Surface-treated steel sheet
The surface-treated steel sheet with a specific chemical composition and structure addresses condensation discoloration issues while maintaining corrosion and blackening resistance, ensuring a superior appearance.
Patent Information
- Application Number
- PCT/JP2026/017700
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
Surface-treated steel sheets experience issues with condensation discoloration, which affects their appearance despite having sufficient corrosion resistance and blackening resistance.
A surface-treated steel sheet with a specific chemical composition and structure, including a plating layer with Al, Mg, and Zn, and a chemical conversion film containing Si, Zr, V, P, Co, and Mg, where the emission intensity of Mg peaks before Si in the depth profile, enhancing condensation discoloration resistance.
The steel sheet achieves excellent corrosion resistance, blackening resistance, and improved condensation discoloration resistance, maintaining a superior appearance.
Smart Images

Figure JP2026017700_12112026_PF_FP_ABST
Abstract
Description
Surface-treated steel sheet
[0001] This disclosure relates to steel sheets, and more particularly to surface-treated steel sheets.
[0002] Surface-treated steel sheets comprise a base steel sheet, a plating layer formed on the base steel sheet, and a coating formed on the plating layer. Surface-treated steel sheets are widely used in applications such as building materials, automobiles, and home appliances. The corrosion resistance of surface-treated steel sheets is enhanced by the plating layer and coating.
[0003] As a coating to enhance the corrosion resistance of surface-treated steel sheets, a chemical conversion coating formed by chemical conversion treatment such as chromate treatment or phosphate treatment has been proposed.
[0004] For example, Japanese Patent Publication No. 2003-055777 (Patent Document 1) proposes a surface-treated steel sheet in which a coating made of a zirconium compound and a vanadium compound is formed on a Zn-Al-Mg-Si alloy plating. Also, Japanese Patent Publication No. 2005-097733 (Patent Document 2) proposes a surface-treated steel sheet in which a coating made of a vanadium compound, a phosphate compound, a metal component and an acrylic resin is formed on a Zn-Al alloy plating.
[0005] Surface-treated steel sheets with these coatings can have enhanced corrosion resistance. However, from the viewpoint of appearance, it is also required that these surface-treated steel sheets suppress the blackening phenomenon, that is, improve resistance to blackening.
[0006] Therefore, a surface-treated steel sheet that provides sufficient resistance to blackening along with corrosion resistance has been proposed in International Publication No. 2017 / 155028 (Patent Document 3). The surface-treated steel sheet disclosed in Patent Document 3 comprises a steel sheet, a zinc-containing plating layer formed on the steel sheet, and a film formed on the plating layer. This film contains acrylic resin, zirconium, vanadium, phosphorus, and cobalt, and the area ratio of the acrylic resin in the region from the surface to 1 / 5 of the film thickness in the cross-section of the film is 80 to 100 area percent. Furthermore, in the region consisting of a region from the center of the film thickness toward the surface to 1 / 10 of the film thickness, and a region from the center of the film thickness toward the plating layer to 1 / 10 of the film thickness, the area ratio of the acrylic resin is 5 to 50 area percent.
[0007] Japanese Patent Publication No. 2003-055777, Japanese Patent Publication No. 2005-097733, International Publication No. 2017 / 155028
[0008] The surface-treated steel sheet disclosed in Patent Document 3 provides sufficient corrosion resistance and sufficient resistance to blackening.
[0009] Incidentally, in surface-treated steel sheets, a phenomenon may occur where the condensed area discolors when condensation forms on the surface. In this specification, this phenomenon is referred to as "condensation discoloration." Condensation discoloration does not particularly affect the mechanical properties of the surface-treated steel sheet. However, since a pattern is formed in the condensed area, the appearance of the surface-treated steel sheet deteriorates. Therefore, it is preferable to suppress the occurrence of condensation discoloration in surface-treated steel sheets. In other words, excellent resistance to condensation discoloration is also required of surface-treated steel sheets.
[0010] The purpose of this disclosure is to provide a surface-treated steel sheet that exhibits excellent corrosion resistance, excellent resistance to blackening, and excellent resistance to condensation discoloration.
[0011] The surface-treated steel sheet of this disclosure comprises a base steel sheet, a plating layer formed on the base steel sheet, and a chemical conversion film formed on the plating layer. The chemical composition of the plating layer is, by mass%, Al: more than 5.0% and less than 25.0%, Mg: more than 3.0% and less than 12.5%, and Zn: 65.0% or more. The chemical conversion film contains Si, Zr, V, P, Co, and Mg, and the thickness of the chemical conversion film is 0.03 to 2.00 μm. Glow discharge emission spectroscopy is performed from the surface of the chemical conversion film in the direction of the film thickness to obtain a depth profile showing the relationship between sputtering time and the emission intensity of elements in the chemical conversion film, and at the sputtering time t in the depth profile, the emission intensity of Mg reaches the first peak intensity from the start of sputtering. Mg This is the sputtering time t at which the emission intensity of Si reaches its peak intensity. Si Faster than, sputter time t Mg Peak intensity of Mg at I Mg , and sputtering time t Si The peak intensity of Si at I Si This satisfies equation (1). 0.10 ≤ I Mg / I Si ≤ 1.00 (1)
[0012] The surface-treated steel sheet disclosed herein provides excellent corrosion resistance and excellent resistance to blackening, as well as excellent resistance to condensation discoloration.
[0013] Figure 1 is a cross-sectional view perpendicular to the rolling direction of a surface-treated steel sheet according to one embodiment of the present disclosure. Figure 2 is a graph of the depth profile of elements in the chemical conversion coating and plating layer of the surface-treated steel sheet. Figure 3 is a different example of the depth profile graph of elements in the chemical conversion coating and plating layer of the surface-treated steel sheet from Figure 2.
[0014] The inventors conducted investigations and studies to solve the above problems. As a result, the inventors obtained the following findings.
[0015] A base steel sheet on which a plating layer containing Zn as a main component, and further containing, in mass%, more than 5.0% and less than 25.0% of Al, and more than 3.0% and less than 12.5% of Mg is formed, may achieve excellent corrosion resistance and blackening resistance if the chemical conversion coating formed on the plating layer contains Si, Zr, V, P and Co, and the film thickness of the chemical conversion coating is 0.03 to 2.00 μm.
[0016] However, even the surface-treated steel sheet having the above-described configuration may still fail to obtain sufficient condensation discoloration resistance in some cases. The present inventors therefore conducted further studies. As a result, the present inventors found that the condensation discoloration resistance is affected by V in the chemical conversion coating.
[0017] The present inventors therefore further studied means for enhancing the condensation discoloration resistance. As a result, the present inventors found that the condensation discoloration resistance is enhanced by diffusing a part of Mg in the plating layer into the chemical conversion coating and further concentrating Mg in the surface layer of the chemical conversion coating. Specifically, when the chemical conversion coating contains not only Si, Zr, V, P and Co but also Mg, and glow discharge optical emission spectrometry is performed in the film thickness direction (depth direction) from the surface of the chemical conversion coating to obtain a depth direction profile showing the relationship between the sputtering time and the emission intensity of the elements in the chemical conversion coating, it has been found that excellent condensation discoloration resistance can be obtained if the following two characteristics are satisfied in the depth direction profile. (Characteristic 1) The sputtering time t at which the emission intensity of Mg reaches the first peak intensity from the start of sputtering Mg is earlier than the sputtering time t at which the emission intensity of Si reaches the peak intensity Si . (Characteristic 2) The peak intensity I of Mg at the sputtering time t Mg Mg and the peak intensity I of Si at the sputtering time t Si Si satisfy the formula (1). 0.10 ≤ I Mg / I Si ≤ 1.00 (1)
[0018] The surface-treated steel sheet according to one embodiment of the present disclosure is completed based on the above technical idea, and is as follows.
[0019] A surface-treated steel sheet according to one embodiment of the present disclosure comprises a base steel sheet, a plating layer formed on the base steel sheet, and a chemical conversion film formed on the plating layer. The chemical composition of the plating layer is, in mass%, Al: more than 5.0% and less than 25.0%, Mg: more than 3.0% and less than 12.5%, and Zn: 65.0% or more. The chemical conversion film contains Si, Zr, V, P, Co, and Mg, and the thickness of the chemical conversion film is 0.03 to 2.00 μm. Furthermore, glow discharge emission spectroscopy analysis is performed from the surface of the chemical conversion film in the direction of the thickness of the chemical conversion film to obtain a depth profile showing the relationship between sputtering time and the emission intensity of elements in the chemical conversion film, and in the depth profile, the sputtering time t at which the emission intensity of Mg reaches the first peak intensity from the start of sputtering is determined. Mg This is the sputtering time t at which the emission intensity of Si reaches its peak intensity. Si Faster than, sputter time t Mg Peak intensity of Mg at I Mg and sputtering time t Si The peak intensity of Si at I Si This satisfies equation (1). 0.10 ≤ I Mg / I Si ≤ 1.00 (1)
[0020] In one embodiment of the surface-treated steel sheet of the present disclosure, the chemical composition of the plating layer is further, in mass%, Sn: greater than 0 to 3.00%, Bi: greater than 0 to 5.00%, In: greater than 0 to 2.00%, Ca: greater than 0 to 3.00%, Y: greater than 0 to 3.00%, La: greater than 0 to 3.00%, Ce: greater than 0 to 3.00%, Si: greater than 0 to 2.50%, Cr: greater than 0 to 0.5%, Ti: greater than 0 It may contain one or more elements selected from the group consisting of ~0.5%, Ni: greater than 0 to 0.5%, Co: greater than 0 to 0.5%, V: greater than 0 to 0.5%, Nb: greater than 0 to 0.5%, Cu: greater than 0 to 0.5%, Mn: greater than 0 to 0.5%, Fe: greater than 0 to 5.0%, Sr: greater than 0 to 0.5%, Sb: greater than 0 to 0.5%, Pb: greater than 0 to 0.5%, and B: greater than 0 to 0.5%.
[0021] Hereinafter, a surface-treated steel sheet according to one embodiment of the present disclosure will be described with reference to the drawings. In the drawings, substantially identical components are denoted by the same reference numerals, and their descriptions are omitted. When describing the content of each element, "%" means mass percent unless otherwise specified.
[0022] [Structure of Surface-Treated Steel Sheet] Figure 1 is a cross-sectional view perpendicular to the rolling direction of a surface-treated steel sheet according to one embodiment of the present disclosure. Referring to Figure 1, the surface-treated steel sheet 1 comprises a base steel sheet 10, a plating layer 20, and a chemical conversion film 30. The plating layer 20 is formed on the surface of the base steel sheet 10. The chemical conversion film 30 is formed on the surface of the plating layer 20. The plating layer 20 may be formed on one side of the base steel sheet 10, or the plating layer 20 may be formed on each of the surfaces of both sides of the base steel sheet 10. When the plating layer 20 is formed on both sides of the base steel sheet 10, the chemical conversion film 30 may be formed only on the plating layer 20 on one side, or it may be formed on the plating layer 20 on each of the surfaces of both sides.
[0023] [Regarding the base steel sheet 10] The base steel sheet 10 is not particularly limited. For example, it may be a steel sheet whose microstructure mainly consists of ferrite. It may be a steel sheet whose microstructure mainly consists of ferrite and pearlite. It may be a steel sheet whose microstructure mainly consists of ferrite and one or more of martensite and bainite. It may be a steel sheet whose microstructure mainly consists of martensite and bainite. The type of base steel sheet 10 does not particularly affect the effect of the surface-treated steel sheet 1 of this embodiment. Therefore, the base steel sheet 10 is not particularly limited. The chemical composition of the base steel sheet 10 is also not particularly limited.
[0024] [About the plating layer 20] The plating layer 20 is formed on the surface (one or both sides) of the base steel sheet 10. The plating layer 20 contains, by mass%, Al: more than 5.0% and less than 25.0%, Mg: more than 3.0% and less than 12.5%, and Zn: 65.0% or more. Each element is described below.
[0025] Al: More than 5.0% and less than 25.0% Aluminum (Al) is an easily oxidized element and enhances the corrosion resistance of the plating layer 20 through sacrificial corrosion protection. The above effect can be sufficiently obtained if the Al content is more than 5.0% and less than 25.0%. The preferred lower limit of the Al content is 5.1%, more preferably 7.5%, even more preferably 10.0%, and even more preferably 12.0%. The preferred upper limit of the Al content is 24.9%, more preferably 24.5%, even more preferably 24.0%, even more preferably 22.0%, and even more preferably 20.0%.
[0026] Mg: More than 3.0% and less than 12.5% Magnesium (Mg) is an easily oxidized element and enhances the corrosion resistance of the plating layer 20 through sacrificial corrosion protection. The above effect can be sufficiently obtained if the Mg content is more than 3.0% and less than 12.5%. The preferred lower limit of the Mg content is 3.1%, more preferably 3.2%, more preferably 3.3%, more preferably 3.4%, more preferably 3.5%, more preferably 4.0%, more preferably 4.5%, more preferably 5.0%, and more preferably 5.5%. The preferred upper limit of the Mg content is 12.4%, more preferably 12.0%, more preferably 11.0%, and more preferably 10.0%.
[0027] The remainder of the chemical composition of the plating layer 20 in this embodiment contains Zn, with a Zn content of 65.0% or more.
[0028] As described above, the plating layer 20 mainly contains Zn. Specifically, the plating layer 20 contains 65.0% or more Zn by mass. Sufficient corrosion resistance can be obtained if the Zn content of the plating layer 20 is 65.0% or more by mass. The preferred lower limit of the Zn content is 67.5%, and more preferably 70.0%. The preferred upper limit of the Zn content is less than 92.0%, more preferably 90.0%, more preferably 85.0%, and still more preferably 80.0%.
[0029] The chemical composition of the plating layer 20 is further as follows: Sn: greater than 0 to 3.00%, Bi: greater than 0 to 5.00%, In: greater than 0 to 2.00%, Ca: greater than 0 to 3.00%, Y: greater than 0 to 3.00%, La: greater than 0 to 3.00%, Ce: greater than 0 to 3.00%, Si: greater than 0 to 2.50%, Cr: greater than 0 to 0.5%, Ti: greater than 0 to 0.5%, Ni: greater than 0 The mixture may contain one or more elements selected from the group consisting of the following: ~0.5%, Co: greater than 0 to 0.5%, V: greater than 0 to 0.5%, Nb: greater than 0 to 0.5%, Cu: greater than 0 to 0.5%, Mn: greater than 0 to 0.5%, Fe: greater than 0 to 5.0%, Sr: greater than 0 to 0.5%, Sb: greater than 0 to 0.5%, Pb: greater than 0 to 0.5%, and B: greater than 0 to 0.5%. These elements are arbitrary elements. The arbitrary elements will be explained below.
[0030] [Group 1 (Sn, Bi, and In)] The chemical composition of the plating layer 20 may further contain one or more elements selected from the group consisting of tin (Sn), bismuth (Bi), and indium (In). These elements are optional and may not be included. That is, the Sn content, Bi content, and In content may each be 0%. If included, these elements form intermetallic compounds with Mg. As a result, the corrosion resistance of the surface-treated steel sheet is increased. The above effect can be obtained to some extent if even a small amount of one or more of Sn, Bi, and In is included. However, if the content of each of these elements is too high, the viscosity of the plating bath will increase, even if the content of other elements is within the range of this embodiment. Therefore, the Sn content is 0 to 3.00%, the Bi content is 0 to 5.00%, and the In content is 0 to 2.00%.
[0031] The preferred lower limit of the Sn content is greater than 0%, more preferably 0.01%, and even more preferably 0.05%. The preferred upper limit of the Sn content is 2.70%, more preferably 2.50%, even more preferably 2.00%, and even more preferably 1.70%.
[0032] The preferred lower limit of the Bi content is greater than 0%, more preferably 0.01%, and even more preferably 0.05%. The preferred upper limit of the Bi content is 4.80%, more preferably 4.50%, and even more preferably 4.00%.
[0033] The preferred lower limit of the In content is greater than 0%, more preferably 0.01%, and even more preferably 0.05%. The preferred upper limit of the In content is 1.90%, more preferably 1.80%, and even more preferably 1.70%.
[0034] [Second Group (Ca, Y, La, and Ce)] The chemical composition of the plating layer 20 may further contain one or more elements selected from the group consisting of calcium (Ca), yttrium (Y), lanthanum (La), and cerium (Ce). Any of these elements are optional and may not be included. That is, the content of these elements may be 0%. If included, these elements form intermetallic compounds with Al and Zn in the plating layer 20. As a result, the corrosion resistance of the surface-treated steel sheet 1 is increased. Even if only a small amount of these elements is included, the above effect can be obtained to some extent. However, if the content of these elements is too high, oxide dross will increase even if the content of other elements is within the range of this embodiment. Therefore, the Ca content is 0 to 3.00%, the Y content is 0 to 3.00%, the La content is 0 to 3.00%, and the Ce content is 0 to 3.00%.
[0035] The preferred lower limit for the content of each element Ca, Y, La, and Ce is greater than 0%, more preferably 0.01%, more preferably 0.05%, and still more preferably 0.10%. The preferred upper limit for the content of each element Ca, Y, La, and Ce is 2.80%, more preferably 2.50%, and still more preferably 2.00%.
[0036] [Group 3 (Si)] The chemical composition of the plating layer 20 may further contain silicon (Si). Si is an optional element and may not be included. That is, the Si content may be 0%. If included, Si enhances the corrosion resistance of the surface-treated steel sheet 1. Even if only a small amount of Si is included, the above effect can be obtained to some extent. However, if the Si content is too high, the viscosity of the plating bath will increase, even if the content of other elements is within the range of this embodiment. Therefore, the Si content is 0 to 2.50%.
[0037] The preferred lower limit of the Si content is greater than 0%, more preferably 0.01%, more preferably 0.05%, and still more preferably 0.10%. The preferred upper limit of the Si content is 2.00%, more preferably 1.50%, more preferably 1.00%, and still more preferably 0.50%.
[0038] [Group 4 (Cr, Ti, Ni, Co, V, Nb, Cu, and Mn)] The chemical composition of the plating layer 20 may further contain one or more elements selected from the group consisting of chromium (Cr), titanium (Ti), nickel (Ni), cobalt (Co), vanadium (V), niobium (Nb), copper (Cu), and manganese (Mn). Any of these elements are optional and may not be included. That is, the content of these elements may be 0%. If included, these elements improve the appearance quality of the surface-treated steel sheet 1. These elements further form intermetallic compounds with Al in the plating layer 20. As a result, the corrosion resistance of the surface-treated steel sheet 1 is improved. Even if only a small amount of these elements is included, the above effects can be obtained to some extent. However, if the content of these elements is too high, the viscosity of the plating bath will increase, even if the content of other elements is within the range of this embodiment. Therefore, the Cr content is 0-0.5%, the Ti content is 0-0.5%, the Ni content is 0-0.5%, the Co content is 0-0.5%, the V content is 0-0.5%, the Nb content is 0-0.5%, the Cu content is 0-0.5%, and the Mn content is 0-0.5%.
[0039] The preferred lower limit for the content of each element Cr, Ti, Ni, Co, V, Nb, Cu, and Mn is greater than 0%, and more preferably 0.1%. The preferred upper limit for the content of each element Cr, Ti, Ni, Co, V, Nb, Cu, and Mn is less than 0.5%, and more preferably 0.4%.
[0040] [Group 5 (Fe)] The chemical composition of the plating layer 20 may further contain Fe. That is, the Fe content may be 0%. If Fe is included, it increases the hardness of the plating layer 20 and improves the workability of the surface-treated steel sheet 1. Even if only a small amount of Fe is included, the above effect can be obtained to some extent. However, if the Fe content is too high, the hardness of the plating layer 20 may increase even if the content of other elements is within the range of this embodiment. Therefore, the Fe content is 0 to 5.0%.
[0041] The preferred lower limit of the Fe content is greater than 0%, more preferably 0.1%, and even more preferably 0.5%. The preferred upper limit of the Fe content is 4.5%, more preferably 4.0%, and even more preferably 3.5%.
[0042] [Group 6 (Sr, Sb, Pb, and B)] The chemical composition of the plating layer 20 may further contain one or more elements selected from the group consisting of strontium (Sr), antimony (Sb), lead (Pb), and boron (B). Any of these elements are optional and may not be included. That is, the content of these elements may be 0%. If included, these elements enhance the metallic luster of the plating layer 20 and improve the appearance quality of the surface-treated steel sheet 1. Even if only a small amount of these elements is included, the above effects can be obtained to some extent. However, if the content of these elements is too high, oxide dross will increase even if the content of other elements is within the range of this embodiment. Therefore, the Sr content is 0 to 0.5%, the Sb content is 0 to 0.5%, the Pb content is 0 to 0.5%, and the B content is 0 to 0.5%.
[0043] The preferred lower limit for the content of each element, Sr, Sb, Pb, and B, is greater than 0%, and more preferably 0.1%. The preferred upper limit for the content of each element, Sr, Sb, Pb, and B, is less than 0.5%, and more preferably 0.4%. The preferred range for the content of each element, Sr, Sb, Pb, and B, is, for example, greater than 0% to less than 0.5%, and more preferably 0.1% to 0.4%.
[0044] The remainder of the chemical composition of the plating layer 20 may further contain impurities. That is, the chemical composition of the plating layer 20 is: Al: more than 5.0% and less than 25.0%, Mg: more than 3.0% and less than 12.5%, Zn: 65.0% or more, Sn: 0 to 3.00%, Bi: 0 to 5.00%, In: 0 to 2.00%, Ca: 0 to 3.00%, Y: 0 to 3.00%, La: 0 to 3.00%, Ce: 0 to 3.00%, Si: 0 to 2.50%, Cr: 0 The composition contains ~0.5% of the following elements: Ti: 0~0.5%, Ni: 0~0.5%, Co: 0~0.5%, V: 0~0.5%, Nb: 0~0.5%, Cu: 0~0.5%, Mn: 0~0.5%, Fe: 0~5.0%, Sr: 0~0.5%, Sb: 0~0.5%, Pb: 0~0.5%, and B: 0~0.5%, with the remainder of the elements other than those listed above being impurities. Here, impurities refer to substances that are introduced from the raw materials of the plating layer 20 or the manufacturing environment during the industrial production of the surface-treated steel sheet 1, and are acceptable within a range that does not adversely affect the plating layer 20 according to this embodiment. Preferably, the remainder of the chemical composition of the plating layer 20 other than the elements listed above consists of impurities.
[0045] [Preferred amount of plating layer 20] Amount of plating layer 20 (g / m 2 The following are not particularly limited. A preferred amount of plating layer 20 is, for example, 20 to 500 g / m². 2 A more preferable lower limit for the amount of plating layer 20 is 30 g / m². 2 And more preferably 40 g / m 2 And more preferably 50 g / m 2 The preferred upper limit for the amount of plating layer 20 is 400 g / m². 2 And more preferably 300 g / m² 2 And more preferably 200 g / m² 2 That is the case.
[0046] [Method for measuring the chemical composition and adhesion amount of the plating layer 20] The content (mass%) of each element in the chemical composition of the plating layer 20 and the adhesion amount (g / m²) of the plating layer 20. 2 ) can be measured by the following method.
[0047] First, the film thickness of the plating layer 20 and the chemical conversion coating 30 of the surface-treated steel sheet 1 are measured. Specifically, a test piece is taken that includes a cross-section perpendicular to the surface of the surface-treated steel sheet 1, with the cross-section serving as the observation surface. The observation surface is mirror-polished. After mirror polishing, a region of the observation surface that includes the chemical conversion coating 30, the plating layer 20, and at least the surface portion of the base steel sheet 10 is observed using a scanning electron microscope (SEM). An example of an observation magnification is one in which the interface between the chemical conversion coating 30 and the plating layer 20 can be clearly identified, for example, 5000 to 10000 times. However, the observation magnification is not limited to this.
[0048] In the observation field, the chemical conversion coating 30 and the plating layer 20 can be clearly distinguished by contrast. The film thickness (μm) of the plating layer 20 and the film thickness (μm) of the chemical conversion coating 30 are determined at five arbitrary locations in the observation field. The arithmetic mean of the film thicknesses of the plating layer 20 at the five locations is taken as the film thickness (μm) of the plating layer 20. The film thickness of the plating layer 20 is the value obtained by rounding the second decimal place of the obtained arithmetic mean to the first decimal place. Similarly, the arithmetic mean of the film thicknesses of the chemical conversion coating 30 at the five locations is taken as the film thickness (μm) of the chemical conversion coating 30. The film thickness of the chemical conversion coating 30 is the value obtained by rounding the third decimal place of the obtained arithmetic mean to the second decimal place (round up if the third decimal place is 5 or greater, and round down if it is 4 or less).
[0049] Next, multiple test pieces containing the chemical conversion coating 30, the plating layer 20, and the base steel sheet 10 are taken from the surface-treated steel sheet 1. Hereinafter, these test pieces will be referred to as basic test pieces. The thickness of the basic test pieces will be the same as the thickness of the surface-treated steel sheet 1. In one basic test piece, the plating layer 20 and the chemical conversion coating 30 are completely dissolved in an aqueous hydrochloric acid solution containing hexamethylenetetramine. Elemental analysis is performed on the solution using ICP-MS (Inductively Coupled Plasma Mass Spectrometry). This determines the total amount of adhesion (mg / m²) of the plating layer 20 and the chemical conversion coating 30. 2 ) and the mass (mg / m³) of each element contained in the plating layer 20 and the chemical conversion film 30 2 )
[0050] Next, a test specimen for plating layer analysis is prepared using another basic test specimen. Specifically, the chemical conversion coating 30 of the other basic test specimen is removed by polishing. At this time, a depth of the chemical conversion coating 30 + (thickness of the plating layer 20 × 0.30) μm is removed from the surface of the basic test specimen by polishing. By the above method, a test specimen for plating layer analysis consisting of the plating layer 20 and the base steel plate 10 is prepared.
[0051] In a test specimen for plating layer analysis, the plating layer 20 is completely dissolved in an aqueous hydrochloric acid solution containing hexamethylenetetramine. Elemental analysis is performed on the solution by ICP-MS. This determines the provisional deposition amount (mg / m²) of the plating layer 20. 2 ) and the provisional mass (mg / m³) of each element contained in the plating layer 20 2 )
[0052] Here, the thickness of the plating layer 20 of the test piece for plating layer analysis corresponds to 0.70 times the thickness of the plating layer 20 of the surface-treated steel sheet 1. Therefore, the provisional adhesion amount (mg / m) of the obtained plating layer 20 is... 2 ) is multiplied by 1 / 0.70, mg / m 2 g / m 2 The converted value is the amount of plating layer 20 deposited (g / m²). 2 ) Also, the provisional mass of each element (mg / m³) 2 The value obtained by multiplying this by 1 / 0.70 is the mass (mg / m³) of each element in the plating layer 20. 2 ) The amount of plating layer 20 attached (mg / m 2 ) and the mass (mg / m³) of each element in the plating layer 20 2 Based on this, the content (mass%) of each element in the plating layer 20 is determined.
[0053] [About the chemical conversion coating 30] The chemical conversion coating 30 is formed on the surface of the plating layer 20. The chemical conversion coating 30 contains Si, Zr, V, P, Co, and Mg. Each element is described below.
[0054] [Regarding Si in the chemical conversion coating 30] Si in the chemical conversion coating 30 forms the framework of the chemical conversion coating 30. For example, Si is contained in the chemical conversion coating 30 as an organosilicon compound. However, Si may also be contained in the chemical conversion coating 30 as a compound other than an organosilicon compound. As long as Si forms the framework of the chemical conversion coating 30, the form of Si in the chemical conversion coating 30 is not particularly limited.
[0055] Preferably, the chemical conversion coating 30 contains an organosilicon compound. More preferably, the organosilicon compound contains a cyclic siloxane bond. A cyclic siloxane bond refers to a cyclic structure having a continuous Si-O-Si bond configuration and composed of Si and O bonds, with 3 to 8 Si-O repeats. If the organosilicon compound contains a cyclic siloxane bond, the apparent degree of crosslinking of the chemical conversion coating 30 increases. Therefore, excellent corrosion resistance can be obtained.
[0056] Preferably, the organosilicon compound contains the formula -SiR in its molecule. 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 Each of these independently represents an alkoxy group or a hydroxyl group, R 1 , R 2 and R 3 The organosilicon compound contains two or more functional groups (a) represented by (at least one of which represents an alkoxy group), and further contains at least one hydrophilic functional group (b) selected from the group consisting of a hydroxyl group (however, if functional group (a) contains a hydroxyl group, a hydrophilic functional group (b) distinct from that hydroxyl group) and an amino group. When the organosilicon compound contains two or more functional groups (a), the chemical conversion coating 30 becomes even denser. As a result, the corrosion resistance of the chemical conversion coating 30 is further enhanced.
[0057] The preferred average molecular weight of the organosilicon compound is 1,000 to 10,000. The preferred lower limit of the average molecular weight is 1,200, and more preferably 1,300. The preferred upper limit of the average molecular weight is 8,000, more preferably 7,000, and still more preferably 6,000.
[0058] In this specification, the average molecular weight of organosilicon compounds refers to the weight-average molecular weight (Mw) on a standard polystyrene basis, measured by gel permeation chromatography (GPC). This weight-average molecular weight is measured using a high-speed GPC instrument, "HLC-8420GPC EcoSEC Elite" (manufactured by Tosoh Corporation), with two polystyrene-divinylbenzene copolymer packed gel permeation chromatography columns (product name: TSKgel HXL, manufactured by Tosoh Corporation) connected in series. The measurement conditions are tetrahydrofuran as the eluent, a flow rate of 1.0 mL / min, a temperature of 40°C, and an RI (refractive index) detector. The sample to be measured is prepared by dissolving the sample in tetrahydrofuran to a concentration of 1 mg / L, filtering it through a membrane filter with a pore size of 0.2 μm, and injecting 20 μL of this sample into the instrument for measurement. A calibration curve prepared using polystyrene as a standard substance is used to calculate the molecular weight.
[0059] Preferably, the Si mass [Si] in the chemical conversion coating 30 is 5.0 to 1200.0 mg / m². 2 It is. Unit area (1 m 2 The Si mass per unit [Si] is 5.0 mg / m³ 2 If the above is true, excellent corrosion resistance can be obtained. On the other hand, if the Si mass [Si] is 1200.0 mg / m³ 2 Excellent film adhesion can be obtained under the following conditions:
[0060] A more preferable lower limit for the Si mass [Si] is 10.0 mg / m³ 2 And more preferably 20.0 mg / m² 2 And more preferably 30.0 mg / m² 2 A more preferable upper limit for the Si mass [Si] is 1000.0 mg / m³. 2 And more preferably 800.0 mg / m² 2 And more preferably 600.0 mg / m² 2 That is the case.
[0061] [Regarding Zr, V, P, and Co in the Chemical Conversion Coating 30] Zirconium (Zr), vanadium (V), phosphorus (P), and cobalt (Co) in the chemical conversion coating 30 all function as corrosion inhibitors for the surface-treated steel sheet 1, improving the corrosion resistance of the surface-treated steel sheet 1. Zr, V, P, and Co each function effectively as corrosion inhibitors in different corrosive environments. Therefore, the chemical conversion coating 30 contains Zr, V, P, and Co as corrosion inhibitors. As a result, corrosion is suppressed in the surface-treated steel sheet 1 under various corrosive environments, and excellent corrosion resistance is obtained.
[0062] [Regarding Zr in the chemical conversion coating 30] The Zr in the chemical conversion coating 30 increases the degree of crosslinking of the chemical conversion coating 30. As a result, the chemical conversion coating 30 provides excellent barrier properties. Consequently, the surface-treated steel sheet 1 exhibits excellent corrosion resistance. Furthermore, Zr also improves the adhesion of the chemical conversion coating 30 to the plating layer 20.
[0063] Preferably, the Zr mass [Zr] in the chemical conversion coating 30 is 0.1 to 5.0 mg / m². 2 It is. Unit area (1 m 2 The Zr mass [Zr] per unit is 0.1 mg / m³ 2 If the above is achieved, the barrier properties of the chemical conversion coating 30 will be further enhanced, and the corrosion resistance will be further improved. Zr mass [Zr] is 5.0 mg / m 2 The following conditions can suppress the occurrence of cracks in the chemical conversion coating 30, further enhancing corrosion resistance.
[0064] A more preferable lower limit for the Zr mass [Zr] is 0.3 mg / m³ 2 And more preferably 0.5 mg / m² 2 And more preferably 0.8 mg / m² 2 A more preferable upper limit for the Zr mass [Zr] is 4.5 mg / m³. 2 And more preferably 3.5 mg / m² 2 And more preferably 2.5 mg / m² 2 That is the case.
[0065] [Regarding V in the chemical conversion coating 30] V in the chemical conversion coating 30 preferentially dissolves into the plating layer 20 under corrosive conditions. This suppresses the rise in pH due to the dissolution of the plating layer 20. As a result, the corrosion resistance of the surface-treated steel sheet 1 is improved.
[0066] Preferably, the mass of V [V] in the chemical conversion coating 30 is 0.5 to 600.0 mg / m². 2 It is. Unit area (1 m 2 The V mass [V] per unit is 0.5 mg / m 2 If the above is true, the corrosion resistance of the surface-treated steel sheet 1 will be further enhanced. The mass V [V] is 600.0 mg / m². 2 The following conditions further improve the resistance to condensation discoloration of the surface-treated steel sheet 1.
[0067] The preferred lower limit for the mass of V [V] is 1.0 mg / m³ 2 And more preferably 10.0 mg / m² 2 And more preferably 30.0 mg / m² 2 And more preferably 50.0 mg / m² 2 The preferred upper limit for the mass [V] is 500.0 mg / m³. 2 And more preferably 400.0 mg / m² 2 And more preferably 300.0 mg / m² 2 That is the case.
[0068] [Regarding P in the chemical conversion coating 30] The P in the chemical conversion coating 30 forms a passivation film such as zinc phosphate on the surface of the plating layer 20. This passivation film enhances the corrosion resistance of the surface-treated steel sheet 1. The passivation film is formed when metal ions generated by the dissolution of a portion of the plating layer 20 react with P. The passivation film is formed by applying an aqueous surface treatment agent containing P, which is a raw material for the chemical conversion coating 30, to the surface of the plating layer 20 and / or by dissolving a portion of the plating layer 20 in a corrosive environment after the formation of the chemical conversion coating 30.
[0069] Preferably, the P mass [P] in the chemical conversion coating 30 is 1.0 to 1000.0 mg / m². 2 It is. Unit area (1 m 2 The P mass per unit [P] is 1.0 mg / m³ 2If it is at least the above value, the corrosion resistance of the surface-treated steel sheet 1 is further enhanced. The P mass [P] is 1000.0 mg / m 2 If it is not more than the above value, the blackening resistance of the surface-treated steel sheet 1 is further enhanced.
[0070] A preferable lower limit of the P mass [P] is 5.0 mg / m 2 , more preferably 10.0 mg / m 2 , still more preferably 30.0 mg / m 2 , even more preferably 50.0 mg / m 2 . A preferable upper limit of the P mass [P] is 800.0 mg / m 2 , more preferably 700.0 mg / m 2 , still more preferably 600.0 mg / m 2 , even more preferably 500.0 mg / m 2 .
[0071] [Regarding Co in chemical conversion coating 30] Co in the chemical conversion coating 30 improves the blackening resistance and corrosion resistance of the surface-treated steel sheet 1. Al and Mg in the plating layer 20 exhibit a sacrificial anticorrosion effect under corrosive environments. In this case, Zn in the plating layer 20 is oxidized in an oxygen-deficient state and discolors to black. Such a phenomenon is referred to as a blackening phenomenon. The blackening phenomenon is likely to occur in easily soluble portions of the plating layer 20. Co in the chemical conversion coating 30 delays the oxidation rate (corrosion rate) of Zn in the plating layer 20. Thereby, the blackening phenomenon is suppressed, and the blackening resistance of the surface-treated steel sheet 1 is enhanced.
[0072] Preferably, the Co mass [Co] in the chemical conversion coating 30 is 0.5 to 80.0 mg / m 2 . The Co mass [Co] per unit area (1 m 2 ) of 0.5 mg / m 2 or more further enhances the blackening resistance of the surface-treated steel sheet 1. The Co mass [Co] of 80.0 mg / m 2 or less further enhances the corrosion resistance of the surface-treated steel sheet 1.
[0073] A preferable lower limit of the Co mass [Co] is 1.0 mg / m 2 , more preferably 2.0 mg / m 2 , still more preferably 3.0 mg / m2 And more preferably 5.0 mg / m² 2 The preferred upper limit for the Co mass [Co] is 60.0 mg / m³. 2 And more preferably 50.0 mg / m² 2 And more preferably 40.0 mg / m² 2 And more preferably 30.0 mg / m² 2 That is the case.
[0074] [Regarding Mg in the chemical conversion coating 30] The Mg in the chemical conversion coating 30 enhances the condensation discoloration resistance of the chemical conversion coating 30. While the V in the chemical conversion coating 30 enhances corrosion resistance, it may reduce condensation discoloration resistance. If the chemical conversion coating 30 contains Mg, the reduction in condensation discoloration resistance caused by V is suppressed, and excellent condensation discoloration resistance can be obtained.
[0075] Preferably, the Mg mass [Mg] in the chemical conversion coating 30 is 0.2 to 500.0 mg / m². 2 It is. Unit area (1 m 2 The Mg mass per unit [Mg] is 0.2 mg / m³ 2 If the above is true, the resistance to condensation discoloration of surface-treated steel sheet 1 will be further improved. Mg mass [Mg] is 500.0 mg / m² 2 The following conditions result in a sufficiently high crosslink density in the chemical conversion coating 30.
[0076] The preferred lower limit for the Mg mass [Mg] is 0.5 mg / m³. 2 And more preferably 1.0 mg / m² 2 And more preferably 5.0 mg / m² 2 And more preferably 10.0 mg / m² 2 The preferred upper limit for the Mg mass [Mg] is 300.0 mg / m³. 2 And more preferably 200.0 mg / m² 2 And more preferably 150.0 mg / m² 2 And more preferably 100.0 mg / m² 2 That is the case.
[0077] [Method for measuring the mass of Si, Zr, V, P, Co, and Mg in the chemical conversion coating 30] The mass of Si, Zr, V, P, Co, and Mg in the chemical conversion coating 30 can be measured by the following method. In accordance with the method described in [Method for measuring the chemical composition and adhesion amount of the plating layer 20] above, the mass (mg / m³) of each element contained in the plating layer 20 and the chemical conversion coating 30 is measured. 2 ) is determined. Furthermore, the mass of each element in the plating layer 20 (mg / m³) is determined. 2 )
[0078] Mass (mg / m³) of each element contained in the plating layer 20 and the chemical conversion film 30 2 ) From this, the mass of each element in the plating layer 20 (mg / m 2 By subtracting the above, the amount of Si contained in the chemical conversion coating 30 is calculated as follows: [Si] (mg / m 2 ), Zr mass [Zr] (mg / m 2 ), V mass [V] (mg / m 2 ), P mass [P] (mg / m 2 ), Co mass [Co] (mg / m 2 ) and Mg mass [Mg] (mg / m 2 )
[0079] [Regarding the film thickness of the chemical conversion coating 30] The film thickness of the chemical conversion coating 30 is 0.03 to 2.00 μm. If the film thickness of the chemical conversion coating 30 is less than 0.03 μm, the formed chemical conversion coating 30 is too thin. In this case, the corrosion resistance of the surface-treated steel sheet 1 will decrease. On the other hand, if the film thickness of the chemical conversion coating 30 exceeds 2.00 μm, the formed chemical conversion coating 30 is too thick. In this case, excellent appearance cannot be obtained. If the film thickness of the chemical conversion coating 30 is between 0.03 and 2.00 μm, the film thickness of the chemical conversion coating 30 is appropriate. In this case, sufficient corrosion resistance can be obtained in the surface-treated steel sheet 1. The preferred lower limit for the film thickness of the chemical conversion coating 30 is 0.20 μm, more preferably 0.27 μm, and still more preferably 0.33 μm. The preferred upper limit for the thickness of the chemical conversion coating 30 is 1.00 μm, more preferably 0.80 μm, and even more preferably 0.67 μm.
[0080] The preferred amount of the chemical conversion coating 30 is 50 to 3000 mg / m². 2The preferred lower limit for the amount of the chemical conversion coating 30 is 300 mg / m². 2 And more preferably 400 mg / m² 2 And more preferably 500 mg / m² 2 The preferred upper limit for the amount of the chemical conversion coating 30 is 1500 mg / m². 2 And more preferably 1200 mg / m² 2 And more preferably 1000 mg / m² 2 That is the case.
[0081] [Method for measuring the thickness of the chemical conversion coating 30] The thickness of the chemical conversion coating 30 can be determined by the method described in [Method for measuring the chemical composition and adhesion amount of the plating layer 20].
[0082] [Method for measuring the amount of chemical conversion coating 30] The amount of chemical conversion coating 30 can be determined by the following method. In accordance with the method described in [Method for measuring the chemical composition and amount of coating of plating layer 20] above, the total amount of coating (mg / m²) of the plating layer 20 and the chemical conversion coating 30 is determined. 2 Furthermore, the amount of plating layer 20 (mg / m²) is determined. 2 )
[0083] Total amount of plating layer 20 and chemical conversion film 30 (mg / m 2 ) From the amount of plating layer 20 (mg / m 2 Subtracting this, the amount of chemical conversion coating 30 attached (mg / m 2 )
[0084] [Regarding the depth profile obtained by glow discharge emission spectroscopy] In the surface-treated steel sheet 1 of this embodiment, glow discharge emission spectroscopy is performed from the surface of the chemical conversion coating 30 in the film thickness direction (depth direction) to obtain a depth profile showing the relationship between sputtering time and the emission intensity of elements in the chemical conversion coating 30. The depth profile satisfies the following two characteristics: (Characteristic 1) The sputtering time t at which the emission intensity of Mg reaches its first peak intensity from the start of sputtering. Mg However, the sputtering time t at which the Si emission intensity reaches its peak intensity is... Si Faster than (Feature 2) Sputtering time t Mg Peak intensity of Mg at I Mgand sputtering time t Si The peak intensity of Si at I Si This satisfies equation (1). 0.10 ≤ I Mg / I Si ≤ 1.00 (1) Features 1 and 2 will be explained below.
[0085] [Regarding Features 1 and 2] Figure 2 is a diagram showing an example of a depth-direction profile that shows the relationship between sputtering time and the emission intensity of elements in the chemical conversion film, obtained by performing glow discharge optical emission spectroscopy (GD-OES) analysis from the surface of the chemical conversion film 30 in the film thickness direction (depth direction) on a surface-treated steel sheet 1. The curves shown for Si, V, P, and Mg in the figure are the depth-direction profiles of each element.
[0086] Referring to Figure 2, in the depth profile, the emission intensity of P is equal to the sputtering time t. P It shows an intensity peak. Subsequently, as the sputtering time progresses, the emission intensity of P gradually decreases. In the chemical composition of the plating layer 20, the P content is at the impurity level. Therefore, in the depth direction profile, the region of the conversion coating 30 can be defined based on the emission intensity profile of P.
[0087] In this embodiment, in the depth profile, the emission intensity of P is equal to the sputtering time t. P At intensity peak I P After that, the sputtering time t when the luminescence intensity becomes half of the peak intensity is reached. P/2 This is the interface between the chemical conversion coating 30 and the plating layer 20. Therefore, in this embodiment, the sputtering time is 0 to sputtering time t. P/2 The region corresponding to this is considered to be the region of the chemical conversion coating 30. Therefore, the sputtering time t P/2 The subsequent sputtering time region is the region of the plating layer 20.
[0088] In the region of the chemical conversion coating 30 of this embodiment, the luminescence intensity of Si, which is the main component of the chemical conversion coating 30, increases from the surface as the sputtering time progresses, and the sputtering time t Si And one intensity peak I SiIt forms and then decreases as the sputtering time progresses. In other words, the depth profile of Si has a single intensity peak.
[0089] On the other hand, the depth profile of Mg shows a different distribution from that of Si. Specifically, the emission intensity of Mg is determined by the sputtering time t. Si Faster sputtering time t Mg The first peak intensity I Mg This is shown. Subsequently, the emission intensity of Mg decreases as the sputtering time progresses (Feature 1).
[0090] The emission intensity of Mg is determined by the sputtering time t. Si It rises again in the vicinity, sputter time t Si Slower sputtering time t Mg2 And the first peak intensity I Mg The second peak intensity I is higher than Mg2 This shows that the depth profile of Mg in the chemical conversion coating 30 has two intensity peaks (I Mg and I Mg2 ) indicates.
[0091] Also, sputtering time t Si and t Mg is the sputtering time t P/2 Faster than that. In other words, sputtering time t Si and t Mg This is within the region of the chemical conversion coating 30.
[0092] Furthermore, the sputtering time t Mg Peak intensity of Mg at I Mg and sputtering time t Si The peak intensity of Si at I Si The equation (1) is satisfied. 0.10 ≤ I Mg / I Si ≤ 1.00 (1)
[0093] In the chemical conversion coating 30 of this embodiment, in the depth direction of the chemical conversion coating 30, the luminescence intensity of Mg is equal to the luminescence intensity of Si, with peak intensity I Si The sputtering time t is such that Si Faster sputtering time t Mg And the first peak intensity I MgThis indicates that, near the surface of the chemical conversion coating 30, there is a peak intensity I Mg This means that a region of Mg enrichment is formed. Hereafter, this Mg enrichment region will also be referred to as the "surface Mg enrichment region."
[0094] Here, we define F1 as follows: F1 = I Mg / I Si If F1 is 0.10 or higher, the Mg concentration in the surface Mg-enriched region of the chemical conversion coating 30 is sufficiently high. Therefore, condensation discoloration caused by V in the chemical conversion coating 30 can be sufficiently suppressed, and excellent resistance to condensation discoloration can be obtained. If F1 is 1.00 or lower, the crosslinking density in the chemical conversion coating 30 becomes sufficiently high, and the barrier properties are enhanced. Therefore, F1 is between 0.10 and 1.00.
[0095] The preferred lower limit of F1 is 0.12, more preferably 0.15, more preferably 0.18, more preferably 0.20, more preferably 0.22, and more preferably 0.25. The preferred upper limit of F1 is 0.95, more preferably 0.90, more preferably 0.80, more preferably 0.75, more preferably 0.70, more preferably 0.65, and more preferably 0.60.
[0096] [Method for measuring depth profile and determining F1] The depth profile and F1 can be determined by the following method. First, a test piece having the same thickness as the surface-treated steel sheet 1 is taken from the surface-treated steel sheet 1. The size of the test piece is not particularly limited, as long as it includes the measurement area described later. For example, the size of the test piece is 50 mm × 50 mm × thickness.
[0097] In the collected test specimen, glow discharge emission spectroscopy is performed from the surface of the chemical conversion coating 30 in the thickness direction (depth direction) of the chemical conversion coating 30 to obtain a depth direction profile showing the relationship between the emission intensity of Si, P, and Mg in the chemical conversion coating 30 and the sputtering time. Here, the thickness direction of the chemical conversion coating 30 is considered to be the thickness direction of the base steel plate 10 of the test specimen. A high-frequency glow discharge emission spectrometer is used for the measurement. Under an argon atmosphere (Ar pressure: 3 hPa), the test specimen is used as the cathode and a power output of 30 W is applied. The diameter of the measurement area is 4 mm, the measurement time is 200 seconds, and the measurement interval is 0.025 seconds. For example, a high-frequency glow discharge emission spectrometer, product name: GDA750 manufactured by Rigaku Corporation, is used.
[0098] From the obtained depth profile, the emission intensity of P is the peak intensity I P The sputtering time t is such that P (Seconds) is calculated. Furthermore, the P emission intensity is the peak intensity I P Sputtering time t becomes 1 / 2 of the original time. P/2 Calculate the time in seconds. Sputtering time 0 to sputtering time t P/2 The region corresponding to this is considered to be the region of the chemical conversion coating 30.
[0099] Furthermore, from the obtained depth profile, the peak intensity I of the Si emission intensity was determined. Si and sputtering time t Si (seconds), and the first peak intensity I of the Mg emission intensity Mg and sputtering time t Mg The time in seconds is calculated. The obtained sputtering time t Si and t Mg By comparing these, we determine whether or not Feature 1 is satisfied. Note that the sputtering time t Si and t Mg is the sputtering time t P/2 Faster than that. In other words, sputtering time t Si and t Mg This is within the region of the chemical conversion coating 30. Furthermore, the obtained peak intensity I Si and I Mg Based on this, F1 is calculated. Note that F1 is the value obtained by rounding the third decimal place of the result to two decimal places.
[0100] Furthermore, as shown in Figure 3, in the depth profile of Mg, the emission intensity increases with the progression of sputtering time, then decreases slightly, and a provisional intensity peak PI is observed. Mg In some cases, a temporary intensity peak PI may be formed. Mg After formation, the emission intensity decreases over time, but the emission intensity reaches a provisional peak PI. Mg Before it drops by more than 10%, the luminescence intensity rises again, and a provisional intensity peak PI Mg If the emission intensity is higher than the specified value, the provisional intensity peak PI Mg This will not be recognized as an intensity peak.
[0101] In the depth profile of Mg in Figure 3, the emission intensity of Mg increases with the sputtering time, and the emission intensity PI Mg Although it decreases from, the luminescence intensity PI Mg It has risen again without falling by more than 10%. And the luminescence intensity I Mg After reaching the emission intensity, the emission intensity becomes emission intensity I Mg It has decreased by more than 10%. Therefore, in Figure 3, the luminescence intensity PI Mg Without recognizing it as the intensity peak, the luminescence intensity I Mg This is identified as the intensity peak.
[0102] [Effects of Surface-Treated Steel Sheet 1] In the surface-treated steel sheet 1 of this embodiment, the plating layer 20 and the chemical conversion film 30 have the above-described chemical composition, the thickness of the chemical conversion film 30 is 0.03 to 2.00 μm, and the chemical conversion film 30 satisfies features 1 and 2. Therefore, the surface-treated steel sheet 1 of this embodiment provides excellent corrosion resistance and excellent resistance to blackening, and furthermore, excellent resistance to condensation discoloration.
[0103] [Method for Manufacturing Surface-Treated Steel Sheet 1] An example of a method for manufacturing the surface-treated steel sheet of this embodiment will be described. The surface-treated steel sheet having the above-described configuration may be manufactured by methods other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing the surface-treated steel sheet according to this embodiment.
[0104] An example of the manufacturing method for surface-treated steel sheets according to this embodiment includes the following steps: (Step 1) Base material steel sheet preparation step (Step 2) Plating layer formation step (Step 3) Chemical conversion film formation step Each step will be described below.
[0105] [(Step 1) Preparation of base steel sheet] In the preparation of base steel sheet, the base steel sheet 10 described above is prepared.
[0106] [(Step 2) Plating layer formation step] In the plating layer formation step, a plating treatment (hot-dip plating treatment) is performed on the base steel sheet 10 to form a plating layer 20 on the surface of the base steel sheet 10. Specifically, a plating bath is prepared. The composition of the plating bath is adjusted according to the composition of the plating layer 20 to be formed. After immersing the base steel sheet 10 in the plating bath for a certain period of time, the base steel sheet 10 is pulled out of the plating bath by a well-known method. For example, a sink roll is placed in the plating bath. The direction of movement of the base steel sheet 10 immersed in the plating bath is changed upward by the sink roll.
[0107] The surface of the base steel sheet 10, which has been removed from the plating bath, has plating attached to it. The amount of plating attached to the base steel sheet 10 is adjusted using a well-known gas wiping device. The plating attached to the base steel sheet 10, which has been removed from the plating bath, is cooled. The plating solidifies through cooling, forming a plating layer 20.
[0108] [(Step 3) Chemical Conversion Film Formation Step] The chemical conversion film formation step includes the following steps: (Step 31) Plating surface activation step (Step 32) Water-based surface treatment agent application step (Step 33) Mg diffusion step (Step 34) Drying step In the chemical conversion film formation step, a chemical conversion film 30 is formed. At this time, a portion of the Mg in the plating layer 20 is diffused into the chemical conversion film 30. As a result, the chemical conversion film 30 contains Mg. The diffusion of Mg from the plating layer 20 into the chemical conversion film 30 is achieved by the plating surface activation step and the Mg diffusion step. Each step will be described below.
[0109] [(Step 31) Plating surface activation step] In the plating surface activation step, before applying the aqueous surface treatment agent, which is the raw material for the chemical conversion film 30, to the surface of the plating layer 20, an acidic chemical solution is applied to the plating layer 20 to activate the surface of the plating layer 20. This makes it easier for Mg in the plating layer 20 to dissolve.
[0110] At this time, the pH of the acidic solution should be 3.0 or less. If the pH exceeds 3.0, the surface of the plating layer 20 may not be sufficiently activated. In this case, the manufactured surface-treated steel sheet may not satisfy characteristic 1 or characteristic 2. The lower limit of the pH is not particularly limited, but for example, it is 1.0. The pH of the acidic solution can be measured, for example, using a pH meter (model number: HM-30R) manufactured by Toa DKK Corporation at a measurement temperature of 25°C. The acidic solution is, for example, an aqueous solution of cobalt nitrate or an aqueous solution of cobalt sulfate.
[0111] Furthermore, the surface is held for at least 2.0 seconds after the application of the acidic chemical solution until the application of the aqueous surface treatment agent in the next step. If the holding time is less than 2.0 seconds, the surface of the plating layer 20 may not be sufficiently activated. In this case, the manufactured surface-treated steel sheet may not satisfy feature 1 or feature 2. The upper limit of the holding time is not particularly limited, but for example, it is 60.0 seconds.
[0112] [(Step 32) Water-based surface treatment agent application step] In the water-based surface treatment agent application step, a water-based surface treatment agent is applied to the surface of the plating layer 20 after the plating surface activation step.
[0113] [Regarding Aqueous Surface Treatment Agents] Aqueous surface treatment agents are not particularly limited as long as they contain Si, Zr, V, P, and Co in amounts that constitute the chemical conversion film 30. Aqueous surface treatment agents include, for example, silane coupling agents, zirconium compounds, vanadium compounds, phosphorus compounds, and cobalt compounds. Each compound will be described below.
[0114] [Silane Coupling Agent] The aqueous surface treatment agent contains, as a raw material for organosilicon compounds, a silane coupling agent (A) containing at least one amino group in its molecule and a silane coupling agent (B) containing at least one glycidyl group in its molecule, in a solid content mass ratio [(A) / (B)] of 0.5 to 1.7.
[0115] Silane coupling agents (A) and silane coupling agents (B) are not particularly limited. Silane coupling agent (A) is, for example, one or more selected from the group consisting of 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane. Silane coupling agent (B) is, for example, one or more selected from the group consisting of 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and 3-glycidoxypropylmethyldimethoxysilane.
[0116] [Zirconium Compounds] The zirconium compounds contained in aqueous surface treatment agents are not particularly limited. For example, the zirconium compound is one or more selected from the group consisting of zirconium hydrofluoric acid, zirconium ammonium fluoride, zirconium sulfate, zirconium oxychloride, zirconium nitrate, zirconium acetate, and zirconium carbonate compounds. For example, the zirconium carbonate compound is one or more selected from the group consisting of zirconium carbonate, zirconium ammonium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate.
[0117] [Vanadium Compounds] The vanadium compounds contained in aqueous surface treatment agents are not particularly limited. For example, vanadium compounds are obtained by reducing a pentavalent vanadium compound to a divalent to tetravalent vanadium compound with a reducing agent, or vanadium compounds with an oxidation state of 4 to 2. Specifically, the vanadium compound is vanadium pentoxide (V 2 O 5 ), metavanadic acid (HVO 3 ), ammonium metavanadate, sodium metavanadate and vanadium oxytrichloride (VOCl 3 ) reduced to divalent to tetravalent with a reducing agent, and vanadium trioxide (V 2 O3 ), vanadium dioxide (VO 2 ), vanadium oxysulfate (VOSO 4 ), vanadium oxyoxalate [VO(COO) 2 ], vanadium oxyacetylacetonate [VO(OC(CH 3 ) = CHCOCH 3 ) 2 ], vanadium acetylacetonate [V (OC (CH 3 ) = CHCOCH 3 ) 3 ], vanadium trichloride (VCl 3 ), Lymphanadomolybdate {H 15-x [PV] 12-x Mo x O 40 ]・nH 2 O (6 < x < 12, n < 30), vanadium sulfate (VSO 4 8H 2 O), vanadium chloride (VCl 2 It is one or more selected from the group consisting of ) and vanadium oxide (VO).
[0118] [Phosphorus Compounds] The phosphorus compounds contained in aqueous surface treatment agents are not particularly limited. For example, the phosphorus compounds are one or more selected from the group consisting of phosphoric acid, ammonium phosphate salts, potassium phosphate salts, sodium phosphate salts, inorganic acid anions having a phosphorus-containing acid group, and organic acid anions having a phosphorus-containing acid group.
[0119] Inorganic acid anions having a phosphorus-containing acid group are, for example, inorganic acid anions or salts thereof obtained by liberating at least one hydrogen atom from an inorganic acid. Specifically, inorganic acid anions having a phosphorus-containing acid group are one or more selected from the group consisting of inorganic acid anions obtained by liberating at least one hydrogen atom from any of orthophosphoric acid, metaphosphoric acid, condensed phosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, tetraphosphoric acid, and hexametaphosphoric acid, as well as their salts.
[0120] Organic acid anions having a phosphorus-containing acid group are, for example, organic acid anions or salts thereof in which at least one hydrogen atom of an organic phosphonic acid or organic phosphoric acid has been liberated. Specifically, the organic acid anions having a phosphorus-containing acid group are one or more selected from the group consisting of organic acid anions in which at least one hydrogen atom is liberated from any of the organic phosphonic acids such as 1-hydroxymethane-1,1-diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, 1-hydroxypropane-1,1-diphosphonic acid, 1-hydroxyethylene-1,1-diphosphonic acid, 2-hydroxyphosphonoacetic acid, aminotri(methylenephosphonic acid), ethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), hexamethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), diethylenetriamine-N,N,N',N'',N''-penta(methylenephosphonic acid), 2-phosphonate butane-1,2,4-tricarboxylic acid, inositol hexaphosphonic acid, and phytic acid, as well as their salts.
[0121] [Cobalt Compounds] The cobalt compounds contained in aqueous surface treatment agents are not particularly limited. For example, the cobalt compound is one or more selected from the group consisting of cobalt sulfate, cobalt nitrate, and cobalt carbonate.
[0122] [Lubricant] The water-based surface treatment agent may further contain a lubricant. In other words, the lubricant is an optional component and may not be included. If included, the lubricant enhances the scratch resistance of the surface-treated steel sheet 1. The lubricant is, for example, one or more selected from the group consisting of polyethylene wax, oxidized polyethylene wax, and oxidized polypropylene wax.
[0123] [Regarding the pH of the aqueous surface treatment agent] Preferably, the pH of the aqueous surface treatment agent is 4.0 to 6.5. The pH of the aqueous surface treatment agent can be measured at a measurement temperature of 25°C using, for example, a pH meter (model number: HM-30R) manufactured by Toa DKK Corporation.
[0124] The adjusting agent used to adjust the pH of an aqueous surface treatment agent is not particularly limited. For example, the adjusting agent may be one or more selected from the group consisting of ammonia, guanidine carbonate, carbonic acid, acetic acid, and hydrofluoric acid.
[0125] [Regarding other additives] The water-based surface treatment agent may further contain, as needed, alcohol, ketone, cellosolve-based water-soluble solvent, surfactant, defoamer, leveling agent, antibacterial and antifungal agent, thickener, conductive substance for improving weldability, coloring pigment and matting material for improving aesthetics. The content of these components is preferably less than 5% by mass relative to the total solid content of the water-based surface treatment agent.
[0126] [Preparation of Aqueous Surface Treatment Agent] The aqueous surface treatment agent is obtained by mixing the above-mentioned components with water such as deionized water and distilled water. Preferably, in the resulting chemical conversion film 30, the Si mass [Si] is 5.0 to 1200.0 mg / m². 2 , Zr mass [Zr] is 0.1 to 5.0 mg / m³ 2 , V mass [V] is 0.5 to 600.0 mg / m 2 , P mass [P] is 1.0 to 1000.0 mg / m³ 2 Co mass [Co] is 0.5 to 80.0 mg / m³ 2 The content of each compound is adjusted to achieve the desired result.
[0127] The above-mentioned aqueous surface treatment agent is applied to the surface of the plating layer 20 by a well-known method to form a coating film. For example, the aqueous surface treatment agent is applied using a roll coater. In this case, the film thickness can be adjusted by adjusting the peripheral speed ratio of the roll coater. The amount of the chemical conversion coating 30 is 50 to 3000 mg / m². 2 The film thickness of the coating is adjusted to achieve the desired result.
[0128] [(Step 33) Mg Diffusion Step] In the Mg diffusion step, before carrying out the drying step, the Mg in the plating layer 20 is diffused into the coating of the water-based surface treatment agent. Specifically, after applying the water-based surface treatment agent to the surface of the plating layer 20 in the water-based surface treatment agent application step, the steel sheet is held for 2.0 to 3.8 seconds with the coating of the water-based surface treatment agent formed before being inserted into the drying oven in the next drying step. Hereinafter, this holding time will be referred to as the "holding diffusion time".
[0129] If the holding diffusion time is less than 2.0 seconds, Mg will not diffuse sufficiently into the coating film of the aqueous surface treatment agent. In this case, in the depth profile of Mg in the chemical conversion film 30 after manufacturing, the first peak intensity of the emission intensity of Mg I Mg In some cases, the expression may not occur, or F1 may fall below the lower limit of equation (1).
[0130] On the other hand, if the retention diffusion time exceeds 3.8 seconds, the chemical conversion film 30 will contain an excess of Mg. In this case, the first peak curve of the emission intensity of Mg may become broad in the depth profile of Mg. In this case, the peak intensity I Mg Sputtering time t shown Mg However, sputtering time t Si It may be slower than that. Also, F1 may exceed the upper limit of equation (1). Therefore, the holding diffusion time is set to 2.0 to 3.8 seconds.
[0131] The holding and diffusion time can be determined based on the distance from the point where the aqueous surface treatment agent is applied to the entrance of the drying oven and the sheet passing speed.
[0132] [(Step 34) Drying Step] In the drying step, the steel sheet after the Mg diffusion step is inserted into a drying oven to dry the water-based surface treatment agent coating and form a chemical conversion film 30. The drying temperature is, for example, 50 to 180°C. The holding time at the drying temperature is, for example, 1 to 60 seconds.
[0133] The surface-treated steel sheet 1 of this embodiment is manufactured through the above process.
[0134] The effects of the surface-treated steel sheet of this embodiment will be further explained in detail by the following examples. The conditions in the following examples are just one example of conditions adopted to confirm the feasibility and effects of the surface-treated steel sheet of this embodiment. Therefore, the surface-treated steel sheet of this embodiment is not limited to this one example of conditions.
[0135] A base steel sheet was prepared in which a plating layer having the chemical composition described in Table 1 (Table 1A and Table 1B) was formed.
[0136]
[0137]
[0138] The plating layer was formed by hot-dip galvanizing. The amount of plating layer adhered was 40 to 300 g / m² in all test numbers. 2 It was within the range. The amount of plating layer adhesion for each test number was determined by the method described in [Method for measuring the chemical composition and adhesion amount of plating layer 20] above.
[0139] The aqueous surface treatment agents shown in Table 2 were prepared by the following method. Each component shown in Table 2 was added to a fixed amount of deionized water while being stirred using a propeller agitator, until the solid content concentration reached 10% by mass. The pH of the aqueous surface treatment agent was adjusted to 4.0–6.5. Carbonic acid and / or ammonia were used as pH adjusters for the aqueous surface treatment agent. The types of each component shown in Table 2 are as follows. Note that the content in Table 2 represents the mass percentage relative to the total solid content of the aqueous surface treatment agent.
[0140]
[0141] [Coupling Agents] The following compounds were prepared as coupling agents: A1: 3-aminopropyltriethoxysilane (silane coupling agent (A)) A2: 3-glycidoxypropyltrimethoxysilane (silane coupling agent (B)) A3: 3-aminopropyltrimethoxysilane (silane coupling agent (A)) A4: 3-glycidoxypropylmethyldimethoxysilane (silane coupling agent (B)) The solid content mass ratio of A1 to A2 (A1 / A2) was adjusted to 0.5 to 1.7. The solid content mass ratio of A3 to A4 (A3 / A4) was also adjusted to 0.5 to 1.7.
[0142] The following compounds were prepared as Zr compounds, V compounds, P compounds, and Co compounds: [Zirconium compounds (Zr compounds)] The following three compounds were prepared as Zr compounds: B1: Potassium zirconium carbonate B2: Ammonium zirconium carbonate B3: Ammonium zirconium fluoride [Vanadium compounds (V compounds)] C1: Vanadium acetylacetonate C2: Vanadium oxyoxalate [Phosphorus compounds (P compounds)] D1: Phosphoric acid D2: 1-Hydroxyethane-1,1-diphosphonic acid [Co compounds] E1: Cobalt carbonate E2: Cobalt nitrate
[0143] An acidic solution was applied to the plating layer of steel plates with plating layers formed on both sides, as shown in Table 1 (indicated as "Applied" in the "Acidic Solution" column of Table 3). The acidic solution was an aqueous cobalt sulfate solution. The pH of the acidic solution was as shown in Table 3. The time between the application of the acidic solution and the application of the aqueous surface treatment agent in the next step (holding time after application of acidic solution) was as shown in Table 3. In tests 29 and 30, the acidic solution was not applied to the surface of the plating layer (indicated as "Not Applied" in the "Acidic Solution" column of Table 3).
[0144] A water-based surface treatment agent was applied to the surface of the plated layer of the steel sheet after the plated surface activation process. Specifically, the water-based surface treatment agent was applied using a roll coater. At this time, the film thickness of the coating was adjusted by adjusting the peripheral speed ratio of the roll coater. In tests 29 and 30, the plated surface activation process was not performed, and the water-based surface treatment agent was applied to the surface of the plated layer. The pH of the water-based surface treatment agent in each test was 4.0 to 6.5.
[0145] For each test number, the time (holding and diffusion time) (seconds) from the application of the water-based surface treatment agent to the insertion of the steel sheet into the drying oven was as shown in Table 3. In the drying process, the drying temperature (°C) and the holding time (drying time) (seconds) at the drying temperature for each test number were as shown in Table 3.
[0146]
[0147] The surface-treated steel sheets for each test number were manufactured using the above process. The thickness of the base steel sheet for each surface-treated steel sheet for each test number was 2.3 mm.
[0148] [Evaluation Tests] The following evaluation tests were performed on the surface-treated steel sheets for each test number: (Test 1) Chemical composition analysis test of the plating layer (Test 2) Thickness measurement test of the chemical conversion coating (Test 3) Measurement test of Si mass, Zr mass, V mass, P mass, Co mass and Mg mass in the chemical conversion coating (Test 4) Depth profile measurement and F1 determination test (Test 5) Corrosion resistance evaluation test (Test 6) Blackening resistance evaluation test (Test 7) Condensation discoloration resistance evaluation test Tests 1 to 7 are described below.
[0149] [(Test 1) Chemical Composition Analysis Test of the Plating Layer] Based on the method described in [Method for Measuring the Chemical Composition and Adhesion Amount of Plating Layer 20] above, the content (mass%) of each element in the chemical composition of the plating layer for each test number was determined. As a result, the chemical composition of the plating layer for each test number was as shown in Table 1 (Table 1A and Table 1B).
[0150] [(Test 2) Measurement Test of Chemical Conversion Coating Thickness] Based on the method described in [Method for Measuring the Thickness of Chemical Conversion Coating 30] above, the thickness (μm) of the chemical conversion coating for each test number was measured. The results obtained are shown in the "Chemical Conversion Coating Thickness (μm)" column of Table 4.
[0151]
[0152] [(Test 3) Measurement test of Si mass, Zr mass, V mass, P mass, Co mass and Mg mass in the chemical conversion coating] Based on the method described in [Method for measuring Si mass, Zr mass, V mass, P mass, Co mass and Mg mass in the chemical conversion coating 30] above, the Si mass [Si] (mg / m³) in the chemical conversion coating for each test number was measured. 2 ), Zr mass [Zr] (mg / m 2 ), V mass [V] (mg / m 2 ), P mass [P] (mg / m 2 ), Co mass [Co] (mg / m 2 ) and Mg mass [Mg] (mg / m 2 The following was calculated. The results are shown in Table 4.
[0153] [(Test 4) Depth Profile Measurement and F1 Determination Test] Based on the method described in [Method for Depth Profile Measurement and F1 Determination] above, the depth profile was determined for each chemical conversion coating of the test number, and the peak intensity I Si and sputtering time t Si , and also, peak intensity I Mg and sputtering time t Mg We calculated and then calculated F1. The results obtained are shown in Table 4 as "t Mg <t Si This is shown in the "" column and the "F1" column. Mg <t Si In the column, "T (True)" represents the sputtering time t. Mg Sputtering time t Si This indicates that it was faster than [the specified time]. "F (False)" represents the sputtering time t. Mg Sputtering time t Si Same as or the sputtering time t Si This indicates that it was slower than [the specified value]. "-" indicates peak intensity I Mg This indicates that it did not appear.
[0154] [(Test 5) Corrosion Resistance Evaluation Test] Flat test pieces were taken from the surface-treated steel plates of each test number. The size of the flat test pieces was 50 mm x 100 mm x plate thickness. A salt spray test in accordance with JIS Z 2371:2015 was performed on the flat test pieces for 72 hours. The surface of the flat test pieces was observed after the test, and the area percentage of white rust was determined. Based on the obtained area percentage of white rust, the following evaluation was performed: E (Excellent): Area percentage of white rust is 5.0% or less B (Bad): Area percentage of white rust is greater than 5.0% The results obtained are shown in the "Corrosion Resistance" column in Table 4.
[0155] [(Test 6) Blackening Resistance Evaluation Test] Test specimens measuring 50 mm x 100 mm x plate thickness were taken from the surface-treated steel plates of each test number. Using a constant temperature and humidity testing machine, the test specimens were stacked and left standing for 168 hours in an atmosphere of 50°C and 80% relative humidity (RH).
[0156] L * Value, a * Value and b * The value was determined. Specifically, the surface of the test specimen before and after the test was examined using a CIE standard light source D65 as the light source, with a viewing angle of 10°, and the value was calculated using the SCE method with CIE LAB display colors L. * Value, a * Value and b * The value was calculated. The definition of the SCE method is specified in JIS Z 8722:2009. L before and after the test. * Value, a * Value and b * Based on the value, the color difference ΔE is calculated using the following formula. * We calculated ΔE. * = {(ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2} 1/2 ΔL * = L after the exam * - L before the exam * Δa * = a after the exam * - a before the exam * Δb* = b after the exam * - Before the exam * Note that L before and after the exam * Value, a * value, and b * The values were obtained using a colorimeter manufactured by Konica Minolta, Inc. (product name: CM-2600d). * Based on this, the resistance to blackening was evaluated as follows: E (Excellent): ΔE * ≦3.0 B (Bad): ΔE * >3.0 The results obtained are shown in the "Blackening Resistance" column of Table 4.
[0157] [(Test 7) Dewiness Resistance Evaluation Test] A 50 mm x 100 mm x thickness test piece was taken from each surface-treated steel plate of the test number. Pure water was dropped one drop at each of 12 locations on the surface of the test piece. At this time, the droplets were placed in separate areas so that they did not come into contact with each other. The test piece was left in the air at room temperature for 12 hours after the pure water was dropped to allow the water droplets to dry. After 12 hours, the color difference (ΔE) between the undropped area (normal area) and the dropped area was measured for each of the 12 dropped areas. * The color difference was measured. A colorimeter manufactured by Konica Minolta, Inc. (product name: CM-2600d) was used to measure the color difference. In the measurement, a D65 light source was used, and under the conditions of a viewing angle of 10° and a measurement diameter of Φ3 mm, L * a * b * Each value in the color system was measured. The center of the drying mark in each droplet area and the surrounding normal area were measured, and the color difference (ΔE) was calculated from the obtained values. * ) was calculated. Based on the calculation results, the measured value is ΔE * Regions where ≤ 3.0 are classified as "no discoloration", ΔE * Areas with a rating of >3.0 were judged as "discolored," and the number of areas judged as "discolored" (discolored areas) was counted. The resistance to condensation discoloration was evaluated as follows according to the number of discolored areas: E: Two or fewer discolored areas. G: Three to five discolored areas. B: Six or more discolored areas. The results obtained are shown in the "Resistance to Condensation Discoloration" column in Table 4. In the case of evaluation E, it was determined that excellent resistance to condensation discoloration was obtained.
[0158] [Evaluation Results] Referring to Tables 1 to 4, the surface-treated steel sheets of test numbers 1 to 28 had an appropriate chemical composition of the plating layer, and the conversion coating contained Si, Zr, V, P, Co, and Mg. Furthermore, the thickness of the conversion coating was appropriate, and features 1 and 2 were also satisfied. As a result, these surface-treated steel sheets of test numbers showed excellent corrosion resistance and excellent resistance to blackening, and furthermore, excellent resistance to condensation discoloration.
[0159] On the other hand, in test numbers 29 and 30, the plating surface activation process was not performed. Therefore, in test number 29, the peak intensity was I Mg The desired result did not appear. Furthermore, in test number 30, F1 was too low. As a result, sufficient resistance to condensation discoloration was not achieved.
[0160] In tests 31 and 32, the pH of the acidic chemical solution was too high during the plating surface activation process. As a result, peak intensity I Mg The desired result did not occur. As a result, sufficient resistance to condensation discoloration was not achieved.
[0161] In tests 33 and 34, the holding time after application of the acidic chemical solution during the plating surface activation process was too short. As a result, the peak intensity I Mg The desired result did not occur. As a result, sufficient resistance to condensation discoloration was not achieved.
[0162] In tests 35 and 36, the holding diffusion time in the Mg diffusion process was too short. Therefore, in test 35, the peak intensity was I Mg The desired result did not appear. Furthermore, in test number 36, F1 was too low. As a result, sufficient resistance to condensation discoloration was not achieved.
[0163] In tests 37 and 38, the holding diffusion time in the Mg diffusion process was too long. Therefore, in test 37, the sputtering time t Mg Sputtering time t Si It was slower than expected. Also, in test number 38, F1 was too low. As a result, sufficient resistance to condensation discoloration was not achieved.
[0164] In test number 39, the holding diffusion time in the Mg diffusion process was too long. As a result, F1 was too high. Consequently, sufficient resistance to condensation discoloration was not obtained.
[0165] The embodiments of this disclosure have been described above. However, the embodiments described above are merely examples for implementing this disclosure. Therefore, this disclosure is not limited to the embodiments described above, and the embodiments described above can be modified as appropriate without departing from the spirit of this disclosure.
Claims
1. The invention comprises a base steel sheet, a plating layer formed on the base steel sheet, and a chemical conversion film formed on the plating layer, wherein the chemical composition of the plating layer is, in mass%, Al: more than 5.0% and less than 25.0%, Mg: more than 3.0% and less than 12.5%, and Zn: 65.0% or more, the chemical conversion film contains Si, Zr, V, P, Co, and Mg, the film thickness of the chemical conversion film is 0.03 to 2.00 μm, and a glow discharge emission spectroscopy analysis is performed from the surface of the chemical conversion film in the direction of the film thickness to obtain a depth profile showing the relationship between sputtering time and the emission intensity of elements in the chemical conversion film, and in the depth profile, the sputtering time t at which the emission intensity of Mg reaches the first peak intensity from the start of sputtering is determined. Mg The sputtering time t is when the luminescence intensity of the Si reaches its peak intensity. Si Faster than the aforementioned sputtering time t Mg The peak intensity of Mg at I Mg , and the sputtering time t Si The peak intensity of Si at I Si A surface-treated steel sheet that satisfies equation (1). 0.10 ≤ I Mg / I Si ≤ 1.00 (1) 2. The surface-treated steel sheet according to claim 1, wherein the chemical composition of the plating layer is further, in mass%, Sn: greater than 0 to 3.00%, Bi: greater than 0 to 5.00%, In: greater than 0 to 2.00%, Ca: greater than 0 to 3.00%, Y: greater than 0 to 3.00%, La: greater than 0 to 3.00%, Ce: greater than 0 to 3.00%, Si: greater than 0 to 2.50%, Cr: greater than 0 to 0.5%, Ti: greater than 0 to 0.5%, Ni: greater than 0 to 0.5%, Co: greater than 0 to 0.5%, V: greater than 0 to 0.5%, Nb: greater than 0 to 0.5%, Cu: greater than 0 to 0.5%, Mn: greater than 0 to 0.5%, Fe: greater than 0 to 5.0%, Sr: greater than 0 to 0.5% A surface-treated steel sheet containing one or more elements selected from the group consisting of Sb: greater than 0 to 0.5%, Pb: greater than 0 to 0.5%, and B: greater than 0 to 0.5%.