Steel strip and manufacturing method
A dual-phase steel strip manufacturing process addresses the challenge of achieving high strength and ductility in packaging steels by employing controlled hot rolling, annealing, and overaging, resulting in a product suitable for packaging applications with enhanced mechanical properties.
Patent Information
- Application Number
- PCT/GB2026/050794
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for manufacturing high-strength packaging steels struggle to achieve a balance of strength and ductility, particularly in ultrathin sheets, while being cost-effective and compatible with existing production lines, limiting their applicability in the packaging industry.
A method for producing ferrite/bainite dual-phase steel strip involves specific composition and processing steps, including hot rolling, primary cold-rolling, annealing, and overaging, with controlled temperatures and cooling rates to achieve a steel strip with tensile strength greater than 800 MPa and elongation of 5-10%, suitable for packaging applications.
The method results in a high-strength, ductile steel strip with improved formability, meeting the demands of the packaging industry and ensuring consistent production within existing plant capabilities.
Smart Images

Figure GB2026050794_12112026_PF_FP_ABST
Abstract
Description
[0001] STEEL STRIP AND MANUFACTURING METHOD
[0002] The present invention relates to steel strip manufacturing methods, particularly methods for manufacturing low-carbon dual phase steel strip for use in packaging.
[0003] BACKGROUND
[0004] The use of steels in packaging, such as food and drinks cans and aerosols, is well known. Packaging steels include tinplate, chromium coated steel and blackplate. In order for such steels to be suitable for their intended purpose, they must have the required strength, surface finish and forming properties. The EN10202:2022 standard sets forth steel composition guidelines (via EN10334:2005) for packaging in the food industry in Europe.
[0005] Low-carbon sheet steels such as tinplate and tin-free steels have found extensive applications in the packaging industry. However, the growing industry inclination towards the production of ultrathin sheets (down to 200 pm thick, or even less) in order to decrease raw material costs has increased the demand for high-strength steels, especially for the Easy Open Ends (EoE) market.
[0006] High-strength packaging steels include low carbon steel with varying quantities of manganese and nitrogen. High-nitrogen steels in particular provide a good balance of strength and elongation.
[0007] Double-reduction processes (wherein the steel is subjecting to cold-roll reduction both before and after annealing) can increase steel strengths to 550 MPa and higher if the sheets are subjected to a heavy (i.e. >10%) cold rolling reduction. However, this also reduces total elongation.
[0008] In conventional processes for manufacturing packaging steel, the steel is hot rolled from slab to a gauge of 2.1 -3mm in thickness before coiling at temperature up to 700 °C in the hot strip mill.
[0009] Following this stage, the material undergoes a cold rolling process to achieve its near-final gauge, and subsequently enters a continuous annealing cycle in which temperatures can surpass 600 °C. This high heat environment allows for complete recrystallization of the previously cold-worked material. The resultant annealed sheet then undergoes another round of cold rolling. This cold rolling can involve areduction of less than 5% through temper / skinpass rolling for single processed material, resulting in ‘single reduced grades’, or a greater reduction (from 5% to 40%) for double processed material, known as ‘double reduced grades’.
[0010] The extent of cold rolling both before and after annealing is contingent upon the specific strength and gauge requirements for the steel. There are several restrictions to this process route, including line speeds, peak temperature (determined by the annealing furnace and the tensile strength of the thin gauge material at high temperature), and rolling loads, for example.
[0011] Various methods have been used to improve the balance of strength and ductility in low carbon sheet steels, for example by controlling the level of recrystallisation during annealing (Y.Z. Li, S.L. Zhao, S.H. He, C.P. Huang, M.X. Huang, Enhancing yield stress and uniform elongation in an ultrathin packaging steel via controlling dislocation density, Int J Plast. 155 (2022) 103334. https: / / doi.Org / 10.1016 / j.ijplas.2022.103334), accumulative roll bonding (M. Oliaei, R. Jamaati, Improvement of the strength-ductility-toughness balance in interstitial free steel by gradient microstructure, (2022), https: / / doi.Org / 10.1016 / j.msea.2022.143237) and a double nitriding route (US10920309B2).
[0012] While the high-strength packaging sector is growing, it still represents a small proportion of the total packaging steels manufactured in relation to softer and more formable grades. Therefore, the commercial applicability of these methods to the manufacturing of packaging steels is limited. The packaging steel sector for food and drinks cans, aerosols, paint tins and luxury packaging, for example, require continuous improvement in sustainability and performance through process optimisation and cost reduction and it is therefore necessary for manufacturing processes to be cost effective and consistent, and to fall within the capability of existing plant production.
[0013] The automotive industry has been revolutionised by dual phase (DP) steels with improved strength and formability characteristics. These dual phase steels typically comprise martensite as a hard second phase, but mixed martensite / bainite second phases within a ferrite matrix are also common. The strength of such steels can be tailored by varying the volume fraction of the second phase. However, productionroutes for the automotive industry are not generally applicable to the production of packaging steels in relation to gauge, for example.
[0014] It is an object of the present invention to provide cost efficient and consistent dual phase (i.e. ferrite and bainite) low carbon steels and manufacturing processes therefor, particularly with application as high strength packaging steels, and more particularly steels with strength greater than 600MPa and elongation greater than 5% in an uncoated state (i.e. blackplate packaging steel strip).
[0015] SUMMARY OF INVENTION
[0016] According to a first aspect of the invention there is provided a method of manufacturing a ferrite / bain ite dual-phase steel strip product with improved strength and formability, wherein the steel is manufactured by:
[0017] providing steel slab or thick strip with a composition in weight percent comprising 0.12-0.15 C, 0.2-0.3 Si, 1.65-1.88 Mn, 0.009-0.02 P, 0.013-0.035 Ni, 0.033-0.083 Al, 0.02-0.03 Nb, 0.25-0.58 Cr, 0.002- 0.007 Mo and 0.0033-0.0087 N with the balance being Fe and impurities;
[0018] hot rolling the steel strip at a hot rolling finishing temperature of at least 850 °C to a first thickness;
[0019] coiling the hot-rolled strip at a coiling temperature of 550-625 °C; subjecting the hot-rolled strip to a primary cold-rolling reduction of 83-90% to a second thickness;
[0020] annealing the primary cold-rolled strip at a peak temperature of 720-755 °C; and
[0021] overaging the annealed strip at 430-530 °C.
[0022] Carbon can increase the strength of the steel, but increasing the carbon content can reduce ductility and weldability.
[0023] Silicon can increase the strength and hardenability of steel to a lesser extent than manganese and carbon, but at high levels can reduce formability.Manganese can increase the strength of steel and in medium manganese steels can exhibit good formability but increasing levels (>10%) can reduce formability.
[0024] Phosphorus can increase the strength of steel, but increasing the phosphorus content can reduce ductility and impact toughness.
[0025] Nickel can increase the corrosion resistance of steel and can improve formability and ductility.
[0026] Aluminum can improve the corrosion resistance of steel with moderate hardenability. Niobium can increase the strength of steel and improve toughness.
[0027] Chromium can harden steel and improve its corrosion resistance.
[0028] Molybdenum can strengthen steel and improve its corrosion resistance.
[0029] Nitrogen can improve the mechanical properties and corrosion resistance of steel when controlled but at large amount can reduce formability and ductility.
[0030] In an embodiment, the composition contains 0.3-0.55 wt.% Cr, preferably 0.35-0.52 wt.% Cr, and more preferably 0.4-0.5 wt. % Cr.
[0031] The dual phase may comprise 6-15% bainite, preferably 8-12% bainite.
[0032] The hot rolling finishing temperature may be 860-880 °C and preferably may be 865-875 °C.
[0033] The first thickness may be 2.5-3.5 mm, preferably 2.75-3.25 mm, and more preferably 2.9-3.1 mm.
[0034] The coiling temperature may be 575-620 °C, preferably 575-625 °C, more preferably 585-625°C and even more preferably 590-610 °C.
[0035] The second thickness may be 0.12-0.53 mm, preferably 0.16-0.51 mm. Even more preferably, the second thickness may be 0.25-0.51 mm, 0.25-0.4 mm, 0.29-0.31 mm, or 0.3 mm.
[0036] The annealing peak temperature may be 730-752 °C, and preferably 740-750 °C. Following annealing, the cooling rate may be 15-160 °C / s, 58-160 °C / s, preferably 68-150 °C / s, and more preferably 78-150 °C / s. Where the cooling rate is 58-160 °C / s, the second thickness may be 0.25-0.53 mm.The annealing may be a continuous annealing cycle with a peak temperature hold having a minimum duration of 45 s, preferably 50 s.
[0037] The overaging temperature may be 440-460 °C, preferably 445-455 °C, and more preferably 450 °C.
[0038] Following overaging, the cooling rate may be 10-32 °C / s, preferably 14-32 °C / s. The overaging temperature may be above the Msfor the composition and within a process window of bainite formation.
[0039] The ferrite / bainite dual phase is formed by the annealing soak and overaging steps. The duration of overaging may be greater than 40 s.
[0040] The overaged strip may be subjected to a secondary cold-rolling reduction of up to 5%.
[0041] The hot-rolled strip may be pickled.
[0042] The steel may be a packaging steel.
[0043] The steel may be aged or bake hardened (BH), for example at 200 °C for 20 minutes, following the annealing, overaging and skinpass / temper or secondary coldrolling reduction up to 5%. Although the preferred BH treatment is 200 °C ± 2°C for 20mins, a temperature as low as 170 °C can be used in line with the EN 10325:2006 standard to measure / report the bake hardening index BH2.
[0044] Prior to tensile testing, the piece may be air cooled to room temperature, which may be approximately 23 °C ± 5°C.
[0045] According to a second aspect of the invention there is provided a ferrite / bainite dualphase steel strip product with improved strength and formability, wherein the product is manufactured according to the method of the first aspect.
[0046] According to a third aspect of the invention there is provided a ferrite / bainite dualphase steel strip product with improved strength and formability, wherein: the strip has a composition in weight percent comprising 0.12-0.15 C, 0.2-0.3 Si, 1.65-1.88 Mn, 0.009-0.02 P, 0.013-0.035 Ni, 0.033-0.083 Al, 0.02- 0.03 Nb, 0.25-0.58 Cr, 0.002-0.007 Mo and 0.0033-87 N with the balance being Fe and impurities;the dual-phase comprises 6-15% bainite;
[0047] the strip has a thickness of 0.16-0.51 mm;
[0048] the strip has a tensile strength greater than 800MPa; and an elongation of 5-10%.
[0049] The strip may have a thickness of 0.2-0.4mm
[0050] The dual phase may comprise 8-12% bainite.
[0051] The steel may be a packaging steel.
[0052] BRIEF DESCRIPTION OF DRAWINGS
[0053] Figure 1 shows a typical profile for the continuous annealing cycle used for the baseline packaging material example.
[0054] Figure 2 shows the tensile behaviour of the baseline steel samples subjected to 0% (i.e. ‘Annealed’), 5%, 7%, 10.7%, 12%, 20% or 24% secondary reduction.
[0055] Figure 3 shows the phase diagram for the composition shown in Table 2.
[0056] Figure 4 shows the Time-Temperature-Transformation (TTT) prediction for the steel shown in Table 2.
[0057] Figure 5 shows a typical profile for the continuous annealing cycle used in Example 1.
[0058] Figure 6 shows the tensile behaviour of the first set of samples of Example 1.
[0059] Figure 7 shows the tensile behaviour of the second set of samples of Example 1 , which have been subjected to a 5% secondary reduction.
[0060] Figure 8 shows a typical profile for the continuous annealing cycle used in Example 2.
[0061] Figure 9 shows the tensile behaviour of the first set of samples of Example 2.
[0062] Figure 10 shows the tensile behaviour of the second set of samples of Example 2, which have been subjected to a 5% secondary reduction.
[0063] Figure 11 shows a typical profile for the continuous annealing cycle used in Example 3.Figure 12 shows the tensile behaviour of the first set of samples of Example 3.
[0064] Figure 13 is an EBSD image showing the microstructure of one of the first set of samples of Example 3.
[0065] Figure 14 shows the tensile behaviour of the second set of samples of Example 3, which have been subjected to a 5% secondary reduction.
[0066] Figure 15 shows a typical profile for the continuous annealing cycle used in Example 4.
[0067] Figure 16 shows the tensile behaviour of the first set of samples of Example 4.
[0068] Figure 17 shows an EBSD image showing the microstructure from a first set samples of Example 4.
[0069] Figure 18 shows the tensile behaviour of the second set of samples of Example 4, which have been subjected to a 5% secondary reduction.
[0070] Figure 19 shows the tensile behaviour of the first set of Example 7 samples.
[0071] Figure 20 is an EBSD image showing the microstructure of one of the first set of samples of Example 7.
[0072] Figure 21 shows the tensile behaviour of the Example 7 samples subjected to a range of tertiary reductions.
[0073] Figure 22 shows the tensile behaviour of the Example 8 samples.
[0074] Figure 23 shows the tensile behaviour of the first set of samples of Example 8.
[0075] Figure 24 shows the tensile behaviour of the second set of samples of Example 8 subjected to a range of tertiary reductions.
[0076] Figure 25 shows the range of tensile behaviour achieved for the baseline packaging example and Examples 2-9.
[0077] DETAILED DESCRIPTION
[0078] The invention will now be described with reference to comparative examples and non-limiting examples according to the invention.All cold rolling reduction was carried out on a Durston F160 single stand mill to 0.1mm accuracy for thicknesses over about 0.4mm and to 0.05mm for thicknesses up to about 0.4mm. The following equation is used to calculate the % reduction:
[0079] % reduction = 100 x (initial thickness - final thickness) / initial thickness
[0080] In each of the stress-strain curves, the strain shown in the X-axis is the engineering strain (% elongation = engineering strain x 100%). The Y-axis represents the corresponding engineering stress. Each line on the stress-strain curves represents a sample.
[0081] Where used, optional pickling was carried out prior to the first cold rolling.
[0082] Primary cold rolling reduction (‘primary reduction’ or PR) refers to a cold reduction from hot rolled steel or band to a primary gauge, which takes place before a first continuous anneal.
[0083] Secondary cold rolling reduction (‘secondary reduction’ or SR) refers to a cold reduction of >5% from the primary gauge following the first continuous anneal (and before a final continuous or batch anneal, where relevant). This is the process used for a conventional double reduced product (so called double reduced grades).
[0084] (Alternatively, following the first continuous anneal, a reduction of less than 5% could be imposed via a temper mill to guarantee flatness and yield point suppression. A reduction of less than 5% is generally not referred to as a reduction, so such a product would generally be referred to as a single reduced material or single reduced grade. However, it will be noted that reductions of 2% in this specification are also referred to as reductions for conciseness.)
[0085] Tertiary cold rolling reduction (‘tertiary reduction’ or TR) refers to a third cold rolling reduction (>5%) following the second continuous anneal or batch anneal process. Continuous annealing was carried out on a Gleeble 3800 coupled with a proportional quench unit. This produces a region of uniform temperature (± 5°C) of around 50 mm length.
[0086] Batch annealing was carried out in a Carbolite RWF 1200 furnace. The temperature was controlled through the furnace temperature. After a 2hr hold, the batch-annealed samples were allowed to air-cool to room temperature.Once the steel samples had been processed according to the described methods, subsize tensile specimens according to the ASTM E8 standard were obtained using a die and 10t hydraulic press. The longitudinal direction of the tensile samples is along the rolling direction of the material. The tensile samples had a gauge length of 25mm and gauge width of 6mm and were tested with an Instron 5985 static machine equipped with a 10 kN load cell and a video extensometer. The cross-head speed used was 1mm / min before 1% strain and 5 mm / min afterwards, and the criteria for end of test was a drop of load by 40%.
[0087] The ASTM E8 samples were mounted in the rolling-normal plane in conductive bakelite (KonductoMet, Buehler (RTM)) and then ground and polished using conventional metallographic preparation procedures. A final colloidal silica (MasterMet 2, Buehler (RTM)) polish was applied using a vibratory polisher (VibroMet 2, Buehler (RTM) for 30 mins to remove any deformation induced during the polishing procedures.
[0088] Where microstructures have been analysed, a JEOL (RTM) 7800F Field Emission Gun (FEG) Scanning Electron Microscope (SEM) equipped with a Symmetry 2 Electron Backscatter Diffraction (EBSD) detector (Oxford Instruments (RTM)) was used. EBSD analysis was performed at 20 kV with a current of ~30 nA with the rolling direction horizontal and the sample tilted to 70°. Data was collected from the centre of the sample at two set magnifications. All maps contained 2048 x 1408 pixels corresponding to step sizes of 0.0516 pm and 0.1135 pm, depending on magnification and were collected at ~2000 Hz. All data was processed in AZtecCrystal software (Oxford Instruments (RTM)).
[0089] Baseline packaging material
[0090] A baseline packaging material example is described to show the strength and elongation of a baseline commercial packaging steel subjected to a range of secondary cold rolling reductions.
[0091] Steel representing a baseline commercial packaging steel with the composition shown in Table 1 was produced using a known manufacturing method.
[0092] Table 1: Composition in wt.% of baseline commercial packaging steelFe Si Mn P Ni Al Nb Ta Cr N Balance 0.071 0.078 0.463 0.007 0.005 0.019 0.004 0.025 0.025 0.012
[0093] (120ppm)
[0094]
[0095] The baseline commercial packaging steel was hot-rolled to a thickness of 2.5mm
[0096] with coil cooling simulated in a laboratory coiling furnace. The hot-rolled strip was pickled using sulfuric acid solution and subjected to cold rolling to a thickness 0.25mm. Samples of 300mm x 25m were cut from the 0.25mm thick strip.
[0097] Continuous annealing was carried out on each of the samples. A peak hold temperature of 635 °C and an overage temperature of 310 °C was used. The typical profile for the continuous annealing cycle is shown in Figure 1 , with the hold temperature usually within the recrystallisation regime, ideally with the avoidance of grain growth within a range of 625-665 °C. The overage temperature can be 300-350 °C. Both the peak hold and overaging temperature are important for imparting the correct balance of properties and phases (especially tempered martensite during overaging depending on C content), as well as influencing the amount of solute C and carbide precipitation.
[0098] At this stage, a first set of the baseline samples was analysed, i.e. without any
[0099] further cold rolling (i.e. 0% secondary reduction) after the described annealing and overage steps. The remaining samples were subjected to cold rolling to achieve a range of secondary reductions, including 5%, 7%, 10.7%, 12%, 20% and 24% SR.
[0100] Figure 2 shows the tensile behaviour of the baseline steel samples subjected to 0% (i.e. ‘Annealed’), 5%, 7%, 10.7%, 12%, 20% or 24% secondary reduction. This
[0101] shows that for the example baseline steel, the resulting strength of the product can be tailored using the secondary reduction, with increasing secondary reductions resulting in increasing strength. However, it is difficult to achieve strengths of over 600 MPa while maintaining any ductility in the strip as the elongation for a strength less than 600MPa falls below 5%.
[0102] Examples
[0103] Examples 1-4 utilise a single continuous annealing cycle. These examples demonstrate the importance of the secondary phase (whether martensite or bainite)on the final mechanical properties of the resulting product. A range of peak hold temperatures were used in Examples 2-4 since reducing the peak hold temperature is important for a number of reasons, including energy savings, oxidation reduction, and buckling changes brought on by phase transformations, continuous annealing steering issues and entry gauge.
[0104] Examples 5-7 utilise two continuous annealing cycles: an initial intercritical continuous annealing cycle followed by cold-rolling and a second sub-intercritical continuous annealing cycle.
[0105] Examples 8-9 utilise a an initial intercritical continuous annealing cycle followed by cold-rolling and a second sub-intercritical batch anneal. Such a process is particularly relevant for offering a less intrusive annealing process to the production line while giving stable properties.
[0106] For each of the following examples, steel with a composition shown in Table 2 was produced using a known manufacturing method. The steel was cast into slabs and hot rolled in both roughing and finishing stands to a gauge of 3mm with a finish rolling temperature of 870°C ±10 °C and coiled at 600 °C, and comprised a ferrite and pearlite microstructure with typical hot strength of 600 ±50 MPa. The ferrite / pearlite microstructure is formed by these hot rolling and coiling steps. (A 3mm gauge is a typical hot rolled gauge used for the automotive sector to produce hard iron of 1-2mm before continuous annealing and galvanising.)
[0107] Table 2: Composition in wt.% of steel use for examples 1-9
[0108] Fe C Si Mn P Ni Al Nb Cr Mo N Balanc 0.14 0.25 1.83 0.015 0.02 0.05 0.03 0.55 0.00 0.0055 e 5 (55ppm)
[0109]
[0110] Figure 3 shows the phase diagram for this material using Thermo-Calc (RTM) software and the TCFe10 database. Ae1 and Ae3 temperatures of 676 °C and 802 °C, respectively, are predicted and shown. In order to achieve high strength and ductility, during annealing a peak hold temperature of around or below 750 °C isused, therefore forming less than 50% austenite in equilibrium during the peak temperature hold. Figure 3 indicates that an austenitic phase developed during heating depends on cementite dissolution. The cementite dissolution temperature is predicted to be about 710 °C so the peak temperature is higher than 710 °C.
[0111] It is noted that the composition has a wt.% of Cr which is outside the range specified in the EN10202:2022 standard. For the claimed range of chromium in the composition, calculations show that Ae1 and Ae3 temperatures will not be affected. The main role of Cr in low carbon DP steels is to retard the formation of pearlite and improve hardenability, as well as corrosion and wear resistance. Cr levels lower than the claimed range will result in slight changes to the Ac1 / Ac3, as well as the martensite start (Ms). Reducing the Cr level (to 0.25 and below) will also affect microstructure refinement, especially the ferrite grain size and subsequent recrystallisation. However, for a reduction in Crfrom 0.55 wt.% to 0.5 wt. %, or even 0.25 wt. %, for compliance with EN10202:2022, no major changes in behaviour are anticipated.
[0112] Figure 4 shows the Time-Temperature-Transformation (TTT) prediction for the steel shown in Table 2, with a predicted austenite grain size of 10 pm. The TTT predictions were performed using JMatPro 14 (RTM) software and the “General steels” database, and a prior austenite grain size of 10 pm with an austenitisation temperature of 820 °C has been assumed. TTT rather than Continuous-Cooling-Transformation (CCT) predictions were used due to rapid cooling and isothermal hold during the overage portion of the annealing cycle.
[0113] An Ms temperature of 385 °C (and Mf temperature of 273 °C) has been predicted with bainite forming at temperatures below 560 °C. The nose of the bainite curve (bainite 0.1%) has been predicted via JMatpro 14 to be around 500 °C, so a window of 430-530 °C should give complete bainite transformation within the hold / overaging times appropriate for continuous annealing of packaging steels (i.e. 40-90s, preferably 40-80s). These values are compatible with a speed line of 250-500 m / min, as per the TTT diagram of Figure 4. Typical cooling rates of 68 °C / s to over 150 °C / s prior to overaging are consistent with current practices and speed ranges (e.g. 250-500 m / min). The TTT of Figure 4 also indicates that wider cooling rates are possible for bainite transformation to occur. Cooling rates as low as 15 °C / s or slightly belowcan be employed and still form a ferrite and bainite structure within the bainite formation regime, for example as in Examples 5-9.
[0114] The 3 mm hot-rolled strip was subjected to a range of processing conditions, as described in the below examples.
[0115] 1) Single continuous annealing cycle
[0116] Example 1:
[0117] This method was used to produce a martensitic second phase, for comparison with Examples 2-4, which comprise a bainite second phase as described below.
[0118] Specifically, in order to allow a martensitic second phase to form, an overage temperature of 310°C was used, which is within the lower range of a usual overage. However, because this temperature is between the steel's Msand Mf temperatures (385 °C and 273 °C, respectively, as shown in Figure 4), there is a chance for untempered martensite and conseguently free carbon to form.
[0119] The 3mm hot-rolled strip was HCI pickled and primary cold rolled to give an 83% total reduction and a thickness of 0.51mm, which is within the upper range of packaging steel grade. (It should be noted that increasing the reduction to 85-90% would have minimum effects on subseguent transformation and the properties of the resulting product, with only the recrystallisation kinetics being faster. It would also be possible to start with a hot rolled gauge of 2.5-3 mm.)
[0120] Samples of 300mm x 25mm were cut from the 0.51 mm thick strip. Each of the samples was subjected to a continuous annealing cycle with a peak temperature of 740 °C. The samples were then overaged at a temperature of 310 °C. The typical profile for the continuous annealing cycle is shown in Figure 5. At this stage, a first set of the samples was analysed, and the tensile behaviour of the first set of samples is shown in Figure 6.
[0121] Figure 6 shows a substantial amount of discontinuous yielding, which is followed by a phase of minimal work hardening. A UTS of 648 MPa is observed.
[0122] A second set of the samples were subjected to a secondary reduction of 5% after the annealing and overaging steps. Figure 7 shows the tensile behaviour of the samplesfollowing 5% secondary reduction. Figure 7 shows that the samples no longer exhibit discontinuous yielding.
[0123] Example 2:
[0124] This method utilises a peak temperature of 740 °C and an overage temperature of 450°C to form a ferrite / bainite dual phase. The overage temperature has been selected to produce a bainite second phase according to the data presented in Figure 4, which indicates that the overage temperature is well within the range of bainite formation between for a hold between 45s (soak) and 90s (overage), and slightly below the bainite nose temperature predicted by the TTT diagram in Figure 4. The overage temperature may be selected in relation to achievable hold temperatures on a continuous annealing line. For these conditions, typical cooling rates from the peak hold temperature and high continuous annealing line speed (to reach the overage hold temperature) are around 125 ±5 °C Is or higher, in line with cooling rate regime for bainite formation. At lower speeds, typical cooling rate for bainite formation (250mpm speed or below) will be in the range of 68 ±5 °C Is or lower for the gauges considered.
[0125] The 3mm hot-rolled strip was HCI pickled and primary cold rolled to a thickness of 0.51mm giving an 83% total reduction. Samples of 300mm x 25mm were cut from the 0.51 mm thick strip.
[0126] Each of the samples was subjected to a continuous annealing cycle with a peak temperature of 740 °C, which is above the cementite dissolution temperature shown in Figure 3. The samples were then overaged at a temperature of 450 °C. The typical profile for the continuous annealing cycle is shown in Figure 8, which shows a cooling rate of 93 °C / s following continuous annealing, and a cooling rate of 21.5 °C / s following overaging. However, cooling rates of 78-150 °C / s and above (between the peak hold and overage) and 14-32 °C / s and above (from overage to room temperature), respectively, are possible. Heating rates of 15 ±7 °C / s for the range of speeds to be considered (250-500mpm) are well within Figure 4 limits. However, the key parameters are the critical cooling rate ranges and soak / overage time.
[0127] At this stage, a first set of the samples was analysed, and the tensile behaviour of the first set of samples is shown in Figure 9.Figure 9 shows that the resulting samples exhibit a substantially lower initial yield strength than the samples in Example 1 (i.e. with the martensitic second phase) before secondary reduction. A smooth work hardening curve is evident, leading to a significantly higher UTS of 810 MPa. This may be the result of cementite spheroidization, which significantly decreased the amount of discontinuous yielding. A second set of samples were subjected to a secondary reduction of 5% after annealing and overaging. Figure 10 shows the tensile behaviour of the samples following secondary reduction. The samples show more work hardening than the Example 1 samples (i.e. those with the martensitic second phase) after secondary reduction, and no discontinuous yielding with a UTS of up to 900 MPa.
[0128] Example 3:
[0129] This method utilises an overage temperature of 450 °C to produce a bainite second phase (according to Figure 4), and a hold temperature of 720 °C which is very close to the cementite dissolution temperature predicted in Figure 3.
[0130] At 720 °C, the driving force for austenitisation is relatively low, and dissolution of cementite is required (which will be dependent on the cementite carbide size and composition). It is known that Mn can substitute Fe in cementite and increase its stability to dissolution (Mueller, J.J.et a, In Proceedings of the International Symposium on New Developments in Advanced High-Strength Sheet Steels Vail, Colorado, USA 19-22 June, 2023; pp. 215-223 , Briki et al, Journal of Metallurgy 2012, 2012, 841901, https: / / doi.org / 10.1155 / 2012 / 841901.), as well as the austenite fraction having high temperature sensitivity (Figure 3). This is expected to give greater variability in the amount of austenite achieved during the hold at 720°C compared to the hold at 750 °C.
[0131] The 3 mm hot-rolled strip was HCI pickled and cold rolled to a thickness of 0.51mm giving an 83% total reduction. Samples of 300mm x 25mm were cut from the 0.51mm thick strip.
[0132] Each of the samples was subjected to a continuous annealing cycle with a peak hold temperature of 720 °C and overaged at a temperature of 450 °C. The typical profile for the continuous annealing cycle is shown in Figure 11 which shows a cooling rate of 87 °C / s following continuous annealing, and a cooling rate of 21.5 °C / s followingoveraging. However, cooling rates of 72-130 °C / s and 14-32 °C / s, respectively, are possible, which are well within the range of cooling rates possible for bainite formation as per Figure 4 (68-150 °C / s, or above). This is also compatible with a range of line speeds considered (250-500 m / min). More generally, a cooling rate of 20-160 °C / s is appropriate for the formation of bainite within the bainite transformation regime.
[0133] At this stage, a first set of the samples was analysed, and the tensile behaviour of the first set of samples is shown in Figure 12, with a maximum UTS of 800 MPa. Figure 12 shows that the repeatability of the samples processed with a peak hold temperature of 720 °C is poor. The development of the early 20-30% austenite phase during heating is relatively rapid and likely depends on cementite dissolution, as observed in Figure 3. This crucial area causes the second phase to be less consistent.
[0134] Figure 13 is an EBSD image showing the microstructure of the sample after continuous annealing with a peak hold temperature of 720°C and with an overage temperature of 450°C (with no secondary reduction). A 6% volume fraction of bainite has been measured, although it was observed in the tensile tests a large scatter macroscopically is present, demonstrating that at this hold temperature, the second phase fraction is variable. The weighted mean grain size is 3.5 pm.
[0135] A second set of samples were subjected to a secondary reduction of 5% after annealing and overaging. Figure 14 shows the tensile behaviour of the samples following SR, with a UTS of 840-880MPa.
[0136] Example 4:
[0137] This method utilises an overage temperature of 450 °C to produce a bainite second phase according to Figure 4, and a peak hold temperature of 750 °C, which is well above the cementite dissolution temperature as predicted in Figure 3.
[0138] The 3 mm hot-rolled strip was HCI pickled and cold rolled to a thickness of 0.51mm giving a 83% total reduction. Samples of 300mm x 25mm were cut from the 0.51 mm thick strip.Each of the samples was subjected to a continuous annealing cycle with a peak hold temperature of 750 °C away from the cementite dissolution temperature predicted in Figure 3. The samples were then overaged at a temperature of 450 °C. The typical profile for the continuous annealing cycle is shown in Figure 15 which shows a cooling rate of 97 °C Is following continuous annealing, and a cooling rate of 21.5 °C Is following overaging. However, cooling rates of 68-150 °C Is and above and 14-32 °C Is, respectively, are possible, well within the bainite formation predicted by Figure 4. These cooling rates are also compatible with line speeds of considerations 250-500 m / min. More generally, a cooling rate of 20-160 °C / s is appropriate for the formation of bainite within the bainite transformation regime.
[0139] At this stage, a first set of the samples was analysed, and the tensile behaviour of the first set of samples is shown in Figure 16, which shows that the repeatability of the results dramatically increased with a peak temperature of 750 °C, as well as reading UTS of around 900 MPa. This temperature is well above the cementite dissolution temperature predicted in Figure 3, which seems to be adequate to enable the material to become much more homogeneous. As explained in Example 3, 750 °C is preferable for cementite dissolution and austenite formation.
[0140] Figure 17 is an EBSD image showing the microstructure of a sample of the resulting product produced at a 750°C hold with an overage temperature of 450°C (without any secondary reduction). A 12% volume fraction of bainite is present, which is greater than the bainite fraction produced in Example 3. The weighted mean grain size is 3.5 pm.
[0141] A second set of samples were subjected to a secondary reduction of 5% after annealing and overaging. Figure 18 shows the tensile behaviour of the samples following secondary reduction, highlighting the consistency of the tensile results by intercritically annealing well above the cementite dissolution temperature (predicted to be about 710°C) unlike Example 3, with UTS reaching close to 1000MPa with max 8% elongation.
[0142] 2) First intercritical continuous annealing cycle and second sub-intercritical continuous annealing cycle
[0143] Due to line restrictions during continuous annealing, annealing at intercritical temperatures at a final gauge (for example 0.25-0.51 mm) can be challenging due tothe phase transformation and maintaining line tension, while managing steering and buckling propensity. However, intercritical annealing in strip product with a gauge of 1 ,2mm and above is commonplace as this feeds the automotive sector.
[0144] The first continuous annealing cycle of examples 5-7 aims to achieve a dual-phase microstructure similar to that resulting from the single continuous annealing cycle of Examples 2-4, but in a 1.2mm gauge intermediate product. This is followed by secondary reduction to achieve a gauge of 0.3mm. The 0.3 mm strip then undergoes a more conventional low-temperature (or sub-critical) annealing process and overage to facilitate recrystallization.
[0145] Example 5
[0146] The 3mm hot-rolled strip was subjected to primary reduction to a thickness of 1 ,2mm (60% reduction). Samples of 300mm x 25mm were cut from the 1 ,2mm thick strip. Each of the 1 ,2mm samples was subjected to an initial continuous annealing cycle with a peak hold temperature of 750 °C, with cooling at a rate of 25-40 °C / s which is sufficient to form bainite according to the TTT plot in Figure 4 with an overage of 450 °C, with cooling at a rate of 4 °C / s. Heating rates were 2-6 °C / s.
[0147] At a 1.2 mm gauge (which is used to integrate the process with automotive sector processes), the effective cooling rate is reduced compared to Examples 2-4.
[0148] However, cooling rates of 15-50 °C / s (from the initial annealing cycle) to form bainite and 2-15 °C / s (post overaging), respectively, are possible, within the bainite transformation regime.
[0149] The samples were then subjected to a secondary cold roll reduction to a thickness of 0.3mm (75% reduction) and then to continuous annealing at 650 °C (for 45s) with a cooling rate of 130 °C / s, although a range of 58-144 °C / s is possible. The samples were then overaged at 380 °C (for 60s) with a cooling rate of 27 °C / s. A cooling rate of 12-30 °C / s following overaging is possible.
[0150] At this stage, the samples were analysed. Figure 19 shows the tensile behaviour of the resulting samples. It is observable that the strip has not undergone recrystallization after the second continuous annealing cycle of 650 °C, resulting in poor ductility.Example 6:
[0151] The 3mm hot-rolled strip was subjected to cold roll reduction to a thickness of 1 ,2mm (60% reduction). Samples of 300mm x 25mm were cut from the 1 ,2mm thick strip. Each of the 1 ,2mm samples was subjected to an initial continuous annealing cycle with a peak hold temperature of 750 °C, with a cooling at a rate of 25-40 °C / s, which is sufficient to form bainite according to the TTT plot of Figure 4 with an overage of 450 °C, with cooling at a rate of 4 °C / s. Heating rates were 2-6 °C / s.
[0152] At a 1.2 mm gauge (which is used to integrate the process with automotive sector processes), the effective cooling rate is reduced compared to Examples 2-4.
[0153] However, cooling rates of 15-50 °C / s (from the initial annealing cycle) to form bainite and 2-15 °C / s (post overaging), respectively, are possible, within the bainite transformation regime.
[0154] The samples were then subjected to a secondary cold roll reduction to a thickness of 0.3mm (75% reduction) and then to continuous annealing at 675 °C (for 45s), with cooling at a rate of 140 °C / s, although rates of 63-158 °C / s are possible. The samples were then overaged at 380 °C (for 60s), with cooling at a rate of 27 °C / s, with a possible rate of 12-30 °C / s.
[0155] Figure 19 shows the tensile behaviour of the resulting samples, annealed at 650 °C, 675 °C and 685 °C. Following the secondary reduction, complete recrystallisation is anticipated to occur at 675 °C with a typical UTS of 600 MPa, similar to Example 7, below.
[0156] It can be seen that similar properties are achieved for the 675 °C and 685 °C continuous annealing cycles suggesting the material has a relatively wide process window to achieve consistent properties
[0157] Example 7:
[0158] The 3mm hot-rolled strip was subjected to cold roll reduction to a thickness of 1 ,2mm (60% reduction). Samples of 300mm x 25mm were cut from the 1 ,2mm thick strip. Each of the 1 ,2mm samples was subjected to an initial continuous annealing cycle with a peak hold temperature of 750 °C, with a cooling at a rate of 25-40 °C / s, whichis sufficient to form bainite according to the TTT plot of Figure 4 with an overage of 450 °C, with cooling at a rate of 4 °C / s. Heating rates were 2-6 °C / s.
[0159] At a 1.2 mm gauge (which is used to integrate the process with automotive sector processes), the effective cooling rate is reduced compared to Examples 2-4.
[0160] However, cooling rates of 15-50 °C / s (from the initial annealing cycle) to form bainite and 2-15 °C / s (post overaging), respectively, are possible, within the bainite forming regime.
[0161] The samples were then subjected to a secondary cold roll reduction to a thickness of 0.3mm (75% reduction) and then to continuous annealing at 685 °C (for 45s), with a cooling rate of 150 °C / s. The samples were then overaged at 380 °C (for 60s), with a cooling rate of 27 °C / s. Cooling rates of 66-165 °C / s and 12-30 °C / s, respectively, are possible, within the bainite transformation regime.
[0162] At this stage, a first set of the samples (i.e. with 0% secondary reduction) were analysed, and Figure 19 shows the tensile behaviour of the resulting samples. Figure 20 is an EBSD image showing the microstructure of a sample of the resulting strip. Figure 20 shows complete recrystallisation and a quasi-equiaxed grain structure. Furthermore, the samples of Example 6 and Example 7 demonstrate consistent tensile properties, indicating a reasonable process window.
[0163] Notably, there is no apparent substantial grain growth at the higher temperature (i.e between the peak temperature of 675 °C and 685 °C), thereby mitigating the potential reduction in strength that could result from such growth. However, the grain size is coarser than when utilising single processing (i.e. a single continuous annealing cycle, as shown in Examples 1-4).
[0164] This double processing method using a first continuous annealing cycle with a peak temperature of 750 °C and a second continuous annealing cycle with a peak temperature of 685 °C has resulted in a final grain size of 6.5 pm, which is greater than the final grain size of 3.5pm shown for the single processing method in Examples 3 and 4, for example. This is likely due to the reduced deformation prior to annealing, reducing the driving force for recrystallisation and therefore obtaining a coarser microstructure.According to the below Hall-Petch relationship (UTS = 700 + 1000D-1 / 2, where D = grain size in microns), the difference in grain size between Example 4 and Example 7 would account for approximately 160 MPa drop in UTS. However, compared to Example 4, around 230 MPa has been lost, which is 70 MPa more than 160 MPa and therefore the fragmentation and likely spheroidisation of the bainite during the secondary rolling and annealing may have also contributed to the loss of strength. At this stage, a second set of the samples were subjected to a final, tertiary cold rolling reduction of 2%, 5% or 7%.
[0165] Figure 21 and Table 3 show the tensile behaviour of the samples subjected to 0%, 2%, 5% and 7% tertiary reduction, and specifically the strength evolution attained through tertiary reduction following the 685°C sub-critical annealing cycle. Notably, while an enhancement in strength is evident, there is a pronounced decrease in total elongation (% elongation = engineering strain x 100%).
[0166] Table 3: Tensile behaviour of Example 7 samples subjected to 0%, 2%, 5% and 7% tertiary reduction
[0167] Tertiary reduction UTS Elongation
[0168] 0% 600 23%
[0169] 2% 605 18%
[0170] 5% 610 14%
[0171] 7% 651 12%
[0172]
[0173] Specifically, an average increase of 51 MPa in UTS was observed alongside a 11% reduction in elongation following a 7% tertiary reduction. Comparatively, employing the same secondary reduction in the baseline material led to an 80 MPa increase in UTS; however, this was accompanied by nearly a 20% loss in elongation (as shown in Figure 2).
[0174] 3) First intercritical continuous annealing cycle and second sub-intercritical batch annealing cycleExample 8:
[0175] The 3mm hot-rolled strip was subjected to cold roll reduction to a thickness of 1 ,2mm (60% reduction) prior to the first continuous annealing process. Samples of 300mm x 25mm were cut from the 1 ,2mm thick strip.
[0176] Each of the samples was subjected to an initial continuous annealing cycle with a peak temperature of 750 °C, with a cooling at a rate of 25-40 °C / s, which is sufficient to form bainite according to the TTT plot of Figure 4 with an overage of 450 °C, with a cooling rate of 4 °C / s. Heating rates were 2-6 °C / s.
[0177] At a 1.2 mm gauge (which is used to integrate the process with automotive sector processes), the effective cooling rate is reduced compared to Examples 2-4.
[0178] However, cooling rates of 15-50 °C / s (from the initial annealing cycle) to form bainite and 2-15 °C / s (post overaging), respectively, are possible, within the bainite forming regime. The samples were then subjected to further cold rolling reduction to a thickness of 0.3mm (75% reduction).
[0179] At this stage, the samples underwent batch annealing at 650 °C for 2 hours, followed by air cooling in the furnace (i.e. with the furnace door open) to room temperature, with a typical cooling rate of 0.5 °C / s (with a range of 0.3-10 °C / s).
[0180] Figure 22 shows the tensile behaviour of the resulting samples. The samples had an average 0.2% proof stress of 490±10 MPa and UTS of 550±9 MPa and total elongation values of 23±2%.
[0181] Example 9:
[0182] The 3mm hot-rolled strip was subjected to primary cold roll reduction to a thickness of 1 ,2mm (60% reduction) prior to the first continuous annealing process. Samples of 300mm x 25mm were cut from the 1 ,2mm thick strip.
[0183] Each of the samples was subjected to an initial continuous annealing cycle with a peak temperature of 750 °C, with a cooling at a rate of 25-40 °C / s, which is sufficient to form bainite according to the TTT plot of Figure 4 with an overage of 450 °C, with a cooling rate of 4 °C / s. Heating rates were 2-6 °C / s.
[0184] At a 1.2 mm gauge (which is used to integrate the process with automotive sector processes), the effective cooling rate is reduced compared to Examples 2-4.However, cooling rates of 15-50 °C / s (from the initial annealing cycle) to form bainite and 2-15 °C / s (post overaging), respectively, are possible, within the bainite forming regime.
[0185] The samples were then subjected to secondary cold rolling reduction to a thickness of 0.3mm (75% reduction).
[0186] At this stage, the samples underwent batch annealing at 670 °C for 2 hours, followed by air cooling in the furnace (i.e. with the furnace door open) to room temperature, with a typical cooling rate of 0.5 °C / s (with a range of 0.3-10 °C / s).
[0187] Figure 23 shows the tensile behaviour of a first set of the resulting samples (i.e. with 0% SR). The samples had an average 0.2% proof stress of 470±4 MPa, UTS of 520±5 MPa and total elongation values of 23±3%.
[0188] A second set of the samples was subjected to tertiary cold rolling reduction of 5%, 8% or 10%, and Figure 24 shows their tensile behaviour. A UTS of 632 MPa is achieved through a 10% tertiary reduction while maintaining an 8% total elongation, giving a final gauge of 0.27mm.
[0189] Conclusion
[0190] Figure 25 shows the range of tensile behaviour achieved for the baseline packaging example and Examples 2-9.
[0191] Examples 1-9 exhibit enhanced properties compared to the baseline grade.
[0192] Examples 2-4 demonstrate the most favourable combination of strength and ductility. The formation of fine grain size and isolated bainite during the annealing process contributes to the preferential enhancement of strength and ductility properties.
[0193] However, when transitioning to the two annealing cycles of Examples 5-9, little discrepancy is observed between them.
[0194] In Examples utilising a second annealing cycle, the second phase (bainite) is generated during the first continuous annealing cycle. Consequently, during subsequent cold rolling, the bainite undergoes fragmentation while providing limited strain to achieve the final gauge (true strain of 1.3). This, in turn, results in a less refined final ferrite grain size compared to cold rolling directly from 3mm gauge (true strain of around 2.3).The single continuous annealing cycle used in Examples 2-4 to generate a ferrite I bainite microstructure offers an excellent balance of strength and ductility.
[0195] The single continuous annealing cycle used in Example 1 to generate a ferrite I martensite microstructure also showed an increase in performance compared to conventional packaging steel. However, a significant amount of discontinuous yielding was seen which in turn gave a reduced performance compared to ferrite I bainite, which shows a smoother work hardening profile.
[0196] While intercritical annealing at a peak hold temperature of 720 °C and 750 °C shows significant improvements, 750 °C showed a much greater level of consistency both pre- and post-tertiary or final reduction.
[0197] The double processing method use in Examples 5-9 (either with continuous annealing for Examples 5-7 or batch annealing for Examples 8 and 9) shows very consistent performance with an improvement over conventional packaging steel and uses pre-existing annealing cycles, but is less effective and more costly than single processing, unless the process utilises a versatile intermediate product such as the 1 ,2mm strip which can be used in the automotive sector and be further processed for use in the packaging sector.
[0198] The role of the final reduction (whether secondary or tertiary) appears to be consistent between the dual phase and conventional packaging steels with approximately 5 MPa of strength coming at the cost of 1% total elongation. Overall, for a product requiring 10% total elongation, via single processing a strength of 900 MPa can be achieved, while via two step-annealing approximately 650 MPa can be achieved. Examples 1-9 show improved properties compared to the conventional packaging steel which offers a strength of approximately 515 MPa.
[0199] While the present invention is particularly relevant to the packaging industry, it will be appreciated that the properties of the invention make it applicable to other industries, for example the automotive industry.
Claims
CLAIMS1. A method of manufacturing a ferrite / bainite dual-phase steel strip product with improved strength and formability, wherein the steel is manufactured by:providing steel slab or thick strip with a composition in weight percent comprising 0.12-0.15 C, 0.2-0.3 Si, 1.65-1.88 Mn, 0.009-0.02 P, 0.013-0.035 Ni, 0.033-0.083 Al, 0.02-0.03 Nb, 0.25-0.58 Cr, 0.002- 0.007 Mo and 0.0033-0.0087 N with the balance being Fe and impurities;hot rolling the steel strip at a hot rolling finishing temperature of at least 850 °C to a first thickness;coiling the hot-rolled strip at a coiling temperature of 550-625 °C; subjecting the hot-rolled strip to a primary cold-rolling reduction of 83-90% to a second thickness;annealing the primary cold-rolled strip at a peak temperature of 720-755 °C; andoveraging the annealed strip at 430-530 °C.
2. A method of manufacturing according to claim 1 , wherein the composition contains 0.3-0.55 wt.% Cr, preferably 0.35-0.52 wt.% Cr, and more preferably 0.4-0.5 wt. % Cr.
3. A method of manufacturing according to claim 2 or 3, wherein the hot rolling finishing temperature is 860-880 °C and preferably 865-875 °C.
4. A method of manufacturing according to any preceding claim, wherein the first thickness is 2.5-3.5 mm, preferably 2.75-3.25 mm, and more preferably 2.9- 3.1 mm.
5. A method of manufacturing according to any preceding claim, wherein the coiling temperature is 575-620 °C, preferably 590-610 °C.
6. A method of manufacturing according to any preceding claim, wherein the second thickness is 0.25-0.51 mm.
7. A method of manufacturing according to any of preceding claim, wherein the annealing peak temperature is 730-752 °C, preferably 740-750 °C.
8. A method of manufacturing according to any preceding claim, wherein the annealing is a continuous annealing cycle with a peak temperature hold having a minimum duration of 45s.
9. A method of manufacturing according to any preceding claim, wherein the overaging temperature is 440-460, preferably 445-455 °C, and more preferably 450 °C.
10. A method of manufacturing according to any preceding claim, wherein the overaging temperature is above the Msfor the composition and within a process window of bainite formation.
11. A method of manufacturing according to any preceding claim, wherein the duration of overaging is greater than 40 s.
12. A method of manufacturing according to any preceding claim, wherein the overaged strip is subjected to a secondary cold-rolling reduction of up to 5%.
13. A method of manufacturing according to any preceding claim, wherein the hot- rolled strip is pickled.
14. A method of manufacturing according to any preceding claim, wherein the steel is a packaging steel.
15. Aferrite / bainite dual-phase steel strip product with improved strength and formability, wherein the product is manufactured according to the method of any of claims 1-14.
16. Aferrite / bainite dual-phase steel strip product with improved strength and formability, wherein:the strip has a composition in weight percent comprising 0.12-0.15 C, 0.2-0.3 Si, 1.65-1.88 Mn, 0.009-0.02 P, 0.013-0.035 Ni, 0.033-0.083 Al, 0.02- 0.03 Nb, 0.25-0.58 Cr, 0.002-0.007 Mo and 0.0033-87 N with the balance being Fe and impurities;the dual-phase comprises 6-15% bainite;the strip has a thickness of more than 0.16-0.51 mm;the strip has a tensile strength greater than 800MPa; and an elongation of 5-10%.
17. A product according to claim 16 wherein the strip has a thickness of 0.17-0.48mm.
18. A product according to claim 16 or 17, wherein the dual phase comprises 8-12% bainite.
19. A product according to any of claims 16-18, wherein the steel is a packaging steel.