A fire-resistant glazing

A fire-resistant glazing using specific monomers and cross-linkers in a polymer hydrogel interlayer with inorganic salts addresses stability and performance issues, achieving high fire resistance and efficient cooling in glass laminates.

WO2026234144A1PCT designated stage Publication Date: 2026-11-12PILKINGTON TECH MANAGEMENT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063191
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing fire-resistant glazings, particularly those using hydrogels, face challenges in achieving optimal fire resistance and mechanical stability due to the selection of monomers, cross-linkers, and inorganic salts, which affect their fire performance and water retention capabilities.

Method used

A fire-resistant glazing comprising a laminate of glass panes with a polymer hydrogel interlayer formed by specific monomers, such as acrylamides or methacrylamides with alkyl sulfonic acid groups, and cross-linkers like polyethylene glycol dimethacrylate, along with inorganic salts like magnesium chloride, to create a heat-insulating crust that enhances fire resistance and water vapor release.

Benefits of technology

The solution achieves fire resistance classifications of EI60 or more without additional glass panes or layers, providing lightweight and stable glazings with improved mechanical stability and efficient water vapor cooling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026063191_12112026_PF_FP_ABST
    Figure EP2026063191_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A fire-resistant glazing (10) comprising a laminate of at least two opposing glass panes (11, 12) and at least one fire-resistant layer (13), wherein each fire-resistant layer (13) is an interlayer for two glass panes (11, 12) and is enclosed by a peripheral spacer bar (14) separating the two glass panes (11, 12) adjacent their edges, wherein the at least one fire-resistant layer (13) comprises a polymer hydrogel formed by polymerising a single monomer in water, wherein the single monomer is selected from one of the following groups: I an acrylate, methacrylate or itaconate including an alkyl sulfonic acid group, wherein the alkyl sulfonic acid moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt; and II an acrylamide, methacrylamide or itaconamide including an alkyl sulfonic acid group, wherein the alkyl sulphonic moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] A FIRE-RESISTANT GLAZING

[0002] The present invention relates to a fire-resistant glazing as well as to a method for the manufacture of a fire-resistant glazing.

[0003] In many countries, building regulations exist which specify the fire resistance needed for use of building products, such as doors, windows, or facades, in particular locations.

[0004] A building regulation may, for example, require that a door has a fire classification of E60 -meaning that the door retains its structural integrity so that it forms a barrier to the passage of fire and / or smoke for 60 minutes when it is exposed to fire.

[0005] Alternatively, a building regulation may require that a door has a fire classification of EW60 -meaning that the door must also provide a passage of heat that is no more than 15 kW / m2for 60 minutes when it is exposed to fire.

[0006] Alternatively, a building regulation may require a fire classification of EI60 - meaning that the door completely prevents the passage of heat for 60 minutes when it is exposed to fire.

[0007] A glazing that is used in a building product having a particular fire classification must also have that fire classification. Such glazings are known as fire-resistant glazings.

[0008] Fire-resistant glazings which achieve a fire resistance classification of EW30 or more often comprise two glass panes and a fire-resistant layer wherein the fire-resistant layer is an interlayer for the glass panes.

[0009] In these glazings, the fire-resistant layer is preferably transparent, strongly adhered to the glass panes and is substantially free from optical distortion over the recommended lifetime of the building product.

[0010] A suitable transparent fire-resistant layer comprises a hydrogel containingpolyacrylamides or polyacrylates and one or more inorganic salts, such as sodium chloride or magnesium chloride.

[0011] A fire-resistant glazing having a fire-resistant layer comprising such a hydrogel may be manufactured by the so-called "cast-in-place" (CIP) method.

[0012] In the CIP method, an aqueous solution of one or more monomers and a polymerisation initiator is poured into a cavity formed by an assembly of two opposing glass panes and anear-peripheral spacer bar provided between the glass panes. Thereafter, the cavity is sealed by completing the periphery of the spacer bar and the aqueous solution is cured to a solid or semi-solid hydrogel layer in the sealed cavity by exposure of the glazing to heat and / or to visible and / or UV light.

[0013] The assembly may comprise three or more glass panes and two or more near-peripheral spacer bars such that it provides two or more solid hydrogel layers in the same way at the same time. A secondary circumferential seal may be provided adjacent the outer edge of the circumferential spacer bar after the curing.

[0014] Fire-resistant glazings manufactured in this way may be described as a one, two or three CIP-cell glazing wherein the number corresponds to the number of fire-resistant layers.

[0015] In fire-resistant glazings of this type, the polymer hydrogel releases water vapour and burns so that a heat insulating crust is formed on the gel. The heat insulating crust, which consists largely of inorganic salts, protects the remainder of the gel from the fire whilst also permitting the release of more water vapour so cooling the glass pane further from the fire side.

[0016] Fire-resistant glazings of this type can achieve a fire resistance classification of EI60 or more without the need for additional glass panes or multiple fire-resistant layers.

[0017] Such fire-resistant glazings are relatively light as compared to fire-resistant glazings requiring multiple layers of an alkali metal silicate. The fire-resistant layer has normally to be adhered to the glass panes by a coating and so is not susceptible to the slumping which can limit the thickness of a fire-resistant layer based on an alkali metal silicate.

[0018] International patent publication WO 2017 / 137148 Al discloses a fire protection gel containing a polymer produced from polymerizing sulfonated derivates of unsaturated aliphatic carboxylic acids as monomers and water.

[0019] Whilst this application refers to examples, in which the monomer mixture includes specified amounts of monomers, cross linker, and inorganic salts, the application is silent as to the resistance to fire performance which can be achieved by fire-resistant glazings including the fire protection gel.

[0020] The present inventors have found that the resistance to fire performance of fire-resistant glazings including this fire protection gel is highly dependent on the selection of the monomer, fire-resistance is also further improved by the selection of the cross linker as well as theselection of the relative amounts of inorganic salts.

[0021] The selection of the monomer and the cross-linker (including relative amounts) influences the mechanical stability of the fire protection gel and its ability to hold water.

[0022] In a first aspect, therefore, the present invention provides a fire-resistant glazing comprising a laminate of at least two opposing glass panes and at least one fire-resistant layer, wherein each fire-resistant layer is an interlayer for two glass panes and is enclosed by a peripheral spacer bar separating the two glass panes adjacent their edges, wherein the at least one fire-resistant layer comprises a polymer hydrogel formed by polymerising a single monomer in water, wherein the single monomer is selected from one of the following groups:

[0023] I an acrylate, methacrylate or itaconate including an alkyl sulfonic acid group, wherein the alkyl sulfonic acid moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt; and

[0024] II an acrylamide, methacrylamide or itaconamide including an alkyl sulfonic acid group, wherein the alkyl sulphonic moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt.

[0025] Suitable monomers of groups I and II include 3-(acryloyloxy)propane-l-sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, 3-(methacryloyloxy)propane-l-sulfonate, 4-[[2-(methacryloyloxy)ethyl]dimethylammonio]-butane-l-sulfonate, 3-((3-methacrylamidopropyl)-dimethylammonio)propane-l-sulfonate, and bis(3-sulfoproproyl) itaconate, preferably as potassium or sodium salt.

[0026] Preferably, the single monomer is selected from group II.

[0027] Preferably, however, the monomer is 2-acrylamido-2-methylpropane sulfonic acid, this is preferably in tha form of an alkali metal salt which is more preferably the sodium salt (NaAMPS).

[0028] Optionally, though not preferably the alkyl sulfonic acid moiety comprises 1 to 4 carbon atoms and has a nitrogen atom (especially a quaternary nitrogen atom) along the backbone of carbon atoms. More preferably, the alkyl sulfonic acid moiety has 1 to 4 carbon atoms and only carbon atoms and hydrogen atoms along the backbone of the alkyl group along with the sulfonic acid group or groups.

[0029] In embodiments, the at least one fire-resistant layer comprises from 5% to 15% by weight of polymerised monomer.

[0030] In preferred embodiments, the at least one fire-resistant layer is formed by polymerisation ofthe monomer and a cross-linker, preferably ensuring that the polymer is a solid or semi-solid hydrogel. Preferably, the cross linker comprises one or more of methylene bisacrylamide, a polyethylene glycol dimethacrylate) or a polyethylene glycol diacrylate), preferably a polyethylene glycol dimethacrylate) or a polyethylene glycol diacrylate) having a mean molar mass from 200 g / mol to 8000 g / mol.

[0031] The cross-linker may, in particular, comprise one or more of polyethylene glycol dimethacrylate) 8000 (g / mol), poly(ethylene glycol dimethacrylate) 750 (g / mol), poly(ethylene glycol dimethacrylate) 600 (g / mol), poly(ethylene glycol diacrylate) 600 (g / mol), poly(ethylene glycol diacrylate) 400 (g / mol) and poly(ethylene glycol diacrylate) 200 (g / mol).

[0032] In preferred embodiments, the at least one fire-resistant layer generally comprises from 5% to 15% by weight of polymerised monomer, and preferably from 0.05% to 2.0%, in particular, from 0.05% to 1.5% by weight of crosslinker, especially where the cross-linker is methylene bisacrylamide, a poly(ethylene glycol di methacrylate) or a poly(ethylene glycol diacrylate), preferably, more especially where the cross-linker is a poly(ethylene glycol dimethacrylate) or a poly(ethylene glycol diacrylate) having a mean molar mass from 200 g / mol to 8000 g / mol.

[0033] In some embodiments, the at least one fire-resistant layer comprises at least one inorganic salt, preferably providing a heat insulating crust on the polymer when the fire-resistant glazing is exposed to fire.

[0034] Preferably, the fire-resistant layer comprises magnesium chloride and sodium chloride (as the inorganic salts).

[0035] Suitable inorganic salts include (or comprise) one or more of sodium chloride, potassium chloride, calcium chloride, magnesium chloride and zinc chloride - as well as the corresponding bromides and iodides.

[0036] In preferred embodiments, the at least one fire-resistant layer comprises from 10% to 22% by weight of at least one inorganic salt (preferably calculated as anhydrous salt). This content of inorganic salt includes the inorganic ion which originates from the monomer as well as inorganic salt which is added to the mixture of monomer and water.

[0037] The at least one fire-resistant layer may also comprise one or more of a foaming agent, preferably regulating the transport of water vapour through the heat insulating crust.

[0038] Suitable foaming agents include inorganic salts such as potassium azide, sodium azide, potassium nitrite, sodium nitrite, potassium nitrate, sodium nitrate, ammonium nitrate,ammonium carbonate as well as urea, citric acid, ascorbic acid, and tartaric acid and, as the case may be, their sodium or potassium salts.

[0039] When the at least one fire-resistant layer includes a foaming agent comprising one or more inorganic salt or organic salt, the total amount thereof may be less than or equal to 5% by weight of the inorganic salts - but when the at least one fire-resistant layer includes a foaming agent comprising urea or an organic acid, the total amount of organic acid may be less than or equal to 5% by weight, for example, 2% by weight of the fire-resistant layer.

[0040] The inventors have also found that the selection of the relative amounts of inorganic salts influences the ability of the crust that is formed to release water from the fire protection gel towards the fire side of the glazing.

[0041] In preferred embodiments, therefore, the fire-resistant layer has a molar ratio of sodium ion and / or potassium ion to magnesium ion from 3:1 to 1:3, preferably from 2.5 to 1:1 and most preferably about 2.3:1, for example, from 2.1:1 to 2.5:1. Other preferred molar ratios of sodium ion and / or potassium ion to magnesium ion are from 2.0:1 to 3.0:1, from 2.1:1 to 2.8:1 and from 2.1:1 to 2.7:1. Preferably, these ratios relate to the molar ratios of sodium ions to magnesium ions. The mixture may also include calcium ion in an amount not exceeding 2% by weight of the inorganic salts.

[0042] The at least one fire-resistant layer may also comprise, up to 10% by weight of an organic solvent, more especially a water miscible organic solvent, typically this will be in place of some of the water. Suitable water miscible organic solvents include ethylene glycol, glycerol, diethylene glycol, methanol, ethanol, and isopropanol.

[0043] The at least one fire-resistant layer may also comprise one or more of a water soluble polymerisation inhibitor or a water soluble UV light stabiliser, such as 4-hydroxy-2, 2,6,6-tetramethypiperidin-l-oxyl, which may be present in the monomer which is commercially available or added to the monomer.

[0044] The polymerisation inhibitor or UV light stabiliser acts to prevent premature polymerisation of the mixture and discolouring of the fire-resistant layer by auto-oxidation - but preferably should not be present to an extent (for example, above 100 ppm) that the at least one fire-resistant layer comprises more than 10% by weight of unpolymerized monomer.

[0045] The at least one fire-resistant layer may include other additives ensuring that its pH is about 7.0. A pH below about 6.0 may lead to hydrolysis of the polymer hydrogel whilst a pHabove about 8.0 may lead to precipitation of inorganic salts, especially magnesium hydroxide.

[0046] The remaining content of the at least fire-resistant layer may be made up by water. In the most preferred embodiments, the at least one fire-resistant layer has a water content from 55% to 80% by weight, and in particular, from 65% to 75% by weight, for example, from 70% to 75% by weight.

[0047] In a particularly preferred embodiment, the at least one fire-resistant layer comprises from 9% to 14% by weight of sodium 2-acrylamido-2-methylpropane sulfonate, and preferably from 0.05% to 2.0% by weight of methylene bisacrylamide, or polyethylene glycol diacrylate) having a mean molar mass of 200 g / mol or 400 g / mol or 600 g / mol, or poly(ethylene glycol dimethacrylate) having a mean molar mass of 8000 g / mol, and preferably from 7% to 12% by weight of sodium chloride, from 7% to 12% by weight of magnesium chloride and 0.001% to 0.05% by weight of an initiator.

[0048] The weight ratio of sodium ion to magnesium ion in the at least one fire-resistant layer is preferably about 2:3.

[0049] At least one glass pane may have a coating on an interior surface thereof for adhering the polymer hydrogel to the at least one glass pane. Preferably, the coating is provided on the interior surface of the at least one glass pane which is on the cold side of the fire-resistant glazing in use.

[0050] The coating may comprise a primer or adhesion promoter which can bond to glass but optionally does not bind covalently to the polymer or binds only to a limited extent. Suitable primers or adhesion promoters include silanes having a primary amine group and / or a secondary amine group, or an epoxy group or a vinyl group.

[0051] The coating may, in particular, comprise one or more of 3-a mi nopropyltriethoxysilane (for example, Dynasylan® AMEO from Evonik Industries), N-2-aminoethyl-3-aminopropyl-triethoxysilane (for example, Dynasylan® DAMO from Evonik Industries), 3-(2,3-epoxy-propoxy)propyltrimethoxysilane (for example, Primer 4299 from 3M), or vinyltri methoxysilane (for example, Dynasylan® VTMO from Evonik Industries), or an aqueous oligomeric aminoalkyl- and vinyl-functional silane hydrolysate (for example, Dynasylan® HYDROSIL 2907 from Evonik Industries).

[0052] The present inventors have also found that the ratio of salts providing for optimal release of water vapour from the crust can lead to the formation and coalescence of water vapour bubbles on the cold side of the fire-resistant glazing. And that the accompanying build-up of pressure there may lead to separation of at least part of the polymer from the interior surfaceof the pane (possibly, even if it is provided with one or more of the silanes) and early exhaustion of the fire-resistant layer.

[0053] Preferably, therefore, the coating comprises a primer or adhesion promoter which covalently bonds to the polymer. Suitable primers or adhesion promoters include silanes comprising one or more of an acrylate or a methacrylate group.

[0054] Preferably, the coating comprises a silane including (within its chemical structure) one or more of an acrylate, a methacrylate, a primary amine, a secondary amine, an epoxy, or a vinyl group.

[0055] In preferred embodiments, the coating comprises one or more of (preferred silanes which are or comprise) 3-methacryl-oxypropyltrimethoxysilane (for example, KBM-503 from Shin-Etsu or Dynasylan® MEMO from Evonik Industries), 3-methacryloxypropyltriethoxysilane (for example, KBE-503 from Shin-Etsu), and 8-methacryloxyoctyltrimethoxysilane (for example, KBM-5803 from Shin-Etsu), 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxy-silane, vinyltri methoxysilane, 3-(2,3-epoxypropoxy) propyltrimethoxysilane, or an aqueous oligomeric aminoalkyl- and vinyl-functional silane hydrolysate. In the most preferred embodiments, however, the coating comprises 3-methacryloxypropyltrimethoxysilane or 3-methacryloxypropyltriethoxysilane.

[0056] In some embodiments, the coating may also comprise a base layer on which the primer or adhesion promoter is to be applied. Suitable base layers comprise one or more of the metal oxides and metal nitrides described in EP 2 760 665 Bl. Preferably, the base layer comprises silica, silicon nitride or silicon oxynitride, but it may alternatively comprise hafnium

[0057] oxide, vanadium oxide, niobium oxide, zinc nitride, tin nitride, hafnium nitride, vanadium nitride or niobium nitride.

[0058] Preferred coatings comprise at least one metal oxide or nitride.

[0059] In some embodiments, the interior surface on which the coating is provided is a surface which has been plasma treated or flame treated, preferably so as to enhance covalent bonding of the primer or adhesion promotor or the base layer. Preferably, at least one pane is plasma treated or flame treated on an interior surface thereof.

[0060] The glass panes may be formed from any suitable glass. Suitable glasses include alkali silicate glass, alkali borosilicate glass and alkali aluminosilicate glass as well as ceramic glasses such as that sold by Nippon Electric Glass Company under the trade name Firelite®.

[0061] In preferred embodiments, the glass is a soda-lime glass, such as a float glass. In that case,the interior surface upon which the coating for adhering the polymer hydrogel is applied is preferably The "tin side" of the glass. The phrase "tin side" refers to float glass made using molten tin and the tin side is the side of the float glass facing the molten tin during production. The tin may be present in the float glass in the form of metallic tin and / or in the form of tin oxide. In these and other embodiments, each of the glass panes may be heat-strengthened, chemically strengthened or a fully toughened. Preferaby, each glass pane is a toughened float glass.

[0062] The fire-resistant glazing may also include a coating, such as an anti-reflective coating, an antibacterial coating, an antiviral coating, an easy clean coating, or a self-cleaning coating on an exterior surface of one or each outer glass pane. Float glass panes having an anti-reflective coating are sold under the trade name Optiview™ and float glass panes having a self-cleaning coating are sold under the trade names Activ™ and SaniTise™.

[0063] The peripheral spacer bar which encloses each fire-resistant layer extends along the sides of the glass panes which it separates. The spacer bar may comprise a thermoplastic polymer, such as polyisobutylene, and / or a metal, such as aluminium or steel, preferably the metal is protected against corrosion from the fire-resistant layer.

[0064] Preferably, however, the peripheral spacer bar comprises a fibre-reinforced composite material, such as a glass fibre-reinforced polyurethane or a glass fibre-reinforced polyester or a glass fibre-reinforced vinyl ester resin.

[0065] In these and other embodiments, each of the glass panes may have a thickness from 4 mm to 12 mm, in particular, from 5 mm to 8 mm. The at least one fire-resistant layer may have a thickness from 2 mm to 45 mm.

[0066] In the most preferred embodiments, the fire-resistant glazing comprises a single fire-resistant layer. The single fire-resistant layer may have a thickness greater than or equal to 6 mm, or 18 mm or 25 mm or 30 mm or 45 mm. The single fire-resistant layer may have a thickness of from 6 mm to 45 mm.

[0067] In some embodiments, the fire-resistant glazing incorporates a safety glazing. Preferably, at least one glass pane is a safety glazing.

[0068] In these embodiments, a safety glazing is used in place of at least one glass pane so that the fire-resistant glazing comprises at least three glass panes, at least one fire-resistant layer and at least one adhesive plastics film wherein the fire-resistant layer and the adhesive plastics film are interlayers for two glass panes.The adhesive plastics film may be selected from any of those known for use in safety glazings. Preferably, the adhesive plastics film is transparent. It may, in particular, comprise one or more layers of a polyvinyl acetal, especially a polyvinyl butyral, an ionomer, a polyethylene vinyl acetate, a polyurethane, a polycarbonate or an acrylic resin.

[0069] In other embodiments, the fire-resistant glazing includes a polymer layer which greatly enhances the impact resistance of the glazing. In these embodiments, the polymer layer may be provided by curing a mixture of monomers alongside the curing of the mixture providing the fire-resistant layer. In any case, the fire-resistant glazing comprises at least three glass panes, at least one fire-resistant layer and at least one polymer layer wherein the fire-resistant layer and the polymer layer are interlayers for two glass panes.

[0070] The polymer layer may be selected from any of those known for use in anti-theft glazings, blast resistance glazing or bullet proof glazings. Preferably, it is transparent. It may, in particular, comprise an epoxy resin, a polyacrylate, a polycarbonate or a polyurethane, and, optionally at least one fire retardant additive.

[0071] In these embodiments, the thickness of the adhesive plastics film or the polymer layer may be between 0.1 mm and 10 mm, for example, less than 5 mm or 1 mm.

[0072] In still other embodiments, the fire-resistant glazing incorporates an integrated glazing unit (IGU). In these embodiments, an IGU is used in place of at least one glass pane so that the fire-resistant layer comprises at least three glass panes, at least one fire-resistant layer and at least one gas layer, wherein the at least one fire-resistant layer and the at least one gas layer are interlayers for two glass panes.

[0073] In these embodiments, the fire-resistant glazing may also have a low emissivity coating on an outward facing surface or inward facing surface of one or each inner glass pane of the IGU. Float glass panes having a low emissivity coating are sold under the trade name K Glass™ and Suncool™.

[0074] In these embodiments, the IGU may comprise a double or triple glazing unit in which the glass panes are separated by a gap containing a vacuum, or air, or an inert gas. The IGU may also include one or more of the exterior coatings mentioned above.

[0075] In embodiments in which there is a single fire-resistant layer, the fire-resistant glazing achieves EW 30 or above when tested in accordance with EN 1634-1 (2014) or EN 13501-1 (2016).

[0076] In other such embodiments, in which the fire-resistant layer has a thickness of about 10 mmor about 18 mm, the fire-resistant glazing achieves respectively El 30 or El 60 when tested in accordance with EN 1634-1 (2014) or EN 13501-1 (2016).

[0077] In further such embodiments, in which the fire-resistant layer has a thickness of about 25 mm, or about 30 mm or about 45 mm, the fire-resistant glazing may achieve respectively El 90 or El 120 or El 180 when tested in accordance with EN 1634-1 (2014) or EN 13501-1 (2016).

[0078] The fire-resistant glazing also offers excellent reaction to fire performance and may conform to A2-sl, dl determined according to EN 13501-2 (2016). It may alternatively or additionally conform to A0, A15, A30, A60, B0 or B15 measured according to International Maritime Organisation standard IMO A.754(18). Furthermore, the fire-resistant glazing may conform to Al-15, Al-30, A2-15, or A2-30 measured according to European standard (railway vehicles) EN 45545-3.

[0079] In a second aspect, the present invention provides a method for the production of a fire-resistant glazing comprising a laminate of at least two transparent glass panes and at least one transparent fire-resistant layer, the method comprising pouring a mixture comprising a single monomer and water into a cavity provided by a peripheral spacer bar located adjacent the edges of two opposing transparent glass panes, sealing the peripheral spacer bar and allowing the mixture to polymerise in the cavity to form a polymer hydrogel, wherein the single monomer is selected from one of the following groups:

[0080] I an acrylate, methacrylate or itaconate including an alkyl sulfonic acid group, wherein the alkyl sulfonic acid moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt; and

[0081] II an acrylamide, methacrylamide or itaconamide including an alkyl sulfonic acid group, wherein the alkyl sulphonic moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt.

[0082] Suitable monomers of group I and II include 3-(acryloyloxy)propane-l-sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, 3-(methacryloyloxy)propane-l-sulfonate, 4-[[2-(methacryloyloxy)ethyl]dimethylammonio]-butane-l-sulfonate, 3-((3-methacrylamidopropyl)-dimethylammonio)propane-l-sulfonate, and bis(3-sulfoproproyl) itaconate, preferably as a potassium or a sodium salt. Preferably, however, the monomer is 2-acrylamido-2-methylpropane sulfonic acid, preferably in the form of an alkali metal salt which is more preferably the sodium salt (NaAMPS).

[0083] Preferably, the single monomer is selected from group II.In embodiments, the mixture may comprise from 5% to 15% by weight of monomer. In preferred embodiments, the mixture further comprises a cross linker, preferably ensuring that the polymer is a solid or semi-solid hydrogel.

[0084] Preferably, the cross-linker comprises one or more of methylene bisacrylamide, or a polyethylene glycol dimethacrylate) or a polyethylene glycol diacrylate). Preferably polyethylene glycol dimethacrylate) or a polyethylene glycol diacrylate having a mean molar mass of between 200 g / mol and 8000 g / mol.

[0085] The cross-linker may, in particular, comprise one or more of polyethylene glycol dimethacrylate) 8000 (g / mol), poly(ethylene glycol dimethacrylate) 750 (g / mol), poly(ethylene glycol dimethacrylate) 600 (g / mol), poly(ethylene glycol diacrylate) 600 (g / mol), poly(ethylene glycol diacrylate) 400 (g / mol) and poly(ethylene glycol diacrylate) 200 (g / mol).

[0086] In preferred embodiments, the mixture generally comprises from 5% to 15% by weight of monomer, and preferably from 0.05% to 2.0% by weight of one or more cross-linker. Preferably the cross-linker is a poly(ethylene glycol dimethacrylate) or a poly(ethylene glycol diacrylate) having a mean molar mass from 200 g / mol to 8000 g / mol or methylene bisacrylamide.

[0087] In some embodiments, the mixture further comprises at least one inorganic salt providing a heat insulating crust on the polymer when the fire-resistant glazing is exposed to fire.

[0088] Suitable inorganic salts include (or comprise) sodium chloride, potassium chloride, calcium chloride, magnesium chloride and zinc chloride - as well as the corresponding bromides and iodides.

[0089] In preferred embodiments, the at least one fire-resistant layer comprises from 10% to 22% by weight of at least one inorganic salt (preferably calculated as anhydrous salt). This content of inorganic salt includes the inorganic ion which originates from the monomer as well as the at least one inorganic salt which are added to the mixture. The mixture may also comprise one or more of a foaming agent, preferably regulating the transport of water vapour through the heat insulating crust.

[0090] Suitable foaming agents include inorganic salts such as potassium azide, sodium azide, potassium nitrite, sodium nitrite, potassium nitrate, sodium nitrate, ammonium nitrate, ammonium carbonate as well as urea, citric acid, ascorbic acid, and tartaric acid and, as the case may be, their sodium or potassium salts.

[0091] When the mixture includes a foaming agent comprising one or more inorganic salt or organicsalt, the total amount thereof may be less than or equal to 5% by weight of the inorganic salts - but when the at least one fire-resistant layer includes a foaming agent comprising urea or an organic acid, the total amount of organic acid may be less than or equal to 5% by weight, for example, 2% by weight of the fire-resistant layer.

[0092] In preferred embodiments, therefore, the mixture has a molar ratio of sodium and / or potassium ion to magnesium ion from 3:1 to 1:3, preferably from 2.5 to 1:1 and most preferably about 2.3:1, for example, from 2.1:1 to 2.5:1. Preferably, these ratios relate to the molar ratios of sodium ions to magnesium ions. The mixture may also include calcium ion, preferably in an amount not exceeding 2% by weight of the inorganic salts.

[0093] The mixture may also comprise, in place of water, up to 10% by weight of an organic solvent, especially a water miscible organic solvent. Suitable water miscible organic solvents include ethylene glycol, glycerol, diethylene glycol, methanol, ethanol, and isopropanol.

[0094] In that case, the mixture may comprise from 5% to 15% by weight of monomer, preferably from up to 10% by weight of the organic solvent, and from 0.2% to 1.5% by weight of cross linker.

[0095] The mixture may also comprise a polymerisation initiator. Suitable polymerisation initiators may be redox initiators such as sodium persulfate and triethanolamine or ammonium persulfate and N,N,N,N-tetramethylethylenediamine (TMEDA) or UV initiators such as 1-hydroxycyclohexyl phenyl ketone (generally used in amounts up to 0.01% by weight of the mixture).

[0096] Preferably, however, the polymerisation initiator is a thermal initiator, and in particular, a water soluble azo initiator. The azo initiator provides a near complete polymerization, especially when it is present in the mixture in an amount not exceeding 0.005% by weight - without leaving bubbles in the fire-resistant layer. Suitable azo initiators include 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride and 2,2-azobis(2-methylpropionamidine) which are sold under the trade names VA-044 and V-50 respectively.

[0097] In any case, the method may comprise allowing the mixture to polymerise in the sealed cavity with heating to a temperature of about 70°C or about 80°C.

[0098] The mixture may also comprise one or more polymerisation inhibitors or a UV light stabilisers, such as 4-hydroxy-2,2,6,6-tetramethypiperidin-l-oxyl, which may be present in the commercially available monomer or is added to the mixture.The polymerisation inhibitor or UV light stabiliser may act to prevent premature polymerisation of the mixture and discolouring of the fire-resistant layer by autooxidation - but preferably should not be present to an extent that the at least one fire-resistant layer comprises more than 10% by weight of unpolymerized monomer.

[0099] The mixture may include other additives ensuring that the pH of the fire-resistant layer is about 7.0. A pH which below about 6.0 may lead to an hydrolysis of polymer hydrogel whilst a pH above about 8.0 may lead to precipitation of inorganic salts, especially magnesium hydroxide.

[0100] The remaining content of the mixture may be made up by water. In the most preferred embodiments, the mixture has a water content from 55% to 80% by weight, and in particular, from 65% to 75%, for example, from 70% to 75% by weight.

[0101] In a particularly preferred embodiment, the mixture comprises from 9% to 14% by weight of sodium 2-acrylamido-2-methylpropane sulfonate, from 0.05% to 2.0% by weight of methylene bisacrylamide, or poly(ethylene glycol diacrylate) having a mean molar mass of

[0102] 200 g / mol or 400 g / mol or 600 g / mol, or poly(ethylene glycol dimethacrylate) having a mean molar mass of 8000 g / mol, from 7% to 12% by weight of sodium chloride, from 7% to 12% by weight of magnesium chloride and 0.001% to 0.05% by weight of an initiator. The weight ratio of sodium ion to magnesium ion in the at least one fire-resistant about 2:3.

[0103] At least one glass pane may have a coating on an interior surface thereof for adhering the polymer hydrogel to the at least one glass pane. Preferably, the coating is provided on the interior surface of the at least one glass pane which is on the cold side of the fire-resistant glazing in use.

[0104] The coating may comprise a primer or adhesion promoter which can bond to glass but optionally does not bind covalently to the polymer or binds only to a limited extent. Suitable primers or adhesion promoters include silanes having a primary amine group and / or a secondary amine group, or an epoxy group or a vinyl group.

[0105] The coating may, in particular, comprise one or more of 3-a mi nopropyltriethoxysilane (for example, Dynasylan® AMEO from Evonik Industries), N-2-aminoethyl-3-aminopropyl-triethoxysilane (for example, Dynasylan® DAMO from Evonik Industries), 3-(2,3-epoxy-propoxy)propyltrimethoxysilane (for example, Primer 4299 from 3M), or vinyltri methoxysilane (for example, Dynasylan® VTMO from Evonik Industries), or an aqueous oligomeric aminoalkyl- and vinyl-functional silane hydrolysate (for example, Dynasylan® HYDROSIL 2907 from Evonik Industries).Preferably, however, the coating comprises a primer or adhesion promoter which covalently bonds to the polymer. Suitable primers or adhesion promoters include silanes comprising one or more of an acrylate or a methacrylate group. Preferably, the coating comprises a silane including (within its chemical structure) one or more of an acrylate, a methacrylate, a primary amine, a secondary amine, an epoxy, or a vinyl group.

[0106] In preferred embodiments, therefore, the coating comprises one or more of (preferred silanes which are or comprise) 3-methacryl-oxypropyltrimethoxysilane (for example, KBM-503 from Shin-Etsu or Dynasylan® MEMO from Evonik Industries), 3-methacryloxypropyltriethoxysilane (for example, KBE-503 from Shin-Etsu), and 8-methacryloxyoctyltrimethoxysilane (for example, KBM-5803 from Shin-Etsu) 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxy-silane, vinyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, or an aqueous oligomeric aminoalkyl- and vinylfunctional silane hydrolysate.. Most preferably, however, the coating comprises 3-methacryloxypropyltrimethoxy-silane or 3-methacryloxypropyltriethoxysilane.

[0107] In some embodiments, the coating may comprise a base layer on which the primer or adhesion promoter has been applied. Suitable base layers comprise one or more of the metal oxides and metal nitrides described in EP 2 760 665 Bl. Preferably, the base layer comprises silica, silicon nitride or silicon oxynitride, but it may alternatively comprise hafnium oxide, vanadium oxide, niobium oxide, zinc nitride, tin nitride, hafnium nitride, vanadium nitride or niobium nitride. Preferably, the coating comprises at least one metal oxide or metal nitride.

[0108] In some embodiments, the interior surface on which the coating is provided is a surface of a glass pane which has been plasma treated or flame treated. Preferably, at least one pane is plasma treated or flame treated on an interior surface thereof.

[0109] The glass panes may be formed from any suitable glass. Suitable glasses include alkali silicate glass, alkali borosilicate glass and alkali aluminosilicate glass as well ceramic glasses such as that sold by Nippon Electric Glass Company under the trade name Firelite®.

[0110] In preferred embodiments, the glass is a soda-lime glass, such as a float glass. In that case, the interior surface upon which the coating for adhering the polymer hydrogel is applied is preferably the "tin side" of the glass. The "tin side" has the same meaning as previously mentioned. In these and other embodiments, each of the glass panes may be heat-strengthened, chemically strengthened or a fully toughened. Preferaby, each glass pane is a toughened float glass.

[0111] The method may provide that the fire-resistant glazing includes a coating, such as an anti-reflective coating, an antibacterial coating, an antiviral coating, an easy clean coating, or a self-cleaning coating on an exterior surface of one or each outer glass pane. Float glass panes having an anti-reflective coating are sold under the trade name Optiview™ and float glass panes having a self-cleaning coating are sold under the trade names Activ™ and SaniTise™.

[0112] The peripheral spacer bar which encloses each fire-resistant layer extends along the sides of the glass panes which it separates. The spacer bar may comprise a thermoplastic polymer, such as polyisobutylene, a metal, such as aluminium or steel. Preferably, however, the peripheral spacer bar comprises a fibre-reinforced composite material, such as a glass fibre-reinforced polyurethane or a glass fibre-reinforced polyester or a glass fibre-reinforced vinyl ester resin.

[0113] In these and other embodiments, each of the glass panes may have a thickness from 4 mm to 12 mm, in particular, from 5 mm to 8 mm. The at least one fire-resistant layer may have a thickness between 2 mm and 35 mm. Preferably, however, the thickness of the fire-resistant layer is greater than or equal to 10 mm, or 18 mm, or 25 mm, or 30 mm.

[0114] In these and other embodiments, each of the glass panes may have a thickness from 4 mm to 12 mm, in particular, from 5 mm to 8 mm. The at least one fire-resistant layer may have a thickness from 2 mm to 45 mm.

[0115] In a preferred embodiment, the method provides a fire-resistant glazing comprises a single fire-resistant layer. The single fire-resistant layer may have a thickness greater than or equal to 6 mm, or 18 mm or 25 mm or 30 mm or 45 mm. Preferably, single fire-resistant layer has a thickness of from 6 mm to 45 mm.

[0116] In some embodiments, the method provides a fire-resistant glazing incorporating a safety glazing. Preferably, at least one glass pane is a safety glazing. In these embodiments, a safety glazing is used in place of at least one glass pane

[0117] so that the fire-resistant glazing comprises at least three glass panes, at least one fire-resistant layer and at least one adhesive plastics film wherein the fire-resistant layer and the adhesive plastics film are interlayers for two glass panes.

[0118] The adhesive plastics film may be selected from any of those known for use in safety glazings. Preferably, the adhesive plastics film is transparent. It may, in particular, comprise one or more layers of a polyvinyl acetal, especially a polyvinyl butyral, an ionomer, a polyethylene vinyl acetate, a polyurethane, a polycarbonate or an acrylic resin.In other embodiments, the method provides a fire-resistant glazing including a polymer layer which greatly enhances the impact resistance of the glazing. In these embodiments, the polymer layer may be provided by curing a mixture of monomers alongside the curing of the mixture providing the fire-resistant layer. In any case, the fire-resistant glazing comprises at least three glass panes, at least one fire-resistant layer and at least polymer layer wherein the fire-resistant layer and the polymer layer are interlayers for two glass panes.

[0119] The polymer layer may be selected from any of those known for use in anti-theft glazings, blast resistance glazing or bullet proof glazings. Preferably, it is transparent. It may, in particular, comprise an epoxy resin, a polyacrylate, a polycarbonate or a polyurethane, and, optionally at least one fire retardant additive.

[0120] In these embodiments, the thickness of the adhesive plastics film or the polymer layer may be between 0.1 mm and 10 mm, for example, less than 5 mm or 1 mm.

[0121] In still other embodiments, the method provides a fire-resistant glazing incorporating an integrated glazing unit (IGU). In these embodiments, an IGU is used in place of at least one glass pane so that the fire-resistant layer comprises at least three glass panes, at least one fire-resistant layer and at least one gas layer, wherein the at least one fire-resistant layer and the at least one gas layer are interlayers for two glass panes.

[0122] In these embodiments, the method may also provide that the fire-resistant glazing has a low emissivity coating on an outward facing surface or inward facing surface of one or each inner glass pane of the IGU. Float glass panes having a low emissivity coating are sold under the trade name K Glass™ and Suncool™.

[0123] In these embodiments, the IGU may comprise a double or triple glazing unit in which the glass panes are separated by a gap containing a vacuum, or air, or an inert gas. The IGU may also include one or more of the exterior coatings mentioned above.

[0124] In preferred embodiments, the method provides a fire-resistant glazing having a single fire-resistant layer.

[0125] In these embodiments, the method provides a fire-resistant glazing which achieves EW 30 or above when tested in accordance with EN 1634-1 (2014) or EN 13501-1 (2016). In other such embodiments, in which the fire-resistant layer has a thickness of about 10 mm or about 18 mm, the fire-resistant glazing achieves respectively El 30 or El 60 when tested inaccordance with EN 1634-1 (2014) or EN 13501-1 (2016).

[0126] In further such embodiments, in which the fire-resistant layer has a thickness of about 25 mm, or about 30 mm or about 45 mm, the fire-resistant glazing may achieve respectively El 90 or El 120 or El 180 when tested in accordance with EN 1634-1 (2014) or EN 13501-1 (2016).

[0127] The method offers a fire-resistant glazing having a fire performance which may conform to A2-sl, dl determined according to EN 13501-2 (2016). The fire-resistant glazing may alternatively or additionally conform to A0, A15, A30, A60, B0 or B15 measured according to International Maritime Organisation standard IMO A.754(18). Furthermore, the fire-resistant glazing may conform to Al-15, Al-30, A2-15, or A2-30 measured according to European standard (railway vehicles) EN 45545-3.

[0128] In a third aspect, the present invention provides use of a fire-resistant glazing according to the first aspect or prepared by the method according to the second aspect for incorporation into a building product such as a door, a window, a partition, or a fagade for a building, a ship, a car or a train.

[0129] Referring now to Figure 1, a fire-resistant glazing 10 according to the present invention comprises a single CIP cell. The CIP cell includes two toughened float glass panes 11, 12 of dimensions 1.5 m x 3.0 m x 5 mm and a single fire-resistant interlayer 13 between the two panes 11, 12. Figure 1 is schematic only and is not drawn to scale. No measurements or ratios can be ascertained from this schematic.

[0130] A circumferential spacer bar 14 surrounds the fire-resistant interlayer 13. The spacer bar 14 has a thickness separating the glass panes 11, 12 of 18 mm and is located 10 mm from their edges. A secondary sealant 15 comprises a polysulphide, a polyurethane, or a silicone, and seals the gap between the spacer bar 14 and the edges of the glass panes 11, 12. The overall thickness of the fire-resistant glazing is 28 mm to 29 mm, and its total weight is about 50 kg / m2.

[0131] The fire-resistant glazing 10 is manufactured by a convergent processes in which a first process prepares the CIP cell, and a second process prepares the monomer mixture.

[0132] In the first process, the glass panes 11, 12 are washed and a primer is applied to a surface of each glass pane by wiping. The CIP cell is assembled by adhesion of the circumferential spacer bar 14 to the primed surface of each glass pane 11, 12.In the second process, the mixture is made up by mixing the monomer, the inorganic salts, and any additives in water, optionally containing the water miscible organic solvent. The mixture is filtered, transferred into a vacuum vessel, and degassed in the vacuum vessel (at least 2 hours, below 20 mbar pressure).

[0133] The manufacturing process continues by introducing the degassed mixture (which is preferably not stored) into the assembled cell and curing it in the cell. A calculated volume of the degassed mixture is introduced from the bottom of the cell whilst the cell is in its vertical orientation. During this operation a gentle press or vacuum is applied to the cell in order to prevent it from bulging. The filled cell is temporarily sealed and brought into its horizontal orientation and immediately transferred into a curing oven. The mixture is cured for four hours at an oven temperature of 70°C. After removal from the oven and cooling, the cell is permanently sealed.

[0134] Fire Tests

[0135] The performance of several fire-resistant glazings according to the present invention in fire tests carried according to EN 13501-2. The fire-resistant glazings consisted of the single CIP cell described above. The single fire-resistant interlayer 13 was formed by polymerisation of the monomer mixtures set out in Examples 1 to 5 below. But, as may be seen, the fire-resistant glazings use a different primer coating on the interior surface of the cold side glass pane.

[0136] Example 1

[0137] % by weight

[0138] Sodium 2-acrylamido-2-methylpropane sulfonate 12

[0139] Methylene bisacrylamide 0.08

[0140] Sodium Chloride 9

[0141] Magnesium Chloride 8

[0142]

[0143] VA-044 0.0035

[0144] Molar ratio of sodium ion to magnesium ion = 2.46:1

[0145] Primer: KBM-503 / Dynasylan® MEMO (3-methacryloxypropyltrimethoxysilane)

[0146] Example 2

[0147] % by weight

[0148] Sodium 2-acrylamido-2-methylpropane sulfonate 12

[0149] Poly(ethylene glycol diacrylate) 200 g / mol 0.3

[0150] Sodium Chloride 9

[0151] Magnesium Chloride 8

[0152]

[0153] VA-044 0.0035Molar ratio of sodium ion to magnesium ion = 2.46:1

[0154] Primer: KBE-503 (3-methacryloxypropyltriethoxysilane)

[0155] Example 3

[0156] % by weight

[0157] Sodium 2-acrylamido-2-methylpropane sulfonate 10

[0158] polyethylene glycol dimethacrylate) 8000 g / mol 1.5

[0159] Sodium Chloride 8

[0160] Magnesium Chloride 9

[0161]

[0162] VA-044 0.0035

[0163] Molar ratio of sodium ion to magnesium ion = 2.35:1

[0164] Primer: Dynasylan® HYDROSIL 2907 (an aqueous oligomeric aminoalkyl- and vinylfunctional silane hydrolysate)

[0165] Example 4

[0166] % by weight

[0167] Sodium 2-acrylamido-2-methylpropane sulfonate 11

[0168] Polyethylene glycol diacrylate) 400 g / mol 0.25

[0169] Sodium Chloride 9

[0170] Magnesium Chloride 8

[0171]

[0172] VA-044 0.0035

[0173] Molar ratio of sodium ion to magnesium ion = 2.4:1

[0174] Primer: KBM-503 / Dynasylan® MEMO (3-methacryloxypropyltriethoxysilane)

[0175] Example 5

[0176] % by weight

[0177] Sodium 2-acrylamido-2-methylpropane sulfonate 13

[0178] Poly(ethylene glycol diacrylate) 600 g / mol 0.35

[0179] Sodium Chloride 8

[0180] Magnesium Chloride 8

[0181] Ammonium Persulfate 0.0025

[0182]

[0183] N,N,N,N-Tetramethylethylenediamine 0.005

[0184] Molar ratio of sodium ion to magnesium ion = 2.3:1

[0185] Primer: KBM-5803 (8-methacryloxyoctyltrimethoxysilane)

[0186] In examples 1 to 5 water was added to each example to make up to 100% by weight.Example 6

[0187] % by weight

[0188] Potassium 3-(Acryloyloxy)propane-l-sulfonate 12

[0189] N,N'-Methylene bisacrylamide 0.08

[0190] Water 70.92

[0191] Magnesium Chloride 7

[0192] Sodium Chloride 10

[0193]

[0194] Wako V-50 Initiator 0.002

[0195] Molar ratio of sodium ion to magnesium ion = 2.33:1

[0196] Example 7

[0197] % by weight

[0198] [2-(Methacryloyloxy)-ethyl]-dimethyl-(3-sulfopropyl)- 10

[0199] ammoniumhydroxide

[0200] N,N'-Methylene bisacrylamide 0.06

[0201] Water 72.92

[0202] Magnesium Chloride 8

[0203] Sodium Chloride 9

[0204]

[0205] Wako V-50 Initiator 0.002

[0206] Molar ratio of sodium ion to magnesium ion = 1.83:1

[0207] All of the fire-resistant glazings showed a resistance to fire performance of El 60 or above - but only the fire resistant glazing of Example 4 formed water vapour bubbles during the fire test at the interior surface of the room side pane which led to separation of the polymer from that surface and early exhaustion of the glazing as compared to the other fire-resistant glazings.

[0208] As used herein the words "about" or "approximately" preferably mean within 10%, 5%, 2%, 1% or 0.1% of the value. Thus a ratio of about 2.3: 1 can vary by all of the above percentages.

[0209] Items mention as "a" or "an" item mean one or more unless the description states otherwise. Thus, a crosslinker means one or more crosslinkers. A foaming agent means one or more foaming agents. Of course, this does not apply to "a single monomer" which clearly means one and only one monomer.

[0210] Any item, feature, list, selection, preference, range or value etc expressed in relation to one aspect of the present invention is also to be applied equally to all the other aspects of the invention. Thus, by example, the salts in the first aspect of the invention may be used in thesecond aspect or third aspect of the present invention. Equally, the foaming agents mentioned in the second aspect of the present invention may be used in the first aspect or third aspect of the present invention.

[0211] When a feature is mentioned such as A and / or B, this is equivalent to saying A, B or both A and B.

Claims

CLAIMS1. A fire-resistant glazing comprising a laminate of at least two opposing glass panes and at least one fire-resistant layer, wherein each fire-resistant layer is an interlayer for two glass panes and is enclosed by a peripheral spacer bar separating the two glass panes adjacent their edges, wherein the at least one fire-resistant layer comprises a polymer hydrogel formed by polymerising a single monomer in water, wherein the single monomer is selected from one of the following groups:I an acrylate, methacrylate or itaconate including an alkyl sulfonic acid group, wherein the alkyl sulfonic acid moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt; andII an acrylamide, methacrylamide or itaconamide including an alkyl sulfonic acid group, wherein the alkyl sulphonic moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt.

2. A fire-resistant glazing according to Claim 1, wherein the single monomer is 3-(acryloyloxy)propane-l-sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, 3-(methacryloyloxy)propane-l-sulfonate, 4-[[2-(methacryloyloxy)ethyl]dimethylammonio]-butane-1 -sulfonate, 3-((3-methacrylamidopropyl)-dimethylammonio)propane-l-sulfonate, and bis(3-sulfoproproyl) itaconate, preferably as a potassium or a sodium salt.

3. A fire-resistant glazing according to Claim 1 or Claim 2, wherein the polymer hydrogel contains one or more of a cross-linker selected from methylene bisacrylamide, or a polyethylene glycol dimethacrylate) or a polyethylene glycol diacrylate) having a mean molar mass of between 200 g / mol and 8000 g / mol.

4. A fire-resistant glazing according to any preceding Claim, wherein the at least one fire-resistant layer comprises from 5% to 15% by weight of polymerised monomer and from 0.05% to 2.0% by weight of one or more cross linker.

5. A fire-resistant glazing according to any preceding Claim, wherein the at least one fire-resistant layer comprises from 10% to 22% by weight of at least one inorganic salt.

6. A fire-resistant glazing according to Claim 5, wherein the at least one inorganic salt comprises one or more of sodium chloride, potassium chloride, calcium chloride, magnesium chloride and zinc chloride.

7. A fire-resistant glazing according to Claim 6, wherein the at least one fire-resistant layer further comprises one or more foaming agent comprising one or more of potassium azide, sodium azide, potassium nitrite, sodium nitrite, potassium nitrate, sodium nitrate, ammonium nitrate, ammonium carbonate, andurea, citric acid, ascorbic acid, tartaric acid and their potassium or sodium salts.

8. A fire-resistant glazing according to any of Claims 5 to 7, wherein the at least fire-resistant layer comprises magnesium chloride and sodium chloride, and the molar ratio of sodium ion to magnesium ion therein is from 3:1 to 1:3.

9. A fire-resistant glazing according to any preceding Claim, wherein the at least one fire-resistant layer comprises up to 10% by weight of a water miscible organic solvent.

10. A fire-resistant glazing according to any preceding Claim, wherein the at least one fire-resistant layer comprises from 55% to 80% by weight of water.

11. A fire-resistant glazing according to any preceding Claim, wherein at least one pane has a coating on an interior surface thereof for adhering the polymer hydrogel to the at least one glass pane.

12. A fire-resistant glazing according to Claim 11, wherein the coating comprises a silane including one or more of an acrylate, a methacrylate, a primary amine, a secondary amine, an epoxy, or a vinyl group.

13. A fire-resistant glazing according to Claim 12, wherein the coating comprises 3- methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 8-methacryloxy- octyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxy-silane, vinyltri methoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, or an aqueous oligomeric aminoalkyl- and vinyl-functional silane hydrolysate.

14. A fire-resistant glazing according to any of Claims 11 to 13, wherein the coating comprises at least one metal oxide or metal nitride.

15. A fire-resistant glazing according to any preceding Claim, wherein at least one pane is plasma treated or flame treated on an interior surface thereof.

16. A fire-resistant glazing according to any preceding Claim wherein the peripheral spacer bar comprises a fibre-reinforced composite material.

17. A fire-resistant glazing according to any preceding Claim, wherein each glass pane is a toughened float glass.

18. A fire-resistant glazing according to any preceding Claim, wherein at least one glass pane is a safety glazing.

19. A fire-resistant glazing according to any preceding Claim, comprising a single fire-resistant layer.

20. A fire-resistant glazing according to Claim 19, wherein the single fire-resistant layer has a thickness from 6 mm to 45 mm.

21. A method for the production of a fire-resistant glazing comprising a laminate of at least two transparent glass panes and at least one transparent fire-resistant layer, the method comprising pouring a mixture comprising a single monomer and water into a cavity provided by a peripheral spacer bar located adjacent the edges of two opposing transparent glass panes, sealing the peripheral spacer bar and allowing the mixture to polymerise in thecavity to form a polymer hydrogel, wherein the single monomer is selected from one of the following groups:I an acrylate, methacrylate or itaconate including an alkyl sulfonic acid group, wherein the alkyl sulfonic acid moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt; andII an acrylamide, methacrylamide or itaconamide including an alkyl sulfonic acid group, wherein the alkyl sulphonic moiety comprises 1 to 4 carbon atoms, preferably as a potassium or sodium salt.

22. A method according to Claim 21, wherein the mixture comprises one or more of a crosslinker selected from methylene bisacrylamide, or a poly(ethylene glycol di methacrylate) or a poly(ethylene glycol diacrylate) having a mean molar mass of between 200 g / mol and 8000 g / mol.

23. A method according to Claim 21 or Claim 22, wherein the single monomer is 3-(acryloyloxy)propane-l-sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, 3-(methacryloyloxy)propane-l-sulfonate, 4-[[2-(methacryloyloxy)ethyl]dimethylammonio]-butane-l-sulfonate, 3-((3-methacrylamidopropyl)-dimethylammonio)propane-l-sulfonate, and bis(3-sulfoproproyl) itaconate, preferably as a potassium or a sodium salt.

24. A method according to any of Claims 21 to 23, wherein the mixture comprises from 5% to 15% by weight of monomer and from 0.05% to 2.0% by weight of one or more cross linker.

25. A method according to any of Claims 21 to 24, wherein the mixture comprises from 10% to 22% by weight of at least one inorganic salt.

26. A method according to Claim 25, wherein the at least one inorganic salt comprises one or more of sodium chloride, potassium chloride, calcium chloride, magnesium chloride and zinc chloride.

27. A method according to Claim 26, wherein the mixture further comprises a foaming agent comprising one or more of potassium azide, sodium azide, potassium nitrite, sodium nitrite, potassium nitrate, sodium nitrate, ammonium nitrate, ammonium carbonate, and urea, citric acid, ascorbic acid, tartaric acid and their potassium or sodium salts.

28. A method according to any of Claims 25 to 27, wherein the mixture comprises magnesium chloride and sodium chloride, and the molar ratio of sodium ion to magnesium ion therein is from 3:1 to 1:3.

29. A method according to any of Claims 21 to 28, wherein the mixture comprises up to 10% by weight of a water miscible organic solvent.

30. A method according to any of Claims 21 to 29, wherein the mixture comprises from 55% to 80% by weight of water.

31. A method according to any of Claims 21 to 30, wherein at least one pane has a coating on an interior surface thereof for adhering the polymer hydrogel to the at least one glass pane.

32. A method according to Claim 31, wherein the coating comprises a silane including one or more of an acrylate, a methacrylate, a primary amine, a secondary amine, an epoxy, or a vinyl group.

33. A method according to Claim 32, wherein the coating comprises 3-methacryloxypropyltri methoxysilane, 3-methacryloxypropyltriethoxysilane, 8-methacryloxy-octyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxy-silane, vinyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, or an aqueous oligomeric aminoalkyl- and vinyl-functional silane hydrolysate.

34. A method according to any of Claims 31 to 33, wherein the coating comprises at least one metal oxide or metal nitride.

35. A method according to any of Claims 21 to 34, wherein at least one pane is plasma treated or flame treated on an interior surface thereof.

36. A method according to any of Claims 21 to 35, wherein the peripheral spacer bar comprises a fibre-reinforced composite material.

37. A method according to any of Claims 21 to 36, wherein each glass pane is a toughened float glass.

38. A method according to any of Claims 21 to 37, wherein at least one glass pane is a safety glazing.

39. A method according to any of Claims 21 to 38, providing a fire-resistant glazing having a single fire-resistant layer.

40. A method according to Claim 39, providing that the single fire-resistant layer has a thickness from 6 mm to 45 mm.

41. A use of a fire-resistant glazing according to any one of claims 1 to 20 or prepared by a method according to any one of claims 21 to 40 for incorporation into a building product such as a door, a window, a partition, or a facade for a building, a ship, a car, or a train.