Conductive room temperature-curable organopolysiloxane composition

The composition addresses the challenge of achieving high conductivity and shielding by using a specific organopolysiloxane with diverse inorganic fillers, providing effective electromagnetic shielding and conductivity in a wide frequency range.

WO2026234921A1PCT designated stage Publication Date: 2026-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/013497
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-03-31
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional room-temperature curable organopolysiloxane compositions struggle to achieve high electrical conductivity and electromagnetic shielding performance, especially in the high-frequency band, often requiring large amounts of conductive metal powders and volatile organic solvents, leading to poor durability and stability under high-temperature and high-humidity conditions.

Method used

A conductive, room-temperature curable organopolysiloxane composition comprising an organopolysiloxane with hydrolyzable silyl groups and two or more inorganic fillers with different shapes, such as metals, metal oxides, or metal-coated powders, to enhance conductivity and electromagnetic shielding across a wide frequency range.

Benefits of technology

The composition achieves low volume resistivity and high electromagnetic shielding with a rate of -80 dB or less across a wide frequency range, suitable for electronic equipment and switch part contacts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a room temperature-curable organopolysiloxane composition which has a low volume resistivity, exhibits good conductivity, has an electromagnetic wave shielding rate of -80 dB or less in a wide frequency band, and forms a cured product that has high electromagnetic wave shielding properties. The conductive room temperature-curable organopolysiloxane composition comprises (A) a linear organopolysiloxane which is blocked with a hydrolyzable silyl group having two or three organooxy groups each bonded to a silicon atom at both terminals of the molecular chain, (B) a silane compound having a hydrolyzable group or a partial hydrolysis-condensation product thereof, (C) an inorganic filler, and (D) a curing catalyst. The inorganic filler (C) contains two or more materials that are selected from the group consisting of a metal containing a transition metal, an oxide of a transition metal, and a powder coated with a transition metal, and have different shapes.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive, room-temperature curable organopolysiloxane composition

[0001] The present invention relates to a conductive room-temperature curable organopolysiloxane composition that hardens at room temperature (23°C ± 15°C) due to atmospheric moisture (water) to provide a cured silicone rubber product (silicone elastomer elastic body). The present invention relates to a conductive room-temperature curable organopolysiloxane composition that, through a specific combination of inorganic fillers, achieves high electrical conductivity and improved electromagnetic wave shielding rate over a wide frequency range, which were difficult to achieve with conventional room-temperature curable organopolysiloxane compositions.

[0002] Room-temperature curable (RTV) silicone rubber compositions, which crosslink and harden upon contact with moisture, are easy to handle and possess excellent weather resistance and electrical properties, making them suitable for a variety of applications, such as sealants for building materials and adhesives in the electrical and electronic fields. Typical room-temperature curable organopolysiloxane compositions contain a diorganopolysiloxane (base polymer) having silanol groups (hydroxyl groups bonded to silicon atoms) or alkoxysilyl groups at the ends of the molecular chain, a curing agent, an aminoalkyl group-containing alkoxysilane, and a curing catalyst. Various fillers are added as needed to impart properties such as flame retardancy, thermal conductivity, and tensile strength.

[0003] Deoxime-type, room-temperature curable organopolysiloxane compositions, commonly known as building and structural sealants, are widely used due to their curability, durability, and adhesion to various substrates. However, the resulting cured product undergoes significant changes in rubber properties when exposed to high-temperature and high-humidity environments, resulting in poor durability. Deacetic acid-type, room-temperature curable organopolysiloxane compositions are also widely used as building and structural sealants. They are known for their excellent curability and adhesion, as well as minimal discoloration from UV irradiation. However, the acetic acid generated during curing makes them difficult to work with.

[0004] Furthermore, conductive metal powders, carbon black, or conductive silicone rubber compositions using a combination of these have been conventionally known as sealing materials used for electromagnetic shielding in electrical and electronic equipment and for contacts in switch parts. However, in order to design a silicone rubber composition with the desired shielding and conductivity, it was necessary to incorporate a large amount of metal powder. For this reason, Patent Document 1 proposes a room-temperature curable composition in which conductivity is improved by adding a volatile organic solvent together with conductive metal powder to a known one-component room-temperature curable silicone rubber.

[0005] Furthermore, a room-temperature curable silicone rubber composition with stable conductivity has also been proposed, which is achieved by blending a silanol-terminated diorganopolysiloxane with conductive metal powder, a conductive filler such as carbon black, and a volatile organic solvent (Patent Document 2).

[0006] However, the silicone rubber compositions described in Patent Document 1 or Patent Document 2 cured slowly, and even when silver powder with high conductivity was used, sufficient conductivity could not be obtained.

[0007] On the other hand, Patent Document 3 discloses a room-temperature curable organopolysiloxane composition based on an organopolysiloxane having hydrolyzable alkoxy groups at its molecular ends, and incorporating predetermined amounts of silver powder, silver plating powder, and conductive carbon black. This composition exhibits good curability, excellent workability, and the cured product is stable over time, while also possessing conductivity and electromagnetic shielding properties. In the examples of Patent Document 3, the electromagnetic shielding performance was measured at 1 GHz, and a room-temperature curable organopolysiloxane composition with high shielding performance was obtained. However, shielding performance in the high-frequency band required for modern communication equipment and electrical and electronic equipment has not been confirmed.

[0008] Japanese Patent Publication No. 60-199057, Japanese Patent Publication No. 63-117065, Japanese Patent Publication No. 2005-162827

[0009] Therefore, the object of the present invention is to provide a room-temperature curable organopolysiloxane composition that exhibits low volume resistivity and good conductivity, and has a high electromagnetic shielding performance with an electromagnetic shielding rate of -80 dB or less over a wide frequency range.

[0010] The present inventors, through diligent research to solve the above problems, have found that the above objective can be achieved by a conductive, room-temperature curable organopolysiloxane composition comprising an organopolysiloxane having hydrolyzable silyl groups at the molecular chain ends as the main component (base polymer) and two or more specific inorganic fillers with different shapes, and thus have come to the present invention. That is, the present invention provides the following conductive, room-temperature curable organopolysiloxane composition, etc. <1> (A) 100 parts by mass of an organopolysiloxane represented by the following general formula (1), (In the formula, R 1 R is an independent unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, n is a number of 10 or more, X is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, 2 (A) is an independent substituted or unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, and a is independently 0 or 1 for each silicon atom to which it is bonded.) (B) A silane compound represented by the following general formula (2) or a partially hydrolyzed condensate thereof 0.1 to 30 parts by mass, (In the formula R 3(1) is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and (2) is 3 or 4. (3) is a hydrolyzable group. (4) A conductive room-temperature curable organopolysiloxane composition comprising (C) 1 to 1000 parts by mass of an inorganic filler and (D) 0.01 to 10 parts by mass of a curing catalyst, wherein (C) the inorganic filler comprises two or more types with different shapes selected from the group consisting of metals containing transition metals, oxides of transition metals, and powders coated with transition metals. <2> The conductive room-temperature curable organopolysiloxane composition according to <1>, wherein at least one of (C) the inorganic filler is in flake form. <3> The conductive room-temperature curable organopolysiloxane composition according to <1>, wherein at least one of (C) the inorganic filler is in flake form and the other is spherical. <4> A conductive room-temperature curable organopolysiloxane composition according to any one of <1> to <3>, wherein (C) a powder coated with a transition metal is used as an inorganic filler, and the powder coated with the transition metal is one or more selected from the group consisting of a metal containing a transition metal coated with a transition metal, an oxide of a transition metal coated with a transition metal, glass particles coated with a transition metal, and carbon particles coated with a transition metal. <5> A conductive room-temperature curable organopolysiloxane composition according to any one of <1> to <4>, wherein Y in formula (2) is an alkoxy group or an amino group. <6> The volume resistivity of the cured product is 1 × 10⁻⁶ -3 A conductive room-temperature curable organopolysiloxane composition according to any one of <1> to <5>, wherein the impedance is less than Ω·m and the electromagnetic shielding rate at frequencies of 1 to 20 GHz is -80 dB or less. <7> An article bonded or sealed with the conductive room-temperature curable organopolysiloxane composition according to any one of <1> to <6>.

[0011] The cured product of the composition of the present invention exhibits low volume resistivity and good conductivity, and has high electromagnetic shielding properties with an electromagnetic shielding rate of -80 dB or less across a wide frequency band. Therefore, the composition of the present invention can be suitably used for electromagnetic shielding applications in electronic equipment that have sufficient shielding properties in the high frequency band, and as a sealing material used in the contacts of switch parts.

[0012] Hereinafter, the present invention is described in detail. [(A) Component] The component (A) of the organopolysiloxane composition of the present invention acts as the main agent (base polymer) in the composition of the present invention, and is a linear organopolysiloxane blocked with hydrolyzable silyl groups each having 2 or 3 organooxy groups bonded to silicon atoms at both molecular chain terminals, which is represented by the following general formula (1). In formula (1), R 1 is independently an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, n is a number of 10 or more, X is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, and R 2 is independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, and a is independently 0 or 1 for each bonded silicon atom.

[0013] In the above formula (1), R 1 is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, for example, alkyl groups such as methyl group, ethyl group and propyl group; cyclic alkyl groups such as cyclohexyl group; alkenyl groups such as vinyl group and allyl group; aryl groups such as phenyl group and tolyl group; and groups in which part of the hydrogen atoms of these groups are substituted with halogen atoms, such as 3,3,3-trifluoropropyl group and the like. Among these, a methyl group is particularly preferred. A plurality of R 1 may be the same group or different groups.

[0014] In the above formula (1), n is a number of 10 or more, preferably a number of 10 to 2,000, more preferably a number of 20 to 1,500, still more preferably a number of 30 to 1,000, and particularly preferably a number of 50 to 800. The value of n is particularly preferably a number such that the viscosity of the diorganopolysiloxane of component (A) at 25°C is in the range of 25 to 500,000 mPa·s, preferably 500 to 100,000 mPa·s. In the present invention, the ((R 1 ) 2 SiO 2/2The number of repeating units n (or the degree of polymerization) of the bifunctional diorganosiloxane unit represented by ) can usually be determined as the polystyrene-equivalent number average degree of polymerization (or number average molecular weight) in gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent. In addition, the viscosity can usually be measured at 25°C with a rotational viscometer (for example, BL type, BH type, BS type, cone-plate type, rheometer, etc.).

[0015] In the above formula (1), X is an oxygen atom or an alkylene group having 1 to 4 carbon atoms. Examples of the alkylene group having 1 to 4 carbon atoms include a methylene group, ethylene group, trimethylene group, propylene group, propylidene group, isopropylidene group, tetramethylene group, butylene group, butylidene group, isobutylidene group, sec-butylidene group and the like. As X, an oxygen atom or an ethylene group is particularly preferred. In the case of an ethylene group, it is extremely versatile because it can be easily produced by subjecting an α,ω-divinyl-terminated polyorganosiloxane to an addition reaction with the corresponding hydrosilane in the presence of a metal catalyst.

[0016] In addition, in the above formula (1), R 2 is independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, for example, an alkyl group such as methyl group, ethyl group, propyl group; an alkoxy-substituted alkyl group such as methoxymethyl group, methoxyethyl group, methoxyethyl group, ethoxyethyl group; a cyclic alkyl group such as cyclohexyl group; an alkenyl group such as vinyl group, allyl group, propenyl group, phenyl group and the like, among which methyl group is particularly preferred.

[0017] a is independently 0 or 1 for each bonded silicon atom.

[0018] [(B) Component] The component (B) is a silane compound represented by the following general formula (2) or a partial hydrolytic condensate thereof, and acts as a crosslinking agent for the component (A). In formula (2), R 3 is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and a plurality of R 3 may be the same or different. Y is a hydrolyzable group. b is 3 or 4.

[0019] Here, in the above general formula (2), R 3 The unsubstituted or halogen-substituted monovalent hydrocarbon group has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and may be the same or different. Examples thereof include alkyl groups such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, tert-butyl group, pentyl group, neopentyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, octadecyl group, nonadecyl group and eicosyl group; cycloalkyl groups such as cyclopentyl group and cyclohexyl group; alkenyl groups such as vinyl group, allyl group, propenyl group, isopropenyl group, butenyl group, pentenyl group and hexenyl group; aryl groups such as phenyl group, tolyl group, xylyl group, α- and β-naphthyl groups; aralkyl groups such as benzyl group, 2-phenylethyl group and 3-phenylpropyl group; and groups in which part or all of the hydrogen atoms in these groups are substituted with halogen atoms such as F, Cl and Br, for example, 3-chloropropyl group, 3,3,3-trifluoropropyl group and the like. Among these, alkyl groups having 1 to 10 carbon atoms such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, tert-butyl group, pentyl group, neopentyl group, hexyl group, heptyl group, octyl group, nonyl group and decyl group, and phenyl group are preferred.

[0020] b in the general formula (2) is 3 or 4.

[0021] Y in the general formula (2) represents a hydrolyzable group, which is preferably a group selected from the group consisting of alkoxy groups having 1 to 4 carbon atoms, ketoxime groups having 3 to 5 carbon atoms, alkenyloxy groups having 2 to 4 carbon atoms such as isopropenoxy group, acyloxy groups having 2 to 3 carbon atoms such as acetoxy group, dialkylaminoxy groups having 2 to 4 carbon atoms such as dimethylaminoxy group, and amino groups having 1 to 6 carbon atoms. Among these, alkoxy groups, ketoxime groups and amino groups are preferred, and alkoxy groups and amino groups are particularly preferred. The hydrolyzable groups Y may be the same or different.

[0022] (B) Specific examples of components include ketoxime silanes such as methyltris(dimethylketoxime)silane, methyltris(methylethylketoxime)silane, ethyltris(methylethylketoxime)silane, methyltris(methylisobutylketoxime)silane, vinyltris(methylethylketoxime)silane, and phenyltris(methylethylketoxime)silane; methyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, n-decyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, tetra- Examples include alkoxysilanes such as toxysilane; isopropenoxy group-containing silanes such as methyltriisopropenoxysilane, ethyltriisopropenoxysilane, vinyltriisopropenoxysilane, and phenyltriisopropenoxysilane; acetoxysilanes such as methyltriacetoxysilane, ethyltriacetoxysilane, and vinyltriacetoxysilane; silanes in which nitrogen and silicon are bonded, such as N,N',N''-tributyl-1-methylsilanetriamine, and partially hydrolyzed condensates of these silanes. Component (B) may be used alone or in combination of two or more. Among these, alkoxysilanes such as methyltrimethoxysilane, vinyltrimethoxysilane, n-decyltrimethoxysilane, and tetraethoxysilane, and N,N',N''-tributyl-1-methylsilanetriamine are preferred.

[0023] The amount of component (B) is 0.1 to 30 parts by mass, preferably 0.5 to 20 parts by mass, and more preferably 1 to 15 parts by mass, per 100 parts by mass of component (A). If the amount of component (B) is too small, the end sealing rate will be poor and storage stability may decrease. If the amount of component (B) is too large, the resulting cured product may have drawbacks such as reduced mechanical properties and a slower curing speed.

[0024] [Component (C)] Component (C), an inorganic filler, is an important component added to the composition of the present invention for the purpose of providing electrical conductivity and electromagnetic shielding properties over a wide frequency range. The inorganic filler is selected from the group consisting of metals containing transition metals, oxides of transition metals, and powders coated with transition metals, and includes two or more types that have different shapes from each other. Examples of transition metals include first transition metals such as titanium, manganese, iron, nickel, and copper; second transition metals such as zirconium, molybdenum, ruthenium, palladium, and silver; and third transition metals such as cerium, samarium, ytterbium, tantalum, tungsten, and osmium. Among these, first and second transition metals are preferred. The metal containing a transition metal may be the aforementioned transition metals. The metal containing a transition metal may also be an alloy of the aforementioned transition metals. The alloy of a transition metal may be an alloy of the above first and second transition metals. The metal containing a transition metal may be an alloy containing the above transition metals and metals other than transition metals such as zinc and aluminum. Examples of alloys containing metals other than transition metals include copper-nickel-zinc and aluminum-zinc-magnesium-copper.

[0025] Furthermore, examples of transition metal-coated powders include metals containing transition metals coated with these transition metals (i.e., metal powders with a transition metal-containing metal as the core and coated with a transition metal), transition metal oxides coated with transition metals (i.e., metal oxide powders with a transition metal oxide as the core and coated with a transition metal), transition metal-coated glass particles (i.e., glass particle powders with a glass particle core and coated with a transition metal), and transition metal-coated carbon particles (i.e., carbon particle powders with a carbon particle core and coated with a transition metal). The transition metals used for coating are preferably silver, nickel, copper, etc. In transition metal-coated powders, the amount of transition metal coating is preferably 5 to 80% by mass, and more preferably 5 to 60% by mass. Furthermore, examples of metal processing methods include atomization, chemical reduction, plasma rotating electrode method, and uniform droplet spraying method.

[0026] Examples of particle shapes for inorganic fillers include spherical (in this specification, "spherical" includes not only perfect spheres but also "rounded" particles with few corners and a smooth, rounded shape), flake (scale-like, flake-like, plate-like), crushed, irregularly shaped, needle-like, etc., and the composition of the present invention is characterized by containing two or more different shapes from these as inorganic fillers. The particle shape of the inorganic filler can be confirmed by observing the inorganic filler in question with an electron microscope. Preferably, at least one of the inorganic fillers is flake-shaped, and more preferably, at least one is flake-shaped and the other is spherical (including rounded). In particular, in order for the resulting cured product to have excellent electromagnetic wave shielding properties, the total content of metals containing flake-shaped transition metals and powders coated with flake-shaped transition metals is preferably 5 to 80% by mass of the total mass of the inorganic filler, and more preferably 5 to 60% by mass.

[0027] Furthermore, the particle size of the inorganic filler is preferably 0.1 μm to 200 μm, and particularly preferably 1 μm to 150 μm. If the particle size exceeds 200 μm, the surface roughness of the silicone rubber sheet formed from the composition of the present invention increases, and it may not be suitable for the manufacture of articles equipped with electronic components, etc. If the particle size is less than 0.1 μm, the dispersibility and filling properties with component (A) will be poor, and the overall elasticity of the silicone rubber may be impaired. The above particle size can be measured by methods such as laser diffraction, sieve analysis, or sedimentation analysis, depending on the composition and shape of the inorganic filler.

[0028] Component (C) is used in an amount of 1 to 1,000 parts by mass, preferably 1 to 800 parts by mass, relative to 100 parts by mass of organopolysiloxane (Component (A)). If the amount is less than 0.1 parts by mass, the composition will not have sufficient strength, nor will it have sufficient conductivity and electromagnetic shielding properties. If the amount exceeds 1,000 parts by mass, the processability of the silicone will decrease, the elasticity of the resulting rubber properties will be impaired, and problems may arise that make it economically disadvantageous.

[0029] [Component (D)] The curing catalyst for component (D) is not particularly limited as long as it has condensation catalytic activity, but metal-based condensation catalysts and non-metal-based condensation catalysts can be suitably used, and one type may be used alone or as a mixture of two or more types.

[0030] Examples include organic carboxylates and alkoxides of metals such as tin, titanium, zirconium, iron, antimony, bismuth, and manganese; organotitanic acid esters; and organotitanium chelate compounds. More specifically, tin compounds such as dibutyltin dilaurate, dibutyltin dioctoate, dioctyltin dilaurate, dibutyltin maleate ester, dimethyltin dineodecanoate, dibutyltin dimethoxide, dioctyltin dineodecanoate, and stanus octoate; titanate esters or titanium chelate compounds such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetrakis(2-ethylhexoxy)titanium, isopropoxytitanium bis(ethyl acetacetate), isopropoxybis(acetylacetonate)titanium, and titanium isopropoxyoctylene glycol; aluminum alcoholates or aluminum chelate compounds such as aluminum isopropylate, aluminum sec-butyrate, aluminum ethyl acetacetate aluminum diisopropylate, aluminum tris(ethyl acetacetate), and alkylacetate aluminum diisopropylate; Examples of catalysts include silanes or siloxanes containing a guanidyl group, such as tetramethylguanidylpropyltrimethoxysilane, tetramethylguanidylpropylmethyldimethoxysilane, and tetramethylguanidylpropyltris(trimethylsiloxy)silane; amine compounds and their salts, such as dibutylamine and laurylamine; organosilazane compounds, such as hexamethyldisilazane; and conventionally known catalysts such as lead octoate and other acidic or basic catalysts. Among these, tin compounds, organotitanium compounds, aluminum alcoholates, or aluminum chelate compounds are preferred, with tin compounds and organotitanium compounds being particularly preferred. The amount added is 0.01 to 10 parts by mass, preferably 0.05 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, per 100 parts by mass of component (A). If the amount is less than 0.01 parts by mass, sufficient crosslinking (curability) may not be obtained, and if it exceeds 10 parts by mass, it may be disadvantageous in terms of price or cause problems such as a decrease in curing speed.

[0031] [Other Components] In order to further improve the adhesion of the cured product of the present invention to various adherends, a silane coupling agent (a hydrolyzable silane compound such as an alkoxysilane having a monovalent hydrocarbon group having a functional group (excluding a guanidyl group) containing a heteroatom selected from nitrogen, sulfur, and oxygen in one molecule, or a so-called carbon functional silane compound) may be added to the composition as an adhesion imparting agent as an optional component that can be added as needed. Examples of silane coupling agents include silane compounds having an alkoxysilyl group or an alkenoxysilyl group as the hydrolyzable group, such as vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-(N-amino Examples include methylbenzylamino)propyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N,N-bis[3-(trimethoxysilyl)propyl]amine, γ-mercaptopropyltrimethoxysilane, γ-glycidoxypropyltriisopropenoxysilane, γ-glycidoxypropylmethyldiisopropenoxysilane, reaction products of (meth)acrylsilane and aminosilane, reaction products of epoxysilane and aminosilane, and reaction products of aminosilane and halogenated alkyl group-containing silane. In particular, the use of a silane coupling agent having at least one amino group in one molecule is preferred.

[0032] When a silane coupling agent is included, the amount included is usually 0.1 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass, per 100 parts by mass of component (A). If the amount is less than 0.1 parts by mass, sufficient adhesion may not be obtained, and if it exceeds 20 parts by mass, good mechanical properties may not be obtained, or it may be unfavorable in terms of cost.

[0033] Furthermore, various additives may be blended as optional components. Known additives may be added as long as they do not impair the objectives of the present invention. The optional additive components exemplified below have known blending ranges depending on their purpose, and in particular, known blending ranges in the field of organopolysiloxane compositions, especially conductive room-temperature curable organopolysiloxane compositions, can be referenced. The known blending ranges differ for each type of additive and are not particularly limited, but as an example, per 100 parts by mass of component (A), the amount may be 300 parts by mass or less, 100 parts by mass or less, 50 parts by mass or less, or 30 parts by mass or less. An example of an additive is a wetter (for example, a single-terminated trialkoxysilyl group-blocked organopolysiloxane represented by formula (3)). In the formula, R 4 R is independently an unsubstituted or substituted monovalent hydrocarbon group. 5 R is independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group, m is a number from 2 to 100, and x is an integer from 1 to 3. In formula (3), R 4 These are independently unsubstituted or substituted monovalent hydrocarbon groups, preferably having 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 3 carbon atoms. Examples include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, and octyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, pentenyl, and hexenyl groups; aryl groups such as phenyl, tolyl, xylyl, and α-,β-naphthyl groups; aralkyl groups such as 2-phenylethyl and 3-phenylpropyl groups; and groups in which some or all of the hydrogen atoms of these groups are substituted with halogen atoms such as F, Cl, Br, or cyano groups, such as halogenated alkyl groups such as 3,3,3-trifluoropropyl, 2-(nonafluorobutyl)ethyl, and 2-(heptadecafluorooctyl)ethyl groups; and cyanoalkyl groups such as cyanoethyl groups. 4 Preferably, R is a methyl group, a phenyl group, or a vinyl group. In formula (3), R5 R is independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group. 5 The C1 is preferably C1 to C8, and more preferably C1 to C3. Examples of alkyl groups include R 4 Examples of alkyl and cycloalkyl groups are similar to those exemplified above. Examples of alkoxyalkyl groups include methoxyethyl group and methoxypropyl group. Examples of acyl groups include acetyl group and octanoyl group. 5 The group is preferably an alkyl group, and more preferably a methyl group or an ethyl group. m is a number from 2 to 100, preferably a number from 5 to 80. x is an integer from 1 to 3, preferably 3.

[0034] Other examples of additives include polyether compounds as thixotropy enhancers, non-reactive dimethyl silicone oil (dimethylpolysiloxane with trialkylsilyl groups sealed at both ends of the molecular chain) and isoparaffins as plasticizers, and trimethylsiloxy units [(CH4] as crosslink density enhancers]. 3 ) 3 SiO 1/2 Units] and SiO 2 Examples include organopolysiloxane resins with a three-dimensional network structure consisting of units. Furthermore, if necessary, colorants such as pigments, dyes, and fluorescent whitening agents; antifungal agents; antibacterial agents; bleed oils such as non-reactive phenyl silicone oil (methylphenylpolysiloxane with trialkylsilyl groups sealed at both ends of the molecular chain) and fluorosilicone oil (methyl(3,3,3-trifluoropropyl)polysiloxane with trialkylsilyl groups sealed at both ends of the molecular chain); surface modifiers such as organic liquids that are incompatible with silicone; and solvents such as toluene, xylene, solvent volatile oils, cyclohexane, methylcyclohexane, and low-boiling point isoparaffins may also be added. The room-temperature curable organopolysiloxane composition of the present invention may contain volatile solvents such as toluene and xylene as optional components, but the desired electromagnetic shielding properties will be achieved even if they are not included.

[0035] The room-temperature curable organopolysiloxane composition of the present invention can be stored in a moisture-free atmosphere, and when left at room temperature (23°C ± 15°C) in an airy atmosphere, it usually hardens in 5 minutes to 1 week due to moisture in the air.

[0036] The following examples and comparative examples illustrate the present invention in detail, but the present invention is not limited to the following examples. In the examples, viscosity is measured using a rotational viscometer at 25°C, and the degree of polymerization is the number-average degree of polymerization in polystyrene terms obtained by gel permeation chromatography analysis using toluene as the developing solvent.

[0037] The inorganic filler (C) used in the example is shown below. (C-1): A rounded metal powder with a copper-nickel-zinc alloy core prepared by atomization, coated with silver (specific surface area 0.34 m²). 2 / g, particle size (volume-based D50 by laser diffraction method in accordance with JIS Z8825) 3.0 μm, silver coating amount 10.5% by mass (C-2): Flake-shaped metal powder with a copper-nickel-zinc alloy core prepared by atomization method and silver coated (specific surface area 0.48 m²) 2 / g, particle size (volume-based D50 according to laser diffraction method in accordance with JIS Z8825) 3.3 μm, silver coating amount 10.5 mass%) (C-3): Silver-coated spherical glass beads (particle size (value calculated from particle size according to JIS R3301) 6 μm, silver coating amount 50 mass%) (C-4): Nickel-coated flake carbon particles (Oerlikon Metco E-Fill 2801, particle size (value according to sieve analysis test method in accordance with ASTM-B214) 80 μm, nickel coating amount 75 mass%) (C-5): Silver-coated spherical glass beads (particle size (value calculated from particle size according to JIS R3301) 20 μm, silver coating amount 12 mass%)

[0038] [Example 1] Both ends of the molecular chain are sealed with dimethoxymethylsilyl groups, and the viscosity at 25°C is 20,000 mm². 2 / s polydimethylsiloxane (in general formula (1), R 1 is a methyl group, R 2(where a is a methyl group, X is an oxygen atom, a=1, n=610) 100 parts by mass, with a viscosity of 30 mm at 25°C. 2 Mixture A was prepared by uniformly mixing and stirring 20 parts by mass of the organopolysiloxane of the following structural formula (3-1) of / s, 5 parts by mass of n-decyltrimethoxysilane, 1 part by mass of N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and 0.05 parts by mass of dioctyltin dilaurate for 30 minutes. Then, composition 1 was obtained by mixing 30 parts by mass of toluene, 100 parts by mass of (C-1), 100 parts by mass of (C-2), and 300 parts by mass of (C-3) with 100 parts by mass of the above mixture A under reduced pressure for 20 minutes.

[0039]

[0040] [Example 2] Both ends of the molecular chain are sealed with dimethoxymethylsilyl groups, and the viscosity at 25°C is 20,000 mm². 2 / s polydimethylsiloxane (in general formula (1), R 1 is a methyl group, R 2 (where a is a methyl group, X is an oxygen atom, a=1, n=610) 100 parts by mass, with both ends of the molecular chain sealed with trimethylsilyl groups, and a viscosity of 100 mm at 25°C. 2 250 parts by mass of organopolysiloxane at 0 / s, 100 parts by mass of (C-2), 300 parts by mass of (C-3), and 100 parts by mass of (C-4) were mixed under reduced pressure for 20 minutes. Then, 5 parts by mass of n-decyltrimethoxysilane, 1 part by mass of N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and 0.05 parts by mass of dioctyltin dilaurate were mixed under reduced pressure for 20 minutes to obtain composition 2.

[0041] [Comparative Example 1] Both ends of the molecular chain are sealed with dimethoxymethylsilyl groups, and the viscosity at 25°C is 20,000 mm². 2 / s polydimethylsiloxane (in general formula (1), R 1 is a methyl group, R 2 (where a is a methyl group, X is an oxygen atom, a=1, n=610) 100 parts by mass, with both ends of the molecular chain sealed with trimethylsilyl groups, and a viscosity of 100 mm at 25°C. 2250 parts by mass of organopolysiloxane at 0 / s, 30 parts by mass of xylene, and 1000 parts by mass of (C-5) were mixed under reduced pressure for 20 minutes. Then, 5 parts by mass of n-decyltrimethoxysilane, 1 part by mass of N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and 0.05 parts by mass of dioctyltin dilaurate were mixed under reduced pressure for 20 minutes to obtain composition 3.

[0042] [Comparative Example 2] Both ends of the molecular chain are sealed with dimethoxymethylsilyl groups, and the viscosity at 25°C is 20,000 mmHg. 2 / s polydimethylsiloxane (in general formula (1), R 1 is a methyl group, R 2 (where a is a methyl group, X is an oxygen atom, a=1, n=610) 100 parts by mass, with both ends of the molecular chain sealed with trimethylsilyl groups, and a viscosity of 100 mm at 25°C. 2 250 parts by mass of organopolysiloxane at 0 / s, 100 parts by mass of (C-1), and 300 parts by mass of (C-3) were mixed under reduced pressure for 20 minutes. Then, 5 parts by mass of n-decyltrimethoxysilane, 1 part by mass of N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and 0.05 parts by mass of dioctyltin dilaurate were mixed under reduced pressure for 20 minutes to obtain composition 4.

[0043] [Comparative Example 3] Both ends of the molecular chain are sealed with dimethoxymethylsilyl groups, and the viscosity at 25°C is 20,000 mm². 2 / s polydimethylsiloxane (in general formula (1), R 1 is a methyl group, R 2 (where a is a methyl group, X is an oxygen atom, a=1, n=610) 100 parts by mass, with both ends of the molecular chain sealed with trimethylsilyl groups, and a viscosity of 100 mm at 25°C. 2 250 parts by mass of organopolysiloxane at 0 / s, 300 parts by mass of (C-2), and 300 parts by mass of (C-4) were mixed under reduced pressure for 20 minutes. Then, 5 parts by mass of n-decyltrimethoxysilane, 1 part by mass of N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and 0.05 parts by mass of dioctyltin dilaurate were mixed under reduced pressure for 20 minutes to obtain composition 5.

[0044] The following properties were measured using the prepared compositions 1 to 5: • Tack-free time: The tack-free time (minutes) of each of the prepared compositions 1 to 5 was evaluated by touch in a 23°C / 50% RH environment according to the method described in JIS K 6249. The results are shown in Table 1.

[0045] Each of the curable compositions 1 to 5 was left to cure for 7 days at 23°C / 50% RH until it reached a thickness of 3 mm, and its hardness was measured according to JIS K 6249. The results are shown in Table 1.

[0046] • Conductivity (Volume Resistivity) Each of the prepared compositions 1 to 5 was left to cure for 7 days at 23°C / 50% RH until it reached a thickness of 1 mm, and the volume resistivity was measured according to JIS K 6249. The volume resistivity was 1 × 10⁻⁶ -3 It is preferable that it be less than Ω·m, 5 × 10 -4 It is more preferable that the value be Ω·m or less. The results obtained are shown in Table 1.

[0047] Each of the electromagnetic shielding compositions 1 to 5 was cured in a 23°C / 50% RH environment for 7 days until it reached a thickness of 0.5 mm, to produce sheet-like cured materials. The shielding effect (dB) at 1 to 20 GHz was measured using a vector network analyzer (Keysight PNA N5222B) with these cured materials. It is preferable that the electromagnetic shielding rate at frequencies of 1 to 20 GHz be -80 dB or less. The obtained results are shown in Table 1.

[0048]

[0049] (C) Composition 1 of Example 1 and Composition 2 of Example 2, which include two or more inorganic fillers with different shapes, were found to have high electromagnetic shielding rates of -80 dB or less across a wide frequency band. On the other hand, in Composition 3 of Comparative Example 1, although the volume resistivity itself was low due to the use of silver-coated glass beads, the desired electromagnetic shielding performance was not achieved. Furthermore, in Composition 4 of Comparative Example 2, which includes two inorganic fillers classified as spherical in shape, and Composition 5 of Comparative Example 3, which includes two inorganic fillers classified as flake-shaped, the desired electromagnetic shielding performance was not achieved.

Claims

1. (A) 100 parts by mass of organopolysiloxane represented by the following general formula (1), (In the formula, R 1 R is an independent unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, n is a number of 10 or more, X is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, 2 (A) is an independent substituted or unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, and a is independently 0 or 1 for each silicon atom to which it is bonded.) (B) A silane compound represented by the following general formula (2) or a partially hydrolyzed condensate thereof 0.1 to 30 parts by mass, (In the formula R 3 (c) is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and (d) is 3 or 4. Y is a hydrolyzable group.) A conductive room-temperature curable organopolysiloxane composition comprising (c) 1 to 1000 parts by mass of an inorganic filler, and (d) 0.01 to 10 parts by mass of a curing catalyst, wherein (c) the inorganic filler comprises two or more types with different shapes selected from the group consisting of metals containing transition metals, oxides of transition metals, and powders coated with transition metals.

2. (C) The conductive room-temperature curable organopolysiloxane composition according to claim 1, wherein at least one of the inorganic fillers is in flake form.

3. (C) The conductive room-temperature curable organopolysiloxane composition according to claim 1, wherein at least one of the inorganic fillers is in flake form and the other is spherical.

4. (C) A conductive room-temperature curable organopolysiloxane composition according to claim 1, comprising a powder coated with a transition metal as an inorganic filler, wherein the powder coated with the transition metal is one or more selected from the group consisting of a metal containing a transition metal coated with a transition metal, an oxide of a transition metal coated with a transition metal, glass particles coated with a transition metal, and carbon particles coated with a transition metal.

5. The conductive room-temperature curable organopolysiloxane composition according to claim 1, wherein Y in formula (2) is an alkoxy group or an amino group.

6. The volume resistivity of the cured material is 1 × 10⁻⁶. -3 The conductive, room-temperature curable organopolysiloxane composition according to claim 1, wherein the electromagnetic shielding rate is less than Ω·m and less than -80 dB at frequencies of 1 to 20 GHz.

7. An article bonded or sealed with a conductive room-temperature curable organopolysiloxane composition according to any one of claims 1 to 6.