Hydrophobic vapor-phase silica fine particles and resin composition

Hydrophobic vapor-phase silica fine particles with controlled surface treatment and shear force application address non-uniform treatment issues, resulting in improved dispersibility and mechanical properties in resin compositions.

WO2026235002A1PCT designated stage Publication Date: 2026-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016147
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-04-22
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for hydrophobizing fumed silica fine particles result in non-uniform surface treatment, leading to increased silanol group exposure, high viscosity in resin compositions, and limited filling amounts due to re-aggregation, which affects handleability and molding defects.

Method used

Hydrophobic vapor-phase silica fine particles with specific surface area, particle size, and hydrophobicity criteria, produced through a method involving physical shear force and controlled surface treatment, ensuring uniform treatment and suppressed re-aggregation.

Benefits of technology

The method achieves high hydrophobicity, improved dispersibility, and reduced viscosity in resin compositions, allowing for enhanced filling capacity and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention provides hydrophobic vapor-phase silica fine particles which are characterized by satisfying all of the following conditions (1)-(3), and which have a high degree of hydrophobization and suppressed reaggregation, and have a smaller average particle diameter in a methanol dispersion medium than conventional particles. (1) The BET specific surface area is 20-400 m2 / g, (2) the volume-based median diameter (D50L) in the methanol dispersion medium as measured by a laser diffraction method is 200 nm or less, the volume-based median diameter (D50D) in the methanol dispersion medium as measured by a dynamic light scattering method is 150 nm or less, and D50L≥D50D, and (3) the degree of hydrophobicity determined by a methanol titration method is 70% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Hydrophobic fumed silica fine particles and resin composition

[0001] The present invention relates to hydrophobic fumed silica fine particles, which are dry-process silica fine particles exhibiting hydrophobicity, and a resin composition.

[0002] The method of hydrolyzing a halogenated silane such as tetrachlorosilane in an oxyhydrogen flame is called a gas phase method. The dry-process silica fine particles (also referred to as fumed silica fine particles) obtained by this method are used as fillers for silicone resins, inks, paints and the like, and have effects of imparting reinforcing effect and thixotropy.

[0003] Fumed silica fine particles have silanol (Si-OH) groups on their surfaces and exhibit hydrophilicity. Although they may be used as they are, the silanol groups on the surface are often subjected to hydrophobic treatment with a reactive organosilicon compound in order to meet a wide range of applications.

[0004] Methods for hydrophobizing the surface of fumed silica fine particles are generally well-known techniques. For example, when fumed silica fine particles are placed in a mechanical mixer or a fluidized tank at normal pressure and brought into contact with an organosilicon compound in a liquid or gaseous state under an inert gas atmosphere, the surface of the silica fine particles (hereinafter sometimes referred to as silica fine particles or simply particles) is hydrophobized.

[0005] However, in these treatment methods, since the fumed silica fine particles come into contact with the organosilicon compound in the state of agglomerates, it is difficult to uniformly treat the fine details of the surfaces of the primary particles constituting the agglomerated aggregates. Such hydrophobic fumed silica fine particles are disadvantageous in handling after being filled into a resin such as silicone. That is, when kneading with the resin, mechanical pulverization occurs on the agglomerated aggregates of the fumed silica fine particles, so that non-hydrophobized fractured surfaces (particle surfaces) are exposed, and the amount of silanol groups on the surface of the silica fine particles, which was apparently low, increases. The resin composition obtained thereby has an increased viscosity due to the interaction between silanol groups, and the handleability during molding is extremely deteriorated. In addition, when the filler is filled into the resin, if the filling amount is increased beyond a certain level, the filler will not integrate with the resin and molding defects will occur, so the filling amount is limited.

[0006] As a way to improve these conditions, Japanese Patent Publication No. 2000-256008 (Patent Document 1) describes a method to improve the degree of surface treatment by hydrophobizing dry silica fine particles, then mechanically grinding the agglomerate aggregates to expose the untreated silanol groups on the surface of the silica fine particles, and then hydrophobizing them again. However, since mechanical grinding is performed in a dry state, re-aggregation associated with grinding is unavoidable, and the effect of improving the degree of hydrophobicity was limited. In addition, the surface treatment had to be repeated, which was a process that consumed a lot of energy and time.

[0007] Furthermore, Japanese Patent Publication No. 2-189370 (Patent Document 2) describes a method for improving the surface treatment degree of silica fine particles by forming a reaction mixture consisting of gas-phase silica fine particles and a surface treatment agent into a paste and reacting it while applying mechanical stress. However, in this method, a strong aggregated state is formed through hydrogen crosslinking via the liquid, and mechanical stress from stirring alone is insufficient to break it down to the smallest constituent unit, the aggregate. Therefore, it was not satisfactory in terms of the degree of hydrophobic treatment.

[0008] JP 2000-256008 JP 2-189370

[0009] The present invention has been made in view of the above circumstances, and aims to provide hydrophobic vapor-phase silica fine particles and resin compositions that have a high degree of hydrophobicity treatment, suppress re-aggregation, and have an average particle size in methanol dispersion medium that is smaller than that of conventional methods.

[0010] The inventors of the present invention conducted diligent studies to achieve the above objective and found that hydrophobic vapor-phase silica fine particles satisfying all of the following conditions (1) to (3) have a high degree of hydrophobicity (surface carbon content), suppress re-aggregation, and have a small average particle size after dispersion, leading to the present invention. (1) BET specific surface area is 20 to 400 m² 2 (2) The volume-based median diameter (D50) in the methanol dispersion medium measured by laser diffraction. L The median diameter (D50) in the methanol dispersion medium is 200 nm or less, and measured by dynamic light scattering. D ) is 150 nm or less, and D50 L≧D50 D , (3) the degree of hydrophobicity determined by the methanol titration method is 70% or more.

[0011] Accordingly, the present invention provides the following hydrophobic fumed silica fine particles and resin composition. 1. Hydrophobic fumed silica fine particles characterized by satisfying all of the following conditions (1) to (3). (1) The BET specific surface area is 20 to 400 m 2 / g, (2) the volume-based median diameter (D50) in a methanol dispersion medium measured by a laser diffraction method L is 200 nm or less, and the volume-based median diameter (D50) in a methanol dispersion medium measured by a dynamic light scattering method D is 150 nm or less, and D50 L ≧D50 D , (3) the degree of hydrophobicity determined by the methanol titration method is 70% or more. 2. The hydrophobic fumed silica fine particles according to 1, wherein the loose bulk density measured by a powder tester is 200 g / L or more. 3. The hydrophobic fumed silica fine particles according to 1 or 2, characterized in that in a methanol dispersion with a hydrophobic fumed silica fine particle content of 1.5 mass%, which is prepared by irradiating 150 W ultrasonic waves for 3 minutes to disperse the hydrophobic fumed silica fine particles in methanol, the transmittance (optical path length 10 mm) at a wavelength of 700 nm measured using a spectrophotometer is 80% or more. 4. A resin composition comprising the hydrophobic fumed silica fine particles according to any one of 1 to 3 and a polymer that is liquid at 25°C. 5. The resin composition according to 4, wherein the liquid polymer is an organopolysiloxane or a perfluoropolyether group-containing compound.

[0012] The hydrophobic fumed silica fine particles of the present invention are uniformly treated down to the fine details of the surface of each individual silica fine particle, and reaggregation is suppressed, so that thickening after resin filling is extremely low. In particular, the affinity with nonpolar polymers such as organopolysiloxanes and perfluoropolyethers is extremely high, they can be kneaded with high dispersibility, and a resin composition excellent in transparency and mechanical properties can be obtained.

[0013] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.

[0014] -Hydrophobic vapor-phase silica nanoparticles- The hydrophobic vapor-phase silica nanoparticles of the present invention are characterized by satisfying all of the following conditions (1) to (3). (1) BET specific surface area is 20 to 400 m² 2 (2) The volume-based median diameter (D50) in the methanol dispersion medium measured by laser diffraction. L The median diameter (D50) in the methanol dispersion medium is 200 nm or less, and measured by dynamic light scattering. D ) is 150 nm or less, and D50 L ≥ D50 D (3) The degree of hydrophobicity obtained by methanol titration is 70% or higher.

[0015] The details are described below. [BET specific surface area] The hydrophobic vapor-phase silica fine particles of the present invention have a BET specific surface area of ​​20 to 400 m². 2 It is characterized by being / g. Preferably 50 to 300m 2 / g, more preferably 100 to 250m 2 It is / g. The BET specific surface area is 20m². 2 If the amount is less than 1 / g, the particle size is large, and the processing effect of the present invention cannot be fully realized, which is undesirable. The BET specific surface area is 400 m². 2 A value exceeding / g is undesirable because it indicates insufficient hydrophobicity treatment.

[0016] In this invention, the BET specific surface area is the value measured by the following method (the same applies to hydrophilic vapor-phase silica nanoparticles described later). <Measurement Method> The specific surface area of ​​the hydrophobic vapor-phase silica nanoparticles of this invention is measured by the BET single-point method based on the amount of nitrogen adsorbed. Specifically, a fully automatic BET specific surface area device Macsorb (Model-1201) manufactured by Mountec Co., Ltd. is used. A mixed gas (helium: 70 vol%, nitrogen: 30 vol%) is flowed at 0.15 MPa for 25 mL / min into a cell containing hydrophobic vapor-phase silica nanoparticles in the device, and the hydrophobic vapor-phase silica nanoparticles are degassed at 300°C for 20 minutes. Then, nitrogen is adsorbed onto the hydrophobic vapor-phase silica nanoparticles while the cell is cooled with liquid nitrogen. The specific surface area is calculated from the amount of nitrogen adsorbed per unit mass of the hydrophobic vapor-phase silica nanoparticles.

[0017] [Volume-based median diameter (D50) measured by laser diffraction method] L )] The hydrophobic vapor-phase silica fine particles of the present invention have a volume-based median diameter (D50) in a methanol dispersion medium measured by laser diffraction. L ) is characterized by being 200 nm or less. Preferably it is 150 nm or less, more preferably 148 nm or less, even more preferably 146 nm or less, and particularly preferably 50 to 130 nm. D50 L When the wavelength exceeds 200 nm, the dispersibility of hydrophobic vapor-phase silica nanoparticles into liquid polymers (especially non-polar polymers such as organopolysiloxanes and perfluoropolyethers) deteriorates, which is undesirable.

[0018] Furthermore, in the present invention, the volume-based median diameter (D50) in the methanol dispersion medium measured by the above laser diffraction method is also used. L The median diameter (D50) obtained here is the value measured by the following method (the same applies to hydrophilic vapor phase silica fine particles described later). L The particle size distribution, also known as the average particle diameter, is the 50% cumulative diameter based on the volume of the particles. That is, the cumulative curve is determined with the total volume of the particles set to 100%, and the particle diameter at the point where the cumulative volume reaches 50% is used. <Measurement Method> 1.5 g of the hydrophobic vapor-phase silica fine particles of the present invention are weighed, methanol is added to make a total of 100 g, and then the particles are dispersed by irradiating them with 150 W ultrasonic waves for 3 minutes. The particle size distribution based on volume is measured using a laser diffraction particle size distribution analyzer Mastersizer 3000+ (manufactured by Malvern).

[0019] [Volume-based median diameter (D50) measured by dynamic light scattering method] D )] The hydrophobic vapor-phase silica fine particles of the present invention have a volume-based median diameter (D50) in a methanol dispersion medium measured by dynamic light scattering. D ) is characterized by being 150 nm or less. Preferably it is 120 nm or less, and more preferably 30 to 100 nm. D50 DWhen the median diameter exceeds 150 nm, the dispersibility of hydrophobic vapor-phase silica nanoparticles into liquid polymers (especially non-polar polymers such as organopolysiloxanes and perfluoropolyethers) deteriorates, which is undesirable. The median diameter obtained here (D50 D The particle diameter (PDI), also known as the average particle diameter, is the 50% cumulative diameter based on the particle's volume. In other words, it represents the particle diameter at the point where the cumulative volume reaches 50% when the cumulative curve is calculated with the total volume of the particle set to 100%.

[0020] Furthermore, in the present invention, the volume-based median diameter (D50) in the methanol dispersion medium measured by the dynamic light scattering method is also used. D The values ​​are measured by the following method. <Measurement Method> 1.5 g of the hydrophobic vapor-phase silica fine particles of the present invention are weighed, methanol is added to make a total volume of 100 g, and then the particles are dispersed by irradiating them with 150 W ultrasonic waves for 3 minutes. The dispersion is diluted 100 times with methanol, and the volume-based particle size distribution is measured using a dynamic light scattering particle size analyzer, Zetasizer Ultra (manufactured by Malvern).

[0021] Between the volume-based median diameters in methanol dispersions measured by the two measurement methods described above, D50 L ≥ D50 D The fact that this relationship holds is also a feature of the present invention. D50 L ≥ D50 D This indicates that silica fine particles are sufficiently dispersed in the methanol dispersion medium, D50 L <D50 D This results in insufficient dispersion of silica fine particles in the methanol dispersion medium.

[0022] [Degree of Hydrophobicity] The hydrophobic vapor-phase silica fine particles of the present invention are characterized by having a degree of hydrophobicity of 70% or more as determined by methanol titration. Preferably it is 71% or more, more preferably 72% or more, and even more preferably 72-80%. A degree of hydrophobicity of less than 70% is undesirable because it impairs the dispersibility of the hydrophobic vapor-phase silica fine particles into liquid polymers (particularly nonpolar polymers such as organopolysiloxanes and perfluoropolyethers).

[0023] Furthermore, in this invention, the degree of hydrophobicity by methanol titration is the value measured by the following method (the same applies to hydrophilic vapor-phase silica nanoparticles described later). <Measurement Method> 0.2 g of the hydrophobic vapor-phase silica nanoparticles of this invention are weighed into a 200 mL beaker, 50 mL of pure water is added, and the mixture is stirred with a magnetic stirrer. Methanol is then added dropwise using a burette, and the endpoint is defined as the point when the suspended fine particle powder is completely dispersed in the liquid (i.e., when the entire amount of suspended fine particles has settled). The degree of hydrophobicity is calculated using the amount of methanol added at the endpoint from the following formula. Degree of hydrophobicity (%) = (Amount of methanol added × 100) / (50 + Amount of methanol added)

[0024] [Loose Bulk Density] The hydrophobic vapor-phase silica fine particles of the present invention preferably have a loose bulk density of 200 g / L or more, as measured by a powder tester. More preferably, it is 250 g / L or more, and even more preferably 300 g / L or more. There is no particular upper limit to the loose bulk density, but for example, it is 700 g / L or less. Within this range, it is preferable because it is easy to handle when filling into a composition.

[0025] In this invention, the loosened bulk density is the value measured by the following method (the same applies to hydrophilic vapor-phase silica fine particles described later). <Measurement Method> The loosened bulk density of the hydrophobic vapor-phase silica fine particles of this invention is measured as follows using a powder tester (model PT-X) manufactured by Hosokawa Micron Corporation. An appropriate amount of the sample to be measured is placed on a sieve and allowed to free-fall by sinusoidal vibration until the 0.1 L container overflows. After scraping off any excess powder on the cup with a blade, the container is removed and the loosened bulk density is obtained by dividing the mass of the filled powder by the volume of the container (0.1 L).

[0026] [Light transmittance of methanol dispersion] Furthermore, in a methanol dispersion containing 1.5% by mass of hydrophobic vapor-phase silica fine particles obtained by irradiating with 150 W ultrasound for 3 minutes, it is preferable that the transmittance at a wavelength of 700 nm (optical path length 10 mm) measured with a spectrophotometer is 80% or more. More preferably, the transmittance is 90% or more, and even more preferably 92% or more. Within this range, it is preferable because the hydrophobic vapor-phase silica fine particles do not aggregate and are uniformly dispersed in the liquid polymer (particularly non-polar polymers such as organopolysiloxanes and perfluoropolyethers).

[0027] Furthermore, in this invention, the light transmittance of the dispersion is a value measured by the following method. <Measurement Method> 1.5 g of the hydrophobic vapor-phase silica fine particles of this invention are weighed, methanol is added to make a total volume of 100 g, and then the particles are dispersed by irradiating them with 150 W ultrasonic waves for 3 minutes. An absorbance spectrophotometer DR3900 (manufactured by HACH) is used to measure the transmittance of the dispersion at a wavelength of 700 nm (optical path length 10 mm).

[0028] [Surface carbon content (carbon ratio)] Furthermore, it is preferable that the hydrophobic vapor-phase silica fine particles of the present invention have a surface carbon content (carbon ratio) of 3.5% by mass or more. If it is 3.5% by mass or more, it can be said that the surface of the silica fine particles has been sufficiently treated with the treatment agent and has sufficient hydrophobicity for dispersion in liquid polymers (especially nonpolar polymers such as organopolysiloxanes and perfluoropolyethers).

[0029] In the present invention, the surface carbon content (carbon percentage) is a value measured by the following method. <Measurement Method> The surface carbon content (carbon percentage) of hydrophobic vapor-phase silica fine particles of the present invention is measured as follows using a carbon-sulfur analyzer (tubular electric resistance heating furnace type, EMIA-Step manufactured by Horiba, Ltd.). Hydrophobic vapor-phase silica fine particles on a boat are burned at 1,350°C under an oxygen gas (purity 99.5% by volume or higher) airflow of 0.3 MPa, and the generated CO2 / CO is detected by an infrared detector. The carbon percentage of the hydrophobic vapor-phase silica fine particles is quantified based on calibration curves created using standard samples JSS057-10 (carbon percentage 0.58% by mass) and JSS102-9 (carbon percentage 4.59% by mass).

[0030] [Method for producing hydrophobic vapor-phase silica nanoparticles] The hydrophobic vapor-phase silica nanoparticles of the present invention are obtained by mixing hydrophilic vapor-phase silica nanoparticles, a surface treatment agent, a dispersion medium (liquid for kneading), and water added as needed, and then surface-treating them in a device to which physical shear force is applied.

[0031] The present invention relates to a method for producing hydrophobic vapor-phase silica fine particles, characterized by applying a physical shear force to a mixture of hydrophilic vapor-phase silica fine particles, a surface treatment agent, a dispersion medium, and water added as needed, within a predetermined apparatus to perform surface treatment (hydrophobicization treatment) on the hydrophilic vapor-phase silica fine particles. The present invention relates to a method for producing hydrophobic vapor-phase silica fine particles, which preferably includes a mixing step of mixing hydrophilic vapor-phase silica fine particles, a surface treatment agent, a dispersion medium, and water added as needed, and a surface treatment step of kneading the mixture obtained in the mixing step and performing surface treatment.

[0032] (Hydrophilic vapor-phase silica nanoparticles) In the method for producing hydrophobic vapor-phase silica nanoparticles of the present invention, the hydrophilic vapor-phase silica nanoparticles used as raw materials are produced by the combustion reaction of a silicon compound such as tetrachlorosilane, and obtained by the growth of primary particles (generation of secondary particles) in a flame and aggregation in a cooling zone. For example, vaporized tetrachlorosilane is mixed with hydrogen and air to a predetermined ratio, and this mixed gas is introduced into the mixing chamber of a burner and burned at a temperature of 1,000 to 3,000°C. The silica nanoparticles aggregated in the cooling zone are collected by known methods such as cyclones and bag filters after a dehydrochlorination process as needed.

[0033] Specific examples of silicon compounds used as raw materials for hydrophilic vapor-phase silica nanoparticles include halogenated silanes such as tetrachlorosilane, methyltrichlorosilane, dimethidyldichlorosilane, methyldichlorosilane, trichlorosilane, dimethylchlorosilane, and dichlorosilane; siloxane compounds such as hexamethyldisiloxane, octamethyltrisiloxane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and decamethylcyclopentasiloxane; and alkoxysilanes such as tetramethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, and dimethyldimethoxysilane.

[0034] The hydrolysis and combustion reactions of such silicon compounds in a flame are carried out by purifying them by distillation or other means as needed, then heating and evaporating them before supplying them, or by atomizing them using a spray nozzle and supplying them to the flame. In this case, flammable gases such as hydrogen, methane, or CNG may be used as auxiliary combustion gases.

[0035] Hydrophilic vapor-phase silica nanoparticles have a BET specific surface area of ​​40 to 400 m². 2 A concentration of / g is preferred, and more preferably 100 to 380 m 2 This value is / g. Within this range, re-aggregation after surface treatment, as described later, is suppressed, and hydrophobic vapor-phase silica fine particles with excellent dispersibility in liquid polymers (especially non-polar polymers such as organopolysiloxanes and perfluoropolyethers) can be obtained.

[0036] Furthermore, the volume-based median diameter (D50) measured by laser diffraction of hydrophilic vapor-phase silica nanoparticles L The wavelength is preferably 80 to 400 nm, and more preferably 100 to 200 nm.

[0037] The degree of hydrophobicity of hydrophilic vapor-phase silica nanoparticles obtained by methanol titration is not particularly limited, but is usually less than 50% due to their hydrophilic nature.

[0038] Hydrophilic vapor-phase silica fine particles preferably have a loosened bulk density of 20 to 100 g / L, and more preferably 40 to 80 g / L, as measured by a powder tester.

[0039] The hydrophilic vapor-phase silica fine particles used as raw materials may be used individually or in mixtures of two or more types. Furthermore, for the purpose of further increasing the degree of hydrophobicity, hydrophobic vapor-phase silica fine particles treated by known methods (i.e., those that do not satisfy all of the above conditions (1) to (3)) may be used as raw materials.

[0040] (Surface treatment agent) The surface treatment agent used in the hydrophobic vapor phase silica fine particle manufacturing method of the present invention is preferably a disilazane compound represented by the following general formula (1) and / or an organosilicon compound represented by the following general formula (2). (R 1 3Si)2NR 2 (1) (wherein, R 1 R is independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. 2 (This is a hydrogen atom or a methyl group.) 3 4-n Six n (2) (wherein, R 3 X is a monovalent hydrocarbon group having 1 to 20 carbon atoms, which may contain a heteroatom or a fluorine atom, and X is a halogen atom, -OH or -OR 4 (R 4 (where n is an alkyl group having 1 to 5 carbon atoms, and n is an integer from 1 to 4.)

[0041] In the above formula (1), R 1R is independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 5 carbon atoms, more preferably 1 or 2 carbon atoms. 1 Specific examples include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups; branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-pentyl, 3-pentyl, and tert-pentyl groups; saturated hydrocarbon groups such as cyclic alkyl groups such as cyclopropyl, cyclopentyl, cyclohexyl, and cyclooctyl groups; alkenyl groups such as vinyl, allyl, 1-propenyl, 1-methylpropenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, and octadecenyl groups; and aryl groups such as phenyl, tolyl, xylyl, and mesityl groups.

[0042] In the above equation (2), R 3 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 12, more preferably 1 to 10 carbon atoms, which may contain a heteroatom or a fluorine atom. 3 Specific examples include methyl group, ethyl group, propyl group, butyl group, pentyl group, hexyl group, octyl group, cyclohexyl group, decyl group, dodecyl group, hexadecyl group, octadecyl group, vinyl group, acrylic group, methacrylic group, 3-glycidyloxypropyl group, 3-aminopropyl group, 3-(2-aminoethylamino)-propyl group, phenyl group, 3,3,3-trifluoropropyl group, 1H,1H,2H,2H-nonafluorohexyl group, and the like.

[0043] In the above formula (2), X is a halogen atom, -OH, -OR 4 Group (R 4 R is an alkyl group having 1 to 5 carbon atoms. 4X is an alkyl group having 1 to 5 carbon atoms, and examples include linear alkyl groups such as methyl, ethyl, n-propyl, and n-butyl groups; branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-pentyl, 3-pentyl, and tert-pentyl groups; and cyclic alkyl groups such as cyclopropyl and cyclopentyl groups. For X, a chlorine atom, a hydroxyl group (-OH), a methoxy group, and an ethoxy group are preferred.

[0044] In the above formula (2), n is an integer from 1 to 4, preferably from 1 to 3.

[0045] Specific examples of the disilazane compound represented by formula (1) above include hexamethyldisilazane, 1,1,3,3-tetramethyldisilazane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, N-methyl-hexamethyldisilazane, N-ethyl-hexamethyldisilazane, 1,3-diphenyltetramethyldisilazane, and 1,3-dimethyl-1,1,3,3-tetraphenyldisilazane, with hexamethyldisilazane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, and 1,1,3,3-tetramethyldisilazane being particularly preferred.

[0046] Specific examples of organosilicon compounds represented by the above formula (2) include trimethylsilanol, chlorotrimethylsilane, trichloromethylsilane, dimethyldichlorosilane, tetrachlorosilane, dimethylethylchlorosilane, chlorotriethylsilane, ethyltrichlorosilane, chlorodimethylpropylsilane, trichloropropylsilane, dichloromethylpyrropyrsilane, dimethylisopropylchlorosilane, chlorodiethylisopropylsilane, chlorotriisopropylsilane, chlorohexyldimethylsilane, and trichlorohexylsilane. Halide alkylsilanes such as cyclohexyltrichlorosilane, dimethyl-n-octylchlorosilane, n-octyltrichlorosilane, chloro(decyl)dimethylsilane, decyltrichlorosilane, chlorododecyldimethylsilane, dodecyltrichlorosilane, trichlorohexadecylsilane, dimethyloctadecylchlorosilane, trichlorooctadecylsilane; trimethoxymethylsilane, dimethyldimethoxysilane, trimethylmethoxysilane, triethoxymethylsilane, ethyltrimethoxysilane, triethoxysilane Nethylsilane, Butyltrimethoxysilane, Butyltriethoxysilane, Hexyltrimethoxysilane, Hexyltriethoxysilane, Methoxydimethyl-n-octylsilane, Dimethoxymethyl-n-octylsilane, Trimethoxy-n-octylsilane, Triethoxy-n-octylsilane, Decyltrimethoxysilane, Decyltriethoxysilane, Dodecyltrimethoxysilane, Dodecyltriethoxysilane, Hexadecyltrimethoxysilane, Hexadecyltriethoxysilane, Methoxydimethyloctadecylsilane, Octadecyl Alkoxyalkylsilanes such as trimethoxysilane; olefinylsilanes such as chlorodimethylvinylsilane, trichlorovinylsilane, and vinyltrimethoxysilane; acroyloxyalkylsilanes such as 3-(methoxydimethylsilyl)-propyl acrylate, 3-(trimethoxysilyl)-propyl acrylate, and 3-(trimethoxysilyl)propyl methacrylate; glycidyloxyalkylsilanes such as 3-glycidyloxypropyltrimethoxysilane and 3-glycidyloxypropyl(dimethoxy)methylsilane;Examples include aminoalkylsilanes such as 3-aminopropyldimethoxysilane, 3-aminopropyltrimethoxysilane, and 3-(2-aminoethylamino)-propyltrimethoxysilane; arylsilanes such as chlorodimethylphenylsilane, phenyltrichlorosilane, dimethoxymethylphenylsilane, and trimethoxyphenylsilane; and fluoroalkylsilanes such as (3,3,3-trifluoropropyl)-methyldichlorosilane, trimethoxy(3,3,3-trifluoropropyl)silane, and trimethoxy(1H,1H,2H,2H-nonafluorohexyl)silane. Among these, trimethylsilanol, chlorotrimethylsilane, dimethyldichlorosilane, methyltrichlorosilane, trimethylmethoxysilane, and dimethyldimethoxysilane are particularly preferred.

[0047] The amount of surface treatment agent to be added varies depending on the BET specific surface area of ​​the hydrophilic vapor-phase silica fine particles used as raw material. It is preferable to calculate the amount of surface treatment agent to be added per 100 parts by mass of hydrophilic vapor-phase silica fine particles using the following formula: Amount of surface treatment agent added (parts by mass) = BET specific surface area of ​​vapor-phase silica fine particles (m²) 2 ( / g) / A In the above calculation formula, A is preferably 3 to 30, more preferably 3 to 25, and even more preferably 3 to 20. When hydrophobic vapor-phase silica fine particles are used as a raw material, A in the above calculation formula is preferably 2 to 30, more preferably 2.5 to 25, and even more preferably 2.8 to 20.

[0048] When adding both the disilazane compound represented by general formula (1) and the organosilicon compound represented by general formula (2), it is preferable that the blending ratio of the disilazane compound represented by general formula (1) to the organosilicon compound represented by general formula (2) (disilazane compound represented by general formula (1):organosilicon compound represented by general formula (2)) be 1:1 to 1:20, and more preferably 1:2 to 1:5.

[0049] (Dispersion medium) The dispersion medium (liquid for kneading) used in the hydrophobic vapor phase silica fine particle manufacturing method of the present invention may be a general organic solvent, or the surface treatment agent itself may be used as the dispersion medium.

[0050] Suitable organic solvents include hydrocarbon solvents such as pentane, hexane, cyclohexane, heptane, isooctane, toluene, xylene, and mesitylene; alcohol solvents such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol; siloxane solvents such as hexamethyldisiloxane and octamethylcyclotetrasiloxane; ether solvents such as diethyl ether, tetrahydrofuran, dioxane, and dimethoxyethane; and aprotic polar solvents such as ethyl acetate, acetonitrile, propionitrile, N,N-dimethylformamide, and N-methylpyrrolidone. Among these, ethanol, hexamethyldisiloxane, and octamethylcyclotetrasiloxane are particularly preferred.

[0051] Furthermore, when the surface treatment agent is used as a dispersion medium, examples include disilazane compounds such as hexamethyldisilazane, 1,1,3,3-tetramethyldisilazane, and 1,3-divinyl-1,1,3,3-tetramethyldisilazane, and organosilicon compounds such as trimethylsilanol. Among these, hexamethyldisilazane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, and trimethylsilanol are particularly preferred.

[0052] These dispersion media may be used individually or in combination of two or more types.

[0053] The amount of dispersion medium used is 25 to 1,000 parts by mass, more preferably 40 to 600 parts by mass, and even more preferably 60 to 200 parts by mass, per 100 parts by mass of hydrophilic vapor-phase silica fine particles of the raw material. When hydrophobic vapor-phase silica fine particles are used as the raw material, the amount of dispersion medium is preferably 60 to 200 parts by mass, more preferably 40 to 600 parts by mass, and even more preferably 60 to 200 parts by mass, per 100 parts by mass of hydrophobic vapor-phase silica fine particles of the raw material.

[0054] Furthermore, when the surface treatment agent itself is used as a dispersion medium, the amount of the surface treatment agent used should be such that the total amount of the surface treatment agent added and the amount used as a dispersion medium falls within the range of the amount of the dispersion medium used.

[0055] (Water) Furthermore, when producing the silica fine particles of the present invention, it is preferable to add water to promote the hydrolysis of the surface treatment agent and increase its reactivity. The amount of water used is preferably 1 to 30 parts by mass, more preferably 3 to 20 parts by mass, and even more preferably 5 to 10 parts by mass, per 100 parts by mass of hydrophilic vapor-phase silica fine particles of the raw material. When hydrophobic vapor-phase silica fine particles are used as the raw material, the amount of water used is preferably 1 to 30 parts by mass, more preferably 2 to 20 parts by mass, and even more preferably 2.5 to 10 parts by mass, per 100 parts by mass of hydrophobic vapor-phase silica fine particles of the raw material.

[0056] By applying physical shear force to a mixture of these raw materials and surface-treating it through kneading or other methods, the surface treatment agent penetrates even to the finest silica microparticles, resulting in silica microparticles with a high degree of hydrophobicity.

[0057] Specific examples of equipment used include single-screw extruders, twin-screw extruders, kneaders, stirring and grinding machines, Banbury mixers, open rolls, internal mixers, ultrasonic reactors, and bead mills. Among these, single-screw extruders, twin-screw extruders, kneaders, and Banbury mixers are particularly preferred, with kneaders and Banbury mixers being more preferred.

[0058] From a safety standpoint, the above surface treatment process is preferably carried out under an inert gas atmosphere such as nitrogen or argon.

[0059] Furthermore, it is preferable to pre-mix the above raw material mixture before the surface treatment step (mixing step). Examples of mixing equipment include Henschel mixers, intensive mixers, Lödige mixers, V-type blenders, Ribocorn mixers, and Nauter mixers.

[0060] In the manufacturing method of the present invention, the mixture of raw materials is preferably in a wet powder state in which at least a portion of the surface of the hydrophilic vapor-phase silica fine particles is thinly covered with liquid (surface treatment agent, solvent, and water added as needed) and the silica fine particles are in contact with each other, rather than in a slurry state in which the solid hydrophilic vapor-phase silica fine particles are dispersed in a liquid (surface treatment agent, solvent, and water added as needed) and are in a discontinuous state.

[0061] The hydrophobic vapor-phase silica fine particles of the present invention, i.e., (1) having a BET specific surface area of ​​20 to 400 m² 2 (2) The volume-based median diameter (D50) in the methanol dispersion medium measured by laser diffraction. L The median diameter (D50) in the methanol dispersion medium is 200 nm or less, and measured by dynamic light scattering. D ) is 150 nm or less, and D50 L ≥ D50 D In order to obtain hydrophobic vapor-phase silica fine particles that satisfy all of the following conditions, (3) the degree of hydrophobicity by methanol titration is 70% or more, it is important to perform surface treatment in the above manufacturing method using an apparatus that kneads the mixture of raw materials while applying physical shear force using friction and compressive stress. The temperature for this surface treatment may be room temperature (20 ± 15°C).

[0062] Furthermore, in the manufacturing method of the present invention, it is preferable to perform a heat treatment after the surface treatment step described above. The heat treatment temperature is not particularly limited, but from the viewpoint of reactivity and removal of by-products, it is preferably 60 to 500°C, more preferably 80 to 300°C, and even more preferably 100 to 200°C. The reaction time is not particularly limited, but is preferably 0.1 to 20 hours, more preferably 0.5 to 10 hours, and even more preferably 1 to 5 hours.

[0063] The resin composition of the present invention is characterized by containing the hydrophobic vapor-phase silica fine particles of the present invention described above and a polymer that is liquid at 25°C. Here, it is preferable that the liquid polymer is an organopolysiloxane or a perfluoropolyether group-containing compound. The hydrophobic vapor-phase silica fine particles of the present invention are uniformly processed down to the finest details of the silica particles, and re-aggregation is suppressed, so when added to a resin composition, the increase in viscosity after addition is extremely small. Furthermore, if the hydrophobic vapor-phase silica fine particles of the present invention are kneaded with a polymer to form a resin composition, a highly transparent and low-viscosity resin composition can be obtained, and effects such as increased filling capacity and improved mechanical strength can also be obtained. In particular, they have extremely high affinity with non-polar polymers such as organopolysiloxanes and perfluoropolyethers, and can be kneaded with high dispersibility, making it possible to obtain a resin composition with excellent transparency and mechanical properties.

[0064] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. Furthermore, in the following examples, the BET specific surface area of ​​hydrophilic or hydrophobic vapor-phase silica fine particles, the average particle size in the methanol dispersion medium measured by laser diffraction and dynamic light scattering, the degree of hydrophobicity, loose bulk density, surface carbon content (carbon content), and dispersion permeability were measured by the following methods.

[0065] <BET Specific Surface Area> The specific surface area of ​​hydrophilic vapor-phase silica nanoparticles used as raw materials and the obtained hydrophobic vapor-phase silica nanoparticles was measured using the BET single-point method based on nitrogen adsorption amount with a fully automatic BET specific surface area instrument, Macsorb (Model-1201), manufactured by Mountec Co., Ltd. Hydrophilic or hydrophobic vapor-phase silica nanoparticles were sealed in a cell in the instrument, and a mixed gas (helium: 70 vol%, nitrogen: 30 vol%) was flowed at 0.15 MPa at 25 mL / min while the hydrophobic vapor-phase silica nanoparticles were degassed at 300°C for 20 minutes. Then, nitrogen was adsorbed onto the hydrophilic or hydrophobic vapor-phase silica nanoparticles while the cell was cooled with liquid nitrogen. The specific surface area was calculated from the amount of nitrogen adsorbed per unit mass of the hydrophilic or hydrophobic vapor-phase silica nanoparticles.

[0066] <Average particle size in methanol dispersion medium measured by laser diffraction (D50L > 1.5 g of hydrophilic vapor-phase silica fine particles used as raw materials and the obtained hydrophobic vapor-phase silica fine particles were weighed, methanol was added to make a total volume of 100 g, and then the particles were dispersed by irradiating with 150 W ultrasonic waves for 3 minutes. The obtained dispersion was measured using a laser diffraction particle size distribution analyzer Mastersizer 3000+ (Malvern), and the volume-based particle size distribution was measured to determine the average particle size (D50). L The average particle size (D50) obtained here was calculated. L This represents the 50% cumulative diameter of the particle based on its volume. In other words, it is the particle diameter (volume-based median diameter) at the point where the cumulative volume reaches 50% when the cumulative curve is calculated with the total volume of the particle set to 100%.

[0067] <Average particle size in methanol dispersion medium measured by dynamic light scattering (D50 D > 1.5 g of the obtained hydrophobic vapor-phase silica fine particles were weighed, methanol was added to make a total volume of 100 g, and then the particles were dispersed by irradiating them with 150 W ultrasonic waves for 3 minutes. The obtained dispersion was diluted 100 times with methanol, and the volume-based particle size distribution was measured using a dynamic light scattering particle size analyzer, Zetasizer Ultra (Malvern), to determine the average particle size (D50). D The average particle size (D50) obtained here was calculated. D This represents the 50% cumulative diameter of the particle based on its volume. In other words, it is the particle diameter (volume-based median diameter) at the point where the cumulative volume reaches 50% when the cumulative curve is calculated with the total volume of the particle set to 100%.

[0068] <Hydrophobicity> The hydrophobicity of the hydrophilic vapor-phase silica fine particles used as raw materials and the obtained hydrophobic vapor-phase silica fine particles was measured as follows. 0.2 g of fine particle powder was weighed into a 200 mL beaker, 50 mL of pure water was added, and the mixture was stirred with a magnetic stirrer. Methanol was then added dropwise using a burette, and the endpoint was defined as the point when the suspended fine particle powder was completely dispersed in the liquid (i.e., when the entire amount of suspended fine particles had settled). The hydrophobicity was calculated from the amount of methanol added at the endpoint. Hydrophobicity (%) = (Amount of methanol added × 100) / (50 + Amount of methanol added) Note that a hydrophobicity of 0% means that when 0.2 g of fine particle powder was weighed into a 200 mL beaker, 50 mL of pure water was added, and the mixture was stirred with a magnetic stirrer, the fine particle powder was completely dispersed in the liquid.

[0069] <Loose Bulk Density> The loose bulk density of the hydrophilic vapor-phase silica fine particles used as raw materials and the obtained hydrophobic vapor-phase silica fine particles was measured using a powder tester (Hosokawa Micron Corporation, model PT-X) as follows. An appropriate amount of the sample was placed on a sieve and allowed to free-fall using sinusoidal vibration until the 0.1 L container overflowed. After scraping off the excess powder on the cup with a blade, the container was removed, and the loose bulk density was defined as the mass of the filled powder divided by the volume of the container (0.1 L).

[0070] <Surface Carbon Content> The surface carbon content of the obtained hydrophobic vapor-phase silica nanoparticles was measured using a carbon-sulfur analyzer (tubular electric resistance heating furnace type, EMIA-Step manufactured by Horiba, Ltd.). Hydrophobic vapor-phase silica nanoparticles on a boat were burned at 1,350°C under an oxygen gas (purity 99.5% by volume or higher) airflow of 0.3 MPa, and the generated CO2 / CO was detected with an infrared detector. Calibration curves were created using JSS057-10 (carbon content 0.58 mass%) and JSS102-9 (carbon content 4.59 mass%) as standard samples, and the carbon content of the hydrophobic vapor-phase silica nanoparticles was quantified.

[0071] <Measurement of Dispersion Transmittance> 1.5 g of the obtained hydrophobic vapor-phase silica fine particles was weighed, methanol was added to make a total volume of 100 g, and then the particles were dispersed by irradiating them with 150 W ultrasonic waves for 3 minutes. The transmittance of the dispersion at a wavelength of 700 nm (optical path length 10 mm) was measured using a spectrophotometer DR3900 (HACH).

[0072] [Example 1] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L Three kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.6 kg of hexamethyldisilazane, 2 kg of trimethylsilanol, and 0.27 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a kneader (manufactured by Satake Chemical Machinery Industry Co., Ltd., the same applies hereafter), and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 2.8 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0073] [Example 2] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L Two kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.4 kg of 1,3-divinyl-1,1,3,3-tetramethyldisilazane, 1.3 kg of trimethylsilanol, and 0.18 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a kneader, and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 1.2 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0074] [Example 3] A 150L mixing and stirring machine was used with a BET specific surface area of ​​240 m². 2 / g, D50 measured by laser diffraction method L4 kg of hydrophobic vapor-phase silica nanoparticles (Evonik, product name: Aerosil R976S) with a wavelength of 288 nm, a degree of hydrophobicity of 42%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.2 kg of hexamethyldisilazane, 3.2 kg of trimethylsilanol, and 0.1 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a kneader, and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 2.8 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0075] [Example 4] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L Two kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 1.7 kg of hexamethyldisilazane and 0.18 kg of water were added while stirring, and the mixture was stirred for a further 10 minutes. The resulting wet powder was kneaded in a twin-screw kneading extruder (manufactured by Toshiba Machine Co., Ltd. (now Shibaura Machine Co., Ltd.), model: TEM-50, the same applies hereafter), and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 1.3 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0076] [Example 5] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L Two kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.4 kg of hexamethyldisilazane, 1.3 kg of hexamethyldisiloxane, and 0.18 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a twin-screw extruder, and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 1.7 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0077] [Example 6] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method LTwo kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.4 kg of hexamethyldisilazane, 1.3 kg of octamethylcyclotetrasiloxane, and 0.18 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a twin-screw extruder, and the discharged solid was dried in a vacuum dryer under a nitrogen stream at 180°C / 75 kPa for 4 hours. By cooling this, 1.4 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0078] [Example 7] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L Two kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.6 kg of hexamethyldisilazane, 0.9 kg of trimethylsilanol, and 0.18 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a Banbury mixer (Kobe Steel, Ltd., model: MIXTRON BB-16, the same applies hereafter), and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 1.7 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0079] [Example 8] A 150L mixing and stirring machine was used to mix a BET with a specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L Two kilograms of hydrophilic vapor-phase silica nanoparticles with a wavelength of 314 nm, a degree of hydrophobicity of 0%, and a loose bulk density of 50 g / L were added. After replacing the mixing and stirring chamber with nitrogen, 0.6 kg of hexamethyldisilazane, 2.0 kg of trimethylsilanol, and 0.18 kg of water were added while stirring, and the mixture was stirred for another 10 minutes. The resulting wet powder was kneaded in a Banbury mixer, and the discharged solid was dried in a vibrating dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 1.8 kg of hydrophobic vapor-phase silica nanoparticles were obtained.

[0080] [Example 9] A 150L mixing and stirring machine was used with a BET specific surface area of ​​300 m². 2 / g, D50 measured by laser diffraction method L2 kg of hydrophilic fumed silica fine particles with a value of 314 nm, a hydrophobicity of 0%, and a loose bulk density of 50 g / L were charged. After the inside of the mixing stirrer was purged with nitrogen, 0.6 kg of hexamethyldisilazane, 1.3 kg of ethanol, and 0.18 kg of water were added while stirring, and the mixture was further stirred for 10 minutes. The obtained wet powder was kneaded with a Banbury mixer, and the discharged solid was dried with a vibratory dryer at 140°C for 3 hours under a nitrogen stream. By cooling this, 1.6 kg of hydrophobic fumed silica fine particles were obtained.

[0081] [Comparative Example 1] 200 g of hydrophilic fumed silica fine particles having a BET specific surface area of 300 m 2 / g and a D50 measured by a laser diffraction method of L 150 nm, a hydrophobicity of 0%, and a loose bulk density of 50 g / L were charged into a 10 L mixing stirrer equipped with a stirrer, a spraying device, a thermometer, and a reaction apparatus. After the air in the reaction apparatus was replaced with nitrogen, 14.8 g of water and 75.6 g of hexamethyldisilazane were sequentially sprayed while stirring. After reacting at 90°C for 1 hour, the mixture was dried at 150°C for 2 hours under a nitrogen stream. By cooling this, 188 g of hydrophobic fumed silica fine particles were obtained.

[0082] [Comparative Example 2] Into a fluidized tank having an internal volume of 1.2 m 3 , 3 kg of hydrophilic fumed silica fine particles having a BET specific surface area of 300 m 2 / g and a D50 measured by a laser diffraction method of L 150 nm, a hydrophobicity of 0%, and a loose bulk density of 50 g / L were charged. In the fluidized tank, surface treatment was performed for 0.5 hours under the conditions of nitrogen at 9.2 Nm 3 / hr, dimethyldichlorosilane at 2.9 kg / hr, a steam amount of 3.9 kg / hr, and a temperature of 500°C. After cooling, 2.8 kg of hydrophobic fumed silica fine particles were recovered.

[0083] [Comparative Example 3] The above items were measured using a commercially available hydrophobic fumed silica fine particle (trade name: AEROSIL RY200, manufactured by Nippon Aerosil Co., Ltd.).

[0084] The results of measurements performed on the above hydrophobic fumed silica fine particles are shown in Table 1.

[0085]

[0086] As shown in Table 1, the hydrophobic vapor-phase silica nanoparticles obtained in Examples 1 to 9 exhibit a higher degree of hydrophobicity and surface treatment compared to Comparative Examples 1 to 3. Furthermore, the average particle size (D50) in the methanol dispersion medium of Examples 1 to 9 is smaller than that of the hydrophobic vapor-phase silica nanoparticles of Comparative Examples 1 to 3, as measured by both laser diffraction and dynamic light scattering. Examples 1 to 9 also have a higher bulk density and significantly higher transmittance of the methanol dispersion than Comparative Examples 1 to 3.

Claims

1. Hydrophobic vapor-phase silica fine particles characterized by satisfying all of the following conditions (1) to (3): (1) BET specific surface area of ​​20 to 400 m² 2 (2) The volume-based median diameter (D50) in the methanol dispersion medium measured by laser diffraction. L The median diameter (D50) in the methanol dispersion medium is 200 nm or less, and measured by dynamic light scattering. D ) is 150 nm or less, and D50 L ≥ D50 D (3) The degree of hydrophobicity obtained by methanol titration is 70% or higher.

2. Furthermore, the hydrophobic vapor-phase silica fine particles according to claim 1, wherein the loosened bulk density measured by a powder tester is 200 g / L or more.

3. The hydrophobic vapor-phase silica nanoparticles according to claim 1, characterized in that, in a methanol dispersion containing 1.5% by mass of hydrophobic vapor-phase silica nanoparticles, obtained by irradiating the hydrophobic vapor-phase silica nanoparticles in methanol by 150 W ultrasound for 3 minutes, the transmittance at a wavelength of 700 nm (optical path length 10 mm) measured with a spectrophotometer is 80% or more.

4. A resin composition characterized by containing hydrophobic vapor-phase silica fine particles according to any one of claims 1 to 3 and a polymer that is liquid at 25°C.

5. The resin composition according to claim 4, wherein the liquid polymer is an organopolysiloxane or a perfluoropolyether group-containing compound.