Method for producing liquid resistant paperboard

A multi-ply paperboard production method using kraft pulp and internal sizing agents addresses the challenge of maintaining structural integrity and recyclability in hot beverage cups, achieving plastic-free, recyclable, and environmentally friendly packaging solutions.

WO2026234545A1PCT designated stage Publication Date: 2026-11-12STORA ENSO OYJ
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054387
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-04
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Traditional paperboard used for food packaging, especially for hot beverage cups, faces challenges in maintaining structural integrity and recyclability due to the use of plastic coatings, which are difficult to recycle and contribute to environmental issues.

Method used

A multi-ply paperboard production method involving specific pulp compositions, refining levels, and processing conditions to create a plastic-free paperboard with enhanced liquid resistance and mechanical strength, using kraft pulp, internal sizing agents, and controlled pressing and drying processes.

Benefits of technology

The method produces a paperboard that maintains structural integrity when exposed to hot liquids, is recyclable, and reduces environmental impact by minimizing plastic content, while achieving improved strength, density, and water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000021_0001_TABLE
    Figure IMGF000021_0001_TABLE
Patent Text Reader

Abstract

The present invention relates to a method for producing a multi-ply paperboard suitable for hot beverage cups, the method comprising: providing a first back-ply pulp suspension, a second mid-ply pulp suspension, and a third top-ply pulp suspension, wherein each suspension comprises an internal sizing agent in a range of 1-8 kg / tn; forming three plies wherein the fibers in the outer back- and top-ply suspensions have been refined to a Schopper-Riegler value between 28 - 40 and comprise more than 80 wt% kraft pulp; couching the plies to form a wet multi-ply web; subjecting the web to a dewatering procedure including applying a total wet press impulse greater than 110 kPa*s; drying the web to form the multi-ply paperboard; and subjecting the paperboard to a calendering step. The invention also relates to a multi-ply paperboard.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR PRODUCING LIQUID RESISTANT PAPERBOARD FIELD OF INVENTION

[0002] The present disclosure relates to paperboard materials for food packaging, and to a method for producing a recyclable paperboard suitable for hot beverage cups with good liquid resistance and good rigidity.

[0003] BACKGROUND

[0004] Paper or paperboard for disposable containers and food packaging items, such as cups and trays, are commonly used in the food service industry. These products provide a convenient and hygienic way to serve hot and cold beverages, as well as various food items. The paperboard used for such applications needs to possess certain properties to ensure proper functionality and consumer safety.

[0005] Traditionally, paperboard for food packaging has been coated with plastic materials to enhance its barrier properties against liquids and moisture. This plastic coating helps prevent leakage and maintains the structural integrity of the container when in contact with hot or cold liquids. The plastic layer also provides additional strength and rigidity to the paperboard structure. However, the use of plastic coatings on paperboard presents several challenges from an environmental perspective. Plastic-coated paperboard products are difficult to recycle efficiently, as the plastic and paper components need to be separated. This complicates the recycling process and reduces the overall recyclability of the material. Additionally, many commonly used plastic coatings are not biodegradable or compostable, contributing to longterm environmental issues.

[0006] While paperboard itself offers advantages such as rigidity, stiffness, and thermal insulation compared to plastic alternatives, these properties can be compromised when the board comes into contact with liquids, especially hot beverages. Without a plastic coating, moisture can quickly penetrate the paperboard structure, leading to a loss of rigidity and grip stiffness. This makes it challenging to use uncoated paperboard for applications such as hot beverage cups. It has been appreciated that a method is needed that overcomes one or more of these problems.SUMMARY

[0007] The present invention aims to provide a multi-ply paperboard material suitable for single-use liquid containers, including those for hot beverage paper cups. The present invention also aims to provide a method for producing such a material. One object of the present invention is to enable production of such containers with a minimized plastic content while maintaining sufficient liquid resistance, thus enabling efficient fiber recyclability and fiber reuse and also reduce plastics in disposable containers.

[0008] This summary is provided to introduce a selection of concepts in a simplified form that are further described below in the detailed description. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0009] In a first aspect, a method for producing a multi-ply paperboard suitable for hot beverage cups is provided. The method comprises providing a first back-ply suspension, a second mid-ply suspension, and a third top-ply suspension, wherein each suspension comprises an internal sizing agent in a range of 1-8 kg / t calculated as dry internal sizing weight content per dry fiber weight content; forming three plies from said first, second and third pulp suspensions wherein the fibers in the back- and top-ply suspensions are refined to a Schopper-Riegler value between 28 - 40 according to ISO 5267-1:1999 and comprise more than 80 wt% kraft pulp based on the total fiber content; subjecting the three plies to couching to form a wet multi-ply web; subjecting the wet multi-ply web to a press dewatering procedure using a total wet press impulse greater than 110 kPa*s to obtain a web with a solids content greater than 43% after at least a second or third press; drying the web to form the paperboard with an end moisture content of 5-12%; and subjecting the paperboard to a calendaring step with a calender line load less than 50 kN / m.

[0010] This method allows for production of a paperboard with increased density, reduced permeability, good liquid resistance and improved mechanical properties, suitable for use in production of hot and cold beverage cups, frozen food packages, dry food packages and / or trays without the need for additional plastic coating.The total wet press impulse may be greater than 150 kPa*s, such as greater than 200 kPa*s and below 350 kPa*s. Increasing the total wet press impulse results in higher densification of the paperboard, further reducing air permeability and improving mechanical strength.

[0011] The outer plies, i.e. the back- and top-ply, may be composed of 100% kraft pulp, preferably with an average fiber length between 0.6 - 1.8 mm, more preferably 0.8 - 1.6 mm, where fiber length is length-weighted according to ISO 16065-2:2014 determined e.g. by using Valmet Fiber Analyser FS5 equipped with UHD. In one example, the outer plies are made from bleached hardwood kraft pulp free from OBA / fluorescence whitening agent. Using kraft pulp in the outer plies of the paperboard enhances the strength and barrier properties of the paperboard surface, and bleached pulp may provide advantages in terms of improved organoleptic properties, i.e. cleaner pulp for instance in terms of lower extractives and lower lignin content, low levels of metal ions and other inorganics, and less microbial contaminants. At least one pulp suspension used for an outer ply of the paperboard may be refined to a Schopper-Riegler value above 30 according to standard ISO 5267-1:1999, such as between 30 - 40. Preferably, this is the pulp suspension for the back-ply intended to form an inside surface of a container made from the paperboard according to the invention. It may also be that both back- and top-ply pulp suspensions used to form the outer plies of the final paperboard may be refined to a Schopper-Riegler value greater than or equal to 30 according to ISO 5267-1:1999. Higher refining of the fibers forming the outer plies leads to increased densification and reduced air permeability of the material. It also improves the formation and smoothness of the paperboard surface, enhancing its printability and barrier properties. According to the invention, at least the back-ply of the multi-layer paperboard may have a specific formation lower than 0.7 gA0.5 / m, preferably lower than 0.6 gA0.5 / m measured according to standard SCAN-P 92:09.

[0012] The internal sizing agent may be selected from the group consisting of alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), waxes, rosin, fatty acid, fatty acid derivative, and combinations thereof. These internal sizing agents provide effective liquid repellence, improving the water resistance of the paperboard without the need for external plastic coating. In a second aspect, a multi-ply paperboard suitable for producing hot beverage cups is provided. The paperboard comprises:-a basis weight above 150 g / m2, such as above 200 g / m2 and below 400 g / m2 based on dry weight measured according to standard ISO 536:2019;

[0013] -a density greater than 720 kg / m3, such as greater than 750 kg / m3 or even greater than 800 kg / m3 and less than 1000 kg / m3 measured according to standard ISO 534:2011 based on a single sheet;

[0014] -a compression strength index, GM, greater than 22 Nm / g, such as greater than 24 Nm / g at 50% relative humidity and 23°C measured according to standard ISO 9895:2008;

[0015] -a Cobb300 value less than 40 g / m2 measured according to ISO 535:2023;

[0016] -a hot water Cobb300 value less than 45 g / m2; and

[0017] -a Bendtsen air permeability value less than 120 ml / min measured according to standard ISO 5636-3:2013.

[0018] The paperboard preferably contains at least three plies, wherein the outer plies may have a grammage between 35 - 95 gsm, and the mid-ply of the paperboard may have a grammage between 120 - 250 gsm.

[0019] This paperboard exhibits good liquid resistance, good mechanical strength, and provides barrier properties, making it suitable for producing hot beverage cups without the need for plastic coating or at least significantly reduce the amount of plastic used in coating. The density of the paperboard may be greater than 750 kg / m3, such as greater than 800 kg / m3. In the example where the multi-ply paperboard is a three-ply paperboard, the outer plies comprise a higher density than the mid-ply: for example the outer plies may have a density greater than 700 kg / m3, and the mid-ply may have a density greater than 500 kg / m3. Higher density further improves the strength and barrier properties of the paperboard, enhancing its material’s performance in hot beverage applications with regards to mechanical strength, e.g. SCT-value, and barrier function, e.g. Bendsen air permeability.

[0020] The Cobb300 value may be less than 35 g / m2. A low Cobb300 value indicates good water resistance, further enhancing the paperboard's suitability for hot beverage cups.

[0021] The hot water Cobb300 value for the liquid-contact side of the paperboard (i.e. forming the inside of a papercup), may be less than 40 g / m2. A low hot water Cobb300 value demonstratesgood resistance to hot liquids, making the paperboard particularly suitable for hot beverage applications.

[0022] The paperboard may further have a total reject value or amount of less than 10%, or even less than 5%, according to PTS RH 021 / 97 test method for Category II products. This low PTS reject value indicates efficient disintegration and pulping and thus good recyclability, contributing to the product's sustainability and circular economy potential.

[0023] In summary, in paperboard production, the combination of high total press impulse, specific selection of fibers in the suspensions forming the different plies, balanced level of refining and achieved high solids content after press section contributes to several beneficial properties in the final paperboard product. These properties include:

[0024] -Increased density: The high pressure applied during wet pressing leads to a more compact fiber structure, resulting in a higher density paperboard. Without being bound to any theories, it is believed that fines and / or MFC migrate together with the water toward the web surface during the wet pressing procedure, creating a density gradient, i.e. densifying the surface of the material.

[0025] -Improved strength: The enhanced fiber-to-fiber bonding achieved through wet pressing contributes to high compression strength (SCT), tensile strength, burst strength, and other beneficial mechanical properties. These strength properties, such as the SCT-value, are beneficial particularly for converting the material into containers such as cups, requiring rim roll formation.

[0026] -Enhanced water resistance: The densification of the paperboard structure can improve its resistance to water penetration, which is particularly important for hot beverage cup applications.

[0027] -Improved surface smoothness: The wet pressing process can help create a more uniform surface, potentially enhancing printability and appearance of the final product.

[0028] The foregoing general description of the illustrative examples and the following detailed description thereof are merely exemplary aspects of the teachings of this disclosure and are not restrictive.DETAILED DESCRIPTION

[0029] The following description sets forth exemplary aspects of the present disclosure. It should be recognized, however, that such description is not intended as a limitation on the scope of the present disclosure. Rather, the description also encompasses combinations and modifications to those exemplary aspects described herein.

[0030] The present disclosure relates to a method for producing a multi-ply paperboard suitable for hot beverage cups and the resulting paperboard product. The paperboard produced by this method is designed to be plastic-free or substantially plastic-free while maintaining properties that make it suitable for use in hot beverage applications. This paperboard addresses the need for environmentally friendly packaging solutions that do not compromise on performance. As used herein, "paper" or "paperboard" refers to a paper-based substrate comprising cellulose fibers that include wood and / or plant fibers. A typical paperboard substrate used for packaging material comprises at least one ply, often several plies. The paperboard substrate referred to herein is a multi-ply or multi-layer packaging paperboard, comprising at least three plies: a top- and a back-ply and at least one mid-ply. The paperboard substrate may comprise one or several mid-plies. The paperboard substrate may have a basis weight of at least 150 g / m2, preferably at least 200 g / m2 and below 400 g / m2. Such a multi-ply paperboard is particularly suitable for liquid and / or food packaging.

[0031] It is to be understood that “substantially plastic-free" means that the product comprises a total plastic content of less than 5wt%, or less than 4wt%, or less than 3wt%.

[0032] The present method involves a specific combination of papermaking steps and parameters that result in a paperboard with enhanced properties. These properties include improved rigidity, good liquid resistance, and improved mechanical strength, which are particularly beneficial for food packaging board intended to be used as cup stock, i.e. which is to be converted into single-use cup applications including those for hot beverages. The resulting paperboard can be used to produce cups that maintain their structural integrity when filled with hot liquids, without the need for a plastic lining or coating or with need for a very thin applied barrier thereby reducing the plastic content in the product.

[0033] By eliminating or at least reducing the need for plastic components, the paperboard produced by this method offers advantages in terms of recyclability and environmental impact. Thepaperboard can be more easily recycled or composted compared to traditional plastic-lined cup materials, aligning with growing consumer and industry demands for sustainable packaging solutions.

[0034] The method and resulting paperboard described herein provide a novel approach to addressing the challenges associated with producing plastic-free hot beverage cups, offering a potential alternative to conventional cup materials in the food packaging industry.

[0035] The paperboard preferably contains at least three plies, wherein the outer plies may have a grammage between 35 - 95 gsm, and the mid-ply of the paperboard may have a grammage between 120 - 250 gsm. The compositions of each ply in said paperboard play an important role in achieving the desired properties for e.g. trays or containers such as including hot beverage cup applications, without the need for plastic lining.

[0036] The outer back- and top plies of the paperboard may comprise more than 70 wt%, or more than 80 wt% hardwood kraft pulp made from eucalyptus or birch, preferably bleached hardwood kraft pulp having brightness >78% such as 79-88% according to ISO 2470-1:2009. This contributes to good formability and reduced air permeability as well as increased densification of the final product. In some examples, the outer plies may comprise 100 wt% hardwood kraft pulp to maximize these benefits. The weight-percentages are calculated on the total fiber weight (dry) of the respective layer.

[0037] The mid-ply of the paperboard is preferably predominantly made from kraft pulp. In some examples, the mid-ply comprises more than 50 wt% kraft pulp by dry weight. In some examples, the mid-ply comprises more than 80 wt% kraft pulp, such as more than 90 wt% kraft pulp. The kraft pulp of the mid-ply may be made from hardwood or softwood or a mixture of both. Furthermore, the kraft pulp of the mid-ply may be bleached or unbleached. The kraft pulp of the mid-ply may have a Schopper-Riegler value between 28 - 45.

[0038] In some examples, the mid-ply may contain a combination of kraft pulp and chemithermomechanical pulp (CTMP), preferably bleached softwood CTMP. In such examples, the proportion of kraft pulp in the mid-ply is greater than 50 wt% and the proportion of CTMP in the mid-ply is less than 50 wt%, such as between 10 - 40 wt% of the total fiber content. Preferably, the proportion of kraft pulp in the mid-ply exceeds the proportion of CTMPby dry weight. Preferably, the proportion of kraft pulp in such a mid-ply fiber composition, i.e. based on a combination of kraft pulp and CTMP, is greater than 50 wt%.

[0039] In some other examples, the mid-ply may contain a combination of kraft pulp and broke and optionally CTMP, such as between 40 - 80 wt% kraft pulp, such as between 50 - 70 wt% kraft pulp; 0 - 50 wt% broke; and 0 - 30 wt% CTMP, preferably bleached softwood CTMP.

[0040] The CTMP used in the mid-ply is preferably bleached softwood CTMP. Preferably, the CTMP used in the mid-ply has a Schopper-Riegler value between 20 - 40, such as between 25 - 35 to promote densification. The inclusion of CTMP in the mid-ply provides additional rigidity and stiffness to the paperboard while maintaining a cost-effective composition.

[0041] In addition to kraft pulp and optional CTMP and / or broke, the mid-ply may include microfibri Hated cellulose (MFC) in an amount between 1 - 15 wt%, such as 1.5 - 7.5 wt% or between 1.5- 5 wt% of the total fiber content in the mid-ply. The addition of MFC may increase strength of the material and prevent delamination e.g. during converting operations, and can also further enhance the densification of the paperboard, contributing to improved barrier properties. Microfibrillated cellulose (MFC) shall in the context of the patent application be understood to mean a cellulose particle, fiber or fibril having a width or diameter of from 20 nm to 1000 nm. MFC can also refer to highly refined cellulose having a SR value above 85, or cellulose fines, or combination thereof. Various methods exist to make MFC, such as single or multiple pass refining, pre-hydrolysis followed by refining or high shear disintegration or liberation of fibrils. One or several pre-treatment steps is usually required in order to make MFC manufacturing both energy efficient and sustainable. The cellulose fibers of the pulp used when producing MFC may thus be native or pre-treated enzymatically or chemically, for example to reduce the quantity of hemicellulose or lignin. MFC can be produced from wood cellulose fibers, both from hardwood and softwood fibers. It can also be made from microbial sources, agricultural fibers such as wheat straw pulp, bamboo, bagasse, or other non-wood fiber sources. It can be made from pulp, including pulp from virgin fiber, e.g. mechanical, chemical and / or thermomechanical pulps. It can also be made from broke or recycled paper. In a preferred example, the outer plies comprise a higher density than the mid-ply: for example the outer plies may have a density greater than 700 kg / m3, and the mid-ply may have a density greater than 500 kg / m3, such as greater than 550 kg / m3.The combination of said pulp types in specific proportions allows for a dense paperboard structure that balances strength, rigidity, and liquid resistance. Internal sizing of the different paperboard layers further provides liquid resistance, and refining the fibers of the outer plies combined with wet pressing during production leads to increased density and reduced air permeability, making the end material suitable for hot beverage cup applications. The use of refined hardwood kraft pulp in high proportions, particularly in the outer plies, in combination with wet pressing at higher loads provides several benefits. Kraft pulp fibers provides good formation, good retention of internal sizing agents, good strength and ability to form strong inter-fiber bonds, which contributes to the overall structural integrity of the paperboard. This is particularly important for maintaining cup rigidity when the cup contacts hot liquids.

[0042] The optional inclusion of CTMP in the mid-ply provides bulk and opacity to the paperboard while maintaining good strength properties.

[0043] By carefully balancing these components in the paperboard composition, it is possible to achieve a product that meets the requirements for hot beverage cup applications without relying on plastic linings or coatings. This composition strategy supports the goal of creating a more environmentally friendly and recyclable packaging solution for the food service industry. The paperboard comprises internal sizing agents to enhance water resistance properties. Internal sizing agents are chemical additives that are mixed into the pulp suspension during the papermaking process. These agents provide hydrophobic properties to the cellulose fibers, reducing the rate of liquid absorption and improving the water resistance of the final paperboard product.

[0044] In the present invention, an internal sizing agent is added to each of the first suspension, second suspension, and third suspension used to form the paperboard plies. The concentration of the internal sizing agent in each suspension ranges from 1 to 8 kg per tonne of pulp (kg / t), or from 2 to 7 kg per tonne of pulp calculated as dry internal sizing agent weight content per dry fiber weight content. This concentration range allows for effective internal sizing of the paperboard while maintaining other desirable properties such as printability and convertibility. In one example of the invention, at least the first back-ply suspension comprises an internal sizing agent in a range of 2-8 kg / t, preferably 3-8 kg / tn more preferably 4-7 kg / tn(dry / dry) . The back-ply is intended to form an inside surface (e.g. the food- or beverage-contact surface) of a container made from the paperboard according to the invention.

[0045] Various types of internal sizing agents may be used. Suitable internal sizing agents include alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), rosin, fatty acids, fatty acid derivatives, or combinations thereof. These sizing agents are known in the papermaking industry for their ability to impart water resistance to paper and paperboard products.

[0046] Alkyl ketene dimer (AKD) is a synthetic sizing agent that reacts with cellulose fibers to form covalent bonds, creating a highly effective hydrophobic barrier. AKD is particularly effective in neutral to alkaline papermaking conditions.

[0047] Alkenyl succinic anhydride (ASA) is another synthetic sizing agent that provides excellent water resistance. ASA reacts quickly with cellulose fibers and can be effective in both acidic and alkaline papermaking conditions.

[0048] Rosin-based sizing agents are derived from natural sources and have been used in papermaking for many years. These agents can be modified to improve their performance and compatibility with other papermaking additives.

[0049] Fatty acids and fatty acid derivatives can also be used as internal sizing agents. These compounds interact with the cellulose fibers to create a hydrophobic surface, reducing water absorption.

[0050] One aspect which influences the choice of internal sizing agent is its curing behavior. Different internal sizing agents are cured in different ways depending on the sizing chemical. The term "curing" refers to the process of allowing the sizing agent to adequately react, anchor, spread and / or orient on the fibers within the paper or fiber matrix to develop the desired sizing effect. The on-machine curing or fast-curing typically occurs in the drying section of a paper or board machine. ASA and rosin are examples of sizing agents that mainly provide on-machine curing, whereas AKD sizing typically shows a significant post-curing feature, i.e. the sizing effect continues to develop in storage reels even after production, even for weeks after production. In some examples, at least one of the internal sizing agents provides on-machine curing, meaning that the sizing effect is fully or almost fully developed for at least one sizing agent early in the production process. In some examples, one or both of the pulp suspensions used to form the outer plies, i.e. the back-ply and / or the top-ply, comprise at least one on-machinecuring internal sizing agent such as ASA and / or rosin. In some examples, the suspension used to form the mid-ply comprises at least one slow-curing internal sizing agent such as AKD. In the present invention a surface size composition may optionally be applied on at least the surface of the back-ply of the paperboard, said surface size composition being added in amounts between 0.5 - 5 gsm and comprising at least one polysaccharide and one hydrophobizing agent selected from the group consisting of AKD, ASA, wax, rosin resin, latexes or polymeric dispersions such as styrene maleic anhydride (SMA), styrene acrylate (SA), PE and PHA or combinations thereof. Preferably, in examples where the paperboard is surface sized, the back-ply suspension comprises at least one on-machine curing internal sizing agent such as ASA and / or rosin.

[0051] The use of internal sizing agents, and in some cases also surface sizing agents, contributes significantly to the water resistance properties of the resulting paperboard. By reducing the rate of liquid absorption, the internal sizing helps maintain the structural integrity and rigidity of the paperboard when in contact with hot liquids. This is particularly important for the intended application of hot beverage cups, where the paperboard must resist rapid softening and maintain its shape when filled with hot liquids.

[0052] The combination of internal sizing with other aspects of the method, such as the specific pulp composition and selected press section parameters, results in a paperboard with good water resistance properties. This is evidenced by the low Cobb300 and hot water Cobb300 values achieved in the final paperboard product, which indicate excellent resistance to water absorption under both ambient and elevated temperature conditions.

[0053] In one example of the invention, said three plies are formed on at least two wires using at least two headboxes. This multi-ply formation process allows for precise control over the composition and properties of each ply of the resulting paperboard.

[0054] At least the first back-ply pulp suspension is refined to a Schopper-Riegler value above 30 according to standard ISO 5267-1:1999. The back-ply pulp suspension is intended to form an inside surface of a container made from the paperboard according to the invention. It is also possible that both pulp suspensions used to form the outer plies (back and top) are subjected to a refining process to achieve specific properties. Refining involves mechanically treating the pulp fibers to increase their surface area and improve their bonding potential. The degree ofrefining is measured using the Schopper-Riegler (SR) value according to ISO 5267-1:1999, which indicates the drainage rate of the pulp.

[0055] In the present method, the first back-ply pulp suspension and the third top-ply pulp suspension are refined to a Schopper-Riegler value greater than 28. More specifically, the Schopper-Riegler value for the pulps forming the outer plies may range from 28 to 40 according to ISO 5267-1:1999. This level of refining is selected to achieve a balance between fiber bonding strength and densification effect.

[0056] The higher Schopper-Riegler values for the outer plies contribute to several beneficial properties in the final paperboard. Increased refining leads to greater fiber fibrillation, which enhances inter-fiber bonding and improves the strength and density of the outer layers. This increased bonding potential is particularly advantageous for achieving the desired water resistance and structural integrity in hot beverage cup applications.

[0057] Additionally, the refined outer plies with higher Schopper-Riegler values can contribute to improved surface smoothness and printability of the paperboard. The increased fiber bonding in the outer layers can result in a more closed and uniform surface, which may enhance the appearance and performance of the final product.

[0058] During the ply formation process, a bonding agent may be added between at least one outer ply and the middle bulk ply during the couching step. Couching is the process where the individual wet plies are brought together to form a single, multi-ply web. The addition of a bonding agent at this stage can enhance the inter-ply bonding strength, contributing to the overall structural integrity of the paperboard.

[0059] The bonding agent may be selected from various chemical additives known in the papermaking industry for improving ply bonding. These may include starch-based adhesives, synthetic polymers, microfibri Hated cellulose or other suitable bonding agents compatible with the pulp composition and intended end-use of the paperboard. For example, amounts between 1 - 7 gsm of starch, preferably starch granules or pre-gelled starch particles with or without internal sizing agent may be applied between plies in the paperboard using e.g. curtain application procedure or by spraying.

[0060] By carefully controlling the ply formation process, refining parameters, and bonding agent application, the method produces a multi-ply paperboard structure with enhanced propertiessuitable for food packaging and / or hot beverage cup applications. The combination of refined outer plies and strategic bonding between layers contributes to the overall strength, water resistance, and performance characteristics of the final paperboard product.

[0061] The wet press section in the paperboard production process for dewatering and consolidating the material plays an important role in achieving the desired properties of the final product. The solids content of the wet multi-ply web before entering the press section may range from 15 - 33%, such as between 17 - 25%, and temperature of the web may be above 35°C. Said wet press section involves a press dewatering procedure with a series of conventional press roll nips, such as at least two, possibly three or four consecutive nips pressing the wet web thereby squeezing out water therefrom. The wet press section may also involve at least one shoe press, possibly in combination with one or more of said nip / s. The removed water is typically received and absorbed by a fabric or felt applied on the rolls, i.e. one or more of the nip / s may be felted, such as single- or double felted. For example, at least said two first press nip rolls are double felted for efficient removal of excess water and prevent reabsorbtion. This process removes water from the wet web while compressing and consolidating the fiber network, enhancing fiber-to-fiber bonding and thereby increasing strength and density. According to the invention, the wet web is subjected to a total press impulse greater than 110 kPa*s, such as over 150 kPa*s. This high total press impulse densifies the paperboard structure and improves its strength. In some cases, the total press impulse may exceed 200 kPa*s but remain below 350 kPa*s, depending on the final product's requirements. Another effect of wet pressing according to the invention is that fines and potential MFC content in the web, such as in the mid-ply, migrate with the squeezed-out water towards the material's surface. This increases surface density, which is beneficial for the end product's function by enhancing barrier properties.

[0062] The high total press impulse used in this method also results in a more efficient dewatering and subsequent drying process, potentially allowing for higher production speeds and / or improved energy efficiency.

[0063] Optionally, a smoothing press is arranged downstream of the wet press section, where the web may be subjected to pressing at above 30 kN / m, or above 40 kN / m, such as above 50kN / m to further contribute to surface densification of the board material. Optionally, the smoothing press is one-felted in order to capture water or prevent excess water in the nip. According to the invention, the production line's machine speed should be at least 300 m / min, preferably at least 500 m / min.

[0064] After the wet pressing step, the web achieves a solids content greater than 43%. This high solids content is indicative of effective dewatering and contributes to the overall efficiency of the papermaking process. The increased solids content at this stage of production allows for more efficient drying in subsequent steps, potentially reducing energy consumption in the drying section.

[0065] The wet pressing with the high nip press impulse and resulting high solids content, contribute to the production of a paperboard suitable for food and beverage packaging such as hot beverage cups. These steps help create a dense, strong, and water-resistant structure that can maintain its integrity when in contact with hot liquids.

[0066] After the wet pressing and dewatering steps, the paperboard web is subjected to a drying process to remove the remaining moisture and achieve the desired final moisture content. The drying process is controlled to ensure that the paperboard reaches an end moisture content between 5% and 12%.

[0067] The specific drying conditions may be adjusted based on factors such as the initial moisture content of the web, the thickness of the paperboard, and the desired properties of the final product. The drying process may involve the use of various drying technologies, such as steam-heated cylinders, air dryers, or infrared dryers, to efficiently remove moisture from the paperboard while maintaining its structural integrity.

[0068] Achieving the target moisture content of 5-12% is desirable for several reasons:

[0069] -Dimensional stability: A consistent moisture content within this range helps maintain the dimensional stability of the paperboard, reducing the risk of warping or curling during subsequent processing or use.

[0070] -Strength properties: The final moisture content affects the strength properties of the paperboard. A moisture content within the specified range helps optimize the strength characteristics for hot beverage cup applications.-Convertibility: The specified moisture content range ensures that the paperboard has suitable properties for downstream converting processes, such as cup forming and sealing.

[0071] -Storage stability: Paperboard with a moisture content between 5% and 12% is less susceptible to moisture-related issues during storage and transportation.

[0072] Following the drying process, the paperboard is subjected to a calendering step. Calendering is a finishing process that involves passing the paperboard through one or more nips formed by rotating rolls. The purpose of calendering is to improve the surface properties and uniformity of the paperboard.

[0073] In the present method, the calendering step is performed using at least one nip, such as a soft nip or a hard nip or a combination of both. According to the invention, the calender line load is less than 50 kN / m and the temperature of the board material during treatment is between 75 -250°C. This relatively low calender line load is selected to achieve specific benefits while avoiding potential drawbacks associated with excessive calendering, and elevated temperatures during treatment promotes curing of sizing improving liquid resistance properties.

[0074] The use of a calender line load less than 50 kN / m offers several advantages:

[0075] -Preservation of bulk: A low calendering pressure helps maintain the bulk of the paperboard, which contributes to its stiffness and insulating properties. This is particularly important for hot beverage cup applications, where thermal insulation and cup rigidity are desirable characteristics.

[0076] -Maintenance of porosity: The moderate calendering pressure allows the paperboard to retain a degree of porosity, which can be beneficial for certain converting processes and end-use performance.

[0077] -Surface improvement: Despite the low line load, the calendering step can still enhance the surface smoothness of the paperboard, improving its printability and appearance.

[0078] -Minimal fiber damage: The low calendering pressure reduces the risk of excessive fiber crushing or damage, helping to preserve the strength properties of the paperboard.

[0079] The combination of controlled drying to achieve a specific moisture content range and the use of a low calender line load contributes to the production of a paperboard which may be plastic-free or substantially plastic-free while still having properties suitable for hot beverage cup applications. These processing steps help create a paperboard structure that balances strength, water resistance, and insulation properties while maintaining good convertibility and end-use performance.

[0080] The paperboard produced by the method described herein exhibits specific beneficial properties in terms of e.g. strength, water resistance, and overall structural integrity.

[0081] The density of the paperboard is an important characteristic that influences its performance. The paperboard has a density greater than 720 kg / m3 and less than 1000 kg / m3. This density range provides a balance between strength and weight, which is beneficial for hot beverage cup applications. A higher density generally correlates with improved strength and barrier properties, while still maintaining a reasonable weight for the final product.

[0082] Compression strength is an important property for maintaining the structural integrity of hot beverage cups. The paperboard has a compression strength index greater than 22 Nm / g, such as greater than 24 Nm / g when measured at 50% relative humidity and 23°C. This high compression strength index indicates the paperboard's ability to resist deformation under load, which is particularly important for maintaining cup shape and stability, e.g. when filled with hot liquids.

[0083] Water resistance is a key factor in the performance of paperboard used for hot beverage cups. The Cobb300 value, which measures water absorption, is less than 40 g / m2 for the paperboard. This low Cobb300 value indicates good resistance to water penetration under standard conditions. Additionally, the hot water Cobb300 value is less than 45 g / m2, demonstrating the paperboard's ability to resist water absorption even when exposed to hot liquids. These low Cobb values contribute to the paperboard's ability to maintain its structural integrity and performance in hot beverage cup applications.

[0084] Air permeability is another property that affects the paperboard's barrier characteristics. The paperboard has an air permeability Bendtsen value less than 120 ml / min measured according to standard ISO 5636-3:2013. The paperboard further has an in-plane air permeability, GM, below 0.30 pm2, preferably below 0.25 pm2. This low air permeability indicates a relatively closed or sealed sheet structure, which contributes to improved liquid holdout and potentially better insulation properties in cup applications for hot beverages such as coffee or tea.The performance of the paperboard in actual cup applications can be assessed through grip stiffness measurements. Grip stiffness is measured for both empty cups and cups filled with hot liquid, typically coffee. The loss in grip stiffness due to filling with coffee serves as a performance metric, indicating how well the cup maintains its structural integrity when in use. A lower percentage loss in grip stiffness suggests better performance in maintaining cup rigidity when filled with hot liquids. The paperboard exhibits a loss in grip stiffness below 55% due to filling with hot liquid.

[0085] These properties collectively contribute to the paperboard's suitability for e.g. hot beverage cup applications without the need for plastic lining. The combination of high density, good compression strength, low water absorption, and low air permeability results in a paperboard that can maintain its structural integrity and performance when exposed to hot liquids, while also providing environmental benefits due to its plastic-free composition.

[0086] The method for producing a plastic-free paperboard suitable for hot beverage cups involves the interaction of various elements that work together to achieve the desired properties and performance characteristics. The combination of specific pulp compositions, refining levels, wet pressing conditions, and finishing processes contributes to the creation of a paperboard that can withstand hot liquids without the need for plastic lining.

[0087] The use of kraft pulp in high proportions, particularly in the outer plies, provides strength and fiber bonding capabilities. When combined with the refining process that increases the Schopper-Riegler value to greater than 28 such as greater than 30, the resulting paperboard exhibits improved strength, density, and water resistance. The refined fibers create a more closed sheet structure, which enhances the barrier properties of the paperboard.

[0088] The internal sizing agents added to each pulp suspension work in conjunction with the fiber network to impart hydrophobic properties to the paperboard. These agents reduce water absorption, contributing to the low Cobb300 and hot water Cobb300 values observed in the final product. The interaction between the sized fibers and the densified structure created through wet pressing results in a paperboard with enhanced water resistance properties. The wet pressing process, utilizing a total wet pressing nip impulse greater than 110 kPa*s plays an important role in densifying the paperboard structure. This process enhances fiber-to-fiber bonding and increases the overall strength of the paperboard. The high solids contentachieved after pressing allows for more efficient drying and contributes to the development of a dense, strong paperboard structure.

[0089] The drying process, which brings the paperboard to a final moisture content between 5% and 12%, interacts with the previously established fiber network and sizing to stabilize the paperboard structure. This controlled moisture content contributes to the dimensional stability and strength properties of the final product.

[0090] The calendering step, performed with a calender line load less than 50 kN / m, interacts with the previously developed paperboard structure to enhance surface properties while maintaining bulk and porosity. This process helps achieve a balance between surface smoothness and the preservation of beneficial structural characteristics.

[0091] The plastic-free or substantially plastic-free nature of the paperboard, achieved through the careful selection and interaction of these elements, provides environmental benefits. The paperboard can be more easily recycled or composted compared to traditional plastic-lined alternatives, aligning with sustainability goals in the packaging industry.

[0092] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as “40 wt.%” is intended to mean “about 40 wt.%”.

[0093] EXAMPLES

[0094] Three samples of paperboard were provided, one reference and two test samples:

[0095] Reference Sample 1: a conventional three-ply paperboard suitable for cup stock, where the outer plies were made from hardwood kraft pulp and the mid-ply was made from a pulp composition containing 29 wt% softwood CTMP, 23 - 32 wt% hardwood kraft pulp and 39 -48 wt% broke based on the total fiber content.

[0096] Test Sample 2: A three-ply paperboard produced by means forming three plies using three headboxes, on two wires. The outer plies were made from 100 wt% hardwood kraft pulp withSR value of 30 and the mid-ply was made from a furnish comprising 50 wt% hardwood kraft pulp with SR value of 30, and 50 wt% softwood kraft pulp with SR value of 23. The outer plies comprised internal sizing in the form of rosin at a dosage of 6 kg / ton and the mid-ply comprised internal sizing in the form of AKD at a dosage of 5 kg / ton calculated on the total fiber dry weight in the respective ply. Before wet pressing, the wet multi-ply web had a solids content of about 20%. The wet three-ply web was subjected to press dewatering using a total wet press nip impulse of 201 kPa*s. After wet pressing, the web had a solids content of 46%.

[0097] Test Sample 3: A three-ply paperboard produced by means forming three plies using three headboxes, on two wires. Here, the outer plies were made from hardwood kraft pulp and the mid-ply was made from a furnish comprising 40 wt% softwood CTMP, 60 wt% hardwood kraft pulp and 5 wt% MFC. The SR value of the suspensions used to produce the two outer plies was 30. The outer plies comprised internal sizing in the form of rosin at a dosage of 6 kg / ton and the mid-ply comprised internal sizing in the form of AKD at a dosage of 5 kg / ton calculated on the total fiber dry weight. Before wet pressing, the wet multi-ply web had a solids content of about 20%. The wet three-ply web was subjected to press dewatering using a total wet pressing nip impulse of 210 kPa*s. After wet pressing, the web had a solids content of 46%.

[0098] The three paperboard samples were tested for various properties, and the results are summarized in Table 1 below. The compression strength (SCT) and Bendtsen air permeability were measured according to standards as indicated in Table 1. The Cobb values were measured according to standard ISO 535:2023 (determination of water absorptiveness), and for the hot water Cobb, water temperature during evaluation was 80°C, and a blotting paper was placed underneath the test sample to prevent the condensing water from wetting the sample from the reverse side.

[0099] Measurements of “in-plane permeability” and the “Grip stiffness” were performed in the following ways:

[0100] In-plane permeabilityThe purpose of testing in-plane permeability of the paperboard is to measure air permeance (mean air flow rate through unit area under unit pressure difference in unit time) through a sample, where the air is directed to flow through the paperboard in a planar direction.

[0101] Before measurement, the samples were prepared as follows. The paperboard samples 1-3 were conditioned in the relative humidity RH=50% and the absolute temperature 23°C according to ISO 187:2022. After conditioning, the samples were laminated on both sides with an impermeable polymer. A number of pieces of the size 10 X 10 cm were punched out from each laminated paperboard sample. Each piece was then provided with two parallel cutout slits placed symmetrically of a distance 20 mm from each other. The width and length of each slit were 2 mm and 50 mm respectively. Plastic tape was attached over one side of each slit to cover the respective slits at opposite sides of the paperboard. This was done to prevent air from flowing straight through the paperboard via the same slit. As a result, each slit presented one opening through the top laminate into the inner paperboard material.

[0102] The air permeance through the sample in planar direction, via an inlet opening of the first slit to the outlet opening of the second slit, was then measured in the same environment as the samples were conditioned, i.e. RH=50% and 23°C, using an L&WAir Permeance Tester, low range - Code 168. The results for in-plane air permeability are shown in Table 1 as geometric mean, GM.

[0103] Grip stiffness

[0104] Paperboard according to the three samples referred to above were converted into paper cups comprising the following dimensions: a top outer diameter of 80 mm; a height of 90 mm; and a bottom outer diameter of 56 mm.

[0105] The grip stiffness of the cups was evaluated using Grip Stiffness Tester RH-BT-10 used for measuring the resistance compression of cylindrical objects such as cups under controlled conditions. The tester fulfills the requirements of standards QB / T 2294, GB / T2759, and JJG15. Grip stiffness for each type of paper cup, i.e. for cups made from each of the three types of paperboard, was evaluated for empty cups as well as for cups filled with 215 mL coffee having a temperature of 78°C. The filled cups were tested immediately after filling with said hot coffee. For each test round, ten parallel determinations were made.Reference

[0106] Sample ID Standard Test Sample 2 Test Sample 3

[0107] Sample 1

[0108] Basis weight, g / m2ISO 536:2019 234 289 266 Thickness, pm ISO 534:2019 333 360 366 Density, kg / m3ISO 534:2011 704 803 726

[0109] SCT index, GM, Nm / g ISO 9895:2008 23.4 24.9 26.1 Cobb300, g / m2ISO 535:2023 34 35 38

[0110] Hot water Cobb300, (80°C);

[0111] ISO 535:2023 38 42 45

[0112] g / m2

[0113] Air permeability

[0114] ISO 5636-3:2013 489 90 93 (Bendtsen), ml / min

[0115] In-plane air permeability,

[0116] - 0.33 0.21 0.21 GM, pm2

[0117] Grip stiffness, empty cup,

[0118] - 4.48 5.01 4.88

[0119] N

[0120] Grip stiffness, cup filled

[0121] - 1.68 2.88 2.43 with 78 °C coffee, N

[0122] Loss in grip stiffness due

[0123] - 63 43 50

[0124]

[0125] to filling with coffee, %

[0126] Table 1

[0127] The results in Table 1 indicate a clear improvement of grip stiffness, in particular with regards to “Loss in grip stiffness due to filling with coffee" where Test Samples 2 and 3 have a loss of 43% and 50% respectively, compared to a loss of 63% for the Reference Sample 1. This may be explained by the increased densification of Test Samples 2 and 3 respectively, both seen as increased density as well as significantly lowered Bendtsen and in-plane air permeability. Both Test Samples 2 and 3 also exhibit a good water resistance with Cobb300 below 40.

[0128] A number of implementations have been described. Nevertheless, it will be understood that various modifications may be made without departing from the spirit and scope of the disclosure. Accordingly, other implementations are within the scope of the following claims.

Claims

CLAIMS1. A method for producing a multi-ply paperboard suitable for producing hot beverage cups, the method comprising:providing a first back-ply pulp suspension, a second mid-ply pulp suspension, and a third topply pulp suspension, wherein each suspension comprises an internal sizing agent in a range of 1-8 kg / t (dry / dry);forming three plies from said pulp suspensions wherein the fibers in the outer back- and topply suspensions have been refined to a Schopper-Riegler value between 28 - 40 according to ISO 5267-1:1999 and comprise more than 80 wt% kraft pulp based on total fiber content; subjecting the three plies to couching to form a wet multi-ply web;subjecting the wet multi-ply web to a press dewatering procedure including applying a total wet press impulse greater than 110 kPa*s to obtain a web with a solids content greater than 43%; drying the web to form the multi-ply paperboard with an end moisture content of 5-12%; and subjecting the paperboard to a calendering step with a calender line load less than 50 kN / m.

2. The method according to claim 1, wherein the total wet press impulse is greater than 150 kPa*s, such as greater than 200 kPa*s and below 350 kPa*s.

3. The method according to any one of the previous claims, wherein the back- and top-plies comprises 100 wt% kraft pulp based on the total fiber content.

4. The method according to any one of the previous claims, wherein the mid-ply comprises more than 50 wt% kraft pulp, preferably hardwood kraft pulp.

5. The method according to any one of claims 1 - 3, wherein the mid-ply comprises between 40 - 80 wt% kraft pulp, 0 - 50 wt% broke and 0 - 30 wt% CTMP.

6. The method according to any one of the previous claims, wherein the mid-ply comprises 1 - 15 wt%, such as 1.5 - 7.5 wt% or between 1.5 - 5 wt% microfibri Hated cellulose (MFC) based on the total fiber content.

7. The method according to any one of the previous claims, wherein the back- and top-ply suspensions are refined to a Schopper-Riegler value between 30 - 40 according to ISO 5267-1:1999.

8. The method according to any one of the previous claims, wherein the internal sizing agent is selected from the group consisting of alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), rosin, fatty acid, fatty acid derivative, and combinations thereof.

9. The method according to any one of the previous claims, wherein at least the back-ply suspension comprises an internal sizing agent in a range of 2-8 kg / t, preferably 3-8 kg / tn more preferably 4-7 kg / tn (dry / dry).

10. The method according to any one of the previous claims, further comprising applying a surface size composition on at least the surface of the back-ply of the paperboard, said surface size composition being added in amounts between 0.5 - 5 gsm and comprising at least one polysaccharide and one hydrophobizing agent selected from the group consisting of AKD, ASA, wax, rosin resin, latexes or polymeric dispersions such as styrene maleic anhydride (SMA), styrene acrylate (SA), PE and PHA or combinations thereof.

11. The method according to any one of the previous claims, wherein the wet multi-ply web at entering the press dewatering procedure comprises a solids content in the range of 15 - 33%, such as 17 - 25% at entering the press dewatering procedure.

12. The method according to any one of the previous claims, wherein said three plies are formed on at least two wires using at least two headboxes.

13. A plastic-free paperboard suitable for producing hot beverage cups, wherein the paperboard has:a basis weight above 150 g / m2, such as above 200 g / m2 and below 400 g / m2 measured according to standard ISO 536:2019;a density between 720 - 1000 kg / m3 measured according to standard ISO 534:2011;a compression strength index, GM, greater than 22 Nm / g, such as greater than 24 Nm / g measured according to standard ISO 9895:2008 at 50% relative humidity and 23°C;a Cobb300 value less than 40 g / m2 measured according to standard ISO 535:2023;a hot water Cobb300 value less than 45 g / m2 measured according to standard ISO 535:2023; andan air permeability Bendtsen value less than 120 ml / min measured according to standard ISO 5636-3:2013.

14. The paperboard according to claim 13, comprising a density greater than 750 kg / m3, such as greater than 800 kg / m3.

15. The paperboard according to any one of claims 13 - 14, exhibiting an in-plane air permeability, GM, below 0.30 pm2, preferably below 0.25 pm2.

16. The paperboard according to any one of claims 13 - 15, comprising an outer top-ply, an outer back-ply and at least a mid-ply sandwiched between said top- and back-plies, wherein the densities of the outer top- and back-plies are greater than the density of the mid-ply, wherein the outer plies each has a density greater than 700 kg / m3, and the mid-ply has a density greater than 500 kg / m3.

17. The paperboard according to claim 16, wherein the outer top- and back plies comprise more than 80 wt% kraft pulp, and the mid-ply comprises more than 50 wt% kraft pulp based on the total fiber content.

18. The paperboard according to any one of claims 13 - 17, comprising a total reject of less than 10%, such as less than 5% according to PTS RH 021 / 97 test method for Category II products.