Iron-based powder for producing iron sulfate and method for producing iron sulfate

By using an iron-based powder with controlled carbon, oxygen, and silicon contents, along with specific crystallinity, the odor issue in producing iron sulfate is mitigated, enhancing production efficiency and yield.

WO2026235012A1PCT designated stage Publication Date: 2026-11-12JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016370
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-23
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for producing iron sulfate from iron-based powder in sulfuric acid generate odors due to the formation of dimethyl sulfide, affecting efficiency and yield.

Method used

An iron-based powder with specific component compositions of C: 0.08% or less, O: 0.4% to 5.0%, and optionally Si: 0.01% to 0.50%, along with controlled full width at half maximum of the (110) plane of α-Fe, is used to suppress odor and enhance production efficiency.

Benefits of technology

The solution effectively reduces odor generation and improves the yield of iron sulfate by stabilizing the reaction rate and preventing excessive formation of iron oxide, ensuring efficient dissolution in sulfuric acid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provide is iron-based powder for producing iron sulfate, enabling suppression of odor generated during sulfuric acid dissolution and enabling efficient production of iron sulfate. The iron-based powder for producing iron sulfate has a component composition containing 0.08 mass% or less of C and 0.4-5.0 mass% of O.
Need to check novelty before this filing date? Find Prior Art

Description

Iron-based powder for manufacturing iron sulfate and method for producing iron sulfate

[0001] The present invention relates to an iron-based powder for manufacturing iron sulfate and a method for producing iron sulfate.

[0002] Iron sulfate is used in flocculants for wastewater treatment, rust inhibitors, soil conditioners, pigments, magnetic materials, reducing agents, disinfectants, preservatives and the like. In recent years, it has also attracted attention as a raw material for lithium iron phosphate, which is one of the positive electrode active materials for lithium ion batteries.

[0003] Main methods for producing iron sulfate include (1) a method utilizing a by-product from titanium oxide production, (2) a method of recovering from waste acid solution generated in the thin plate pickling process at steelworks, and (3) a method of reacting iron-based powder with sulfuric acid. As an example of (3), Patent Document 1 discloses that in the production of iron oxide powder, iron sulfate is obtained by sulfating the surface of iron particles and then peeling the sulfated layer from the base iron.

[0004] Japanese Unexamined Patent Publication No. 1-308835

[0005] In relation to the above (3), efficient production of iron sulfate by dissolving iron-based powder in sulfuric acid has been studied. However, when iron-based powder is dissolved in sulfuric acid, there was a problem that an odor containing dimethyl sulfide (rational formula: CH 3 SCH 3 ) as the main component is generated.

[0006] The present invention has been made in view of the above circumstances, and an object thereof is to provide an iron-based powder for manufacturing iron sulfate, which can suppress odor during dissolution in sulfuric acid and can efficiently produce iron sulfate.

[0007] The present invention has been made to solve the above problems, and the gist thereof is as follows.

[0008] 1. An iron-based powder for manufacturing iron sulfate, having a component composition of C: 0.08 mass% or less and O: 0.4 mass% or more and 5.0 mass% or less.

[0009] 2. The iron-based powder for manufacturing iron sulfate according to the above 1, wherein in the component composition, Si is 0.01 mass% or more and 0.50 mass% or less.

[0010] 3. The iron-based powder for producing iron sulfate according to claim 1 or 2, wherein the full width at half maximum of the peak of the (110) plane of α-Fe obtained by powder X-ray diffraction using Cu-Kα rays as an X-ray source is 0.10° or more and 0.40° or less.

[0011] 4. A method for producing iron sulfate, comprising dissolving the iron-based powder described in any of items 1 to 3 above in sulfuric acid.

[0012] According to the present invention, it is possible to provide an iron-based powder for producing iron sulfate that can suppress the odor during sulfuric acid dissolution and efficiently produce iron sulfate.

[0013] The present invention will be described in detail below. The following description illustrates preferred embodiments of the present invention, and the invention is not limited thereto. Unless otherwise specified, "%" as a unit of content refers to "mass%".

[0014] [Iron-based powder] First, an iron-based powder for producing iron sulfate according to one embodiment of the present invention will be described.

[0015] The iron-based powder can be any iron-based powder without any particular limitations. Here, "iron-based" refers to a powder containing 50% or more Fe. Examples of the iron-based powder include iron powder and iron-based alloy powder. Iron powder refers to a powder consisting of Fe and unavoidable impurities, and is generally referred to as "pure iron powder" in this art. As for the iron-based alloy powder, any powder can be used, such as pre-alloyed steel powder, partially-diffused alloyed steel powder, and hybrid steel powder. Pre-alloyed steel powder refers to an iron-based alloy powder in which alloying elements have been pre-alloyed during the melting process, and is also called fully alloyed steel powder. Partially-diffused alloyed steel powder refers to a powder in which alloying elements have been partially diffused into iron powder. Hybrid steel powder refers to a powder in which alloying elements have been further partially diffused into pre-alloyed steel powder. As for the alloying elements of the iron-based alloy powder, for example, one or more selected from the group consisting of C, Cu, Ni, Mo, Mn, Cr, V, S, P, Ca, Al, and Si can be used. However, using iron-based alloy powder incurs the cost of adding alloying elements, so it is preferable to use iron powder. Furthermore, when using alloying elements, it is preferable to use iron-based powder that does not generate sulfates other than iron sulfate during sulfuric acid dissolution in order to simplify the process of removing sulfates other than iron sulfate in the production of iron sulfate. Specifically, it is preferable to use iron powder or iron-based alloy powder using one or both of C and Si as alloying elements.

[0016] (Component Composition) As a result of diligent research, the inventors discovered that carbon in the iron-based powder reacts with sulfuric acid to produce dimethyl sulfide. Further investigation revealed that by setting the component composition of the iron-based powder to C: 0.08% or less and O: 0.4% to 5.0%, the odor during sulfuric acid dissolution can be suppressed. The individual components are described below.

[0017] C: 0.08% or less. C reacts with sulfuric acid to produce dimethyl sulfide, which significantly affects the generation of odor during iron sulfate production. If the C content exceeds 0.08%, the odor generated during sulfuric acid dissolution cannot be sufficiently suppressed. Therefore, the C content should be 0.08% or less, preferably 0.05% or less, more preferably 0.03% or less, and even more preferably 0.01% or less. The lower limit of the C content is not particularly limited and may be 0%, or C may not be present at all.

[0018] When carbon (C) is present in iron-based powder, it may exist in a solid solution state or as a carbide depending on the C content and thermal history, but the state of C is not particularly limited in the present invention.

[0019] O: 0.4% to 5.0% O is an element that controls the reaction rate in the reaction between iron-based powder and sulfuric acid. If the amount of O is low, the reaction between iron-based powder and sulfuric acid becomes significantly faster. As a result, the heat of the reaction causes the iron-based powder to react with the oxygen present in the sulfuric acid to produce iron oxide, which reduces the yield of iron sulfate. Therefore, the O content should be 0.4% or more, preferably 0.5% or more. On the other hand, if there is an excess of O, the reaction will be significantly slowed down by the iron oxide contained in the iron-based powder, which will reduce the yield of iron sulfate. Therefore, the O content should be 5.0% or less, preferably 2.5% or less, and more preferably 0.8% or less.

[0020] In the above component composition, components other than C and O are not particularly limited. The remainder of the component composition may consist of Fe and other unavoidable impurities. In other words, the component composition of the iron-based powder may be C: 0.08% or less and O: 0.4% to 5.0%, with the remainder consisting of Fe and other unavoidable impurities. Furthermore, the component composition may optionally include the following components. The following components may be included as alloying elements or unavoidable impurities.

[0021] (Si content) Si may be present as an unavoidable impurity in iron-based powder, and it is an element that can be used to adjust the oxygen content. If the Si content exceeds 0.50%, the yield of iron sulfate when used in the production of iron sulfate may decrease. For this reason, when Si is included, it is preferable to keep the Si content at 0.50% or less, and more preferably at 0.10% or less. On the other hand, excessive reduction leads to an increase in the time required for Si removal treatment and a corresponding increase in manufacturing costs. For this reason, when Si is included, it is preferable to keep the Si content at 0.01% or more. Furthermore, by adding Si to the production of iron-based powder, the oxygen content can be adjusted without increasing the carbon content. Moreover, by adding Si, the reaction rate during sulfuric acid dissolution can be stabilized, and runaway reactions and local oxidation reactions can be further suppressed. From the viewpoint of obtaining these effects by adding Si, it is more preferable to keep the Si content at 0.03% or more, and even more preferable to keep it at 0.05% or more. Si in the iron-based powder may be pre-alloyed, specifically in a solid solution state or as an Fe-Si alloy.

[0022] In one embodiment, the iron-based powder for producing iron sulfate has a component composition of C: 0.08% or less, O: 0.4% to 5.0%, and Si: 0.01% to 0.50%, with the remainder being Fe and other unavoidable impurities.

[0023] (Full width at half maximum of the peak of the (110) plane of α-Fe) When the full width at half maximum of the peak of the (110) plane of α-Fe is wide, the crystallinity of α-Fe is low, which prevents the excessive formation of iron oxide due to the reaction between the iron-based powder and the oxygen present in the sulfuric acid when dissolved in sulfuric acid. Therefore, in order to further increase the yield of iron sulfate, it is preferable that the full width at half maximum be 0.10° or higher. On the other hand, if the full width at half maximum is excessively wide, the reaction between the iron-based powder and sulfuric acid will be significantly slower, which may reduce the yield of iron sulfate. Therefore, in order to further increase the yield of iron sulfate, it is preferable that the full width at half maximum be 0.40° or lower.

[0024] The above half-width is obtained by powder X-ray diffraction using Cu-Kα rays as the X-ray source. Specifically, the measurement is performed using an X-ray diffractometer (SmartLab manufactured by Rigaku Corporation) under the following measurement conditions: Source: Cu-Kα (wavelength 1.5418 Å) Tube voltage: 40 kV Tube current: 30 mA Scanning speed: 4° / min Scanning range: 30° to 60° The half-width of the (110) plane of α-Fe is calculated from the X-ray diffraction pattern obtained under the above conditions.

[0025] The average particle size (D50) of the iron-based powder is not particularly limited and can be any value. However, it is preferable to set the average particle size to 30 μm or more in order to improve workability by improving the fluidity of the iron-based powder. Furthermore, it is preferable to set the average particle size to 150 μm or less in order to further enhance the reactivity when the iron-based powder is dissolved in sulfuric acid. The average particle size can be determined by calculating the mass-based cumulative particle size distribution from the particle size distribution measured by the dry sieving method described in JIS Z 2510, and then interpolating the particle size at which this value becomes 50%.

[0026] The apparent density of the iron-based powder is not particularly limited and can be any value. However, in order to improve workability by improving the fluidity of the iron-based powder, the apparent density is set to 2.3 Mg / m³. 3 It is preferable to keep the above. Furthermore, in order to further enhance the reactivity when the iron-based powder is dissolved in sulfuric acid, the apparent density should be 3.6 Mg / m³. 3 The following is preferable. The apparent density can be measured by the method specified in JIS Z 2504.

[0027] The iron-based powder can be manufactured by any method. For example, the iron-based powder may be reduced iron-based powder, atomized iron-based powder, or a mixture thereof. Reduced iron-based powder is iron-based powder manufactured by reducing iron oxide. As iron oxide, for example, hematite iron ore, magnetite iron ore, mill scale, etc., can be used. Atomized iron-based powder is iron-based powder manufactured by the atomization method. It is preferable that the iron-based powder is atomized iron-based powder. By using the atomization method, it is relatively easy to control the C content, O content and the above-mentioned full width at half maximum by adjusting the molten steel components and atomization conditions. Furthermore, while the properties of the reduction method tend to depend on the properties of the raw material iron oxide, the atomization method is more likely to suppress variations in the product powder compared to the reduction method. The atomized iron-based powder may be either gas-atomized iron-based powder or water-atomized iron-based powder. Furthermore, it is preferable that the reduced iron-based powder or atomized iron-based powder is subjected to a treatment in which carbon and oxygen are reduced by heating in a reducing atmosphere (e.g., a hydrogen atmosphere). However, as the reduced iron-based powder or atomized iron-based powder, iron-based powder in its as-reduced or as-atomized state without such heat treatment can also be used.

[0028] The method for adjusting the carbon content, oxygen content, and full width at half maximum of the iron-based powder is not particularly limited, and any method can be used.

[0029] For example, to adjust the carbon and oxygen content of atomized iron-based powder, the composition of the molten steel used in its production can be adjusted. The composition of the molten steel can be adjusted by modifying the refining conditions and other steelmaking conditions. Refining can be carried out using a general converter.

[0030] From the standpoint of adjusting the viscosity, melting point, and preventing oxidation of molten steel, carbon is usually added to the molten steel used in the atomization process. In order to reduce the carbon content in atomized iron-based powder, in addition to adjusting the manufacturing conditions as described above, it is also possible to reduce the amount of carbon added to the molten steel. However, when the amount of carbon added to the molten steel is reduced, productivity decreases as the viscosity of the molten steel increases, and this decrease in productivity leads to blockage of the molten steel during atomization, increasing the oxygen content in the iron-based powder. Therefore, when reducing the amount of carbon added to the molten steel, elements selected from S, P, Si, Mn, Ca, Al, etc. should be added to suppress the increase in viscosity and oxidation of the molten steel.

[0031] To adjust the above-mentioned full width at half maximum (FWHM) in atomized iron-based powder, methods such as adjusting the refining conditions and other steelmaking conditions, or adjusting the elements added to the molten steel, can be used. Furthermore, the FWHM and the oxygen content of the atomized iron-based powder can be adjusted by adjusting the conditions of the atomization process. Adjustable atomization conditions include the injection rate of molten steel, the spray pressure of gas or water, the spray volume, the ratio of molten steel to gas or water injected per unit time, and the oxygen concentration in the spray tank.

[0032] [Method for Producing Iron Sulfate] Next, a method for producing iron sulfate according to one embodiment of the present invention will be described. The method for producing iron sulfate according to this embodiment includes a step of dissolving the iron-based powder in sulfuric acid.

[0033] The specific method for dissolving the iron-based powder in sulfuric acid is not particularly limited, and known methods can be used. For example, one method involves adding the iron-based powder to sulfuric acid and allowing the reaction to proceed while stirring. The reaction temperature and reaction time can be appropriately adjusted depending on the type of iron-based powder and the concentration of sulfuric acid. Generally, it is preferable that the reaction temperature be within the range of room temperature to 80°C.

[0034] The processing method after dissolving the iron-based powder in sulfuric acid to obtain an aqueous solution of iron sulfate is not particularly limited, and known methods can be used. For example, a process to precipitate iron sulfate or a process to purify iron sulfate may be performed. In one embodiment, the method for producing iron sulfate may include the steps of dissolving the iron-based powder in sulfuric acid to obtain an aqueous solution of iron sulfate and precipitating iron sulfate from the aqueous solution of iron sulfate. Precipitation of iron sulfate can be carried out using methods such as cooling or evaporation and concentration. The precipitated iron sulfate can be separated by methods such as filtration or centrifugation and dried.

[0035] Furthermore, it is desirable to perform a purification process to remove impurities from the iron sulfate or an aqueous solution of iron sulfate. That is, a method for producing iron sulfate in one embodiment may include the steps of: dissolving the iron-based powder in sulfuric acid to obtain an aqueous solution of iron sulfate; precipitating iron sulfate from the aqueous solution of iron sulfate; and purifying the precipitated iron sulfate to remove impurities. A method for producing iron sulfate in another embodiment may include the steps of: dissolving the iron-based powder in sulfuric acid to obtain an aqueous solution of iron sulfate; purifying the aqueous solution of iron sulfate to remove impurities; and precipitating iron sulfate from the aqueous solution of iron sulfate. Examples of purification processes include recrystallization, treatment using ion exchange resin, and solvent extraction. This makes it possible to obtain high-purity iron sulfate.

[0036] As described above, in the method for producing iron sulfate according to this embodiment, by using iron-based powder, which is an iron source with a large specific surface area, and by keeping the component composition of the iron-based powder within a specific range, the production efficiency of iron sulfate can be improved and the odor during iron sulfate production can be suppressed.

[0037] The present invention will be described in detail below based on examples.

[0038] (Example 1) Iron-based powder was produced by the water atomization method. In the water atomization method, molten steel was charged into a tundish, the molten steel was dropped into a spray tank from a molten steel injection nozzle at the bottom of the tundish, and the iron-based powder was produced by causing a water jet to collide with the molten steel flow.

[0039] In Example 1, the oxygen content of the iron-based powder was adjusted by changing the amount of Si added to the molten steel. Furthermore, in order to further adjust the oxygen content of the iron-based powder and the above-mentioned full width at half maximum, the molten steel injection rate during atomization, the water jet pressure, the water volume, and the oxygen concentration in the spray tank were adjusted. Specifically, the rate at which the molten steel fell into the spray tank was set to 10 kg / min, the water jet pressure to 10 MPa, the water jet volume to 180 L / min, and the oxygen concentration in the spray tank to 5%.

[0040] The component composition of the obtained iron-based powder was determined by the following methods: C content: JIS G 1211-3 Iron and steel - Determination of carbon - Part 3: Combustion - Infrared absorption method O content: JIS G 1239 Iron and steel - Determination of oxygen - Inert gas fusion - Infrared absorption method Si content: JIS G 1258 Iron and steel - ICP emission spectrometry method The full width at half maximum of the peak of the (110) plane of α-Fe in the obtained iron-based powder was measured by the above method. The results are shown in Table 1. In the component composition of Table 1, the remainder is Fe and unavoidable impurities.

[0041] Next, the iron-based powder was dissolved in a fume hood. The concentration of the sulfuric acid solution was adjusted to 2.5 mol / L using distilled water, and the temperature of the sulfuric acid solution was maintained at 50°C using a water bath. 135 g of the sulfuric acid solution was placed in a 500 ml glass beaker, and the beaker was placed in the water bath set to 50°C. While stirring, 15 g of the obtained iron-based powder was added and dissolved, and the evaluation was performed according to the following procedure.

[0042] (Dimethyl sulfide concentration and odor intensity) The evaluation of dimethyl sulfide concentration and odor intensity was performed after stopping the exhaust of the draft chamber. The concentrations of dimethyl sulfide at 10 minutes, 30 minutes, and 60 minutes after the introduction of the iron-based powder were confirmed using a gas sampler Model GV-100 manufactured by Gastec Corporation, Pyrotec 840 manufactured by Gastec Corporation, and detector tube 53 (for dimethyl sulfide) manufactured by Gastec Corporation. At the same time, the odor intensity was determined according to the following criteria. (Criteria for determining odor intensity) 5: Intense offensive odor 4: Strong odor 3: Easily perceptible odor 2: Weak odor with distinguishable type (recognition threshold) 1: Barely perceptible odor, almost odorless (detection threshold) 0: Odorless In addition, odor intensity values of 2.5 and 3.5 are defined as intensities intermediate between 2 and 3, and between 3 and 4, respectively. When the odor intensity was 2.5 or lower, it was evaluated that the odor during sulfuric acid dissolution was suppressed.

[0043] (Temperature rise) The difference between the temperature before the introduction of the iron-based powder and the temperature 5 minutes after the introduction was determined as the temperature rise.

[0044] (Dissolution amount) 60 minutes after the introduction of the iron-based powder, the undissolved residue was collected according to the following procedures 1 to 6, and the dissolution amount of the iron-based powder was calculated. When the dissolution amount was 95% or more, it was evaluated that the iron-based powder was efficiently dissolved in sulfuric acid. 1: After standing for 10 minutes, the supernatant sulfuric acid was removed. 2: 100 g of distilled water set at 30°C was added to dissolve the produced hydrate. 3: After standing for 10 minutes, the supernatant distilled water was removed. 4: Steps 2 to 3 were repeated twice (that is, the hydrate dissolution was performed a total of 3 times). 5: The residue was filtered, dried, and weighed. 6: The dissolution amount was calculated using the following formula. (Amount of introduced iron-based powder (g) - Residue amount (g)) / Amount of introduced iron-based powder (g) × 100 = Dissolution amount (%)

[0045] The results are shown in Table 1. The concentration of dimethyl sulfide was below the lower detection limit of the detector tube (0.15 ppm or lower) at all time points after 10 minutes, 30 minutes, and 60 minutes. In addition, the odor intensity after 10 minutes was 2, and the odor intensity after 30 minutes and after 60 minutes was both 1. Furthermore, the dissolution amount determined by the above method was 95% or more. As described above, under the conditions of Example 1, the odor generated during sulfuric acid dissolution was suppressed, and the iron-based powder was efficiently dissolved in sulfuric acid.

[0046] (Examples 2 to 9) Iron-based powders having the component compositions and half-value widths described in Table 1 were produced by a water atomization method. In Examples 2 and 7 to 9, Si was added to the molten steel to adjust the O content of the iron-based powder. In Examples 3 to 6, the component composition of the molten steel was adjusted to adjust the O content and C content of the iron-based powder. In Examples 2 to 9, the molten steel pouring rate during atomization, the pressure and water volume of the water jet, and the oxygen concentration in the atomization tank were further adjusted to adjust the O content of the iron-based powder and the aforementioned half-value width. The obtained iron-based powder was dissolved in sulfuric acid in the same manner as in Example 1 for evaluation. In all cases, the reactivity of dimethyl sulfide generated during dissolution in sulfuric acid and the reactivity between the iron powder and sulfuric acid were evaluated. Under all conditions, the odor generated during dissolution in sulfuric acid was suppressed, and the iron-based powder was efficiently dissolved in sulfuric acid.

[0047] (Comparative Example 1) An iron-based powder having the component composition and half-value width described in Table 1 was produced by a water atomization method. Here, in order to adjust the O content of the iron-based powder, C was added to the molten steel, and the atomization conditions were adjusted. The obtained iron-based powder was dissolved in sulfuric acid in the same manner as in Example 1 for evaluation. The odor intensity exceeded 2.5 after 10 minutes and after 30 minutes, and the dimethyl sulfide concentration after 10 minutes was higher than that in the Examples. As such, under the conditions of Comparative Example 1, the odor generated during dissolution in sulfuric acid could not be suppressed.

[0048] (Comparative Examples 2 to 12) Iron-based powders having the component compositions and half-value widths described in Table 1 were produced by a water atomization method. Here, in order to adjust the O content of the iron-based powder, C was added to the molten steel, and the atomization conditions were adjusted. The obtained iron-based powders were dissolved in sulfuric acid adjusted to the concentration and temperature shown in Table 1 for evaluation. In all cases, the odor intensity exceeded 2.5 after 10 minutes, 30 minutes, and 60 minutes, and the dimethyl sulfide concentration after 10 minutes, 30 minutes, and 60 minutes was higher than that in the Examples. As such, under the conditions of Comparative Examples 2 to 12, the odor generated during dissolution in sulfuric acid could not be suppressed.

[0049] (Comparative Example 13) Iron-based powder was produced by the water atomization method, and then heated in a hydrogen atmosphere at 900°C for 1 hour to remove carbon and oxygen from the iron-based powder, resulting in iron-based powder having the component composition and full width at half maximum described in Table 1. The obtained iron-based powder was dissolved in sulfuric acid in the same manner as in Example 1 and evaluated. In Comparative Example 13, although the odor generated during sulfuric acid dissolution was suppressed, the iron-based powder could not be dissolved efficiently.

[0050] (Comparative Example 14) Iron-based powder having the component composition and full width at half maximum described in Table 1 was produced by the water atomization method. The obtained iron-based powder was dissolved in sulfuric acid in the same manner as in Example 1 and evaluated. In Comparative Example 14, although the odor generated during sulfuric acid dissolution was suppressed, the iron-based powder could not be dissolved efficiently.

[0051]

Claims

1. Iron-based powder for producing iron sulfate having a component composition of C: 0.08% by mass or less and O: 0.4% by mass or more and 5.0% by mass or less.

2. The iron-based powder for producing iron sulfate according to claim 1, wherein the component composition is Si: 0.01% by mass or more and 0.50% by mass or less.

3. The iron-based powder for producing iron sulfate according to claim 1 or 2, wherein the full width at half maximum of the peak of the (110) plane of α-Fe obtained by powder X-ray diffraction using Cu-Kα rays as an X-ray source is 0.10° or more and 0.40° or less.

4. A method for producing iron sulfate, comprising dissolving the iron-based powder described in any one of claims 1 to 3 in sulfuric acid.