cooled and the molten material had solidified. SCHOTT AG 9 06.05.2026 P06193 WO

[0048] The process according to the present disclosure preferably enables the corresponding solid formed in the process to be obtained not only in a predetermined form, i.e., with the desired microstructure, but also in the form of a powdered and / or platelet-shaped bulk material. The process is therefore particularly designed as a continuous process.

[0049] For the purposes of this disclosure, a bulk material is understood to be a single starting material or a mixture of starting materials, wherein the starting material or materials comprise grains of a solid, i.e., for example, a powder (which is understood to mean that the particles are those whose outer lateral dimensions are each of the same order of magnitude to each other, i.e., for example, spherical with a diameter which, within the limits of measurement accuracy, is preferably of the same order of magnitude) or platelets (which are understood to mean grains in which one lateral dimension is at least one order of magnitude smaller than the other two lateral dimensions, in other words, the thickness of the particle or grain is one order of magnitude smaller than its length and width).Of course, it is also possible for the grains of the bulk material to be needle-shaped, i.e., in a form where the length of the grain is at least one order of magnitude greater than its width and thickness. In particular, it is also possible for the bulk material to comprise both needle-shaped and plate-shaped grains, and additionally grains with lateral dimensions of the same order of magnitude. However, the process according to the present disclosure preferably yields bulk materials in which the solid is in the form of a powder and / or a plate-shaped bulk material. This is readily compatible with conventional downstream processing methods used to obtain a powder, for example, in the manufacture of electrical energy storage devices such as batteries.

[0050] It may be intended that the entire processing area is traversed with the cooling rate Ki. However, it is possible, and may also be preferred, that the processing area is traversed with at least one further cooling rate K2. In this case, this is generally referred to as staged cooling. Generally, SCHOTT AG 10 06.05.2026 P06193 WO

[0051] It is also possible to provide more than two cooling rates for cooling the melt, for example three, four or five cooling rates or more.

[0052] In particular, it can be provided that the cooling rate Ki is greater than the further cooling rate K2 and, especially, also greater than further cooling rates, provided the process includes staged cooling. This can be particularly preferred if the inorganic non-metallic material according to the disclosure is one that has a high tendency to crystallize and would therefore crystallize completely during "free" cooling, i.e., without the targeted rapid cooling of the process according to embodiments of the disclosure. In this case, the rapid cooling with the at least one cooling rate K1 according to the disclosure ensures that the melt is quenched.

[0053] In this way, it is possible, for example, to obtain a solid that is at least partially amorphous, even with very low-viscosity melts and materials with a generally high tendency to crystallize. Alternatively or additionally, the microstructure can also be specifically adjusted in a melt where, during cooling, a crystallization sequence occurs in such a way that a first crystal phase is formed and a second crystal phase forms at a lower temperature, or in a melt where the composition of the resulting crystal phase changes with decreasing temperature, such that a zoned crystal would be obtained with slow cooling, by selectively and rapidly passing through critical temperature ranges of the processing area.It can then be advantageous that, according to one embodiment, a staged cooling process takes place, so that, for example, a crystal phase with a defined composition is formed.

[0054] The method according to the disclosure is, as explained, particularly suitable for producing inorganic non-metallic materials that exhibit a high tendency to crystallize. According to one embodiment, the inorganic non-metallic material is or comprises a material with a high tendency to crystallize, and the proportion of crystal phases in the resulting solid is adjusted depending on the at least one cooling rate K1, with the crystal phase proportion being between 0 wt.% and 100 wt.%. Generally, the solid may contain several crystal phases. SCHOTT AG 11 06.05.2026 P06193 WO

[0055] This includes the following: the solid may be completely amorphous or completely crystalline. Depending on the precise composition of the inorganic non-metallic material or the resulting solid, different crystal phases are present in varying proportions. For example, with a crystal phase content of 0 wt%, the inorganic non-metallic material could be glass.

[0056] In particular, this makes it possible to produce a glass even from highly crystallizing materials, if desired, with a crystalline phase content of 0 wt%, but also to form the material as a glass-ceramic, i.e., semi-crystalline. According to one embodiment, it is also possible for the material to comprise different crystalline phases (and possibly an amorphous component). It has already been explained that advantages have been demonstrated when processing such a glass-ceramic material.

[0057] In particular, this is now possible by means of a continuous melting process, and, as explained, special features resulting from the melt composition or the mixture composition can also be taken into account, since these are usually not presented exactly according to the stoichiometry of a desired crystal phase, but take into account the mixing behavior of the material system under consideration with solid solution formation or the formation of eutectics or certain crystallization sequences (so-called melt differentiation).

[0058] The removal of the melt can generally be done in different ways.

[0059] In particular, according to one embodiment, it may be provided that the removal of the melt takes place:

[0060] - by immersing a contact surface of a cold body, preferably a metal body, into the melt and subsequently withdrawing the wetted contact surface of the body from it, or

[0061] - by a feeder under the influence of gravity.

[0062] According to one embodiment, it can therefore be provided that a cold body, in particular a metal body, is immersed directly in the molten metal. In this case, the surface of the SCHOTT AG 12 06.05.2026 P06193 WO

[0063] The contact surface of the corresponding body is immersed in the melt, and it may be provided that the body is wholly or partially immersed. However, immersion in the form of "dip" into the melt is only one embodiment; for example, the body may also be rotatable, such as a wheel or roller, which is preferably cooled. When the rotatable body is rotated, this occurs in such a way that, during rotation, a portion of the body's surface is immersed in the melt and, with continued rotation, is moved back out of it. In any case, with such an embodiment of the method in which a contact surface of a body is immersed in the melt, a layer of the corresponding material forms on the contact surface of the corresponding body. Since the body or its contact surface is cooler than the melt, and the body or its surface is therefore cooled, the material is dispersed in the melt.When the contact surface is withdrawn from the melt, or when it is only temporarily and partially contacted, a thin film of the melt forms on its surface, which then solidifies to form the solid body. If the melt is removed by immersing a contact surface of a body, as described above, it is generally preferred, without limitation to a specific embodiment of the method, that the contact time between the contact surface and the melt is at most 5 s, particularly preferably at most 3 s, and especially at most 1 s, and at least 0.03 s, preferably 0.1 s.

[0064] In this way, it is quite easy to set a predetermined shape for the formed solid. Rapid cooling can be achieved, on the one hand, by quickly withdrawing the body or the corresponding contact surface, but also by the body itself. For example, the temperature difference between the melt and the surface / contact area of ​​the body itself can have a quenching effect. This can be further advantageously supported by the design of the body itself. For example, the body can be designed as a metal body, with the metal preferably having a heat capacity of at least 1,000 J-K, preferably at least 1.700 J- K, and a thermal conductivity A at 20 °C of at least 15 W / (mK), preferably at least 20 W / (mK), particularly preferably at least 70 W / (mK) and in particular at least 145 W / (mK) and / or in the range of 15 W / (mK) to 450 W / (mK), which can be achieved, for example, by dimensioning the body and its precise design, and / or it can be provided that the body is SCHOTT AG 13 06.05.2026 P06193 WO.

[0065] cooled body, for example water-cooled, in particular a cooled metal body, for example water-cooled.

[0066] Advantageously, the initial cooling of the melt can occur during its free fall from the feeder onto a cool or cooled surface of a plate or roller (cooling step 1). The duration of cooling step 1 can be adjusted via the drop height, thus enabling precise control of the crystal-gas phases. Furthermore, the drop height determines the momentum of the impacting melt, thereby controlling the splashing away from the cooled surface. The drop height range can be from 0.01 m to 2 m; preferably, the range is between 0.5 m and 1.5 m.

[0067] With regard to the cool or cooled surface, the term "cool" refers to temperatures in a range of 0°C to 120°C, particularly preferably 35°C to 80°C.

[0068] Immersing a contact surface of a body into the melt, as described above, also allows, in principle, cooling with a staged cooling rate. Preferably, after immersion, the body or the corresponding contact surface is withdrawn from the melt after a time of at least 0.03 s and at most 5 s, or more preferably at least 0.1 s and at most 3 s, as already explained above. The melt that has come into contact with the body has already cooled down very rapidly at the contact surface, corresponding to the generally high cooling rate Ki. When the body or the corresponding part of its surface (i.e., the contact surface) with the thin layer of material is now withdrawn from the melt, the subsequent cooling process slows down; it can be provided that this occurs within the processing area itself.

[0069] Although the process for extracting the melt by immersion, as described, can be flexibly adjusted and therefore offers many possibilities for precisely controlling the microstructure of the inorganic non-metallic material according to the present disclosure, it also has certain disadvantages. In particular, material extraction in this process is discontinuous, and only a small amount of material is removed in one step. SCHOTT AG 14 06.05.2026 P06193 WO

[0070] Alternatively, it can be provided that the molten metal is extracted by a feeder under the influence of gravity.

[0071] For this purpose, the feeder is preferably attached to the bottom of the melting unit. A lateral attachment of the feeder to the melting unit is also conceivable. In the process, after the mixture is provided, heated, and melted to obtain a melt, and the melt is then homogenized, the melt is extracted by a feeder, which in this case must first be opened. In general, the process according to the disclosure, in the case of extracting the melt by a feeder according to one embodiment, therefore also includes the step of opening the feeder so that the melt can then exit the melting unit under the influence of gravity.

[0072] The method described here is particularly advantageous because it allows for continuous extraction of the melt. Furthermore, the amount of melt extracted can be controlled in this way, and is especially greater per unit of time than is possible with extraction by immersion.

[0073] It can be particularly advantageous if the melt is extracted in such a way that the solid is obtained directly in the form of a powdery and / or platelet-shaped bulk material. This can be achieved, for example, by allowing the melt, after extraction by the feeder, to fall onto a cool surface, the surface being positioned in the direction of the melt's fall so that the melt impacts the surface and cools, thus forming the solid and splashing away from the surface.

[0074] Various embodiments are possible. For example, in a very simple embodiment, the surface can be the surface of a plate-shaped or disc-shaped body, such as a metal plate. However, the body can also be cuboid or cylindrical. The surface can, for example, be the base of a generally prismatic body, preferably with a relatively small height compared to the dimensions of the corresponding base. In other words, the body can be a very thin plate. SCHOTT AG 15 06.05.2026 P06193 WO

[0075] However, such a design is only one possible embodiment. For example, it can also be provided that the surface is the outer surface of a cylinder, wherein the cylinder is rotatable and preferably also rotates. In this case, the cylinder can also be understood as a roller onto whose outer surface the melt impinges, with the roller preferably rotating.

[0076] In general, without being limited to a specific embodiment of the method, the surface onto which the melt impinges may be cooled, for example by a fluid, particularly by means of an aqueous cooling fluid, such as water. If the cooled surface is designed as a plate, it may be fluid-cooled, for example by water. Similarly, if the surface is designed as the outer surface of a cylinder (i.e., as the outer surface of a roller), the cylinder or roller may be fluid-cooled.

[0077] In the process as described, it can generally be provided that a surface which also serves for quenching is also used for deflection or as a deflection surface or deflection plate, so that the solid formed on the surface by quenching is deflected, for example directed into a collecting device where the formed solid is collected.

[0078] The quenching of the melt takes place directly on the cooled surface. Parameters such as the drop height of the melt and / or the contact time with the surface can be adjusted, for example, by the angle formed between the direction of the melt's fall and the normal vector to the surface. After the resulting solid rebounds or splashes away, it cools more slowly. Here, too, the process parameters can be set so that the entire processing area of ​​the melt is traversed with a single cooling rate Ki, or so that a staged cooling process occurs within the processing area. SCHOTT AG 16 06.05.2026 P06193 WO

[0079] According to one embodiment, the melt is extracted by a feeder under the influence of gravity, and the solid is obtained in the form of a powdery and / or plate-shaped bulk material, wherein the melt, after extraction by the feeder, falls onto a cooled surface, and wherein the surface is a plate and the plate is arranged in such a direction of fall of the melt that the melt hits the surface of the plate and cools down, so that the solid is formed and splashes away from the surface of the plate.

[0080] In further developments, it can be provided that the surface, which is then preferably designed as a plate, is arranged at an angle to the direction in which the melt falls, so that the resulting solid is deflected laterally, preferably perpendicular to the direction of fall. It can also be provided that the solid is then collected and gathered in a collection device. The angle between the surface and the direction in which the melt falls can be described in particular by the angle formed by the direction in which the melt falls onto the surface and the normal vector to the surface.

[0081] In a further development of the method, it can generally be provided, without limiting the method to a specific embodiment, that the plate is moved so that the point of impact of the melt on the plate or the surface varies over time.

[0082] Consequently, the process can generally be designed such that the plate is arranged at an angle to the direction in which the melt falls, so that the resulting solid is deflected laterally, preferably perpendicular to the direction of fall, and / or that it is moved in such a way that the point of impact of the melt on the plate varies over time. In this way, the point of impact of the melt on the surface of the plate is varied over time, so that the plate does not overheat.

[0083] Such heating can be avoided not only if the cool surface onto which the melt strikes after being removed from the melting unit is the surface of a plate, but also, for example, if the surface is designed as the surface of a roller, for example a cool one, preferably a cool one. SCHOTT AG 17 06.05.2026 P06193 WO

[0084] Roller which is designed to rotate and which also rotates in the method according to a preferred embodiment.

[0085] In such an embodiment of the method, in which the surface is the area of ​​a roller, as described above, the melt is also extracted by a feeder under the influence of gravity, and the solid is obtained in the form of a powdery and / or platelet-shaped bulk material, wherein, after extraction by the feeder, the melt impacts a preferably cool roller (or its surface) and cools down, so that the solid is formed.

[0086] The cooling of the melt on the roller or its surface occurs in a similar manner to when the melt strikes the surface of a plate, i.e., as in the embodiment already described in detail above, including further developments. Thus, even with a roller, the cooling of the melt, and therefore the cooling rate or rates, can be precisely controlled so that the solid has a predetermined shape.

[0087] However, it has been shown that using a roller can have further advantages over using a plate, especially when the process is further developed.

[0088] For example, the process can be designed so that the roller rotates, allowing the formed solid to be separated from the roller by centrifugal force. Here, too, the solid can then be directed towards a collection device or at least collected in one. At the same time, this approach also has the advantage that the point of impact of the melt on the roller varies over time.

[0089] In this further development of the process, the rotation of the roller allows for the creation of very specific solid shapes. The molten droplets that strike the roller are drawn long and thin across the roller surface by the rotation. Through contact with the cool surface and heat radiation, the melt cools rapidly, then solidifies into flakes and is separated from the roller surface by centrifugal force. SCHOTT AG 18 06.05.2026 P06193 WO

[0090] In general, the advantages of this process, especially when using a roller, lie in the high cooling rate achievable and the accuracy with which this rate can be adjusted. Furthermore, the process is suitable for continuous operation and high throughput. By selecting appropriate parameters, the flake geometry of the bulk material, as the resulting solid, can also be precisely controlled to minimize grinding effort.

[0091] In a further development of the method, it is advantageously provided that the roller comprises a thermally conductive, mechanically robust material such as copper, stainless steel, or aluminum. According to a preferred embodiment, the surface of the roller may be coated to protect it and prevent metal abrasion. For example, such a coating may comprise or be made of a high-temperature-resistant material. An exemplary material could be Al₂O₃, but other materials, such as SiO₂ and / or ZrÜ₂ or mixtures thereof, are also suitable.

[0092] In general, the roller can be made of a metallic material with a thermal conductivity A at 20 °C of at least 15 W / (mK), preferably at least 20 W / (mK), particularly preferably at least 70 W / (mK), and especially at least 145 W / (mK) and / or in the range of 15 W / (mK) to 450 W / (mK). The material can, for example, include copper, aluminum, and / or stainless steel.

[0093] In a further preferred embodiment, it can be provided that the roller is cooled, in particular cooled by a fluid, for example with water.

[0094] According to a further embodiment, it can be provided that the solid body is separated from the surface of the roller after impact by means of an airflow, in particular a targeted airflow.

[0095] The individual embodiments of the method, for example, cooling the surface of the roller, separating by means of an airflow and / or the special design of the roller. SCHOTT AG 19 06.05.2026 P06193 WO

[0096] Made from a specific material, they are of course all combinable with each other and, according to a preferred embodiment, can also be combined with each other.

[0097] As described, in embodiments of the process where the surface is the area of ​​a roller, after the melt impacts the roller and immediately after the solid is formed, the temperature of the solid particles preferably obtained in this way, for example in the form of flakes, can still be high enough at the moment of being flung off the roller to allow for a second, slower cooling step in the processing area. This second cooling step, with cooling rate K2 and any subsequent further cooling rates, can be used to further adjust the predetermined shape of the solid, in particular, for example, to adjust the desired crystal phase. The cooling rate(s) can be adjusted passively via the transport conditions themselves (e.g., height of the bulk material in a transport container, insulation of the subsequent transport route, etc.), or by targeted active cooling or heating (e.g., cooled vibrating trough, cooling oven, etc.).

[0098] To protect personnel, such as employees and plant operators, and the plant itself, suitable protective plates are generally fitted, without limitation to a specific embodiment of the process, but particularly for an embodiment with a preferably rotating roller, to prevent uncontrolled splashing of material. Ideally, the protective plates are water-cooled to protect them from overheating and to prevent adhesion of sintered material.

[0099] Another method for extracting the melt, where the melt is extracted by gravity through a feeder and the solid is obtained in the form of a powdery and / or platelet-shaped bulk material, involves atomizing the melt with air after extraction by the feeder, thereby cooling it and forming the solid. This can also be generally referred to as the "spraying method".

[0100] In the spraying process, air from an air nozzle is directed at high pressure onto the molten jet from the feeder. This atomizes the molten metal into fine droplets. SCHOTT AG 20 06.05.2026 P06193 WO

[0101] Cooling is achieved through radiation via the increased specific surface area and compressed air. The size of the melt droplets, and thus their cooling rate, can be adjusted by positioning the nozzle relative to the melt, selecting the type of air nozzle, and determining the air pressure and volume. The advantages of this method are that very high cooling rates can be achieved and that shaping is contactless.

[0102] The present disclosure also relates to an apparatus for producing an inorganic non-metallic material in a melting process to obtain a solid with a predetermined shape, in particular for carrying out a process according to one of the embodiments described above. The apparatus generally comprises:

[0103] - a melting unit with a cooled wall,

[0104] - a device for providing a mixture,

[0105] - a device for heating the mixture to obtain a melt and / or for heating the melt,

[0106] - preferably a device for homogenizing the melt,

[0107] - a device for extracting the melt,

[0108] - a device for forming a solid body with a predetermined shape.

[0109] The device is characterized in that the device for forming a solid body with a predetermined shape is a device designed to increase the surface area of ​​the melt.

[0110] The device is thus designed in such a way that, for the first time, inorganic non-metallic materials can be obtained from a continuous melting process that are inaccessible to conventional methods, for example, because the resulting melts are highly aggressive or have only a very short processing range. This is achieved through the interaction of two devices encompassed by the device for producing the inorganic non-metallic material: the device for extracting the melt and the preferred device for forming a solid with a predetermined shape. SCHOTT AG 21 06.05.2026 P06193 WO

[0111] These two devices work together in such a way that, for the first time, a cooling rate Ki of such a high that even highly crystallizing materials, i.e., those with a high tendency to crystallize, can be obtained in a predetermined shape. If necessary, further cooling rates for staged cooling can also be achieved. Furthermore, adjusting the shape of the body from the corresponding solid of the inorganic non-metallic material, and in particular obtaining it directly as bulk material, is now easily possible for the first time in this way.

[0112] According to an advantageous embodiment, the device for extracting the molten metal can comprise a body, in particular a metal body, preferably a cool or cooled metal body. The device for extracting the molten metal can, for example, be a feeder.

[0113] The cooled metal body preferably has a specific heat capacity of at least 1,000 J / K, more preferably at least 1,700 J / K, and a thermal conductivity A at 20 °C of at least 15 W / (mK), and is suitable for being at least partially immersed in and removed from the melt. As described in detail with regard to the process, the body can be configured as a body that is at least partially immersed in the melt, or, for example, as a rotatable or rotating wheel or rotatable or rotating roller. As also described with regard to the process, the body generally comprises a contact surface that is part of the surface of the body, and it is the contact surface of the body that is immersed in and removed from the melt – as also described in great detail above.The device for extracting the melt is generally preferably designed to perform repeated immersion in the melt, preferably at a predetermined, but modifiable, frequency. For example, the body can be movably mounted on an articulated arm. In this case, the solid forms as a thin layer of material on the body itself, so that, as already described above, the device for extracting the melt also acts as a device for forming a solid. Furthermore, the body can also be designed as a wheel or roller. SCHOTT AG 22 06.05.2026 P06193 WO.

[0114] Another preferred embodiment provides that the device includes a feeder for extracting the molten metal. In its simplest form, the feeder can be designed as a preferably reversibly closable outlet, for example in the base of the melting unit with a cooled wall. When the outlet is opened, the molten metal can then easily exit the melting unit by the influence of gravity.

[0115] A device for extracting the melt, which includes a feeder or is designed as a feeder, is therefore preferred because in this way - as has already been discussed in a corresponding manner with regard to the method - continuous extraction of the melt is particularly possible.

[0116] This can be particularly advantageous for material systems of an inorganic non-metallic material that is designed as a solid solution and / or eutectic forming system. Furthermore, this method, or such a device, allows for very precise adjustment of cooling rates, thus ensuring that the predetermined shape of the resulting solid can be obtained with high reproducibility. If the device for extracting the melt is configured as a feeder or includes one, the device for producing an inorganic non-metallic material in a melting process while obtaining a solid with a predetermined shape also comprises a device for forming a solid with a predetermined shape.

[0117] In a further development of the embodiment, in which the device for extracting the melt is a feeder, it can be provided that the device for forming the solid with a predetermined shape comprises the following:

[0118] - a cool surface, wherein the surface is preferably a plate arranged such that it defines an angle between a falling direction of the melt from the feeder and a normal vector to the plate, which is not zero; - a device for blowing air into the melt emerging from the feeder. SCHOTT AG 23 06.05.2026 P06193 WO

[0119] The surface can, for example, be the base of a generally prismatic body, such as the base of a plate or disk. Alternatively, the surface can be the lateral surface of a cylinder. In this case, for example, the device can be a roller or comprise one, which can be cool, for example, fluid-cooled, in particular water-cooled. Embodiments of the device for forming a solid with a predetermined shape have already been described in detail above in the description of the method and can be included accordingly in the device for producing an inorganic non-metallic material in a melting process to obtain a solid with a predetermined shape according to the present disclosure.

[0120] In the case that the device for extracting the melt is or comprises a body immersed in it, the device for extracting the melt itself is the device for forming the solid, as already discussed above. This is because, in this case, the corresponding layer of a solid forms on the body itself, as already described above with reference to the process. The solid is then obtained in the form of a thin layer on the body and must be removed. After removal, which can be carried out mechanically and / or thermomechanically, a bulk material is formed from the solid.

[0121] If the device for extracting the melt includes a feeder or is designed as a feeder, the solid can be obtained with particular precision with regard to the predetermined shape, i.e., with regard to its microstructure. Furthermore, the shape in which the solid is obtained, for example, the particle shape of the bulk material, can be easily and simply adjusted in this way.

[0122] If the device for extracting the melt includes a cooled surface, this surface can be designed such that the point of impact of the melt on the surface varies over time. This can be achieved, for example, if the surface is the area of ​​a plate, by moving the plate, particularly by moving it laterally; if the surface is the lateral surface of a cylinder, i.e., if the device for forming the solid is a cylinder, this can be achieved by rotating the cylinder. SCHOTT AG 24 06.05.2026 P06193 WO

[0123] Moving the process so that the point of impact of the melt varies over time is particularly advantageous in order to minimize or keep low the heating of the cooled surface at the point of impact or contact of the melt with the surface.

[0124] The device for forming the solid body with a predetermined shape can, as described, also be designed as or comprise a cooled roller. In this case, the roller is preferably rotatable. This allows the point of impact of the melt on the roller to be varied very easily without, for example, having to provide a lateral movement in addition to the rotational movement, while the rotational movement further facilitates the separation of the formed solid body from the roller.

[0125] Finally, the device for forming the solid can also be designed as a device for blowing in air or include one.

[0126] Examples

[0127] 1. A molten LLZO is prepared in a skull-shaped crucible. The crucible has a capacity of approximately 13 liters. After adding and melting the raw materials, the melt is homogenized by blowing in oxygen. A copper block with dimensions of 200 x 50 x 50 mm is then formed. 3 The piece is dipped into the molten metal for approximately 1 second and then withdrawn. The material adhering to the block is chipped off and, after further processing, can be used in a battery.

[0128] 2. The crucible from Example 1 has an opening of approximately 20 mm in its base. This opening is axially sealed with a graphite tube with an outer diameter of approximately 30 mm and an inner diameter of approximately 3 mm. A molten metal is prepared analogously to Example 1. The base cooling of the crucible prevents spontaneous escape of the molten metal. After homogenization, the graphite tube is heated by induction heating, allowing the molten metal to flow downwards. After falling from a height of 1 m, the molten metal strikes a water-cooled, rotating copper wheel. The wheel has a diameter of approximately 300 mm and rotates at approximately...

[0129] 150 rpm. The material remains in contact with the wheel for approximately 75% of its circumference before [SCHOTT AG 25 06.05.2026 P06193 WO].

[0130] the wheel. The material hitting the wheel solidifies quickly, cools further, and can be used in a battery after further processing steps.

[0131] 3. The crucible from Example 2 has an opening of approximately 3 mm in the bottom area.

[0132] Analogous to Example 1, a molten metal is prepared. Bottom cooling of the crucible prevents spontaneous outflow of the molten metal. After homogenization, the opening is mechanically cleared of solidified material, allowing the molten metal to flow downwards. After falling from a height of 1 m, the molten metal strikes a water-cooled, rotating copper wheel. The wheel has a diameter of approximately 300 mm and rotates at approximately 150 rpm. The material remains in contact with the wheel for approximately 25% of its circumference before exiting it. The material striking the wheel solidifies rapidly, cools further, and can be used in a battery after further processing steps.

[0133] 4. After homogenization, the molten material from the crucible in Example 2 flows downwards. After falling from a height of 10 cm, the emerging jet of liquid is dispersed by an airflow from a side nozzle. This causes the molten material to atomize into tiny droplets, which cool and solidify rapidly in flight. After further processing, the atomized material can be used in a battery.

[0134] Description of the drawings

[0135] The invention will be further explained below with reference to figures.

[0136] Fig. 1 shows the schematic structure of a device for producing an inorganic non-metallic material according to one possible embodiment.

[0137] Fig. 2 shows the schematic setup of a device for producing an inorganic non-metallic material according to a further embodiment. SCHOTT AG 26 06.05.2026 P06193 WO

[0138] Fig. 3 shows the schematic structure of a device for producing an inorganic non-metallic material according to a further embodiment.

[0139] Fig. 1 shows a schematic representation of a device 100 for producing an inorganic non-metallic material in a melting process while obtaining the solid 9 with a predetermined shape according to one embodiment.

[0140] The device 100 is one that enables the execution of a process for producing an inorganic non-metallic material in a melting process according to the embodiments described above. The device 100 comprises a melting unit 1 with a cooled wall, a device 2 for providing a mixture 3, and a device 4 for heating the mixture 3 to obtain the melt 5 or for heating the melt 5. The melt 5 has a processing range characterized by a starting viscosity of < 10 9 dPa s. The device 100 further comprises a device 6 for homogenizing the melt 5 and a device 7 for removing it.

[0141] The device 100 is generally, without limitation to a specific embodiment of the method and / or the device, constructed as a so-called "skull" or "sculp crucible". This generally means that the melting unit 1 comprises a cooled wall, which is or may be made, for example, of cooled metal tubes.

[0142] In general, the device 100 also includes a device 4 for heating the mixture 3 to obtain a melt 5 or for heating the melt 5. In such a device 100, as described here in general terms, the heating of the crucible contents, i.e., mixture 3 and / or melt 5, is known to be carried out by high-frequency energy coupled into the crucible contents. For this to occur, the crucible contents should have a certain conductivity. This is the case, for example, with some glass melts or with melts that generally contain ions. However, this is generally not the case for the mixture 3, which is present in solid form as bulk material. SCHOTT AG 27 06.05.2026 P06193 WO

[0143] To initiate the melting process, it can therefore be arranged that initially no high-frequency energy is coupled into the crucible contents, but rather, for example, the mixture 3 is heated using thermal energy to such an extent that it at least partially melts, thus achieving a conductivity of the at least partially melted mixture sufficient for high-frequency energy to be coupled into the crucible contents. The supply of thermal energy, for example, can then be stopped, and the subsequent heating of the crucible contents is carried out solely by high-frequency energy. In this way, both the melt 5 and the mixture 3, which is continuously fed into the melting unit 1, can be heated in the further course of the process.

[0144] The embodiment of the device 100 shown in Fig. 1 also includes a device 8 for forming the solid body 9 with a predetermined shape.

[0145] The device 2 for supplying the mixture 3 is shown in Fig. 1 as comprising, for example, a hopper 21 from which the mixture 3 flows onto a trough 22, from where it can be continuously fed to the melting unit 1. In the illustration of Fig. 1, the mixture 3 falls from the trough onto the melt 5 or is placed onto it. Of course, it is also possible to first transfer the mixture 3, which is initially in solid form, from the device 2 into the melting unit 1 and only then start the melting process. Generally, the melting unit 1 can also be filled differently than shown before the melting process is started. However, for carrying out a continuous process, it is advantageous to provide a device 2 for supplying the mixture 3 that allows for the continuous feeding of the mixture 3.

[0146] The device 4 for heating the mixture 3 to obtain a melt 5 and / or for heating the melt 5 is designed here such that it includes a generator 41 for providing high-frequency energy, which can be inductively coupled into the crucible contents, i.e., melt 5 and, if applicable, mixture 3, by means of the coil 42. As described, the device 100 can also include a further device for heating, in particular, the mixture 3, for example, by means of thermal energy, specifically for the initiation process of the melting process. This further device is not shown here for the sake of simplicity. SCHOTT AG 28 06.05.2026 P06193 WO

[0147] The device 100 preferably further comprises a device 6 for homogenizing the melt 5, which is shown schematically here in the form of a stirring rod immersed in the melt 5. However, other devices 6 are also conceivable. In its simplest form, this device 6 is not strictly necessary, since the introduction of high-frequency energy into the melt 5 induces an electric current, which is then homogenized by convection currents. However, it can be advantageous if the device 100 also includes a special component, for example, in the form of a device 6, which facilitates efficient homogenization of the melt 5.

[0148] The device 100 further comprises a device 7 for extracting the melt 5, which here is designed in the form of a feeder. However, as discussed above, other designs of the device 7 for extracting the melt are also possible. For example, this device 7 can also be designed as a body immersed in the melt 5, as discussed above.

[0149] The device 100 also includes a device 8 for forming the solid 9 with a predetermined shape. Generally, without limiting itself to the specific embodiment of the device 100 shown in Fig. 1, the device 7 for extracting the melt 5 and / or the device 8 for forming the solid 9 with a predetermined shape are designed such that the processing area of ​​the melt 5 is at least partially traversed, or can be traversed, with a cooling rate Ki, which lies in the range of 3.3 K / s to 7,500 K / s, preferably between 500 K / s and 1,500 K / s. In this way, the solid 9 is obtained from the melt 5 and is present in a predetermined shape, the predetermined shape containing a crystalline phase fraction, preferably determined by weight.-% in a Rietveld analysis of an X-ray diffractogram, and / or has a mean crystallite size of a crystal phase, preferably determined from a Rietveld analysis of an X-ray diffractogram, wherein preferably the solid 9 is or is obtained in the form of a powdered and / or a plate-shaped bulk material 10.

[0150] The device 100 shown in Fig. 1 represents a particularly preferred embodiment in which the device 100 includes a device 7 for removing the melt 5 in the form of a SCHOTT AG 29 06.05.2026 P06193 WO

[0151] The device 100 includes a feeder, which is shown here by way of example in the base of the melting unit 100. Furthermore, the device 100 comprises a device 8 for forming the solid body 9 with a predetermined shape. This device 8 is designed to include a cool, preferably cooled, roller 81. The roller 81 is preferably rotatable, as also shown here. This is particularly advantageous because in this way the point of impact of the melt 5 on the roller 81 can be varied very easily without, for example, having to provide a lateral movement in addition to the rotational movement, as might be the case, for example, in a device 8 comprising a cool, preferably cooled, plate 84 in order to heat the point of impact of the melt 5 as little as possible.

[0152] If, as here, the device 100 or the device 8 is designed such that the roller 81 is rotatable or rotates, the formed solid body 9 is separated from the roller 81 by centrifugal force and can then, as schematically shown here, also be flung away from it. The solid body 9 can then, for example, be directed towards a collecting device 83 or at least collected in such a device. At the same time, this procedure, as described, has the advantage that the point of impact of the melt 5 on the roller 81 varies over time.

[0153] In this further development of the method or device 100, the rotation of the roller 81 allows for the production of highly specific shapes (i.e., shaped bodies) of the solid body 9. The molten droplets impacting the roller 81 are drawn long and thin on the roller surface (generally the cooled surface of the device for forming the solid body with a predetermined shape) by the rotation. Through contact with the cooled surface and heat radiation, the melt 5 cools rapidly, then solidifies into flakes and is separated from the roller surface by centrifugal force.

[0154] In general, the advantages of the method when using a roller 81, or correspondingly the device 100 comprising a roller 81 as part of the device 8 for forming the solid 9, in particular a rotating roller 81, lie in the achievable high cooling rate and the accuracy with which the cooling rate can be set. Furthermore, the method and corresponding device 100 are suitable for continuous operation. SCHOTT AG 30 06.05.2026 P06193 WO

[0155] Suitable for high throughputs. By selecting appropriate parameters, the flake geometry of the bulk material 10, as which the formed solid body 9 is obtained, can also be well adjusted to minimize the grinding effort.

[0156] In a further development of the method and / or device 100, it can be advantageously provided that the roller 81 comprises a thermally conductive, mechanically robust material such as copper, stainless steel, or aluminum. According to a preferred embodiment, the surface of the roller 81 can be coated to protect the surface and prevent metal abrasion. For example, such a coating can comprise or be made of a high-temperature-resistant material. An exemplary material could be Al₂O₃, but other materials, such as Si₂ and / or ZrC or mixtures thereof, are also suitable.

[0157] In general, the roller 81 can be made of a metallic material with a thermal conductivity A at 20 °C of at least 15 W / (mK), preferably at least 20 W / (mK), particularly preferably at least 70 W / (mK), and especially at least 145 W / (mK) and / or in the range of 15 W / (mK) to 450 W / (mK). The material can, for example, include copper, aluminum, and / or stainless steel.

[0158] In a further preferred embodiment, it can be provided that the roller 81 is cooled, in particular cooled by a fluid, for example by an aqueous liquid or water.

[0159] As explained, after the melt 5 impacts and immediately after the solid 9 forms from it, the temperature of the solid particles preferably obtained in this way, for example in the form of flakes, can still be high enough at the moment of being flung off the rotating roller 81 to necessitate a second, slower cooling step in the processing area. This second cooling step with the cooling rate K2 and any subsequent further cooling rates can be used to further adjust the predetermined shape of the solid 9, in particular, for example, to adjust the desired crystal phase. The cooling rate(s) can be passively adjusted via the transport conditions themselves (e.g., the height of the bulk material 10 in a transport container). SCHOTT AG 31 06.05.2026 P06193 WO

[0160] Isolation of the further transport route, etc.), or targeted active cooling or heating (e.g. cooled vibrating trough, cooling oven, etc.).

[0161] To protect personnel, such as employees and plant operators, and the plant itself, suitable protective plates 82 are generally fitted, without limitation to a specific embodiment of the method and / or the device 100, but particularly for an embodiment with a preferably rotating roller 81, to prevent uncontrolled splashing of material. Ideally, the protective plates 82 are water-cooled to protect them from overheating and to prevent adhesion of sintered material. They can also, if necessary, direct the splashing solid 9 into a collection device 83 for the bulk material 10, as schematically indicated in Fig. 1.

[0162] The device 100 can generally include further devices. The hood 11, which can at least partially cover the upper area of ​​the melting unit 1, is shown schematically here. The hood 11 can be arranged at a distance from the upper edge of the melting unit 1, as shown here, or it can close it completely in the form of a lid. In this way, excessive heat loss can be avoided.

[0163] The device shown in Fig. 2 differs from the embodiment shown in Fig. 1 in that the device 8 for forming the solid body 9 with a predetermined shape is, in the case of Fig. 2, a plate 84 instead of a roller 81. As shown in Fig. 2, the plate can be arranged obliquely, i.e., at an angle to the direction in which the melt 5 falls, so that the formed solid body is deflected laterally, preferably perpendicular to the direction in which it falls. The plate 84 can also be moved laterally such that the point of impact of the melt 5 on the plate varies over time.

[0164] Fig. 3 differs from the devices in Fig. 1 and Fig. 2 in that the device 8 for forming the solid body 9 with a predetermined shape according to Fig. 3 comprises one or more laterally arranged nozzles 85 instead of a cool or cooled surface 8. The molten jet from the feeder 7 is preferably directed at high pressure through the nozzles 85. The melt 5 is thus atomized into fine droplets. SCHOTT AG 32 06.05.2026 P06193 WO

[0165] Cooling is achieved through radiation via the increased specific surface area and compressed air. The size of the melt droplets 5, and thus their cooling rate, can be adjusted by positioning the nozzle 85 relative to the melt 5, selecting the type of air nozzle 85, and controlling the air pressure and volume. SCHOTT AG 33 06.05.2026

[0166] P06193 WHERE

[0167] List of reference signs

[0168] 100 Device for producing an inorganic non-metallic material in a melting process 1 Melting unit

[0169] 2 Device for providing a mixture

[0170] 3 Mixture

[0171] 4. Heating device

[0172] 5 Melt

[0173] 6 Device for homogenizing the melt

[0174] 7 Device for removing the melt

[0175] 8 Device for forming a solid body with a predetermined shape

[0176] 9 Solids

[0177] 10 bulk goods

[0178] 11 Hood

[0179] 41 Generator for providing high-frequency energy 42 Coils

[0180] 81 roller

[0181] 82 mudguards

[0182] 83 Containment device

[0183] 84 plates

[0184] 85 Spray nozzle

[0185]

Claims

SCHOTT AG 34 May 6, 2026 P06193 WHERE Patent claims 1. Method for producing an inorganic non-metallic material in a melting process to obtain a solid (9) with a predetermined shape, comprising the steps - Providing a mixture (3) in a melting unit (1), - Heating the mixture (3) to obtain a melt (5), - Extraction of the melt (5), wherein the extraction of the melt (5) is carried out in such a way that a processing area of ​​the melt (5) is traversed, wherein a solid (9) is obtained from the melt (5) which is in a predetermined shape, wherein the predetermined shape has a defined crystal phase fraction and / or comprises an average crystallite size, characterized in that the processing area of ​​the melt (5) has a starting viscosity of < 10 9dPa s is included and is at least partially crossed with a cooling rate Ki that is in the range of 3.3 K / s to 7,500 K / s.

2. Method according to claim 1, characterized in that the initial viscosity of the melt (5) is preferably < 10 6 dPa-s, especially preferred < 10 4 dPa s and in particular < 10 dPa-s.

3. Method according to one of claims 1 or 2, characterized in that the cooling rate Ki is preferably in a range of 3.3 K / s to 50 K / s or preferably in a range of 500 K / s to 1,500 K / s.

4. Method according to one of the preceding claims, characterized in that the processing area is traversed with at least one further cooling rate K2.

5. A method according to any of the preceding claims, characterized in that the solid (9) is or is obtained in the form of a powdered and / or platelet-shaped bulk material (10). SCHOTT AG 35 06.05.2026 P06193 WO 6. Method according to one of the preceding claims, characterized in that the crystal phase fraction is determined as wt.% in a Rietveld analysis of an X-ray diffractogram and that the mean crystallite size is determined from a Rietveld analysis of an X-ray diffractogram.

7. Method according to one of the preceding claims, characterized in that the inorganic non-metallic material is or comprises a material with a high tendency to crystallize and wherein, depending on the at least one cooling rate Ki, the total crystal phase fraction of the solid formed (9) is adjusted, wherein the crystal phase fraction is from 0 wt.% to 100 wt.%.

8. Method according to one of the claims, characterized in that the removal of the melt (5) is carried out as follows: - by immersing a contact surface of a body, preferably a metal body, into the melt (5) and subsequently withdrawing the contact surface of the body from the melt (5), or - by a feeder under the influence of gravity.

9. Method according to claim 8, characterized in that the removal of the melt (5) by a feeder is carried out under the influence of gravity and the solid (9) is or is obtained in the form of a powdery and / or a platelet-shaped bulk material (10), wherein - the melt (5) falls onto a cool surface after being removed by the feeder, and the surface is arranged in such a direction of fall of the melt (5) that the melt (5) impacts the surface and cools down, so that the solid (9) forms and splashes away from the surface; and / or - the melt (5) is atomized by a fluid after being removed by the feeder and cools down, so that the solid (9) is formed. SCHOTT AG 36 06.05.2026 P06193 WO 10. Method according to one of claims 8 or 9, characterized in that the melt (5) impacts a cool surface, wherein the surface is an area of ​​a plate, and wherein - the surface and / or the plate is arranged at an angle to the direction of fall of the melt (5) so that the solid formed is deflected laterally, preferably perpendicular to the direction of fall; or - the solid is separated from the plate (81) after impact by means of an airflow, in particular a targeted airflow; or - the surface is moved in such a way that the point of impact of the melt (5) on the surface varies over time.

11. Method according to one of claims 8 or 9, characterized in that the melt (5) preferably impacts a cooled surface, wherein the surface is a roller (81), and wherein the roller (81) comprises at least one of the following features: - the roller (81) rotates so that the formed solid body (9) is separated from the roller (81) by centrifugal force; - the solid body (9) is separated from the surface of the roller (81) after impact with the surface of the roller (81) by means of an airflow, in particular a targeted airflow; - the roller (81) is cooled by a fluid.

12. Device (100) for producing an inorganic non-metallic material in a melting process to obtain a solid (9) with a predetermined shape, in particular for carrying out a method according to any one of claims 1 to 7, comprising - a melting unit (1), - a device (2) for providing a mixture (3), - a device (4) for heating the mixture (3) to obtain a melt (5) and / or for heating the melt (5), - a device (7) for extracting the melt (5), - a device (8) for forming a solid body (9) with a predetermined shape, SCHOTT AG 37 06.05.2026 P06193 WO characterized in that the device (8) for forming a solid body (9) with a predetermined shape is designed to increase the surface area of ​​the melt (5).

13. Device (100) according to claim 12, characterized in that the device (8) for forming a solid (9) comprises a cool surface, wherein the cool surface is a roller (81) or a plate.

14. Device (100) according to one of claims 12 or 13, characterized in that device (8) for forming a solid (9) comprises a spray nozzle.

15. Device (100) according to one of claims 12 to 14, characterized in that the device (7) for removing the melt (5) - comprises a body, in particular a metal body, preferably a cool and / or cooled metal body, and / or - includes a dining table.

16. Device (100) according to claim 15, characterized in that the device (7) comprises a feeder and that the device (8) for forming a solid with a predetermined shape comprises the following: - a plate arranged such that it defines an angle between a fall direction of the melt (5) from the feeder and a normal vector to the plate, which is not 0; and - a device for blowing air into the melt exiting the feeder (5).