Method for recycling cellulosic textiles
A recycling process for cellulosic textiles addresses the challenge of recycling blended materials by shredding, dissolving in NaOH, shaping, and drying, producing 3D objects efficiently and sustainably.
Patent Information
- Application Number
- PCT/EP2026/063096
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-06
- Filing Date
- 2026-05-06
- Publication Date
- 2026-11-12
AI Technical Summary
Existing recycling processes for cellulosic textiles are limited to pure cotton textiles and struggle with recycling blended textiles due to different physicochemical properties and the lack of suitable solvents, leading to low-value reuse or disposal methods.
A recycling process involving shredding, partial dissolution in an aqueous NaOH solution below 0°C, shaping, coagulation, and drying to produce valuable materials like 3D objects, optionally with separation of undissolved fibers, using minimal solvents and no additives.
Enables the recycling of cellulosic textiles into valuable materials and objects, such as 3D printed items, without the need for complete dissolution and using additives, while accommodating blends of cellulose and synthetic fibers.
Smart Images

Figure 00000019_0000 
Figure 00000020_0000
Abstract
Description
[0001] Cellulosic textile recycling process
[0002] FIELD OF INVENTION
[0003] The present invention relates to the field of cellulosic textile recycling processes.
[0004] STATE OF THE ART
[0005] Cellulose fibers are a widely used raw material in consumer goods such as clothing and textiles in general. Cellulose is a natural polymer, the main component of plant cells. In recent years, the demand for textiles has steadily increased due to new consumption habits and the continued growth of the world's population. This increase in consumption is accompanied by a rise in textile waste production: millions of tons of textile waste are generated annually. For example, it is estimated that 85% of purchased clothing is thrown away within a year of purchase.
[0006] An example of a cellulose-based fiber is cotton. Cotton fibers are harvested from cotton plants and consist of long, intertwined chains of cellulose. The growing global population is impacting increasingly limited resources such as agricultural land and water. Demand for cotton continues to rise, but its production requires increased use of these resources, while also generating a significant amount of waste that pollutes the areas where it is discarded. Recycling textile waste therefore appears to be a virtuous path to limiting the environmental and societal impact of this industry.
[0007] Besides cotton fibers, there are so-called "artificial" cellulosic fibers such as viscose and Lyocell. Viscose production can have a negative impact on the environment due to the chemical reagents used and the generation of byproducts. Another manufacturing process for artificial cellulosic fibers is the Lyocell process, which uses the solvent N-Oxide-N-methylmorpholine monohydrate or ionic liquids. This process is expensive and / or requires the use of stabilizers to prevent the risk of explosion. It therefore appears that a more sustainable and environmentally friendly alternative would be to reuse the abundant source of cellulosic fibers found in textile waste.
[0008] There are various processes for recycling cellulosic textile waste. For example, patent application W02018213117 A1 describes a cotton waste recycling process comprising cellulose hydrolysis, dissolution of the hydrolyzed cellulose, and finally extrusion of the dissolved cellulose solution to regenerate it as yarn.
[0009] This type of process is, however, limited to the recycling of pure cotton textiles. Textiles composed of a mixture of cotton fibers and other fibers, particularly synthetic ones, are difficult to recycle due to their different physicochemical properties and the lack of common (or prohibitively expensive) solvents to completely dissolve the textile and spin new fibers, as described in patent application W02018115584 A1. Blended textiles, i.e., woven from several types of fibers, are therefore generally reused as second-hand products or materials, cut up to be transformed into rags, shredded to produce low-value-added stuffing or paneling, or burned.
[0010] Other processes for recycling cellulosic textiles have been developed. Patent application W02019140245 A1 describes a process involving a subcritical water reaction to produce materials comprising cellulose and terephthalic acid from cotton and cotton / polyester blend textile waste. Finally, patent application W02023062316 A1 describes a process for obtaining cellulose pulp from textiles including cotton and synthetic fibers. This process involves grinding the textile waste to obtain a first mixture of fibers and ground residues. After a first step of chemically separating the cellulosic and non-cellulosic fibers, a second mixture richer in cellulosic fibers is obtained. This second mixture is then filtered to recover a solid phase of cellulosic fibers.The cellulosic fibers are then dissolved to obtain a cellulose paste, which is subsequently filtered, removing undissolved particles.
[0011] However, there remains a need for recycling processes for cellulosic textile waste that are not limited to recycling purely cellulose-based textiles intended for the manufacture of fibers and films through cellulose dissolution. It is therefore necessary to develop recycling processes for cellulosic textile waste that result in valuable materials such as 3D printed objects made from pure cellulose or cellulose blended with other fibers, and that also offer the possibility of recovering synthetic fibers.
[0012] DESCRIPTION OF THE INVENTION
[0013] One aim of the invention is therefore to design a process for recycling cellulosic textiles into valuable materials and objects, such as 3D objects, meeting the needs mentioned above.
[0014] To this end, the present invention proposes a process for recycling cellulosic textiles comprising the steps of:
[0015] (i) shredding of cellulosic textiles;
[0016] (ii) at least partial dissolution of shredded cellulosic textiles in an aqueous solution comprising 6 to 10% by weight of NaOH at a temperature below 0°C to obtain a cellulosic solution;
[0017] (iii) shaping of the cellulosic solution;
[0018] (iv) coagulation of the shaped cellulose solution and washing of the coagulated cellulose material in a cellulose-free solvent; and
[0019] (v) drying of the cellulosic material obtained in (iv) to give a cellulosic object.
[0020] This process thus allows the recycling of cellulosic textiles, by optionally operating a separation, using a minimum of solvents and without using additives, while avoiding the limitations due to the presence of undissolved fibers, the degree of polymerization of the cellulose used and the viscosity of the mixture obtained.
[0021] Depending on other advantageous but optional features, possibly taken in combination:
[0022] The process comprises, between step (i) shredding and step (ii) dissolution, the following steps:
[0023] o (i') contacting the shredded cellulosic textiles with an aqueous acid solution to achieve a degree of cellulose polymerization of less than 400; eto (i”) washing away the acid present in the treated shredded cellulosic textiles, the shaping step (iii) is carried out by pressure flow of the cellulosic solution obtained at the end of step (ii) through a nozzle and coagulation of the cellulosic solution obtained in a non-solvent bath.
[0024] the process includes, between step (iii) and (iv), a step (iii') of gelling the cellulosic solution;
[0025] Cellulosic textiles include cotton, polycotton, viscose, or fibers obtained via the Lyocell process, alone or in blends with polyester, polyamide, acrylic, metallic fibers, polyurethane, or elastane;
[0026] the aqueous acid solution used in step (i') is an aqueous solution comprising 0.1 mol / L to 1 mol / L of hydrochloric or sulfuric acid;
[0027] step (i') is carried out at a temperature between 50 and 95 °C, preferably between 70 and 90 °C, for a period of 30 minutes to 6 hours;
[0028] the process includes, after the dissolution step (ii), a step (ii') of separating undissolved fibers by filtration;
[0029] Filtration is carried out using a sieve with a mesh size between 50 µm and 1 mm, in particular less than 300 µm, preferably between 100 and 200 µm;
[0030] the separated fibres obtained at the end of step (ii') are subjected to a step (ii”) in which they are washed first with an aqueous solution of NaOH at a concentration of 6 to 10% by weight at a temperature below 0°C, then in water;
[0031] during the water washing in step (ii”), the mixture of water, separated fibers and residual cellulose is agitated at a speed between 100 and 1000 rpm to remove the residues of dissolved and coagulated cellulose;
[0032] the washed separated fibres obtained at the end of step (ii”) are then subjected to a drying step (ii'”);
[0033] Coagulation and washing in step (iv) are carried out using a cellulose non-solvent selected from water, distilled water, an aqueous solution of acid, in particular hydrochloric acid at a concentration between 0.01 and 0.5 mol / L, methanol, ethanol and isopropanol.
[0034] Another object of the invention relates to the product that can be obtained by the recycling process according to the invention. DESCRIPTION OF FIGURES
[0035] [Fig. 1] represents a first embodiment of the invention in which the process does not include a step of separating the fibers of different materials. MP represents the raw material and PF the final product, Y the shaping by 3D printing and Z the shaping by granulation, i.e. the formation of particles.
[0036] [Fig. 2] represents a second embodiment of the invention in which the process includes a step of separating the fibers of different materials. MP represents the raw material, CP the co-product (i.e., the dry synthetic fibers or particles), and PF the final product, Y the shaping by 3D printing, and Z the shaping by granulation.
[0037] DETAILED DESCRIPTION OF THE INVENTION
[0038] The invention relates to a process for recycling cellulosic textiles comprising the steps of:
[0039] (i) shredding of cellulosic textiles;
[0040] (ii) dissolution, at least partial, of shredded cellulosic textiles in an aqueous solution comprising 6 to 10% by weight of NaOH at a temperature below 0°C to obtain a cellulosic solution;
[0041] (iii) shaping of said cellulosic solution;
[0042] (iv) coagulation of the shaped cellulosic solution and washing of the coagulated cellulosic material in a cellulose non-solvent; and (v) drying of the coagulated cellulosic material to give a cellulosic object.
[0043] For the purposes of this invention, the term "cellulosic textiles" refers to textiles containing at least 25% by weight of cellulose-based fibers, or between 40% and 100% by weight, preferably between 40% and 90% by weight, and even more preferably between 50% and 80% by weight. The cellulose content can be determined by any method known to those skilled in the art. Generally, the fraction is indicated on the textile label. An experimental method of determination can be by weighing the undissolved fraction under the conditions described below, i.e., the non-cellulosic fraction. Potentially, traces of lubricants, detergents, and other dirt and contaminants may be found in cellulosic textiles.
[0044] Typically, cellulosic textiles include naturally sourced cellulose fibers such as cotton and linen, synthetic cellulose fibers such as those produced using the viscose or Lyocell processes, and blends of these fibers with each other or with other fibers. These blends may include other naturally sourced fibers (e.g., wool), synthetic fibers, or even metal filaments such as aluminum, silver, gold, or copper. In particular, synthetic non-cellulosic fibers may include polyester, as in polycotton (a blend of cotton and polyester), polyamide, acrylic, polyurethane, and / or elastane. The described process is considered particularly advantageous for recycling textiles containing cotton or viscose, or Lyocell blended with synthetic fibers, especially cotton and polyester, i.e., polycotton.
[0045] The term "cellulose solution" should be understood, for the purposes of this invention, as meaning all types of flowing materials based on dissolved cellulose and based on dissolved cellulose solutions containing undissolved fibers.
[0046] For the purposes of this invention, the term "cellulosic material" means all types of non-flowing, gelled or coagulated materials based on cellulose, whether or not they contain undissolved, cellulosic or synthetic fibers.
[0047] The term "cellulosic object" should be understood, for the purposes of this invention, as meaning all types of dry 3D materials or objects based on pure cellulose or cellulose mixed with other cellulosic or synthetic fibers.
[0048] The term "co-product" should be understood, for the purposes of the present invention, as referring to the separated dry or wet synthetic fibers that can be obtained by the process according to the invention.
[0049] The process according to the invention first comprises a step (i) of shredding the cellulosic textiles. Shredding consists of unraveling the weave and transforming the textiles into fibers or fiber bundles. Step (i) of shredding can be carried out by any method known to those skilled in the art. In particular, shredding can be carried out automatically by robotic lines. In step (ii), the shredded textiles are at least partially dissolved in an aqueous solution comprising 6 to 10% by weight of sodium hydroxide (NaOH, or caustic soda) at a temperature below 0°C. The dissolution is advantageously carried out at a temperature between 0 and -18°C.
[0050] The process does not necessarily require complete dissolution of the cellulose or stabilization of the dissolved cellulose solution. Therefore, as a strong base, NaOH alone is sufficient to dissolve cellulose without the need for additives such as urea or zinc oxide. Furthermore, NaOH is a widely available, inexpensive, easy-to-store solvent with well-established industrial applications. In addition, the absence of additives minimizes environmental impact and simplifies solvent recycling.
[0051] According to some embodiments, the process includes, between steps (i) and (ii), the additional optional steps (i') and (i”).
[0052] Step (i') involves contacting the shredded textiles obtained in step (i) with an aqueous acid solution. This step allows the degree of polymerization of the cellulose to be adjusted to a value below 1000, preferably between 100 and 600, particularly below 400, and even more preferably between 200 and 300. The term "degree of polymerization" (DP) refers to the average number of anhydroglucose units in the polymer, cellulose. It can be calculated, for example, from the measurement of the limiting viscosity index of cellulose in a dilute cupriethylenediamine (CED) solution. In general, cotton has a degree of polymerization of cellulose between 1000 and 6000, while the cellulose in artificial cellulose fibers has a degree of polymerization between 300 and 500. Lowering the degree of polymerization facilitates the dissolution of cellulose and thus increases its concentration in the resulting solution.The viscosity of the solution increases with the concentration of cellulose and its DP.
[0053] The aqueous acid solution can be chosen from aqueous solutions containing hydrochloric acid or sulfuric acid. Generally, the acid concentration is between 0.1 and 1 mol / L, preferably 0.4 mol / L.
[0054] Step (i') is carried out at a temperature between 50 and 95°C, preferably between 70 and 90°C, for a period of 30 minutes to 6 hours.
[0055] Step (i”) is the washing of the acid from the shredded cellulosic textiles treated in step (i'). This washing can, for example, be carried out with water. Optionally, the fibers are dried at a temperature of 50°C at ambient pressure. These steps (i') and (i”), by reducing the degree of polymerization of the cellulose, facilitate its dissolution, but they are not mandatory.
[0056] According to a first embodiment of the process according to the invention, the subsequent steps of the process are carried out on blended fibers comprising cellulose and non-cellulosic fibers or on pure cellulose fibers. In this embodiment, the recycling process does not include any step of separating undissolved non-cellulosic fibers. This first embodiment is illustrated in Figure 1.
[0057] Step (iii) is a shaping step of the cellulosic solution obtained in step (ii), including, where appropriate, non-cellulosic fibers. It can be carried out by pressurizing the cellulosic solution through a nozzle (see the two embodiments described below).
[0058] In a first embodiment, the cellulose solution is shaped by 3D printing. In this embodiment, the cellulose solution has a viscosity, for example, between 10 and 10,000 Pa·s at 20°C. High viscosity can result from a higher concentration or a greater degree of polymerization of the cellulose used. The cellulose solution is printed onto a suitable support, for example, glass, and then immersed in a coagulation bath in step (iv), described below.
[0059] In a second embodiment, the cellulose solution is shaped by granulation. Droplets of the extruded cellulose solution are formed at the nozzle outlet. Conditions such as pressure, nozzle size, distance between the nozzle and the coagulation bath, etc., can be adjusted according to the desired properties of the final particles, for example, spherical beads.
[0060] Step (iv) comprises coagulating the shaped cellulose solution and washing the coagulated cellulose material. The cellulose solution shaped in step (iii) can, for example, be immersed in a coagulation bath in the case of 3D printing. In the case of granulation, droplets of cellulose solution are formed and then fall into the coagulation bath. This coagulation bath contains a cellulose non-solvent, regardless of the shaping method. The coagulation of the cellulose solution according to the present invention corresponds to the regeneration of cellulose; these terms are equivalent. The non-solvent can be chosen, in particular, from water, distilled water, an aqueous solution of acid such as hydrochloric acid dilute to a concentration between 0.01 and 0.5 mol / L, methanol, ethanol, and isopropanol.
[0061] The washing of coagulated cellulosic material is carried out using a non-solvent, which can be chosen from water, distilled water, an aqueous solution of an acid such as hydrochloric acid dilute to a concentration between 0.01 and 0.5 mol / L, methanol, ethanol, and isopropanol. This can be a single wash or a series of washes. This washing removes the NaOH contained in the coagulated cellulosic material.
[0062] In this discussion, "coagulation" refers to the transformation of dissolved cellulose chains (solution or gel in NaOH-water) into undissolved cellulose.
[0063] The process according to the invention optionally includes a gelation step (iii') between steps (iii) and (iv). During this optional step, the shaped cellulose solution is gelled for several hours until it solidifies in the desired shape. This step can last from 30 minutes to 24 hours, at temperatures between 20 and 60°C. For example, gelation can last 12 hours at 40°C. This optional step is only feasible in the case of shaping by 3D printing.
[0064] In this discussion, "gelation" refers to the transformation of a solution into a three-dimensional polymer network (in this case, cellulose) filled with its solvent. A gel can have properties ranging from soft and ductile to hard and brittle. A gel exhibits no flow when in its stable state.
[0065] Step (v), drying the coagulated and washed cellulosic material from step (iv), can be carried out at a temperature between 20 and 90°C, at ambient pressure. It is continued until the resulting cellulosic objects are dry. Alternatively, drying can be carried out by freeze-drying or under supercritical conditions. For freeze-drying, the water-filled cellulosic material is frozen and placed at -80°C at a pressure below 10 mTorr (or approximately 13 mbar). For supercritical drying, the water in the cellulosic material is replaced by ethanol, then by CO₂, at 37°C at a pressure of 80 bar.
[0066] In this way, a material and objects based on cellulose and, possibly, non-cellulosic fibers and / or undissolved cellulose fibers are obtained, with a variable density, ranging from 0.05 to 1.5 g / cm³. 3 , preferably between 0.08 and 1.4g / cm² 3, with controlled porosity, rigidity or elasticity depending on drying conditions, the chosen non-solvent, optional steps and the raw material used.
[0067] Advantageously, the final material obtained can be recycled after use by repeating the process according to the invention, except for step (i) of shredding. However, it will be necessary to grind the material.
[0068] According to a second variant of the process according to the invention, which is particularly advantageous for textiles comprising a blend of fibers, the process includes a step (1T) of separating undissolved residues, notably non-cellulosic fibers, carried out after step (ii) of dissolving the cellulose. This second variant is illustrated in Figure 2.
[0069] This step allows the separation of fibers according to their nature, cellulosic or non-cellulosic, by filtration. Advantageously, the filtration, i.e., the separation of the cellulosic solution from the undissolved fibers, is carried out using a sieve, for example, with a mesh size between 50 µm and 1 mm, particularly less than 300 µm, preferably between 100 and 200 µm. Non-cellulosic fibers do not dissolve. These can be synthetic fibers such as polyester or acrylic fibers, metallic fibers, or other non-cellulosic fibers of natural origin (wool, for example). Furthermore, if cellulosic fibers with a high degree of polymerization are present, these also do not dissolve.
[0070] This filtration step can be followed by a step (ii”) in which the undissolved fibers and dissolved cellulose residues are first washed with a cold aqueous NaOH solution, i.e., at a temperature below 0°C, preferably between 0 and -18°C, and then with water. Preferably, the sodium hydroxide concentration in the aqueous solution is between 6 and 10% by weight. During the water washing, the mixture of water, separated fibers, and residual cellulose is advantageously stirred for 5 to 30 min, preferably 15 min, at a speed between 100 and 1000 rpm, preferably 500 rpm. The water regenerates the dissolved cellulose residues. The non-cellulosic fibers float while the coagulated cellulose residues settle, thus allowing their separation.To achieve this, the mixture of water, non-cellulosic fibers, and cellulosic residues can be filtered again through a sieve (for example, with a mesh size between 20 and 200 µm). The non-cellulosic fibers are rinsed with water and then, if necessary, dried. This yields a co-product: separate, reusable synthetic fibers, either dry or wet. Finally, the washed fibers are dried during step (ii'”). Drying is typically carried out at a temperature between 20 and 80°C, preferably between 40 and 60°C, at ambient pressure. Alternatively, drying can be performed in a vacuum oven.
[0071] The cellulosic portion of the solution is shaped in step (iii). This can be achieved by pressurizing the cellulosic solution through a nozzle (i.e., 3D printing or granulation; see both embodiments). These shaping methods are as described previously for the first variant.
[0072] Step (iv) includes coagulating the shaped cellulose solution and washing the coagulated cellulose material. In the case of 3D printing, the cellulose solution shaped in step (iii) is immersed in a coagulation bath. In the case of granulation, droplets of the solution fall into the coagulation bath. This coagulation bath contains a non-solvent, regardless of the shaping method used.
[0073] The coagulated cellulosic material is washed using a non-solvent agent. This washing removes the NaOH contained in the coagulated cellulosic material.
[0074] The non-solvent, for coagulation as for washing, is as defined previously.
[0075] The process according to the invention may optionally include a gelation step between steps (iii) and (iv). During this optional step, the shaped cellulose solution is gelled until it is "set" in the desired shape. This step can be carried out by maintaining the cellulose solution at a temperature between 20 and 60°C for a period of between 30 minutes and 24 hours. For example, gelation can be achieved by heating at 40°C for 12 hours. Advantageously, the gelation step is carried out at ambient pressure. This optional step is only feasible in the case of shaping by 3D printing.
[0076] Step (v), drying the coagulated and washed cellulosic material from step (iv), is carried out at a temperature between 20 and 90°C until the resulting cellulosic objects are dry. Optionally, drying can be achieved by freeze-drying or under supercritical conditions. For freeze-drying, the water-filled cellulosic material is frozen and placed at -80°C at a pressure below 10 mTorr (or approximately 13 mbar). For supercritical drying, the water in the cellulosic material is replaced first with ethanol, then with CO₂, at 37°C and a pressure of 80 bar. This process yields a material with a variable density between 0.05 and 1.5 g / cm³. 3 , preferably between 0.08 and 1.4 g / cm² 3The process is controlled according to drying conditions, the chosen non-solvent, optional steps, and the raw material used. Advantageously, the final material obtained can be recycled by applying the protocol according to the invention. Not all steps are necessary for recycling the final material, such as shredding. However, the material must be ground prior to the protocol according to the invention.
[0077] EXAMPLES
[0078] The raw materials used are as follows:
[0079] A: Frayed textiles: 100% from the viscose process or 100% from the Lyocell process, with a DP between 200 and 500
[0080] B: 100% cotton frayed textiles, with a DP between 1000 and 6000 (sheets, shirts, t-shirts or jeans with 96% cotton and 4% elastane)
[0081] C: Frayed polycotton (polyester / cotton) textiles, often 50 / 50 or 65 / 35, with a cotton DP between 1000 and 6000
[0082] D: Frayed cotton / polyamide textiles, often 60 / 40 or 80 / 20, with a cotton DP between 1000 and 6000
[0083] E: Textile dust composed of a mixture of cotton, polyester, elastane, polyamide, with a DP of cotton between 1000 and 6000
[0084] Example 1: Process without acid treatment
[0085] In this example, the raw materials used are shredded textiles A and B, which have at least 95% cellulosic fibers.
[0086] The shredded textiles are mixed with a NaOH-water solvent containing 8% NaOH by weight, with stirring for 2 hours at a temperature of -5 °C. A cellulose solution is obtained with a total cellulose concentration, dissolved or undissolved, of between 4 and 12% by weight. The resulting cellulose solution may be translucent if the cellulose concentration is low and the cellulose fibers are completely dissolved. The cellulose solution may be opaque if the cellulose concentration is high and the cellulose fibers are partially dissolved. The cellulose solution is then shaped by 3D printing. The printer used is a CELLINK printer. The parameters used are: a speed of 8 to 20 mm / s, a pressure of 20 to 200 kPa, and a nozzle diameter ranging from 200 µm to 1 mm.
[0087] The shaped cellulose solution is then gelled by maintaining it at 50°C, at ambient pressure for 12 hours until it sets in the desired shape.
[0088] After the shaped cellulose solution has gelled, coagulation is achieved by adding a non-solvent, which can be water. The coagulated cellulose material is washed several times with water until the sodium hydroxide in the cellulose is replaced by the non-solvent.
[0089] Finally, the resulting material is dried at 50°C until completely dry. This yields a cellulose-based object that has been completely dissolved (based on raw material A) or partially dissolved (based on raw material B), transparent (based on raw material A) or opaque (based on raw material B), with a density between 0.05 and 1.5 g / cm³. 3 .
[0090] Example 2: Process with acid treatment
[0091] In this example, the raw materials used are the frayed textiles C and D.
[0092] The frayed textiles are placed in a 0.4 mol / L hydrochloric acid solution at 80°C for 4 hours, then washed with water until neutral. This pretreatment step reduces the degree of cellulose polymerization to a DP between 100 and 400.
[0093] The treated textiles are dissolved under the same conditions as in example 1. The cellulosic solution obtained results from the total dissolution of the cellulosic fibers but is opaque due to the presence of undissolved non-cellulosic fibers.
[0094] The cellulosic solution is shaped by 3D printing under the conditions explained in example 1. The gelation and coagulation of the cellulosic solution, as well as the drying of the resulting material, are carried out under the same conditions as in example 1.
[0095] In this way, an opaque composite object made from regenerated cellulose and non-cellulosic fibers is obtained, with a density between 0.05 and 1.5 g / cm³. 3 The final appearance of the cellulosic object obtained is similar to that of example 1 for raw material B.
[0096] Example 3: Process with acid treatment and filtration - 3D printing
[0097] In this example, the raw materials used are frayed textiles A, B, C and D.
[0098] The shredded textiles are treated as described in example 2. The treated textiles obtained are then dissolved under the same conditions as in example 2. The dissolution of the cellulose is also total for this example but there remain undissolved fibers in the case of raw materials C and D.
[0099] The cellulosic solution is then filtered using a 200 µm mesh sieve to separate the undissolved fibers. This process makes the resulting solution transparent.
[0100] The resulting solution is then shaped by 3D printing under the conditions explained in example 1. The gelation and coagulation of the shaped cellulosic solution, as well as the drying of the resulting cellulosic material, are carried out under the same conditions as in example 1.
[0101] In this way, a transparent object made of regenerated cellulose is obtained. The final cellulosic object has a density between 0.8 and 1.5 g / cm³. 3 The final appearance of the cellulosic object is similar to a piece of PET (polyethylene terephthalate), PP (polypropylene) or cellulose acetate.
[0102] Example 4: Process with acid treatment and filtration - granulation
[0103] In this example, the raw materials used are shredded textiles A, B, C and D. The process implemented is that described in example 3 up to the shaping stage.
[0104] The resulting translucent cellulose solution is shaped by granulation. Droplets are formed using a piston system or a dedicated device on a 3D printer. The solution is forced through a nozzle, forming droplets that fall into a cellulose non-solvent bath where the cellulose material coagulates. The non-solvent bath is distilled water or ethanol. The pressure, nozzle size, distance between the nozzle and the bath, etc., are adjustable depending on the desired final size and shape of the particles. The resulting cellulose material is dried under the same conditions as in Example 1.
[0105] In this way, transparent or opaque beads with a density between 0.8 and 1.5 g / cm³ are obtained. 3The final appearance of the beads is similar to that of PET (polyethylene terephthalate), PP (polypropylene) or cellulose acetate beads.
[0106] Example 5: Process with acid treatment and filtration - 3D printing
[0107] In this example, the raw materials used are shredded textiles A, B, C and D. The process implemented is that described in example 3 up to the shaping stage.
[0108] The resulting translucent cellulose solution is shaped by 3D printing using a CELLINK printer. The parameters used are as follows: a speed of 8 to 20 mm / s, a pressure of 20 to 200 kPa, and a nozzle diameter ranging from 200 µm to 1 mm. The printed cellulose solution is coagulated by placing it in a non-solvent bath, in this case, water. The washing and drying of the coagulated cellulose material are carried out under the same conditions as in Example 1.
[0109] In this way, customizable 3D objects with a density between 0.8 and 1.5 g / cm³ are obtained. 3 The final appearance of cellulosic objects is similar to objects made of PET (polyethylene terephthalate), PP (polypropylene) or cellulose acetate.
[0110] Example 6: Process from textile dust with acid treatment and filtration
[0111] In this example, the raw material used is textile dust E.
[0112] The dust is treated as described in Example 2 with a hydrochloric acid solution. The treated dust is washed to neutralize the acid and mixed with NaOH-water to obtain an 8% NaOH-water concentration, as in Example 1. The resulting solution is the result of the complete dissolution of the cellulose. The cellulose solution is then filtered under the same conditions as in Example 3. Thus, the resulting solution is opaque because it still contains non-cellulosic components.
[0113] The solution is shaped by granulation under the same conditions as in example 4, or by 3D printing under the same conditions as in example 5. The gelation of the cellulosic solution, if it takes place, the coagulation of the cellulosic solution, as well as the drying of the cellulosic material obtained are carried out under the same conditions as in example 1.
[0114] In this way, an opaque object is obtained, composed of regenerated cellulose and possibly non-cellulosic fibers or particles. The final cellulosic object has a density between 0.05 and 1.5 g / cm³. 3 .
Claims
DEMANDS 1. Process for recycling cellulosic textiles comprising the steps of: (i) shredding of cellulosic textiles; (ii) at least partial dissolution of shredded cellulosic textiles in an aqueous solution comprising 6 to 10% by weight of NaOH at a temperature below 0°C to obtain a cellulosic solution; (iii) shaping of the cellulosic solution by 3D printing or by granulation by pressure flow of the cellulosic solution obtained at the end of step (ii) through a nozzle, (iv) coagulation of the shaped cellulose solution and washing of the coagulated cellulose material in a cellulose-free solvent; and (v) drying of coagulated cellulosic material to give a cellulosic object.
2. A recycling process according to claim 1, comprising, between the shredding step (i) and the dissolution step (ii), the following steps: (i') contacting the shredded cellulosic textiles with an aqueous solution of acid to achieve a degree of cellulose polymerization of less than 400; and (i") washing away the acid present in the treated shredded cellulosic textiles.
3. Recycling process according to claim 1 or 2, comprising between step (iii) and (iv) a step (iii') of gelling the cellulosic solution.
4. Recycling process according to any one of claims 1 to 3, wherein the cellulosic textiles comprise cotton, polycotton, viscose or fibers obtained via the lyocell process, alone or in mixture with polyester, polyamide, acrylic, metallic fibers, polyurethane or elastane.
5. A recycling process according to any one of claims 2 to 4, wherein the aqueous acid solution used in step (i') is an aqueous solution comprising 0.1 mol / L to 1 mol / L of hydrochloric or sulfuric acid.
6. A recycling process according to any one of claims 2 to 5, wherein step (i') is carried out at a temperature between 50 and 95 °C, preferably between 70 and 90 °C, for a period of 30 minutes to 6 hours.
7. Recycling process according to any one of claims 1 to 6, comprising after the dissolution step (ii) a step (1T) of separating the undissolved fibers by filtration.
8. Recycling process according to claim 7, wherein the filtration is carried out using a sieve with a mesh size between 50 pm and 1 mm, in particular less than 300 pm, preferably between 100 and 200 pm.
9. Recycling process according to claim 8, wherein the separated fibers obtained at the end of step (ii') are subjected to a step (ii”) in which they are washed first with an aqueous solution of NaOH at a concentration of 6 to 10% by weight at a temperature below 0°C, and then in water.
10. Recycling process according to claim 9, wherein during the water washing in step (ii”), the separated fibers containing residual cellulose are agitated at a speed between 100 and 1000 rpm to remove the coagulated cellulose residues.
11. Recycling process according to claim 9 or 10, wherein the washed separated fibers obtained at the end of step (ii”) are then subjected to a drying step (ii'”).
12. Recycling process according to any one of claims 1 to 11, wherein the coagulation and washing in step (iv) are carried out using a cellulose non-solvent selected from water, distilled water, an aqueous solution of acid, in particular hydrochloric acid at a concentration between 0.01 and 0.5 mol / L, methanol, ethanol and isopropanol.