Polycrystalline diamond and tool
By segregating boron in the grain boundaries of polycrystalline diamond within a specific atomic concentration range, the tool's oxidation resistance and hardness are significantly improved, addressing the limitations of existing polycrystalline diamond tools.
Patent Information
- Application Number
- PCT/JP2026/017368
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
Existing polycrystalline diamond tools suffer from inadequate oxidation resistance, which limits their tool life and performance in high-temperature conditions.
The polycrystalline diamond is engineered with a specific boron content of 1.0 × 10¹⁶ /cm³ to 1.0 × 10²² /cm³, segregating boron in the grain boundary regions between adjacent diamond crystal grains, ensuring improved oxidation resistance and maintaining hardness.
The solution enhances the oxidation resistance and hardness of the polycrystalline diamond, providing improved tool performance and longevity by minimizing boron clustering and reducing oxygen content in the grain boundaries.
Smart Images

Figure JP2026017368_12112026_PF_FP_ABST
Abstract
Description
Polycrystalline Diamond and Tool
[0001] The present disclosure relates to polycrystalline diamond and a tool. This application claims priority based on Japanese Patent Application No. 2025-078007 filed on May 8, 2025. The entire contents described in the Japanese patent application are incorporated herein by reference.
[0002] Development of techniques for imparting various properties such as electrical conductivity to diamond by adding an element other than carbon (for example, boron) to insulating polycrystalline diamond has been progressing.
[0003] Patent Document 1 discloses polycrystalline diamond in which a first element such as boron is dispersed by subjecting graphite containing boron to high-temperature and high-pressure treatment to convert graphite into diamond, and a cutting tool including the same.
[0004] Japanese Unexamined Patent Publication No. 2013-28498
[0005] In the polycrystalline diamond of the present disclosure, the content of boron on an atomic number basis is 1.0×10 16 / cm 3 or more and 1.0×10 22 / cm 3 or less, the polycrystalline diamond includes a plurality of diamond crystal grains, and boron is segregated in a grain boundary region between adjacent diamond crystal grains.
[0006] FIG. 1 is an example of a first image of the polycrystalline diamond according to Embodiment 1. FIG. 2 is an example of a second image of the polycrystalline diamond according to Embodiment 1. FIG. 3 is an example of a first graph obtained for the polycrystalline diamond according to Embodiment 1. FIG. 4 is a perspective view showing an example of a state where graphite is formed on a base material. FIG. 5 is a perspective view showing an example of a state where polycrystalline diamond is produced by directly converting graphite on the base material.
[0007] In recent years, the demand for improvement in tool life has been increasing more and more. As one of the measures for improving tool life, improvement in oxidation resistance of polycrystalline diamond used as a cutting edge material is conceivable.
[0008] Therefore, this disclosure aims to provide polycrystalline diamond and tools with improved oxidation resistance.
[0009] According to this disclosure, it is possible to provide polycrystalline diamond and tools with improved oxidation resistance.
[0010] [Description of Embodiments of the Disclosure] First, embodiments of the Disclosure will be listed and described. (1) The polycrystalline diamond of the Disclosure has a boron content of 1.0 × 10¹ 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following is a polycrystalline diamond, wherein the polycrystalline diamond contains multiple diamond crystal grains, and boron is segregated in the grain boundary regions between adjacent diamond crystal grains.
[0011] According to this disclosure, it is possible to provide polycrystalline diamond with improved oxidation resistance. This is presumed to be because the presence of boron on the surface of the diamond crystal grains improves the oxidation resistance of the polycrystalline diamond.
[0012] (2) In the above (1), the diamond crystal grains include a first diamond crystal grain and a second diamond crystal grain that are adjacent to each other. In an elemental mapping image of boron obtained by observing a cross section of the polycrystalline diamond with an electron energy loss spectrometer attached to a transmission electron microscope, from a measurement start point X1 provided inside the first diamond crystal grain to a measurement end point X2 provided inside the second diamond crystal grain, along a direction perpendicular to the grain boundary between the first diamond crystal grain and the second diamond crystal grain, a first graph showing the result obtained by line extraction from the elemental mapping image of boron in a coordinate system where the X-axis is the distance from the measurement start point X1 and the Y-axis is the atomic concentration of boron may satisfy the following Condition 1 to Condition 4. Condition 1: There exists a maximum value A of the atomic concentration of boron. Condition 2: The atomic concentration of boron monotonically decreases from the distance P1 of the maximum value A to a distance P2 that is 1.5 nm away from the distance P1 toward the origin side of the first graph. Condition 3: The atomic concentration of boron monotonically decreases from the distance P1 of the maximum value A to a distance P3 that is 1.5 nm away from the distance P1 toward the side opposite to the origin of the first graph. Condition 4: The average B of the atomic concentration of boron in the first region between the distance P2 and the distance P3 is greater than the average C of the atomic concentration of boron in the second region between the distance P2 and a distance P4 that is 5 nm away from the distance P2 toward the origin side of the first graph, and in the third region between the distance P3 and a distance P5 that is 5 nm away from the distance P3 toward the side opposite to the origin of the first graph.
[0013] According to this, the oxidation resistance of the polycrystalline diamond is further improved.
[0014] (3) In the above (1) or (2), the content of the polycrystalline diamond on an atomic number basis of oxygen may be 1.0×10 18 / cm 3 or less. The content of the oxygen in the polycrystalline diamond on an atomic number basis is measured by secondary ion mass spectrometry. According to this, the oxidation resistance of the polycrystalline diamond is further improved.
[0015] (4) In any of (1) to (3) above, the oxygen content in the grain boundary region may be below the detection limit when measured by electron energy loss spectroscopy using a transmission electron microscope. This further improves the oxidation resistance of polycrystalline diamond.
[0016] (5) In any of (1) to (4) above, the average grain size of the diamond crystal grains may be 10 nm or more and 50,000 nm or less. The lower limit of the average grain size of the diamond crystal grains may be 10 nm or more from a manufacturing standpoint. When the average grain size of the diamond crystal grains is 50,000 nm or less, the hardness of the polycrystalline diamond tends to be higher.
[0017] (6) In any of (1) to (5) above, the Knoop hardness of the polycrystalline diamond may be 50 GPa or higher. The Knoop hardness is measured in accordance with JIS Z 2251:2009 at a temperature of 18°C to 28°C and a test load of 4.9 N.
[0018] According to this, polycrystalline diamond can possess excellent hardness.
[0019] (7) In any of (1) to (6) above, the volume resistivity of the polycrystalline diamond may be 1 mΩ·cm or more and 1000 Ω·cm or less. The volume resistivity is measured at 20°C or more and 25°C or less in accordance with JIS C2141-1992. Here, 1 mΩ·cm is 1 × 10⁻⁶ -3 It is synonymous with Ω·cm.
[0020] If the volume resistivity of polycrystalline diamond is 1 mΩ·cm or higher, it will not behave as a metal, but it will maintain hardness while possessing conductivity. If the volume resistivity of polycrystalline diamond is 1000 Ω·cm or lower, it becomes possible to prevent wear caused by static electricity.
[0021] (8) In any of (1) to (7) above, the polycrystalline diamond may consist of diamond crystal grains, boron, and unavoidable impurities. This further improves the performance of the tool comprising the polycrystalline diamond.
[0022] (9) The tools of this disclosure are tools comprising polycrystalline diamond as described in any of (1) to (8) above. The tools may have excellent oxidation resistance.
[0023] [Details of Embodiments of the Disclosure] Specific examples of polycrystalline diamond and tools of the Disclosure will be described below with reference to the drawings. In the drawings of the Disclosure, the same reference numerals indicate the same or corresponding parts. In addition, dimensional relationships such as length, width, thickness, and depth have been modified as appropriate for clarity and simplification of the drawings and do not necessarily represent actual dimensional relationships.
[0024] In this specification, the notation "A to B" means A or greater and B or less. If no unit is specified for A, but a unit is specified only for B, then the unit for A and the unit for B are the same.
[0025] In this specification, when compounds and other elements are represented by chemical formulas, unless otherwise specified, the atomic ratios should include all conventionally known atomic ratios and should not necessarily be limited to those within the stoichiometric range.
[0026] In this disclosure, if one or more numerical values are listed as the lower and upper limits of a numerical range, any combination of any one numerical value listed as the lower limit and any one numerical value listed as the upper limit shall also be disclosed.
[0027] In this disclosure, “equipment,” “includes,” “possesses,” and variations thereof are open-ended terms. Open-ended terms may or may not include additional elements in addition to the essential elements. The statement “consists of” is a closed term. However, even a configuration expressed in closed terms may include additional elements that are usually incidental or irrelevant to the subject technology.
[0028] [Embodiment 1: Polycrystalline Diamond] The polycrystalline diamond according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") has a boron content on an atomic basis of 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following is a polycrystalline diamond, wherein the polycrystalline diamond contains multiple diamond crystal grains, and boron is segregated in the grain boundary regions between adjacent diamond crystal grains.
[0029] <Structure and Composition> The polycrystalline diamond of Embodiment 1 is a polycrystalline material composed of multiple diamond crystal grains. That is, the polycrystalline diamond has diamond crystal grains as its basic composition and does not contain a metallic bonding phase (binder). Therefore, the polycrystalline diamond possesses extremely high hardness and strength. Furthermore, even under high-temperature conditions, the polycrystalline diamond does not experience deterioration of mechanical properties or grain shedding due to differences in thermal expansion coefficients with the binder or catalytic action of the binder.
[0030] The polycrystalline diamond of Embodiment 1 is a polycrystalline body composed of multiple diamond crystal grains. Therefore, the polycrystalline diamond does not have the directionality (anisotropy) and cleavage of a single crystal, and has isotropic hardness and wear resistance in all directions.
[0031] The boron content of the polycrystalline diamond of Embodiment 1, based on the number of atoms, is 1.0 × 10⁻¹⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following applies: The lower limit of the boron content in polycrystalline diamond, based on the number of atoms, is 1.0 × 10¹⁶, from the viewpoint of improving oxidation resistance. 16 / cm 3 That is all, 1.0 × 10 17 / cm 3 The above is also acceptable, 1.0 × 10 19 / cm 3 The above is also acceptable, or 1.0 × 10 20 / cm 3 The above is also acceptable. The upper limit of the boron content in polycrystalline diamond, based on the number of atoms, is 1.0 × 10¹⁶, from the perspective of maintaining hardness. 22 / cm 3 The following is true: 1.0 × 10 21 / cm 3 The following is also acceptable: 8.0 x 10 20 / cm 3The following is also acceptable, or 6.0 x 10 20 / cm 3 The following is also acceptable: The boron content of polycrystalline diamond, based on the number of atoms, is 1.0 × 10⁻¹⁶. 17 / cm 3 The above 1.0 x 10 21 / cm 3 The following is also acceptable: 1.0 × 10 19 / cm 3 The above 8.0 x 10 20 / cm 3 The following is also acceptable, or 1.0 × 10 20 / cm 3 The above 6.0 x 10 20 / cm 3 The following is also acceptable.
[0032] The oxygen content of the polycrystalline diamond of Embodiment 1, based on the number of atoms, is 3.0 × 10¹⁶, from the viewpoint of improving oxidation resistance. 18 / cm 3 The following is also acceptable: 1.5 × 10 18 / cm 3 The following is also acceptable: 1.0 × 10 18 / cm 3 The following is also acceptable: 1.5 × 10 17 / cm 3 The following is also acceptable, or 1.5 × 10 17 / cm 3 The following is also acceptable. The oxygen content in polycrystalline diamond, based on the number of atoms, is preferable to be as low as possible, and may be below the detection limit by secondary ion mass spectrometry. This oxygen falls under the category of unavoidable impurities, as described later.
[0033] The polycrystalline diamond of Embodiment 1 may contain unavoidable impurities, as long as the effects of the present disclosure are not impaired. Examples of unavoidable impurities include hydrogen, oxygen, nitrogen, alkali metal elements (lithium (Li), sodium (Na), potassium (K), etc.) and alkaline earth metal elements (calcium (Ca), magnesium (Mg), etc.). In the polycrystalline diamond of Embodiment 1, the content of each element that is an unavoidable impurity may be 0% by mass or more and 0.01% by mass or less. In the polycrystalline diamond of Embodiment 1, the total content of unavoidable impurities may be 0.05% by mass or less.
[0034] The boron content (based on atomic number) of polycrystalline diamond, the oxygen content (based on atomic number) of polycrystalline diamond, and the content of unavoidable impurities in polycrystalline diamond are measured by secondary ion mass spectrometry (SIMS). The SIMS conditions are, for example, using a "CAMECA IMS-7f" instrument (manufactured by AMETEK), and the primary ion species Cs + The primary acceleration voltage is 16.0 kV, and the detection area is φ30 μm.
[0035] In the polycrystalline diamond of Embodiment 1, at least a portion of the boron is doped into the crystalline structure composed of carbon. The polycrystalline diamond of Embodiment 1 may contain carbon and boron doped into the crystalline structure composed of carbon. The polycrystalline diamond of Embodiment 1 may contain carbon, boron doped into the crystalline structure composed of carbon, and unavoidable impurities. The polycrystalline diamond of Embodiment 1 may consist of carbon, boron doped into the crystalline structure composed of carbon, and unavoidable impurities.
[0036] In this disclosure, "boron doped into the crystal structure" refers to a state in which boron exists in a state in which some of the carbon atoms are replaced and dispersed within the crystal structure of diamond, which is composed of covalent bonds between carbon atoms.
[0037] The polycrystalline diamond of Embodiment 1 may be in a form that includes boron clustered within the crystal structure, as long as it does not impair the effects of the present disclosure.
[0038] "Clustered boron within the crystal structure" refers to a state in which multiple boron atoms exist within the crystal structure in an aggregated form. When polycrystalline diamond contains clustered boron within its crystal structure, the boron is unevenly distributed within the crystal structure, which reduces the homogeneity of the polycrystalline diamond and may degrade the performance of the tool material made from it. Furthermore, it can cause significant distortion in the crystal structure, potentially reducing the hardness of the polycrystalline diamond. Therefore, the less clustered boron there is within the crystal structure of the polycrystalline diamond, the better the performance of the tool material made from it. The polycrystalline diamond of Embodiment 1 does not necessarily have to contain clustered boron.
[0039] In the X-ray diffraction pattern of the polycrystalline diamond of Embodiment 1, the ratio of peak intensities originating from other crystal structures to peak intensities originating from the carbon crystal structure may be 0.0001 or less. In this case, the proportion of other crystalline phases in the polycrystalline diamond, such as the boron crystal phase, is sufficiently reduced, resulting in good performance for the tool material made of the polycrystalline diamond.
[0040] In polycrystalline diamond, whether or not boron is doped into the crystal structure can be confirmed, for example, by (1) observing whether or not a boron crystalline phase exists in the polycrystalline diamond, by (2) measuring the distribution of the boron content on an atomic basis in the polycrystalline diamond, or by appropriately combining (1) and (2) above.
[0041] Regarding (1) above, boron doped within the crystal structure does not constitute a different crystalline phase from that of diamond. Therefore, if all the boron in polycrystalline diamond is doped within the crystal structure, no boron crystalline phase is observed in the polycrystalline diamond. In contrast, clustered boron constitutes a different crystalline phase from that of diamond. Therefore, if polycrystalline diamond contains clustered boron, a boron crystalline phase is observed in the polycrystalline diamond. The presence or absence of a boron crystalline phase can be observed, for example, by X-ray diffraction. Depending on the size of the boron crystalline phase, it can also be observed visually.
[0042] Regarding (2) above, when boron is dispersed within the crystal structure, the distribution of the boron content, based on the number of atoms, is more uniform compared to when it exists in a clustered state. The distribution of the boron content, based on the number of atoms, can be measured, for example, by secondary ion mass spectrometry (SIMS). The distribution of the boron content, based on the number of atoms, can be considered uniform if the difference in the boron content measured at any two points in the crystal structure is less than or equal to a predetermined value. In other words, boron can be considered to be dispersed within the crystal structure and not in a clustered state.
[0043] The polycrystalline diamond of Embodiment 1 may consist of diamond crystal grains, boron, and unavoidable impurities. The content of diamond crystal grains in the polycrystalline diamond of Embodiment 1 may be 98% by volume or more and 100% by volume or less.
[0044] The diamond grain content (volume %) in polycrystalline diamond can be measured by combining a method using an energy-dispersive X-ray analyzer (EDX) attached to a scanning electron microscope (SEM) (e.g., JEOL's "JSM-7800F" (product name)) (e.g., Oxford's X-MAX80 EDS system) (hereinafter also referred to as "SEM-EDX") and X-ray diffraction. The specific measurement method is as follows.
[0045] First, a sample containing the cross-section of the polycrystalline diamond is prepared by cutting the diamond at an arbitrary position. A focused ion beam apparatus, a cross-section polisher, etc., can be used to prepare the cross-section. Next, the cross-section is observed using a scanning electron microscope (SEM) to obtain a backscattered electron image. In the backscattered electron image, the regions containing diamond crystal grains and non-diamond-like carbon appear as black regions, while other regions (e.g., elements derived from the binder) appear as gray or white regions. The magnification when observing the cross-section with the SEM is adjusted appropriately so that the number of diamond crystal grains observed in the measurement field of view is 100 or more. For example, the magnification when observing the cross-section with the SEM may be 10,000x.
[0046] Next, the backscattered electron image is subjected to binarization using image analysis software (such as "Win ROOF ver. 7.4.5" or "WinROOF2018" from Mitani Corporation). The image analysis software automatically sets an appropriate binarization threshold based on the image information (the measurer does not arbitrarily set the threshold). The inventors have also confirmed that there is no significant change in the measurement results even when the brightness of the image is varied. From the image after binarization, the area ratio of pixels originating from the dark field (pixels originating from diamond crystal grains and non-diamond-like carbon) to the area of the measurement field of view is calculated. By considering the calculated area ratio as a volume percentage, the sum (volume percentage) of the content of diamond crystal grains and the content of non-diamond-like carbon can be determined.
[0047] By calculating the area ratio of pixels originating from the brightfield (pixels originating from other regions) to the area of the measurement field of view from the binarized image, the content (volume %) of other regions can be determined.
[0048] As long as the sum (by volume) of the diamond grain content and the non-diamond-like carbon content in polycrystalline diamond is measured in the same sample, it has been confirmed that there is almost no variation in the measurement results even when the measurement field is changed and calculations are performed multiple times.
[0049] Furthermore, the fact that pixels originating from dark-field imaging are derived from diamond crystal grains and non-diamond-like carbon can be confirmed by performing elemental analysis on polycrystalline diamond using SEM-EDX.
[0050] Next, an X-ray diffractometer (Rigaku's "MiniFlex 600" (product name)) is used to obtain the X-ray spectrum of the above cross-section of polycrystalline diamond. The conditions for the X-ray diffractometer at this time are as follows: Characteristic X-ray: Cu-Kα (wavelength 1.54 Å) Tube voltage: 45 kV Tube current: 40 mA Filter: Multilayer mirror Optical system: Focusing method X-ray diffraction method: θ-2θ method.
[0051] In the obtained X-ray spectrum, the following peak intensities A and B are measured.
[0052] Peak intensity A: Peak intensity of non-diamond-like carbon, obtained by removing background noise from peak intensity at diffraction angle 2θ = 27.5° to 29.5°. Peak intensity B: Peak intensity of diamond crystal grains, obtained by removing background noise from peak intensity at diffraction angle 2θ = 43.8° to 44.0°.
[0053] The diamond grain content (volume %) is obtained by calculating the value of {peak intensity B / (peak intensity A + peak intensity B)} × {the sum of the diamond grain content and non-diamond-like carbon content obtained in the above-mentioned SEM-EDX (volume %)}. Since non-diamond-like carbon and diamond grains all have roughly the same electronic weight, the above X-ray peak intensity ratio can be considered as the volume ratio in polycrystalline diamond.
[0054] <Grain boundary regions between diamond crystal grains> The polycrystalline diamond of Embodiment 1 contains a plurality of diamond crystal grains, and boron is segregated in the grain boundary regions between adjacent diamond crystal grains. Here, the first diamond crystal grain and the second diamond crystal grain are two adjacent crystal grains arbitrarily selected from the plurality of diamond crystal grains contained in the polycrystalline diamond.
[0055] In this disclosure, the method for confirming that boron is segregated in the grain boundary region between adjacent diamond crystal grains is as follows:
[0056] First, a sample containing the cross-section of the polycrystalline diamond is prepared by cutting the polycrystalline diamond at an arbitrary position. A focused ion beam apparatus, a cross-section polisher apparatus, etc., can be used to prepare the cross-section. Next, the above cross-section is observed with a JEM-ARM300F2 to obtain a dark-field STEM image (hereinafter also referred to as the "first image"). The conditions for acquiring the first image are an observation magnification of 500,000x and an acceleration voltage of 200kV. An example of a dark-field STEM image (first image) of polycrystalline diamond according to Embodiment 1 is shown in Figure 1.
[0057] In the dark-field STEM image (first image), identify the grain boundaries between adjacent diamond crystal grains. It is necessary to analyze the areas where the grain boundaries are parallel to the observation direction. To do this, the following points should be kept in mind when identifying grain boundaries: - Identify grain boundaries where there is a difference in contrast (brightness / darkness) between adjacent grains. - Select grain boundaries that are clearly defined rather than blurred. - Exclude twin grain boundaries, as they are not grain boundaries between diamond crystal grains, when identifying grain boundaries.
[0058] The selected grain boundary is positioned so that it passes near the center of the image, and the elemental mapping image of boron (hereinafter also referred to as the "second image") is obtained by observing it with an electron energy loss spectroscopy (TEM-EELS) attached to a transmission electron microscope. The second image was accumulated 10 times under the conditions of a field size of 45 nm × 70 nm, an acceleration voltage of 200 kV, a camera length of 3 cm, a pixel count of 90 × 140 pixels, and a duel time of 0.005 s / pixel. An example of the elemental mapping image of boron (second image) of polycrystalline diamond according to Embodiment 1 is shown in Figure 2. Figure 2 is the second image of the region enclosed by the dotted line in the first image shown in Figure 1. In Figure 2, the level of boron concentration is indicated by the intensity of the color of each pixel.
[0059] If there are pixels in the elemental mapping image of boron (second image) that show a higher boron concentration than in areas other than the grain boundary, corresponding to the location identified as a grain boundary in the dark-field STEM image (first image), then it can be confirmed that boron is segregated in the grain boundary region between adjacent diamond crystal grains.
[0060] In the same polycrystalline diamond, five non-overlapping first images are arbitrarily acquired, and a second image is obtained based on each first image, and the above analysis is performed. If boron segregation is confirmed in the grain boundary regions between adjacent diamond crystal grains in four or more fields of view, it is determined that boron segregation exists in the grain boundary regions between adjacent diamond crystal grains in that polycrystalline diamond.
[0061] As long as the measurements are performed on the same polycrystalline diamond, it has been confirmed that there is no variation in the measurement results even when the cutting location of the cross-section of the polycrystalline diamond is arbitrarily set, the measurement field of view on the cross-section is arbitrarily changed, and the above analysis is performed multiple times. Therefore, as long as the above method for confirming boron segregation is applied to the polycrystalline diamond and it is confirmed that boron is segregated in the grain boundary region, the oxidation resistance of the polycrystalline diamond is improved.
[0062] In the polycrystalline diamond of Embodiment 1, the diamond crystal grains include a first diamond crystal grain and a second diamond crystal grain that are adjacent to each other. Observing the cross-section of the polycrystalline diamond with an electron energy loss spectrometer (TEM-EELS) attached to a transmission electron microscope, a boron elemental mapping image is obtained. The first graph, which shows the results obtained by extracting lines from the boron elemental mapping image (corresponding to the second image above) along a direction perpendicular to the grain boundary between the first diamond crystal grain and the second diamond crystal grain, from a measurement start point X1 located inside the first diamond crystal grain to a measurement end point X2 located inside the second diamond crystal grain, in a coordinate system where the X axis is the distance from the measurement start point X1 and the Y axis is the atomic concentration of boron, may satisfy the following conditions 1 to 4. Condition 1: There exists a maximum value A for the atomic concentration of boron. Condition 2: The atomic concentration of boron decreases monotonically from a distance P1 at the maximum value A to a distance P2 1.5 nm away from the origin of the first graph. Condition 3: The atomic concentration of boron decreases monotonically from distance P1, where the maximum value A is located, to distance P3, which is 1.5 nm away from the origin on the first graph. Condition 4: The average concentration B of the number of boron atoms in the first region between distances P2 and P3 is greater than the average concentration C of the number of boron atoms in the second region between distance P2 and distance P4, which is 5 nm away from distance P2 towards the origin on the first graph, and in the third region between distance P3 and distance P5, which is 5 nm away from distance P3 towards the origin on the first graph.
[0063] The conditions for acquiring the above boron elemental mapping image were: field of view size 45 nm × 70 nm, acceleration voltage 200 kV, camera length 3 cm, pixel count 90 × 140 pixels, duel time 0.005 s / pixel, and number of integrations 10 times. When analyzing the data acquired from the first graph, the data was averaged to a width of 10 nm and quantified at a pitch of 0.5 nm.
[0064] In this disclosure, the direction perpendicular to the grain boundary between the first diamond grain and the second diamond grain means the direction along a straight line that intersects the elongation direction of the grain boundary at an angle of 90° ± 5°.
[0065] As long as the measurements are performed on the same polycrystalline diamond, it has been confirmed that there is no variation in the measurement results even when the cutting point of the polycrystalline diamond cross-section is arbitrarily set, the measurement field of view on the cross-section is arbitrarily changed, and the above analysis is performed multiple times.
[0066] Figure 3 is an example of a first graph obtained from the polycrystalline diamond of Embodiment 1. In the graph of Figure 3, the X axis represents the distance from the measurement start point X1, and the Y axis represents the atomic concentration of boron. In Figure 3, it is determined that the atomic concentration of boron reaches its maximum value A at a distance of 21.5 nm.
[0067] In Figure 3, P1 is 21.5 nm, P2 is 20.0 nm, P3 is 23.0 nm, P4 is 15.0 nm, and P5 is 28.0 nm. The first graph in Figure 3 satisfies condition 1 because it has a maximum value A. The first graph satisfies condition 2 because the atomic concentration of boron decreases monotonically from P1 to P2. The first graph satisfies condition 3 because the atomic concentration of boron decreases monotonically from P1 to P3. In the first graph, the average concentration B of boron atoms in the first region between P2 and P3 is 2.9 atomic percent. The average concentration C of boron atoms in the second region between P2 and P4, and in the third region between P3 and P5, is 2.35 atomic percent. Therefore, condition 4 is satisfied.
[0068] In the first graph of the polycrystalline diamond of Embodiment 1, the average concentration B of the number of boron atoms in the first region between distance P2 and distance P3 may be 1 atomic% or more and 5 atomic% or less, or 1 atomic% or more and 3 atomic% or less.
[0069] In the first graph of the polycrystalline diamond of Embodiment 1, the average concentration C of boron atoms in the second region between distance P2 and distance P4, which is 5 nm away from distance P2 toward the origin of the first graph, and in the third region between distance P3 and distance P5, which is 5 nm away from distance P3 toward the opposite side of the origin of the first graph, may be 1 atomic% or more and 4 atomic% or less, or 1 atomic% or more and 3 atomic% or less.
[0070] The difference between the above average B and the above average C may be between 0.1 atomic percent and 3 atomic percent, or between 0.1 atomic percent and 1 atomic percent.
[0071] In the polycrystalline diamond of Embodiment 1, the oxygen content in the grain boundary region between adjacent diamond crystal grains may be below the detection limit when measured by electron energy loss spectroscopy using a transmission electron microscope. The specific measurement method is as follows.
[0072] The first image is acquired using the same method as described above for confirming the segregation of boron in the grain boundary region between adjacent diamond grains, and the grain boundary between adjacent diamond grains is identified. The selected grain boundary is positioned so that it passes near the center of the image, and an elemental mapping image of oxygen (hereinafter also referred to as the "third image") is obtained by observation with TEM-EELS. The conditions for acquiring the third image are the same as those for acquiring the second image. If there are no pixels indicating oxygen at the location in the elemental mapping image of oxygen (third image) corresponding to the location identified as a grain boundary in the dark-field STEM image (first image), it is determined that the oxygen content in the grain boundary region between adjacent diamond grains is below the detection limit.
[0073] In the same polycrystalline diamond, two non-overlapping first images are arbitrarily acquired, and a third image is obtained based on each first image, and the above analysis is performed. If it is confirmed that the oxygen content in the grain boundary region between adjacent diamond crystal grains is below the detection limit in the two fields of view, it is determined that the oxygen content in the grain boundary region between adjacent diamond crystal grains in that polycrystalline diamond is below the detection limit.
[0074] <Average grain size of diamond crystal grains> The polycrystalline diamond of Embodiment 1 contains a plurality of diamond crystal grains. The average grain size of the diamond crystal grains may be 10 nm to 50,000 nm, 50 nm to 1,000 nm, 50 nm to 500 nm, or 50 nm to 200 nm.
[0075] The average grain size of diamond crystals in polycrystalline diamond can be determined by a scanning electron microscope (SEM) sectioning method. Specifically, the polycrystalline diamond is first observed using a scanning electron microscope at a magnification of 1,000 to 100,000 times to obtain an SEM image.
[0076] Next, draw a circle on the SEM image, and draw eight straight lines radially from the center of the circle (so that the intersection angles between each line are approximately equal) to the outer circumference of the circle. In this case, it is preferable to set the observation magnification and the diameter of the circle so that the number of diamond crystal grains that lie on each of the straight lines is approximately 10 to 50.
[0077] Next, for each of the above lines, count the number of times the line crosses the grain boundaries of the diamond crystal grains, and calculate the average intercept length by dividing the length of the line by the number of crossings. Multiply this average intercept length by 1.128 to obtain the value obtained as the first average grain size. Calculate the average of the first average grain sizes for the eight lines (the second average grain size). Calculate the second average grain size for each of the five SEM images using the above procedure, and calculate the average of these second average grain sizes. This average value is the average grain size of the diamond crystal grains in the polycrystalline diamond.
[0078] Furthermore, it has been confirmed that, as long as the average grain size of diamond crystals is measured in the same sample, there is almost no variation in the measurement results even when the selection of the measurement field of view is changed and calculations are performed multiple times.
[0079] <Knoop Hardness> The Knoop hardness of the polycrystalline diamond of Embodiment 1 may be 50 GPa or higher. The Knoop hardness of the polycrystalline diamond may be 50 GPa or higher and 120 GPa or lower, 60 GPa or higher and 100 GPa or lower, or 60 GPa or higher and 90 GPa or lower.
[0080] In this disclosure, the Knoop hardness of polycrystalline diamond shall be measured by a method conforming to "JIS Z 2251:2009 Knoop hardness test - Measurement method". A general microhardness tester can be used to measure the Knoop hardness. The measurement environment may be room temperature (for example, around 23°C ± 5°C). A Knoop-type indenter (an indenter with a rhombic pyramidal shape) shall be used. The material of the indenter shall be single-crystal diamond. The test force (load) shall be 4.9 N (0.5 kgf). The holding time of the test force shall be 10 seconds. The approach speed of the indenter shall be 60 μm / s.
[0081] The Knoop hardness is measured at five locations on the polycrystalline diamond to be measured. The average value of the three measurements obtained by excluding the minimum and maximum values from the five measurements is calculated. In this disclosure, this average value corresponds to the Knoop hardness of the polycrystalline diamond.
[0082] <Volume Resistivity> The volume resistivity of the polycrystalline diamond of Embodiment 1 may be 1 mΩ·cm or more and 1000 Ω·cm or less, 10 mΩ·cm or more and 1000 Ω·cm or less, 20 mΩ·cm or more and 100 Ω·cm or less, or 100 mΩ·cm or more and 10 Ω·cm or less.
[0083] In this disclosure, the volume resistivity of polycrystalline diamond is measured at a temperature of 20°C to 25°C in accordance with JIS C2141-1992.
[0084] <Method for Manufacturing Polycrystalline Diamond> The polycrystalline diamond of Embodiment 1 can be manufactured, for example, by the following method. The manufacturing method described below will be explained step by step with reference to Figures 4 and 5.
[0085] <<Preparation Process>> This process is for preparing graphite. As shown in Figure 4, in the preparation process, graphite 1 containing carbon and boron doped into the crystalline structure composed of carbon is prepared on a substrate 2. The prepared graphite 1 is converted into polycrystalline diamond by a conversion process described later. The grain size of the single crystals in graphite 1 and the boron content in graphite 1 on an atomic basis are related to polycrystalline diamond. The grain size of the single crystals constituting graphite 1 may be 100 μm or less. The boron content in graphite 1 on an atomic basis is 1 × 10⁻¹⁶ 16 / cm 3 The above 1 x 10 22 / cm 3 The following applies. Graphite 1 that satisfies the above-mentioned single crystal grain size and boron content based on the number of atoms can be formed on a substrate 2, for example, by the following chemical vapor deposition (CVD) method.
[0086] ≪CVD Method≫ A substrate 2 for vapor-phase growth of graphite is placed in a vacuum chamber on its main surface. Any metal, inorganic ceramic material, or carbon material can be used as the material for the substrate 2, as long as it can withstand temperatures of approximately 1500°C to 3000°C. However, from the viewpoint of reducing impurities mixed into the graphite that will become the raw material for polycrystalline diamond, at least the main surface of the substrate may be made of carbon material, or it may be diamond or graphite with very few impurities.
[0087] Next, the substrate 2 placed in the vacuum chamber is heated to a temperature of approximately 1500°C to 3000°C. Known heating methods can be employed, for example, by installing a heater capable of directly or indirectly heating the substrate 2 in the vacuum chamber.
[0088] Next, hydrocarbon gas and boron-containing gas are introduced into the vacuum chamber. At this time, the vacuum level (pressure) inside the vacuum chamber is set to below atmospheric pressure. This allows the hydrocarbon gas and boron-containing gas to be uniformly mixed inside the vacuum chamber.
[0089] As the hydrocarbon gas, ethane, butane, methane, etc., can be used. Methane may be used because, due to its small molecular weight, it does not easily produce by-products such as ethylene when thermally decomposed. In addition, as the boron-containing gas, gases consisting of boron hydride, hydrocarbon gases containing boron, and halogenated gases containing boron may be used. When a gas consisting of boron hydride is used, the gas can be easily decomposed at high temperatures, so boron can be efficiently supplied to the substrate. When a hydrocarbon gas containing boron is used, boron that is already bonded to carbon can be supplied to the substrate, so boron can be doped into the graphite more efficiently. When a halogenated gas containing boron is used, graphite can be synthesized while removing unintended metal impurities through the action of halogens, so the concentration of metal impurities in the graphite can be reduced more effectively. For example, boron fluoride gas can be used.
[0090] Then, by thermally decomposing the mixed gas at a constant temperature of 1600°C or higher, graphite containing carbon and boron doped into the carbon-based crystalline structure is formed on the main surface of the substrate. In the graphite, boron is dispersed within the crystalline structure. Here, "thermally decomposing the mixed gas at a constant temperature of 1600°C or higher" means maintaining the heating temperature of the mixed gas within a predetermined temperature ± 5°C.
[0091] In the above CVD method, the temperature and pressure in the synthesis conditions may be set to 1600°C or higher and 13 Torr or higher, respectively, in order to reduce the grain size of the single crystals contained in graphite 1 to 100 μm or less. By reducing the grain size of the single crystals contained in graphite 1 to 100 μm or less, the grain size of the diamond crystals in polycrystalline diamond produced by direct conversion can be reduced to 50,000 nm or less. Furthermore, by adjusting the grain size of the single crystals contained in graphite 1 to 10 nm or more and 100,000 nm or less, the grain size of the diamond crystals in polycrystalline diamond can be reduced to 10 nm or more and 50,000 nm or less. Note that the composition of graphite 1 may include single crystals in part, with the rest being in the state of amorphous, amorphous carbon, carbon nanotubes, fullerenes, etc., or it may be a polycrystalline material composed of single crystals. To obtain polycrystalline diamond with more uniform grain size, it is preferable to form graphite 1 in which each graphite phase is formed by a single phase. Here, grain size refers to the average grain size as described above.
[0092] In the above CVD method, the boron content in graphite 1, based on the number of atoms, is 1.0 × 10⁻⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3 To achieve the following, the mixing ratio of hydrocarbon gases and each boron-containing gas is adjusted. Specifically, by increasing the mixing ratio of boron-containing gases to hydrocarbon gases, the amount of boron on an atomic basis in graphite 1 can be increased. Furthermore, the amount of boron on an atomic basis can also be adjusted by changing the type of boron-containing gas. The amount of boron on an atomic basis in graphite 1 is 1.0 × 10⁻⁶. 16 / cm3 The above 1.0 x 10 22 / cm 3 By doing the following, the boron content on an atomic basis in polycrystalline diamond is 1.0 × 10⁻¹⁶ 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following can be done:
[0093] To segregate boron in the grain boundary regions between diamond crystal grains, the flow rate per unit time of the hydrocarbon gas introduced into the vacuum chamber, the flow rate per unit time of the boron-containing gas, and the flow rate ratio of the hydrocarbon gas to the boron-containing gas are adjusted. Specifically, the flow rate per unit time of the hydrocarbon gas is 50 sccm or more. The flow rate per unit time of the boron-containing gas is 0.5 sccm or more. The flow rate ratio of the hydrocarbon gas to the boron-containing gas must be such that the flow rate of the boron-containing gas is greater than 100:1. That is, if the flow rate of the hydrocarbon gas is 100, the flow rate of the boron-containing gas should be greater than 1. The flow rates are constantly controlled using mass flow equipment or the like.
[0094] In this process, by using the above CVD method, graphite 1 containing carbon and boron doped into a crystalline structure composed of carbon is produced on the substrate 2, wherein the boron content on an atomic basis is 1.0 × 10⁻¹⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following graphite 1 is formed. In other words, boron is 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 Graphite 1, which is dispersed within the crystalline structure in the following atomic number-based content, is grown on the substrate 2 using vapor phase growth.
[0095] Furthermore, with respect to the graphite prepared in this process, it is preferable that the distribution of boron content, based on the number of atoms, is uniform in both the thickness direction and the in-plane direction. By uniformly doping the graphite with boron, the distribution of boron in the polycrystalline diamond produced by the conversion process described later can be made uniform.
[0096] To ensure a uniform distribution of boron content based on the number of atoms, it is preferable to simultaneously introduce hydrocarbon gases and each boron-containing gas into the vacuum chamber. This allows for easy and uniform mixing of the gases, enabling the efficient formation of uniformly boron-doped graphite on the substrate.
[0097] Furthermore, the density of the graphite prepared in this process is 0.8 g / cm³. 3 2.2g / cm or more 3 The following is also acceptable, or 1.4 g / cm³. 3 2.1g / cm or more 3 The following is also acceptable: Graphite density of 0.8 g / cm³ 3 In the above case, the volume change when graphite is directly converted to polycrystalline diamond in the conversion process described later can be sufficiently reduced, thereby suppressing the probability of cracks occurring in the manufactured polycrystalline diamond, and also suppressing changes in the environment inside the apparatus, which in turn can improve the manufacturing yield. 3 Under the following conditions, polycrystalline diamond can be synthesized with a high yield of over 80%.
[0098] The density of graphite can be adjusted, for example, by the temperature (°C) and the introduction rate (sccm) of each gas when growing graphite on the main surface of the substrate. Specifically, the density of graphite can be increased by raising the temperature and by increasing the introduction rate of hydrocarbons.
[0099] Furthermore, it is preferable that the graphite prepared in this process has a low content of unavoidable impurities. Specifically, the content of each element that is an unavoidable impurity in graphite may be 0.01 mass% or less. This is because the content of unavoidable impurities in the graphite is carried over to the polycrystalline diamond produced. In addition, by keeping the content of unavoidable impurities low, grain growth caused by the presence of unavoidable impurities can be suppressed, so that single crystals of a more uniform size can be contained in the graphite. Note that analytical instruments used for analysis that can measure the content of unavoidable impurities in graphite, such as SIMS analysis and ICP analysis, generally have a detection limit of 0.01 mass%, so elements with a content of 0.01 mass% or less will not be detected by the above analytical instruments.
[0100] The inclusion of unavoidable impurities in graphite can be suppressed by setting a relatively high vacuum level in the vacuum chamber during the thermal decomposition of the gas. Specifically, the inventors have found that by maintaining the pressure in the vacuum chamber between 20 Torr and 200 Torr, more preferably between 20 Torr and 120 Torr, the content of each element, which is an unavoidable impurity, can be controlled to 0.01 mass% or less.
[0101] In the CVD method described above, the substrate is heated before the mixed gas is introduced into the vacuum chamber. However, the substrate may also be heated after the mixed gas is introduced, or both methods may be performed simultaneously.
[0102] <<Conversion Process>> This process involves sintering the graphite produced in the preparation process to directly convert it into polycrystalline diamond. As a result, polycrystalline diamond 3 is produced on the substrate 2, as shown in Figure 5.
[0103] Specifically, first, the graphite 1 on the substrate 2 shown in Figure 4 is placed in a high-temperature, high-pressure apparatus. The high-temperature, high-pressure apparatus can be any apparatus that can accommodate graphite and control the internal conditions as described above. For example, a vacuum chamber used in the CVD method can be used.
[0104] Graphite 1 is exposed to high-temperature and high-pressure conditions of 1700°C to 2500°C and 15 GPa to 25 GPa. As a result, graphite 1 is instantaneously sintered and converted into polycrystalline diamond 3, as shown in Figure 5. In this case, the shape of the polycrystalline diamond 3 will inherit the shape of graphite 1, except for a slight change in volume. Alternatively, graphite 1 may be exposed to high-temperature and high-pressure conditions after the substrate 2 has been removed from it, and in this case as well, the produced polycrystalline diamond will basically inherit the shape of graphite 1.
[0105] In this process, it is preferable not to use additives such as sintering aids, catalysts, and binders. According to this process, polycrystalline diamond in which single crystals are strongly bonded can be produced without the use of additives, and by not using additives, polycrystalline diamond with higher hardness can be produced compared to when additives are used.
[0106] According to the manufacturing method described in detail above, the polycrystalline diamond of Embodiment 1 can be manufactured.
[0107] Furthermore, according to the above manufacturing method, since boron is uniformly dispersed in the graphite, it is possible to effectively suppress localized abnormal growth of diamond crystal grains when directly converting graphite to diamond. As a result, the grain size of the single crystals constituting polycrystalline diamond can be made more uniform, and consequently, homogeneous polycrystalline diamond can be manufactured.
[0108] [Embodiment 2: Tools] A tool according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 2") is a tool comprising the polycrystalline diamond described in Embodiment 1. Each tool may be composed entirely of polycrystalline diamond, or only a part thereof (for example, the cutting edge portion in the case of a cutting tool) may be composed of polycrystalline diamond. Furthermore, a coating film may be formed on the surface of each tool. Examples of tools include cutting tools, wear-resistant tools, wire drawing tools, and grinding tools.
[0109] Examples of cutting tools include drills, end mills, replaceable cutting tips for drills, replaceable cutting tips for end mills, replaceable cutting tips for milling machines, replaceable cutting tips for turning machines, metal saws, gear cutting tools, reamers, taps, and cutting tools.
[0110] Examples of wear-resistant tools include scribers, scribing wheels, dressers, water and other fluid jet nozzles, and stitchels. Examples of wire drawing tools include dies. Examples of grinding tools include grinding wheels.
[0111] The tool can be manufactured by machining the polycrystalline diamond of Embodiment 1 into a desired shape, for example, by electrical discharge machining.
[0112] This embodiment will be described in more detail by reference to examples. However, this embodiment is not limited by these examples.
[0113] [Preparation of Polycrystalline Diamonds] Polycrystalline diamonds were prepared from each sample using the following method.
[0114] <<Preparation Process>> Boron-containing graphite was prepared on a substrate using the CVD method. The main surface of the substrate was diamond. After placing the substrate in a vacuum chamber, the substrate was heated to 1850°C, and the vacuum level (pressure) inside the vacuum chamber was reduced to below atmospheric pressure. In this state, methane gas and a gas containing boron (boron fluoride gas) were then introduced into the vacuum chamber for more than one hour.
[0115] For each sample, the flow rate of methane gas per unit time and the flow rate of boron-containing gas per unit time were as shown in Table 1. The boron-containing gas was introduced into the vacuum chamber along with argon as a carrier. The flow rate was constantly controlled using a mass flow instrument. The substrate temperature was maintained at 1850°C. Through the above process, graphite with a thickness of more than 100 μm was produced on the main surface of the substrate.
[0116]
[0117] <<Conversion Process>> Next, the graphite on the substrate was converted into polycrystalline diamond at 1750°C and 15 GPa under ultra-high pressure using a large press capable of generating high temperature and pressure, thereby producing polycrystalline diamond for each sample.
[0118] [Evaluation] For each sample of polycrystalline diamond, the content of boron (based on the number of atoms), the content of oxygen (based on the number of atoms), the presence or absence of boron segregation in the grain boundary region between adjacent diamond grains, the oxygen content in the grain boundary region, the average grain size of the diamond grains, the Knoop hardness of the polycrystalline diamond, and the volume resistivity of the polycrystalline diamond were measured using the method described in Embodiment 1. The results are shown in Tables 2 and 3. In the tables, "ND" means below the detection limit.
[0119] Cross-sections of polycrystalline diamond samples were observed using an electron energy loss spectrometer attached to a transmission electron microscope to obtain elemental mapping images of boron. In the elemental mapping images of boron, lines were extracted from the boron elemental mapping image along a direction perpendicular to the grain boundary between the first and second diamond grains, from a measurement start point X1 located inside the first diamond grain to a measurement end point X2 located inside the second diamond grain adjacent to the first diamond grain. The results obtained are shown in the first graph, which is a coordinate system in which the X axis is the distance from the measurement start point X1 and the Y axis is the atomic concentration of boron. It was confirmed whether the first graph for each sample satisfies the following conditions 1 to 4. Condition 1: A maximum value A of the atomic concentration of boron exists. Condition 2: The atomic concentration of boron decreases monotonically from a distance P1 of the maximum value A to a distance P2 1.5 nm away from the origin of the first graph. Condition 3: The atomic concentration of boron decreases monotonically from distance P1, where the maximum value A is located, to distance P3, which is 1.5 nm away from the origin on the first graph. Condition 4: The average concentration B of the number of boron atoms in the first region between distances P2 and P3 is greater than the average concentration C of the number of boron atoms in the second region between distance P2 and distance P4, which is 5 nm away from distance P2 towards the origin on the first graph, and in the third region between distance P3 and distance P5, which is 5 nm away from distance P3 towards the origin on the first graph.
[0120] The first graphs of polycrystalline diamond samples 1 to 6 satisfied conditions 1 to 4. Average B and average C are shown in Table 2. The first graphs of polycrystalline diamond samples 101 to 102 did not satisfy conditions 1 to 4.
[0121] The oxidation initiation temperature of each polycrystalline diamond sample in air was measured using a conventionally known method. The results are shown in Table 3. The oxidation initiation temperature is the temperature at which the mass of the polycrystalline diamond begins to decrease when it is oxidized in air. In other words, it is the temperature at which the slope of the graph becomes negative in a coordinate system where the X axis is temperature and the Y axis is the mass of the polycrystalline diamond. A higher oxidation initiation temperature of polycrystalline diamond indicates better oxidation resistance of the polycrystalline diamond.
[0122]
[0123]
[0124] [Discussion] The polycrystalline diamonds of Sample 1 and Sample 2 correspond to the examples. The polycrystalline diamond of Sample 101 corresponds to the comparative example. The polycrystalline diamonds of Sample 1 and Sample 2 had superior oxidation resistance compared to the polycrystalline diamond of Sample 101.
[0125] While embodiments and examples of this disclosure have been described above, it is intended from the outset that the configurations of each of the embodiments and examples described above may be combined or modified in various ways as appropriate. The embodiments and examples disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than the embodiments and examples described above, and all modifications within the scope of the claims are intended to be included in the meaning of equivalences.
[0126] 1. Graphite, 2. Substrate, 3. Polycrystalline diamond.
Claims
1. The boron content, based on the number of atoms, is 1.0 × 10⁻⁶ 16 / cm 3 The above 1.0 x 10 22 / cm 3 A polycrystalline diamond, wherein the polycrystalline diamond contains a plurality of diamond crystal grains, and boron is segregated in the grain boundary regions between adjacent diamond crystal grains.
2. The polycrystalline diamond according to claim 1, wherein the diamond crystal grains include a first diamond crystal grain and a second diamond crystal grain adjacent to each other, and in the elemental mapping image of boron obtained by observing the cross-section of the polycrystalline diamond with an electron energy loss spectrometer attached to a transmission electron microscope, the first graph obtained by extracting a line from the elemental mapping image of boron along a direction perpendicular to the grain boundary between the first diamond crystal grain and the second diamond crystal grain, from a measurement start point X1 provided inside the first diamond crystal grain to a measurement end point X2 provided inside the second diamond crystal grain, and the result is shown in a coordinate system where the X axis is the distance from the measurement start point X1 and the Y axis is the atomic concentration of boron, satisfies the following conditions 1 to 4. Condition 1: There exists a maximum value A of the atomic concentration of boron. Condition 2: The atomic concentration of boron decreases monotonically from a distance P1 of the maximum value A to a distance P2 1.5 nm away from the origin side of the first graph. Condition 3: The atomic concentration of boron decreases monotonically from distance P1, where the maximum value A is located, to distance P3, which is 1.5 nm away from the origin of the first graph. Condition 4: The average concentration B of the number of boron atoms in the first region between distance P2 and distance P3 is greater than the average concentration C of the number of boron atoms in the second region between distance P2 and distance P4, which is 5 nm away from distance P2 towards the origin of the first graph, and in the third region between distance P3 and distance P5, which is 5 nm away from distance P3 towards the origin of the first graph.
3. The oxygen content of the polycrystalline diamond, based on the number of atoms, is 1.0 × 10⁻¹⁶. 18 / cm 3 The polycrystalline diamond according to claim 1 or claim 2, wherein the oxygen content of the polycrystalline diamond on an atomic basis is measured by secondary ion mass spectrometry.
4. The polycrystalline diamond according to any one of claims 1 to 3, wherein the oxygen content in the grain boundary region is below the detection limit as measured by electron energy loss spectroscopy using a transmission electron microscope.
5. The polycrystalline diamond according to any one of claims 1 to 4, wherein the average grain size of the diamond crystal grains is 10 nm or more and 50,000 nm or less.
6. The polycrystalline diamond according to any one of claims 1 to 5, wherein the Knoop hardness of the polycrystalline diamond is 50 GPa or higher, and the Knoop hardness is measured in accordance with JIS Z 2251:2009 at a temperature of 18°C or higher and 28°C or lower, and with a test load of 4.9 N.
7. The polycrystalline diamond according to any one of claims 1 to 6, wherein the volume resistivity of the polycrystalline diamond is 1 mΩ·cm or more and 1000 Ω·cm or less, and the volume resistivity is measured at 20°C or more and 25°C or less in accordance with JIS C2141-1992.
8. The polycrystalline diamond according to any one of claims 1 to 7, wherein the polycrystalline diamond comprises carbon, boron, and unavoidable impurities.
9. A tool comprising polycrystalline diamond as described in any one of claims 1 to 8.