Α-alumina particles and method for producing same
The production of non-spherical α-alumina particles with high α-crystallization rates and low sulfur, chlorine, and uranium contents addresses the limitations of conventional methods, enhancing thermal conductivity and reliability in semiconductor encapsulants.
Patent Information
- Application Number
- PCT/JP2026/011406
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-03-23
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional methods for producing alumina particles for semiconductor encapsulants fail to achieve high α-crystallization rates, leading to insufficient thermal conductivity, and are hindered by high manufacturing costs, spherical shape limitations, and inadequate reduction of sulfur, chlorine, and uranium contents, which can cause ion migration and radiation issues.
A method involving firing aluminum hydroxide particles in a high-alumina firing container preheated at high temperature, with controlled contact area and specific firing conditions to produce non-spherical α-alumina particles with low sulfur, chlorine, and uranium contents, ensuring high α-crystallization rates.
The produced α-alumina particles exhibit enhanced thermal conductivity, improved heat dissipation, and increased reliability by minimizing impurities, reducing the risk of ion migration and radiation, while maintaining mechanical strength and fluidity.
Smart Images

Figure JP2026011406_12112026_PF_FP_ABST
Abstract
Description
α-alumina particles and method for producing the same
[0001] The present invention relates to alpha-alumina particles and a method for producing them.
[0002] With the miniaturization, weight reduction, and performance improvement of semiconductors, semiconductor devices are becoming more highly integrated and high-performance. In semiconductor devices, semiconductors are encapsulated using encapsulating materials containing inorganic fillers and resins to protect them from external environmental factors such as moisture and to increase the strength of the device.
[0003] Inorganic fillers contained in semiconductor encapsulants enhance both the strength of the encapsulant and its heat dissipation. Especially as semiconductor devices become more integrated and higher-performing, the amount of heat generated increases, creating a demand for improved heat dissipation in encapsulants. In response to this demand, it has been proposed to use α-alumina particles (α-aluminum oxide particles), which possess excellent thermal conductivity, chemical stability, and mechanical strength, as inorganic fillers in semiconductor encapsulants.
[0004] As a document disclosing such technology, Patent Document 1 discloses a method for producing spherical alumina powder characterized by spraying aluminum hydroxide powder having a predetermined particle size into a flame (Claim 1 of Patent Document 1). Furthermore, it is stated that this spherical alumina powder has excellent packing properties, a low uranium content, and imparts high thermal conductivity to resin compositions such as semiconductor encapsulants (
[0006] of Patent Document 1).
[0005] Patent Document 2 discloses a method for producing spherical particle material, comprising: a first pickling step of immersing a crude raw material particle material mainly composed of alumina in an acid solution to produce a raw material particle material; a melt spheroidizing step of melting and rapidly cooling the raw material particle material to produce a spheroidized crude spherical particle material; and a second pickling step of immersing the crude spherical particle material in an acid solution to produce a spherical particle material (Claim 1 of Patent Document 2). Furthermore, it is stated that semiconductors are sealed with a encapsulant in which a filler material is dispersed in a resin, and that there is a particular need to improve the thermal conductivity of the filler material, and that alumina is used as a filler material with excellent thermal conductivity (
[0002] and
[0003] of Patent Document 2).
[0006] Patent Document 3 discloses non-spherical alumina particles having an average particle diameter of 0.1 to 100 μm, a uranium content of 8 ppb or less, and having multiple faces due to an α-crystal structure (Claim 1 of Patent Document 3). It also states that the challenge is to provide non-spherical alumina particles with high thermal conductivity, low α-ray emission, and high purity that are suitable for encapsulating large-capacity, highly integrated memory semiconductors (
[0010] of Patent Document 3).
[0007] Japanese Patent Publication No. 5417248, Japanese Patent Publication No. 7406444, Japanese Unexamined Patent Publication No. 2024-123900
[0008] As described above, the use of α-alumina particles as an inorganic filler in semiconductor encapsulants has been proposed for some time, but our inventors have found that there is room for improvement in the conventional technology.
[0009] In other words, it is desirable for alumina particles for semiconductor encapsulants to have a high proportion of α-type crystals, i.e., a high α-crystallization rate. This is because the higher the α-crystallization rate of alumina particles, the higher the thermal conductivity. By increasing the thermal conductivity of the filler, it is possible to improve the heat dissipation of the encapsulant. Furthermore, in order to improve heat dissipation, it is desirable for the alumina particles to be non-spherical. This is because using non-spherical particles increases the contact area between particles, reducing interfacial resistance, and thereby achieving high thermal conductivity.
[0010] Furthermore, high purity is desirable for alumina particles used in semiconductor encapsulants. In particular, if α-alumina particles contain large amounts of sulfur (S) or chlorine (Cl) as impurities, a phenomenon called ion migration may occur, where the metal used as the wiring material dissolves and precipitates onto the electrodes and wiring, or the components used may corrode. Therefore, from the perspective of preventing ion migration and corrosion, it is desirable to reduce the sulfur and chlorine content in the alumina particles as much as possible.
[0011] Furthermore, it is important to reduce the uranium (U) content in alumina particles. Uranium is a component derived from the raw materials of alumina particles. It can also be introduced from external sources during the manufacturing process. Uranium is an alpha emitter that emits alpha rays, a type of radiation. If alumina particles used in semiconductor encapsulants contain a large amount of uranium, a large amount of alpha rays will be emitted from the encapsulant, which can cause semiconductor damage. Specifically, the emitted alpha rays may destroy memory data in semiconductor chips, potentially inducing single-bit errors. To improve the reliability of semiconductor devices, it is desirable to minimize the uranium content in alumina particles.
[0012] In contrast, conventional technologies have found it difficult to meet these requirements simultaneously. For example, Patent Documents 1 and 2 describe a method for producing spherical alumina particles by melting raw materials in a flame, which is said to reduce the uranium content of the resulting spherical alumina particles (Patent Documents
[0051] to
[0052] , Patent Documents
[0033] to
[0043] ). However, in this method of melting and sphericalizing raw materials in a flame, the crystallization of the resulting alumina particles is insufficient, making it difficult to increase the α-crystallization rate. Furthermore, this method has the problem of high manufacturing costs and difficulty in producing fine particles with a particle size of 2 μm or less. Moreover, the resulting alumina particles are spherical, which limits their ability to improve thermal conductivity.
[0013] Furthermore, Patent Documents 1 to 3 do not acknowledge the amount of sulfur (S) and chlorine (Cl), which are impurities contained in alumina particles, nor do they propose any specific means to sufficiently reduce their amounts. Patent Document 2 describes providing pickling steps (first pickling step, second pickling step) before and after the melting spheroidizing step for the purpose of reducing impurities (Patent Document 2,
[0015] ). Patent Document 3 also describes performing alkaline cleaning and acid cleaning after calcining of the aluminum compound (Patent Document 3, claims 5,
[0049] and
[0050] ). However, the present inventors have investigated and confirmed that when acid cleaning is performed, sulfur and chlorine components derived from the acid remain in the alumina particles, leading to an increase in the amount of impurities. In addition, acid cleaning and alkaline cleaning also have the problem of increasing manufacturing costs due to wastewater treatment and cleaning.
[0014] Based on these circumstances, the inventors conducted diligent research. As a result, they developed a method for manufacturing alumina particles in which aluminum hydroxide particles having predetermined physical properties are fired at a predetermined temperature using a high-alumina firing container of a predetermined composition that has been preheated (heat-treated) at a high temperature. They found that this method makes it possible to obtain non-spherical α-alumina particles that have the desired particle size, a high α-crystallization rate, low sulfur and chlorine content, and extremely low uranium content. They also confirmed that these α-alumina particles have excellent thermal conductivity. Because of the above-mentioned characteristics, these α-alumina particles are particularly promising as inorganic filler materials for semiconductor encapsulants.
[0015] This invention was completed based on such findings, and aims to provide non-spherical α-alumina particles having a desired particle size, a high α-crystallization rate, low sulfur and chlorine content, and an extremely low uranium content, as well as a method for producing the same.
[0016] The present invention encompasses the following embodiments (1) to (4). In this specification, the expression "~" includes the numerical values at both ends. That is, "X~Y" is synonymous with "X or more and Y or less".
[0017] (1) The circularity is 0.80 or less, the aspect ratio is 1.30 or more, the average particle size is 0.1 μm or more and 1.0 μm or less, and the specific surface area is 12.0 m². 2 Alpha-alumina particles having a concentration of 0.5 / g or less, a sulfur (S) content of 20 ppm or less, a chlorine (Cl) content of 40 ppm or less, a uranium (U) content of 5 ppb or less, and an alpha crystallization rate of 70% or more.
[0018] (2) The α-alumina particles of (1) above, wherein the sodium (Na) content is 50 ppm or less and the amount of dissolved sodium (Na) is 10 ppm or less.
[0019] (3) A method for producing α-alumina particles, comprising a step of firing aluminum hydroxide particles filled in a firing container at a temperature of 1100°C or higher and 1200°C or lower to produce a fired product, wherein the uranium (U) content of the aluminum hydroxide particles is 3 ppb or less, and as the firing container, alumina (Al 2 O 3 ) in a proportion of 85 mass% or more and 93 mass% or less, and a high-alumina container containing silica (SiO 2 ) in a proportion of 7 mass% or more and 14 mass% or less that has been pre-fired at a temperature of 1100°C or higher is used, and when firing the aluminum hydroxide particles, the firing is performed in a state where the contact area between the aluminum hydroxide particle compact and the firing container is 30% or less of the surface area of the compact.
[0020] (4) The method according to (3) above, wherein when filling the aluminum hydroxide particles into the firing container, a sheet material that disappears during firing is interposed between the aluminum hydroxide particle compact and the firing container.
[0021] According to the present invention, non-spherical α-alumina particles having a desired particle size, a high α crystallization rate, low sulfur and chlorine contents, and an extremely low uranium content, and a method for producing the same are provided.
[0022] It is a cross-sectional explanatory view showing a state of firing aluminum hydroxide using a firing container. It is a perspective explanatory view of an aluminum hydroxide compact obtained by press-molding aluminum hydroxide. It is an assembly explanatory view of a sheet material used when firing aluminum hydroxide.
[0023] Specific embodiments of the present invention (hereinafter referred to as "the present embodiments") will be described below. However, the present invention is not limited to the following embodiments, and various modifications are possible within the scope that does not alter the gist of the present invention. In addition, in the present specification, any combination of preferred aspects can be adopted as long as technical consistency can be achieved. For example, one and the other of the preferred numerical ranges can be arbitrarily combined.
[0024] <<1. α-alumina particles>> The α-alumina particles of the present embodiment (hereinafter sometimes referred to as "alumina particles") have a circularity of 0.80 or less, an aspect ratio of 1.30 or more, an average particle diameter of 0.1 μm to 1.0 μm, and a specific surface area of 12.0 m 2 / g or less, a sulfur (S) content of 20 ppm or less, a chlorine (Cl) content of 40 ppm or less, a uranium (U) content of 5 ppb or less, and an α crystallization rate of 70% or more. Such α-alumina particles have excellent thermal conductivity. In addition, despite the high α crystallization rate, the contents of sulfur and chlorine are low, and the uranium content is extremely low. Therefore, when these α-alumina particles are used as a filler for a semiconductor encapsulating material, a semiconductor device excellent in various characteristics such as reliability can be obtained.
[0025] The α-alumina particles of the present embodiment mainly contain alumina (aluminum oxide) having an α-type crystal. Specifically, the α crystallization rate is 70% or more. Here, the α crystallization rate is the proportion of α-type crystals occupying the crystal forms contained in the alumina particles. Alumina has various crystal forms such as α, β, γ, δ, and θ. Among these, the α-type crystal has the highest thermal conductivity. From the viewpoint of enhancing the heat dissipation property of the encapsulating material by utilizing the high thermal conductivity of the α-alumina particles, a higher α crystallization rate is desirable. The α crystallization rate is preferably 75% or more, more preferably 80% or more, and even more preferably 85% or more. The α crystallization rate is 100% or less. In the present specification, the α-alumina particles mean an aggregate of a plurality of independent particles. The α-alumina particles can be read as α-alumina powder.
[0026] The α-alumina particles of the present embodiment have a non-spherical shape. Specifically, the α-alumina particles have a circularity of 0.80 or less and an aspect ratio of 1.30 or more. Non-spherical α-alumina particles are more excellent in thermal conductivity than spherical particles. By making the shape of the α-alumina particles non-spherical, it is possible to further enhance the heat dissipation property of an encapsulating material produced using these α-alumina particles. From the viewpoint of enhancing thermal conductivity, the circularity is more preferably 0.50 or more and 0.80 or less. The aspect ratio is more preferably 1.30 or more and 1.80 or less.
[0027] Circularity is an index indicating the degree of sphericity of α-alumina particles. A perfect sphere has a circularity of 1, and the smaller the degree of sphericity, the lower the circularity. Circularity is determined by observing α-alumina particles with a scanning electron microscope (SEM) and performing image analysis on the resulting SEM image. Specifically, one particle in the SEM image is examined, and its projected area and perimeter are determined. Then, the circularity of this particle is calculated from the area and perimeter according to equation (1) below. The circularity is determined for multiple particles, and the average value is calculated to determine the circularity of the α-alumina particle.
[0028]
[0029] Although particles have a three-dimensional shape, in this embodiment, since the particle shape is determined based on a two-dimensional particle projection image obtained by SEM observation, "circularity" is used as an index of particle sphericity.
[0030] The aspect ratio can also be determined by image analysis of the SEM image of the α-alumina particle. Specifically, one particle in the SEM image is examined, and the minimum circumscribing rectangle of the projection image of this particle is determined. Here, the minimum circumscribing rectangle is the rectangle with the smallest area among the rectangles (quadrilaterals) that circumscribe the particle in the projection image. Next, the length of the long side and the short side of the minimum circumscribing rectangle are determined, and the aspect ratio of this particle is calculated according to equation (2) below. The aspect ratio is determined for multiple particles, and the average value is calculated to determine the aspect ratio of the α-alumina particle.
[0031]
[0032] The α-alumina particles of this embodiment have a predetermined particle size. Specifically, the average particle size is 0.1 μm or more and 1.0 μm or less, and the specific surface area is 12.0 m². 2 The particle size is less than / g. Using α-alumina particles with such particle size, it becomes possible to obtain semiconductor encapsulants with not only high heat dissipation and mechanical strength, but also excellent fluidity. Average particle size is less than 0.1 μm or specific surface area is 12.0 m². 2Excessively fine alumina particles exceeding 1 / g increase the contact surface between the filler surface and the encapsulating resin material, leading to increased interaction and reduced fluidity of the encapsulating material containing them as filler. Furthermore, their low crystallinity can result in inferior properties such as thermal conductivity and mechanical strength. Additionally, excessively coarse alumina particles with an average particle size exceeding 1.0 μm can make it difficult to fill narrow gaps. From the viewpoint of more reliably avoiding the above problems, an average particle size of 0.2 μm to 1.0 μm is preferable. The specific surface area should be 10 m². 2 It is preferable to have a value of 0.1 / g or less. The average particle size is the cumulative 50% diameter obtained by accumulating from the smallest particle size in the particle size distribution determined by volume. The average particle size and specific surface area may be determined by the method described in the examples below or a similar method.
[0033] The α-alumina particles of this embodiment have suppressed sulfur and chlorine content. Specifically, the sulfur (S) content is 20 ppm or less, and the chlorine (Cl) content is 40 ppm or less. By suppressing the content of sulfur and chlorine, it is possible to improve the reliability of semiconductor devices when these α-alumina particles are applied as a encapsulating filler. In other words, in semiconductor devices, fine wiring such as wires is used to electrically connect the semiconductor chip to external terminals. If the filler (α-alumina particles) contained in the encapsulating material contains a large amount of sulfur and chlorine, there is a risk that the metal used as the wiring material will dissolve and precipitate on the electrodes and wiring (ion migration phenomenon). In addition, there is a risk that the fine wiring will be corroded. Furthermore, the sulfur and chlorine components contained in the α-alumina particles may degrade the resin components in the encapsulating material, which may reduce the reliability of the semiconductor device.
[0034] To avoid such problems, it is desirable to keep the sulfur and chlorine content in α-alumina particles as low as possible. A sulfur content of 10 ppm or less is more preferable. A chlorine content of 30 ppm or less is more preferable. Note that the sulfur and chlorine components contained in α-alumina particles are not limited to elemental sulfur and chlorine. Even if ions or compounds are formed within the particles, their content is calculated. However, if sulfur or chlorine forms compounds, their respective contents are determined by converting them to the amounts of elemental sulfur and chlorine. The sulfur and chlorine content can be determined by the method described in the examples below or a similar method.
[0035] The α-alumina particles of this embodiment have a uranium (U) content of 5 ppb or less. Uranium is an α-emitter that emits α-rays, which are a type of radiation. If the uranium content of the α-alumina particles is high, the amount of α-rays emitted will increase. Therefore, when α-alumina particles are applied as a filler in semiconductor encapsulating materials, there is a risk that the emitted α-rays may corrupt the memory data of the semiconductor chip and induce single-bit errors. By reducing the uranium content, it is possible to improve the reliability of semiconductor devices. From the viewpoint of improving reliability, a lower uranium content is desirable. The uranium content is preferably 5 ppb or less. The uranium content may be determined by the method described in the embodiment below or a similar method.
[0036] The α-alumina particles of this embodiment preferably have a sodium (Na) content of 50 ppm or less and an amount of dissolved sodium (Na) of 10 ppm or less. The sodium component is mainly derived from the raw materials of the α-alumina particles. Because the sodium component is hygroscopic, it may reduce the moisture resistance reliability of semiconductor devices. In addition, the sodium component may promote ion migration of wiring materials and may be a factor that hinders electrical insulation. Furthermore, it may cause curing defects in the resin curing process. From the viewpoint of improving moisture resistance reliability and electrical insulation, it is desirable to have a low amount of sodium component. The sodium content is preferably 50 ppm or less. The amount of dissolved sodium is also preferably 10 ppm or less. Note that dissolved sodium refers to the sodium component that dissolves into the water when α-alumina particles are placed in water. The sodium content and the amount of dissolved sodium may be determined by the method of the example described later or a similar method.
[0037] The α-alumina particles of this embodiment may contain minor components other than aluminum (Al), oxygen (O), sulfur (S), chlorine (Cl), and sodium (Na) in amounts exceeding the amount of impurities. Examples of such minor components include silicon (Si), iron (Fe), and calcium (Ca). However, from the viewpoint of utilizing the excellent effects based on alumina, it is desirable to have a low content of minor components other than Al, O, S, Cl, and Na. The content of minor components is preferably 5% by mass or less, preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.1% by mass or less. For example, the molybdenum (Mo) content is preferably 5% by mass or less, 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less.
[0038] The α-alumina particles of this embodiment may have a surface treatment component on their surface. The surface treatment component is a surface treatment agent or a component derived therefrom, and is formed by treating the α-alumina particles with a surface treatment agent. Examples of surface treatment agents include silane coupling agents and titanate coupling agents. However, the surface treatment component is not an essential component.
[0039] The α-alumina particles of the present embodiment have low sulfur and chlorine contents and an extremely low uranium content despite a high α crystallization rate. In addition, these α-alumina particles are non-spherical. Therefore, they are excellent in mechanical and chemical stability as well as in thermal conductivity, and by taking advantage of these characteristics, they are particularly promising as a material for the inorganic filler of semiconductor encapsulants.
[0040] However, the α-alumina particles of the present embodiment are not limited to those used for semiconductor encapsulant applications. It goes without saying that they can be applied to known uses of α-alumina particles such as refractory materials, abrasives, insulators, electronic components, structural members, semiconductor manufacturing apparatuses such as electrostatic chucks, spark plugs, fillers, and catalyst carriers.
[0041] <<2. Method for Producing α-Alumina Particles>> The method for producing α-alumina particles of the present embodiment includes a step of filling aluminum hydroxide particles in a firing container and firing them at a temperature of 1100°C or higher and 1200°C or lower to produce a fired product. The uranium (U) content of the aluminum hydroxide particles is 3 ppb or less. In addition, as the firing container filled with the aluminum hydroxide particles, alumina (Al 2 O 3 ) in a proportion of 85 mass% or more and 93 mass% or less, and a high-alumina container containing silica (SiO 2 ) in a proportion of 7 mass% or more and 14 mass% or less that has been pre-fired in air at a temperature of 1100°C or higher is used. Furthermore, when firing the aluminum hydroxide particles, the firing is performed in a state where the contact area between the aluminum hydroxide particle filler and the firing container is 30% or less of the surface area of the filler. According to such a production method, α-alumina particles having a desired particle size, low sulfur and chlorine contents, and an extremely low uranium content despite a high α crystallization rate can be obtained.
[0042] <Preparation Step> In producing the α-alumina particles of the present embodiment, aluminum hydroxide particles are prepared as a raw material. The aluminum hydroxide particles are composed of aluminum hydroxide (Al(OH) 3The particles mainly consist of ) . The aluminum hydroxide may be either γ-type gibbsite or α-type Bayerlite. The aluminum hydroxide particles are preferably those produced by the Bayer process. In this specification, aluminum hydroxide particles can be read as aluminum hydroxide powder.
[0043] In the manufacturing method of this embodiment, aluminum hydroxide particles with a uranium (U) content of 3 ppb or less are used as raw materials. This is α-alumina (Al) obtained by calcination. 2 O 3 In order to limit the amount to 5 ppb or less, considering the weight reduction due to the dehydration reaction during calcination, aluminum hydroxide (Al(OH) 3 This is because the uranium (U) content contained in the material must be approximately 3.3 ppb or less. By using high-purity aluminum hydroxide particles in this way, it becomes possible to obtain the α-alumina particles targeted in this embodiment, in conjunction with the effects of the subsequent calcination process. Furthermore, from the viewpoint of suppressing the sodium (Na) content and Na elution amount of the α-alumina particles, the Na content of the raw material aluminum hydroxide particles is preferably 500 ppm or less.
[0044] <Casturing Process> Next, the prepared aluminum hydroxide particles are filled into a calcination container and calcined. During calcination, a dehydration reaction and crystallization transition occur, and the aluminum hydroxide changes to α-alumina. That is, at low temperatures, aluminum hydroxide (Al(OH) 3 The hydroxyl group (OH) is removed from the alumina, and α-alumina is formed via intermediate aluminas such as χ-alumina and κ-alumina. Therefore, by going through the calcination process, a calcined product mainly composed of α-alumina is obtained.
[0045] To reduce impurities, alumina (Al) is used as the firing container filled with aluminum hydroxide particles. 2 O 3 ) contains 85% to 93% by mass of silica (SiO 2 It is important to use a high-alumina container that contains 7% to 14% by mass of ) and has been pre-heated at a temperature of 1100°C or higher.
[0046] A commonly used firing container, SiO 2 In so-called silicate-based calcination containers that contain a relatively large amount of SiO, a large amount of Si remains in the alumina after calcination, and the volatilization and adsorption of Ca and Fe reduces the purity of the resulting alumina. On the other hand, SiO 2 In high-alumina calcination containers with relatively low levels of Al, Si contamination can be suppressed, but the effect of reducing Na is small, and there is a problem of significant Ca contamination. The inventors of this invention investigated and found that Al 2 O 3 It contains 85% by mass or more and 93% by mass or less, and SiO 2 We found that by firing aluminum hydroxide particles at a predetermined temperature using a high-alumina container containing 7% to 14% by mass of [a certain substance], a sufficient Na reduction effect can be obtained, and high-purity α-alumina particles can be obtained while suppressing contamination by impurity metals such as Si, Ca, and Fe.
[0047] Incidentally, uranium (U) has been confirmed to exist in minerals and is contained in mineral-derived calcination containers (saggers, saggars). Therefore, the inventors have found that when aluminum hydroxide packing is calcined using such uranium-containing calcination containers, the uranium in the calcination container diffuses into the packing, resulting in a higher uranium content in the final α-alumina particles.
[0048] Therefore, in the manufacturing method of this embodiment, a firing container that has been preheated (heat-treated) at a high temperature (1100°C or higher) is used. Furthermore, firing is performed in a state where the contact area between the aluminum hydroxide packing and the firing container is reduced (to 30% or less of the surface area of the packing). By using these methods in combination, it becomes possible to produce α-alumina particles with a reduced uranium content. That is, by preheating the firing container at a high temperature, the uranium contained in the firing container volatilizes, reducing its content. In addition, by reducing the contact area between the aluminum hydroxide packing and the firing container, the diffusion of uranium from the firing container into the packing is further suppressed. Moreover, by adopting this method, it becomes possible to sufficiently suppress the content of sulfur and chlorine components contained in the α-alumina particles.
[0049] There are no particular restrictions on the means of reducing the contact area of the aluminum hydroxide filler with the firing container. For example, aluminum hydroxide (aluminum hydroxide filler) that has been pre-press-formed according to the shape of the firing container may be placed in the firing container via a spacer made of a high-purity alumina sintered piece or the like, so as to form a predetermined gap between it and the inner wall surface of the firing container. Alternatively, aluminum hydroxide (aluminum hydroxide filler) that has been press-formed to have legs that can support its own weight and are in contact with the bottom inner wall surface of the firing container may be placed in the firing container so as to be in contact with the firing container only by the legs.
[0050] Figure 1 is a cross-sectional diagram illustrating the process of firing aluminum hydroxide using firing container 1. The firing container 1 is made of Al 2 O 3 85-93% by weight of, and SiO 2 The firing container 1 consists of a main body 2 and a lid 3 containing 7 to 14% by weight of aluminum hydroxide, and the firing container 1 is filled with pre-press-molded aluminum hydroxide filler 4. As shown in Figure 2, the aluminum hydroxide filler 4 is press-molded into a clog shape with legs 4a, and is positioned at a predetermined distance d from the inner wall surface of the firing container 1 so that only the legs 4a are in contact with the firing container 1.
[0051] When firing aluminum hydroxide using the firing container 1, for example, the sheet material 5 shown in Figure 3 can be used. This sheet material 5 is made of polyethylene, polypropylene, polystyrene, etc., and burns away after firing. This sheet material 5 is used as a liner when filling the firing container 1 with aluminum hydroxide, and it is preferable to prepare four sheets (in Figure 3) that correspond to the inner wall side portion 2a of the firing container body 2 and one sheet (in Figure 3) that corresponds to the inner wall bottom portion 2b, according to the shape of the firing container 1. Of these, it is preferable to provide several openings 5a in the sheet material 5 that corresponds to the inner wall bottom portion 2b of the firing container body 2, so that the filled aluminum hydroxide can form legs that can support its own weight after firing.
[0052] The method of using the sheet material 5 is as follows: First, the sheet material 5 is placed on the inner wall surface of the firing container body 2. At this time, the sheet material 5 with an opening 5a is placed on the bottom surface 2b of the inner wall. Then, the firing container body 2, on which all the sheet materials 5 are placed, is filled with aluminum hydroxide, which is the raw material. At this time, it is preferable to shape the aluminum hydroxide filling while applying pressure. After filling with all the aluminum hydroxide, the firing container body 2 is covered with the lid 3. When aluminum hydroxide is fired and becomes α-alumina, it can maintain a certain shape through sintering. Therefore, if an opening is provided in the sheet material placed on the bottom surface of the inner wall of the firing container, even after the sheet material has burned away, the aluminum hydroxide filled in this opening will act as legs to support its own weight, preventing the parts other than the legs from coming into contact with the firing container.
[0053] A predetermined gap should be provided between the lid of the firing container and the aluminum hydroxide packing. Furthermore, any parts that come into contact with the firing container and may be contaminated with impurities may be removed after firing. Specifically, it is advisable to remove a 5 mm (5 mm deep) portion from the surface of the α-alumina obtained after firing.
[0054] Next, the aluminum hydroxide particles packed into the firing container are fired at a temperature of 1100°C to 1200°C. If the firing temperature is below 1100°C, the removal of sodium components is likely to be insufficient, and there is a risk that the amount of sodium in the resulting α-alumina particles will be high. Also, the crystallization of the α-alumina particles may not progress, and the α-crystallization rate may decrease. On the other hand, if the firing temperature is above 1200°C, the volatilization of residual uranium in the firing container and the resulting contamination may progress, and there is a risk that the amount of uranium in the α-alumina particles will increase. From the viewpoint of achieving both a high α-crystallization rate and a low impurity concentration, a firing temperature of 1100°C to 1200°C is preferable. Furthermore, the firing holding time is preferably 3 hours to 15 hours. In addition, it is preferable to carry out the firing in an atmosphere of air, nitrogen, and / or vacuum.
[0055] <Washing Process> If necessary, the calcined product obtained in the calcination process may be subjected to a washing treatment. This makes it possible to further remove soluble impurities such as sodium components. Specific washing methods include slurring the calcined product with pure water, stirring and washing to dissolve and remove soluble components, and then passing washing water through it. Alternatively, the calcined product may be crushed into a slurry, and the resulting slurry may be brought into contact with an ion exchange resin to remove impurity metals. However, acid washing or alkaline washing may increase the content of sulfur and chlorine components in the final α-alumina particles. Therefore, it is preferable not to perform acid washing or alkaline washing. It is also preferable to dry the calcined product after the washing treatment. The washed calcined product may be subjected to heat treatment and then washed again.
[0056] In this way, α-alumina particles of this embodiment can be obtained. The manufacturing method of this embodiment is characterized by using a high-alumina firing container of a predetermined composition that has been pre-heat-treated at a high temperature to fire aluminum hydroxide particles having predetermined physical properties at a predetermined temperature. With this manufacturing method, it is possible to obtain high-purity non-spherical α-alumina particles in which not only uranium (U) but also sulfur (S) and chlorine (Cl) content is suppressed. In contrast, with conventional manufacturing methods mainly involving acid washing, sulfur (S) and chlorine (Cl) components derived from the acid remain, making it difficult to obtain particles in which these amounts are sufficiently reduced.
[0057] The present invention will be described in more detail using the following examples. However, the present invention is not limited to the following examples.
[0058] (1) Production of α-alumina particles [Example 1] In Example 1, aluminum hydroxide particles were fired using a high-alumina calcined saggar that had been pre-fired at a high temperature of 1100°C or higher as a firing container, and the resulting calcined product was washed to produce α-alumina particles. The specific production procedure was as follows.
[0059] <Preparation Process> Aluminum hydroxide particles (manufactured by Nippon Light Metal Co., Ltd.) were prepared as the raw material. These aluminum hydroxide particles had an average particle size of 40 μm, and the measured uranium (U) content was 0 ppb.
[0060] Also, as a firing container, alumina (Al 2 O 3 ) contains 88% by mass of silica (SiO 2 A high-alumina saggar (internal dimensions: 280 mm x 230 mm x 95 mm) containing 12% by mass of ) was prepared, and this firing container (high-alumina saggar) was heat-treated (empty firing) in air at 1200°C for 2 hours.
[0061] <Firing Process> Next, the raw material (aluminum hydroxide particles) was fired to obtain a fired product. Specifically, 2 kg of aluminum hydroxide particles were filled into a pre-fired high-alumina saggar, and the saggar was covered with a lid made of the same material. At this time, a sheet material (5 mm thick) made of foamed polyethylene that disappears during firing was placed between the aluminum hydroxide particle filling and the inner wall of the saggar to prevent direct contact between the filling and the saggar. Then, the aluminum hydroxide particles were fired in this state. The firing was carried out under conditions of 1150°C for 15 hours in air.
[0062] <Washing Process> Next, the obtained calcined material was removed from the saggar and washed with water to produce a washed material, which was then crushed to obtain α-alumina particles. Specifically, 2 L of pure water (repulping water) was used to form a slurry for 1 kg of calcined material, and the mixture was stirred and washed for 1 hour. After stirring and washing, the slurry was injected into a filter to aspirate and filter out the repulping water, removing the dissolved impurity metals. Furthermore, pure water (washing water) was passed through the filtered calcined material, performing a water-flow wash at a rate of 5 L of washing water per 1 kg of calcined material. After this washing process, the material was dried to obtain a washed material from which impurity metals had been removed. Next, the obtained washed material was subjected to a dry grinding process using a rolling ball mill to obtain a pulverized material (α-alumina particles).
[0063] [Example 2] In Example 2, aluminum hydroxide particles (manufactured by Nippon Light Metal Co., Ltd.) were used as the raw material. These aluminum hydroxide particles had an average particle size of 50 μm and a measured uranium (U) content of 0 ppb. In the calcination process, 0.18 kg of 8.5% hydrochloric acid (HCl) and 0.33 kg of pure water were added to the raw material aluminum hydroxide powder and mixed, and then α-alumina particles were produced using the same procedure as in Example 1. However, the calcination was carried out under conditions of 1150°C for 10 hours in air. In the washing process, 2 L of pure water (repulping water) was added to 1 kg of calcined material to form a slurry, and the material was stirred and washed for 1 hour. After stirring and washing, the slurry was injected into a filter to aspirate and filter out the repulping water, and the dissolved impurity metals were removed. Furthermore, pure water (washing water) was passed through the filtered calcined material in a water flow washing procedure, with 2 L of washing water passed through 1 kg of calcined material. After this washing process, the material was dried to obtain a cleaned product from which impurity metals had been removed. Next, the obtained cleaned product was subjected to a dry grinding process using a vibrating ball mill to obtain a pulverized product (α-alumina particles).
[0064] [Comparative Example 1] In Comparative Example 1, the calcination temperature of the raw material (aluminum hydroxide particles) was changed from 1150°C to 1230°C. Otherwise, α-alumina particles were prepared using the same procedure as in Example 2.
[0065] [Comparative Example 2] In Comparative Example 2, the firing container (high-alumina saggar) was not heat-treated (empty firing), and the raw material (aluminum hydroxide particles) was fired using an unheated high-alumina saggar. Otherwise, α-alumina particles were produced using the same procedure as in Example 2.
[0066] [Comparative Example 3] Commercially available high-purity spherical alumina was obtained and evaluated. This alumina was manufactured by burning and liquefying metal powder, followed by cooling and solidifying it.
[0067] [Comparative Example 4] Commercially available high-purity alumina was obtained and evaluated. This alumina was produced by hydrolysis of aluminum alkoxide.
[0068] [Comparative Example 5] In Comparative Example 5, the pulverized material (α-alumina particles) obtained in Example 1 was further subjected to acid washing and alkaline washing. Specifically, 100 g of the pulverized material that had undergone dry pulverization was dispersed in 1 L of pure water to obtain a suspension. While stirring the obtained suspension, 10% hydrochloric acid (HCl) was added using a volumetric pipette until the pH of the suspension became 1, and the mixture was stirred for another hour. Next, 25% sodium hydroxide (NaOH) solution was added using a volumetric pipette until the pH of the suspension became 7. After that, coarse particles in the suspension were removed using a sieve with a mesh size of 45 μm. While stirring the suspension after the removal of coarse particles, 25% NaOH solution was added using a volumetric pipette until the pH of the suspension became 11, and the mixture was stirred for another hour. While stirring the suspension, 10% HCl was added using a volumetric pipette until the pH of the suspension became 7. Next, a series of operations of solid-liquid separation using a Buchner funnel and water washing were repeated until the conductivity of the filtrate was 10 μS / cm or less. Furthermore, a final solid-liquid separation was performed, and the resulting processed material was dried to obtain α-alumina particles.
[0069] [Comparative Example 6] In Comparative Example 6, the pulverized material (α-alumina particles) obtained in Example 1 was further subjected to acid washing and alkaline washing. Specifically, 100 g of the pulverized material that had undergone dry pulverization was dispersed in 1 L of pure water to obtain a suspension. While stirring the obtained suspension, 20% potassium hydroxide (KOH) solution was added using a volumetric pipette until the pH of the suspension reached 11, and the suspension was stirred for another 30 minutes. Next, 800 mL of the supernatant was removed and replaced with 800 mL of pure water. Then, using a volumetric pipette, 20% sulfuric acid (H) solution was added until the pH of the suspension reached 7. 2 SO 4 ) was added. Furthermore, coarse particles were removed from the suspension using a sieve with a mesh size of 45 μm. Then, using a volumetric pipette, the suspension was heated to 20% H until its pH became 1. 2 SO 4The mixture was added and stirred for another hour. Then, using a volumetric pipette, 20% KOH solution was added until the pH of the suspension reached 8. Next, a series of operations involving solid-liquid separation using a Buchner funnel and washing with water were repeated until the conductivity of the filtrate was 10 μS / cm or less. A final solid-liquid separation was then performed, and the resulting product was dried to obtain α-alumina particles.
[0070] [Comparative Example 7] In Comparative Example 7, the pulverized material (α-alumina particles) obtained in Example 1 was further subjected to acid washing and alkaline washing. Specifically, 100 g of the dry-pulverized material was dispersed in 1 L of pure water to obtain a suspension. While stirring the obtained suspension, 20% sulfuric acid (H) was added using a volumetric pipette until the pH of the suspension reached 2. 2 SO 4 ) was added and stirred for another 30 minutes. Next, 800 mL of the supernatant was removed and replaced with 800 mL of pure water. Then, using a volumetric pipette, 25% sodium hydroxide (NaOH) solution was added until the pH of the suspension reached 7. Then, coarse particles in the suspension were removed using a sieve with a mesh size of 100 μm. Then, using a volumetric pipette, 25% NaOH solution was added until the pH of the suspension reached 11 and stirred for another hour. Then, using a volumetric pipette, 20% H was added until the pH of the suspension reached 7.5. 2 SO 4 The following was added. Next, a series of operations consisting of solid-liquid separation using a Buchner funnel and washing with water was repeated until the conductivity of the filtrate was 10 μS / cm or less. Finally, a final solid-liquid separation was performed, and the resulting processed material was dried to obtain α-alumina particles.
[0071] [Comparative Example 8] In Comparative Example 8, the pulverized material (α-alumina particles) obtained in Example 1 was further subjected to acid washing and alkaline washing. Specifically, 100 g of the dry-pulverized material was dispersed in 1 L of pure water to obtain a suspension. While stirring the obtained suspension, 20% potassium hydroxide (KOH) solution was added using a volumetric pipette until the pH of the suspension reached 11, and the suspension was stirred for another hour. Next, 800 mL of the supernatant was removed, and 800 mL of pure water was added to the suspension in its place. After that, 20% sulfuric acid (H) was added using a volumetric pipette until the pH of the suspension reached 7.2 SO 4 ) was added. Then, coarse particles were removed from the suspension using a sieve with a mesh size of 200 μm. After that, the suspension was heated using a volumetric pipette until the pH of the suspension became 1 with 20% H. 2 SO 4 The mixture was then stirred for another hour. Subsequently, a 25% sodium hydroxide (NaOH) solution was added using a volumetric pipette until the pH of the suspension reached 8. Next, a series of operations involving solid-liquid separation using a Buchner funnel and washing with water were repeated until the conductivity of the filtrate was 10 μS / cm or less. A final solid-liquid separation was then performed, and the resulting product was dried to obtain α-alumina particles.
[0072] (2) Evaluation For each example and comparative example, the various properties of aluminum hydroxide particles (raw material) and α-alumina particles (final product) were evaluated using the following procedure.
[0073] <SEM Observation> The shape of α-alumina particles (final product) was evaluated using a scanning electron microscope (JEOL Ltd., JSM-F100; SEM) and the fully automated AI image analysis service GeXeL (KNiT Corporation, AI number 36). Specifically, α-alumina particles were observed using SEM to obtain SEM images, and based on the obtained SEM images, the circularity and aspect ratio of the α-alumina particles were calculated according to equations (1) and (2) above. In this case, the SEM observation was performed under conditions of magnification of 10,000x. Analysis was also performed on approximately 500 particles.
[0074] <Average Particle Size> The average particle size of aluminum hydroxide particles (raw material) was measured using a laser diffraction type Microtrac particle size distribution analyzer (Nikkiso Co., Ltd., Microtrac 9320HRA (X100)), and the average particle size of α-alumina particles (final product) was measured using a laser diffraction type Microtrac particle size distribution analyzer (Nikkiso Co., Ltd., MT3300 EXII).
[0075] <Specific Surface Area> The specific surface area (BET) of aluminum hydroxide particles (raw material) and α-alumina particles (final product) was measured using an automated specific surface area analyzer (Micromeritics, Flowsorb II 2300).
[0076] <Impurity Amount (Na and Eluted Na)> The amount of impurity (Na) in α-alumina particles was measured using an atomic absorption spectrometer (Hitachi High-Technologies Corporation, Polarized Zeeman Atomic Absorption Spectrophotometer Z-2000). First, α-alumina particles were placed in a pressurized decomposition vessel and dissolved in sulfuric acid, and a sample solution was prepared by diluting it with water to a certain volume. The sample solution was set in the instrument, and the absorbance at a wavelength of 589.0 nm was measured using an air-acetylene flame. Subsequently, the amount of Na was calculated using the absorbance of a standard solution obtained simultaneously.
[0077] Furthermore, the eluted sodium (Na) content of the α-alumina particles (final product) was determined by atomic absorption spectroscopy. Specifically, water was added to the sample (α-alumina particles) so that the mass ratio of the sample to water was 1:60, and the sample was heated in a water bath using boiling water for 30 minutes to elute the eluted Na from the sample into the water. Then, the amount of eluted Na was determined using an atomic absorption spectrophotometer (Hitachi High-Technologies Corporation, Z-2000). The measurement was performed under the conditions of measurement mode: atomic absorption, measurement wavelength range: 589.0 nm.
[0078] <Impurity Amount (S)> The sulfur (S) content of α-alumina particles (final product) was determined by ICP emission spectrometry. Specifically, the sample (α-alumina particles) was placed in a pressurized decomposition vessel and leached under pressure with a sodium carbonate solution. After that, the solution after pressurized decomposition was diluted to a fixed volume with water, and the emission intensity of each element at different wavelengths was measured using an ICP emission spectrometer. The concentration of each element was calculated from a calibration curve created simultaneously.
[0079] <Impurity Amount (Cl)> The chlorine (Cl) content of α-alumina particles (final product) was determined by the mercury thiocyanate-absorbance spectrophotometric method. Specifically, the sample (α-alumina particles) was decomposed under pressure using a sodium hydroxide decomposition solution, cooled, and then acidified with perchloric acid. Iron thiocyanate was generated by adding a portion of the solution to iron perchlorate solution and mercury thiocyanate aqueous solution. The Cl concentration was then calculated by measuring the orange absorbance hardness of the generated iron thiocyanate at a wavelength of 560 nm.
[0080] <Impurity Amount (U)> The uranium (U) content of aluminum hydroxide particles (raw material) and α-alumina particles (final product) was determined by ICP-MS. Specifically, as a pretreatment, the sample (aluminum hydroxide particles or α-alumina particles) was acid-decomposed by microwave, and the amount of U was analyzed using an inductively coupled plasma mass spectrometer (Agilent Technologies, Agilent 8800).
[0081] <α-crystallization rate> The α-crystallization rate was determined by analyzing α-alumina particles (final product) using X-ray diffraction (XRD). During the measurement, the intensity of the crystal planes (012) and (116) was measured. Specifically, an X-ray diffraction analyzer (Rigaku Corporation, RINT Ultima III / PC (3kWHF)) was used to scan the range 2θ: 24.98 to 26.30° to measure the diffraction intensity (I) of the crystal plane (012). (012) ) is determined, and the diffraction intensity (I) of the crystal plane (116) is determined by scanning the range of 2θ: 56.98 to 58.30°. (116) The diffraction intensity (I) of the (012) plane was determined. The measurement was performed under the conditions of Cu / Kα line, 40kV / 40mA, scan speed 2.0 degrees / min, and step 0.02 degrees. Furthermore, a standard sample with 100% alpha-adjustment (Nikkei Kako Co., Ltd., Ultramicron) was used as the sample, and the diffraction intensity (I) of the (012) plane was determined using the same method. st(012) ) and the diffraction intensity of the (116) plane (I st(116) The diffraction intensity was then determined. The degree of alpha-ization (alpha-crystallization rate) was calculated using the obtained diffraction intensity according to equation (3) below.
[0082]
[0083] <Thermal Conductivity> The thermal conductivity of α-alumina particles (final product) was determined by the hot disk method. Specifically, a resin was obtained by mixing silicone rubber (Shin-Etsu Chemical Co., Ltd., KE-103) and a curing agent (Shin-Etsu Chemical Co., Ltd., CAT-103) in a mass ratio of 100:5. Next, α-alumina particles were mixed into the obtained resin to a ratio of 38.1 volume%, and an analytical sample was prepared. The thermal conductivity of this analytical sample was then measured using a thermal conductivity measuring device (Kyoto Electronics Manufacturing Co., Ltd., TPS-500S).
[0084] (3) Evaluation Results The evaluation results obtained are summarized in Table 1 below.
[0085] The α-alumina particles produced by the method of this embodiment (Examples 1 and 2) were found to have a circularity of 0.68 to 0.70 and an aspect ratio of 1.39 to 1.41, indicating a non-spherical shape. Furthermore, the average particle size was 0.4 μm and the specific surface area (BET) was 6.2 to 8.0 m². 2 The particle size was found to be the desired size, with a density of 1 / g. Furthermore, despite a high α-crystallization rate of 76.3% or more, the sulfur (S) content was low at 10 ppm or less, and the chlorine (Cl) content was also low at 20 ppm or less. In addition, the uranium (U) content was extremely low at 5 ppb or less.
[0086] In contrast, α-alumina particles produced by calcining the raw materials at high temperatures (1230°C) (Comparative Example 1) and α-alumina particles produced using calcination containers that were not heat-treated (Comparative Example 2) had relatively high uranium (U) content of 9 to 23 ppb. Commercially available high-purity spherical alumina (Comparative Example 3) and high-purity alumina (Comparative Example 4) also had high uranium (U) content of 14 to 170 ppb. Furthermore, α-alumina particles produced by acid washing and alkaline washing (Comparative Examples 5 to 8) had very high sulfur content of 10 to 380 ppm (Comparative Examples 5 to 8) and chlorine content of 180 ppm (Comparative Example 5).
[0087]
[0088] From the above results, it can be understood that, according to this embodiment, non-spherical α-alumina particles and a method for producing the same can be obtained, which have a desired particle size, a high α-crystallization rate, low sulfur and chlorine content, and an extremely low uranium content.
[0089] 1. Firing container 2. Firing container body 2a. Inner wall side section 2b. Inner wall bottom section 3. Lid 4. Aluminum hydroxide filler 5. Sheet material 5a. Opening
Claims
1. The circularity is 0.80 or less, the aspect ratio is 1.30 or more, the average particle size is 0.1 μm or more and 1.0 μm or less, and the specific surface area is 12.0 m². 2 Alpha-alumina particles having a concentration of 0.5 / g or less, a sulfur (S) content of 20 ppm or less, a chlorine (Cl) content of 40 ppm or less, a uranium (U) content of 5 ppb or less, and an alpha crystallization rate of 70% or more.
2. The α-alumina particles according to claim 1, wherein the sodium (Na) content is 50 ppm or less and the amount of dissolved sodium (Na) is 10 ppm or less.
3. A method for producing α-alumina particles, comprising the step of firing aluminum hydroxide particles in a firing container at a temperature of 1100°C to 1200°C to produce a fired product, wherein the uranium (U) content of the aluminum hydroxide particles is 3 ppb or less, and the firing container is made of alumina (Al 2 O 3 ) contains 85% to 93% by mass of silica (SiO 2 A method in which a high-alumina container containing ) in a proportion of 7% by mass to 14% by mass is pre-fired at a temperature of 1100°C or higher, and when firing the aluminum hydroxide particles, the firing is carried out in a state in which the contact area between the aluminum hydroxide particle filler and the firing container is 30% or less of the surface area of the filler.
4. The method according to claim 3, wherein when filling the firing container with aluminum hydroxide particles, a sheet material that disappears during firing is interposed between the aluminum hydroxide particle filling and the firing container.