Method for manufacturing circuit board, method for manufacturing mounting board, method for preventing back crack of board, and method for coating board

By forming a coating layer on the glass substrate edges before laminating wiring layers, the method addresses microcracks and back cracking issues, enhancing yield and productivity in glass circuit board manufacturing.

WO2026235083A1PCT designated stage Publication Date: 2026-11-12ENATECH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017036
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-29
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The manufacturing of glass circuit boards is hindered by microcracks on cut edges, damage during transport and processing, and back cracking due to thermal expansion coefficient mismatches, leading to reduced yield and productivity.

Method used

A method involving the formation of a coating layer on the end face of the glass substrate before laminating wiring layers, using plasma irradiation and controlled gas spraying to enhance adhesion and uniformity, thereby protecting the glass edges from damage and stress.

Benefits of technology

Prevents microcracks, edge erosion, and back cracking, improving manufacturing yield and productivity by enhancing the protection and uniformity of the coating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017036_12112026_PF_FP_ABST
    Figure JP2026017036_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for manufacturing a circuit board capable of improving the manufacturing yield of a circuit board using glass as a base material or a carrier material. A method for manufacturing a circuit board (10) having a glass substrate (11) and a build-up layer (31) formed so as to overlap the glass substrate (11) is provided with a coating layer formation step for forming a coating layer (21) on at least an end surface of the glass substrate (11) before forming the build-up layer (31).
Need to check novelty before this filing date? Find Prior Art

Description

Circuit board manufacturing method, mounted board manufacturing method, substrate back cracking prevention method, and substrate coating method

[0001] The present invention relates to a circuit board manufacturing method, a mounted board manufacturing method, a substrate back cracking prevention method, and a substrate coating method, and more specifically, relates to a circuit board manufacturing method, a mounted board manufacturing method, a substrate back cracking prevention method, and a substrate coating method that can improve the manufacturing yield of circuit boards and mounted boards that use glass as a base material or carrier material.

[0002] In recent years, along with the higher performance of electronic devices, the demand for higher density of circuit boards constituting semiconductor devices has been increasing. Conventionally, organic materials such as glass epoxy resin have been used as the substrate material for semiconductor package substrates, but with the advancement of glass drilling technology in recent years, circuit boards using glass substrates as the base material for next-generation semiconductor package substrates have been proposed (for example, refer to Patent Document 1 below).

[0003] FIG. 13 is a partial cross-sectional view schematically showing the configuration of the glass circuit board disclosed in Patent Document 1. The glass circuit board 200 includes a glass core 201 with through holes formed therein, and build-up layers 202 formed on both sides of the glass core 201.

[0004] The build-up layer 202 includes circuit layers 205 formed on both sides of the glass core 201, and a first insulating resin layer 207 and a second insulating resin layer 210 as interlayer insulating layers, forming a multi-layered circuit configuration of the circuit layers 205 and the second insulating resin layer 210.

[0005] [Problems to be Solved by the Invention] In the manufacture of the glass circuit board 200 as described above, in order to improve manufacturing efficiency, a large, thin glass panel with a thickness of about 200 μm to 1000 μm, which is cut to a full panel size (SEMI standard size: 510 mm × 515 mm), for example, is used as the glass substrate constituting the glass core 201.

[0006] Glass substrates cut to full panel size often have tiny cracks called microcracks on the cut edges. During the manufacturing process of the glass circuit board 200, these microcracks can easily cause damage such as cracks in the glass core 201.

[0007] For example, in the manufacturing process of the glass circuit board 200 described above, a plating process for forming the circuit layer 205 and a lamination process for forming the first insulating resin layer 207 and the second insulating resin layer 210 are repeatedly performed.

[0008] Therefore, it is necessary to transport the circuit boards in the process of manufacturing between processes. During this inter-process transport, the circuit boards in the process of manufacturing may come into contact with guide rollers or positioning pins of the transport equipment, causing damage such as cracks in the glass core 201. In addition, when cage plating is performed in the plating process, the circuit boards in the process of manufacturing may come into contact with the cage, causing damage such as cracks in the glass core 201.

[0009] Furthermore, in the process of forming the build-up layer 202, after forming via holes in the first insulating resin layer 207 and after forming via holes in the second insulating resin layer 210, a desmear treatment is performed to remove resin residue (smear).

[0010] During this desmearing process, the desmearing solution could erode the edges of the glass core 201, causing damage such as microcracks to spread. This type of damage to the glass core 201 during the manufacturing process resulted in a decrease in the manufacturing yield of the glass circuit board 200.

[0011] Furthermore, after manufacturing a full-panel-sized glass circuit board 200, in the process of manufacturing a mounted substrate by mounting chip components onto the glass circuit board 200, a dicing process is performed to divide the full-panel-sized glass circuit board 200 into multiple sub-subboards, and a process of mounting chip components onto the divided sub-subboards is performed. In addition, a dicing process is performed to divide the sub-subboards with the mounted chip components into package-unit substrates.

[0012] The glass circuit board 200 described above comprises a glass core 201 and a build-up layer 202. However, there is a significant difference between the thermal expansion coefficient (CTE) of the glass and the thermal expansion coefficient of the interlayer insulating layers, such as the first insulating resin layer 207 and the second insulating resin layer 210, which form the build-up layer 202.

[0013] In other words, the thermal expansion coefficient of glass varies depending on its material (alkali, alkali-free, quartz, etc.), but is approximately 3 to 9 ppm / °C, while the thermal expansion coefficient of the interlayer insulating layer varies depending on its resin composition, etc., but is approximately 20 to 60 ppm / °C. Thus, the thermal expansion coefficient of the interlayer insulating layer is several to tens of times larger than that of the glass substrate.

[0014] The glass circuit board 200 has multiple layers of interlayer insulating layers due to lamination, and internal stress accumulates within the board due to the thermal shrinkage of the interlayer insulating layers. Therefore, when a full-panel size glass circuit board 200 is diced into multiple sub-boards during the manufacturing process of the mounted board, the stress accumulated within the board is released, causing warping of the interlayer insulating layer at the cut points, and a phenomenon known as back cracking (SEWARE) may occur, where the glass core 201 is peeled away towards the build-up layer 202.

[0015] Furthermore, even in the full-panel size state before dicing onto the sub-board, warping can occur in the interlayer insulating layer, potentially leading to back cracks from the edges.

[0016] The aforementioned back splitting phenomenon can be prevented to some extent by improvements to dicing equipment, but it can still occur after a certain amount of time has passed since dicing.

[0017] Furthermore, in the process of mounting chip components onto divided sub-substrates, when the sub-substrate with the mounted chip components is reflow-heated, the interlayer insulating layer of the sub-substrate may shrink again, causing the same back cracking phenomenon as described above, which resulted in a decrease in the manufacturing yield of the mounted substrates.

[0018] Furthermore, after the sub-boards with mounted chip components are divided into unit boards, inspection tests such as heat cycle tests are performed to evaluate the reliability of the unit boards as final products.

[0019] In this inspection and testing process, when a heat cycle test is performed, the interlayer insulating layer of the unit substrate may shrink again, causing the same back cracking phenomenon as described above, which resulted in a decrease in the manufacturing yield of the mounted substrate.

[0020] Japanese Patent Publication No. 2017-216398 Means for solving the problem and their effects

[0021] The present invention has been made in view of the above problems, and aims to provide a method for manufacturing a circuit board, a method for manufacturing a mounted circuit board, a method for preventing back cracking of a substrate, and a method for coating a substrate, which can improve the manufacturing yield of circuit boards and mounted circuit boards using glass as a substrate or carrier material.

[0022] To achieve the above objective, the method for manufacturing a circuit board according to the present invention (1) is a method for manufacturing a circuit board having a glass substrate and a laminated wiring layer formed on top of the glass substrate, characterized in that it comprises a coating layer formation step of forming a coating layer on at least the end face of the glass substrate before forming the laminated wiring layer.

[0023] According to the above-described method for manufacturing a circuit board (1), since the coating layer is formed on at least the end face of the glass substrate before the laminated wiring layer is formed by the coating layer formation step, the laminated wiring layer can be formed with at least the end face of the glass substrate protected by the coating layer.

[0024] Therefore, it is possible to prevent the phenomenon of the edge surface of the glass substrate being eroded during chemical treatments such as etching, resist stripping, and desmearing, which are included in the process of forming the multilayer wiring layer.

[0025] Furthermore, even if there are minute chips on the edge surface of the glass substrate, the growth of microcracks from these chips can be prevented. In addition, even if an impact is applied to the edge surface of the glass substrate during the process of forming the multilayer wiring layer, the occurrence of damage such as cracks due to the impact can be prevented, and dust generation from the edge surface of the glass substrate can also be suppressed.

[0026] Furthermore, since at least the end face of the glass substrate is protected by the coating layer, the occurrence of back cracks in the circuit board can be prevented. Therefore, the manufacturing yield of the circuit board can be improved and productivity can be increased.

[0027] Furthermore, the term "back cracking" of the circuit board refers to a phenomenon in which the glass substrate breaks and peels away toward the multilayer wiring layer, caused by a mismatch in the thermal expansion coefficients of the glass substrate and the multilayer wiring layer.

[0028] Furthermore, the method for manufacturing a circuit board according to the present invention (2) is characterized in that, in the method for manufacturing a circuit board according to the present invention (1), the glass substrate includes a glass core layer having one or more glass layers, the laminated wiring layer includes a build-up layer in which a wiring layer and an insulating layer are laminated, the glass core layer formation step includes a through-via formation step of forming through-vias in the glass core layer, and a conductive layer formation step of forming a conductive layer on the glass core layer in which the through-vias have been formed, and the coating layer formation step on the glass end face is performed before the conductive layer formation step.

[0029] According to the above-described method for manufacturing a circuit board (2), since the coating layer is formed on at least the end face of the glass core layer before the conductive layer formation step by the coating layer formation step, the conductive layer can be formed in the conductive layer formation step with at least the end face of the glass core layer protected by the coating layer.

[0030] Therefore, in the conductive layer formation process, the phenomenon of erosion of the end face of the glass core layer can be prevented. Furthermore, even if there are minute chips on the end face of the glass core layer, the growth of microcracks from these chips can be prevented.

[0031] Furthermore, even if an impact is applied to the end face of the glass core layer during the conductive layer formation process, it is possible to prevent damage such as cracks caused by the impact, and to suppress dust generation from the end face of the glass core layer. Therefore, it is possible to improve the manufacturing yield of circuit boards having the glass core layer and increase productivity.

[0032] Furthermore, the circuit board manufacturing method (3) according to the present invention is characterized in that, in the circuit board manufacturing method (2) described above, the build-up layer formation step is performed after the glass core layer formation step, on the surface of the glass core layer on which the conductive layer is formed, in which the coating layer has been formed at least on the end face.

[0033] According to the above-described method for manufacturing the circuit board (3), in the build-up layer formation step, at least the end face of the glass core layer is protected by the coating layer, so that the end face of the glass core layer is not eroded by chemical treatments such as etching, resist stripping, and desmearing, which are included in the step of laminating the wiring layer and the insulating layer.

[0034] Furthermore, even if an impact is applied to the end face of the glass core layer during the build-up layer formation process, it is possible to prevent damage such as cracks caused by the impact.

[0035] Furthermore, even if heat treatment such as thermocompression bonding is performed in the build-up layer formation process, it is possible to prevent the occurrence of back cracks in the glass core layer caused by such thermal history.

[0036] Therefore, the manufacturing yield of the circuit board having the glass core layer can be improved, and productivity can be increased.

[0037] Furthermore, the back cracking of the glass core layer refers to a phenomenon in which the glass core layer fractures in a way that causes it to peel away toward the build-up layer, resulting from a mismatch in the thermal expansion coefficients of the glass core layer and the build-up layer.

[0038] Furthermore, the circuit board manufacturing method (4) according to the present invention is characterized in that, in the circuit board manufacturing method (1) above, the glass substrate includes a glass carrier that serves as a carrier material for a wafer-level package or a panel-level package, the laminated wiring layer includes a rewiring layer for the wafer-level package or the panel-level package, and the step of forming a coating layer on the glass edge is performed before the formation of the rewiring layer.

[0039] According to the above-described method for manufacturing the circuit board (4), the coating layer is formed on at least the end face of the glass carrier before the redistribution layer is formed by the coating layer formation step.

[0040] Therefore, in the process of forming the redistribution layer, the end face of the glass carrier is protected by the coating layer, which prevents the growth of microcracks from minute chipping on the end face of the glass carrier.

[0041] Furthermore, even if the glass carrier is subjected to impact during the process of forming the redistribution layer, the occurrence of cracks and other damage due to such impact can be prevented, and the peelability of the glass carrier can be improved. In addition, dust generation from the end face of the glass carrier can be suppressed. Therefore, the manufacturing yield of the wafer-level package or the panel-level package can be improved, and productivity can be increased.

[0042] Furthermore, the circuit board manufacturing method (5) according to the present invention is characterized in that, in any of the circuit board manufacturing methods (1) to (4) above, a plasma irradiation step is performed in which plasma is irradiated onto at least the end face of the glass substrate before the step of forming a coating layer on the glass end face.

[0043] According to the above circuit board manufacturing method (5), by performing the plasma irradiation step before the step of forming a coating layer on the glass end face, at least the surface modification of the end face of the glass substrate can be achieved.

[0044] For example, active oxygen, ozone and the like in the plasma can decompose and remove dust, oil, organic matter and the like adhering to at least the end face of the glass substrate. In addition, the hydrophilicity of at least the end face of the glass substrate can be improved. Accordingly, it is possible to improve the adhesion, wettability and the like of the coating agent in the subsequent step of forming a coating layer on the glass end face.

[0045] Further, in the circuit board manufacturing method (6) according to the present invention, in any one of the above circuit board manufacturing methods (1) to (5), the step of forming a coating layer on the glass end face includes a spraying step of applying a coating agent to the peripheral edge of the glass substrate and then spraying a gas with directivity so that the coating agent spreads toward the end side of the glass substrate.

[0046] According to the above circuit board manufacturing method (6), the step of forming a coating layer on the glass end face includes the spraying step, and through the spraying step, a gas having directivity toward the end side (outer peripheral direction) of the glass substrate is sprayed onto the applied coating agent.

[0047] Therefore, a shearing force in the outer peripheral direction is applied to the coating agent by the gas flow, and the coating agent can be made to flow toward the end side while being leveled. As a result, the occurrence of coating unevenness and uncoated portions of the coating agent can be suppressed, and the coating quality can be improved.

[0048] Furthermore, by forming a continuous and uniform coating layer from the peripheral edge portion to the end face, the mechanical protection performance of the outer peripheral portion of the glass substrate is improved, and the effect of preventing the occurrence of back cracks caused by external force and stress concentration can be enhanced.

[0049] Furthermore, the circuit board manufacturing method (7) according to the present invention is characterized in that, in the circuit board manufacturing method (6) above, the spraying step is a step in which gas is sprayed using a gas discharge means equipped with a discharge port for discharging the gas, and the gas discharged from the discharge port flows to the edge side of the glass substrate while the gas discharge means is moved relative to the peripheral edge of the glass substrate.

[0050] According to the above-described method for manufacturing a circuit board (7), in the spraying step, the gas discharge means is moved relative to the peripheral edge while the gas discharged from the discharge port flows towards the edge of the glass substrate.

[0051] Therefore, the airflow discharged from the outlet acts on the coating agent as a flow that combines components from the edge and the circumferential direction, continuously applying a uniform shear force across the width direction. This effectively suppresses uneven coating and missed areas of the coating agent on the peripheral edges, enabling the stable formation of a uniform coating layer with no visible irregularities.

[0052] Furthermore, the present invention relates to a method for manufacturing a mounting substrate (1), which is a method for manufacturing a mounting substrate on which chip components are mounted using a glass core substrate having a glass core layer having one or more glass layers and a build-up layer formed on top of the glass core layer, comprising: a first division step of dividing the glass core substrate into a plurality of sub-substrates; and a mounting step of mounting the chip components on each of the divided sub-substrates, characterized in that a coating layer formation step is performed after the first division step and before the mounting step, in which a coating layer is formed on at least the end face of each of the divided sub-substrates.

[0053] According to the above-described method for manufacturing the mounted substrate (1), after the first division step and before the mounting step, a coating layer formation step is performed in which a coating layer is formed on at least the end face of each divided sub-substrate. Therefore, in the mounting step, at least the end face of each sub-substrate is protected by the coating layer.

[0054] Therefore, even when heat treatment such as a reflow process is performed in the mounting process to mount the chip components, it is possible to prevent the occurrence of back cracks in each sub-substrate caused by thermal history, etc. Therefore, the manufacturing yield of the mounted substrate can be improved and productivity can be increased.

[0055] Furthermore, the back crack of the sub-substrate refers to a phenomenon in which the glass core layer of the sub-substrate breaks off and peels away toward the build-up layer, caused by a mismatch in the thermal expansion coefficients of the glass core layer and the build-up layer of the sub-substrate.

[0056] Furthermore, the method for manufacturing a mounting substrate according to the present invention (2) is characterized in that, in the method for manufacturing a mounting substrate (1) described above, a plasma irradiation step is performed in which plasma is irradiated onto at least the end face of the sub-substrate before the step of forming a coating layer on the end face of the sub-substrate.

[0057] According to the above-described method for manufacturing the mounted substrate (2), by performing the plasma irradiation step before the step of forming a coating layer on the end face of the sub-substrate, the surface of at least the end face of the sub-substrate can be modified.

[0058] For example, dust, oil, organic matter, etc. adhering to at least the end face of the sub-substrate can be decomposed and removed. Furthermore, the hydrophilicity of at least the end face of the sub-substrate can be improved.

[0059] Therefore, the adhesion and wettability of the coating agent in the subsequent coating layer formation process on the end face of the sub-substrate can be improved.

[0060] Furthermore, the manufacturing method (3) of the mounting substrate according to the present invention is characterized in that, in the manufacturing method (1) or (2) of the mounting substrate, the step of forming a coating layer on the end face of the sub-substrate includes a spraying step of applying a coating agent to the peripheral edge of the sub-substrate and then blowing gas so that the coating agent spreads in a directional manner along the peripheral edge of the sub-substrate.

[0061] According to the above-described method for manufacturing the mounted substrate (3), the step of forming a coating layer on the end face of the sub-substrate includes the spraying step, in which a gas having directionality along the peripheral edge of the sub-substrate is sprayed onto the coating agent after application.

[0062] Therefore, the coating agent can be flowed while being evenly distributed in a certain direction. This makes it possible to suppress uneven coating and missed spots of the coating agent at the peripheral edges of the sub-substrate, thereby improving the quality of the coating.

[0063] Therefore, the protective properties of the outer periphery of the sub-substrate are improved, and the effect of preventing back cracks in the sub-substrate caused by stress concentration and the like can be enhanced.

[0064] Furthermore, the method for manufacturing a mounting substrate according to the present invention (4) is characterized in that, in the method for manufacturing a mounting substrate (3) above, the spraying step includes a step of spraying gas such that the coating agent applied to the peripheral edge of the sub-substrate spreads toward the edge of the sub-substrate.

[0065] According to the above-described method for manufacturing the mounted substrate (4), the spraying step includes a step of spraying a gas having directionality toward the edge side (outer circumference direction) onto the coating agent applied to the peripheral edge of the sub-substrate.

[0066] Therefore, the flow of the gas applies a shear force to the coating agent in the outer direction, allowing the coating agent to flow evenly towards the edge. This suppresses uneven coating and missed areas of the coating agent in the region from the peripheral edge to the end face of the sub-substrate, thereby improving the coating quality.

[0067] Furthermore, the method for manufacturing a mounting substrate according to the present invention (5) is characterized in that, in the method for manufacturing a mounting substrate (3) or (4) above, the spraying step includes a step of spraying gas such that the coating agent applied to the peripheral edge of the sub-substrate spreads toward the stepped portion formed at the boundary between the glass core layer and the build-up layer.

[0068] According to the above-described method for manufacturing the mounted substrate (5), the spraying step includes a step of spraying a gas that is directional toward the stepped portion onto the coating agent applied to the peripheral edge of the sub-substrate.

[0069] Therefore, the gas flow applies a shear force to the coating agent in the direction of the step, allowing the coating agent to flow toward the step while leveling it. This suppresses the occurrence of uneven coating and missed spots in the coating agent that tend to occur at the step, improves the coverage in the area including the step, and improves the coating quality without increasing the amount of coating agent applied.

[0070] Furthermore, the manufacturing method (6) of the mounted substrate according to the present invention is characterized in that, in any of the above manufacturing methods (1) to (5) of the mounted substrate, a second division step is performed after the mounting step, in which the sub-sub

[0071] According to the above-described method for manufacturing the mounted substrate (6), after the second division step and before the inspection and testing step, the coating layer forming step is performed in which the coating layer is formed on at least the end face of each divided unit substrate.

[0072] Therefore, in the inspection and testing process, at least the end face of each unit substrate is protected by the coating layer. Consequently, even if thermal characteristic tests are performed on each unit substrate during the inspection and testing process, it is possible to prevent back cracks in each unit substrate caused by thermal history or other factors. Consequently, the manufacturing yield of the mounted substrate can be improved, and productivity can be increased.

[0073] Furthermore, the term "back cracking of the unit substrate" refers to a phenomenon in which the glass core layer of the unit substrate breaks in a way that causes it to peel off towards the build-up layer, resulting from a mismatch in the thermal expansion coefficients of the glass core layer and the build-up layer of the unit substrate.

[0074] Furthermore, the method for manufacturing a mounting substrate according to the present invention (7) is characterized in that, in the method for manufacturing a mounting substrate (6) described above, a plasma irradiation step is performed in which plasma is irradiated onto at least the end face of the unit substrate before the step of forming a coating layer on the end face of the unit substrate.

[0075] According to the above-described method for manufacturing the mounted substrate (7), by performing the plasma irradiation step before the step of forming a coating layer on the end face of the unit substrate, the surface of at least the end face of the unit substrate can be modified.

[0076] For example, dust, oil, organic matter, etc. adhering to at least the end face of the unit substrate can be decomposed and removed. Furthermore, the hydrophilicity of at least the end face of the unit substrate can be improved. Consequently, the adhesion and wettability of the coating agent in the subsequent coating layer formation process on the end face of the unit substrate can be improved.

[0077] Furthermore, the manufacturing method (8) of the mounting substrate according to the present invention is characterized in that, in the manufacturing method (6) or (7) of the mounting substrate, the step of forming a coating layer on the end face of the unit substrate includes a spraying step of applying a coating agent to the peripheral edge of the unit substrate and then spraying gas so that the coating agent spreads with directionality along the peripheral edge of the unit substrate.

[0078] According to the above-described method for manufacturing the mounted substrate (8), the spraying step involves spraying a gas that is directional along the peripheral edge of the unit substrate onto the coating agent after application.

[0079] Therefore, the coating agent can be flowed while being evenly distributed in a certain direction. As a result, the same effect as the manufacturing method of the mounted substrate (3) can be obtained even for the unit substrate which is obtained by dividing the sub-substrate, that is, for a smaller unit substrate.

[0080] Furthermore, the method for manufacturing a mounting substrate (9) according to the present invention is characterized in that, in any of the above methods for manufacturing a mounting substrate (1) to (8), the glass core substrate is a circuit board manufactured by the method for manufacturing a circuit board (2) or (3).

[0081] According to the above-described method for manufacturing the mounted substrate (9), since the glass core substrate is a circuit board manufactured by the method for manufacturing the circuit board (2) or (3), the effect of improving the manufacturing yield of the mounted substrate and increasing productivity can be further enhanced.

[0082] Furthermore, the method (1) for preventing back cracking of a substrate according to the present invention is a method for preventing back cracking that occurs when a glass substrate breaks and peels off toward the laminated wiring layer due to a mismatch in the coefficient of thermal expansion between the glass substrate and the laminated wiring layer formed on top of the glass substrate, characterized in that a coating layer is formed on at least the end face of the glass substrate before the laminated wiring layer is formed.

[0083] According to the above-described method for preventing back cracking of the substrate (1), since the coating agent is applied to at least the end face of the glass substrate before forming the multilayer wiring layer, at least the end face of the glass substrate can be protected by the coating layer.

[0084] Therefore, the edge protection effect of the coating layer prevents the occurrence of back cracks. Furthermore, it prevents various types of damage such as cracks, chips, and scratches from occurring on the edge surface of the glass substrate.

[0085] Furthermore, the method (2) for preventing back cracking of a substrate according to the present invention is characterized in that, in the method (1) for preventing back cracking of a substrate, the glass substrate includes a glass core layer having one or more glass layers, the laminated wiring layer includes a build-up layer in which a wiring layer and an insulating layer are laminated, and the coating layer is formed on at least the end face of a sub-substrate obtained by dividing the glass core substrate having the glass core layer and the build-up layer, and / or on at least the end face of a unit substrate obtained by dividing the sub-substrate.

[0086] According to the above-described method for preventing back cracking of the substrate (2), the coating layer is formed on at least the end face of the sub-substrate obtained by dividing the glass core substrate, and / or on at least the end face of the unit substrate obtained by dividing the sub-substrate.

[0087] Therefore, at least the end faces of the sub-substrate and / or the unit substrate can be protected by the coating layer, and the end-face protection effect of the coating layer can prevent the occurrence of back cracks. In addition, it is possible to prevent various types of damage such as cracks, chips, and scratches from occurring on the end faces of the sub-substrate and the unit substrate.

[0088] Furthermore, the substrate coating method (1) according to the present invention is characterized by including a coating step of applying a coating agent to at least the edge face of a substrate, and a spraying step after the coating step of blowing gas so that the coating agent spreads in a directional manner along the peripheral edge of the substrate.

[0089] According to the above substrate coating method (1), the spraying step involves spraying a gas that is directional along the peripheral edge of the substrate onto the coating agent after application. Therefore, the coating agent can be spread and flowed along the peripheral edge of the substrate in a consistent direction.

[0090] This suppresses uneven application and missed areas of the coating agent at the peripheral edges of the substrate, thereby improving coating quality. Consequently, the protective effect on the outer periphery of the substrate can be enhanced.

[0091] Furthermore, the substrate coating method (2) according to the present invention is characterized in that, in the substrate coating method (1) described above, the coating step includes a step of applying the coating agent to the peripheral edge of the substrate such that an uncoated area is left along the edge of the substrate, and the spraying step includes a step of spraying gas such that the coating agent applied to the peripheral edge of the substrate spreads with directionality toward the uncoated area.

[0092] According to the above substrate coating method (2), in the coating step, the coating agent is applied while leaving the uncoated area at the edge of the substrate, and in the spraying step, the coating agent is spread and flowed toward the uncoated area.

[0093] Therefore, even if the coating agent is not applied with high precision to the edges of the substrate in the coating step, the coating agent can be appropriately spread to the edges of the substrate by the spraying step. This makes it possible to obtain stable coating quality.

[0094] Furthermore, the substrate coating method (3) according to the present invention is characterized in that, in the substrate coating method (1) or (2) described above, the coating step includes a step of applying the coating agent to the peripheral edge of the substrate by continuously discharging droplets of the coating agent to form a droplet row, and the spraying step is characterized in that a gas discharge means equipped with a gas discharge port for discharging the gas is used, and the gas discharge means is moved relative to the peripheral edge of the substrate while spraying the gas while the gas discharge means flows to the edge of the substrate.

[0095] According to the above substrate coating method (3), even if the coating agent is applied in such a way that an uncoated area is left along the edge of the substrate when forming a droplet row on the peripheral edge of the substrate during the coating step, the subsequent spraying step can cause the coating agent to flow and spread evenly toward the edge of the substrate.

[0096] This suppresses uneven coating and missed spots of the coating agent at the periphery of the substrate, thereby improving coating quality. Furthermore, in the coating process, when applying the coating agent to the periphery of the substrate, it is no longer necessary to dispense the droplets with high precision to the edge of the substrate. This suppresses collisions of the droplets with the edge of the substrate, preventing the coating agent from scattering due to rebound caused by such collisions.

[0097] This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment of the present invention. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to an embodiment. This is a schematic perspective view showing a circuit board manufactured by the method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a method for manufacturing a mounting This is a schematic perspective view showing the image of dividing a circuit board into sub-substrates in the manufacturing method of a mounting substrate according to an embodiment. This is a cross-sectional view of the end face portion of a glass substrate on which a coating layer according to an example has been formed. This is a schematic diagram showing the main parts of the impact testing apparatus used to evaluate the example and comparative example. This is a table showing the results of a strength evaluation test using a glass substrate according to an example. This is a table showing the results of a strength evaluation test using a glass substrate according to a comparative example. This is a diagram for explaining a manufacturing method of a circuit board according to another embodiment. This is a diagram for explaining a manufacturing method of a circuit board according to another embodiment. This is a diagram for explaining a manufacturing method of a circuit board according to another embodiment.This is a diagram illustrating a method for manufacturing a circuit board according to another embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to another embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to another embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to yet another embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to yet another embodiment. This is a diagram illustrating a method for manufacturing a circuit board according to yet another embodiment. This is a diagram illustrating a modified version of the coating layer formation process on the glass end face in the method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a modified version of the coating layer formation process on the glass end face in the method for manufacturing a circuit board according to an embodiment. This is a diagram illustrating a modified version of the coating layer formation process on the sub-substrate end face in the method for manufacturing a mounting substrate according to an embodiment. This is a diagram illustrating a modified version of the coating layer formation process on the sub-substrate end face in the method for manufacturing a mounting substrate according to an embodiment. This is a diagram illustrating a modified version of the coating layer formation process on the sub-substrate end face in the method for manufacturing a mounting substrate according to an embodiment. This is a schematic partial cross-sectional view showing the configuration of a conventional glass circuit board.

[0098] Hereinafter, embodiments of the circuit board manufacturing method, mounting board manufacturing method, substrate back crack prevention method, and substrate coating method according to the present invention will be described with reference to the drawings. The embodiments described below are preferred specific examples of the present invention and are subject to various technically preferred limitations, but the scope of the present invention is not limited to these forms unless otherwise stated in the following description.

[0099] Figures 1A to 1K are diagrams illustrating a method for manufacturing a circuit board according to an embodiment of the present invention, and schematically show the end view of a cut portion of a circuit board during the manufacturing process. Figure 2 is a schematic perspective view showing a circuit board manufactured by the method for manufacturing a circuit board according to an embodiment.

[0100] As shown in Figure 2, the circuit board 10 manufactured by the circuit board manufacturing method according to the embodiment includes a glass core layer 12 and a build-up layer 31 laminated on the first surface (upper surface) and the second surface (lower surface) facing the first surface of the glass core layer 12. The glass core layer 12 is made of a glass substrate 11 with a coating layer 21 formed on its end face. The build-up layer 31 has a configuration in which a wiring layer 35 and an insulating layer 36 (see Figure 3B, etc.) are laminated.

[0101] In the manufacturing method of the circuit board according to the embodiment, first, a glass substrate 11 is prepared as shown in Figure 1A. The size and shape of the glass substrate 11 are not particularly limited, but for example, it is cut to a full panel size (SEMI standard size: 510 mm x 515 mm). The glass substrate 11 may be a single glass core composed of a single glass layer, or a multi-glass core composed of multiple glass layers.

[0102] The thickness of the glass substrate 11 is not particularly limited, but is preferably about 50 μm to 1000 μm. The cross-sectional shape of the end face of the glass substrate 11 may be a right-angle edge as shown in the figure, or it may be a chamfered edge with the corner beveled, or a curved edge with the corner processed into a curved shape.

[0103] The material of the glass substrate 11 is not particularly limited as long as it is a glass panel mainly composed of SiO2. For example, the glass substrate 11 may be made of alkali-free glass having a thermal expansion coefficient (CTE) of 3 to 7 ppm / °C, or alkali glass having a thermal expansion coefficient of 8 to 12 ppm / °C.

[0104] The thermal expansion coefficient of the glass substrate 11 can be adjusted within the range of 3 to 12 ppm / °C by changing the manufacturing method or by adding metal components such as Na. The thermal expansion coefficient (average linear expansion coefficient) is a value measured by thermomechanical analysis (TMA) in accordance with JIS R3102:1995 for glass or JIS K7197:2012 for plastics.

[0105] Next, as shown in Figure 1B, a process is carried out to form a plurality of through vias 13 in the glass substrate 11. The through vias 13 are through holes for electrically connecting the first surface (top surface) and the second surface (bottom surface) of the glass substrate 11.

[0106] For forming the through via 13, known processing methods such as laser processing, electrochemical processing, plasma etching, and chemical etching can be used, with laser processing being preferred from the viewpoint of throughput. The laser used for the laser processing is CO 2 Lasers, UV lasers, picosecond lasers, femtosecond lasers, etc., can be selected as appropriate.

[0107] Next, as shown in Figure 1C, a coating layer formation step is performed on the glass end face, in which a coating agent is applied to at least the end face of the glass substrate 11 to form a coating layer 21. In this case, since the glass substrate 11 has a full-panel size rectangular shape, the coating agent is applied to at least the end face of the four sides between the first surface (top surface) and the second surface (bottom surface) of the glass substrate 11 to form a coating layer 21.

[0108] The thickness of the coating layer 21 varies depending on the thickness of the glass substrate 11, but is not limited to these ranges, for example, 10 μm to 300 μm, preferably 20 μm to 150 μm, and more preferably 30 μm to 100 μm.

[0109] Applying the coating agent to at least the end face includes not only cases where it is applied only to the end face, but also cases where it is applied to the end face and the peripheral edge. For example, if the cross-sectional shape of the end face of the glass substrate 11 is a right-angle edge, the coating agent may be applied so that the coating layer 21 is formed only on the end face as shown in the figure, or the coating agent may be applied so as to cover the corner of the right-angle edge, that is, to the end face and the peripheral edges of the upper and lower surfaces.

[0110] Furthermore, if the cross-sectional shape of the end face of the glass substrate 11 is a chamfered edge or a curved edge, the coating agent may be applied in such a way that it also covers the chamfered or curved portion.

[0111] The coating agent may consist of a liquid containing one or more water-soluble resins such as acrylic, polyurethane, or silicone, or it may consist of a liquid containing a water-insoluble resin such as fluorine or epoxy. Furthermore, the coating agent may consist of a photocurable resin such as UV resin, or a thermosetting resin.

[0112] Furthermore, it is preferable that the coating agent has a thermal expansion coefficient αc that is close to the thermal expansion coefficient αi of the insulating layer 36 that constitutes the build-up layer 31 described later (for example, αc = αi ± 10 (ppm / °C, 25-150°C), more preferably αi ± 5 (ppm / °C, 25-150°C)).

[0113] Alternatively, it is preferable that the thermal expansion coefficient αc is greater than the thermal expansion coefficient αi of the insulating layer 36 (for example, αi < αc < αi + β (ppm / °C, 25-150°C), β < 10, preferably β < 5).

[0114] Furthermore, it is preferable that the difference between the thermal expansion coefficient αc of the coating agent and the thermal expansion coefficient αg of the glass substrate 11 is smaller than the difference between the thermal expansion coefficient αi of the insulating layer 36 and the thermal expansion coefficient αg of the glass substrate 11 (αc - αg < αi - αg).

[0115] The process of forming a coating layer on the glass edge is carried out using a coating apparatus 51. Such a coating apparatus 51 may be a contact-type coating apparatus that applies the coating agent while bringing a coating tool such as a coating roller into contact with the edge surface of the glass substrate 11, or a non-contact-type coating apparatus that applies the coating agent to the edge surface of the glass substrate 11 while dispensing it from a dispensing tool such as a dispenser.

[0116] The coating roller can be a resin roller, rubber roller, porous roller, or metal roller. For example, a method of supplying the coating agent to such a coating roller can be applied using a dispenser with a needle nozzle to supply the coating agent to the surface of the coating roller.

[0117] Furthermore, the dispenser of a non-contact coating device can be configured as a jet dispenser, an air-pressure dispenser, a piston dispenser, or the like. For jet dispensers, for example, a piezo-driven system, a solenoid-driven system, or a thermal system can be applied. Such dispensers are preferably microdispensers capable of dispensing minute amounts of liquid droplets (for example, on the order of several hundred μl to nl).

[0118] As described above, the process of forming a coating layer on the glass edge may also involve a contact-type coating process in which a coating agent is applied while a coating tool, such as a coating roller, is in contact with at least the edge surface of the glass substrate 11.

[0119] Alternatively, a non-contact coating process may be applied, in which droplets of the coating agent are dispensed from a dispensing device such as a dispenser and applied to the end face and / or peripheral edge of the glass substrate 11.

[0120] Furthermore, in order to stabilize the viscosity and other properties of the coating agent, the coating apparatus 51 may be provided with a heating unit for heating the coating agent, and in the process of forming a coating layer on the glass edge, the coating agent heated to a predetermined temperature range in the heating unit may be applied.

[0121] An example of a non-contact coating process in which a coating agent is applied to the end face of a glass substrate 11 using a dispenser on a coating apparatus 51 is described below. First, the glass substrate 11 is fixed to a holding jig or the like, and the nozzle tip of the dispenser is positioned relative to the end face of the glass substrate 11 so that the main scanning direction of the dispenser coincides with the longitudinal direction of the end face of the glass substrate 11.

[0122] The orientation of the dispenser nozzle tip is not particularly limited, but it may be positioned perpendicular to the end face of the glass substrate 11 (facing it directly), or it may be positioned at an angle in the horizontal or vertical direction.

[0123] Next, the gap between the nozzle tip of the dispenser and the end face of the glass substrate 11 is adjusted. Then, the dispenser is moved in one direction along the longitudinal direction of the end face of the glass substrate 11, and droplets are continuously dispensed from the nozzle tip, thereby forming a first row of droplets.

[0124] The droplet pitch in the longitudinal direction of the end face of the glass substrate 11 is controlled to a predetermined value based on the relationship between the dispenser's movement speed and the dispensing frequency. The droplet pitch is preferably set to approximately 0.5 to 1 times the droplet diameter, for example, so that adjacent droplets are in contact with each other or partially overlap.

[0125] After forming the first row of droplets, the dispenser is shifted by a predetermined pitch relative to the width (thickness) direction of the end face of the glass substrate 11 in order to reverse the direction of movement of the dispenser in the main scanning direction. This movement pitch in the width direction is preferably set to, for example, 0.5 to 1 times the droplet diameter, so that droplets between adjacent droplet rows come into contact with each other or partially overlap.

[0126] Subsequently, the dispenser is moved along the longitudinal direction of the end face of the glass substrate 11 in the opposite direction to the aforementioned one direction, while continuously dispensing droplets from the nozzle tip to form a second row of droplets.

[0127] Then, taking into consideration the relationship between the thickness of the glass substrate 11 and the droplet diameter, multiple rows of droplets are arranged in a grid pattern by repeatedly performing reciprocal scanning with respect to the main scanning direction of the dispenser and shifting in the width direction. The droplets arranged in the grid pattern wet and spread on the edge surface of the glass substrate 11, forming a coating layer 21 consisting of a continuous liquid film.

[0128] Furthermore, in the non-contact coating process described above, it is possible to form a coating layer 21 of a predetermined width not only on the end face of the glass substrate 11, but also on the peripheral edges of the glass substrate 11, i.e., the peripheral edges of the upper and / or lower surfaces, using a dispenser.

[0129] In this process, first, the glass substrate 11 is fixed to a holding jig or the like, and positioned so that the dispenser nozzle can access the peripheral edges of the upper and / or lower surfaces of the glass substrate 11.

[0130] In this case, the dispenser is configured to move in multiple axes using a multi-axis movement mechanism (for example, an XYZ linear motion mechanism, a θ rotation mechanism, a 6-axis robot, etc.) provided on the coating device 51, enabling continuous scanning along the peripheral edge of the glass substrate 11.

[0131] Next, the gap between the nozzle tip of the dispenser and the peripheral edge of the glass substrate 11 is adjusted. Subsequently, when forming a coating layer 21 on the peripheral edge of the upper surface, the dispenser is moved along a trajectory along the peripheral edge, and droplets are continuously discharged from the nozzle tip to form a first row of droplets. The pitch of the droplet row is preferably set so that adjacent droplets are in contact with each other or partially overlap.

[0132] Subsequently, the dispenser's scanning trajectory is shifted by a predetermined amount inward or outward from the substrate, and droplets are continuously dispensed while scanning along the periphery again, thereby sequentially forming the second and subsequent rows of droplets.

[0133] In this case as well, it is preferable to control the overlap ratio between adjacent rows so that the spacing between rows of droplets is appropriate. By repeating this process, multiple rows of droplets are arranged in a region of a predetermined width along the periphery of the upper surface.

[0134] Similarly, when forming a coating layer 21 on the peripheral edge of the lower surface, the relative positional relationship between the dispenser and the glass substrate 11 is changed.

[0135] For example, after the dispenser is reversed and moved from the top to the bottom of the substrate, the same scanning and dispensing control is performed on the peripheral edge of the bottom surface. The droplets dispensed onto the peripheral edge of the glass substrate 11 then wet and spread, fusing together to form a continuous coating layer 21 of a predetermined width across the end face and peripheral edge of the glass substrate 11.

[0136] Furthermore, when forming a coating layer 21 continuously on the end face and peripheral edge of the glass substrate 11, it is preferable to move the dispenser's scanning path continuously from the peripheral edge of the upper surface to the end face, and from the end face to the peripheral edge of the lower surface.

[0137] In this case, to suppress liquid accumulation and increased film thickness at the corners of the substrate, control may be implemented to temporarily reduce the dispenser's discharge volume, set a discharge stop interval, or adjust the scanning speed.

[0138] Next, as shown in Figure 1D, a seed layer formation process is performed to form a seed layer 32, which is a conductive film, on the surface of the glass substrate 11 (i.e., the glass core layer 12) on which the coating layer 21 is formed at the end face.

[0139] The surface of the glass substrate 11 includes a first surface (top surface), a second surface (bottom surface), a surface for forming the coating layer 21 at the end face, and the inner wall of the through via 13. The thickness of the seed layer 32 is, for example, about 0.01 μm or more and 5 μm or less.

[0140] The seed layer formation process is carried out, for example, by an electroless copper plating method. The seed layer formation process by the electroless copper plating method includes, for example, a pretreatment to roughen the surface of the glass substrate 11, an activation treatment to apply a seed metal catalyst (palladium catalyst) to the surface of the glass substrate 11, an electroless copper plating treatment to form a uniform copper thin film on the activated glass substrate 11, and post-treatment such as cleaning or heat treatment as needed.

[0141] The thickness of the seed layer 32 formed by the electroless copper plating method is, for example, about 0.01 μm or more and 5 μm or less. In the seed layer formation process, in addition to the electroless copper plating method described above, known methods such as chemical vapor deposition (CVD) and physical vapor deposition (PVD) may also be used, and it is possible to make the thickness of the seed layer 32 thinner by these methods.

[0142] Next, as shown in Figure 1E, an electrolytic plating layer formation process is performed to form an electrolytic plating layer 33 on the glass substrate 11 on which the seed layer 32 is formed. The electrolytic plating layer formation process is performed, for example, by an electrolytic copper plating method.

[0143] By the electrolytic copper plating method, an electrolytic plating layer 33 is formed on the first surface (top surface), the second surface (bottom surface), and the end surface of the glass substrate 11 on which the seed layer 32 is formed, and electrolytic copper plating is also applied to the inner wall of the through via 13 on which the seed layer 32 is formed.

[0144] In Figure 1E, the through via 13 is embedded in the electroplating layer 33, but it may also be in a hollow form without being embedded. The thickness of the electroplating layer 33 on the surface of the glass substrate 11 is, for example, 1 μm or more and 20 μm or less.

[0145] In addition to the electrolytic copper plating method described above, the electrolytic plating layer formation process may also use an electrolytic plating method using other metals such as nickel. In another embodiment, the electrolytic plating layer formation process may be omitted, and in the subsequent wiring layer formation process, electrolytic copper plating may be applied to the surface on which the coating layer 21 is formed on the end face of the glass substrate 11 on which the seed layer 32 is formed, and to the inner wall portion of the through via 13, thereby forming an electrolytic plating layer 33 on the surface on which the coating layer 21 is formed and the portion of the through via 13.

[0146] Next, the process moves on to forming the build-up layer 31 (see Figure 2). First, as shown in Figure 1F, a patterning process is performed to form a resist pattern 34 on both surfaces (the first surface and the second surface) of the glass substrate 11 on which the seed layer 32 as a conductive layer and the electroplating layer 33 are formed.

[0147] This patterning process is carried out, for example, by using a dry film resist, which is a photosensitive resin film. Specifically, a dry film is attached to the electroplating layer 33 formed on both surfaces of the glass substrate 11 using a roll laminator to form a resist layer.

[0148] Next, a desired resist pattern 34 is formed on the electrolytic plating layer 33 formed on both surfaces of the glass substrate 11 by a known photolithography method. The resist pattern 34 is then patterned after being aligned so that the portion where the wiring layer 35 will be formed in the next step is exposed.

[0149] Next, as shown in Figure 1G, electrolytic copper plating is performed using the conductive layer to form a wiring layer 35. After that, the unnecessary resist pattern 34 is peeled off, and then a wiring layer formation process is performed in which the electrolytic plating layer 33 and seed layer 32 beneath the resist pattern 34 are removed by flash etching.

[0150] This wiring layer formation process forms wiring layers 35 on both surfaces of the glass substrate 11. The thickness of the wiring layer 35 is, for example, 1 μm or more and 20 μm or less.

[0151] In addition, this flash etching process may also reduce the thickness of the electrolytic plating layer 33 formed on the edge of the glass substrate 11, but it is preferable to perform the process in a way that does not expose the coating layer 21.

[0152] Next, the process proceeds to the step of forming an insulating layer 36 as an interlayer insulating layer on top of the wiring layer 35, as shown in Figures 1H to 1K. The method for forming the insulating layer 36 is not particularly limited, but a method of forming it by heat-pressing a film-like insulating resin material 36a with a vacuum laminator is preferred because it is common, simple, and has good productivity.

[0153] For example, a three-layer film material can be used for such a film-like insulating resin material 36a, which consists of a PET film, an insulating resin film layer mainly composed of a thermosetting resin such as epoxy resin or cyanate resin, and a protective film.

[0154] First, as shown in Figure 1H, the insulating resin material 36a, from which the protective film has been peeled off, is placed on both surfaces of the glass substrate 11, and then heat-pressed with a vacuum laminator, thereby laminating the insulating resin material 36a onto both surfaces of the glass substrate 11.

[0155] Next, as shown in Figure 1I, after peeling the PET film from the laminated insulating resin material 36a, a heat-curing treatment (also called curing) is performed. The heat-curing treatment covers the surface of the wiring layer 35 formed on both surfaces of the glass substrate 11 with the heat-cured insulating layer 36. The thickness of the insulating layer 36 is, for example, 10 μm or more and 100 μm or less.

[0156] Next, as shown in Figure 1J, a step is performed to form blind vias 37 at predetermined locations on the insulating layer 36 by laser processing. The blind vias 37 are vias that enable connection to the wiring layer 35.

[0157] The via diameter is, for example, 100 μm or less, preferably 30 μm or less. The laser used for laser processing is CO2. 2It is possible to select from lasers, UV lasers, picosecond lasers, femtosecond lasers, etc., as appropriate.

[0158] Next, as shown in Figure 1K, a desmear treatment is performed to roughen the surface of the insulating layer 36 and clean (remove residue) the inside of the blind vias 37. A known treatment method such as the alkaline manganese salt method can be used for the desmear treatment. After that, the same process as in Figure 1D described above is performed to form a seed layer 32 on the surface of the insulating layer 36 and inside the blind vias 37 by electroless copper plating, thereby enabling conductivity.

[0159] Subsequently, the same process as in Figure 1F described above is performed to form a resist pattern 34 on the newly formed seed layer 32 using a dry film. Then, the same process as in Figure 1G described above is performed to form a wiring layer 35 by electrolytic copper plating, remove the resist pattern 34, and remove the seed layer 32 beneath the resist pattern 34 by flash etching, thereby laminating and forming the next wiring layer 35 on the insulating layer 36.

[0160] Subsequently, the same process as shown in Figures 1H to 1K above is performed to form the next insulating layer 36 on the next wiring layer 35. By repeating these processes to form the build-up layer 31 as a multilayer wiring layer, it is possible to manufacture a circuit board 10 which is a glass core substrate having a glass core layer 12 and a build-up layer 31, as shown in Figure 2.

[0161] In the circuit board 10 shown in Figure 2, the coating layer 21 is formed on at least the end face of the glass substrate 11 that constitutes the glass core layer 12. On the other hand, in a method for manufacturing a circuit board according to another embodiment, after forming the build-up layer 31, a step may be performed to apply a coating agent to the end face of the circuit board (i.e., the end face of the build-up layer 31 and the glass core layer 12) to further form a coating layer.

[0162] Figures 3A to 3K are schematic diagrams illustrating the manufacturing method of a mounting substrate according to the embodiment, with Figures 3A and 3G being plan views and the others being cross-sectional views. The manufacturing method of a mounting substrate according to the embodiment shown in Figures 3A to 3K is a method for manufacturing a mounting substrate on which chip components are mounted using a full-panel size circuit board 10 manufactured by the circuit board manufacturing method described above.

[0163] Figure 3A shows a plan view of a full-panel size circuit board 10. First, as shown in Figures 3A and 3B, a first division process is performed in which the full-panel size circuit board 10 is divided into sub-boards 10A of approximately 1 / 4 size (for example, 240 mm x 240 mm) using a dicing device. Figure 4 is a schematic perspective view showing the image of the circuit board 10 being divided into sub-boards 10A.

[0164] In the first division process, when the circuit board 10 is divided into a sub-substrate 10A, the coating layer 21 formed on the end face of the glass substrate 11 constituting the circuit board 10 is cut off (removed) by the outer shaping process when dividing it into the sub-substrate 10A.

[0165] Therefore, as shown in Figure 3B, the coating layer 21 of the circuit board 10 is not present on the end face of the sub-substrate 10A after it has been divided into approximately 1 / 4 size. Consequently, the end face of the sub-substrate 10A is exposed as a cut surface.

[0166] Therefore, there is a risk of a "back crack" phenomenon occurring, in which the glass substrate 11 of the sub-substrate 10A breaks and peels away toward the build-up layer 31 due to a mismatch in the coefficients of thermal expansion between the glass substrate 11 and the build-up layer 31.

[0167] Next, as shown in Figure 3C, a coating layer formation step is performed on the end faces of the divided sub-substrates 10A, in which a coating agent is applied to the end faces of each sub-substrate 10A to form a coating layer 21A.

[0168] The sub-substrate 10A has a structure in which build-up layers 31 are laminated on both sides of a glass substrate 11 that constitutes the glass core layer 12. In the process of forming a coating layer on the end face of the sub-substrate, a coating agent is applied to at least the end faces of all four sides of the sub-substrate 10A, for example, the end faces of the glass substrate 11 and the build-up layer 31 of the sub-substrate 10A, to form a coating layer 21A.

[0169] If the cross-sectional shape of the end face of the sub-substrate 10A is a right-angle edge, the coating agent may be applied so that the coating layer 21A is formed only on the end face as shown in the figure, or the coating agent may be applied so that the corners of the right-angle edge (outer peripheral edges of the upper and lower surfaces) are also covered. The same coating agent used in the coating layer formation process on the glass end face described above can be used for this coating agent.

[0170] The process of forming a coating layer on the edge face of the sub-substrate can be carried out using the coating apparatus 51 used in the process of forming a coating layer on the glass edge face described above. Since the full-panel size circuit board 10 and the sub-substrate 10A have different substrate sizes, the coating apparatus 51 is equipped with a coating mechanism that can accommodate the difference in substrate size.

[0171] After completing the coating layer formation process on the edge faces of the sub-substrates, the process proceeds to the mounting process in which chip components (not shown) are mounted on each sub-substrate 10A. In the mounting process, first, as shown in Figure 3D, flux is applied to necessary locations on the sub-substrate 10A, such as the chip mounting locations, and then solder balls 41 and chip components (not shown) are mounted.

[0172] The method of applying flux is not particularly limited and can be done by methods such as spray coating or jet coating. In addition, the solder balls 41 may be formed by methods such as vapor deposition, electroplating, or stencil printing, depending on the bump size, in addition to the ball placement method.

[0173] The method of mounting chip components is not particularly limited and can be done using equipment such as chip mounters and bonders. Chip components include passive components such as chip capacitors, active components such as chip transistors and chip ICs, and other mounting components such as chip sensors.

[0174] In the mounting process, as shown in Figure 3E, the sub-substrate 10A on which chip components (not shown) are mounted is heated in a reflow oven 52 to melt the solder balls 41 and join the sub-substrate 10A to the chip components (not shown). After removing the sub-substrate 10A on which the chip components (not shown) are mounted from the reflow oven 52, the flux residue on the sub-substrate 10A is washed off as shown in Figure 3F.

[0175] Figure 3G shows a plan view of a sub-substrate 10A on which chip components (not shown) are mounted. In the next step, as shown in Figures 3G and 3H, a second division step is performed in which the sub-substrate 10A on which chip components (not shown) are mounted is divided into multiple unit substrates 10B of package unit size (for example, 50 mm x 50 mm) using a dicing apparatus.

[0176] In the second division process, when the sub-substrate 10A is divided into the unit substrate 10B, the coating layer 21A formed on the end face of the sub-substrate 10A is cut off (removed) by the outer shaping process when dividing it into the unit substrate 10B.

[0177] After being divided into package unit sizes, the coating layer 21A formed on the end face of the sub-substrate 10A is no longer present on the end face of the unit substrate 10B. Therefore, the end face of the unit substrate 10B is exposed, revealing the cut surface.

[0178] Therefore, there is a risk of a "back crack" phenomenon occurring, in which the glass substrate 11 of the unit substrate 10B breaks and peels away toward the build-up layer 31 due to a mismatch in the coefficients of thermal expansion between the glass substrate 11 and the build-up layer 31.

[0179] Next, as shown in Figure 3I, a coating layer formation step is performed on the end faces of the unit substrates, in which a coating agent is applied to at least the end faces of each divided unit substrate 10B to form a coating layer 21B.

[0180] The unit substrate 10B, like the sub-substrate 10A, has a structure in which build-up layers 31 are laminated on both sides of the glass substrate 11 that constitutes the glass core layer 12. In the process of forming a coating layer on the end face of the unit substrate, a coating agent is applied to at least the end faces of all four sides of the unit substrate 10B, for example, the end faces of the glass substrate 11 and the build-up layer 31 of the unit substrate 10B, to form a coating layer 21B.

[0181] If the cross-sectional shape of the end face of the unit substrate 10B is a right-angle edge, the coating agent may be applied so as shown in the figure that the coating layer 21B is formed only on the end face, or the coating agent may be applied so as to cover the corners of the right-angle edge (the outer peripheral edges of the upper and lower surfaces). The same coating agent used in the coating layer formation process on the end face of the sub-substrate described above can be used as the coating agent.

[0182] The process of forming a coating layer on the end face of the unit substrate can be carried out using the coating apparatus 51 used in the process of forming a coating layer on the end face of the sub-substrate described above. Since the sub-substrate 10A and the unit substrate 10B have different substrate sizes, the coating apparatus 51 is equipped with a coating mechanism that can accommodate the difference in substrate size.

[0183] Next, as shown in Figure 3J, an inspection test process is performed to check whether each divided unit board 10B has the performance required for a product. In the inspection test process, performance tests such as visual inspection, electrical characteristics test, and reliability test are performed.

[0184] Reliability testing includes environmental tests such as high-temperature and high-humidity tests, thermal shock tests, and temperature cycling tests, as well as mechanical tests such as bending tests, impact tests, and compression tests. Figure 3J illustrates a case where temperature cycling tests are being performed on each unit substrate 10B using a temperature cycling test machine 53.

[0185] During the inspection and testing process, there is a risk of back cracking occurring in the unit substrate 10B due to thermal and mechanical loads being applied to it. However, since a coating layer 21B is formed on the end face of the unit substrate 10B, the occurrence of back cracking can be prevented. Therefore, as shown in Figure 3K, it is possible to increase the manufacturing yield of the final mounted substrate 10C after the inspection and testing process.

[0186] [Examples] In Example 1 below, an impact test was performed using a glass substrate 11 with a coating layer 21 formed on its edge, and its strength was evaluated. As Comparative Example 1, a similar impact test was performed using a glass substrate 110 without a coating layer 21 formed on its edge, and the results were compared with those of Example 1. For the glass substrate 11 in Example 1 and the glass substrate 110 in Comparative Example 1, a glass panel with a thickness of 0.8 mm was cut into 100 mm x 100 mm squares.

[0187] Figure 5 shows a cross-sectional view of the end face portion of a glass substrate 11 in which a coating layer 21 is formed on the end face, according to Example 1. The end face of the glass substrate 11 shown in Figure 5 has a chamfered edge, and the coating layer 21 is formed in a frame shape to cover the chamfered portion and the outer edge of the end face.

[0188] In this case, the thickness of the coating layer 21 was thickest near the center of the edge. Note that the thickness of the coating layer 21 will vary depending on the thickness of the glass substrate 11, the shape of the corners, and the properties of the coating agent.

[0189] Figure 6 is a schematic diagram showing the main parts of the impact testing apparatus used for the evaluation of Example 1 and Comparative Example 1.

[0190] The impact testing apparatus 60 comprises a base 61 that forms a horizontal surface, an attacker 62 disposed on the base 61, and two guide columns 63 that are vertically mounted on the base 61, with the attacker 62 positioned between the two guide columns 63. The attacker 62 is a metal projection (projection height: 15 mm). The two guide columns 63 are for guiding the glass substrates 11 and 110 in the vertical direction and are equipped with guide grooves in the vertical direction.

[0191] In the impact test, the glass substrate 11 of Example 1 and the glass substrate 110 of Comparative Example 1 were placed between two guide columns 63, and the glass substrates 11 and 110 were dropped from different height positions (h = 5, 10, 20, and 30 cm) on the guide columns 63, respectively, causing the lower end surfaces of the glass substrates 11 and 110 to collide with the attacker 62, and the damage condition of the lower end surfaces was checked.

[0192] Figure 7 is a table showing the results of an impact test conducted using the glass substrate 11 according to Example 1. As shown in the table in Figure 7, no damage such as cracks, chips, or scratches occurred on the edge surface of the glass substrate 11 according to Example 1, regardless of whether it was dropped from a height of h = 5, 10, 20, or 30 cm.

[0193] Figure 8 is a table showing the results of an impact test conducted using the glass substrate 110 according to Comparative Example 1. As shown in the table in Figure 8, even when dropped from the lowest height of h = 5 cm, scratches occurred on the edge surface of the glass substrate 110. Furthermore, as the height increased to h = 10, 20, and 30 cm, the area of ​​cracks and chips on the edge surface of the glass substrate 110 increased, and at h = 30 cm, a dent occurred on the edge surface.

[0194] As a result of the impact tests described above, it was confirmed that the impact resistance of the glass substrate 11 according to Example 1 can be improved by forming the coating layer 21 on the edge surface.

[0195] Next, in Example 2, a heat treatment test was performed using a sub-substrate 10A with a coating layer 21A formed on its end face to evaluate the back cracking phenomenon. As Comparative Example 2, a similar heat treatment test was performed using a sub-substrate without a coating layer 21A formed on its end face.

[0196] For the sub-substrate 10A of Example 2 and the sub-substrate of Comparative Example 2, a circuit board in which build-up layers 31 were formed on both sides of a glass substrate 11 was diced into a 100 mm x 100 mm square. In the sub-substrate 10A of Example 2, a coating agent was applied to the edges of all four sides after dicing to form a coating layer 21A. In the sub-substrate of Comparative Example 2, no coating layer 21A was formed. The sub-substrate 10A of Example 2 and the sub-substrate of Comparative Example 2 were each subjected to a heating treatment in a high-temperature furnace (182°C) for a predetermined time (30 minutes), and their condition after this heating treatment test was visually confirmed.

[0197] In the sub-substrate according to Comparative Example 2, a back cracking phenomenon occurred in which the glass substrate 11 fractured and peeled away toward the build-up layer 31 due to a mismatch in the thermal expansion coefficients of the glass substrate 11 and the build-up layer 31. On the other hand, in the sub-substrate 10A according to Example 2, the back cracking phenomenon seen in Comparative Example 2 did not occur, confirming that the coating layer 21A is effective in suppressing the occurrence of back cracking.

[0198] According to the circuit board manufacturing method of the above embodiment, since a coating agent is applied to at least the end face of the glass substrate 11 before forming the build-up layer 31 by the coating layer formation step on the glass end face (Figure 1C), the build-up layer 31 can be formed with at least the end face of the glass substrate 11 protected by the coating layer 21.

[0199] Therefore, the phenomenon of the edge surface of the glass substrate 11 being eroded by chemical treatments such as etching, resist stripping, and desmearing, which are included in the process of forming the build-up layer 31, can be prevented.

[0200] Furthermore, even if there are minute chips on the edge of the glass substrate 11, the growth of microcracks from these chips can be prevented. In addition, even if an impact is applied to the edge of the glass substrate 11 during the build-up layer 31 formation process, the occurrence of damage such as cracks due to the impact can be prevented, and dust generation from the edge of the glass substrate 11 can be suppressed. Therefore, the manufacturing yield of the circuit board 10 can be improved, and productivity can be increased.

[0201] Furthermore, according to the manufacturing method of the circuit board according to the embodiment, the glass core layer 12 formation step includes a through-via formation step (Figure 1B) and a conductive layer formation step (Figures 1D and 1E), and a coating layer formation step on the glass end face (Figure 1C) is performed to apply a coating agent to at least the end face of the glass substrate 11 before the conductive layer formation step.

[0202] Therefore, in the conductive layer formation process (Figures 1D and 1E), the end face of the glass substrate 11 is protected by the coating layer 21, and a seed layer 32 and an electroplating layer 33 are formed on the end face of the glass core layer 12 on top of the coating layer 21.

[0203] Therefore, during the conductive layer formation process, the phenomenon of erosion of the end face of the glass core layer 12 can be prevented. Furthermore, even if there are minute chips on the end face of the glass core layer 12, the growth of microcracks from these chips can be prevented.

[0204] Furthermore, even if an impact is applied to the end face of the glass core layer 12 during the conductive layer formation process, it is possible to prevent damage such as cracks caused by the impact, and to suppress dust generation from the end face of the glass core layer 12. Therefore, it is possible to improve the manufacturing yield of circuit boards having the glass core layer 12 and increase productivity.

[0205] Furthermore, according to the circuit board manufacturing method of the embodiment, in the build-up layer 31 formation step, at least the end face of the glass core layer 12 is protected by the coating layer 21, so the phenomenon of the end face of the glass core layer 12 being eroded by chemical treatments such as etching, resist stripping, and desmearing, which are included in the process of laminating the wiring layer 35 and the insulating layer 36, can be prevented.

[0206] Furthermore, even if an impact is applied to the end face of the glass core layer 12 during the build-up layer 31 formation process, it is possible to prevent damage such as cracks caused by the impact.

[0207] Furthermore, it is possible to prevent the occurrence of back cracks in the circuit board 10 during and after manufacturing. Therefore, it is possible to improve the manufacturing yield of the circuit board 10 having the glass core layer 12 and increase productivity.

[0208] Furthermore, according to the manufacturing method of the mounted substrate according to the embodiment, after the first division step (Figures 3A and 3B) and before the mounting step (Figures 3D and 3E), a coating layer formation step (Figure 3C) is performed on the end faces of the sub-substrates, in which a coating agent is applied to at least the end faces of each divided sub-substrate 10A to form a coating layer 21A.

[0209] Therefore, during the mounting process, at least the end face of each sub-substrate 10A is protected by the coating layer 21A. Consequently, even when heat treatment such as the reflow process (Figure 3E) for mounting chip components is performed during the mounting process, it is possible to prevent back cracking of the sub-substrate 10A caused by thermal history, etc. This improves the manufacturing yield of the mounted substrate 10C and increases productivity.

[0210] Furthermore, according to the manufacturing method of the mounted substrate according to the embodiment, after the second division step (Figures 3G and 3H) and before the inspection and testing step (Figure 3J), a coating layer formation step (Figure 3I) is performed on the end faces of the unit substrates, in which a coating agent is applied to at least the end faces of each divided unit substrate 10B to form a coating layer 21B.

[0211] Therefore, during the inspection and testing process, at least the end face of each unit substrate 10B is protected by the coating layer 21B. Consequently, even when reliability tests involving thermal loads are performed during the inspection and testing process (Figure 3J) of each unit substrate 10B, the occurrence of back cracks in each unit substrate 10B can be prevented. This improves the manufacturing yield of the mounted substrate 10C and increases productivity.

[0212] Furthermore, according to the manufacturing method of the mounted substrate in this embodiment, since the circuit board 10 manufactured by the above-described manufacturing method of the circuit board is used, the manufacturing yield of the mounted substrate 10C can be improved, and the effect of improving productivity can be further enhanced.

[0213] Furthermore, according to the substrate crack prevention method of this embodiment, since the coating agent is applied to at least the end face of the glass substrate 11 before forming the build-up layer 31, at least the end face of the glass substrate 11 can be protected by the coating layer 21.

[0214] Therefore, the edge protection effect of the coating layer 21 prevents the occurrence of back cracking. In addition, it is possible to prevent various types of damage such as cracks, chips, and scratches from occurring on the edge surface of the glass substrate 11.

[0215] Furthermore, according to the substrate crack prevention method of the embodiment, a coating agent is applied to at least the end face of the sub-substrate 10A obtained by dividing the circuit board 10, and to at least the end face of the unit substrate 10B obtained by dividing the sub-substrate 10A.

[0216] Therefore, at least the end face of the sub-substrate 10A can be protected by the coating layer 21A, and at least the end face of the unit substrate 10B can be protected by the coating layer 21B. The end face protection effect of these coating layers 21A and 21B prevents back cracking in the sub-substrate 10A and the unit substrate 10B. In addition, it is possible to prevent various types of damage such as cracks, chips, and scratches from occurring on the end faces of the sub-substrate 10A and the unit substrate 10B.

[0217] Figures 9A to 9G are diagrams illustrating a method for manufacturing a circuit board according to another embodiment, and schematically show a cross-sectional view of a circuit board during the manufacturing process. In the manufacturing of the circuit board 10 according to the above embodiment, the glass substrate 11 was used as the glass core layer 12 of the circuit board 10.

[0218] In the manufacturing of a circuit board according to another embodiment described below, a glass substrate is used as a glass carrier 11A that supports the semiconductor package. The glass carrier 11A is an example of a carrier material.

[0219] In a method for manufacturing a circuit board according to another embodiment, first, a glass carrier 11A is prepared as shown in Figure 9A. The glass carrier 11A is composed of a glass substrate, and may, for example, have a temporary fixing layer, a plating seed layer, etc., formed sequentially on the upper surface of the glass panel.

[0220] The temporary fixing layer may consist of an adhesion layer, a release function layer, etc. The size and shape of the glass carrier 11A are not particularly limited, but for example, it may be a square panel for panel-level packages with a diameter of 500 mm or more, or a circular panel for wafer-level packages with a diameter of about 300 mm or more. The thickness of the glass carrier 11A is not particularly limited, but from the viewpoint of ensuring support performance, it is preferably 0.5 mm or more.

[0221] Next, as shown in Figure 9B, a coating layer formation step is performed on the glass end face, in which a coating agent is applied to at least the end face of the glass carrier 11A to form a coating layer 22. If the glass carrier 11A is a rectangular panel for a panel-level package, the coating agent is applied to the end faces of all four sides between the first surface (top surface) and the second surface (bottom surface) of the glass carrier 11A to form a coating layer 22.

[0222] Furthermore, if the glass carrier 11A is a circular panel for wafer-level packaging, a coating agent is applied to the substantially circular outer peripheral end surface between the first surface (top surface) and the second surface (bottom surface) of the glass carrier 11A to form a coating layer 22.

[0223] The thickness of the coating layer 22 varies depending on the thickness of the glass carrier 11A, but is not limited to these ranges, for example, 10 μm to 300 μm, preferably 20 μm to 150 μm, and more preferably 30 μm to 100 μm.

[0224] If the cross-sectional shape of the end face of the glass carrier 11A is a right-angle edge, the coating agent may be applied so as shown in the figure that the coating layer 22 is formed only on the end face, or the coating agent may be applied so as to cover the corners of the right-angle edge (the outer peripheral edges of the upper and lower surfaces).

[0225] If the cross-sectional shape of the end face of the glass carrier 11A is a chamfered edge or a curved edge, it is preferable to apply the coating agent so as to cover the chamfered or curved portion as well. The same coating agent used in the manufacturing method of the circuit board 10 according to the above embodiment can be used.

[0226] The coating apparatus used in the process of forming a coating layer on the glass edge can be an apparatus with the same configuration as the coating apparatus 51 used in the manufacturing method of the circuit board 10 described above.

[0227] Next, as shown in Figure 9C, a redistribution layer 71 is formed on the upper surface of the glass carrier 11A on which the coating layer 22 is formed at the end face. The redistribution layer 71 is a redistribution layer for a fan-out type panel-level package, formed by repeatedly forming a resist, copper plating, removing the resist, and forming an insulating layer on the upper surface of the glass carrier 11A.

[0228] The redistribution layer 71 is a type of multilayer wiring layer. Furthermore, if the glass carrier 11A is a carrier substrate for a wafer-level package, the redistribution layer 71 may be, for example, a redistribution layer for a fan-out type wafer-level package.

[0229] After the redistribution layer 71 is formed, chip components 72 are then mounted on the redistribution layer 71, as shown in Figure 9D. The method for mounting the chip components 72 is not particularly limited and can be performed using equipment such as a chip mounter or bonder.

[0230] After mounting the chip component 72, the chip component 72 is then molded and sealed with a sealing material 73 such as resin, as shown in Figure 9E. Examples of molded sealing methods include transfer molding, compression molding, and film molding.

[0231] After mold sealing, the glass carrier 11A is then peeled off, as shown in Figure 9F, to separate the individual package circuit boards 70. Methods for peeling off the glass carrier 11A include, for example, a thermal slide method, a mechanical method, a solvent peeling method, or a laser peeling method.

[0232] Of these methods, the laser delamination method is preferred because it allows delamination at room temperature and under low mechanical stress, and also offers faster throughput compared to other methods. In the laser delamination method, for example, delamination can be achieved by irradiating the glass carrier 11A with laser light and decomposing the material of the temporary fixing layer by ablation. The laser light may be a short-wavelength laser or a long-wavelength laser, and a UV laser is preferred from the viewpoint of suppressing thermal effects on the chip component 72.

[0233] In the manufacturing method of the packaged circuit board 70 according to the other embodiment described above, the coating agent is applied to at least the end face of the glass carrier 11A before the redistribution layer 71 is formed by the coating layer formation step on the glass end face.

[0234] By performing this coating layer formation process on the glass end face, in the subsequent processes after the redistribution layer 71 is formed, the end face of the glass carrier 11A is protected by the coating layer 22.

[0235] Therefore, it is possible to prevent the growth of microcracks from minute chipping on the end face of the glass carrier 11A. Furthermore, even if the glass carrier 11A is subjected to impact during processes such as the mounting process of the chip component 72 or the mold sealing process, it is possible to prevent the occurrence of cracks caused by such impact, improve the peelability of the glass carrier 11A, and further suppress dust generation from the end face of the glass carrier 11A.

[0236] Therefore, the manufacturing yield of the packaged circuit board 70 at the panel level and the packaged circuit board 70 at the wafer level can be improved, thereby increasing productivity.

[0237] Figures 10A to 10D illustrate a manufacturing method for a circuit board according to yet another embodiment, schematically showing a cross-sectional view of a circuit board during the manufacturing process. In this alternative embodiment of the circuit board manufacturing method, first, as shown in Figure 10A, a glass substrate 11 is prepared, and then, as shown in Figure 10B, a process is carried out to form a plurality of through vias 13 on the glass substrate 11. The process shown in Figures 10A and 10B is basically the same as the process shown in Figures 1A and 1B.

[0238] In the manufacturing method of the circuit board 10 according to the above embodiment, the next step is to form a coating layer on the glass edge, as shown in Figure 1C. However, in the manufacturing method of the circuit board according to this other embodiment, as shown in Figure 10C, a plasma irradiation step is performed in which plasma is irradiated onto at least the edge of the glass substrate 11 before the coating layer formation step on the glass edge shown in Figure 10D.

[0239] The plasma irradiation process to the glass end face shown in Figure 10C is carried out, for example, using a plasma generator 90. It is preferable to use, for example, one or more atmospheric pressure plasma devices as such a plasma generator 90. Examples of such atmospheric pressure plasma devices include dielectric barrier discharge (DBD) type, atmospheric pressure plasma jet (APPJ) type, inductively coupled plasma (ICP), and piezoelectric direct discharge (PDD) type plasma devices.

[0240] For example, a DBD-type atmospheric pressure plasma apparatus is configured to generate a plasma by applying a predetermined voltage between a dielectric and metal electrodes facing each other across a space, then introducing a process gas such as oxygen into the generated plasma, and releasing the plasma-like gas from an emission section to irradiate at least the edge face of a glass substrate 11.

[0241] The shape of the discharge section is preferably, for example, a slit shape or a nozzle shape. The plasma generator 90 can be arranged so as to face the four end faces of the glass substrate 11, or one or more plasma generators 90 can be moved along the end face of the glass substrate 11.

[0242] After the plasma irradiation process on the glass edge is completed, the next step is to form a coating layer on the glass edge as shown in Figure 10D. The process of forming a coating layer on the glass edge as shown in Figure 10D is basically the same as the process shown in Figure 1C, so its explanation will be omitted. Subsequently, by performing the same processes as shown in Figures 1D to 1K, it is possible to manufacture a circuit board in which a build-up layer 31 is formed on the glass core layer 12.

[0243] According to the manufacturing method of the circuit board according to yet another embodiment described above, the surface of the end face of the glass substrate 11 can be modified by performing a plasma irradiation step (Figure 10C) before the coating layer formation step (Figure 10D) on the glass end face.

[0244] For example, active oxygen and ozone in the plasma irradiated from the plasma generator 90 can decompose and remove dust, oil, organic matter, etc., adhering to the edge surface of the glass substrate 11. Furthermore, the hydrophilicity of the edge surface of the glass substrate 11 can be improved. Therefore, the adhesion and wettability of the coating agent in the subsequent coating layer formation process on the glass edge surface can be improved.

[0245] Furthermore, in the method for manufacturing the package circuit board 70 according to another embodiment described with reference to Figures 9A to 9G, a plasma irradiation step may be performed before the coating layer formation step on the glass end face shown in Figure 9B, in which plasma is irradiated onto at least the end face of the glass carrier 11A using one or more plasma generators 90.

[0246] By applying a plasma irradiation process, the surface of the end face of the glass carrier 11A can be modified, achieving the same effects as described above and further enhancing the yield of the package circuit board 70.

[0247] Furthermore, in the manufacturing method of the mounting substrate according to the embodiment described with reference to Figures 3A to 3K, a plasma irradiation step may be performed using one or more plasma generators 90 to irradiate at least the end face of the sub-substrate 10A with plasma before the coating layer formation step on the end face of the sub-substrate shown in Figure 3C.

[0248] Furthermore, prior to the coating layer formation process on the end face of the unit substrate shown in Figure 3I, a plasma irradiation process may be performed using one or more plasma generators 90 to irradiate at least the end face of the unit substrate 10B with plasma.

[0249] In this method for manufacturing a mounting substrate, the surface of the sub-substrate 10A can be modified by applying a plasma irradiation process to the end face of the sub-substrate, and the surface of the unit substrate 10B can be modified by applying a plasma irradiation process to the end face of the unit substrate 10B. Therefore, the same effects as described above can be obtained, and the effect of improving the yield of the mounting substrate 10C can be further enhanced.

[0250] Figures 11A and 11B illustrate a modified example of the coating layer formation process on the glass edge in the manufacturing method of a circuit board according to the embodiment, and schematically show a partial plan view of the peripheral edge of a glass substrate during the manufacturing process.

[0251] The process of forming a coating layer on a glass edge, as described with reference to Figure 1C, involved applying a coating agent to at least the edge of the glass substrate 11 using a coating device 51 to form a coating layer 21. In contrast, the process of forming a coating layer on a glass edge according to this modified example is characterized by including a spraying step in which, after applying a coating agent to the peripheral edge of the glass substrate 11, a gas having directionality toward the outer periphery of the substrate (edge ​​side) is sprayed onto the coating agent to spread it to the edge side.

[0252] First, in the process of forming a coating layer on the glass end face according to this modified example, as shown in Figure 11A, a step of applying a coating agent to the peripheral edge of the glass substrate 11 is performed. Note that the coating agent may be applied to the end face prior to application to the peripheral edge of the glass substrate 11, or the coating agent may be applied to the end face after the application to the peripheral edge and the spraying process. In other words, the timing of the application process to the end face is not particularly limited.

[0253] The step of applying the coating agent to the peripheral edge of the glass substrate 11 is performed using the coating apparatus 51 described above. The type of coating apparatus 51 is not particularly limited, but from the viewpoint of applying the coating agent to a large substrate such as the glass substrate 11 with high throughput and high positional accuracy, it is preferable to use a dispenser, which is a non-contact coating apparatus. When using a dispenser, a coating area of ​​a predetermined width is formed by continuously dispensing droplets of the coating agent along the peripheral edge to form a droplet row. This is the same as the coating method described earlier, so the explanation will be omitted.

[0254] In a coating process using a dispenser, if the process is controlled to directly land droplets on the edge (near the edge) of the glass substrate 11, there is a risk that the droplets may scatter outside the substrate due to variations in droplet flight stability and landing position accuracy. Therefore, in this coating process, as shown in Figure 11A, when applying the coating agent to the peripheral edge of the glass substrate 11, the coating is performed in such a way that an uncoated area 14 is intentionally left along the edge.

[0255] The width of the uncoated area 14 can be set to, for example, several tens of micrometers. By forming the uncoated area 14 in this way, droplet scattering during the coating process can be suppressed, while securing a margin area for stably moving the coating agent toward the end face in the subsequent spraying process.

[0256] In the spraying process following the coating process, as shown in Figure 11B, a gas directional towards the uncoated area 14 (towards the outer periphery of the substrate) is sprayed onto the coating agent applied to the peripheral edge of the glass substrate 11, thereby moving the coating agent towards the outer periphery.

[0257] In this spraying process, an air nozzle section 54 having an outlet 54a that discharges a gas (for example, air) in a flat (strip-shaped) manner is used. The air nozzle section 54 is an example of a gas discharge means. The shape of the outlet 54a is not limited to a narrow slit shape, but may also be a porous shape with multiple minute discharge holes arranged in a row, making it possible to form an airflow with a substantially uniform flow velocity distribution in the width direction.

[0258] Furthermore, the discharge port 54a is not limited to a configuration in which the gas is discharged in a flat shape. For example, the gas may be discharged from a circular or elliptical discharge port, or the airflow may be given directionality by a flow straightening structure inside the nozzle. In addition, a deflection member or guide member may be provided at the discharge port to control the spread angle and flow direction of the airflow after discharge. Moreover, a configuration in which multiple discharge ports are combined may be used to give directionality to the airflow.

[0259] The air nozzle section 54 is configured, for example, integrally with a dispenser, and this integrated device is made movable in multiple axes by a multi-axis movement mechanism provided on the coating device 51, thereby enabling continuous scanning along the periphery of the glass substrate 11. In this case, the coating device 51 is configured to include a dispenser (droplet dispensing section) that dispenses droplets of coating agent and an air nozzle section 54 that generates a band-shaped airflow.

[0260] In the spraying process, the air nozzle 54 is positioned such that the longitudinal direction of the discharge port 54a is oblique to the edge of the glass substrate 11, and the main flow direction of the gas discharged from the discharge port 54a (direction of arrow A in the figure) is toward the edge of the glass substrate 11. In this configuration, by spraying gas while relatively moving the air nozzle 54 along the peripheral edge of the glass substrate 11, it is possible to continuously apply a shear flow that spreads toward the edge of the substrate to the coating agent.

[0261] The angle between the longitudinal direction of the discharge port 54a and the edge of the glass substrate 11 is set to an acute angle, for example, in the range of 10 to 70 degrees, preferably 30 to 60 degrees. This creates an airflow that has both an outer peripheral component and a circumferential component, making it possible to achieve both stable outer peripheral movement of the coating agent and in-plane leveling. The same coating and spraying processes can also be performed on the lower peripheral edge of the glass substrate 11.

[0262] According to the circuit board manufacturing method of the modified example described above, a spraying step is added to the coating layer formation step on the glass edge, and an airflow with directionality toward the substrate edge is applied to the coating agent after application.

[0263] In particular, by positioning the discharge port 54a diagonally with respect to the edge of the glass substrate 11 and setting the discharge direction toward the edge (direction of arrow A), and then moving it relative to the peripheral edge, the band-shaped airflow acts uniformly over the width of the coating agent, allowing the coating agent to spread toward the outer periphery while flowing and leveling within the surface.

[0264] This suppresses variations in film thickness and the occurrence of uncoated areas at the periphery, enabling the formation of a uniform coating layer 21 with excellent appearance quality. Furthermore, even when an uncoated area 14 remains, the flow of the coating agent can be actively controlled by the spraying process, ensuring stable coating quality without excessive reliance on droplet placement accuracy or discharge conditions during application.

[0265] Furthermore, in the manufacturing method of the package circuit board 70 according to another embodiment described with reference to Figures 9A to 9G, the coating layer formation step on the glass end face shown in Figure 9B may be configured to include a spraying step in which, after applying a coating agent to the peripheral edge of the glass carrier 11A, a gas having directionality toward the end side (outer circumference) is sprayed onto the coating agent.

[0266] In the coating layer formation process on the glass edge shown in Figure 9B, by performing a spraying process after application, the coating agent can be stably moved toward the edge, and, as in the embodiment described above, effects such as uniformity of the coating state from the periphery to the edge, suppression of uncoated areas, and improvement of appearance quality can be obtained.

[0267] Furthermore, in the manufacturing method of the mounted substrate according to the embodiment described with reference to Figures 3A to 3K, with regard to the coating layer formation step on the end face of the sub-substrate shown in Figure 3C, a spraying step may be applied in which, after applying a coating agent to the peripheral edge of the sub-substrate 10A, a gas directional in the direction along the peripheral edge is sprayed onto the coating agent.

[0268] Figures 12A to 12C illustrate a modified example of the coating layer formation process on the sub-substrate edge in the manufacturing method of a mounted substrate according to the embodiment, and schematically show a partial plan view of the peripheral edge of the sub-substrate during manufacturing. In the coating layer formation process on the sub-substrate edge according to this modified example, as shown in Figure 12A, a step of applying a coating agent to the peripheral edge of the sub-substrate 10A is performed.

[0269] The coating of the peripheral edge of the sub-substrate 10A can be performed using a coating apparatus 51 equipped with the dispenser and air nozzle 54 described above. When using the dispenser, a coating area of ​​a predetermined width is formed by continuously dispensing droplets of the coating agent along the peripheral edge to form a droplet row. This is the same as the method described above, so its explanation will be omitted.

[0270] In the dispensing process using a dispenser, if the droplets are controlled to land directly near the boundary between the glass core layer 12 and the build-up layer 31, the droplets may diffuse unstably due to differences in height and material, potentially scattering onto the build-up layer 31. Similarly, at the edges of the glass core layer 12, variations in droplet placement may cause them to scatter outside the substrate.

[0271] Therefore, in this coating process, as shown in Figure 12A, when applying the coating agent to the peripheral edge of the sub-substrate 10A, the coating is applied in such a way that an uncoated area 14 along the edge of the glass core layer 12 and an uncoated area 15 along the boundary of the build-up layer 31 are left uncoated.

[0272] The width of the uncoated areas 14 and 15 can be set to, for example, several tens of micrometers. This suppresses droplet scattering during the coating process and ensures a control margin to stably move the coating agent in the desired direction during the subsequent spraying process.

[0273] In the spraying step following the coating step, as shown in Figures 12B and 12C, a gas directional in the direction along the peripheral edge of the sub-substrate 10A is sprayed onto the coating agent, causing the coating agent to flow within the surface. In this spraying step, as described above, an air nozzle section 54 having a discharge port 54a that discharges gas (for example, air) in a strip shape is used.

[0274] In the spraying process shown in Figure 12B, gas is sprayed so that the coating agent spreads toward the stepped portion 16 formed at the boundary between the glass core layer 12 and the build-up layer 31. Specifically, the air nozzle portion 54 is positioned such that the longitudinal direction of the discharge port 54a is oblique to the stepped portion 16, and the main direction of the discharged gas (direction of arrow A in the figure) is toward the stepped portion 16.

[0275] Then, in this configuration, by blowing gas while relatively moving the air nozzle 54 along the periphery of the sub-substrate 10A, a continuous shear flow in the direction of the stepped portion is applied to the coating agent.

[0276] Furthermore, in the spraying process shown in Figure 12C, gas is sprayed to move the coating agent toward the edge of the sub-substrate 10A. In this case, the air nozzle 54 is positioned such that the longitudinal direction of the discharge port 54a is oblique to the edge of the sub-substrate 10A, and the direction of gas discharge (direction of arrow A in the figure) is toward the edge.

[0277] Then, in this configuration, by blowing gas while relatively moving the air nozzle 54 along the periphery of the sub-substrate 10A, a continuous shear flow in the edge direction is applied to the coating agent. The same coating and spraying processes can also be performed on the periphery of the lower surface of the sub-substrate 10A.

[0278] According to the manufacturing method of the mounted substrate described above, in the process of forming a coating layer on the edge face of the sub-substrate, the flow direction of the coating agent can be controlled in stages by combining two spraying steps. Specifically, the spraying step directed toward the stepped portion 16 draws the coating agent towards the stepped portion 16 and smooths it out, and then the spraying step directed toward the edge smooths the coating agent while stretching it in the direction of the edge face.

[0279] This ensures uniformity of the film thickness distribution in the region from the stepped portion 16 to the end face, effectively suppressing uneven coating and missed areas. As a result, it is possible to improve the quality and appearance of the coating layer 21. Furthermore, by adjusting the position of the air nozzle portion 54 and the orientation of the discharge port 54a, it is also possible to evenly distribute the coating agent towards the stepped portion 16 and the end face using only a spraying process directed towards the stepped portion 16.

[0280] Furthermore, in the coating layer formation process on the end face of the unit substrate shown in Figure 3I, similar to the above, a spraying process can be applied in which a coating agent is applied to the peripheral edge of the unit substrate 10B, and then a gas directional in the direction along the peripheral edge is sprayed onto the coating agent.

[0281] This allows for active control of the flow state of the coating agent after application, enabling the formation of a uniform coating layer 21. Furthermore, the above-described embodiment is applicable not only to glass substrates but also to the manufacture of various circuit boards and mounted substrates having substrates made of other materials and multilayer wiring layers formed thereon, and is effective for a wide range of substrate structures.

[0282] Although embodiments of the present invention have been described in detail above, the above description is merely illustrative of the present invention. It goes without saying that various improvements and modifications can be made without departing from the scope of the present invention, and these are also included within the scope of the present invention.

[0283] This invention has broad applicability in fields such as the electronic circuit board industry and the electronic equipment industry, which handle various types of substrates, such as circuit boards and mounting boards, that use glass as a base material or carrier material.

[0284] 10 Circuit board (glass core substrate) 10A Sub-sub 90 Plasma generator 200 Glass circuit board 201 Glass core 202 Build-up layer 205 Circuit layer 207 First insulating resin layer 210 Second insulating resin layer

Claims

1. A method for manufacturing a circuit board having a glass substrate and a laminated wiring layer formed on top of the glass substrate, characterized in that it comprises a coating layer forming step of forming a coating layer on at least the end face of the glass substrate before forming the laminated wiring layer.

2. The method for manufacturing a circuit board according to claim 1, characterized in that the glass substrate includes a glass core layer having one or more glass layers, the laminated wiring layer includes a build-up layer in which a wiring layer and an insulating layer are laminated, the glass core layer formation step includes a through-via formation step of forming through-vias in the glass core layer, and a conductive layer formation step of forming a conductive layer on the glass core layer in which the through-vias have been formed, and the coating layer formation step on the glass end face is performed before the conductive layer formation step.

3. The method for manufacturing a circuit board according to claim 2, characterized in that the build-up layer formation step is performed after the glass core layer formation step, on the surface of the glass core layer on which the conductive layer is formed, in which the coating layer has been formed at least on the end face.

4. The method for manufacturing a circuit board according to claim 1, characterized in that the glass substrate includes a glass carrier which serves as a carrier material for a wafer-level package or a panel-level package, the multilayer wiring layer includes a redistribution layer for the wafer-level package or the panel-level package, and the step of forming a coating layer on the glass edge is performed before forming the redistribution layer.

5. The method for manufacturing a circuit board according to any one of claims 1 to 4, characterized in that a plasma irradiation step is performed in which plasma is irradiated onto at least the end face of the glass substrate before the step of forming a coating layer on the glass end face.

6. The method for manufacturing a circuit board according to any one of claims 1 to 4, characterized in that the step of forming a coating layer on the glass end face includes a spraying step of applying a coating agent to the peripheral edge of the glass substrate and then spraying a gas in a directional manner so that the coating agent spreads toward the edge of the glass substrate.

7. The method for manufacturing a circuit board according to claim 6, characterized in that the spraying step is a step of spraying gas using a gas discharge means equipped with a discharge port for discharging the gas, while moving the gas discharge means relative to the peripheral edge of the glass substrate, such that the gas discharged from the discharge port flows to the edge side of the glass substrate.

8. A method for manufacturing a mounted substrate on which chip components are mounted using a glass core substrate having a glass core layer having one or more glass layers and a build-up layer formed on top of the glass core layer, comprising: a first division step of dividing the glass core substrate into a plurality of sub-substrates; and a mounting step of mounting the chip components on each of the divided sub-substrates, wherein a coating layer formation step is performed after the first division step and before the mounting step, in which a coating layer is formed on at least the end face of each of the divided sub-substrates.

9. The method for manufacturing a mounting substrate according to claim 8, characterized in that a plasma irradiation step is performed in which plasma is irradiated onto at least the end face of the sub-substrate before the step of forming a coating layer on the end face of the sub-substrate.

10. The method for manufacturing a mounting substrate according to claim 8 or 9, characterized in that the step of forming a coating layer on the end face of the sub-substrate includes a spraying step of applying a coating agent to the peripheral edge of the sub-substrate and then spraying a gas so that the coating agent spreads in a directional manner along the peripheral edge of the sub-substrate.

11. The method for manufacturing a mounting substrate according to claim 10, characterized in that the spraying step includes a step of spraying gas such that the coating agent applied to the peripheral edge of the sub-substrate spreads toward the edge of the sub-substrate.

12. The method for manufacturing a mounting substrate according to claim 10, characterized in that the spraying step includes a step of spraying gas such that the coating agent applied to the peripheral edge of the sub-substrate spreads toward the stepped portion formed at the boundary between the glass core layer and the build-up layer.

13. A method for manufacturing a mounted substrate according to claim 8, comprising: a second division step of dividing the sub-sub 14. The method for manufacturing a mounting substrate according to claim 13, characterized in that a plasma irradiation step is performed in which plasma is irradiated onto at least the end face of the unit substrate before the step of forming a coating layer on the end face of the unit substrate.

15. The method for manufacturing a mounting substrate according to claim 13 or 14, characterized in that the step of forming a coating layer on the end face of the unit substrate includes a spraying step of applying a coating agent to the peripheral edge of the unit substrate and then spraying a gas so that the coating agent spreads in a directional manner along the peripheral edge of the unit substrate.

16. The method for manufacturing a mounting substrate according to claim 8 or claim 13, characterized in that the glass core substrate is a circuit board manufactured by the method for manufacturing a circuit board according to claim 2 or claim 3.

17. A method for preventing back cracking of a substrate, which is a fracture in which the glass substrate peels off toward the laminated wiring layer due to a mismatch in the coefficient of thermal expansion between the glass substrate and the laminated wiring layer formed on top of the glass substrate, characterized in that a coating layer is formed on at least the end face of the glass substrate before the laminated wiring layer is formed.

18. The method for preventing back cracking of a substrate according to 17, characterized in that the glass substrate includes a glass core layer having one or more glass layers, the laminated wiring layer includes a build-up layer in which a wiring layer and an insulating layer are laminated, and the coating layer is formed on at least the end face of a sub-substrate obtained by dividing the glass core substrate having the glass core layer and the build-up layer, and / or on at least the end face of a unit substrate obtained by dividing the sub-substrate.

19. A substrate coating method comprising: a coating step of applying a coating agent to at least the edge face of a substrate; and a spraying step of blowing a gas after the coating step so that the coating agent spreads in a directional manner along the peripheral edge of the substrate.

20. The substrate coating method according to 19, characterized in that the coating step includes a step of applying the coating agent to the peripheral edge of the substrate such that an uncoated area is left along the edge of the substrate, and the spraying step includes a step of spraying gas such that the coating agent applied to the peripheral edge of the substrate spreads in a directional manner toward the uncoated area.

21. The substrate coating method according to claim 19 or 20, characterized in that the coating step includes a step of applying the coating agent to the peripheral edge of the substrate by continuously discharging droplets of the coating agent to form a droplet row, and the spraying step is a step of using a gas discharge means equipped with a gas discharge port for discharging the gas, and spraying the gas while relatively moving the gas discharge means along the peripheral edge of the substrate, such that the gas discharged from the discharge port flows towards the edge of the substrate.