Hybrid system for thermal additive manufacturing

The hybrid system using a single build material for support and object, combined with extrusion and microheater printheads, addresses the limitations of FDM systems by enabling high-resolution, fast production with improved surface finish and reduced waste.

WO2026235688A1PCT designated stage Publication Date: 2026-11-12MCANANY YULIYA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2025/028061
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2025-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current FDM additive manufacturing systems are limited by their printing speed and the ability to utilize various types of build materials, often requiring support structures that restrict feature resolution and surface finish, and they must choose between printing speed and resolution.

Method used

The use of a single build material that acts as both support and object, combined with an extrusion printhead for low-resolution layer extrusion and a microheater printhead for high-resolution layer curing, allowing for high-resolution feature production with high strength and toughness, and the ability to reuse uncured build material.

Benefits of technology

This approach enables high-resolution object production without support structure limitations, reduces waste, and allows for faster printing of high-resolution features while maintaining strength and surface finish, while also enabling the reuse of uncured build material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2025028061_12112026_PF_FP_ABST
    Figure US2025028061_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Additive manufacturing systems and associated methods and build materials are described. The additive manufacturing systems herein include extrusion printheads, microheater printheads, and curable build materials. The extrusion printheads produce relatively low-resolution layers of uncured build material, and the microheater printheads cure portions of these low-resolution layers to produce high-resolution layers of cured build material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] HYBRID SYSTEM FOR THERMAL ADDITIVE MANUFACTURING

[0002] BACKGROUND

[0003] Additive manufacturing systems, also referred to as “3D printers’’, generate three-dimensional objects by the addition of material. This technology differs from “subtractive manufacturing’’, wherein material is removed to produce a desired object. The use of an additive manufacturing system often includes a digital model of the desired object. This object is often divided into many thin layers via a software tool. Each layer of the object may then be successively produced by the additive manufacturing system until a physical approximation of the digital model is completed.

[0004] Additive manufacturing systems do not rely on the use of molds or costly tooling designed to produce a specific object. Due to this, these systems are often useful for the production of prototypes or art objects, where few copies of a desired object will be produced. Some desired objects may have a geometry that is not possible to produce through subtractive manufacturing.

[0005] Fused Deposition Modeling (FDM) is an additive manufacturing technology that has become very popular. Within an FDM system, a printhead heats a solid build material to a temperature near the melting point of the matenal, and the material is extruded onto a build plate or a previously extruded layer. As the heated material is extruded, it quickly cools and becomes a solid shortly after contacting the build plate or previous layer. These systems commonly employ a thermoplastic build material. Current FDM systems are limited in their printing speed. They are also limited in their ability to utilize various types of build materials.

[0006] SUMMARY OF THE INVENTION

[0007] Briefly, and in non-limiting terms, described herein are additive manufacturing systems incorporating extrusion printheads, microheater printheads, and curable build materials. Methods of using these systems and build materials useful for the additive manufacturing system embodiments herein are also described. In many of the embodiments herein, extrusion printheads produce relatively low-resolution layers of uncured build material, and microheater printheads cure portions of these low-resolution layers to produce relatively high-resolution layers or voxels of cured build material.

[0008] Embodiments described herein offer advantages relative to current additive manufacturing systems. Some embodiments herein are able to use a single build material to act as both a support material and as the material of the desired object. The uncured build material, which acted as a support material during printing may be reused as build material in future printing. Additionally , the use of curable build material within thesystems herein allows for the production of desired objects with high-resolution features, while also having high strength, toughness, and heat deflection.

[0009] Current additive manufacturing systems often require support structures or support material for the production of an object when portions of the desired object are not adequately supported in the z axis (vertically). Support structures often limit the feature resolution of desired objects and the surface finish achievable without post-processing steps (steps performed after printing is completed). In some embodiments described herein, the uncured build material acts as a support material that can be easily removed and does not limit object resolution or surface finish. The use of a single build material for the desired object and the support material allows for an overall simpler additive manufacturing system and can decrease waste.

[0010] Cunent FDM systems must choose to prioritize printing speed or resolution, as an FDM system with a relatively small nozzle diameter will produce relatively high-resolution desired objects, at the cost of greater time needed for printing. Some embodiments described herein are able to utilize relatively low-resolution FDM-like nozzles that quickly extrude material, while still being able to produce high-resolution desired objects quickly due to a second, high-resolution microheater printhead. In other words, some embodiments described herein can be thought of as quickly extruding a low-resolution layer of uncured build material and then producing a high-resolution layer of cured build material by the action of a microheater printhead.

[0011] BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Fig. 1 shows a front view of an embodiment of an additive manufacturing system.

[0013] Fig. 2 shows a side view of an embodiment of an additive manufacturing system.

[0014] Fig. 3 shows a perspective view7of an embodiment of an additive manufacturing system.

[0015] Fig. 4 illustrates a simplified process for the additive manufacture of a tree-shaped object, which could be performed by embodiments described herein.

[0016] DETAILED DESCRIPTION OF THE INVENTION

[0017] The present disclosure provides systems and methods for additive manufacturing. The present disclosure also provides build materials that may be used with the systems and methods for additive manufacturing provided herein. Some build materials are inherently only useful within the systems and methods described herein. All references cited within this document are incorporated herein by reference in their entirety.

[0018] Embodiments, serving the purpose of examples, are described herein with sufficient detail to enable those of skill in the art to practice the invention. It should be understood that other embodiments may berealized and that various changes to the invention may be made without departing from the spirit and scope of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention. The detailed description is presented to describe the features and characteristics of the present invention, to set forth the best mode of operation of the invention, and to sufficiently enable one skilled in the art to practice the invention. The scope of the present invention is to be defined by the appended claims.

[0019] In the following description, for purposes of explanation, numerous specific details of certain embodiments are set forth. Reference in the specification to "an example", "an embodiment”, or similar language means that a particular feature, structure, or characteristic described in connection with the example is included in at least that one embodiment, but not necessarily in other embodiments.

[0020] Within this specification, the singular forms "a", "an", "the", and others include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a polymer" includes one or more of such materials, and reference to "heating" includes reference to one or more of such steps.

[0021] As used herein, a plurality of items, structural elements, compositional elements, and / or materials may be presented in a common list for convenience. However, these lists should be construed as though each member of the list is individually identified as a separate and unique member. Thus, no individual member of such lists should be constmed as a de facto equivalent of any other member of the same list solely based on their presentation in a common group without indications to the contrary.

[0022] As used herein, numerical values used in combination with “about” will be understood to describe all numerical values 20 % above the numerical value to 20 % below the value. For example, “a diameter of about 3 mm” will be understood to describe diameters of 2.7 to 3.3 mm, inclusive of all values within that range.

[0023] Concentrations, amounts, and other numerical data may be presented herein in a range format. It is to be understood that such a range format is used merely for convenience and brevity and should be interpreted flexibly to include not only the numerical values explicitly recited as the limits of the range, but also to include all the individual numerical values or sub-ranges encompassed within that range as if each numerical value and sub-range is explicitly recited. For example, a numerical range of 1 to 4.5 should be interpreted to include not only the explicitly recited limits of 1 to about 4.5, but also to include individual numerals such as 2, 3, 4, and sub-ranges such as 1 to 3, 2 to 4, etc. The same principle applies to ranges reciting only one numerical value, such as "less than 4.5," which should be interpreted to include all of the above-recited values and ranges. Additionally, such an interpretation should apply regardless of the breadth of the range or the characteristic being described.As used herein, a "desired object” may be a physical object that is produced by the action of an additive manufacturing system, and which may be based upon a digital object model. The desired object does not generally include any support material, although they are frequently physically linked at the time of printing. Support material is not intended to remain attached to the desired object. A desired object can be divided into smaller desired objects for easier production through the action of an additive manufacturing system. As used herein, a “rough object” may include a desired object along w ith any support material, uncured build material, and / or any other build material not part of the desired object but is extruded during the printing of a desired object, such as a purge tower.

[0024] As used herein, a “build material” may refer to any material utilized within an additive manufacturing system that makes up at least a portion of the material extruded during the printing of a desired object, including support material, waste material, and purge material. As used herein, a “melting point” (Tm) may also refer to a “glass transition temperature” (Tg), unless the context dictates otherwise. This is done because it would make many sentences unwieldy to constantly state “a melting point and / or a glass transition temperature”, and the concepts of melting points and glass transition temperatures are similar. For example, “a first polymer has a melting point higher than a second polymer” should be understood to describe a first polymer with a relatively higher: Tmcompared to the Tmof the second polymer; Tgcompared to the Tgof second polymer; Tmcompared to the Tgof the second polymer (wherein the second polymer has no melting point), or Tgcompared to the Tmof the second polymer (wherein the first polymer has no melting point).

[0025] A “curable build material” and variations of this term herein may refer to a material wherein at least a portion of the material undergoes a change in its chemical structure or its material properties when heated to a sufficient temperature (thermally cured) and returned to a temperature low er than the curing temperature. Curing of a curable build material may cause at least a portion of the resulting cured material to have any of the following properties, relative to uncured build material: a higher viscosity, a higher elastic modulus, a different bending modulus, a decreased solubility in a hydrophobic solvent, a decreased solubility in a hydrophilic solvent, a decreased solubility in water, a higher melting temperature, a higher glass transition temperature, a higher Y oung’s modulus, an altered hygroscopicity, a higher heat deflection temperature, a higher tensile strength, an increased impact strength, a greater number of metallic bonds, or a greater number or degree of covalent crosslinks. Curing of a curable build material may also indicate the joining together of particles which were separate in an uncured state. A curable build material does not need to be homogeneous, and may contain: multiple materials, multiple classes of materials, particles, particlesof differing composition, and / or one or more composite materials. Any material referred to simply as a “material” or a “build material” herein may also be a curable build material.

[0026] In some embodiments, curing of a build material describes a process producing cured build material with a decreased solubility in a hy drophobic solvent, relative to uncured build material. A hy drophobic solvent may be one or more of: an alcohol, an ether, a ketone, acetone, acetonitrile, benzene, butanol, butyl acetate, carbon tetrachloride, chloroform, cyclohexane, dichloroethane, dichloromethane, dimethylformamide, dimethyl sulfoxide, dioxane, ethanol, ethyl acetate, diethyl ether, heptane, hexane, methanol, methyl ethyl ketone, pentane, propanol, diisopropyl ether, tetrahydrofuran, toluene, xylenes, pyridine, piperidine, n-methylpyrrolidone, and another similar solvent. In some embodiments, curing of a build material describes a process producing cured build material with a decreased solubility in a hydrophilic solvent, relative to uncured build material. A hydrophilic solvent may be one or more of acetic acid, water, water containing a surfactant, and another similar solvent.

[0027] In some embodiments, curing of a build material describes at least sintering within the build material, and this sintering may take place within or between metallic and / or non-metallic materials. In some embodiments, curing a build material describes at least the build material partially melting or fully melting. In some embodiments, cunng a build material describes at least the build material reaching a temperature greater than the melting temperature of all build material components. In some embodiments, curing a build material describes at least the build material undergoing polymerization and / or crosslinking. In some embodiments, curing a build material describes at least the build material reaching a temperature greater than the melting temperature of all build material components that make up greater than 5 % of the total build material mass. In some embodiments, curing of a build material involves at least one of: a ringforming reaction, a Diels-Alder reaction, an electrocyclic reaction, a ring-opening metathesis polymerization (ROMP), a 1,3-dipolar cycloaddition, a transesterification reaction, an esterification reaction, and a condensation reaction. In some embodiments, curing of a build material involves at least crosslinking of one or more fatty acids or fatty acid derivatives.

[0028] In some embodiments, curing of a build material describes a change in the chemical structure of at least one portion of the build material. In some embodiments, curing of a build material describes a change in the chemical structure of at least one portion of the build material, wherein additional covalent bonds have been formed. In some embodiments, curing of a build material described a change within the material without any additional covalent bonding present within the cured material. In some embodiments, curing increases the melting point and strength of a material without any additional covalent bonding present within the cured material.As used herein, a "printhead” may refer to any component of an additive manufacturing system which interacts with or manipulates the build material for the purpose of producing a desired object and / or support material. The word or prefix ‘’micro”, as used herein, may indicate that the described element is preferred to be less than 1 millimeter in its largest dimension, but embodiments exist outside of this preferred range. Whenever “micro” is used to discuss a printhead herein, the term does not describe a preferred size range of the printhead.

[0029] As used herein, the term “particle” or variations of this term may refer to pieces of a material that possess a low aspect ratio, or in other words, have exterior dimensions that are roughly equal in all directions. However, these terms may, in some embodiments, refer to materials that have a higher aspect ratio. For example, a thermoplastic powder intended for sintering usually contains particles with a low aspect ratio, which fall under the definition of particles herein. In another example, chopped carbon fibers possess a relatively high aspect ratio, but are a useful additive to build materials in additive manufacturing and also fall under the definition of particles herein.

[0030] As used herein, the term “printing” may refer to any action performed by an additive manufacturing system that is performed in the course of producing a desired object. These actions may include: extrusion of build material, extrusion of support material, curing of build material, movement of build material, movement of motors to position printheads, producing a desired object, and other actions.

[0031] As used herein, the terms “build plate” and “print bed” are synonymous, indicating the surface within the additive manufacturing system that supports layers of build material and / or other extruded build material. As used herein, the “build volume” or “build environment” describes the total volume in which build material can be deposited in order to produce a desired object.

[0032] As used herein, a process being “selective”, including “selective extrusion”, “selective deposition”, “selective heating”, and “selective curing”, may refer to the process being applied to specific, non-random locations for the purpose of directly or indirectly producing a desired object and / or support material.

[0033] Wherein an additive manufacturing system performs layer-by-layer production of a desired object and / or support material, a selective process would generally be a process wherein only specific portions of the volume or voxels within that layer are affected by the process. For example, FDM systems incorporate selective deposition and extrusion, because an extrusion nozzle therein only deposits material in locations within the build volume that contribute directly or indirectly to the production of a desired object. In another example, a powder bed fusion (PBF) system typically non-selectively deposits layers of build material powder, because many portions of the deposited powder do not: become part of the desired object, become part of support material, or otherwise act as support material. To explain this in another manner.each deposited layer of powder within a PBF system is identical (this is a non-selective deposition process), regardless of the size and shape of the voxels of powder that must be fused within that particular layer. If a PBF system was modified so that layers of deposited build material powder were unique, based upon the size and shape of material needing to be fused within each layer, this would be a selective deposition process. Deposition is a term that is broader than extrusion, and extrusion is a specific type of deposition.

[0034] In some embodiments, the present invention provides a system for additive manufacturing that includes at least one printhead capable of extruding build material, and at least one printhead having at least a single heating element or at least a microheater array, wherein these limitations may be satisfied by a single printhead capable of extruding build material and having a single heating element or a microheater array. In embodiments of this type, a printhead that performs at least the function of extruding build material will be referred to herein as an extrusion printhead, and a printhead that is made up of at least a single heating element or at least a microheater array will be referred to herein as a microheater printhead. Again, an extrusion printhead may simultaneously be a microheater printhead.

[0035] POWER AND CONTROL

[0036] In some embodiments, the additive manufacturing system is made up of at least: a power source, a computer system that directs the functions of the system, printheads that place and cure the build material, a gantry and motor system that move the printheads, a structure that provides support for all system components, and a build material reservoir. The computer system may be internal or external to the additive manufacturing system. In some embodiments, the computer system is wirelessly attached to the additive manufacturing system through a technology such as WIFI, a Bluetooth connection, radio w aves. infrared light signals, or another similar technology. In some embodiments, a touch screen and / or physical buttons are present on the additive manufacturing system itself to direct functions of the system.

[0037] In some embodiments, the additive manufacturing system can be connected to an external controller such as a personal computer, portable computer (for example a smartphone, tablet, or other similar device), or a specifically designed controller dedicated to operation of the printing system. In some embodiments, a camera system is present local to the additive manufacturing system that allows remote monitoring of the operations of the additive manufacturing system.

[0038] In some embodiments, there is provided a non-transitoiy computer-readable storage medium comprising a set of computer readable instructions stored thereon, which, when executed by a processor for an additive manufacturing system, cause the processor to carry out a number of instructions. In some embodiments, the instructions cause the processor to receive a digital object model. The digital object model defines the shape and nature of the three-dimensional object to be printed; in other words, the digitalobject model is made up of at least data defining an extent of an object in three-dimensions. In some embodiments, a digital object model contains additional data, such as which portions of the desired object are intended to be composed of different materials, wherein the multiple materials may differ in color or elastic modulus for example.

[0039] In some embodiments, software takes a digital object model and produces a plurality of layer definitions. Each layer definition may comprise a plurality of volumetric pixels, also referred to as voxels, which make up a layer of build material useful for constructing the desired object. Each layer definition may define extrusion voxel locations where build material must be deposited by the extrusion pnnthead, and it may define microheater printhead voxel locations where build material is to be cured. Each layer definition may also comprise more complex print data, such as a curing temperature profile for each voxel. In some embodiments, dissimilar curing temperatures for individual voxels produce a difference in the elastic modulus of the resultant voxel of cured build material.

[0040] STRUCTURE AND MOVEMENT

[0041] In the embodiments illustrated by Figures 1-3, a single extrusion printhead 101 and a single microheater printhead 103 are present within an additive manufacturing system. Therein, an open cube-like structure 110 supports the additive manufacturing system. In the embodiments illustrated by Figures 1-3, both printheads are supported by a gantry 107 that allows simultaneous movement of the printheads along the z axis. Lead screws, for example 109, and stepper motors, for example 108, are shown to be involved in the movement of parts of the additive manufacturing system. Two stepper motors, and their associated lead screws, are responsible for movement of the extrusion printhead in the x axis and the y axis. A single stepper motor and its associated lead screw are responsible for movement of the microheater printhead. Two stepper motors, and their associated lead screws, are responsible for movement of the gantry that supports both printheads in the z axis. The extrusion printhead 101 takes in filamentous build material 106, heats the build material, and extrudes the build material through the extrusion nozzle 102. Extruded build material is deposited in a layer onto the print bed 105, or onto a previously extruded layer. As the microheater printhead passes over an extruded layer, a microheater array 104 selectively cures portions and / or voxels within the layer.

[0042] In the embodiments illustrated by Figures 1-3, a microheater printhead is capable of independent movement along the x axis. Therein, an extrusion printhead is capable of independent movement along the x axis and they axis, and a gantry supporting both printheads is moveable along the z-axis. The extrusion printhead is capable of being positioned along three axes in relation to the print bed, and the microheater printhead is capable of being positioned along two axes in relation to the print bed. It is to be understoodthat the axes of motion, in the illustrated embodiments, sen e as examples. It is to be understood that movement along two axes describes any type of movement within a two-dimensional plane, and movement along three axes describes any type of movement within three-dimensional space.

[0043] In some embodiments, the relative positioning of an extrusion printhead, in relation to the print bed, is achieved by movement of the print bed along three axes and movement of the extrusion printhead along zero axes. In other embodiments an extrusion printhead is moved along one axis and the print bed is moved along tw o axes. In other embodiments, an extrusion printhead is moved along two axes and the print bed is moved along a single axis. In other embodiments, an extrusion printhead is moved along three axes and the print bed is moved along zero axes.

[0044] In some embodiments, the relative positioning of a microheater printhead, in relation to the print bed, is achieved by movement of the print bed along tw o axes, and movement of the microheater printhead along zero axes. In other embodiments, a microheater printhead is moved along one axis, and the print bed is moved along one axis. In other embodiments, a microheater printhead is moved along two axes, and the print bed is moved along zero axes. In some embodiments, a microheater printhead performs multiple passes within the X-Y plane during curing of a single layer.

[0045] In some embodiments, the relative positioning of a microheater printhead, in relation to the print bed, is achieved by movement of the print bed along three axes and movement of the microheater printhead along zero axes. In other embodiments a microheater printhead is moved along one axis and the print bed is moved along tw o axes. In other embodiments, a microheater printhead is moved along two axes and the print bed is moved along a single axis. In other embodiments, a microheater printhead is moved along three axes and the print bed is moved along zero axes.

[0046] In some embodiments, the current position of at least one printhead or a print bed is determined by calculating the distance each of these components has moved from a known limit switch (also known as an endstop) location. In some embodiments, the cunent position of at least one printhead or a print bed is determined using a linear encoder, for example, a magnetic or optical linear encoder.

[0047] In some embodiments, movement of a gantiy and / or individual printheads is preferably accomplished by high-resolution stepper motors. Vanous types of motors may be used for the movement of additive manufacturing system components in embodiments herein, including stepper motors, linear motors, servomotors, synchronous motors, D.C. motors, and fluid motors. In some embodiments, multiple types of motors are utilized within a single system to produce the desired motion. In some embodiments, stepper motor-driven screws are utilized to accomplish relative movement of printheads and / or a print bed.Some examples of the use of stepper motors w ithin additive manufacturing systems are disclosed in CRUMP (U.S. Pat. No. 5.121,329). which is incorporated herein by reference, in its entirety.

[0048] In some embodiments, a layer of material is present on top of the print bed for the purpose of increasing adhesion between a build material and the print bed. In some embodiments, this layer is chemically adhesive. In some embodiments, the layer has a high roughness and may be a type of sandpaper.

[0049] In some embodiments, layers of extruded build material are of uniform thickness. In some embodiments, layers of extruded build material vary' in height, as desired for a particular desired object. Varying layer height may be useful to increase the z-axis resolution of a particular portion of a desired object.

[0050] In some embodiments, the printheads are capable of entirely independent movement without the use of a shared gantry system. Other systems of moving the printheads can also be used, such as those used in delta 3D printers, polar 3D printers, robotic arm-ty pe 3D printers, and others. In some embodiments, more than one of each type of printhead can be used to increase printing speed, increase the build volume, or allow for the extrusion and / or curing of a larger number of materials.

[0051] In some embodiments, the print bed is capable of being precisely heated. In some embodiments, the pnnt bed is capable of being heated by ceramic heating elements. In some embodiments, the print bed is capable of being heated using a closed-loop heating system. In some embodiments, an enclosure surrounds an additive manufacturing system. In some embodiments, the interior of an enclosure is capable of being heated to a desired temperature or temperature range. In some embodiments, a heating element is present within an additive manufacturing sy stem for the purpose of heating the interior of an enclosure (this could alternatively be referred to as a chamber heater).

[0052] In some embodiments, an additive manufacturing system is made up of one or more microheater printheads present within a currently known ty pe of additive manufacturing system. The one or more microheater printheads may be present in that type of system in addition to the standard printheads therein or in place of one or more standard printheads therein, but the remaining portions of the system would generally remain the same. In some embodiments, one or more microheater printheads could replace the electron beam in a powder bed fusion (PBF) system and / or an electron beam melting (EBM) system. In some embodiments, one or more microheater printheads could replace the laser in a powder bed fusion system, a direct metal laser sintering (DMLS) system, an electron beam melting (EBM) system, a selective heat sintering (SHS) system, a selective laser melting (SLM) system, or a selective laser sintering (SLS) system. In some embodiments, an additive manufacturing system herein is made up of an SLS system, wherein the powder bed portion of the system is replaced by a print bed and any of the extrusion systemsdescribed herein. In some embodiments, an additive manufacturing system herein is made up of at least one extrusion printhead and at least one laser, wherein an extrusion printhead selectively deposits build material and a laser selectively cures portions of build material.

[0053] GENERAL PRINTING PROCESS

[0054] In some embodiments, the process for the production of a desired object is as follows in this paragraph. A first layer of uncured build material is selectively extruded onto the build plate. This is done by an extrusion nozzle passing over each area that requires build material and selectively extruding build material in those areas. The microheater printhead passes over all portions of this uncured build material that require curing. The individual heating elements within the microheater array are used to selectively cure portions of the build material. In some embodiments, this curing process may be performed on portions of a particular layer while the extrusion printhead is still extruding build material within the same layer. In some embodiments, the microheater printhead moves continuously over the build material. In some embodiments, the microheater printhead: moves to a portion of the build material requiring curing, stops moving while heating of the build material occurs, and begins moving again after the required heating has concluded. The first layer may take any shape dictated by a computer system. The second layer, and each subsequent layer, may take different shapes, as required by the cross section of each layer of the digital object model, including any desired support material. For the process wherein each layer is formed only in a horizontal plane consisting of the x axis and the y axis, at least one motor is selectively actuated after each layer is produced to raise the printheads along the z axis by a height necessaiy for the extrusion and possible curing of the following layer.

[0055] In some embodiments, non-planar printing is utilized. During non-planar printing, at least a single layer is formed wherein the extruded and / or cured build material does not lie within a single plane. In some embodiments, non-planar printing is utilized wherein at least one printhead moves in 3 dimensions relative to the print bed during the extrusion and / or curing of a single layer. In some embodiments, non-planar printing is utilized wherein it is not possible to distinguish where one layer ends and another begins, as at least one printhead is always or nearly always moving in 3 dimensions relative to the print bed. An example of this type of printing is FDM helical printing (sometimes referred to as '‘vase mode”).

[0056] FIG. 4 illustrates the state of build material during printing within some additive manufacturing system embodiments described herein. The printing process begins with the selective deposition of uncured material 202 onto the print bed, or onto previously deposited layers of build material 201. The deposition is performed by an extrusion printhead. Selective curing of the uncured build material is then performed within the most recently deposited layer, if cured build material is desired in that particular layer. An entireextruded layer of build material may be cured, a portion of an extruded layer may be cured 203, or none of an extruded layer may be cured. This process is repeated until the entire desired object has been formed 204. Removal of uncured build material may be performed to produce a desired object free of uncured build material 205.

[0057] In some embodiments, an additive manufacturing system herein is capable of producing at least a portion of one or more of the following objects: a musical instrument, a specific dosage of a pharmaceutical composition, a pharmaceutical tablet, a pharmaceutical dosage with a tunable dissolution time based upon its structure, an impeller, a tool, an artificial organ, and an engine.

[0058] EXTRUSION PRINTHEAD

[0059] In some embodiments, an additive manufacturing system is made up of at least an “extrusion printhead’’ that functions to extrude build material. An extrusion printhead is made up of at least at least one extrusion nozzle. In some embodiments, an extrusion printhead includes a volume for the purpose of heating build material. In some embodiments, an extrusion printhead includes metallic fins for the purpose of cooling a portion of the extrusion printhead. In some embodiments, the extrusion printhead includes at least one cooling fan for the purpose of cooling a portion of the extrusion printhead and / or for the purpose of cooling recently extruded build material. In some embodiments, the functions of an extrusion printhead are equivalent or similar to the functions of the printhead in a Fused Deposition Modeling (FDM) additive manufacturing system. The structure, function, and control of FMD printheads are described in CRUMP (US Pat. No. 5,121,329, the entirety of which is incorporated herein by reference) and other documents and materials. In some embodiments, at least one extrusion printhead deposits build material selectively (this is preferred). In some embodiments, at least one extrusion printhead deposits build material non-selectively (this is not preferred).

[0060] In some embodiments, build material extrusion processes comprise heating a build material and extruding the build material through an extrusion nozzle. In some embodiments, build material is heated until it reaches a non-solid state before extrusion. In some embodiments, a build material is a non-solid at ambient temperature, room temperature, or 25 °C before extrusion. In some embodiments, a build material is a non-solid at ambient temperature, room temperature, or 25 °C and has a relatively high viscosity. A non-solid state may be a liquid state, a rubber}7state, a state of viscous flow, or other similar states not defined as solid. In some embodiments, a build material is heated to a temperature equal to or greater than its glass transition temperature before extrusion through an extrusion nozzle. In some embodiments, a build material is heated to a temperature equal to or greater than its melting temperature before extrusion through an extrusion nozzle. In some embodiments, a build material is heated to a temperature wherein the buildmaterial appreciably decreases in viscosity before extrusion through an extrusion nozzle. In some embodiments, extruded build material cools to a temperature below its glass transition temperature before it is cured by the action of a microheater printhead. In some embodiments, extruded build material cools to a solid state before it is cured by the action of a microheater printhead. In some embodiments, extruded build material cools to a glassy state before it is cured by the action of a microheater printhead. In some embodiments, the maximum temperature reached by the build material before extrusion is controlled by a computer system and a heating element on or near an extrusion printhead. It should be understood that build material has been "extruded” when it has passed through an extrusion nozzle.

[0061] In some embodiments, a ceramic heating element is utilized to heat a build material before extrusion through an extrusion printhead. In some embodiments, a temperature sensor such as a thermistor or a thermocouple is present near a ceramic heating element as part of a closed-loop system for heating a build material. In some embodiments, a resistive heating element is utilized to heat build material before extrusion through an extrusion printhead. In some embodiments, a temperature sensor such as a thermistor or a thermocouple is present near a resistive heating element as part of a closed-loop system for heating the build material. In some embodiments, a temperature sensor such as a thermistor or a thermocouple is present close to a volume wherein build material is heated so that the temperature sensor can determine or approximate the temperature of the heated build material.

[0062] In some embodiments, a build material is heated at a temperature of 30-3500 °C, 160-250 °C, 180-200 °C, 200-240 °C, 500-1500 °C, 650-1100 °C, 30-160 °C, or 45-85 °C before extrusion. In some embodiments, a build material is extruded at a temperature of 30-3500 °C, 160-250 °C, 180-200 °C, 200-240 °C, 500-1500 °C, 650-1100 °C, 30-160 °C, or 45-85 °C. In some embodiments, a build material comprising a polymeric material is heated at a temperature of 160-250 °C, 40-200 °C, or 200-240 °C before extrusion. In some embodiments, a build material comprising a metallic material is heated at a temperature of 40-1500 °C or 650-1100 °C before extrusion. In some embodiments, a build material comprising a wax material is heated at a temperature of 30-160 °C or 45-85 °C before extrusion.

[0063] In some embodiments, a build material is extruded through an extrusion nozzle at a temperature lower than the temperature required to instantaneously cure a build material. In some embodiments, a build material is extruded through an extrusion nozzle at a temperature lower than the temperature required to cure a build material in less than: 1 second, 5 seconds, 10 seconds, 30 seconds, 1 minute, 5 minutes, 10 minutes, 30 minutes, or 1 hour. In some embodiments, the difference between the extrusion temperature of a build material and the curing temperature of the same build material is 1-20 °C, 20-50 °C, 50-100 °C, 100-250 °C, 250-1000 °C or 100-3500 °C.In some embodiments, a build material is preferably heated within an extrusion printhead. In other embodiments, a build material is heated near an extrusion printhead, and the build material is transferred to the extrusion printhead while in a non-solid state.

[0064] In some embodiments, a build material is provided in the form of a filament. In some embodiments, a reservoir of filamentous build material is present as a spool of filament. In some embodiments, a build material is present as: powder, beads, particles, turnings, spheres, granules, or other low-aspect-ratio pieces of a material. In some embodiments, a reservoir of a low-aspect-ratio build material is present as a hopper containing the material.

[0065] In some embodiments, extruded material may be extruded in such a way that build material is present above the intended maximum height of the current layer. In some embodiments, an extrusion nozzle may advantageously function to remove material above the intended maximum height of the current layer. In some embodiments, as an extrusion nozzle moves over a specific layer it removes material above the intended maximum height of the current layer. In some embodiments, a blade, a heated blade, or another object is present for the purpose of removing material above the intended maximum height of the current layer.

[0066] In some embodiments, a build material is non-selectively deposited within the build volume and at least some build material is selectively cured. In some embodiments, a sprayer nozzle may be used for the purpose of depositing build material selectively or non-selectively into the build volume. In some embodiments, a drop-on-demand system may be used to deposit build material into the build volume selectively or non-selectively. In some embodiments, build material is extruded and non-selectively formed into a layer by the movement of a roller, squeegee, doctor blade, or similar object. In some embodiments, a technology currently known to be utilized for the deposition of build material, within a currently known material jetting or binder jetting 3D printer, is present and performs selective or non-selective deposition of build material within the build volume. In some embodiments, a layer of particles is deposited as a method of non-selective deposition, as is performed in known powder-bed fusion additive manufacturing systems.

[0067] BUILD MATERIAL MOVEMENT

[0068] In some embodiments, a filamentous form of build material is utilized, and drive rollers are present for the purposes of forcing the filament into the extrusion printhead and forcing heated build material out of the extrusion nozzle. In some embodiments, these rollers are present within the extrusion printhead. In some embodiments, these rollers are present outside the extrusion printhead. In some embodiments, each roller is driven directly by a motor. In some embodiments, the movement of a plurality of rollers is linked by gears, a belt drive, or a chain drive. In some embodiments, rotational power is supplied to the driverollers by a motor and gears, a belt drive, or a chain drive. These motors may be selected from any suitable type of motor, such as stepper motors, linear motors, servomotors, synchronous motors, D.C. motors, and fluid motors. In some embodiments, a high-resolution stepper motor is utilized for the purpose of delivering power to the drive rollers. In some embodiments, an idler roller is present on the opposite side of filament relative to a drive roller. An idler roller may assist in gripping the filamentous build material.

[0069] In some embodiments, the rollers or gears that apply force to a filamentous build material are located close to or directly connected to an extrusion nozzle. This is often referred to as a "direct drive extruder ’. In some embodiments, the rollers or gears that apply force to a filamentous build material are located far from the nozzle. This is often referred to as a Bowden extruder. In this ty pe of extrusion printhead, a tube guides a filamentous build material from the rollers or gears into the nozzle. The tube is often referred to as a Bowden tube.

[0070] In some embodiments, a hopper containing low-aspect-ratio build material, solid build material, or non-solid build material is connected to, or contains, a volume for heating the build material to a non-solid state, and pressure is generated to force the build material through the extrusion nozzle by at least: a pump, a screw, a fixed or variable displacement pump, and / or another effective means. In some embodiments, a reservoir is present containing a build material in a non-solid or liquid state at room temperature, at ambient temperature, or at 25 °C, and pressure is generated to force the build material through the extrusion nozzle by at least: a pump, a screw, a screw pump, a fixed or variable displacement pump, and / or another effective means. In some embodiments, a single-screw extrusion printhead is present. In some embodiments, a dualscrew (twin-screw) extrusion printhead is present. In some embodiments, a hot melt extrusion process is utilized. Extrusion printheads including a type of screw are preferred for build materials that incorporate a wax.

[0071] ADDITION OF COLORANT

[0072] In some embodiments, a colorant-addition volume is present wherein colorant is added to a build material before it is extruded. In some embodiments, a colorant-addition volume is present wherein colorant is added to a build material after the build material has been heated and before it exits an extrusion nozzle. In some embodiments, a colorant-addition volume is present with a geometry intended to cause mixing (e.g. turbulent flow) of a colorant with a build material as build material is forced through the colorant-addition volume. The addition of colorants within the context of some ty pes of extrusion nozzles is described in PRIDOEHL (US Pat. No. 9,283,714, which is incorporated herein by reference, in its entirety).

[0073] In some embodiments, an additive manufacturing system is made up of at least an extrusion printhead, a microheater printhead, and a colorant printhead, wherein the colorant printhead is capable ofselectively adding at least one of a dye, a pigment, and a colorant to at least a portion of build material deposited by the system during printing. In some embodiments, the colorant printhead is a continuous inkjet (CIJ) printhead, a drop-on-demand printhead, and / or a piezo drop-on-demand (DOD) printhead.

[0074] EXTRUSION NOZZLE SIZE

[0075] In some embodiments, the internal diameter of an extrusion nozzle, at the point where build material exits the extrusion nozzle, is 0.01 mm to 100 mm, 0.10 mm to 1.40 mm, 0.20 mm to 0.40 mm, 0.40 mm to 0.80 mm, 0.80 mm to 1.00 mm, or greater than 1.00 mm. In some embodiments, the internal diameter of an extrusion nozzle, at the point where build material exits the extrusion nozzle, is about 0.20 mm, about 0.30 mm, about 0.35 mm, or about 0.40 mm. In some embodiments, the internal diameter of an extrusion nozzle, at the point where build material exits the extrusion nozzle, is 0.20 mm, 0.30 mm, 0.35 mm, 0.40 mm, 0.60 mm, 0.80 mm, 1.00 mm, or 1.20 mm. In some embodiments, the internal diameter of at least one (largest or smallest) extrusion nozzle, at the point where build material exits the extrusion nozzle, is larger than at least one (largest or smallest) center-to-center distance (pitch) of at least two heating elements of a microheater array within a single additive manufacturing system. In some embodiments, the internal area of at least one (largest or smallest) extrusion nozzle, at the point where build material exits the extrusion nozzle, is larger than the area of at least one (largest or smallest) heating element of a microheater array within a single additive manufacturing system. In some embodiments, the area of the smallest heating element of a microheater array within a microheater printhead is smaller than the internal area of the largest extrusion nozzle, at the point where build material exits the extrusion nozzle, within the same additive manufacturing system. In some embodiments, an array of extrusion nozzles is present.

[0076] MICROHEATER PRINTHEAD

[0077] A microheater printhead is made up of at least a single heating element or at least a plurality of heating elements. A plurality7of heating elements is also referred to herein as a “microheater array”. In some embodiments, a heated extrusion nozzle may also serve as the microheater printhead having only a single heating element, being the heated extrusion nozzle itself. In some embodiments, the microheater printhead additionally includes a physical linkage between the heating elements and other portions of the structure of an additive manufacturing system. In some embodiments, an additive manufacturing system is made up of at least an extrusion printhead and a microheater printhead. In some embodiments, a microheater printhead includes a physical linkage between the heating elements and a gantry, wherein the gantry supports both the microheater printhead and an extrusion printhead. In some embodiments, a microheater printhead additionally includes a mechanism to position the heating elements parallel to the plane of the print bed. In some embodiments, a microheater printhead includes a mechanism to position themicroheater array along the z axis relative to an extrusion printhead. In some embodiments, the microheater printhead and the extrusion printhead are physically linked, and they are not capable of independent movement within the system in at least the x and y axes. In some embodiments, a microheater printhead and an extrusion printhead are positioned such that the extrusion nozzle is surrounded by a 2-dimensional microheater array. In some embodiments, at least one cooling fan and / or at least one thermally conductive component is / are present within an additive manufacturing system are present to cool build material.

[0078] Linear heating element arrays comprising 600 heating elements per inch are often used in thermal printers, and thermal printers are often referred to as receipt or label printers. Linear heating element arrays are often produced with linear array lengths of 303 mm (KYOCERA Corporation, “Thermal Printheads”, January 2018, incorporated herein by reference, in its entirety). Toshiba also offers thermal printheads having linear heating element arrays (TOSHIBA “Thermal Printheads Product Page”, viewed May 2024, incorporated herein by reference, in its entirety ). The disclosure of US patent number 9,421,715, patented August 23, 2016, to Hartmann et al. is incorporated herein by reference in its entirety. These commercially available printheads often cause a heated material to reach at least 250 °C (R. Uyhan, J. A. King-Hele “Modelling of thermal printers” Applied Mathematical Modelling, 2008, 32:405-416, incorporated herein by reference, in its entirety).

[0079] In some embodiments, at least one microheater printhead is preset w ithin an additive manufacturing system. In some embodiments, a microheater printhead is made up of at least resistive heating elements. In some embodiments, each heating element of a microheater printhead is individually addressable. In some embodiments, a microheater printhead possesses all-points addressability7. In some embodiments, a single microheater printhead and a single extrusion printhead are present within an additive manufacturing system. In some embodiments, a single extrusion printhead and multiple microheater printheads are present in an additive manufacturing sy stem. In other embodiments, a single microheater printhead and multiple extrusion printheads are present in an additive manufacturing system. In some embodiments, multiple microheater printheads and multiple extrusion printheads are present in an additive manufacturing system. In some embodiments, multiple extrusion printheads are present within an additive manufacturing sy stem for the purpose of having each extrusion printhead primarily responsible for the extrusion of a single build material, dissimilar from the build materials that the other extrusion printheads are responsible for. In some embodiments, at least one microheater printhead is present within an additive manufacturing system, along with at least one UV light source. In some embodiments, at least one microheater printhead is present within an additive manufacturing sy stem, along w ith at least one UV light source and one extrusion printhead.In some embodiments, resistive heating elements of a microheater printhead are wire heating elements. In some embodiments, resistive heating elements of a microheater printhead are metal or metal alloy heating elements. In some embodiments, resistive heating elements of a microheater printhead are ceramic heating elements. In some embodiments, resistive heating elements of a microheater printhead are semiconductor heating elements. In some embodiments, resistive heating elements of a microheater printhead are thick film heating elements. In some embodiments, resistive heating elements of a microheater printhead are polymeric heating elements. In some embodiments, resistive heating elements of a microheater printhead are composite heating elements. In some embodiments, resistive heating elements of a microheater printhead comprise at least one of titanium, platinum, molybdenum, tungsten, polysilicon, and molybdenum disilicide.

[0080] In some embodiments, molybdenum disilicide heating elements are present in a microheater printhead and operate at a maximum temperature of 100-2100 °C. In some embodiments, platinum heating elements are present in a microheater printhead and operate at a maximum temperature of up to 2000 °C. In some embodiments, tungsten heating elements are present in a microheater printhead and operate at a maximum temperature of up to 3500 °C.

[0081] In some embodiments, resistive heating elements within a microheater printhead are arranged in a 1 -dimensional array (in other words, in a line or in a linear array). In some embodiments, multiple resistive heating elements within a microheater printhead are arranged in a 2-dimensional array (in other words, arranged within a plane). In some embodiments, resistive heating elements within a microheater printhead are arranged in a non-standard arrangement that is not a 1-dimensional array or a 2-dimensional array. For example, a specific non-standard array arrangement appears linear when viewed from the top and bottom but appears curved when viewed from the side.

[0082] In some embodiments, the feature size of cured build material within a desired object and / or support material, produced by the action of a microheater printhead, is smaller than or equal to the center-to-center distance (pitch) of heating elements of the microheater printhead. In some embodiments, the feature size of cured build material, produced by the action of a microheater printhead, is not equal in both axes of a layer of build material. In some embodiments, the feature size of cured build matenal is dictated along a first axis by the pitch of heating elements w ithin a microheater printhead, and is dictated along a second axis by the speed at which the microheater printhead moves over the build material.

[0083] In some embodiments, a 1 -dimensional array of heating elements, within a microheater printhead, is made up of at least: 20-35,000; 100-15,000; 350-7,500; 1,000-2,000; 2,000-3,000; 3,000-4,000; or about 1,920 heating elements. In some embodiments, a 2-dimensional array of heating elements, within amicroheater printhead, is made up of at least: 10,000-33,200,000; 100,000-200,000: 200,000-500,000: 500,000-1,100,000: 1,100,000-2,100,000: 2,100,000-8,300,000; 8,300,000-33,200,000; or 33, 200,000-133,000,000 heating elements.

[0084] In some embodiments, the smallest individual heating element of a microheater printhead has an area equivalent to a circle with a diameter of 0.001-2 mm, 0.001-0.005 mm, 0.005-0.010 mm, 0.010-0.050 mm, 0.050-0.100 mm, 0.100-0.200 mm, 0.200-0.300 mm, 0.300-0.400 mm, or greater than 0.400 mm. In some embodiments, a linear array of heating elements within a microheater printhead has a resolution of about 100 dots per inch (DPI), 200 DPI, 300 DPI, 600 DPI, 1200 DPI, 2400 DPI, or 4800 DPI.

[0085] In some embodiments, heating elements of a microheater printhead are fabricated using at least microelectromechanical systems (MEMS) fabrication techniques. In some embodiments, heating elements of a microheater printhead are fabricated using at least lithographic fabrication techniques. In some embodiments, heating elements of a microheater printhead are fabricated using at least semiconductor lithography fabrication techniques. In some embodiments, heating elements of a microheater printhead are built on a substrate. This substrate may be glass, silicon, sapphire, langasite, or alumina. Glass may be beneficial due to its low thermal conductivity. Silicon may also be used despite its high thermal conductivity due to its ease of processing with MEMS fabrication. Silicon underneath a microheater array can be etched away to leave the microheater on a thin membrane of dielectric material to increase power efficiency. The process of fabricating a microheater array using MEMS techniques may be to grow a dielectric layer, then use photolithography to pattern the substrate, and then deposit the microheater material and conductive leads using sputtering or e-beam evaporation.

[0086] In some embodiments, a microheater printhead is capable of positioning heating element surfaces a distance from build material that is intended to be cured. This distance will be referred to as the microheater printhead “vertical offset’'. In some embodiments, the vertical offset is 0 mm, and the heating element surfaces will contact the build material to be cured. In some embodiments, the vertical offset is 1-10 pm, 10-50 pm, 50-100 pm, 100-300 pm, or greater than 300 pm. In some embodiments, a microheater printhead includes a mechanism to adjust the vertical offset. In some embodiments, a microheater printhead includes a mechanism to adjust the vertical offset manually. In some embodiments, a microheater pnnthead includes a mechanism to adjust the vertical offset using a computer-controlled motor.

[0087] In some embodiments, a protective sheet is present between a heating element array of an additive manufacturing system and the build material. In some embodiments, a protective sheet is in direct contact with both the heating element array and the build material. In some embodiments there is a space between at least one of: the protective sheet and the build material, and the protective sheet and the heating elementarray. It is preferable for a protective sheet herein to have a high thermal conductivity. In some embodiments, a protective sheet is stationary relative to the heating element array during the majority of the time spent printing a desired object. In some embodiments, a protective sheet is stationary relative to the build plate during the majority' of the time spent printing a desired object. In some embodiments, a protective sheet is moved relative to the heating element array to provide a clean and / or non-degraded portion of the protective sheet in contact with the heating element array.

[0088] The temperature of each heating element, within a microheater printhead, must be controlled with adequate accuracy and precision. In some embodiments, one or more temperature sensing components are present within a microheater printhead to monitor the temperature of heating elements. In some embodiments, one temperature sensing component is present for the purpose of monitoring each individual heating element of a microheater printhead. In some embodiments, temperature sensing components within a microheater printhead are thermistors. In other embodiments, temperature sensing components within a microheater printhead are thermocouples. In some embodiments, heating elements of a microheater printhead are controlled in an open-loop manner. In some embodiments, heating elements of a microheater printhead are controlled in a closed-loop manner. In some embodiments, heating elements of a microheater pnnthead are controlled using a PID control system. In some embodiments, heating elements of a microheater printhead are controlled in a closed-loop manner, wherein the temperature of a heating element is determined using the temperature-resistance relationship of the heating element itself.

[0089] In some embodiments, the following curing steps are performed: a microheater printhead is positioned over extruded build material, individual heating elements positioned proximal to voxels of build material that need to be cured are heated, and the individual heating elements continue to be heated for a desired length of time. In some embodiments, the following curing steps are performed: a microheater printhead is positioned over extruded build material, individual heating elements positioned proximal to voxels of build material that need to be cured are heated, and heating elements may be allowed to cool. In some embodiments, the following curing steps are performed: the microheater printhead is constantly moving along at least one axis over extruded build material, individual heating elements proximal to voxels of build material that need to be cured are heated, the individual heating elements continue to be heated for a desired length of time. In some embodiments, the following curing steps are performed: the microheater printhead is constantly moving along at least one axis over extruded build material, heating elements proximal to voxels of build material that need to be cured are heated, and heating elements may be allowed to cool.In some embodiments, heating elements within a microheater printhead reach a temperature of 40-3500 °C, 160-500 °C, 160-250 °C, 250-500 °C, 350-450 °C, 500-1850 °C, 650-1100 °C, 850-1400 °C, 900-1100 °C, or 1100-1400 °C to cause the curing of build material. In some embodiments, heating elements within a microheater printhead reach a temperature of 40-3500 °C, 160-500 °C, 160-250 °C, 250-500 °C, 350-450 °C, 500-1850 °C, 650-1100 °C, 850-1400 °C, 900-1100 °C, or 1100-1400 °C to cause the curing of build material comprising a polymeric build material. In some embodiments, heating elements within a microheater printhead cause portions of a build material to reach a temperature of 40-3500 °C, 160-500 °C, 160-250 °C, 250-500 °C, 350-450 °C, 500-1850 °C, 650-1100 °C, 850-1400 °C, 900-1100 °C, and / or 1100-1400 °C to cause the curing of build material. In some embodiments, an individual heating element of the microheater printhead is capable of reaching the desired temperature needed for build material curing within 0-2000 ms, 0-1 ms, 1-5 ms, 5-10 ms, 10-20 ms, 20-50 ms, or 50-300 ms, or greater than 300 ms.

[0090] In some non-preferred embodiments, a laser or laser array is present in an additive manufacturing system utilizing selective extrusion through an extrusion nozzle, without a microheater printhead.

[0091] BUILD MATERIALS

[0092] Additive manufacturing system embodiments described herein may use multiple materials for the purpose of producing one or more desired objects. In some embodiments, build materials useful herein are able to be cured at a temperature equal to or greater than the temperature at which they are extruded by an extrusion printhead. In some embodiments, a single ty pe of build material is utilized. In other embodiments, multiple types of build materials are utilized. In some embodiments, at least one build material is used for the production of support material and at least one build material is used for production of the desired object. In some embodiments, both curable and non-curable build materials are utilized for the production of a desired object and / or a rough desired object.

[0093] In some embodiments, a curable build material is capable of acting as support material in its uncured state. In some embodiments, multiple build materials are used. In some embodiments, multiple build materials are used, wherein at least one build material is primarily useful to provide cured or uncured support material to the desired object. In some embodiments, support structures attached to a desired object after printing are partially or wholly made up of uncured build material. In some embodiments, uncured build material is only present between a cured portion of a support structure and a cured portion of a desired object. CRUMP 96 (US patent number 5,503,785, patented April 2, 1996, to Crump et al.) is incorporated herein by reference in its entirety, and CRUMP 96 describes useful ways in which to construct support material.In some embodiments, the composition of a build material being deposited is gradually changed (i.e. transitions) from a first composition to another. For example, a desired object in the shape of a golfball may be produced by depositing: a build material of composition A at the exterior of the ball, a build material of composition B at the center of the ball, and mixtures of compositions A and B in the intermediaiy volume, wherein the mixture gradually contains a higher percentage of composition B closer to the center of the ball. In some embodiments, a gradual change in the composition of deposited build material involves the use of a volume wherein two or more build material compositions are mixed before exiting the extrusion nozzle (a mixing chamber). In some embodiments, the composition of build material being deposited is abruptly changed. For example, an alternative desired object in the shape of a golfball may be produced by depositing: a build material of composition A to make up the exterior 2 mm shell of the ball, and a build material of composition B to make up the interior of the ball. Multiple build materials, being used for the direct or indirect production of a single desired object, may differ in at least one of: composition, elastic modulus, bending modulus, melting point, glass transition temperature, solubility in a particular solvent, % elongation at fracture, color, heat deflection temperature, hydrophobicity, contact angle, specific heat capacity, density, toughness, strength, thermal conductivity, and another chemical or physical property.

[0094] In some embodiments, two or more build materials containing metallic particles are deposited so that the deposition gradually or abruptly transitions between build materials. In one example, two or more metallic build materials may be utilized within a single desired object to provide a transition from an inexpensive to a costly alloy, wherein the costly alloy is not needed throughout the desired object. In another example, two or more metallic build materials may be utilized within a single desired object to provide a transition from lesser to greater corrosion resistance.

[0095] In some embodiments, a metallic build material may be deposited along with non-metallic build material for the production of a single desired object. For example, the body of a quadcopter may be produced by depositing a polymeric build material to produce the bulk of the body, wherein metallic build material is also deposited, so that upon curing, continuous metallic wires are present within the quadcopter body. In some embodiments, cured metallic build material serves as structural reinforcement and / or serves to increase the elastic modulus, toughness, or strength of a desired object. In some embodiments of additive manufacturing systems herein, printing may be paused to allow for the insertion of objects, circuits, integrated circuits, optoelectronic devices, microelectromechanical (MEM) devices, or motors into the desired object.In some embodiments, a curable build material is still capable of additional curing after printing is completed, or is in other words, partially cured when printing is completed. In some embodiments, a curable build material is further cured after printing is completed. In some embodiments, a curable build material is further cured after printing is completed, involving the use of an oven. In some embodiments, a curable build material is further cured after printing is completed, involving the use of at least one of heat lamps, UV light sources, an autoclave process, a microwave process, humidity, steam, water, and elevated pressure. In some embodiments, a curable build material includes chemical moieties or structures that allow for two (dual-curing) or more (multi-curing) methods for curing a single curable build matenal. In some embodiments, a dual- or multi-curing build material is capable of being cured using UV curing and thermal curing. In some embodiments, a dual- or multi-curing build material is capable of being cured using one or more of UV curing, dissimilar curing at multiple wavelengths of electromagnetic radiation, thermal curing, dissimilar curing at multiple temperature ranges, autoclave-based curing, microwave-based curing, waterbased curing, and elevated pressure curing. In some embodiments, a dual- or multi-curing build material is utilized to tune portions of a desired object to have a specific degree of a particular property. For example, a UV -thermal dual-curing build material may use the UV curing capability to bind the desired object together, while the thermal curing capability is used to tune the bending modulus of specific regions of a desired object.

[0096] In some embodiments, an additive manufacturing system herein is capable of producing desired objects and / or support material containing continuous fibers. In some embodiments, an additive manufacturing system herein is capable of producing desired objects and / or support material containing fibers having a length greater than the internal diameter of the extrusion nozzle. In some embodiments, an additive manufacturing system herein is capable of producing desired objects and / or support material containing continuous fibers at least partially made up of carbon fiber, aramid, Kevlar®, or fiberglass.

[0097] In some embodiments, a build material for an additive manufacturing system herein contains additives that are known to one of skill in the art. In some embodiments, a build material may contain any number of the following additives: dyes, pigments, colorants, antioxidants, heat stabilizers, light stabilizers, plasticizers, defoaming agents, lubncants, dispersants, flow modifiers, drip retardants, anti-blocking agents, anti-microbials, antistatic agents, flow-promoting agents, processing aids, substrate adhesion agents, mold release agents, toughening agents, low-profile additives, stress-relief additives, hardeners, softeners, reinforcing materials, carbon fiber, aramid, Kevlar®, fiberglass, and similar additives.

[0098] In some embodiments, the curing temperature of a curable build material is equal to or greater than the extrusion temperature of the same material. In some embodiments, the curing temperature of a curablebuild material is greater than the extrusion temperature of the same material by at least: 1-25 °C, 25-60 °C, 60-90 °C, 90-120 °C, 120-150 °C, 150-200 °C, 200-500 °C, 500-1200 °C, 1200-2000 °C, or 2000 °C. In some embodiments, a curable build material is at least partially made up of an interpenetrating network before, during, and / or after curing.

[0099] In some embodiments, a build material is a solid at room temperature or at the ambient temperature outside of the additive manufacturing system. In other embodiments, a build material exists in a non-solid state at room temperature or at the ambient temperature outside of the additive manufacturing system.

[0100] A '‘monomer’' or “oligomer”, as used herein, may be at least partially made up of any monomer or oligomer present within, or needed to produce, a polymer mentioned in this document, or may be at least one of the following: ethylene, propylene, an alkene, an alkyne, styrene, acrylonitrile, an acrylate, a methaciylate, a vinyl chloride, a primaiy or secondary thiol, an acrylate, an aciylate monomer, an acrylate oligomer, isobomyl aciy late (IBOA), phenoxyethyl acrylate (PEA), tripropyleneglycol monomethyl ethyl acrylate (TPGMEMA), hexanediol diacrylate (HDD A), tripropyleneglycol diacrylate (TPGDA), a polyethyleneglycol di aery I ale. polyethyleneglycol 200 diacrylate (PEG200DA), glycerine (3PO) triacrylate (GPTA), trimethylolpropane triaciylate (TMPTA), urethane dimethacrylate (UDMA), benzyl acrylate (BZA), 4-Aciyloylmorpholine, pinene, terpinene, nerolidol, linalool, myrcene, limonene, carvone, an aldehyde, an epoxide, an oxetane, a vinyl ether, a glycidyl ether, a lactam, a lactone, allyl glycyl ether, 1,2, 7, 8-diepoxy octane, l,2-epoxy-5-hexene, styrene oxide, oxetane-3-carboxylic acid, 3-amino-3-methyloxetane, 3-methyl-3-oxetanecarboxaldehyde, a compound capable of undergoing thermal or photo radical polymerization, a compound capable of undergoing thermal or photo ionic (cationic or anionic) polymerization, and a monomer or oligomer similar to one within this list.

[0101] A “polymer” or “polymeric material” or “oligomer’, as used herein, may be at least partially' made up of at least one of: a polymeric material; an organic polymeric material; a thermoplastic; a thermosetting polymer; a biopolymer; poly dimethylsiloxane; low-density polyethylene: high-density polyethylene; polypropylene; polystyrene; polytetrafluoroethylene; polyvinyl chloride; polychlorotrifluoroethylene; polylactic acid; an acrylic polymer; polymethyl methacrylate; polyether ether ketone (PEEK); a polyamide polymer; nylon 6; nylon 6-6; polybenzimidazole; a polycarbonate polymer; a poly ether sulfone polymer; a polyoxymethylene (POM) polymer; a poly ether ether ketone polymer; polyphenylene oxide; polyphenylene sulfide; poly vinylidene fluoride; a polyamide; a poly caprolactone (PCL); a polylactic acid (PLA); polybutylene terephthalate (PBT); a poly(styrene-isoprene-styrene) (SIS); a poly(styrene-ethylene-butylene-styrene) (SEBS); a poly(styrene-butylene-styrene) (SBS); a high-impact polystyrene (HIPS); polystyrene; a thermoplastic polyurethane; apoly(acrylonitrile-butadiene-styrene) (ABS); an acrylate; apolymethylmethacrylate; a poly(vinylpynolidine-vinylacetate); a polyester (e.g., polyethylene terephthalate (PET); polyethylene naphthalate (PEN); polyethylene terephthalate glycol (PETG); and the like); a polycarbonate; a polyethersulfone; a polyether ether ketone; polyether aryl ketone; a polyetherimide; a polyethylene; a poly ethylene oxide; a polyphenylene sulfide; a polypropylene; a polystyrene; a polyvinyl chloride; polyphenylene ethers (PPE); a poly(tetrafluoroethylene); a poly(vinylidene fluoride); a poly(vinylidene fluoride-hexafluoropropylene); a polysaccharide; a polymer of one or more fatty' acids; a polymer or polymer composition known in research; a heat-polymerized acrylate or heat-polymerized acrylate composition; a polymer or polymer composition known to be used for dental applications; a commercial polymer or polymer composition; an engineering plastic or engineering plastic composition; a one part epoxy composition; a heat cure epoxy composition; any combination or composition including at least one monomer, oligomer, or polymer known to be used within a digital light processing (DLP) or stereolithography (SLA) additive manufacturing system; a composition or particles known to be useful for powder coating; a copolymer of any two or more species of monomers in this document; a commercial polymer or polymer composition intended to be cured using UV light; a polymeric material similar to any within this list; and one or more polymers having at least one of an electrophile moiety, a pendant electrophile moiety, a carboxylic acid moiety, an ester moiety, a nucleophile moiety, a pendant nucleophile moiety, an alcohol moiety, a primary amine moiety, an isocyanate moiety, an olefin moiety, a thioester moiety, a silicone moiety, a urethane moiety, a phenol moiety, a cyanate moiety, and an epoxy moiety.

[0102] A '‘curable build material'’, a “binder”, a “binder material”, or a “binding material” referred to herein may be at least partially made up of at least one of: a monomer, an oligomer, a polymer, an inorganic material, a metallic material, a cement, a concrete, a cermet, a natural wax, a synthetic wax, paraffin wax, beeswax, soy wax, palm wax, a gel wax, a fatty acid, a fatty acid derivative, carnauba wax, shellac, a wax material similar to any in this list, a clay, and a ceramic. As used herein, the term “filaments” can also refer to a single filament.

[0103] As used herein, a '‘curable moiety” may be defined as one or more of the following: electrophile moiety, a pendant electrophile moiety, a carboxylic acid moiety, an ester moiety, a nucleophile moiety, a pendant nucleophile moiety, an alcohol moiety, a primary amine moiety, an isocyanate moiety, an olefin moiety, a thioester moiety, a silicone moiety, a urethane moiety', a phenol moiety, a cyanate moiety, and an epoxy moiety. Herein, any monomer, oligomer, or polymer may contain one or more of these curable moieties, except where indicated otherwise.

[0104] As used herein, “metallic'’ is an adjective that may describe a material being at least partially made up of a metal or metal alloy. In the embodiments herein, a metallic particle or a metallic material may bemade up of at least one material of the following list: a metallic material, particles of a metallic material, a metal alloy, aluminum, an aluminum bronze, a brass, admiralty brass, chromium, copper, gold, Inconel, iron, a cast iron, lead, molybdenum, nickel, platinum, silver, a sterling silver, a steel, a carbon steel, a stainless steel, titanium, tungsten, zinc, tin, a babbitt, vanadium, beiy Ilium, a beryllium copper, bismuth, cadmium, cobalt, magnesium, manganese, a manganese bronze, mercury, palladium, rhodium, silicon, niobium, tantalum, carbon, sulfur, phosphorus, zirconium, rhenium, yttrium, hafnium, boron, a metal carbide, carbon fiber, graphite, a eutectic metal alloy, a low melting-point alloy, an alloy or composition known to be useful as a solder, an alloy or composite of any of these matenals, and any similar alloy.

[0105] As used herein, a “thermal initiator’ may be one or more of the following: a peroxide; a peroxy ester; diisopropyl peroxy dicarbonate; 2,2'-azobis[2-(2-imidazolin-2-yl)-propane] dihydrochloride; tert-Butyl hydroperoxide (TBHP); cumene hydroperoxide; di-tert-butyl peroxide; dicumyl peroxide; benzoyl peroxide (BPO); ammonium persulfate (APS); dicyandiamide; cyclohexyl tosylate; (4-hydroxyphenyl)-dimethylsulfonium hexafluorophosphate; diphenyl(methyl)sulfonium tetrafluoroborate; benzyl(4-hydroxyphenyl)-methylsulfonium hexafluoroantimonate; (4-hydroxyphenyl)methyl-(2-methylbenzyl)sul fonium hexafluoroantimonate; triphenylsulphonium nonaflate; tert-amyl peroxybenzoate; 4,4-Azobis(4-cyanovaleric acid); l,r-Azobis(cyclohexanecarbonitrile); 2,2’-azobisisobutyronitrile (AIBN); 2,2-bis(tert-butylperoxy)butane; l.l-bis(tert-butylperoxy)cyclohexane: 2.5-bis( / e / 7-biitylperoxy)-2.5-dimethylhexane; 2,5-bis(tert-butylperoxy)-2,5-dimethyl-3-hexyne; bis( I -( / -buty Iperoxy)- 1 -methylethyl)benzene; l,l-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; tert-Butyl peracetate; tert-But l peroxide; tert-butyl peroxybenzoate; tert-butylperoxy isopropyl carbonate; cyclohexanone peroxide; lauroyl peroxide; peracetic acid; potassium persulfate; a thermal radical initiator; a thermal cationic or anionic initiator; a photoinitiator; a photo cationic initiator; a photo anionic initiator; a metal catalyst; a platinum catalyst; a palladium catalyst; a rhodium catalyst; a compound capable of inducing polymerization upon heating; and / or another known or suitable thermal initiator.

[0106] In some embodiments, a curable build material is made up of at least particles and / or filaments of a first curable build material within a second curable build material. In some embodiments, a curable build material is made up of at least particles and / or filaments of a first curable build material within a second curable build material, wherein the first curable build material has a higher melting point than the second curable build material. In some embodiments, a curable build material is made up of at least particles and / or filaments of an oligomer and / or a polymer within a binder material. In some embodiments, a curable build material is made up of at least particles and / or filaments of an oligomer and / or a polymer within a binder material, wherein the particles and / or filaments have a higher melting point than the binder material. Insome embodiments, a curable build material is made up of at least particles and / or filaments of a first oligomer and / or polymer within a second oligomer and / or polymer. In some embodiments, a curable build material is made up of at least particles and / or filaments of a first oligomer and / or polymer within a second oligomer and / or polymer, wherein the first oligomer and / or polymer has a higher melting point than the second oligomer and / or polymer.

[0107] In some embodiments, a curable build material is made up of at least particles and / or filaments of an oligomer and / or a polymer within a wax, wherein the wax may have a higher melting temperature than the particles and / or filaments. In some embodiments, a curable build matenal is made up of at least particles and / or filaments of a first wax within a second wax, wherein first the wax has a higher melting temperature than the second wax. In some embodiments, at least a portion of a curable build material is curable, and at least a portion of the same curable build material is non-curable. In some embodiments, particles and / or filaments of a build material within a binder material are curable, whereas the binder material is not curable. In some embodiments, a build material is made up of at least multiple compositions of a first curable build material, being present as particles and / or filaments, within a second curable build material.

[0108] In some embodiments, the melting point of at least a portion of the particles and / or filaments, curable build material, or oligomer or polymer is 0-15 °C, 15-30 °C, 30-60 °C, 60-100°C, 150-300 °C, 300-450 °C or greater than 450 °C. In some embodiments, the melting point of a portion of a curable build material at least 0-15 °C, 15-30 °C, 30-60 °C, 60-100°C, 150-300 °C, 300-450 °C or greater than 450 °C different than the melting point of another portion of the same curable build material. In some embodiments, the melting point of at least a portion of the particles and / or filaments, first curable build material, first oligomer and / or polymer, or first wax is at least 0-15 °C, 15-30 °C, 30-60 °C, 60-100°C, 150-300 °C, 300-450 °C or greater than 450 °C different than the melting point of the second curable build material, binder material, second oligomer and / or polymer, or second w ax. In some embodiments, the melting point of at least a portion of the particles and / or filaments, first curable build material, first oligomer and / or polymer, or first wax is at least 0-15 °C, 15-30 °C, 30-60 °C, 60-100°C, 150-300 °C, 300-450 °C or greater than 450 °C higher than the melting point of the second curable build material, binder material, second oligomer and / or polymer, or second wax. In some embodiments, one of skill in the art can assess the compatibility of multiple components of a curable build material by referring to known differential scanning calorimetry (DSC) plots of each component.

[0109] In some embodiments, a curable build material is made up of particles and / or filaments of a high-melting-point oligomer or polymer within a low -melting-point polymer. In some embodiments, a curable build material is made up of at least one of ABS, PC, nylon, nylon 6 (PA6), nylon 6-6 (PA66), nylon 12(PAI 2), polyamide, Poly Ether Ether Ketone PEEK, and POM particles and / or filaments within a polylactic acid (PLA) or poly caprolactone (PCL) binder material. In some embodiments, a filamentous curable build material may be made up of at least nylon 12 particles within a binder made up of at least polylactic acid. Before, during, and after extrusion through an additive manufacturing system described herein, the nylon 12 particles within this curable build material substantially remain as unconnected particles. After thermal curing, by the action of the microheater printhead within this same additive manufacturing system, the nylon 12 material has become connected due to heating. This causes the cured build material to have a greater melting point and / or greater strength than the uncured build material, even though no additional crosslinking is present.

[0110] In some embodiments, a curable build material is made up of at least metallic particles w ithin a binding material, wherein the metallic particles may have a higher melting point than the binding material. In some embodiments, a curable build material is made up of at least metallic particles within an oligomer and / or a polymer, wherein the metallic particles may have a higher melting point than the oligomer and / or polymer. In some embodiments, a curable build material is made up of at least metallic particles w ithin a clay and / or a ceramic composition, wherein the clay and / or ceramic composition may be anon-solid at ambient temperature, room temperature, or 25 °C. In some embodiments, a curable build material is made up of at least metallic particles within a w ax, wherein the metallic particles may have a higher melting point than the wax. In some embodiments, a curable build material is made up of at least metallic particles w ithin a metallic composition, wherein the metallic particles have a higher melting point than the surrounding metallic composition. In some embodiments, a curable build material is a composite of a binder material and metallic particles, formed into a filament. In some embodiments, a curable metallic particle and binder composite material is a filament and is made up of at least a metallic core surrounded by a sheath of binding material. In some embodiments, a curable metallic particle and binder composite material is a filament, wherein metallic particles are surrounded by binding material. In some embodiments, a curable build material includes multiple compositions of metallic particles.

[0111] In some embodiments utilizing a metallic particle and binder composite curable build material, the mass of the metallic particles makes up 1-99 %, 1-60 %, 60-99 %, 70-95 %, 10-40 %, or 20-35 % of the total mass of the composite material. Multiple examples of metallic particle and binder composite materials are currently offered for sale, and one is described in the product description of Filamet™ (The Virtual Foundry “How To 3d Print Metal'’ Accessed November 17, 2022, incorporated by reference herein, in its entirety).In some embodiments, a curable build material is a plastisol, being made up of at least a plasticizer and particles and / or filaments of a polymer and / or an oligomer. In some embodiments, a curable build material is made up of at least a plasticizer and a polymer. In some embodiments, a curable build material is made up of at least plasticizer and polyvinyl chloride. In some embodiments, a curable build material made up of at least a plastisol is a non-solid or liquid state at room temperature, ambient temperature, or at 25 °C. In some embodiments, a curable build material may be produced by starting w ith a first build material known to be useful for selective laser sintering (SLS) additive manufacturing, adding a second material with a lower Tmthan that of the first build material, heating the combination of the first and second materials close to or above the Tmof the second material, and extruding this combination of materials to form a single composite material, which may be in the form of a filament.

[0112] In some embodiments, a build material is made up of at least a solution containing a relatively high concentration of a solute, wherein the additive manufacturing system causes the drying or dehydration of the solution. The solute may be one or more of a saccharide, an oligosaccharide, a polysaccharide, a peptide, a polypeptide, a protein, a salt, an inorganic material, an inorganic salt, a silicate, an aluminate, a hydrate, a carbonate, a sugar, a sand, a clay and / or ceramic material, a clay and / or ceramic composite, an active pharmaceutical ingredient, and a pharmaceutical excipient. For example, a saturated solution of a polysaccharide in water may be deposited and dehydrated using the microheater printhead to yield a structure being more viscous than the saturated solution or being a solid.

[0113] In some embodiments, a curable build material is capable of forming additional chemical bonds when sufficiently heated. In some embodiments, a curable build material is capable of forming additional chemical bonds when sufficiently heated and contains at least one thermal initiator. In some embodiments, a curable build material is made up of at least any number of monomers, oligomers, and polymers, w herein the any number of monomers, oligomers, and polymers are capable of forming additional chemical bonds when sufficiently heated. In some embodiments a curable build material is made up of at least any number of monomers, oligomers, and polymers, and a thermal initiator. In some embodiments a curable build material is made up of at least a monomer and a thermal initiator. A curable build material made up of any number of monomers, oligomers, polymers, and thermal initiators may be homogenous or heterogeneous. In some embodiments, a curable build material is made up of at least a monomer and an oligomer and / or a polymer. In some embodiments, a curable build material is made up of at least a monomer and an oligomer and / or polymer, additionally containing athermal initiator. In some embodiments, athermal initiator may be a thermal radical initiator, a thermal cation initiator, or a catalyst. Chemical bonds produced during thecuring of some curable build materials may be one or more of ionic bonds, covalent bonds, and metallic bonds.

[0114] In some embodiments, a curable build material is primarily made up of a single oligomeric or poly meric material, optionally containing a thermal initiator, and is able to undergo crosslinking or additional crosslinking with heating. In some embodiments, a curable build material is made up of at least a first polymer or oligomer and a second polymer or oligomer, optionally containing a thermal initiator, wherein the first and second polymers and / or oligomers are able to crosslink or covalently bond to each other when heated. In some embodiments, a curable build material is made up of at least a first polymer or oligomer, a second polymer or oligomer, and a thermal initiator. In some embodiments, a curable build material is made up of at least a first polymer or oligomer and a second polymer or oligomer, wherein at least one polymer and / or oligomer contains a curable moiety. In some embodiments, a curable build material is primarily made up of a single poly mer or oligomer, which may also include a thermal initiator. In some embodiments, a curable build material includes any number of oligomers, polymers, and binder materials wherein additional covalent bonds are formed within the material upon heating to a sufficient temperature, without any radical initiator or catalyst being present therein. In some embodiments, a curable build material is made up primarily of a single oligomeric or polymeric material bearing at least one curable moiety.

[0115] In some embodiments, a curable build material is formed into a filament and is made up of at least a curable build material core, surrounded by a sheath of binding material. Herein, these types of build materials will be referred to as filamentous core-sheath materials.

[0116] In some embodiments, a curable build material is at least partially made up of one or more of the following: a saccharide, an oligosaccharide, a polysaccharide, a peptide, a polypeptide, a protein, a salt, an inorganic material, an inorganic salt, a silicate, an aluminate, a hy drate, a carbonate, a sugar, a sand, a clay and / or ceramic material, a clay and / or ceramic composite, a clay- and / or ceramic-polymer composite, a clay- and / or ceramic-metal composite (cermet). In some embodiments, a curable build material is made up of at least an inorganic material and a binding material. In some embodiments, a curable build material is made up of at least metallic particles, a monomer, optionally any number of oligomers and polymers, and optionally containing a thermal initiator. In some embodiments, a curable build material is made up of at least clay and / or ceramic particles, a monomer, optionally any number of oligomers and polymers, and optionally containing athermal initiator.

[0117] In some embodiments, a curable build material is made up of at least a clay and / or a ceramic, wherein the clay and / or ceramic may be capable of forming additional chemical bonds when sufficientlyheated. In some embodiments, a curable build material is made up of at least a clay and / or a ceramic present within a binder material, wherein the clay and / or ceramic may be capable of forming additional chemical bonds when sufficiently heated and the melting temperature of the binder is lower than the curing temperature of the clay and / or ceramic. In some embodiments, a curable build material is made up of at least a clay and / or a ceramic present within a material made up of at least a polymer and / or an oligomer, wherein the clay and / or ceramic may be capable of forming additional chemical bonds when sufficiently heated. In some embodiments, a curable build material is made up of at least a clay and / or a ceramic present within a material made up of at least a wax, wherein the clay and / or ceramic may be capable of forming additional chemical bonds when sufficiently heated. In some embodiments, a build material is made up of at least a binder and particles of a clay and / or a ceramic, formed into a filament. In some embodiments, a curable build material is formed into a filament and is made up of at least a clay and / or a ceramic core, surrounded by a sheath of binding material. In some embodiments, a clay and / or a ceramic and binder composite material is a filament, wherein a binding material is surrounded by a clay and / or a ceramic material. In some embodiments, a curable build material is at least made up of any number of cements, concretes, and cermets.

[0118] In some embodiments of a clay and / or a ceramic and binder composite material, the mass of the clay and / or ceramic makes up 1-99 %, 10-80 %, 20-60 %, or less than 50 % of the total mass of the composite material. Examples of clay and / or ceramic material and binder composite materials are currently offered for sale. One of these commercially available materials is described in the product description of LAYCERAMIC (Kai Parthy, CC-Products, “LAYCERAMIC sinter-able filament for printing’’, June 2017). This product description is incorporated by reference herein, in its entirety’.

[0119] In some embodiments, a curable build material is made up of at least particles having a sheath curable build material with a first melting temperature and a core curable build material with a second melting point, wherein these particles are present within a binder material having a third melting point (herein referred to as a core-sheath particle material). In some embodiments, the first melting temperature (that of the sheath material) of a core-sheath particle material is higher than those of the other two. Heating of this type of curable build material to a sufficient temperature causes the sheath material to rupture (or become permeable) and causes the core material to interact with the binder material. In some embodiments, the interaction of a core material and a binder material causes curing to occur in a core-sheath particle material. In some embodiments, the interaction of a core material and a binder material with heating causes curing to occur in a core-sheath particle material. In some embodiments, a core-sheath particle material contains at least one thermal initiator. In some embodiments, a core-sheath particle material is made up ofat least any number of monomers, oligomers, and polymers on either or both sides of the sheath, while a thermal initiator is present in only the sheath materials or only the core materials.

[0120] In some embodiments, a curable build material is made up of at least any number of monomers, oligomers, and polymers, wherein the any number of monomers, oligomers, and polymers include at least one acrylate species. In some embodiments, a curable build material is made up of at least an acrylate monomer and an acrylate oligomer or polymer, wherein the curable build material optionally contains a thermal initiator. In some embodiments, a curable build material is made up of at least polymethyl methaciylate and methyl methaciylate monomer. In some embodiments, a curable build matenal is made up of at least polymethyl methaciy late and polyethylene glycol. In some embodiments, a curable build material is made up of at least poly dimethylsiloxane (PDMS), or oligomers or monomers thereof.

[0121] In some embodiments, a curable build material is one of the following commercially' available compositions: Sylgard 184, Sylgard 186, DragonSkin 30, DragonSkin 10, Ecoflex 00-30, Ecoflex 00-10, 3M™ Scotch-Weld™ One Part Epoxy Adhesive 6101, MasterBond EP3HT, or an Opti-Cryl Heat Curing resin. In some embodiments, a curable build material is a resin composition known to be cured by UV light, but can also undergo thermal polymerization. In some embodiments, a curable build material is a composition known to be useful within an DLP and / or SLA additive manufactunng system. The disclosure of RULF (WO 2023 / 084517 Al, International Publication Date 19 May 2023) is incorporated herein by reference, in its entirety. In some embodiments, a build material herein is any material disclosed by RULF. In some embodiments, a build material herein is made up of at least particles of a composition disclosed by RULF w ithin a binder. In some embodiments, a build material is made up of at least a composition disclosed by RULF present as the core material of a core-sheath particle material or a filamentous coresheath material.

[0122] In some embodiments, a support material for an additive manufacturing system herein is a non-curable build material. In some embodiments, a support material for an additive manufacturing system herein is a relatively high melting-point polymer, such as PEEK, nylon 6-6, or HIPS. In some embodiments, a support material is a non-curable build material primarily composed of a single polymer, such as PLA, ABS, ASA, a nylon, polyamide, or polycarbonate.

[0123] A build material may be present in one or more of the following forms: a filamentous form that may be stored on a spool, a granulated form (powder, beads, particles, turnings, spheres, granules, or other low-aspect-ratio pieces of a material) that may be stored in a hopper, a solid form that may be stored in a hopper, a non-solid form that may be stored in a hopper, a filamentous core-sheath form that may be stored on a spool, or a coated core particle form that may be stored in a hopper. The core and sheath of a core-sheath build material may each contain any number of curable build materials, as long as the core and sheath are dissimilar in their makeup. A coated core particle build material may have any number of coating layers around a core, and each coating layer and the core may each contain any number of curable build materials, as long as the materials on either side of each core-coating or coating-coating interface are dissimilar in their makeup. In some embodiments, an additive manufacturing system may utilize multiple forms of build material.

[0124] In some embodiments, a curable build material may be filled with a non-curable material to change the properties of the overall build material. In some embodiments, a curable build material may be filled with glass particles and / or fibers. In some embodiments, a curable build material may be filled wi th carbon fibers. In some embodiments, a curable build material may be filled with fibers and / or particles of an inorganic material. In some embodiments, a curable build material may be filled with fibers and / or particles of a ceramic material. In some embodiments, a curable build material is food safe, biocompatible, and / or capable of use in cell culture.

[0125] In some embodiments, particles within a build material may be 1 nm to 3 mm, 100 pm to 50 nm, 15 pm to 85 pm, or 30 pm to 65 pm in average diameter. In some embodiments, a build material that is not a curable build material may be utilized by an additive manufacturing system in addition to a curable build material. In some embodiments, a non-curable build material may be utilized by a system herein to provide support material to the desired object.

[0126] In some embodiments, an additive manufacturing system incorporates a multi-material system, wherein the multi-material system is capable of altering a build material being extruded during printing, without the interaction of a human user. In some embodiments, a multi-material system operates by switching from extrusion of a first build material to extrusion of a second build material, with additional switches being possible. In some embodiments, a multi-material system operates by adjusting the ratio of two or more build materials that are being extruded simultaneously.

[0127] In some embodiments, an additive manufacturing system herein is capable of being used in a sub-optimal manner by using a non-curable material, wherein a thermal printhead is used to increase the adhesion betw een layers of extruded, non-curable build material. In some embodiments, an additive manufacturing system herein is capable of being used in a sub-optimal manner by using a non-curable material and intentionally not using a thermal printhead, so that the system operates in a manner similar to an FDM additive manufacturing system.

[0128] In some embodiments, an additive manufacturing system herein is capable of being used in a sub-optimal manner wherein non-selective curing is performed along with selective extrusion of build material.In these embodiments, the extrusion nozzle or nozzles are entirely responsible for the feature size of the objects produced.

[0129] GASES FOR USE WITHIN THE BUILD VOLUME

[0130] In some embodiments, at least a portion of the build volume contains a gas or mixture of gases that is less flammable than air. In some embodiments, at least a portion of the build volume contains a gas or mixture of gases that is less chemically reactive than air. In some embodiments, at least a portion of the build volume contains at least one inert gas and / or noble gas at a concentration higher than is present in air. In some embodiments, at least a portion of the build volume contains nitrogen at a higher concentration than is present in air. In some embodiments, at least a portion of the build volume contains oxygen in a lower concentration than is present in air. In some embodiments, at least a portion of the build volume contains 1-10 % oxygen. In some embodiments, at least a portion of the build volume contains one or more of the following gases at a higher concentration than is present in air: neon, argon, helium, nitrogen, and carbon dioxide. In some embodiments, a gas or mixture of gases known to be useful for welding applications, as a shielding gas or an active gas, has been added to at least a portion of the build volume. In some embodiments, the microheater printhead vertical offset is filled with air, neon, helium, argon, nitrogen, carbon dioxide, a plasma, or any of the gaseous mixtures described in this paragraph. The thermal conductivity' of a gas or plasma filling a space between the heating elements of a microheater printhead and the build material is an important variable, and preferably the gas or plasma has a high thermal conductivity'.

[0131] PROCESSING AFTER PRINTING

[0132] In some embodiments, after the printheads have completed their actions for the production of a desired object or a rough object, additional processing steps are performed. These additional processing steps may be performed while the desired object is still, in some manner, tethered to the print bed or after it has been removed from the print bed. In some embodiments, processing after printing serves to remove uncured build material from the cured build material. In some embodiments, processing after printing serves to remove uncured build material by mechanical agitation, such as scrapping, brushing, or sandblasting away the uncured build material. A solvent for the purpose of processing a rough or desired object after printing, may be a single solvent or a solution of multiple solvents selected from the following list: a hydrophilic solvent, a hydrophobic solvent, w ater, an oil, limonene, a plant-based oil, a synthetic oil, a silicone oil, acetic acid, acetone, acetonitrile, benzene, butanol, butyl acetate, carbon tetrachloride, chloroform, cyclohexane, dichloroethane, dichloromethane, dimethylformamide, dimethyl sulfoxide, dioxane, ethanol, ethyl acetate, diethyl ether, heptane, hexane, methanol, methyl ethyl ketone, pentane.propanol, diisopropyl ether, tetrahydrofuran, toluene, xylenes, pyridine, piperidine, n-methylpyrrolidone, an solvent of this list made to be acidic, a solvent of this list made to be alkaline, and / or another similar solvent. In some embodiments, processing after printing includes removing uncured build material by at least partially dissolving or solubilizing the uncured build material using a solvent. In some embodiments, uncured build material is dissolved or solubilized using a solvent that is at a temperature of greater than 22 °C. In some embodiments, support material or portions of a rough desired object may be removed using at least an acidic or alkaline solvent bath. In some embodiments, the uncured build material is dissolved or solubilized using a solvent that is at a temperature of greater than 40 °C. In some embodiments, after uncured build material is dissolved, solubilized, and / or melted, the uncured build material is precipitated or otherwise is returned to a solid and non-soluble state by cooling the solvent. In some embodiments, a surfactant is used to at least partially dissolve or solubilize uncured build material. Any of the procedures for processing after printing herein may be combined.

[0133] In some embodiments, an additive manufacturing system is capable of producing a desired object having a surface roughness of such a degree that the desired object is generally considered safe to contact food. In some embodiments, an additive manufacturing system is capable of producing a desired object having an Ra roughness of less than 5 pm, 3 pm, 1 pm, and / or 0.8 pm.

[0134] ENUMERATED EMBODIMENTS

[0135] 1) A system for additive manufacturing comprising at least one microheater array, at least one extrusion nozzle, and at least one curable build material, wherein the microheater array comprises at least 20 heating elements.

[0136] 2) The system of embodiment 1, wherein at least one extrusion nozzle is capable of selectively extruding a curable build material and at least one microheater array is capable of selectively curing a curable build material.

[0137] 3) The system of embodiments 1 or 2, wherein the area of the smallest heating element of a microheater array within a microheater printhead is smaller than the internal area of the largest extrusion nozzle, at the point where build material exits the extrusion nozzle, within the same additive manufacturing system.

[0138] 4) The system of any one of embodiments 1-3, wherein the microheater array is capable of curing a curable build material by directly contacting the curable build material.

[0139] 5) The system of any one of embodiments 1-3, wherein the microheater array is capable of curing a curable build material without directly contacting the curable build material.

[0140] 6) The system of any one of embodiments 1-5, wherein the microheater array is a linear array.7) The system of any one of embodiments 1-5, wherein the microheater array is a 2-dimensional array.

[0141] 8) The system of any one of embodiments 1-7, wherein one microheater array and one extrusion nozzle are present.

[0142] 9) The system of any one of embodiments 1-8, wherein the microheater array elements surround the extrusion nozzle.

[0143] 10) The system of any one of embodiments 1-9, wherein a protective sheet is present between the build material and the microheater array.

[0144] 11) The system of any one of embodiments 1-10, wherein at least a portion of the build volume contains a greater proportion of at least one of the following gases compared to the atmosphere of Earth at sea level: neon, helium, argon, nitrogen, carbon dioxide, an inert gas, and a nonflammable gas.

[0145] 12) The system of any one of embodiments 1-11, wherein a blade, a doctor blade, a protrusion, or a tool is present to make extruded build material level.

[0146] 13) The system of any one of embodiments 1-12, wherein at least one curable build material comprises particles primarily made up of a polymer, having a first melting temperature, surrounded by a composition primarily made up of a polymer, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

[0147] 14) The system of embodiment 14, wherein the particles have a glass transition temperature that is up to 150 °C higher than the glass transition temperature and / or the melting temperature of the surrounding composition.

[0148] 15) The system of any one of embodiments 1-12, wherein at least one curable build material comprises particles primarily made up of a polymer, having a first melting temperature, within a composition primarily made up of a wax, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

[0149] 16) The system of any one of embodiments 13-15, wherein the first melting temperature is up to 150 °C higher than the second melting temperature.

[0150] 17) The system of any one of embodiments 1-12, wherein at least one curable build material comprises metallic particles, having a curing temperature, within a binding material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

[0151] 18) The system of embodiment any one of embodiments 1-12, wherein at least one curable build material comprises particles of a clay and / or a ceramic, having a curing temperature, within a binder material, having a melting temperature, wherein curing temperature is higher than the melting temperature.19) The system of embodiment 17 or 18, wherein the melting temperature of the binder material is up to 2000 °C lower than the curing temperature.

[0152] 20) The system of any one of embodiments 1-12, wherein at least one curable build material comprises a plastisol.

[0153] 21) The system of any one of embodiments 1-12, wherein at least one curable build material comprises a solution containing a high concentration of a solute, wherein the additive manufacturing system causes dehydration of the solution.

[0154] 22) The system of any one of embodiments 1-12, wherein at least one curable build material comprises any number of monomers, oligomers, polymers, additives, and a thermal initiator.

[0155] 23) The system of embodiment 22, wherein the any number of monomers, oligomers, and polymers includes at least one acrylate compound.

[0156] 24) The system of embodiment any one of embodiments 1-12, wherein at least one curable build material comprises a type of clay and / or ceramic.

[0157] 25) The system of embodiment any' one of embodiments 1-12, wherein at least one curable build material comprises a core-sheath particle material.

[0158] 26) The system of embodiment any one of embodiments 1-12, wherein at least one curable build material is a filamentous core-sheath material.

[0159] 27) The system of any one of embodiments 1-26, wherein at least one curable build material is in the form of a filamentous form, a powdered form, a solid form, a non-solid form, a core-sheath particle form, a filamentous core-sheath form, and a coated core particle form.

[0160] 28) The system of any one of embodiments 1-27, wherein at least one curable build material is filled with at least one of glass particles, glass fibers, aramid fibers, sand, a continuous carbon fiber, carbon fibers, chopped carbon fibers, a ceramic material, and a stone material.

[0161] 29) A system for additive manufacturing comprising at least one thermal array, having a plurality of heating elements, and at least one extrusion nozzle.

[0162] 30) A system for additive manufacturing comprising at least one microheater array and a curable build material, wherein the microheater array comprises at least 20 heating elements.

[0163] 31) A system for additive manufacturing comprising a deposition printhead and a selective energy' source, wherein the selective energy’ source is capable of producing cured voxels of build material smaller in size than the deposition printhead is capable of depositing, and wherein the deposition printhead selectively deposits build material.

[0164] 32) A method of producing a three-dimensional obj ect comprising:a) selectively extruding build material through an extrusion nozzle; and

[0165] b) selectively curing build material by heating caused by a heating array.

[0166] 33) The method of embodiment 32, wherein the method further comprises the production of at least a portion of: a musical instrument, a specific dosage of a pharmaceutical composition, an impeller, a tool, an artificial organ, or an engine.

[0167] 34) The method of embodiment 33, wherein the pharmaceutical composition possesses a specific release profile, based upon its structure.

[0168] 35) A material for use within an additive manufacturing system compnsing a material wherein:

[0169] a) the material is capable of being extruded through an extrusion nozzle at an extrusion temperature;

[0170] and

[0171] b) the material is capable of being cured through the action of a heating array, and wherein curing takes place at a curing temperature that is higher than the extrusion temperature.

[0172] 36) The material of embodiment 35, further comprising particles primarily made up of a polymer, having a first melting temperature, surrounded by a composition primarily made up of a polymer, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

[0173] 37) The material of embodiment 36, wherein the particles have a glass transition temperature that is up to 150 °C higher than the glass transition temperature and / or the melting temperature of the surrounding composition.

[0174] 38) The material of embodiment 35, further comprising particles primarily made up of a polymer, having a first melting temperature, within a composition primarily made up of a wax, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

[0175] 39) The material of any one of embodiments 36-38, wherein the first melting temperature is up to 150 °C higher than the second melting temperature.

[0176] 40) The material of embodiment 35, further comprising metallic particles, having a curing temperature, within a binding material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

[0177] 41) The material of embodiment 35, further comprising particles of a clay and / or a ceramic, having a curing temperature, within a binder material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

[0178] 42) The material of embodiment 40 or 41, wherein the melting temperature of the binder material is up to 2000 °C lower than the curing temperature.43) The material of embodiment 35, further comprising any number of monomers, oligomers, polymers, additives, and a thermal initiator.

[0179] 44) The material of embodiment 43, wherein the any number of monomers, oligomers, and polymers includes at least one acry late compound.

[0180] 45) The material of any one of embodiments 35-44, wherein at least one curable build material is in the form of a filamentous form, a powdered form, a solid form, a non-solid form, a core-sheath particle form, a filamentous core-sheath form, and a coated core particle form.

[0181] 46) The material of any one of embodiments 35-45, wherein at least one curable build matenal is filled with at least one of: glass particles, glass fibers, aramid fibers, sand, a continuous carbon fiber, carbon fibers, chopped carbon fibers, a ceramic material, and a stone material.

[0182] EXAMPLES

[0183] Example 1: An Additive Manufacturing System using a Filamentous Build Material

[0184] A single extrusion printhead and two microheater printheads are present within this additive manufacturing system. The two microheater printheads present herein allow the width of the usable printing area to be larger than a single microheater printhead, and these printheads are not able to move independently from each other. The extenor support structure of the system is in the shape of a cube. The print bed is w ithin the cube at the bottom and is not capable of movement along any axis. The print bed is 220 mm w ide and 220 mm deep, with a useable printing area of 200 mm by 200 mm. The print bed is capable of being heated by a closed-loop system using ceramic heating elements. The printheads are attached to a square-shaped gantry' on the interior of the cube. This gantry' is capable of vertical movement (movement in the z axis). The z axis height of the microheater printheads, independent of the extrusion printhead, is manually adjustable. The extrusion printhead and the set of microheater printheads are capable of movement, independent from each other, along the x and y axes. The extrusion printhead and the set of microheater printheads are capable of movement in all 3 axes relative to the print bed. Stepper motors are present for the positioning of the printheads and movement of filamentous build material. A computer control unit is connected to the outside of the cube support structure.

[0185] The extrusion printhead is a direct drive extruder, wherein rollers apply force to filamentous build material. This applied force causes the build material to enter the extrusion printhead and causes heated build material to be extruded through an extrusion nozzle. The internal diameter of the extrusion nozzle is 0.4 mm. The build material is heated at 165-179 °C within the extrusion printhead.

[0186] Each microheater printhead contains a 1 -dimensional array of 2,496 individual heating elements over a distance of 106 mm. The build material is cured by heating elements within the microheaterprinthead by heating the build material to 179-195 °C. The build material being used in this additive manufacturing system is a filament comprising nylon 12 (PAI 2) particles within a binding material of polylactic acid polymer. The reservoir of build material is present on a spool, and the build material filament has a diameter of 1.75 mm. After printing, uncured build material is removed by soaking the rough object in a hot oil bath at 165-179 °C, aided by stirring and / or mechanical agitation.

[0187] Example 2: A Dual Extruder Additive Manufacturing System using a Filament

[0188] Two extrusion printheads and one microheater printhead are present within this additive manufacturing system. The exterior support structure of the system is in the shape of a cube. The print bed is within the cube at the bottom and is not capable of movement in any axis. The print bed is 220 mm wide and 120 mm deep, with a useable printing area of 200 mm by 106 mm. The print bed is capable of being heated by a closed-loop system using ceramic heating elements. The printheads are attached to a squareshaped gantiy on the interior of the cube. This gantiy is capable of vertical movement (movement in the z axis). The z axis height of the microheater printhead, independent of the extrusion printhead, is manually and automatically adjustable. The first extrusion printhead is capable of movement, independent of the other printheads in the x and y axes. The second extrusion printhead and the microheater printhead are capable of independent movement relative to each other only in the y axis. The second extrusion printhead and the microheater printhead are capable of movement in the x and y axes relative to the first extrusion printhead. Each printhead is capable of movement in all 3 axes relative to the print bed. Stepper motors are present for the positioning of both printheads and movement of filamentous build material. A computer control unit is connected to the outside of the cube support structure.

[0189] Both extrusion printheads are direct drive extruders, wherein rollers apply force to filamentous build material. This applied force causes the build material to enter the extrusion printhead and causes heated build material to be extruded through an extrusion nozzle. The internal diameter of the extrusion nozzle is 0.4 mm. The build material is heated at 165-179 °C within the extrusion printhead. One extrusion printhead is responsible for deposition of curable build material, and the second is responsible for the deposition of non-curable build material, being a filament primarily made up of poly lactic acid. The non-curable polylactic acid build material is deposited as support matenal, which the curable build matenal rests upon. The use of this non-curable build material decreases the cost of producing a desired object by limiting the required amount of the more costly curable build material.

[0190] The microheater printhead contains a 1 -dimensional array of 2,496 individual heating elements over a distance of 106 mm. The build material is cured by heating elements within the microheater printhead through heating the build material to 200-230 °C. The build material being used in this additivemanufacturing system is a filament comprising nylon 6 (PA6) particles within a binding material of polylactic acid polymer. The reservoir of build material is present on a spool, and the build material filament has a diameter of 1.75 mm. After printing, uncured build material is removed by soaking the rough object in hot oil bath at 165-190 °C, aided by stirring and / or mechanical agitation.

[0191] Example 3: An Additive Manufacturing System using a Thermal Initiator

[0192] A single extrusion printhead and a single microheater printhead are present within this additive manufacturing system. The exterior support structure of the system is in the shape of a cube. The print bed is within the cube at the bottom and is not capable of movement in any axis. The print bed is 220 mm wide and 130 mm deep, with a useable printing area of 200 mm by 106 mm. The print bed is capable of being heated by a closed-loop system using ceramic heating elements. The two printheads are attached to a square-shaped gantry on the interior of the cube. This gantry is capable of vertical movement (movement in the z axis). The z axis height of the microheater printhead, independent of the extrusion printhead, is manually adjustable. Each printhead is capable of movement, independent from the other printhead, along the x and y axes. Each printhead is capable of movement in all 3 axes relative to the print bed. Stepper motors are present for the positioning of both printheads and operation of the screw pump. A computer control unit is connected to the outside of the cube support structure.

[0193] The extrusion printhead is a direct drive extruder with a screw pump used to force a non-solid curable build material through the extrusion nozzle. The internal diameter of the extrusion nozzle is 0.4 mm. The build material is not heated within the extrusion printhead.

[0194] The microheater printhead contains a 1 -dimensional array of 7,584 individual heating elements over a distance of 160 mm. The build material is cured by heating elements within the microheater printhead by heating the build material to 100-300 °C. The build material being used in this additive manufacturing system is a non-solid curable build material comprising urethane dimethacrylate (UDMA), tri ethylene glycol dimethacrylate (TEGDMA), and lauroyl peroxide. The reservoir of build material is present in a vat, a tank, a hopper, or a reservoir. After printing, uncured build material is removed by soaking the rough object in a hydrophobic solvent, such as acetone or an ether, aided by agitation.

[0195] Example 4: An Additive Manufactunng System using a Ceramic Composite Material

[0196] A single extrusion printhead and a single microheater printhead are present w ithin this additive manufacturing system. The exterior support structure of the system is in the shape of a cube. The print bed is within the cube at the bottom and is not capable of movement along any axis. The print bed is 220 mm wide and 130 mm deep, with a useable printing area of 200 mm by 106 mm. The print bed is capable of being heated by a closed-loop system using ceramic heating elements. The two printheads are attached to asquare-shaped gantty on the interior of the cube. This gantry' is capable of vertical movement (movement in the z axis). The z axis height of the microheater printhead, independent of the extrusion printhead, is manually adjustable. The extrusion printhead is capable of movement, independent from the other printhead, along the x and y axes. The microheater printhead is capable of movement, independent from the other printhead, along only the y axis. The extrusion printhead is capable of movement in all 3 axes relative to the print bed, and the microheater printhead is capable of movement along 2 axes relative to the print bed. Stepper motors are present for the positioning of both printheads and movement of filamentous build material. A computer control unit is connected to the outside of the cube support structure.

[0197] The extrusion printhead is a direct drive extruder, wherein rollers apply force to filamentous build material. This applied force causes the build material to enter the extrusion printhead and causes heated build material to be extruded through an extrusion nozzle. The internal diameter of the extrusion nozzle is 0.6 mm. The build material is heated at 180-240 °C within the extrusion printhead.

[0198] The microheater printhead contains a 1 -dimensional array of 2,496 individual heating elements over a distance of 106 mm. The build material is cured by heating elements within the microheater printhead by heating the build material to 950-1050 °C. The build material being used in this additive manufacturing system is a filament comprising ceramic particles within poly caprolactone polymer. The resen' oir of build material is present on a spool, and the build material filament has a diameter of 3.0 mm. After printing, uncured build material is removed by soaking the rough object in hot water containing a surfactant, aided by mechanical agitation.

[0199] Example 5: An Additive Manufacturing System using a Metallic Composite Material

[0200] A single extrusion printhead and a single microheater printhead are present within this additive manufacturing system. The exterior support structure of the system is in the shape of a cube. The print bed is within the cube at the bottom and is not capable of movement in any axis. The print bed is 220 mm wide and 220 mm deep, with a useable printing area of 200 mm by 200 mm. The print bed is capable of being heated by a closed-loop system using ceramic heating elements. The two printheads are attached to a square-shaped gantry on the interior of the cube. This gantry is capable of vertical movement (movement in the z axis). The z axis height of the microheater printhead, independent of the extrusion printhead, is manually adjustable. Each printhead is capable of movement, independent from the other printhead, along the x and y axes. Each printhead is capable of movement in all 3 axes relative to the print bed. Stepper motors are present for the positioning of both printheads and movement of filamentous build material. A computer control unit is connected to the outside of the cube support structure.The extrusion printhead is a direct drive extruder, wherein rollers apply force to filamentous build material. This applied force causes the build material to enter the extrusion printhead and causes heated build material to be extruded through an extrusion nozzle. The internal diameter of the extrusion nozzle is 0.4 mm. The build material is heated at 180-240 °C within the extrusion printhead.

[0201] The microheater printhead contains a 1 -dimensional array of 2,496 individual heating elements over a distance of 106 mm. The microheater printhead is moved along two axes for the purpose of extending the area able to be cured by the microheater printhead. The build material is cured by heating elements within the microheater printhead by heating the build material to 750-900 °C. The build material being used in this additive manufacturing system is a filament comprising bronze particles and

[0202] poly caprolactone. The reservoir of build material is present on a spool, and the build material filament has a diameter of 1.75 mm. After printing, uncured build material is removed by soaking the rough object in hot water containing a surfactant, aided by mechanical agitation.

[0203] While the foregoing written description enables one of ordinary skill to make and use what is considered presently to be the best mode thereof, those of ordinary skill will understand and appreciate the existence of vanations, combinations, and equivalents of the specific embodiments, methods, and examples herein. The disclosure should therefore not be limited by the above-described embodiments, methods, and examples, but by all embodiments and methods within the scope and spirit of the disclosure.

Claims

CLAIMS:

1. A system for additive manufacturing comprising at least one microheater array, at least one extrusion nozzle, and at least one curable build material, wherein the microheater array comprises at least 20 heating elements.

2. The system of claim 1, wherein at least one extrusion nozzle is capable of selectively extruding a curable build material and at least one microheater array is capable of selectively curing a curable build material.

3. The system of claims 1 or 2, wherein the area of the smallest heating element of a microheater array within a microheater printhead is smaller than the internal area of the largest extrusion nozzle, at the point where build material exits the extrusion nozzle, within the same additive manufacturing system.

4. The system of any one of claims 1-3, wherein the microheater array is capable of curing a curable build material by directly contacting the curable build material.

5. The system of any one of claims 1-3, wherein the microheater array is capable of curing a curable build material without directly contacting the curable build material.

6. The system of any one of claims 1-5, wherein the microheater array is a linear array.

7. The system of any one of claims 1-5, wherein the microheater array is a 2-dimensional array.

8. The system of any one of claims 1-7, wherein one microheater array and one extrusion nozzle are present.

9. The system of any one of claims 1-8, wherein the microheater array elements surround the extrusion nozzle.

10. The system of any one of claims 1 -9, wherein a protective sheet is present between the build material and the microheater array.

11. The system of any one of claims 1-10, wherein at least a portion of the build volume contains a greater proportion of at least one of the following gases compared to the atmosphere of Earth at sea level: neon, helium, argon, nitrogen, carbon dioxide, an inert gas, and a nonflammable gas.

12. The system of any one of claims 1-11, wherein a blade, a doctor blade, a protrusion, or a tool is present to make extruded build material level.

13. The system of any one of claims 1-12, wherein at least one curable build material comprises particles primarily made up of a polymer, having a first melting temperature, surrounded by a composition primarily made up of a polymer, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

14. The system of claim 14, wherein the particles have a glass transition temperature that is up to 150 °C higher than the glass transition temperature and / or the melting temperature of the surrounding composition.

15. The system of any one of claims 1-12, wherein at least one curable build material comprises particles primarily made up of a polymer, having a first melting temperature, within a composition primarily made up of a wax, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

16. The system of any one of claims 13-15, wherein the first melting temperature is up to 150 °C higher than the second melting temperature.

17. The system of any one of claims 1-12, wherein at least one curable build material comprises metallic particles, having a curing temperature, within a binding material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

18. The system of claim any one of claims 1-12, wherein at least one curable build material comprises particles of a clay and / or a ceramic, having a curing temperature, w ithin a binder material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

19. The system of claim 17 or 18, wherein the melting temperature of the binder material is up to 2000 °C lower than the curing temperature.

20. The system of any one of claims 1-12, wherein at least one curable build material comprises a plastisol.

21. The system of any one of claims 1-12, wherein at least one curable build material comprises a solution containing a high concentration of a solute, wherein the additive manufacturing system causes dehydration of the solution.

22. The system of any one of claims 1-12, wherein at least one curable build material comprises any number of monomers, oligomers, polymers, additives, and a thermal initiator.

23. The system of claim 22, wherein the any number of monomers, oligomers, and polymers includes at least one acrylate compound.

24. The system of claim any one of claims 1-12, wherein at least one curable build material comprises a type of clay and / or ceramic.

25. The system of claim any one of claims 1-12, wherein at least one curable build material comprises a core-sheath particle material.

26. The system of claim any one of claims 1-12, wherein at least one curable build material is a filamentous core-sheath material.

27. The system of any one of claims 1-26, wherein at least one curable build material is in the form of: a filamentous form, a powdered form, a solid form, a non-solid form, a core-sheath particle form, a filamentous core-sheath form, and a coated core particle form.

28. The system of any one of claims 1-27, wherein at least one curable build material is filled with at least one of: glass particles, glass fibers, aramid fibers, sand, a continuous carbon fiber, carbon fibers, chopped carbon fibers, a ceramic material, and a stone material.

29. A system for additive manufacturing comprising at least one thermal array, having a plurality of heating elements, and at least one extrusion nozzle.

30. A system for additive manufacturing comprising at least one microheater array and a curable build material, wherein the microheater array comprises at least 20 heating elements.

1. A system for additive manufacturing comprising a deposition printhead and a selective energy source, wherein the selective energy source is capable of producing cured voxels of build material smaller in size than the deposition printhead is capable of depositing, and wherein the deposition printhead selectively deposits build material.

32. A method of producing a three-dimensional object comprising:(a) selectively extruding build material through an extrusion nozzle; and(b) selectively curing build material by heating caused by a heating array.

33. The method of claim 32, wherein the method further comprises the production of at least a portion of: a musical instrument, a specific dosage of a pharmaceutical composition, an impeller, a tool, an artificial organ, or an engine.

34. The method of claim 33, wherein the pharmaceutical composition possesses a specific release profile, based upon its structure.

35. A material for use within an additive manufacturing system comprising a material wherein:(a) the material is capable of being extruded through an extrusion nozzle at an extrusion temperature; and(b) the material is capable of being cured through the action of a heating array, and wherein curing takes place at a curing temperature that is higher than the extrusion temperature.

36. The material of claim 35, further comprising particles primarily made up of a polymer, having a first melting temperature, surrounded by a composition primarily made up of a polymer, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

37. The material of claim 36, wherein the particles have a glass transition temperature that is up to 150 °C higher than the glass transition temperature and / or the melting temperature of the surrounding composition.

38. The material of claim 35, further comprising particles primarily made up of a polymer, having a first melting temperature, within a composition primarily made up of a wax, having a second melting temperature, wherein the first melting temperature is higher than the second melting temperature.

39. The material of any one of claims 36-38, wherein the first melting temperature is up to 150 °C higher than the second melting temperature.

40. The material of claim 35, further comprising metallic particles, having a curing temperature, within a binding material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

41. The material of claim 35, further comprising particles of a clay and / or a ceramic, having a curing temperature, within a binder material, having a melting temperature, wherein curing temperature is higher than the melting temperature.

42. The material of claim 40 or 41, wherein the melting temperature of the binder material is up to 2000 °C lower than the curing temperature.

43. The material of claim 35, further comprising any number of monomers, oligomers, polymers, additives, and a thermal initiator.

44. The material of claim 43, wherein the any number of monomers, oligomers, and polymers includes at least one acry late compound.

45. The material of any one of claims 35-44, wherein at least one curable build material is in the form of: a filamentous form, a powdered form, a solid form, a non-solid form, a core-sheath particle form, a filamentous core-sheath form, and a coated core particle form.