Method for preparing a partially recycled feedstock for a metal injection-moulding process

The process addresses material waste and cost issues in metal injection molding by recycling granules from discarded parts and sprues, ensuring efficient reuse without disrupting the molding process and maintaining part quality.

WO2026234346A1PCT designated stage Publication Date: 2026-11-12SAFRAN AIRCRAFT ENGINES SAS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/FR2026/050307
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The existing metal injection molding process results in significant losses of metal alloy powder due to discarded raw parts and sprues, which are costly and environmentally undesirable, and requires multiple initial injections to stabilize the molding machine, leading to inefficiencies and material waste.

Method used

A process for preparing a partially recycled raw material by grinding intermediate parts to form recycled granules, mixing them with new granules using a three-dimensional dynamic mixer, and maintaining a low percentage of recycled granules to maintain rheological compatibility, allowing direct injection into molds without disrupting the molding process.

Benefits of technology

Reduces material losses and environmental impact while maintaining process efficiency and performance, enabling multiple reuses of the recycled material without altering injection parameters or causing hopper blockages, and ensuring the final parts have the desired chemical composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FR2026050307_12112026_PF_FP_ABST
    Figure FR2026050307_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a partially recycled feedstock (3) for a metal injection-moulding process, the method comprising the following steps: - grinding (E1) an intermediate green part (0) resulting from a metal injection manufacturing process, the intermediate green part (0) being made up of a powder of a metal alloy dispersed in a plastic binder, the grinding being carried out so as to form recycled granules (1) of a mixture of metal alloy and plastic binder, - mixing (E2) the recycled granules (1) with new granules (2) of the same mixture of metal alloy and plastic binder, the mixing (E2) being carried out by a three-dimensional dynamic mixer, so as to obtain a partially recycled feedstock (3) comprising between 50% and 99%, preferably between 50% and 90%, by mass of new granules (2), the remainder consisting of the recycled granules (1), the new granules (2) having a round shape or a cylindrical shape.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] DESCRIPTION

[0002] TITLE: Process for preparing a partially recycled raw material for a metal injection molding process.

[0003] TECHNICAL FIELD

[0004] The invention relates to a process for preparing a partially recycled raw material intended for use in a metal injection molding process, the raw material obtained from this process, a metal injection molding process for a part using the partially recycled raw material and a part for aeronautics manufactured by this metal injection molding process.

[0005] STATE OF THE ART

[0006] Metal powder injection molding (known in English as "MIM" for "Metal Injection Molding") can be advantageously used for manufacturing complex turbomachine parts to the desired dimensions.

[0007] In general, this injection molding process includes successive steps of mixing a metal alloy powder with at least one plastic binder, granulating this mixture, injection molding, chemical debinding, thermal debinding and sintering.

[0008] In the mixing stage, a metal alloy powder is mixed with at least one plastic binder. During this stage, the temperature is set to a value that makes the plastic pasty, allowing for thorough mixing between the metal alloy powder and the plastic binder.

[0009] In the granulation stage of the mixture of metal alloy powder and plastic binder, the mixture is passed through an extruder to obtain granules of the metal alloy and plastic mixture, known to those skilled in the art as "feedstock" or raw material. Each granule of the mixture thus consists of metal alloy powder dispersed in plastic binder.

[0010] In the injection molding stage, granules of a mixture of metal alloy and plastic, made viscous by heating and pressurization, are injected into the mold of the part to be manufactured. Injection is typically carried out using an injection molding machine (see Figure 7): the granules of the metal alloy and plastic mixture are deposited into a hopper and fall at one end of a tube. Then, the granules are pushed along the tube by a piston or a screw to the other end of the tube, where they are finally injected through a nozzle 8 into a mold 9.

[0011] Referring to Figure 6A, we can see the nozzle 8 and the mold 9. During cooling, the raw material in the mold 9 shrinks, and the raw material in the nozzle 8 acts as a reservoir. As shown in Figure 6B, after cooling and demolding, we obtain a raw part 11, also called a "green part," which is a part made of mixed alloy and plastic powder (alloy grains suspended in the plastic). Adjusting the molding parameters allows us to obtain a part without porosity. The plastic binder ensures the part's stability. During demolding, the material in the nozzle 8 remains attached to the part 11 and forms a quantity of material called the "injection sprue" 10. In Figure 6C, we can see that the injection sprue 10 is then separated from the part 11.

[0012] For each injection campaign corresponding to a given mold 9 and plastic binder, it is necessary, in order to stabilize the injection molding machine in terms of temperature and pressure, to inject the mold 9 approximately 5 to 50 times, resulting in a loss. These injections are particularly necessary to properly fill the injection molding machine tube and eliminate air bubbles. However, the 5 to 50 raw parts 11 resulting from these injections contain holes and will therefore not allow for the production of final parts with the desired mechanical properties. These first 5 to 50 raw parts 11 are therefore discarded. The same applies to the sprues 10 associated with these first discarded parts, as well as to all sprues separated from parts deemed compliant. These sprues 10 can represent a significant portion of the material (for example, up to 1% to 40% by mass of the part 11).

[0013] The injection sprues 10 and the resulting raw parts 11 represent significant losses of metal alloy powder, even though some components of this metal alloy powder are very expensive and / or difficult to source. For all these reasons, as well as for environmental reasons, it would therefore be desirable to recycle the raw material constituting these raw parts or rejected sprues.

[0014] BRIEF DESCRIPTION OF THE INVENTION

[0015] One aim of the invention is therefore to limit the losses of alloy powders generated by the disposal of a certain number of raw parts and sprues during the implementation of a metal injection molding process, while maintaining the performance of this process. Another aim of the invention is to make a metal injection molding process more environmentally friendly and more economical.

[0016] To this end, the invention proposes a process for preparing a partially recycled raw material for a metal injection molding process comprising the following steps:

[0017] - grinding of an intermediate raw part from a metal injection manufacturing process, the intermediate raw part consisting of a powder of a metal alloy dispersed in a plastic binder, so as to form recycled granules of a mixture of metal alloy and plastic binder,

[0018] - mixing of said recycled granules with new granules of the same mixture of metallic alloy and plastic binder, the mixing being carried out by a three-dimensional dynamic mixer, so as to obtain a partially recycled raw material comprising between 50% and 99%, preferably between 50% and 90%, by mass of new granules, the remainder being made up of recycled granules,

[0019] new granules having a round or cylindrical shape.

[0020] Thanks to these features of the invention, the partially recycled raw material from the process can be directly injected into a mold for a part to be manufactured, for example, using an injection molding machine, as part of a metal injection molding process. It can nevertheless be stored and / or transported beforehand without altering its physicochemical properties, and without resulting in sedimentation and / or loss of homogeneity between new and recycled granules.

[0021] Recycled granules are typically obtained by grinding injection sprues and / or rejected raw parts, so that the metal alloy powder they contain is advantageously reused in new raw parts and helps to limit losses of said metal alloy powder. The only defect of the rejected raw parts is that they contain holes: grinding said rejected raw parts eliminates this defect. Thus, the recycled granules of the raw material according to the invention can consist, interchangeably, solely of ground injection sprues, solely of ground rejected raw parts, or of a mixture of ground injection sprues and ground rejected raw parts.

[0022] Using the same plastic binder in both recycled and virgin granules, and maintaining a recycled granule content of 50% or less by mass, advantageously allows the injection molding parameters to remain unchanged compared to those used when injecting only virgin granules—that is, granules directly from the mixing and granulation stages described above. This would not be possible with fully recycled raw material, as it does not exhibit the same rheology (same resistance to stress and deformation) as virgin raw material: during the injection of the intermediate raw part, the plastic binders were heated, resulting in a modification of their polymer chains.Finally, partially recycled raw material according to the invention can easily be prepared and injected during an injection molding campaign without disrupting said campaign and without requiring additional work to optimize new injection parameters. Furthermore, the new granules advantageously allow the recycled granules to be carried into the hopper, thus facilitating flow in the injection molding machine. This contrasts with the use of fully recycled raw material, which, due to the significant heterogeneity in shape of the recycled granules, encounters movement difficulties that can, in extreme cases, lead to hopper blockages.

[0023] The recycled raw material according to the invention can even be formed and injected several times during the same injection campaign (for example, by grinding the injection sprues generated throughout the campaign). In other words, the recycled granules of the material according to the invention may include material (metal alloy powder and plastic binder) that has already been injected more than once in an injection step of the MIM process. However, the rheology of the recycled granules and the chemistry of the powder (for example, its oxidation) may change negatively as a result of successive recycling. A mass percentage of recycled granules consistently below 50% advantageously limits the proportion of material that has undergone n recyclings, especially as n is large.

[0024] Finally, the metal alloy powder of recycled granules and new granules is identical, so the raw part injected from said raw material leads to a final sintered part having the desired chemical composition.

[0025] Depending on other optional characteristics of the process, taken alone or in combination where technically possible:

[0026] - The new granules of the mixture of metal alloy and plastic binder are manufactured by:

[0027] - hot mixing of a new metal alloy powder with a new plastic binder, so as to obtain a mixture of metal alloy and new plastic binder, the new metal alloy powder and the new plastic binder being identical respectively to the metal alloy powder and the plastic binder constituting the intermediate raw part,- granulation of the mixture of metal alloy and new plastic binder, so as to obtain the new granules of the mixture of metal alloy and plastic binder;

[0028] - the granulation of the mixture of metallic alloy and new plastic binder is carried out by an extruder;

[0029] - The new granules of the mixture of metal alloy and plastic binder have a round shape with a diameter between 1 mm and 4 mm or a cylindrical shape with a diameter between 1 mm and 4 mm and a length between 1 mm and 4 mm; - The mixture of metal alloy and plastic binder of the new and recycled granules comprises between 60% and 80% by mass of metal alloy powder, the remainder being made up of the plastic binder,

[0030] The metallic alloy powder of the new and recycled granules has a D50 particle size between 1 µm and 50 µm, the D50 particle size value being measured by laser diffraction according to ISO 13322-2, and / or,

[0031] the plastic binder of new granules and recycled granules includes a primary binder and a secondary binder, the primary binder being able to be chosen from polyethylene glycol and polyoxymethylene, and the secondary binder being for example polypropylene;

[0032] - the process further includes the prior molding of the intermediate raw part by injecting a prior raw material of the intermediate raw part into a mold of the intermediate raw part, the prior raw material of the intermediate raw part comprising between 50% and 100% by mass of new granules of the mixture of alloy and plastic binder, the possible complement being made up of prior recycled granules of said mixture of alloy and plastic binder;

[0033] - the intermediate raw part is chosen from an injection sprue and a discarded raw part.

[0034] The invention also relates to a partially recycled raw material for a metal injection molding process, this partially recycled raw material being characterized in that it comprises between 50% and 99%, preferably between 50% and 90%, by mass, of new granules of a mixture of metal alloy and plastic binder, the new granules being round or cylindrical in shape, the remainder of the raw material being made up of recycled granules of the same mixture of metal alloy and plastic binder, the recycled granules being mixed with said new granules, the raw material being obtained from a preparation process comprising a mixing being carried out by a three-dimensional dynamic mixer.

[0035] The invention also relates to a metal injection molding process for a final part, particularly for aeronautics, comprising: - injection molding of a partially recycled raw material from a preparation process as previously described in a mold, to obtain a final raw part,

[0036] - the unbinding of the final raw piece to obtain a unbound piece,

[0037] - sintering the debound piece to obtain a final, sintered piece.

[0038] The invention also relates to a part for aeronautics manufactured by the metal injection molding process as previously described, characterized in that it is a turbine blade, a turbine distributor, a retaining ring, a sealing sector and a housing part.

[0039] BRIEF DESCRIPTION OF THE FIGURES

[0040] Other features and advantages of the invention will become apparent from the detailed description that follows, with reference to the attached drawings, in which:

[0041] - Figure 1 is a diagram representing the steps of a process for preparing a partially recycled raw material according to the invention,

[0042] - Figure 2 is a diagram representing additional steps to those in Figure 1, which concern the preparation of new granules,

[0043] - Figure 3 is a diagram representing complementary steps to those of Figure 1, which concern the shaping of the intermediate raw part by injecting a prior raw material into a mold, the prior raw material comprising only new granules of the mixture of metallic alloy and plastic binder,

[0044] - Figure 4 is a diagram representing complementary steps to those of Figure 1, which concern the shaping of the intermediate raw part by injecting a previous raw material into a mold, the previous raw material itself comprising a mixture of new granules and recycled granules,

[0045] - Figure 5 is a diagram representing the steps of a metal injection molding process for a final part made from partially recycled raw material obtained by the aforementioned process,

[0046] - Figure 6A represents the molding of a raw part, Figure 6B represents the raw part removed from the mold with its injection sprue, and Figure 6C represents the raw part finally separated from its injection sprue.

[0047] - Figure 7 is a diagram representing an injection molding machine,

[0048] - Figure 8 is a graph representing the effect of successive recyclings in a particular embodiment of the invention where the raw material is formed at each successive recycling by 85% new granules and 15% recycled granules,

[0049] - Figure 9 shows a diagram of an example of the production of new granules, - Figure 10 shows a diagram of an example of the production of recycled granules. For readability, the drawings are not necessarily to scale.

[0050] DETAILED DESCRIPTION OF IMPLEMENTATION METHODS

[0051] Process for preparing a partially recycled raw material for a [unclear] of

[0052] With reference to figure 1, the invention relates to a process for preparing a partially recycled raw material 3 intended for use in a metal injection molding process.

[0053] Intermediate raw piece 0

[0054] The preparation process uses a raw part 0 consisting of a metal alloy powder dispersed in a plastic binder. This raw part 0 is referred to as "intermediate" to distinguish it from a raw part referred to as "previous" and a raw part referred to as "final," which will be described later and which are used respectively before and after in the various processes described in the application.

[0055] The intermediate raw part 0 preferably comprises between 60% and 80% by mass of metal alloy powder, the remainder being made up of the plastic binder.

[0056] The metallic alloy powder preferentially has a D50 particle size between 1 pm and 50 pm, the D50 particle size value being measured by laser diffraction according to ISO 13322-2.

[0057] As a purely illustrative example, the metal alloy powder can be chosen, for instance, from a nickel-based, titanium-based, or iron-based alloy powder. In other words, the metal alloy powder contains more than 50% nickel, titanium, or iron.

[0058] The plastic binder preferably comprises a primary binder and a secondary binder. The primary binder is, for example, chosen from polyethylene glycol and polyoxymethylene. For example, the secondary binder is polypropylene.

[0059] Preferably, the intermediate raw part 0 is an injection sprue and / or a rejected raw part. A "rejected raw part" is defined as a raw part from an injection step of a MIM process that was not deemed compliant. Typically, such a part is obtained during the necessary stabilization of the injection molding machine at the beginning of an injection molding campaign.

[0060] Grinding E1 of the intermediate raw piece 0 to obtain recycled granules 1

[0061] The preparation process includes grinding E1 of the aforementioned intermediate raw piece 0, so as to form granules, called "recycled granules" 1.

[0062] The term “recycled granules 1 of a mixture of alloy and plastic binder” means granules each comprising metallic alloy powder dispersed in plastic binder in the same mass proportions as in the intermediate raw part 0.

[0063] E1 grinding is typically carried out using a grinder, for example, one comprising two metal combs, each metal comb having parallel bars of the same width and regular spacing. The width of the gap between the bars is strictly greater than the width of the bars, so the grinding action is achieved by the interlacing of the two metal combs (each bar of the first comb fits into the gap of the second comb and vice versa), the intermediate raw material to be ground being previously positioned between the two combs. More precisely, the intermediate raw material to be ground is initially positioned in a container and falls by gravity into the space between the combs.

[0064] Preferably, the width of the bars is between 1 mm and 5 mm and the width of the gap is between 5 mm and 15 mm. Such ranges of bar widths and gaps advantageously allow for an average size of the largest dimension of the recycled granules to be between 1 mm and 5 mm.

[0065] However, with reference to Figure 10, the recycled granules 1 obtained after grinding have an irregular shape. In other words, the recycled granules 1 do not have a regular shape such as a round, cylindrical, cubic, or rectangular parallelepiped shape. Typically, each recycled granule 1 has an average size defined as the average of the dimensions of the recycled granule 1 in all spatial directions, and the standard deviation around this average size is strictly greater than the standard deviation around the average size of a new granule 2 as defined below. Furthermore, considering the average size of the recycled granules 1 to be the average of the average sizes of each recycled granule 1, the particle size distribution of the recycled granules 1 around this average size is wider than the particle size distribution of the new granules 2 around their average diameter or average length.For example, recycled granules 1 have an average length (understood as the average of the largest dimension of each recycled granule) of between 1 mm and 6 mm and an average width (understood as the average of their largest dimension measured perpendicular to the length) of between 1 mm and 3 mm when the average diameter or average length of new granules as defined hereafter is between 1 mm and 4 mm.

[0066] Mixture E2 of recycled granules 1 with new granules 2

[0067] The preparation process further includes mixing E2 of said recycled granules 1 with new granules 2 of the mixture of metal alloy and plastic binder, so as to obtain a partially recycled raw material 3.

[0068] With reference to Figure 9, the new granules 2 of the alloy and plastic binder mixture are either round or elongated, for example, cylindrical. Preferably, the average diameter of the new granules 2, whether round or cylindrical, is between 1 mm and 4 mm. Preferably, the average length of the new granules 2, which are elongated and possibly cylindrical, is between 1 mm and 4 mm.

[0069] Furthermore, the new granules 2 exhibit a low particle size distribution. For example, when the average diameter of the new granules 2, whether round or cylindrical, is between 1 mm and 4 mm, the standard deviation around said average diameter of the new granules 2 is preferentially between 1 mm and 3 mm. For example, when the average length of the new granules 2, whether elongated, is between 1 mm and 4 mm, the standard deviation around said average length of the new granules 2 is preferentially between 1 mm and 3 mm.

[0070] New granules 2 are granules made from the same mixture of metal alloy and plastic binder as recycled granules 1. In other words, new granules 2 contain the same metal alloy powder and plastic binder as recycled granules, mixed in the same proportions. For example, if recycled granules 1 contain 70% by mass of metal alloy powder and 30% of plastic binder, new granules 2 contain 70% by mass of the same metal alloy powder and 30% of the same plastic binder.

[0071] The term "same" metal alloy powder means a metal alloy powder having the same chemical composition (with the effects of recycling ready) and the same particle size as that contained in the recycled granules 1. The term "with the effects of recycling ready" means that the metal alloy powder contained in the recycled granules 1 may contain an oxygen content higher than the oxygen content of the metal alloy powder contained in the new granules 2 by 1 ppm to 50 ppm.

[0072] The term "same" plastic binder refers to a plastic binder containing the same plastic materials in the same proportions. For example, the plastic binder in new granules 2 consists of the same primary binder and the same secondary binder in the same proportions as the plastic binder in recycled granules 1. However, recycling can lead to a change in the rheology of the plastic binder in recycled granules 1, for example, a change of 5% to 30% in the volumetric melt flow rate (more commonly known to those skilled in the art by the acronym MVR).

[0073] In summary:

[0074] - the mixture of alloy and plastic binder constituting each new granule 2 can comprise between 60% and 80% by mass of the metallic alloy powder, the remainder being made up of the plastic binder;

[0075] - the metallic alloy powder of the new granules 2 preferably has a D50 particle size between 1 µm and 50 µm, the D50 particle size value being measured by laser diffraction according to ISO 13322-2; and / or,

[0076] - the plastic binder of the new granules 2 may comprise a main binder and a secondary binder, the main binder being able to be chosen from polyethylene glycol and polyoxymethylene, and the secondary binder being for example polypropylene.

[0077] Recycled granules 1 preferentially have dimensions close to those of new granules 2. For example, recycled granules 1 have an average dimension equal to the average diameter or average length of new granules 2. For example, the average dimension of recycled granules 1 equal to the average diameter or average length of new granules 2 means that the average dimension of recycled granules 1 is equal to the average diameter of new granules 2 plus or minus 5%.

[0078] The process for preparing a partially recycled raw material 3 for a metal injection molding process according to the invention may further include the prior preparation of said new granules 2 of the mixture of metal alloy and plastic binder, as will be explained with reference to the left part of Figure 2, which incorporates these steps.

[0079] As an example, this preparation process may include: - the hot mixing EO of a new metal alloy powder 2a with a new plastic binder 2b, so as to obtain a mixture of metal alloy and new plastic binder, the new metal alloy powder 2a and the plastic binder 2b being identical respectively to the metal alloy powder and the plastic binder constituting the intermediate raw part 0, then,

[0080] - the granulation EO' of the mixture of metal alloy powder 2a and new plastic binder 2b, so as to obtain the new granules 2 of the mixture of metal alloy and plastic binder.

[0081] The term "new" metal alloy powder 2a refers to a powder of that alloy that has not been previously used in a metal injection molding (MIM) process, for example, a powder obtained directly by atomization and / or a powder obtained commercially. The term "new" plastic binder 2b refers to a plastic binder that has not undergone any prior injection molding process.

[0082] The EO' granulation of the new alloy and plastic binder mixture can be carried out by an extruder. This granulation makes it possible to obtain new granules 2 with a low size dispersion, for example a standard deviation around the average diameter, respectively the average length, of the new granules 2 between 1 mm and 3 mm when the average diameter (round or cylindrical shape), respectively the average length (elongated shape including cylindrical shape), of the new granules 2 is between 1 mm and 4 mm.

[0083] Mixing E2, for example, is carried out using a three-dimensional dynamic mixer, such as those from the registered trademark Turbula®: the mixer container is subjected to an off-axis rotation, thus continuously applying opposing and rhythmic movements to its contents. Indeed, due to their irregular shapes, recycled granules 1 are more difficult to set in motion than new granules 2, and in a conventional mixer, they are therefore likely to become stuck, leading to poor mixing of the recycled granules 1 and new granules 2. A three-dimensional dynamic mixer advantageously prevents the segregation of the recycled granules 1 by generating a chaotic movement, thus ensuring good mixing. The mixing time is preferably between 1 and 30 minutes.

[0084] The mixture E2 of recycled granules 1 with new granules 2 of the alloy and plastic binder mixture is prepared to obtain a partially recycled raw material 3 comprising between 50% and 99% by mass of new granules 2, the remainder being made up of recycled granules 1. A mass percentage of recycled granules 1 less than or equal to 50% advantageously allows obtaining a partially recycled raw material 3 with a rheology comparable to that of a raw material consisting solely of new granules. Thus, the raw material 3 according to the invention can advantageously be used in an injection molding campaign of the corresponding new raw material in a given mold without disrupting said injection molding campaign and without requiring additional work to determine new injection parameters.

[0085] Preferably, the partially recycled raw material 3 comprises between 50% and 90% by mass of new granules 2, preferably still between 60% and 90% by mass of new granules 2, even more preferably between 70% and 90% by mass of new granules 2, the remainder being made up of recycled granules 1.

[0086] Raw material used for injection molding of the intermediate raw part 0 and recycling

[0087]

[0088] With reference to Figures 3 and 4, the process for preparing a partially recycled raw material 3 according to the invention may further include a prior molding step E30 of the intermediate raw part 0 by injecting a so-called "prior" raw material 0c of the intermediate raw part 0 into a mold.

[0089] The intermediate raw piece 0 may have been obtained entirely by the use of new granules 2, as previously described or by the use of a partially recycled raw material 3.

[0090] Indeed, the prior raw material of the intermediate raw part 0c comprises between 50% and 100% by mass of new granules 2 of the same mixture of metallic alloy and plastic binder as previously described, the possible complement being made up of prior recycled granules 0b of said mixture of alloy and plastic binder.

[0091] If the initial raw material 0c of the intermediate raw part 0 consists of 100% new granules 2, then the process is shown schematically in Figure 3. In this case, the use of the partially recycled raw material 3 in the MIM injection molding process, which will be described later, allows for the initial recycling of said initial raw material 0c. If the initial raw material Oc of the intermediate raw part 0 consists of less than 100% new granules 2, the remainder being recycled granules Ob, then the process is shown schematically in Figure 4.In this case, the recycled material preparation process may include the grinding step E10 of a previous raw part 0a, so as to obtain the previous recycled granules 0b and the mixing E20 of said previous recycled granules 0b with new granules 2 so as to obtain the previous raw material Oc of the intermediate raw part Oc.

[0092] Thus, when the prior raw material Oc of the intermediate raw part 0 itself comprises prior recycled granules Ob, the use of the partially recycled raw material 3 according to the invention allows a second or more recycling of the prior recycled granules Ob and a first recycling of the new granules 2 of the prior raw material Oc (see Figure 4).

[0093] As a purely illustrative example, with a percentage of 50% of recycled granules 1 in the partially recycled raw material 3 according to the invention, said recycled granules 1 being derived from a prior raw material 0c itself comprising 50% of prior recycled granules 0b, advantageously allows the partially recycled raw material 3 according to the invention to consist of only 25% of these prior recycled granules 0b.

[0094] Figure 8 shows, on bar 1, a raw material consisting exclusively of virgin granules, and then, on bars 2 to 6, five partially recycled raw materials resulting from successive recycling processes. The partially recycled raw material n+1 comprises 15% recycled granules resulting from the grinding of a raw piece formed from raw material n, where n varies from 1 to 5. The remainder of the partially recycled raw material n+1 consists of virgin granules. On the bar associated with raw material n, the percentage of the raw material that has not been recycled is shown differently: zero times (virgin granules), once, twice, three times, four times, and five times, respectively.For example, with reference to Figure 8, a percentage of 15% recycled granules 1 in the partially recycled raw material 3 according to the invention, said recycled granules 1 being derived from a prior raw material 0c itself comprising 15% of prior recycled granules 0b, advantageously allows the partially recycled raw material 3 according to the invention to comprise only 2.25% of these prior recycled granules 0b. If these prior recycled granules 0b are themselves derived from an even prior raw material consisting of 85% new granules 2 and 15% even prior recycled granules, the partially recycled raw material according to the invention comprises only 0.3375% of these even prior recycled granules. Thus, after 5 recyclings, out of 100 kg of raw material, the raw material comprises only 45 g of material recycled 4 times and 2 g of material recycled 5 times.The impact of this material being recycled 4 or 5 times is therefore negligible.

[0095] Thus, the partially recycled raw material 3 according to the invention advantageously limits the negative effects of successive material recycling by reducing the proportion of material recycled n times, as the number of recycling cycles n increases. Indeed, successive recycling cycles alter the rheology of the plastic binder because, during the injection molding process, the plastic binder is heated, which modifies the polymer chains. Furthermore, successive recycling cycles pose a risk of contamination of the metal alloy powder by light elements such as oxygen, carbon, and nitrogen. It is therefore advisable to limit the number of recycling cycles.

[0096] It is therefore possible to recycle all the material in a given injection campaign.

[0097] Finally, it should be noted that the intermediate raw part 0 typically includes at least one injection sprue and / or a rejected raw part, for example, from a turbine blade, a turbine distributor, a retaining ring, a sealing sector or a cladding part.

[0098] Raw material for a metal injection molding process

[0099] The invention also relates to the partially recycled raw material 3 for a metal injection molding process comprising between 50% and 99%, preferably between 50% and 90%, preferably still between 60% and 90%, even more preferably between 70% and 90%, by mass of new granules 2 of a mixture of metal alloy and plastic binder, the remainder being made up of recycled granules 1 of the same mixture of metal alloy and plastic binder, the recycled granules 1 being mixed with said new granules 2.

[0100] The new granules 2 and the recycled granules 1 can be according to any of the embodiments previously described.

[0101] Typically, the metal alloy powder contained in recycled granules 1 may contain an oxygen content higher than the oxygen content of the first metal alloy powder contained in new granules 2, by 1 ppm to 50 ppm, and the volumetric melting rate of the plastic binder in recycled granules 1 may differ by 5% to 30% from the volumetric melting rate of the plastic binder in new granules 2. Metal injection molding process for a final part

[0102] With reference to Figure 5, the invention also relates to a method for manufacturing a final part, particularly for aeronautics, comprising:

[0103] - injection molding E3 of a partially recycled raw material 3 obtained from a preparation process as previously described, in a mold, to obtain a final raw part 4,

[0104] - the debinding E4,E5 of the final raw part 4 to obtain a debinded part 6, - the sintering E6 of the debinded part 6 to obtain a final sintered part 7.

[0105] Finally, the final sintered part 7 can undergo one or more additional heat treatments to perfect its mechanical, thermal or other properties depending on the chosen metal alloy and the intended application.

[0106] Advantageously, the use of the partially recycled raw material 3 according to the invention requires no adaptation of the various stages of the manufacturing process for a final part compared to the use of a raw material of the same mixture of metal alloy and plastic binder that would consist solely of virgin granules. Thus, the partially recycled raw material according to the invention can easily be used during a production run without disrupting said run and, moreover, allows for the full utilization of the metal alloy powder.

[0107] E3 Molding

[0108] The partially recycled raw material 3, produced using a preparation process as previously described, is injected into the mold of the part to be manufactured, for example, using a previously stabilized injection molding machine. The values ​​of parameters such as the injection temperature (temperature of the raw material upon entering the mold), the injection pressure, the injection speed, and the dwell time of the part in the mold depend on the part being injected. The temperature of the raw material at the injection point must not be too low, otherwise the raw material would be too solid and would not enter the mold. The injection temperature must also not be too high, so that the raw material is not too liquid: the alloy powder and the plastic binder could then separate, and the alloy powder would not be carried along.The injection temperature is preferably between 50 °C and 250 °C, the injection speed is preferably between 10 cm. 3 / s and 100 cm 3 / s and the injection pressure preferably between 50 bars and 1500 bars.

[0109] Following the molding step E3, a final raw part 4, also called the final "green part," is removed from the mold after cooling, along with its injection sprue. The final raw part 4 is then separated from the injection sprue, and the injection sprue can in turn be ground to form partially recycled raw material according to the invention.

[0110] E4A, E4B, E5 Debinding

[0111] We successively carry out two debinding steps of the final raw part 4, one of a chemical nature called "primary debinding" E4A, E4B, the other of a thermal nature E5.

[0112] Primary debinding E4A, E4B

[0113] Primary debinding E4 results in a partially debinded part 5. This debinding can be either: debinding using a solvent E4B, or preferably catalytic debinding E4A. The latter has the advantage of being faster.

[0114] The E4A catalytic debinding process involves vaporizing and then burning the plastic binder by injecting acid vapors into a furnace. The catalytic debinding is carried out, for example, at a temperature between 50°C and 250°C for a duration of between 1 and 30 hours, under a nitrogen atmosphere, in the presence of acid vapors, for example nitric acid vapors, with the nitric acid flow rate preferably between 2 mL / min and 5 mL / min.

[0115] The E4B debinding process using a solvent involves immersing the final raw part 4 in a bath of said solvent to dissolve the plastic. For example, the solvent is selected from water, an acid, and a base. The final raw part 4 can be immersed for a period of between 10 and 200 hours in said bath, with agitation, at a temperature preferably between 20 °C and 100 °C.

[0116] At the end of the chemical debinding step E4, a partially debinded part 5 is obtained, the chemical debinding having made it possible to remove more than 95% of the plastic binder.

[0117] Thermal unbinding E5: Thermal unbinding E5 is preferably achieved by applying at least one temperature step to the partially unbound part 5, under a protective atmosphere, for example, an argon atmosphere. The temperature step is preferably between 250 °C and 650 °C, and applied for a duration preferably between 100 and 300 minutes.

[0118] At the end of the thermal unbinding step E5, we obtain a unbound part or "brown part" 6, the thermal unbinding having made it possible to remove the remaining plastic binder (i.e. the less than 5% remaining).

[0119] The debinding part 6, resulting from the primary debinding step E4 and the thermal debinding step E5, has the same dimensions as the final raw part 4. However, unlike the final raw part 4, the debinding part 6 is very porous because the plastic binder has been removed. The density of the debinding part 6 is typically between 50% and 75% of the density of a cast part made of the same alloy. Furthermore, the debinding part 6 is very brittle because the plastic binder that ensured the part's stability has been removed.

[0120] E6 Sintering

[0121] The E6 sintering of the debinded part 6 is performed. As previously mentioned, sintering involves subjecting the debinded part 6 to a sintering temperature plateau close to the melting point of the alloy powder so that the powder grains bond together. During sintering, the debinded part 6 shrinks and its density increases.

[0122] Sintering is carried out in a furnace, preferably at a temperature between 1000 °C and 1500 °C for a period of time preferably between 2 hours and 20 hours under a protective atmosphere or under vacuum, for example under an argon atmosphere.

[0123] Preferably, the thermal debinding step E5 and the sintering step E6 are carried out in the same furnace, because the debinded part 6 is fragile.

[0124] At the end of the sintering step E6, a final sintered part 7 is obtained which is more compact, and whose density is preferably greater than 95% of the density of the same alloy from casting.

[0125] The dimensions of the final sintered part 7 are smaller than those of the final unbound or brown part 6. A size reduction of between 14% and 18% is typically observed. However, the final sintered part 7 may contain residual porosity that is detrimental to its mechanical properties. Finishing heat treatments can be implemented to eliminate this residual porosity.

[0126] These finishing heat treatments include, for example, hot isostatic compaction E7, a possible high-temperature heat treatment E8, quenching E9 or a tempering heat treatment step E10.

[0127] Final piece

[0128] The invention also relates to a final alloy part for aeronautical applications manufactured by the manufacturing process according to any of the embodiments described above. Preferably, the part is a turbine blade, a turbine distributor, a retaining ring, a sealing sector, or a housing component.

Claims

DEMANDS 1. A process for preparing a partially recycled raw material (3) for a metal injection molding process, comprising the following steps: - grinding (E1) of an intermediate raw part (0) from a metal injection manufacturing process, the intermediate raw part (0) being made up of a powder of a metal alloy dispersed in a plastic binder, so as to form recycled granules (1) of a mixture of metal alloy and plastic binder, - mixing (E2) of said recycled granules (1) with new granules (2) of the same mixture of metallic alloy and plastic binder, the mixing (E2) being carried out by a three-dimensional dynamic mixer, so as to obtain a partially recycled raw material (3) comprising between 50% and 99%, preferably between 50% and 90%, by mass of new granules (2), the remainder being made up of recycled granules (1), the new granules (2) having a round or cylindrical shape.

2. A preparation method according to claim 1, characterized in that the new granules (2) of the mixture of metal alloy and plastic binder are manufactured by: - ​​hot mixing (E0) of a new metal alloy powder (2a) with a new plastic binder (2b), so as to obtain a mixture of metal alloy and new plastic binder, the new metal alloy powder (2a) and the new plastic binder (2b) being identical respectively to the metal alloy powder and the plastic binder constituting the intermediate raw part (0), - granulation (E0') of the mixture of new metal alloy and plastic binder, so as to obtain new granules (2) of the mixture of metal alloy and plastic binder.

3. Preparation method according to claim 2, wherein the granulation (E0') of the mixture of new metal alloy and plastic binder is carried out by an extruder.

4. A preparation method according to any one of claims 1 to 3, wherein the new granules (2) of the mixture of metal alloy and plastic binder have a round shape with a diameter between 1 mm and 4 mm or a cylindrical shape with a diameter between 1 mm and 4 mm and a length between 1 mm and 4 mm.

5. A preparation method according to any one of claims 1 to 4, wherein the mixture of metal alloy and plastic binder of the new granules (2) and recycled granules (1) comprises between 60% and 80% by mass of metal alloy powder, the remainder being made up of the plastic binder, wherein the metal alloy powder of the new granules (2) and recycled granules (1) has a D50 particle size of between 1 µm and 50 µm, the D50 particle size value being measured by laser diffraction according to ISO 13322-2, and / or, in which the plastic binder of the new granules (2) and of the recycled granules (1) comprises a main binder and a secondary binder, the main binder being able to be chosen from polyethylene glycol and polyoxymethylene, and the secondary binder being for example polypropylene.

6. A preparation method according to any one of claims 1 to 5 further comprising the prior molding (E30) of the intermediate raw part (0) by injection of a prior raw material (0c) of the intermediate raw part (0) into a mold of the intermediate raw part, the prior raw material (0c) of the intermediate raw part (0) comprising between 50% and 100% by mass of new granules (2) of the alloy and plastic binder mixture, the possible complement being made up of prior recycled granules (0b) of said alloy and plastic binder mixture.

7. A preparation method according to any one of claims 1 to 6, wherein the intermediate raw part (0) is selected from an injection sprue and a discarded raw part.

8. Partially recycled raw material (3) for a metal injection molding process, this partially recycled raw material (3) being characterized in that it comprises between 50% and 99%, preferably between 50% and 90%, by mass, of new granules (2) of a mixture of metal alloy and plastic binder, the new granules (2) being round or cylindrical in shape, the remainder of the raw material being made up of recycled granules (1) of the same mixture of metal alloy and plastic binder, the recycled granules (1) being mixed with said new granules (2), the partially recycled raw material (3) being obtained by a preparation process comprising a mixing step (E2) implemented by a three-dimensional dynamic mixer.

9. A metal injection molding process for a finished part (7), particularly for aeronautical applications, comprising: - an injection molding (E3) of a partially recycled raw material (3) obtained from a preparation process according to any one of claims 1 to 7 in a mold, for obtaining a final raw part (4), - a debinding (E4A, E4B, E5) of the final raw piece (4) to obtain a debinded piece (6), - a sintering (E6) of the debonded part (6) to obtain a final sintered part (7).