Production method for fe-based soft magnetic material, method for restoring magnetic properties of fe-based soft magnetic material in which magnetic properties have changed over time, fe-based soft magnetic material, electromagnet, and electromagnet system
By annealing Fe-based soft magnetic materials in a mixed gas atmosphere with controlled hydrogen and inert gas concentrations, the method stabilizes magnetic properties and reduces explosion risk, improving the performance and safety of electromagnets in etching apparatuses.
Patent Information
- Application Number
- PCT/JP2026/017447
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
The magnetic properties of Fe-based soft magnetic materials used in electromagnets deteriorate over time, leading to reduced microfabrication accuracy in etching apparatuses, and annealing in pure hydrogen gas poses an explosion risk due to the high concentration of hydrogen gas.
Perform annealing in a mixed gas atmosphere containing hydrogen at a concentration of 0-30% and the remainder as an inert gas, such as argon or nitrogen, to produce an Fe-based soft magnetic material with restricted carbon, nitrogen, and other impurities, thereby suppressing property changes and reducing explosion risk.
The method stabilizes the magnetic properties of Fe-based soft magnetic materials over time, enhancing microfabrication accuracy and safety by minimizing the risk of explosions.
Smart Images

Figure JP2026017447_12112026_PF_FP_ABST
Abstract
Description
Method for manufacturing Fe-based soft magnetic material, method for restoring the magnetic properties of Fe-based soft magnetic material whose magnetic properties have changed over time, Fe-based soft magnetic material, electromagnet, and electromagnet system.
[0001] The present invention relates to a method for manufacturing an Fe-based soft magnetic material, a method for restoring the magnetic properties of an Fe-based soft magnetic material whose magnetic properties have changed over time, an Fe-based soft magnetic material, an electromagnet, and an electromagnet system.
[0002] An etching apparatus is a device that uses chemical reactions (corrosive action) of chemicals or ions to process a thin film (such as an oxide film) formed on a substrate (such as a wafer) into a desired shape. The etching apparatus is equipped with an etching chamber, and the etching process is performed within this chamber. To improve the controllability of the etching process, an electromagnet made of Fe-based soft magnetic material is mounted above the etching chamber.
[0003] Regarding such Fe-based soft magnetic materials, Non-Patent Document 1 discloses ELCH® 2 and ELCH® 2S, which are pure iron-based soft magnetic materials that exhibit high magnetic properties. Non-Patent Document 1 describes reducing the nitrogen concentration of ELCH® 2 by performing annealing in a nitrogen atmosphere, argon atmosphere, or hydrogen atmosphere.
[0004] Kobe Steel Technical Report, Mar. 2017, Vol. 66, No. 2, pp. 31-35
[0005] Upon diligent investigation of the etching apparatus described above, the inventors discovered that after using the etching apparatus for a predetermined period, the magnetic properties of the electromagnet mounted on the etching apparatus may change over time. This change in the magnetic properties of the electromagnet over time alters its initial magnetic field control performance, which is undesirable as it affects the microfabrication accuracy of the etching apparatus. The above-mentioned change in the magnetic properties of the electromagnet over time is due to a change in the magnetic properties of the Fe-based soft magnetic material contained in the electromagnet.
[0006] Furthermore, the inventors investigated the aforementioned annealing in a hydrogen atmosphere and found that, as shown in the [Examples] described later, heat treatment (annealing) of Fe-based soft magnetic materials in a hydrogen gas atmosphere (100% hydrogen gas pressure) can suppress changes in the magnetic properties of Fe-based soft magnetic materials over time. However, using only hydrogen gas during this annealing process increases the likelihood of explosion because the concentration of hydrogen gas in the atmosphere easily falls within the explosive range. In particular, electromagnet products are often large in size, and attempting to perform annealing in a hydrogen gas-only atmosphere requires handling a large amount of high-concentration hydrogen gas, further increasing the risk of explosion. Thus, from the standpoint of explosion prevention, the use of annealing with only hydrogen gas is restricted.
[0007] In view of these circumstances, the present invention aims to provide a method for manufacturing an Fe-based soft magnetic material that can suppress changes in the magnetic properties of the Fe-based soft magnetic material over time and reduce the risk of explosion.
[0008] The inventors of the present invention conducted intensive research to solve the above problems and found that the above problems can be solved by performing an annealing treatment in an atmosphere of a mixed gas containing hydrogen gas at a pressure of more than 0% and 30% or less and the remainder being an inert gas, and thus completed the present invention. Specific embodiments of the present invention are as follows.
[0009] [1] A method for producing an Fe-based soft magnetic material, comprising the step of performing an annealing treatment on an Fe-based soft magnetic material in an atmosphere of a mixed gas containing hydrogen gas at a concentration of more than 0 pressure% and 30 pressure% or less and the remainder being an inert gas, to obtain an Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less. [2] The method according to [1], wherein the Fe-based soft magnetic material after the annealing treatment is further restricted to containing Si at 0.3 mass% or less, Mn at 0.3 mass% or less, P at 0.02 mass% or less, S at 0.02 mass% or less, and Pb at 0.05 mass% or more and 0.25 mass% or less. [3] The method according to [1] or [2], wherein the inert gas includes nitrogen gas, argon gas, or a combination thereof. [4] The method according to any one of [1] to [3], further comprising a molding step of shaping the Fe-based soft magnetic material before the annealing treatment. [5] A method according to any one of [1] to [4], further comprising at least one of the following steps after the annealing treatment: - A machining step of machining an Fe-based soft magnetic material; and - A coil molding step of setting a coil on the Fe-based soft magnetic material, impregnating the set coil with a resin, and then curing the resin. [6] A method for restoring the magnetic properties of an Fe-based soft magnetic material whose magnetic properties have changed over time, comprising the step of performing an annealing treatment on the Fe-based soft magnetic material whose magnetic properties have changed over time in an atmosphere of a mixed gas containing hydrogen gas at more than 0 pressure% and 30 pressure% or less and the remainder being an inert gas, to obtain an Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less. [7] The method according to [6], wherein the Fe-based soft magnetic material after annealing is further restricted to containing 0.3% by mass or less of Si, 0.3% by mass or less of Mn, 0.02% by mass or less of P, 0.02% by mass or less of S, and 0.05% by mass or more and 0.25% by mass or less of Pb. [8] The method according to [6] or [7], wherein the inert gas comprises nitrogen gas, argon gas, or a combination thereof. [9] An Fe-based soft magnetic material wherein C is restricted to 0.02% by mass or less and N is restricted to 60 ppm by mass or less.
[10] The Fe-based soft magnetic material according to [9], further restricted to containing 0.3% by mass or less of Si, 0.3% by mass or less of Mn, 0.02% by mass or less of P, 0.02% by mass or less of S, and 0.05% by mass or more and 0.25% by mass or less of Pb.
[11] An electromagnet comprising the Fe-based soft magnetic material according to [9] or
[10] .
[12] An electromagnet system comprising the electromagnet according to
[11] .
[0010] The present invention provides a method for producing an Fe-based soft magnetic material that can suppress changes in the magnetic properties of the Fe-based soft magnetic material over time and reduce the risk of explosion.
[0011] The present invention provides a method for restoring the magnetic properties of Fe-based soft magnetic materials whose magnetic properties have changed over time. This method can restore deteriorated magnetic properties while reducing the risk of explosion.
[0012] The Fe-based soft magnetic material of the present invention can suppress changes in the magnetic properties of Fe-based soft magnetic materials over time.
[0013] The electromagnet of the present invention can suppress changes in magnetic properties over time.
[0014] The electromagnet system of the present invention can exhibit a stable magnetic field control function because the change in the magnetic properties of the electromagnet over time is suppressed.
[0015] This is a cross-sectional view showing the structure of an etching apparatus equipped with an etching chamber. This is the magnetic hysteresis curve for test sample No. 1. This is the magnetic hysteresis curve for test sample No. 2. This is the magnetic hysteresis curve for test sample No. 3. This is the magnetic hysteresis curve for test sample No. 4. This is the magnetic hysteresis curve for test sample No. 5. This is the magnetic hysteresis curve for test sample No. 6. This is a graph showing the relationship between nitrogen content (horizontal axis) and characteristic change rate (vertical axis). This is a graph showing the relationship between hydrogen pressure % (horizontal axis) and nitrogen content (vertical axis) during heat treatment.
[0016] In this specification, the "pressure %" of gas A in a gas mixture means the value calculated by dividing the partial pressure of gas A by the total pressure of the gas mixture (where the total pressure of the gas mixture is 1 atm) and multiplying by 100. In this specification, when a numerical range is expressed using "X to Y", the range includes the values at both ends.
[0017] The following describes the method for producing the Fe-based soft magnetic material of the present invention, a method for restoring the magnetic properties of an Fe-based soft magnetic material whose magnetic properties have changed over time, the Fe-based soft magnetic material itself, and an electromagnet system.
[0018] [1 Method for Manufacturing Fe-Based Soft Magnetic Material] The method for manufacturing an Fe-based soft magnetic material of the present invention includes the steps of annealing an Fe-based soft magnetic material in an atmosphere of a mixed gas containing hydrogen gas at more than 0 pressure% and 30 pressure% or less and the remainder being an inert gas, to obtain an Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less (annealing step, magnetic annealing step). The method for manufacturing an Fe-based soft magnetic material of the present invention can suppress changes in the magnetic properties of the Fe-based soft magnetic material over time and can reduce the risk of explosion.
[0019] (Fe-based soft magnetic material before annealing) The Fe-based soft magnetic material before annealing consists of Fe and unavoidable impurities. Examples of unavoidable impurities include, but are not limited to, C, N, P, and S. Furthermore, the Fe-based soft magnetic material before annealing may contain the following elements (Si, Mn, and Pb) in place of some of the Fe.
[0020] The carbon (C) content in the Fe-based soft magnetic material before annealing is not particularly limited, but is preferably 0.02% by mass or less, more preferably 0.01% by mass or less, and most preferably 0.005% by mass or less. A carbon content within the above numerical range improves magnetic flux density and coercivity. The carbon content may be greater than 0% by mass. The silicon (Si) content in the Fe-based soft magnetic material before annealing is not particularly limited, but is preferably 0.3% by mass or less, and more preferably 0.25% by mass or less. A silicon content within the above numerical range increases strength without impairing ductility and toughness. The silicon content may be greater than 0% by mass. The manganese (Mn) content in the Fe-based soft magnetic material before annealing is not particularly limited, but is preferably 0.3% by mass or less, and more preferably 0.25% by mass or less. A manganese (Mn) content within the above numerical range increases strength without impairing toughness. The manganese (Mn) content may be greater than 0% by mass. The P content in the Fe-based soft magnetic material before annealing is not particularly limited, but is preferably 0.02% by mass or less, and more preferably 0.01% by mass or less. By keeping the P content within the above numerical range, a decrease in strength and toughness can be suppressed. The P content may be greater than 0% by mass. The S content in the Fe-based soft magnetic material before annealing is not particularly limited, but is preferably 0.02% by mass or less, and more preferably 0.015% by mass or less. By keeping the S content within the above numerical range, toughness and weldability are improved. The S content may be greater than 0% by mass. The Pb content in the Fe-based soft magnetic material before annealing is not particularly limited, but is preferably 0.05 to 0.25% by mass, and more preferably 0.1 to 0.15% by mass. By keeping the Pb content within the above numerical range, machinability is improved. The N content in the Fe-based soft magnetic material before annealing is not particularly limited, but may be greater than 60 ppm by mass, 100 ppm or more by mass, or 150 ppm or more by mass. The N content may be 150 ppm or less by mass, 100 ppm or less by mass, or 60 ppm or less by mass. The numerical ranges for the upper and lower limits of the content of each of the above elements (C, Si, Mn, P, S, Pb, or N) can be any combination.
[0021] (Mixed Gas) The pressure percentage of hydrogen gas contained in the mixed gas is greater than 0 pressure% and 30 pressure% or less, preferably greater than 0 pressure% and 20 pressure% or less, and more preferably greater than 0 pressure% and 4 pressure% or less. By keeping the pressure percentage of hydrogen gas within the above numerical range, the risk of explosion during the annealing process can be reduced.
[0022] The remaining inert gas in the gas mixture is not particularly limited, but may include or consist of helium, neon, argon, krypton, xenon, radon, nitrogen, carbon dioxide, or a combination of two or more of these. Of these, argon, nitrogen, or a combination thereof is preferred from the viewpoint of suppressing procurement costs, and argon or nitrogen is more preferred.
[0023] (Annealing Treatment) The temperature in the annealing treatment is not particularly limited, but is preferably 700 to 900°C, and more preferably 800 to 900°C. By keeping the temperature in the annealing treatment within the above numerical range, it is possible to reduce the amount of nitrogen and restore the magnetic properties. The duration of the annealing treatment is not particularly limited, but is preferably 3 hours or more, and may be 3 to 7 hours. By keeping the duration of the annealing treatment within the above numerical range, it is possible to reduce the amount of nitrogen and restore the magnetic properties.
[0024] (Fe-based soft magnetic material after annealing) The Fe-based soft magnetic material after annealing consists of Fe and unavoidable impurities. Examples of unavoidable impurities include, but are not limited to, C, N, P, and S. Furthermore, the Fe-based soft magnetic material after annealing may contain the following elements (Si, Mn, and Pb) in place of some of the Fe.
[0025] The N content in the Fe-based soft magnetic material after annealing is restricted to 60 mass ppm or less, preferably 40 mass ppm or less, more preferably 30 mass ppm or less, and most preferably 20 mass ppm or less. The N content in the Fe-based soft magnetic material after annealing may be 55 mass ppm or less, 50 mass ppm or less, or 45 mass ppm or less. By keeping the N content within the above numerical range, the change in the magnetic properties of the Fe-based soft magnetic material over time can be suppressed. The N content in the Fe-based soft magnetic material after annealing may be greater than 0 mass ppm. The numerical ranges for the upper and lower limits of the N content can be arbitrarily combined. The C content in the Fe-based soft magnetic material after annealing is restricted to 0.02 mass% or less, preferably 0.01 mass% or less, and more preferably 0.005 mass% or less. By keeping the C content within the above numerical range, the magnetic flux density and coercivity are improved. The C content may be greater than 0% by mass. The numerical ranges for the upper and lower limits of the C content can be any combination. The numerical range for the Si, Mn, P, S, or Pb content in the Fe-based soft magnetic material after annealing treatment may be the same as the numerical range for the Si, Mn, P, S, or Pb content described above (Fe-based soft magnetic material before annealing treatment).
[0026] (Forming Process) The method for manufacturing the Fe-based soft magnetic material may further include a forming process in which the Fe-based soft magnetic material is formed before the annealing process. The forming process allows the Fe-based soft magnetic material to be formed into a predetermined shape. The type of forming is not particularly limited, but examples include casting, forging, and press working, and among these, forging is preferred from the viewpoint of making the Fe-based soft magnetic material the size of an electromagnet yoke.
[0027] (Rough Machining Process) The method for manufacturing the Fe-based soft magnetic material may further include a rough machining process in which the Fe-based soft magnetic material is roughly machined before the annealing process. The rough machining process can be carried out after the molding process described above. The rough machining process may also be a process of providing at least one groove (recess) in the Fe-based soft magnetic material. The type of rough machining is not particularly limited, but examples include cutting and grinding, and among these, cutting is preferred from the viewpoint of suppressing processing costs.
[0028] (Machining Process) The method for manufacturing Fe-based soft magnetic material may further include a machining process in which the Fe-based soft magnetic material is machined after annealing. The machining process allows the Fe-based soft magnetic material to be processed to the required dimensions and shape. The type of machining is not particularly limited, but examples include cutting, grinding, drilling, etc., and among these, cutting is preferred from the viewpoint of suppressing processing costs.
[0029] (Coil Molding Process) The method for manufacturing the Fe-based soft magnetic material may further include a coil molding process in which, after annealing, a coil is placed on the Fe-based soft magnetic material, the placed coil is impregnated with a resin, and the resin is cured. The coil molding process protects the coil and increases its mechanical strength. The method for placing the coil on the Fe-based soft magnetic material as described above may be either a method in which a coil is manufactured in advance in a predetermined shape (e.g., an annular shape) and the manufactured coil is combined with the Fe-based soft magnetic material, or a method in which the coil is directly wound around the Fe-based soft magnetic material. Of these, the method of combining a manufactured coil with the Fe-based soft magnetic material is preferred from the viewpoint of workability. The coil on the Fe-based soft magnetic material may be placed in at least one groove (recess) provided in the Fe-based soft magnetic material. Alternatively, the coil on the Fe-based soft magnetic material may be placed in at least one groove (recess) of the Fe-based soft magnetic material by manufacturing a coil in advance in a predetermined shape (e.g., an annular shape).
[0030] The type of metal used to form the coil is not particularly limited, but examples include copper, aluminum, and silver. Of these, copper is preferred from the viewpoint of availability. The type of resin used for impregnation is not particularly limited, but examples include epoxy resin, silicone resin, and urethane resin. Of these, epoxy resin is preferred from the viewpoint of electrical insulation. The temperature at which the resin is cured is not particularly limited, but 80 to 100°C is preferred. The curing time for the resin is not particularly limited, but 3 to 5 hours is preferred.
[0031] The composite material of the Fe-based soft magnetic material and the coil after the coil molding process can be used to make an electromagnet. In this case, the Fe-based soft magnetic material in the electromagnet functions as a yoke.
[0032] The method for manufacturing the Fe-based soft magnetic material may include the annealing step, machining step, and coil molding step described above in this order.
[0033] In conventional methods for manufacturing Fe-based soft magnetic materials, a heat treatment step (aging step) is sometimes performed after annealing to adjust the magnetic properties of the Fe-based soft magnetic material. On the other hand, in the manufacturing method of Fe-based soft magnetic material of this embodiment, the annealing treatment is performed in an atmosphere of a mixed gas containing hydrogen gas at a pressure of more than 0% and 30% or less and the remainder being an inert gas, thereby suppressing changes in the magnetic properties of the Fe-based soft magnetic material over time. Therefore, in the manufacturing method of Fe-based soft magnetic material of this embodiment, the above-mentioned aging step can be omitted, and as a result, manufacturing efficiency can be improved.
[0034] [2. Method for restoring the magnetic properties of Fe-based soft magnetic materials whose magnetic properties have changed over time] The present invention provides a method for restoring the magnetic properties of Fe-based soft magnetic materials whose magnetic properties have changed over time, comprising the step of performing an annealing treatment on an Fe-based soft magnetic material whose magnetic properties have changed over time in an atmosphere of a mixed gas containing hydrogen gas at more than 0 pressure% and 30 pressure% or less and the remainder being an inert gas, to obtain an Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less. The present invention provides a method for restoring the magnetic properties of Fe-based soft magnetic materials whose magnetic properties have changed over time, which can suppress changes in the magnetic properties of Fe-based soft magnetic materials over time and reduce the risk of explosion.
[0035] (Fe-based soft magnetic material whose magnetic properties change over time) Fe-based soft magnetic material whose magnetic properties change over time consists of Fe and unavoidable impurities. Examples of unavoidable impurities include, but are not limited to, C, N, P, and S. Furthermore, Fe-based soft magnetic material whose magnetic properties change over time may contain the following elements (Si, Mn, and Pb) in place of some of the Fe.
[0036] The content of C in the Fe-based soft magnetic material with magnetically deteriorated properties over time is not particularly limited, but is preferably 0.02 mass% or less, more preferably 0.01 mass% or less, and most preferably 0.005 mass% or less. When the content of C falls within the above numerical range, the magnetic flux density and coercive force are improved. The content of C may be more than 0 mass%. The upper and lower numerical limits of the C content can be arbitrarily combined. The content of N in the Fe-based soft magnetic material with magnetically deteriorated properties over time is not particularly limited, and may be more than 60 mass ppm, 100 mass ppm or more, or 150 mass ppm or more. The content of N may be 150 mass ppm or less, 100 mass ppm or less, or 60 mass ppm or less. The upper and lower numerical limits of the N content can be arbitrarily combined. In the present embodiment, the content of Si, Mn, P, S, or Pb in the Fe-based soft magnetic material with magnetically deteriorated properties over time can be the same as the content of Si, Mn, P, S, or Pb described in (Fe-based soft magnetic material before annealing treatment) of the above [1 Method for producing Fe-based soft magnetic material].
[0037] The Fe-based soft magnetic material with magnetically deteriorated properties over time in the present embodiment is not particularly limited, and examples thereof include an Fe-based soft magnetic material that is taken out from an electromagnet system after the electromagnet system provided with the Fe-based soft magnetic material has been operated for a predetermined period. The electromagnet system may be included in a substrate processing apparatus, and in this case, the above-mentioned Fe-based soft magnetic material may be taken out from the substrate processing apparatus after the substrate processing apparatus has been operated for a predetermined period.
[0038] (Mixed Gas) The configuration of the mixed gas in the present embodiment (pressure% of hydrogen gas, type of inert gas, etc.) can be the same as the configuration described in (Mixed Gas) of the above [1 Method for producing Fe-based soft magnetic material].
[0039] (Annealing Treatment) The conditions of the annealing treatment in the present embodiment (temperature, time, etc.) can be the same as the conditions described in (Annealing Treatment) of the above [1 Method for producing Fe-based soft magnetic material].
[0040] (Fe-based soft magnetic material after annealing treatment) The Fe-based soft magnetic material after annealing treatment consists of Fe and unavoidable impurities. Examples of unavoidable impurities include, but are not limited to, C, N, P, S and the like. Further, the Fe-based soft magnetic material after annealing treatment may contain the following elements (Si, Mn, and Pb) in place of a part of Fe.
[0041] The N content in the Fe-based soft magnetic material after annealing treatment is regulated to 60 mass ppm or less, preferably 40 mass ppm or less, more preferably 30 mass ppm or less, and most preferably 20 mass ppm or less. The N content in the Fe-based soft magnetic material after annealing treatment may be 55 mass ppm or less, 50 mass ppm or less, or 45 mass ppm or less. When the N content falls within the above numerical range, the change over time in the magnetic properties of the Fe-based soft magnetic material can be suppressed. The N content in the Fe-based soft magnetic material after annealing treatment may be more than 0 mass ppm. The upper limit and lower limit numerical ranges of the N content can be arbitrarily combined. The C content in the Fe-based soft magnetic material after annealing treatment is regulated to 0.02 mass% or less, preferably 0.01 mass% or less, and more preferably 0.005 mass% or less. When the C content falls within the above numerical range, the magnetic flux density and coercive force are improved. The C content may be more than 0 mass%. The upper limit and lower limit numerical ranges of the C content can be arbitrarily combined. The numerical ranges of the contents of Si, Mn, P, S, or Pb in the Fe-based soft magnetic material after annealing treatment may be the same as the numerical ranges of the contents of Si, Mn, P, S, or Pb described in the above (Fe-based soft magnetic material with magnetic properties changed over time).
[0042] [3 Fe-based soft magnetic material] The Fe-based soft magnetic material of the present invention is regulated to have C of 0.02 mass% or less and N of 60 mass ppm or less. The Fe-based soft magnetic material of the present invention can suppress the change over time in the magnetic properties of the Fe-based soft magnetic material.
[0043] The Fe-based soft magnetic material of this embodiment consists of Fe and unavoidable impurities. Examples of unavoidable impurities include, but are not limited to, C, N, P, and S. Furthermore, the Fe-based soft magnetic material may contain the following elements (Si, Mn, and Pb) in place of a portion of Fe.
[0044] In this embodiment, the N content in the Fe-based soft magnetic material is restricted to 60 ppm by mass or less, preferably 40 ppm by mass or less, more preferably 30 ppm by mass or less, and most preferably 20 ppm by mass or less. By keeping the N content within the above numerical range, the change in the magnetic properties of the Fe-based soft magnetic material over time can be suppressed. The N content in this embodiment may be greater than 0 ppm by mass. The numerical ranges for the upper and lower limits of the N content can be arbitrarily combined. In this embodiment, the C content in the Fe-based soft magnetic material is restricted to 0.02% by mass or less, preferably 0.01% by mass or less, and more preferably 0.005% by mass or less. By keeping the C content within the above numerical range, the magnetic flux density and coercivity are improved. The C content may be greater than 0% by mass. The numerical ranges for the upper and lower limits of the C content can be arbitrarily combined. The numerical range of Si, Mn, P, S, or Pb content in the Fe-based soft magnetic material of this embodiment can be the same as the numerical range of Si, Mn, P, S, or Pb content described in (Fe-based soft magnetic material after annealing treatment) in [1 Method for manufacturing Fe-based soft magnetic material] above.
[0045] The Fe-based soft magnetic material in this embodiment can be manufactured by the manufacturing method described in [1 Method for manufacturing Fe-based soft magnetic material] above. The Fe-based soft magnetic material in this embodiment may be an Fe-based soft magnetic material obtained by the manufacturing method described in [1 Method for manufacturing Fe-based soft magnetic material] above, or an Fe-based soft magnetic material obtained by the method described in [2 Method for restoring the magnetic properties of an Fe-based soft magnetic material whose magnetic properties have changed over time] above.
[0046] [4 Electromagnet] The electromagnet of the present invention comprises the Fe-based soft magnetic material described in [3 Fe-based soft magnetic material] above. The electromagnet of the present invention can suppress changes in magnetic properties over time.
[0047] The electromagnet may be a composite material of an Fe-based soft magnetic material and a coil. In this case, the Fe-based soft magnetic material in the electromagnet functions as a yoke. At least one groove (recess) may be provided in the Fe-based soft magnetic material (yoke), and the coil may be installed in the groove. The groove may be annular in shape.
[0048] The type of metal used to make up the coil is not particularly limited, but examples include copper, aluminum, and silver. Of these, copper is preferred from the viewpoint of ease of availability. The shape of the coil is not particularly limited, but a linear shape is preferred. By winding a linear coil around a yoke made of Fe-based soft magnetic material, the composite material of the Fe-based soft magnetic material and the coil described above can be formed.
[0049] [5 Electromagnetic System] The electromagnetic system of the present invention comprises the electromagnet described in [4 Electromagnet] above. The electromagnetic system of the present invention can exhibit a stable magnetic field control function because the change in the magnetic properties of the electromagnet over time is suppressed.
[0050] The electromagnet system is not particularly limited, but may further include an electromagnet control device. The electromagnet control device controls the current flowing through the electromagnet to obtain a desired magnetic flux density.
[0051] In some embodiments, the substrate processing apparatus includes the electromagnet system described above. The substrate processing apparatus is not particularly limited, but an etching apparatus is preferred, and a plasma etching apparatus is particularly preferred. In the plasma etching apparatus described above, the plasma can be controlled by applying an appropriate magnetic field using the electromagnet system.
[0052] The following is an example of a substrate processing device, based on the diagram.
[0053] Figure 1 is a cross-sectional view showing the structure of the etching apparatus 100. The etching apparatus 100 comprises an electromagnet 110, an electromagnet control device 120, a water-cooled plate 130, and an etching chamber 140. The electromagnet 110, together with the electromagnet control device 120, forms an electromagnet system. The electromagnet 110 and the electromagnet control device 120 are electrically connected. The electromagnet 110 comprises a yoke 112 and a coil 114 made of Fe-based soft magnetic material. The yoke 112 has a disc shape and has a plurality of annular grooves (recesses) arranged concentrically. The annular coil 114 is installed in these grooves. A magnetic field is applied to the etching chamber 140 by the electromagnet 110. The etching chamber 140 is in a vacuum state, and a wafer 150 is placed in the etching chamber 140 and subjected to etching.
[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to what is described in the examples.
[0055] [1. Preparation of the electromagnet] Using free-cutting pure iron ME1F (C: ≤0.02, Si: ≤0.3, Mn: ≤0.3, P: ≤0.02, S: ≤0.02, Pb: 0.05 to 0.25 (all by mass%)) (manufactured by Daido Steel Co., Ltd.), a yoke having a disc shape and four grooves (recesses) was prepared by going through the processes of forging, magnetic annealing, and cutting. The four grooves are arranged concentrically on the yoke and are referred to as zones 1 to 4 from the inside out. The shape and size of the yoke and each zone, as well as the conditions for the magnetic annealing described above, are shown below.
[0056] (Yoke) Disc shape, inner diameter 50 mm, outer diameter 468 mm, height 26 mm (Zone 1) Inner diameter 60 mm, outer diameter 142 mm, height 20 mm (Zone 2) Inner diameter 162 mm, outer diameter 244 mm, height 20 mm (Zone 3) Inner diameter 264 mm, outer diameter 346 mm, height 20 mm (Zone 4) Inner diameter 366 mm, outer diameter 448 mm, height 20 mm *Zones 1 to 4 are all annular grooves (Magnetic annealing) Heat treatment at 850°C for 5 hours in an air atmosphere
[0057] Using a wire (copper, 1-1.5 mm in diameter), coils 1-4 (annular in shape) corresponding to the sizes of zones 1-4 were prepared using a winding jig. The obtained coils 1-4 were then placed in zones 1-4. The zones 1-4 in which the coils 1-4 were placed were then impregnated with epoxy resin, and the epoxy resin was sufficiently cured and the coils sealed by heating at 100°C for 5 hours (coil molding process). This resulted in the creation of an electromagnet (disk-shaped, 468 mm in diameter, 26 mm in height).
[0058] [2. Preparation of Test Samples] For the electromagnet obtained in [1. Preparation of Electromagnets] above, an electric current was applied to the coil in the electromagnet under adiabatic conditions in an atmospheric environment. Specifically, the electromagnet was held for 336 hours while adjusting the current so that the yoke temperature was around 100°C due to the self-heating of the coil. As mentioned above, when an etching apparatus equipped with an electromagnet is used for a predetermined period, the magnetic properties of the electromagnet mounted in the etching apparatus may change over time. Similarly, it is presumed that holding the electromagnet under the above conditions will cause a change in its magnetic properties over time. The change over time caused by holding the electromagnet under the above conditions can be estimated to be equivalent to the change over time caused by using the etching apparatus for about one year. Test samples No. 1 to 6 (parts of a ring, inner diameter 24 mm, outer diameter 36 mm, height 4 mm) were cut out from the yoke of the electromagnet after holding under the above conditions.
[0059] [3 Measurement of Magnetic Properties and Nitrogen Content] (1) Initial Magnetic Properties For each test sample No. 1 to 6 obtained in [2 Preparation of Test Samples] above, a DC magnetic measuring device (BHS-40CD, manufactured by RIKEN Electron Systems, Ltd.) was used to obtain magnetic hysteresis curves based on the DC method under room temperature conditions, and the following magnetic properties were measured. B 1 (T): Magnetic flux density at 100 A / m, B 5 (T): Magnetic flux density at 500 A / m, B 10 (T): Magnetic flux density at 1000 A / m, B 50 (T): Magnetic flux density at 5000 A / m, Br(T): Residual magnetic flux density, Hc(A / m): Coercivity, μ m : Maximum relative permeability
[0060] (2) Magnetic Properties After Annealing Treatment (After Heat Treatment) For Test Sample No. 1 obtained in the above [2 Preparation of Test Samples], heating was performed under the conditions of 850°C for 3 hours in an atmosphere of a mixed gas (4% by pressure of hydrogen gas and the balance of argon gas), to obtain Sample No. 1 after heat treatment (hereinafter denoted as "4% H 2 (bal. Ar)"). For Test Sample No. 2 obtained in the above [2 Preparation of Test Samples], heating was performed under the conditions of 850°C for 3 hours in an atmosphere of a mixed gas (4% by pressure of hydrogen gas and the balance of nitrogen gas), to obtain Sample No. 2 after heat treatment (hereinafter denoted as "4% H 2 (bal. N 2 )"). For Test Sample No. 3 obtained in the above [2 Preparation of Test Samples], heating was performed under the conditions of 850°C for 3 hours in an atmosphere of a mixed gas (20% by pressure of hydrogen gas and the balance of argon gas), to obtain Sample No. 3 after heat treatment (hereinafter denoted as "20% H 2 (bal. Ar)"). For Test Sample No. 4 obtained in the above [2 Preparation of Test Samples], heating was performed under the conditions of 850°C for 3 hours in an atmosphere of a mixed gas (20% by pressure of hydrogen gas and the balance of nitrogen gas), to obtain Sample No. 4 after heat treatment (hereinafter denoted as "20% H 2 (bal. N 2 )"). For Test Sample No. 5 obtained in the above [2 Preparation of Test Samples], heating was performed under the conditions of 850°C for 3 hours in an atmosphere of hydrogen gas (100% by pressure of hydrogen gas), to obtain Sample No. 5 after heat treatment (hereinafter denoted as "hydrogen heat treatment"). For Test Sample No. 6 obtained in the above [2 Preparation of Test Samples], heating was performed under the conditions of 850°C for 3 hours in an atmospheric air atmosphere, to obtain Sample No. 6 after heat treatment (hereinafter denoted as "atmospheric heat treatment").
[0061] For each of the obtained heat-treated Test Sample Nos. 1 to 6, a magnetic hysteresis curve was obtained, and the various magnetic properties described above were measured in the same manner as in the above (1).
[0062] (3) Magnetic properties after aging treatment Each of the test samples No. 1 to 6 obtained after heat treatment in (2) above was subjected to aging treatment at 100°C for 200 hours in an atmospheric environment to obtain each of the samples No. 1 to 6 after aging treatment (referred to as "after accelerated magnetic aging test" in Tables 1 and 2 below). Note that the above aging treatment is equivalent to an accelerated test and is carried out in order to understand the degree of deterioration after a long period of time.
[0063] For each of the aged test samples No. 1 to 6 obtained, magnetic hysteresis curves were obtained and the magnetic properties described above were measured in the same manner as in (1) above.
[0064] (4) Nitrogen content and rate of change in properties After holding the electromagnet under the specific conditions obtained in [2 Preparation of test samples] above, a test sample (hereinafter referred to as "untreated") (a part of a ring, inner diameter 24 mm, outer diameter 36 mm, height 4 mm) was cut from the yoke of the electromagnet, in the same manner as for test samples No. 1 to 6. The magnetic properties of the test sample (untreated) obtained in this manner were measured in the same manner as in (1) above. In addition, a 1 mm portion from the surface of the test sample (untreated) was cut and removed, and the nitrogen content (mass ppm) was measured in the exposed portion (a portion 1 mm deep from the surface) based on the inert gas fusion-thermal conductivity method. The nitrogen content was measured only once (N=1).
[0065] Furthermore, test samples No. 1 to 6 obtained after heat treatment as described in (2) above were prepared, and the nitrogen content (mass ppm) of these test samples was measured based on the same procedure and method as the untreated test samples described above.
[0066] Furthermore, using the results obtained in (2) to (4) above for each of the above test samples No. 1 to 6 (untreated) and after heat treatment, B 1 (T), Hc (A / m), and μ m The rate of change of each magnetic property was calculated based on the following formula.
[0067]
[0068] The results of (1) to (3) above are shown in Tables 1 and 2, and the resulting magnetic hysteresis curves are shown in Figures 2 to 7. Furthermore, the results of (4) above are shown in Table 3, and graphs showing the relationship between nitrogen content (horizontal axis) and characteristic change rate (vertical axis), and graphs showing the relationship between hydrogen pressure % during heat treatment (horizontal axis) and nitrogen content (vertical axis) are shown in Figures 8 and 9, respectively.
[0069]
[0070]
[0071] The results for each test sample No. 1 to 4 in Table 1 show that heat treatment in a mixed gas atmosphere (4 or 20 pressure percent hydrogen gas, and the remainder being argon or nitrogen gas) reduced the residual magnetic flux density and coercivity, and increased the maximum relative permeability compared to the initial state. These results indicate that heat treatment in a mixed gas atmosphere restored the magnetic properties lost due to holding under specific conditions.
[0072] Furthermore, the results for each test sample No. 1 to 4 in Table 1 show that the residual magnetic flux density, coercivity, and maximum relative permeability of each test sample after aging treatment did not change significantly compared to the test samples after heat treatment. From these results, it can be inferred that the magnetic properties of each test sample will not change significantly even if they are used as electromagnets in an etching apparatus after heat treatment.
[0073] On the other hand, the results for test sample No. 5 in Table 2 show that heat treatment in a hydrogen gas atmosphere reduces the residual magnetic flux density and coercivity, and increases the maximum relative permeability compared to the initial state. Furthermore, for test sample No. 5, no significant changes were observed in residual magnetic flux density, coercivity, and maximum relative permeability in the aging treatment test sample compared to the heat treatment test sample. However, because test sample No. 5 uses only hydrogen gas during heat treatment, the concentration of hydrogen in the atmospheric gas is more likely to fall within the explosive range, increasing the possibility of explosion. In particular, electromagnet products are large in size, and attempting to heat treat them in a hydrogen gas atmosphere without an inert gas increases the risk of explosion. Thus, from an explosion-proof standpoint, there are limitations to performing heat treatment with only hydrogen gas, and therefore, the aforementioned test samples No. 1 to 4, which limit the hydrogen pressure, are highly effective in terms of explosion protection.
[0074] Furthermore, the results for test sample No. 6 in Table 2 show that heat treatment in an atmospheric environment reduced the residual magnetic flux density and coercivity, and increased the maximum relative permeability compared to the initial state. However, for test sample No. 6, the aging treatment showed increased residual magnetic flux density and coercivity, and decreased maximum relative permeability compared to the heat-treated test sample, resulting in magnetic properties closer to those of the initial test sample. Based on these results, it can be inferred that using test sample No. 6 as an electromagnet in an etching apparatus after heat treatment will significantly degrade its magnetic properties (the hysteresis will widen).
[0075]
[0076] From the results in Table 3 and Figure 8, it was found that the nitrogen content decreased in each of the test samples No. 1 to 4, which were heat-treated in an atmosphere of mixed gas (4 or 20 pressure percent hydrogen gas, and the remainder being argon or nitrogen gas), and in the test sample No. 5, which was heat-treated in an atmosphere of hydrogen gas only, compared to the untreated test sample, reaching 60 ppm or less. In addition, the rate of change in each magnetic property of test samples No. 1 to 5 was also significantly reduced compared to the untreated test sample. On the other hand, the nitrogen content of test sample No. 6, which was heat-treated in an atmosphere of air, actually increased compared to the untreated test sample. Furthermore, the rate of change in each magnetic property of test sample No. 6 actually increased compared to the untreated test sample.
[0077] From the results in Table 3 and Figure 8, test samples No. 1 to 4 and test sample No. 5 all showed low rates of change in their respective magnetic properties. These results indicate that the rate of change in properties can be reduced by limiting the nitrogen content of the test samples to 60 ppm or less. By reducing the rate of change in properties in this way, it can be estimated that the magnetic properties will not change significantly even when used as electromagnets in etching equipment after heat treatment. Furthermore, as mentioned above, test samples No. 1 to 4, in which the hydrogen pressure in the mixed gas with inert gas was limited, are highly effective in terms of explosion prevention. Therefore, test samples No. 1 to 4 can be said to be superior in terms of explosion prevention and preventing changes in magnetic properties.
[0078] The above results are experimental results for Fe-based soft magnetic materials extracted from electromagnets held under specific conditions. As mentioned above, the change in magnetic properties over time caused by holding under the above conditions can be estimated to be equivalent to the change in magnetic properties over time caused by using an etching apparatus for approximately one year. Here, the Fe-based soft magnetic material before magnetic annealing in "1. Preparation of Electromagnets" is not restricted to having N below 60 mass ppm and is a material that is highly likely to cause a change in magnetic properties over time. Therefore, from the viewpoint of magnetic properties, it is presumed to be similar to the Fe-based soft magnetic material extracted from electromagnets held under specific conditions. Accordingly, based on the above experimental results for Fe-based soft magnetic materials extracted from electromagnets held under specific conditions, it can be inferred that similar results will be obtained when the Fe-based soft magnetic material before magnetic annealing in "1. Preparation of Electromagnets" is used as the processing target.
[0079] 100: Etching apparatus 110: Electromagnet 112: Yoke made of Fe-based soft magnetic material 114: Coil 120: Electromagnet control device 130: Water-cooled plate 140: Etching chamber 150: Wafer
Claims
1. A method for producing an Fe-based soft magnetic material, comprising the step of performing an annealing treatment on an Fe-based soft magnetic material in an atmosphere of a mixed gas containing hydrogen gas at more than 0 pressure% and 30 pressure% or less and the remainder being an inert gas, thereby obtaining an Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less.
2. The method according to claim 1, wherein the Fe-based soft magnetic material after the annealing treatment is further restricted to containing 0.3% by mass or less of Si, 0.3% by mass or less of Mn, 0.02% by mass or less of P, 0.02% by mass or less of S, and 0.05% by mass or more and 0.25% by mass or less of Pb.
3. The method according to claim 1 or 2, wherein the inert gas includes nitrogen gas, argon gas, or a combination thereof.
4. The method according to any one of claims 1 to 3, further comprising a molding step of shaping an Fe-based soft magnetic material before the annealing treatment.
5. The method according to any one of claims 1 to 4, further comprising at least one of the following steps after the annealing treatment: - a machining step of machining an Fe-based soft magnetic material; and - a coil molding step of setting a coil on the Fe-based soft magnetic material, impregnating the set coil with a resin, and then curing the resin.
6. A method for restoring the magnetic properties of an Fe-based soft magnetic material whose magnetic properties have changed over time, comprising the step of performing an annealing treatment on the Fe-based soft magnetic material whose magnetic properties have changed over time in an atmosphere of a mixed gas containing hydrogen gas at more than 0 pressure% and 30 pressure% or less and the remainder being an inert gas, to obtain an Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less.
7. The method according to claim 6, wherein the Fe-based soft magnetic material after the annealing treatment is further restricted to containing 0.3% by mass or less of Si, 0.3% by mass or less of Mn, 0.02% by mass or less of P, 0.02% by mass or less of S, and 0.05% by mass or more and 0.25% by mass or less of Pb.
8. The method according to claim 6 or 7, wherein the inert gas includes nitrogen gas, argon gas, or a combination thereof.
9. An Fe-based soft magnetic material in which C is restricted to 0.02 mass% or less and N is restricted to 60 mass ppm or less.
10. The Fe-based soft magnetic material according to claim 9, further comprising Si 0.3% by mass or less, Mn 0.3% by mass or less, P 0.02% by mass or less, S 0.02% by mass or less, and Pb 0.05% by mass or more and 0.25% by mass or less.
11. An electromagnet comprising the Fe-based soft magnetic material according to claim 9 or 10.
12. An electromagnet system comprising the electromagnet described in claim 11.