Li 2ZrCl 6-Li 6PS 5Cl SOLID ELECTROLYTE PAIRING FOR HIGH VOLTAGE DUAL SOLID ELECTROLYTE SOLID-STATE BATTERIES

The Li2ZrCl6-Li6PS5Cl pairing stabilizes electrolyte interfaces in SSBs, addressing instability issues and achieving high energy density and long cycle life by forming a passivated interface with minimal resistance growth.

WO2026235975A1PCT designated stage Publication Date: 2026-11-12RGT UNIV OF CALIFORNIA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/025810
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-04-29
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing solid-state batteries (SSBs) face challenges with unstable interfaces between solid electrolytes, leading to impedance growth and rapid capacity loss due to reactivity at electrode-electrolyte interfaces, particularly in high-voltage dual-electrolyte architectures.

Method used

The pairing of Li2ZrCl6 (LZC) as a catholyte and Li6PS5Cl (LPSC) as an anolyte, stabilized through mixing and heat treatment, forms a passivated interface that maintains chemical and electrochemical stability, reducing interfacial resistance and enhancing ion conductivity.

Benefits of technology

This pairing achieves stable cycling with high voltage cathodes and metallic anodes, increasing energy density and cycle life by minimizing interfacial resistance growth, with capacity retention exceeding 90% after 200 cycles and 83.9% after 500 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026025810_12112026_PF_FP_ABST
    Figure US2026025810_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A device structure useful in a lithium-ion solid-state battery including a composite cathode layer comprising a mixture of a cathode active material, and an LZC compound comprising at least lithium, zirconium, and chlorine, wherein the LZC compound is a catholyte; and an anolyte comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure. The composite cathode layer and the anolyte layer are in direct contact or coupled via a catholyte layer; and the combination of the LZC compound and the LPSC compound is kinetically stabilized under normal operating conditions of an electrochemical cell comprising the device structure.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Li2ZrC16-Li6PS5Cl SOLID ELECTROLYTE PAIRING FOR HIGH VOLTAGE DUAL SOLID ELECTROLYTE SOLID-STATE BATTERIES

[0002] CROSS REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit under 35 U.S.C. Section 119(e) of the following co-pending and commonly-assigned application:

[0004] U.S. Provisional Application Serial No. 63 / 800,730 filed on May 6, 2025, by Elias Sebti, Tyler Pennebaker and Raphaele Clement, entitled “Li2ZrC16-Li6PS5Cl SOLID ELECTROLYTE PAIRING FOR HIGH VOLTAGE DUAL SOLID ELECTROLYTE SOLID-STATE BATTERIES” attorneys’ docket number G&C 30794.0881USP1 (UC-2025-389-1); which application is incorporated by reference herein.

[0005] This Application is related to International Patent Application No.

[0006] PCT / US24 / 55916 entitled “Li2ZrC16-Li6PS5Cl SOLID ELECTROLYTE PAIRING FOR DUAL SOLID ELECTROLYTE SOLID-STATE BATTERIES,” by Elias Sebti, Tyler Pennebaker, and Raphaele Clement., filed November 14, 2024, which application claims the benefit of US provisional application serial number 63 / 598,827, both of which applications are incorporated by reference herein.

[0007] BACKGROUND OF THE INVENTION

[0008] 1. Field of the Invention.

[0009] This invention relates to a Li2ZrC16-Li6PS5Cl solid electrolyte pairing for dual-solid-electrolyte solid-state batteries.

[0010] 2. Description of the Related Art.

[0011] A path towards scalable, high-energy-density SSBs can be imagined by harnessing two solid electrolytes with high ionic conductivities and differing electrochemical stability ranges. An electrolyte with a high oxidative stability is used as the catholyte in the composite cathode, and a layer of a second solid electrolyte with good reductive stability (the anolyte) separates the anode (negative electrode)and the composite cathode (positive electrode). In this architecture, the catholyte ensures stable interfaces with the positive electrode material and conductive additive, and the anolyte layer forms a stable interface with the negative electrode. This "single-layer" approach has been demonstrated in various Li- and Na-based SSBs combining a halide catholyte and thiophosphate anolyte.1 7An additional layer of the catholyte can be inserted between the anolyte and the cathode composite to avoid any possible contact between the cathode active material (and conductive additive) and the anolyte. Several studies have shown that this "bilayer" architecture drastically reduces reactivity and impedance growth at all electrode-electrolyte interfaces.2,5-26However, few studies have investigated the chemical stability and ion transport properties of the additional interface between the catholyte and anolyte in such architectures. Rosenbach et al. employed a bilayer approach that combined LisInCle (LIC) and LPSC in an NMC81 l+LIC|LIC|LPSC|Li-In cell and identified the formation of an interfacial region between the two electrolytes rich in In and S, resulting in significant impedance build-up and rapid capacity loss during cycling.2What is needed, then, are more stable solid electrolyte pairings. The present disclosure satisfies this need by demonstrating, for the first time, that the Li2ZrCle (LZQ-LigPSsCl (LPSC) combination interface is kinetically stabilized both upon mixing the two solid electrolytes and heat treating the mixture up to 260 °C and under battery operating conditions, providing a promising path towards high-voltage dual-solid-electrolyte SSBs.

[0012] SUMMARY OF THE INVENTION

[0013] The present disclosure demonstrates that the pairing of Li2ZrC16 (LZC) and LigPSsCl (LPSC) solid electrolytes (SE) increases the effective chemical and electrochemical stability windows of the electrolyte of Li -based solid-state batteries (SSBs) and enables stable cycling with a high voltage cathode and a metallic anode, with the potential to greatly enhance SSB energy density, safety, and cycle life.LZC is used as the catholyte material, withstanding the highly oxidative potentials in the cathode composite due to its stability up to > 4 V vs. Li / Li+.1,27Meanwhile, an LPSC anolyte layer is placed in contact with the metallic anode, preventing it from contacting the easily reduced LZC, and forms a passivated interface against the anode through decomposition into ionically conductive and electronically insulating products (LiCl, Li ? P- and Li2S)28. As such, interfaces at both electrodes are stabilized, promoting stable cycling of a high-energy-density SSB.

[0014] While maintaining stable interfaces with limited resistance growth is paramount to capacity retention in SSBs, the use of two SEs entrains the possibility of resistance growth at the SE|SE interface since halide and thiophosphate SEs can react, forming insulating interphases that limit Li conduction across the interface2. The LZC-LPSC pairing, on the contrary, shows an extremely low interfacial resistance (7 total, or 8.9 Q / cm2) at room temperature, accounting for only 1.5 % of the pellet’s overall resistance, with minimal interfacial resistance growth even after a 24-hour heat treatment at 110 °C.

[0015] The LZC-LPSC dual electrolyte was evaluated in SSBs comprising a LiNio.8Mno.1Coo.1O2 (NMC811) cathode and a Li-In anode. Although dual -electrolyte cells comprising a single electrolyte layer performed reasonably well, with 63.0 % of their initial capacity retained after 200 cycles, cells with a bilayer architecture exhibited a remarkable 90.4 % capacity retention under similar conditions (all values averaged over 2 cells). In addition, bilayer cells maintained an impressive 83.9 % capacity retention after 500 cycles.

[0016] Those results indicate that the LZC-LPSC interface is kinetically stabilized under battery operating conditions, but an additional layer of the LZC catholyte between the LPSC electrolyte and the cathode composite is necessary to prevent any reactivity between the NMC811 cathode or conductive carbon and the LPSC.

[0017] BRIEF DESCRIPTION OF THE DRAWINGSThe patent or application file contains at least one drawing executed in color. Copies of this patent or patent application publication with color drawing(s) will be provided by the Office upon request and payment of the necessary fee.

[0018] Referring now to the drawings in which like reference numbers represent corresponding parts throughout:

[0019] Figure 1: (a) Nyquist plot of the EIS data collected on an LPSC pellet under 75 MPa of uniaxial pressure and at temperatures from -48.1 to -70 °C. The measurements were conducted using Li-In electrodes to minimize the capacitive tail and facilitate data analysis. The spectra are shifted vertically for ease of comparison. Inset: Diagram of the RQ-RQ-Q equivalent circuit used to fit the spectra, (b) Arrhenius plot of the conductivities obtained by equivalent circuit fitting of the EIS data, shown with linear fits extrapolated to room temperature. For each dataset, the shaded region corresponds to the standard error in the fit.

[0020] Figure 2: (a) Nyquist plot of EIS spectra collected on an LZC pellet. Measurements used Ti electrodes at 75 MPa and temperatures between -48.1 and -70.0 °C. (b) Distribution of relaxation times (DRT) analysis of the EIS data, (c) Arrhenius plot of the conductivities obtained by fitting of the distribution of relaxation times, shown with linear fits extrapolated to room temperature. The lighter shaded regions correspond to the standard error in each fit.

[0021] Figure 3: (a) Nyquist plot of EIS spectra collected on an LPSC|LZC|LPSC sandwich pellet. Measurements used Li-In electrodes at 75 MPa and temperatures between -48.1 and -70.0 °C. Spectra are shifted vertically for ease of viewing, (b) The corresponding distribution of relaxation times (DRT) for the same spectra, (c) Arrhenius plot of the conductivities obtained by fitting of the distribution of relaxation times, shown with linear fits extrapolated to room temperature. The lighter shaded regions correspond to the standard error in each fit.

[0022] Figure 4: (a) Nyquist plot of EIS spectra collected on an LPSC|LZC|LPSC sandwich pellet following a heat treatment at 110 °C and 75 MPa for 24 hours. Measurements used Li-In electrodes at 75 MPa and temperatures between -48.1 and-70.0 °C. Spectra are shifted vertically for ease of viewing, (b) The corresponding distribution of relaxation times (DRT) for the same spectra, (c) Arrhenius plot of the conductivities obtained by fitting of the distribution of relaxation times, shown with linear fits extrapolated to room temperature. The lighter shaded regions correspond to the standard error in each fit.

[0023] Figure 5: Nyquist plots of EIS spectra collected on an LZC pellet (a) before and (b) after a heat treatment at 110 °C and 75 MPa for 24 hours (HT-110). Measurements used Ti electrodes at 75 MPa and 25.5 °C.

[0024] Figure 6: Electrochemical profiles obtained during galvanostatic cycling of (a), (b) bilayer and (c),(d) single-layer cells containing the LZC-LPSC solid electrolyte pairing at a current rate of C / 3 and at 30 °C, following three formation cycles performed at C / 10. The composite cathode comprises 66 wt.% NMC811, 31 wt.% LZC, and 3 wt.% VGCF, and the anode is Lio.sln. Specific discharge capacities were computed with respect to the mass of active material in the composite cathode.

[0025] Figure 7: Evolution of the capacity and coulombic efficiency of individual (a),(b) bilayer and (c), (d) single-layer cells containing the LZC-LPSC solid electrolyte pairing at a current rate of C / 3 and at 30 °C, following three formation cycles performed at C / 10. Outlier data points at approximately cycle 300 and cycle 400 for bilayer cells 1 and 2, respectively, were collected during a power shutdown that affected the temperature chamber containing the cells.

[0026] Figure 8: (a) Capacity retention of single-layer and bilayer LZC-LPSC cells cycled at C / 3 and 30 °C between 4.25-2.5 V vs. Li / Li+after three formation cycles at C / 10. The composite cathode comprises 66 wt.% NMC811, 31 wt.% LZC, and 3 wt.% VGCF, and the anode is Lio.sln. Specific discharge capacities were computed with respect to the mass of active material in the composite cathode. Inset: Schematics of solid-state batteries with single-layer and bilayer architectures, (b) Representative electrochemical profiles obtained during the second cycle of galvanostatic cycling at C / 10 for the single-layer and bilayer cell architectures.Figure 8(c) shows Table 1: Average charge and discharge potentials and coulombic efficiency of bilayer and single-layer LZC-LPSC cells over 200 cycles at C / 3. Energy density for the same cells, measured during their first cycle at C / 3.

[0027] Figure 9: Capacity retention of bilayer cells cycled at C / 3 and 30 °C between 4.25-2.5 V vs. Li / Li+after three formation cycles at C / 10. The HT-110 bilayer cells were subjected to a heat treatment at 110 °C and at 75 MPa of stack pressure for 24 hours prior to cycling. The composite cathode comprises 66 wt.% NMC811, 31 wt.% LZC, and 3 wt.% VGCF, and the anode is Lio.sln. Specific discharge capacities were computed with respect to the mass of active material in the composite cathode.

[0028] Figure 10(a)-10(b). Flowcharts illustrating a method of making the device structure.

[0029] Figure 11(a): Schematic of a solid electrolyte in a single layer configuration.

[0030] Figure 21(b): Schematic of a solid electrolyte in a bilayer configuration. Figure 12. Example battery heating and operating circuit.

[0031] Figure 13. Anode-less battery according to one or more embodiments.

[0032] DETAILED DESCRIPTION OF THE INVENTION

[0033] In the following description of the preferred embodiment, reference is made to the accompanying drawings which form a part hereof, and in which is shown by way of illustration a specific embodiment in which the invention may be practiced. It is to be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present invention.

[0034] Technical description

[0035] The present disclosure describes a device structure useful in a lithium-ion solid-state battery, comprising:

[0036] 1. a composite cathode layer comprising a mixture of a cathode active material, a carbon conductive additive, and an LZC compound comprisingat least lithium, zirconium, and chlorine, wherein the LZC is a catholyte; and

[0037] 2. an anolyte layer comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure,

[0038] wherein the composite cathode layer and the anolyte layer are in direct contact or coupled via a catholyte layer.

[0039] The combination of the LZC compound and the LPSC compound is chemically and electrochemically stable for operating conditions of an electrochemical cell comprising the device structure. The following sections describe experimental characterization of various embodiments of this device structure.

[0040] Experimental details

[0041] Electrochemical analysis of LZC, LPSC and LPSC|LZC|LPSC sandwich pellets was performed using the following techniques.

[0042] All electrochemical measurements were performed in custom pellet cells constructed of 10 mm Grade 5 titanium plungers and polyether ether ketone (PEEK) sleeves.

[0043] Electrochemical impedance spectroscopy (EIS) measurements were conducted at a series of temperatures from -70 to -48 °C on pressed pellets of as-milled LZC, as-received LPSC, and on LPSC|LZC|LPSC sandwich pellets. A low-temperature range was chosen and thick pellets were prepared to facilitate the deconvolution of bulk and grain boundary impedance contributions. An applied voltage amplitude of 10 mV and a frequency range of 7 MHz to 100 mHz were used.

[0044] Impedance contributions were determined by fitting to equivalent circuits and / or by the distribution of relaxation times (DRT) method.29Conductance values were then derived from the inverse resistances, and bulk conductivities were calculated using the dimensions of each pellet layer. Finally, activation energies weredetermined, and room-temperature conductivities were extrapolated, from Arrhenius fits of the low-temperature conductivity data.

[0045] Sample pellets were prepared directly in the custom pellet cells using as-received LPSC and as-milled LZC. Lio.sln, created by densifying a stoichiometric mixture of indium (99.99 % trace metals basis, Sigma-Aldrich) and stabilized lithium metal powders (Livent USA Corp.), served as non-blocking electrodes for EIS measurements.

[0046] To measure the conductivity of the LPSC electrolyte, 275 mg of LPSC was densified at 350 MPa before thin layers of Lio.sln were densified on both sides at 125 MPa.

[0047] To measure the conductivity of the LZC electrolyte, 230 mg of the powder was densified at 190 MPa. In this case, Lio.sln was not used to prevent reaction with the LZC.

[0048] To examine the LZC-LPSC interface, 100 mg of LZC was densified at 350 MPa at the center of the cell, with 100 mg of LPSC subsequently densified at 350 MPa on each side of the LZC layer. Finally, thin layers of Lio.sln were densified on both sides at 125 MPa.

[0049] All cells were sealed using high-vacuum grease to prevent air-exposure outside of a glove-box environment. Prior to the EIS measurements, 75 MPa of pressure was applied to the cells using a custom frame tightened using a torque wrench calibrated with a strain gauge to apply desired pressures. The total conductivity of each cell was measured during the initial tightening and was found to approach an asymptotic regime, indicating that 75 MPa established sufficient interfacial contact between all layers and that additional pressure would not significantly affect the interfacial impedance.

[0050] Heat treatment of the pellets was performed inside the custom cells in a Tenney TJR environmental chamber at 110 °C for 24 hours, maintaining 75 MPa using the custom holder.Further information on characterization (including all of the results on the kinetic stabilization of the LZC and LPSC interface) can be found in International Patent Application No. PCT7US24 / 55916 entitled “Li2ZrC16-Li6PS5Cl SOLID ELECTROLYTE PAIRING FOR DUAL SOLID ELECTROLYTE SOLID-STATE BATTERIES,” which application is incorporated by reference herein.

[0051] Experimental results

[0052] The EIS results on single-phase LPSC are presented in Figure la. The Nyquist plots were fit using an RQ-RQ-Q equivalent circuit, as shown inset in the Figure, where an R represents a resistor and a Q represents a constant-phase element. The bulk and grain boundary contributions are each modeled by parallel RQ blocks and the small capacitive effects of the electrode-pellet interface are modeled by a single constant-phase element. The bulk and grain boundary components were differentiated on the basis of their capacitances: fits of the single-phase LPSC data yielded a bulk capacitance in the range of 5.52-8.65 / 1011F and a grain boundary capacitance in the range of 2.90-5.40 / 109F overthe temperature range of -70. O to -48.1 °C, in good agreement with reported values for such phenomena.30Conductivities were derived from the inverse resistance of the R elements in the fitted equivalent circuits and are plotted in Figure lb across the range of temperatures measured. From these results, a bulk room temperature conductivity of 14 ± 3 mS cm1was extrapolated, and an activation energy of 0.45 ± 0.02 eV was obtained. A similar activation energy of 0.423 ± 0.006 eV was obtained for grain boundary transport, and the grain boundary resistance was found to account for 71 % of the total resistance of the sample at room temperature. Summing over the room temperature bulk and grain boundary contributions extrapolated from the Arrhenius fits, a total conductivity of 4.0 ± 0.4 mS cm1is derived, which is in close agreement with the actual conductivity measured at room temperature for this sample of 3.72 m

[0053]

[0054] S cmThe EIS results collected on the LZC pellet are presented in Figure 2a. For this sample, the grain boundary contribution dominates the impedance response, resulting in Nyquist plots that appear more semicircular than in the case of LPSC. The relatively small contribution from bulk conduction makes the fits to an equivalent circuit unreliable without additional information. Hence, the impedance spectra were further analyzed using the DRT method, as shown in Figure 2b. In the DRT plot, the bulk contribution is observed at small time constants r (high frequencies), and the larger grain boundary contribution appears at larger r values. Minor contributions are observed at even higher r values due to imperfect subtraction of polarization effects from the pellet-electrode interface during data processing.

[0055] The capacitance of each component was determined using C=r / R, where r is the center time constant of the peak, and R is the area under the peak. Once again, the assignment of the bulk and grain boundary contributions was based on reported values for such phenomena.30The conductivity of each component, obtained from the inverse of the area integrated under the corresponding DRT peak, is plotted in Figure 2c. From these results, a bulk conductivity of 0.8 ± 0.2 mS cm1was extrapolated at room temperature, and an activation energy of 0.27 ± 0.02 eV was obtained. A higher activation energy of 0.439 ± 0.005 eV was determined for grain boundary transport, and the grain boundary resistance was found to account for 78 % of the total resistance of the sample at room temperature. The total room temperature conductivity derived from the extrapolated bulk and grain boundary contributions is calculated to be 0.18 ± 0.02 mS cm ', in good agreement with the actual total conductivity measured at room temperature of 0.166 mS cm

[0056] The EIS results collected on the LPSC|LZC|LPSC sandwich pellet are shown in Figure 3a. While the bulk and grain boundary contributions are successfully separated in the case of the single-layer pellets, significant overlap between the bulk and grain boundary contributions from the two electrolytes precludes a full deconvolution of the EIS spectra obtained on the sandwich pellet, even when starting from the parameters derived from the single-phase pellets. However, the interfacialimpedance contribution appears at sufficiently low frequencies (higher time constants) that it can readily be separated from the bulk and grain boundary contributions using the distribution of relaxation times (DRT) method (Figure 3b).

[0057] Fitting this contribution across the -70 to -48 °C temperature range yields capacitances varying from 1.1 x 107to 7.3 x 106F, i.e., in the range expected for conduction across an interface.30A room temperature interfacial resistance of 7 (or 8.9 / cm2) is extrapolated from an Arrhenius fit of the low-temperature data, along with an interfacial activation energy of 0.47 ± 0.02 eV (Figure 3c). The total impedance of the sandwich pellet was measured to be 453 Q at room temperature, corresponding to a conductivity of 0.659 mS cm Thus, the interfacial resistance only accounts for 1.5 % of the pellet’s total impedance, suggestive of facile Li+ion transport between the LZC and LPSC phases.

[0058] Finally, EIS measurements were conducted on the same LPSC|LZC|LPSC sandwich pellet after it was subjected to a 24-hour, 110 °C heat treatment under a uniaxial pressure of 75 MPa, with results presented in Figure 4. At room temperature, the total impedance of the pellet is 638 and its conductivity is 0.468 mS cm1. The increase in the pellet’s impedance is primarily attributed to crystallization of LZC at moderate temperatures, which decreases its conductivity as shown in Figure 5. The interfacial activation energy remains constant (within error) at 0.43 ± 0.03 eV after the heat treatment (Figure 4c). The room temperature interfacial resistance increases by an order of magnitude to 70 . but still only accounts for 11 % of the pellet’s total impedance.

[0059] Overall, the low interfacial resistances measured on the sandwich pellet underscore the formation of a highly conductive LZC-LPSC interface that is not drastically affected by a 110 °C heat treatment. Hence, this pairing is viable for dualelectrolyte solid-state batteries and compatible with typical processing and operating conditions.

[0060] Evaluation of electrochemical performance of SSBsElectrochemical cells were assembled using as-received LPSC (NEI Corporation) as the separator layer, as-milled LZC as the catholyte in the composite cathode, and as an additional separator layer in bilayer cells. As-received LiNio.8Mno.1Coo.1O2 (NMC811, LG Energy Solution) with a boron-based surface coating layer was used as the cathode (positive electrode) active material in the composite cathode.

[0061] Composite cathodes were prepared by mixing NMC811, LZC, and vapor-grown carbon fibers (VGCF, Sigma- Aldrich) in a weight ratio of 66:31 :3 (NMC811:LZC:VGCF). The Lio.sln alloy anode material was prepared by mixing stoichiometric amounts of as-received stabilized lithium metal powder (Livent USA Corp.) and indium powder (325 mesh, Fisher Scientific) using a vortex mixer.

[0062] For single-layer cells, 75 mg of LPSC powder was first compressed at 1 ton (125 MPa) for one minute, resulting in a ~600 pm-thick layer. This was followed by adding 22-24 mg of NMC811 composite cathode (corresponding to approximately 21 mg cm2) and compressing at 3 tons (375 MPa) for three minutes, producing a ~110 pm-thick cathode. Afterward, 50 mg of Lio.sln alloy powder was added to the other side of the cell with a Cu foil disc serving as the current collector. Finally, the entire cell was compressed at 1 ton for 10 seconds to densify the Lio.sln alloy anode.

[0063] For bilayer cells, another 20 mg of LZC was added on top of the LPSC layer and compressed at 1 ton for one minute before adding the cathode composite, resulting in a ~90 pm-thick catholyte layer separating the anolyte and the composite cathode. To investigate the impact of hot pressing on cell performance, bilayer cells designated "HT-110" were subjected to 75 MPa of stack pressure at 110 °C for 24 hours before cycling.

[0064] Galvanostatic cycling was performed on a battery tester (Neware, CT-4000 Battery Testing System) with a voltage range of 1.9-3.65 V vs. Li+ / Li-In (or approximately 2.5-4.25 V vs. Li+ / Li). Three formation cycles were performed for each cell at C / 10 before long-term cycling tests at C / 3. C-rates were calculated assuming a theoretical capacity of 200 mAh g1for the NMC811 cathode activematerial. All cells were cycled in a temperature chamber maintained at 30 °C inside an Ar-filled glovebox.

[0065] Experimental results

[0066] The LZC-LPSC electrolyte pairing was tested in solid-state full cells comprising a Li-In anode and a LiNio.8Mno.1Coo.1O2 (NMC811) + LZC + vapor-grown carbon fiber (VGCF) composite cathode. Duplicate cells were assembled using a Lio.5ln|LPSC|NMC811+LZC+VGCF single-layer or Lio.sIn|LPSC|LZC|NMC811+LZC+VGCF bilayer architecture and cycled at C / 3 and 30 °C between 2.5-4.25 V vs. Li / Li+for 200 cycles after three formation cycles at C / 10. The evolution of the electrochemical profile, discharge capacity and coulombic efficiency with cycling, for individual cells, is presented in Figure 6 and Figure 7, respectively.

[0067] The capacity retention of single-layer and bilayer cells, averaged over duplicate cells, are plotted in Figure 8a, and representative voltage curves obtained during the second cycle at C / 10 are presented in Figure 8b. The bilayer cells show significantly higher capacity retention (90.4 % on average) than the single-layer cells (62.6 % on average) after 200 cycles, and an impressive 83.9 % capacity retention after 500 cycles, as shown in Figure 6a, b. Bilayer cells additionally exhibit a slightly lower voltage hysteresis, a higher energy density, and higher coulombic efficiencies on average than single-layer cells (see Table 1). While both cell architectures exhibit similar capacities and low overpotentials during the formation cycles (Figure 8b), the performance of the single-layer cells rapidly degrades, which is likely due to oxidation of the LPSC on contact with the NMC811 and VGCF components of the composite cathode during cycling. Hence, the additional layer of the LZC catholyte is necessary to maintain stable electrode-electrolyte interfaces and cycling performance. Although the capacity retention observed for both cell architectures is significantly higher than that reported for similar halide |thiophosphate dual-electrolyte cells using NMC811 cathodes, the specific capacities observed are still low relative to thetheoretical capacity of the NMC811 cathode (200 mAh g1) _31Hence, further optimization of the cell architecture, cell assembly, and of the processing of individual components is required to achieve greater cathode utilization, improve the cell’s energy and power density, and further reduce the overpotential.

[0068] We also investigated the impact of hot pressing the cell on the electrochemical performance, by subjecting bilayer cells to 75 MPa of stack pressure at 110 °C for 24 hours before cycling. The capacity retention of hot-pressed (HT-110) bilayer cells and standard bilayer cells (maintained at room temperature throughout), averaged over duplicate cells, are compared in Figure 9. Hot pressing reduces the capacity retention of bilayer cells from 90.4 to 85.7 % on average after 200 cycles, which could be due in part to the reduced ionic conductivity of the LZC catholyte upon recrystallization. However, the performance of the HT-110 bilayer cells is still significantly greater than that of the single-layer cells (62.3 % on average) discussed earlier.

[0069] Overall, the impressive capacity retention observed for bilayer LZC-LPSC cells indicates that this pairing is kinetically stabilized under normal battery operating conditions and could enable the development of high-energy -density solid-state batteries comprising a high-voltage oxide cathode and low-voltage metallic anode.

[0070] In conclusion, the results demonstrate:

[0071] • The LZC-LPSC pairing is a highly conductive, stable solid electrolyte pairing with high potential for implementation in energy-dense solid-state batteries.

[0072] • The LZC-LPSC phase boundary is highly conductive to Li, with a remarkably low interfacial resistance accounting for only 1.5 % of the total resistance of the constructed sandwich LPSC|LZC|LPSC pellet (or 8.9 Q / cm2).

[0073] • When the electrolyte pellet subjected to a 24-hour, 110 °C heat treatment under a uniaxial pressure of 75 MPa, the room temperature interfacial resistance increases by an order of magnitude to 70 Q. but still only accounts for 11 % of the pellet’s total impedance.• Cells assembled with the LZC-LPSC solid electrolyte pairing in a bilayer configuration and comprising a LiNio.8Mno.1Coo.1O2 cathode and a Li-In anode display excellent cycling stability, with 90.4 % capacity retention observed after 200 cycles and 83.9 % capacity retention after 500 cycles.

[0074] Example process steps for manufacturing a solid electrolyte useful in a lithium-ion battery

[0075] Figure 10A illustrates a method of making a solid electrolyte combined with a catholyte, comprising the following steps:

[0076] Block 900 represents obtaining a catholyte powder comprising LZC and an anolyte powder comprising LPSC. The catholyte powder can be manufactured by ball milling or an equivalent method.

[0077] Block 902 represents densifying the catholyte powder to form a pelletized catholyte layer or densifying the anolyte powder to form a pelletized anolyte layer — i.e., densifying the catholyte (anolyte) powder to form a catholyte (anolyte) pelletized layer.

[0078] Block 904 represents depositing the anolyte (catholyte) powder on the catholyte (anolyte) pelletized layer and densifying the anolyte (catholyte) powder on the catholyte (anolyte) pelletized layer to form the anolyte (catholyte) pelletized layer.

[0079] In one embodiment, the densification comprises cold pressing. In one cold pressing process, pressure is applied with a hydraulic press at room temperature.

[0080] In one or more embodiments, the densifying comprises or further comprises hot pressing or hot rolling (calendering) to form a more intimate interfacial contact between the pelletized layers. In one hot-pressing process, the sample is previously cold pressed in a cell, then the sample cell is clamped into a vice (e.g., at 70 MPa), and then the sample cell is placed in environmental chamber for 24 hours at 110 °C.

[0081] Refs [21-23] in International Patent Application No. PCT / US24 / 55916 describe example processes for cold and hot pressing processes in solid electrolytes that can be used for the cold and hot pressing described herein. Ref. (23) describes anexample hot calendering process for solid-state batteries that can be used for densification. Other fabrication methods are described in Refs (35-36).

[0082] Block 906 represents the anolyte and catholyte formed by the process, wherein the catholyte pelletized layer and the anolyte pelletized layer form a bilayer, or wherein the first pelletized layer is a densified composite cathode containing the catholyte in a single-layer configuration.

[0083] Block 908 represents optionally combining the electrolyte with the electrodes of a battery. In one embodiment, the combining comprises pressing the catholyte layer to a cathode and pressing the anolyte layer to an anode.

[0084] Figure 10B illustrates a method of making the anolyte combined with the catholyte according to another embodiment.

[0085] Block 910 represents combining an LZC powder comprising the LZC compound with a first binder in a LZC solution.

[0086] Block 912, 914 represents combining an LPSC powder comprising the LPSC compound with a second binder in an LPSC solution.

[0087] Block 916 represents drying the solutions to form an LZC layer and an LPSC layer.

[0088] Block 918 represents contacting the LZC layer with the LPSC layer.

[0089] Fig. 11(a) and 11(b) illustrate an example device structure 100, 200 useful in a lithium-ion solid-state battery, comprising:

[0090] a composite cathode layer 102 comprising a mixture of a cathode active material 116, and an LZC compound (LZC / 104 in Fig. 11A and 1 IB) comprising at least lithium, zirconium, and chlorine, wherein the LZC compound is a catholyte; an anolyte layer 103 comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure, wherein:

[0091] the composite cathode layer 102 and the anolyte layer 103 are in direct contact or coupled via a catholyte layer 108; and

[0092] the combination of the LZC compound and the LPSC compound is kinetically stabilized under normal operating conditions of an electrochemical cell comprisingthe device structure. Also shown in Fig. 11(a) and 11(b) are the anode 118 and current collector 120 (e.g., aluminum) and current collector 122 (e.g., copper) which typically comprise a metal foil.

[0093] Fig. 12 illustrates a lithium-ion solid-state battery comprising the device structure of any of the embodiments comprising an anode. Fig. 12 further illustrates a circuit 1202 configured to charge and / or operate the electrochemical cell at a voltage ( > 3.6 V) applied across the anode and the composite cathode layer 102 and / or current collectors 120, 122, through the use of the anolyte layer 103 comprising the LPSC compound and the catholyte layer 108 comprising the LZC compound, wherein the voltage is larger than that applied in an electrochemical cell comprising a single layer separating the anode and the composite cathode layer comprising either the LPSC compound without the LZC compound, or the LZC compound without the LPSC compound while still retaining at least 90% capacity after 200 cycles of charging and discharging. In one or more embodiments, the voltage applied between the cathode 102 and anode 118 is in a range of 3.6V-5V at the end of each charging step.

[0094] In one or more embodiments, the cathode active material is LiNixMnyCoi-x-yO2 (NMC). In one or more embodiments, the cathode optionally can comprise x > 0.8, LiNixCoi-x-yAlyCh (NCA)-type cathodes or “Li-rich” NMC cathodes, Lii+aNixMnyCoi-x-y-aC>2, or spinel cathodes. In one or more embodiments, the cathode active material is (NMC811 = LiNio.8Mno.1Coo.1O2). In one or more embodiments, the cathode active material comprises a lithium transition metal compound and / or the anode comprises lithium metal, a lithium alloy, silicon, or a lithium -silicon alloy (e.g., lithium transition metal compound comprises a lithium transition metal oxide, a lithium transition metal oxyfluoride, a lithium transition metal polyanionic compound, a lithium transition metal fluoride, or a lithium transition metal sulfide).

[0095] Fig. 13 illustrates an anode-less battery 1300 comprising the device structure of any of the embodiments, comprising the anolyte layer 103 between the composite cathode layer 102 and a current collector 1302 such that lithium extracted from thecomposite cathode layer 102 upon charging of the battery is plated directly onto the current collector to form an anode. The anode-less battery may optionally further comprise a carbon / alloy interlayer between the anolyte layer 103 and current collector 1302.

[0096] In one or more embodiments, the LZC compound and the LPSC compound have chemical compositions such that a LZC-LPSC phase boundary is conductive to Li as characterized by measurement of a pellet comprising the LZC compound sandwiched between layers of the LPSC compound having an interfacial resistance accounting for at most 88 / cm2after the pellet is subjected to a 24-hour, 110 °C heat treatment under a uniaxial pressure of 75 MPa, e.g. using the apparatus of Fig. la of (37).

[0097] Further information on characterization of the performance of embodiments of the devices described herein can be found in (38).

[0098] Device embodiments

[0099] Illustrative embodiments of the inventive subject matter manufactured according to embodiments described herein include, but are not limited to, the following.

[0100] 1. A device structure useful in a lithium-ion solid-state battery, comprising:

[0101] a composite cathode layer comprising a mixture of a cathode active material, and an LZC compound comprising at least lithium, zirconium, and chlorine, wherein the LZC compound is a catholyte;

[0102] an anolyte comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure, wherein:

[0103] the composite cathode layer and the anolyte layer are in direct contact or coupled via a catholyte layer; andthe combination of the LZC compound and the LPSC compound is kinetically stabilized under normal operating conditions of an electrochemical cell comprising the device structure.

[0104] 2. The device structure of clause 1, wherein the LZC compound has a trigonal structure (P-3ml) or a monoclinic structure (C2 / m).

[0105] 3. The device structure of clause 1 or 2, wherein the LZC compound comprises Li2ZrClg and the LPSC compound comprises LigPSsCl.

[0106] 4. The device structure of any of the clauses 1-3, wherein:

[0107] the LZC compound comprises Li2-xZrC16-x(0 < x < 2) or Li2Zn-xC16-4X(0 < x < 1) or a variant thereof swapping out at least one of Li, Zr, or Cl by another element; and

[0108] the LPSC compound comprises Li6-xPSs-xQi+x(0 < x < 1).

[0109] 5. The device structure of any of the clauses 1-4, further comprising a catholyte layer between and in direct contact with the anolyte layer and the composite cathode layer, wherein the LZC compound, the LPSC compound, and the cathode active material consist of chemical compositions resulting in a capacity retention of at least 90 % over 200 cycles and at least 83 % after 500 cycles, with each cycle comprising a charge and discharge of the cell under C / 3 conditions (charging over 3 hours and discharging over 3 hours) or at higher rates, when the electrochemical cell comprises the bilayer between and in contact with the anode and the composite cathode layer and a pressure of no more than 75 MPa is applied.

[0110] 6. The device structure of any of the clauses 1-5, wherein the LZC compound and the LPSC compound have chemical compositions such that an LZC-LPSC phase boundary is conductive to Li, as characterized by measurement of a pellet comprising the LZC compound sandwiched between layers of the LPSC compound having an interfacial resistance of at most 9 Q / cm2.

[0111] 7. The device structure of any of the clauses 1-6, wherein the LZC compound and the LPSC compound have chemical compositions such that a LZC-LPSC phase boundary is conductive to Li as characterized by measurement of a pelletcomprising the LZC compound sandwiched between layers of the LPSC compound having an interfacial resistance accounting for at most 88 / cm2after the pellet is subjected to a 24-hour, 110 °C heat treatment under a uniaxial pressure of 75 MPa.

[0112] 8. The device structure of any of the clauses 1-7, wherein:

[0113] the catholyte layer and / or the composite cathode layer each comprise a first plurality of particles comprising the LZC compound and a first diameter D 1 in a range 10 nm < DI < 2 microns, and

[0114] the anolyte layer comprises a second plurality of particles comprising the LPSC compound and a second diameter D2 in a range of 10 nm < D2 < 10 microns.

[0115] 9. A lithium-ion solid-state battery comprising the device structure of any of the clauses 1-8 comprising an anode and wherein the anolyte layer is between the anode and the catholyte layer.

[0116] 10. The battery of clause 9, wherein the anode comprises Li, a Li-In alloy, Si, or a Li-Si alloy.

[0117] IL A lithium-ion solid-state battery system comprising the device structure of any of the clauses 1-10, comprising:

[0118] an electrochemical cell comprising the anolyte layer between an anode layer and the composite cathode layer; and

[0119] a circuit configured to charge and / or operate the electrochemical cell at an increased voltage ( > 3.6 V) applied across the anode and the composite cathode layer, through the use of the anolyte comprising the LPSC compound and the catholyte comprising the LZC compound, wherein the voltage is larger than that applied in an electrochemical cell comprising a single layer separating the anode and the composite cathode layer comprising either the LPSC compound without the LZC compound, or the LZC compound without the LPSC compound e.g,. while still retaining at least 90% capacity after 200 cycles of charging and discharging.

[0120] 12. An anode-less battery comprising the device structure of any of the clauses 1-10, comprising the anolyte layer between the composite cathode layer and acurrent collector such that lithium extracted from the composite cathode layer upon initial charging of the battery is plated directly onto the current collector to form an anode.

[0121] 13. A battery comprising the electrochemical cell of any of the clauses 1-12, comprising the anolyte layer between the composite cathode layer and an anode, wherein the anolyte layer forms a passivating interface against the anode through decomposition into ionically conductive and electronically insulating products (comprising at least one of LiCl, LisP, or Li2S).

[0122] 14. The device structure of any of the clauses 1-13 wherein the cathode active material is LiNixMnyCoi-x-yO2 (NMC) cathodes optionally with x > 0.8, LiNixCoi-x-yAlyCh (NCA)-type cathodes or “Li-rich” NMC cathodes, Lii+aNixMnyCoi-x-y-aO2, or spinel cathodes.

[0123] 15. The device structure of any of the clauses 1-14 wherein the cathode active material is (NMC811 = LiNio.sMno.1Coo.1O2).

[0124] 16. The device structure of any of the clauses 1-1 , wherein the cathode active material comprises a lithium transition metal compound and / or the anode comprises lithium metal, a lithium alloy, silicon, or a lithium-silicon alloy.

[0125] 17. The device structure of clause 16, wherein the lithium transition metal compound comprises a lithium transition metal oxide, a lithium transition metal oxyfluoride, a lithium transition metal polyanionic compound, a lithium transition metal fluoride, or a lithium transition metal sulfide.

[0126] 18. The device structure of any of the clauses 1-17, wherein the cathode active material is polycrystalline or single-crystalline.

[0127] 19. The device structure of any of the clauses 1-18, wherein the composite cathode layer further comprises carbon fibers (e.g., vapor grown carbon fibers).

[0128] 20. The device structure of clause 5, wherein the cycling is performed with the anode that does not include LPSC.

[0129] 21. The device structure of any of the clauses 1-20, wherein the catholyte does not include indium.22. The device of any of the clauses 1-21, wherein the electrified anolytecatholyte interface between the catholyte layer and the anolyte layer is practically stabilized by the slow kinetics of decomposition reactions taking place between the LZC compound and the LPSC compound, and does not contribute significantly to capacity degradation. We have seen no visible decomposition at room temperature when mixing the electrolytes, even after months.

[0130] 23. The device of any of the clauses 1-22, wherein the composite cathode layer comprises a carbon conductive additive.

[0131] 24. A device structure useful in a lithium-ion solid state battery, comprising:

[0132] a composite cathode layer comprising a mixture of a cathode active material, a carbon conductive additive, and an LZC compound comprising at least lithium, zirconium, and chlorine, wherein the LZC is a catholyte, wherein the cathode active material is coated and / or the carbon conductive additive is (e.g., vapor grown) carbon fibers; and

[0133] an anolyte layer comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure, wherein the composite cathode layer and the anolyte layer are in direct contact or coupled via a catholyte layer.

[0134] 25. The device structure of clause 24, wherein the weight percentage of the carbon fibers is in a range of 0.2-5 wt.%.

[0135] 26. The device structure of clause 24 or 25, wherein the cathode active material is coated with at least one of boron, aluminum, or LiNbCL.

[0136] 27. The device structure of any of the clauses 24-26 further comprising the structure of any of the clauses 2-23.

[0137] 28. The device structure of any of the clauses 1-27, wherein the anolyte is an anolyte layer.

[0138] 29. A lithium-ion solid-state battery system comprising the device structure of any of the clauses 1-10 or any of the clauses 12-23, comprising:an electrochemical cell comprising the anolyte layer between an anode layer and the composite cathode layer; and

[0139] a circuit configured to charge and / or operate the electrochemical cell at an increased voltage ( > 3.6 V, or 3.6 V < V < 5 V) applied across the anode and the composite cathode layer.

[0140] Advantages and improvements

[0141] When put together, the limited electrochemical stability window of solid electrolytes (SEs) and the implementation of high voltage cathodes in batteries with high energy density metallic anodes seem mutually exclusive, casting doubt on the possibility of energy density improvements in solid-state batteries (SSBs). No known SE composition is stable against both metallic anodes and high-voltage oxide cathodes. A path forward can be imagined, however, through the combination of different SEs in a single SSB to withstand the electrochemical environments on both sides of the battery. By implementing an oxidation-resistant catholyte and reductionresistant anolyte, a dual-SE approach leverages the differing electrochemical stability windows of the two electrolytes to maximize the stability of SE interfaces at both the cathode and anode, enabling stable high-voltage cycling over a wide potential range. Alternatively, a bilayer architecture can also be implemented, where a thin layer of the catholyte is introduced between the anolyte layer and the cathode composite, preventing any possible contact between the cathode active material and oxidation-prone anolyte layer. This can also be done with a thin layer of the reduction-resistant anolyte to prevent catholyte contact with the anode.

[0142] The present disclosure shows that the Li2ZrC16-Li6PS5Cl (LZC-LPSC) SE pairing exhibits stable behavior under standard cycling operations in single layer and bilayer SSBs assembled with LiNio.8Mno.1Coo.1O2 (NMC811) as the cathode active material and Li-In as the anode. Although dual-electrolyte cells comprising a single electrolyte layer performed reasonably well, with 63.0 % of their initial capacity retained after 200 cycles, cells with a bilayer architecture exhibited a remarkable90.4 % capacity retention under similar conditions, and an impressive 83.9 % capacity retention after 500 cycles. Going forward, we plan to explore the use of additional cathode and anode materials with this pairing, further demonstrating its potential to stabilize interfaces with high-voltage cathodes and high-capacity anode materials. Overall, the LZC-LPSC system is a conductive, scalable, and kinetically-stabilized system with high promise for implementation in energy-dense dual-SE SSBs with steady long-term cycling.

[0143] Implementation of the I^ZrClg-LigPSsCl (LZC-LPSC) SE pairing in SSBs presents an opportunity to achieve high energy densities surpassing those of today’s conventional lithium-ion batteries, and significant safety benefits due to the replacement of flammable organic electrolytes. Energy density and safety are the two most important metrics for the development of batteries for consumer products and with sufficiently small form factors to power mobile devices such as smartphones and electric vehicles. Hence, any battery technology that can enhance either of those two metrics carries enormous commercial advantages. The observed compatibility of the LZC-LPSC system signifies that SSBs incorporating > 4 V oxide cathodes and metallic anodes can be cycled stably.1,11’16’19’32In addition, both LZC and LPSC are deformable, which greatly facilitates their processing and enables full cell fabrication with cold pressing, lowering manufacturing costs relative to SSBs incorporating hard oxide SE materials. While cold pressing is the cheapest manufacturing option, we also demonstrate that their chemical stability up to 260 °C allows for (mild) hot pressing of the bilayer to facilitate densification, with little impact on the resistance at the LZC-LPSC interface. Linally, LZC and LPSC are both composed of earth-abundant elements with robust supply networks meaning that sourcing of their synthetic precursor materials is less subject to market volatility. Both classes of materials (halides and thiophosphates) have also been manufactured with scalable wet synthesis procedures, facilitating their respective production.8’12’33References

[0144] The following references are incorporated by reference herein.

[0145] (1) Cronk, A.; Chen, Y.-T.; Deysher, G.; Ham, S.-Y.; Yang, H.; Ridley, P.; Sayahpour, B.; Nguyen, L. H. B.; Oh, J. A. S.; Jang, J.; Tan, D. H. S.; Meng, Y. S. Overcoming the Interfacial Challenges of LiFePO4 in Inorganic All-Solid-State Batteries. ACS Energy Lett. 2023, 8 (1), 827-835.

[0146] https : / / doi .org / 10.102 l / acsenergylett.2c02138.

[0147] (2) Rosenbach, C.; Walther, F.; Ruhl, J.; Hartmann, M.; Hendriks, T. A.; Ohno, S.; Janek, J.; Zeier, W. Visualizing the Chemical Incompatibility of Halide and Sulfide - Based Electrolytes in Solid - State Batteries. Advanced Energy Materials 2022, 2203673. https: / / doi.org / 10.1002 / aenm.202203673.

[0148] (3) Wu, E. A.; Baneqee, S.; Tang, H.; Richardson, P. M.; Doux, J.-M.; Qi, J.; Zhu, Z.; Grenier, A.; Li, Y.; Zhao, E.; Deysher, G.; Sebti, E.; Nguyen, H.;

[0149] Stephens, R.; Verbist, G.; Chapman, K. W.; Clement, R. J.; Baneqee, A.; Meng, Y. S.; Ong, S. P. A Stable Cathode-Solid Electrolyte Composite for High-Voltage, Long-Cycle-Life Solid-State Sodium -Ion Batteries. Nat Commun 2021, 12 (1), 1256. https: / / doi.org / 10.1038 / s41467-021-21488-7.

[0150] (4) Kim, J. S.; Jung, S.; Kwak, H.; Han, Y.; Kim, S.; Lim, J.; Lee, Y. M.; Jung, Y. S. Synergistic Halide-Sulfide Hybrid Solid Electrolytes for Ni-Rich Cathodes Design Guided by Digital Twin for All-Solid-State Li Batteries. Energy Storage Materials 2023, 55, 193-204. https: / / doi.Org / 10.1016 / j.ensm.2022.ll.038.

[0151] (5) Ye, Q.; Li, X.; Zhang, W.; Xia, Y.; He, X.; Huang, H.; Gan, Y.; Xia, X.; Zhang, J. Slurry-Coated LiNi0.8Co0.1Mn0.102-Li3InC16 Composite Cathode with Enhanced Interfacial Stability for Sulfide-Based All-Solid-State Batteries. ACS Appl. Mater. Interfaces 2023, 15 (15), 18878-18888.

[0152] https : / / doi .org / 10.1021 / acsami .3c00178.

[0153] (6) Kwak, H.; Kim, J.-S.; Han, D.; Kim, J. S.; Park, J.; Kwon, G.; Bak, S.-M.; Heo, U.; Park, C.; Lee, H.-W.; Nam, K.-W.; Seo, D.-H.; Jung, Y. S. Boosting the Interfacial Superionic Conduction of Halide Solid Electrolytes for All-Solid-StateBateries. Nat Commun 2023, 14 (1), 2459. htps: / / doi.org / 10.1038 / s41467-023-38037-z.

[0154] (7) Tron, A.; Beutl, A.; Mohammad, I.; Paolella, A. Insights into the Chemical and Electrochemical Behavior of Halide and Sulfide Electrolytes in All-Solid-State Bateries. Energy Adv. 2025. htps: / / doi.org / 10.1039 / D4YA00618F.

[0155] (8) Wang, C.; Liang, J.; Luo, J.; Liu, J.; Li, X.; Zhao, F.; Li, R.; Huang, H.; Zhao, S.; Zhang, L.; Wang, J.; Sun, X. A Universal Wet-Chemistry Synthesis of Solid-State Halide Electrolytes for All-Solid-State Lithium-Metal Bateries. Sci. Adv.

[0156] 2021, 7 (37), eabhl896. htps: / / doi.org / 10.1126 / sciadv.abhl896.

[0157] (9) Wang, H.; Li, Y.; Tang, Y.; Ye, D.; He, T.; Zhao, H.; Zhang, J.

[0158] Electrochemically Stable Li3-xInl-xHfxC16 Halide Solid Electrolytes for All-Solid-State Bateries. ACS Appl. Mater. Interfaces 2023, 15 (4), 5504-5511.

[0159] htps : / / do i .org / 10.1021 / acsami .2c21022.

[0160] (10) Deng, Z.; Jin, Z.; Chen, D.; Ni, D.; Tian, M.; Zhan, Y.; Li, S.; Sun, Y.; Huang, X.; Zhao, Y. Bilayer Halide Electrolytes for All-Inorganic Solid-State Lithium-Metal Bateries with Excellent Interfacial Compatibility. ACS Appl. Mater. Interfaces 2022, 14 (43), 48619-48626. https: / / doi.org / 10.1021 / acsami.2cl2444.

[0161] (11) Luo, X.; Zhong, Y.; Wang, X.; Xia, X.; Gu, C.; Tu, J. Ionic Conductivity Enhancement of Li2ZrC16 Halide Electrolytes via Mechanochemical Synthesis for All-Solid-State Lithium-Metal Bateries. ACS Appl. Mater. Interfaces 2022, 14 (44), 49839-49846. htps: / / doi.org / 10.1021 / acsami.2cl4903.

[0162] (12) Li, X.; Liang, J.; Chen, N.; Luo, J.; Adair, K. R.; Wang, C.; Banis, M. N.; Sham, T.-K.; Zhang, L.; Zhao, S.; Lu, S.; Huang, H.; Li, R.; Sun, X. Water-Mediated Synthesis of a Superionic Halide Solid Electrolyte. Angewandte Chemie International Edition 2019, 58 (46), 16427-16432.

[0163] htps : / / doi .org / 10.1002 / anie .201909805.

[0164] (13) Hendriks, T. A.; Lange, M. A.; Kiens, E. M.; Baeumer, C.; Zeier, W. G. Balancing Partial Ionic and Electronic Transport for Optimized Cathode Utilization of High - Voltage LiMn 2 O 4 / Li 3 InCi 6 Solid - State Bateries.Bateries & Supercaps 2023, 6 (4), e202200544. htps: / / doi.org / 10.1002 / bat.202200544.

[0165] (14) Ji, W.; Zheng, D.; Zhang, X.; Ding, T.; Qu, D. A Kinetically Stable Anode Interface for Li3YC16-Based All-Solid-State Lithium Bateries. J. Mater. Chem. A 2021, 9 (26), 15012-15018. https: / / doi.org / 10.1039 / DlTA03042F.

[0166] (15) Zhang, H.; Yu, Z.; Cheng, J.; Chen, H.; Huang, X.; Tian, B.

[0167] Halide / Sulfide Composite Solid-State Electrolyte for Li-Anode Based All-Solid-State Bateries. Chinese Chemical Leters 2023, 34 (11), 108228. htps: / / doi.Org / 10.1016 / j.cclet.2023.108228.

[0168] (16) Wang, K.; Ren, Q.; Gu, Z.; Duan, C.; Wang, J.; Zhu, F.; Fu, Y.; Hao, J.; Zhu, J.; He, L.; Wang, C.-W.; Lu, Y.; Ma, J.; Ma, C. A Cost-Effective and Humidity-Tolerant Chloride Solid Electrolyte for Lithium Bateries. Nat Commun 2021, 12 (1), 4410. https: / / doi.org / 10.1038 / s41467-021-24697-2.

[0169] (17) Luo, X.; Cai, D.; Wang, X.; Xia, X.; Gu, C.; Tu, J. A Novel Ethanol-Mediated Synthesis of Superionic Halide Electrolytes for High-Voltage All-Solid-State Lithium-Metal Bateries. ACS Appl. Mater. Interfaces 2022, 14 (26), 29844-29855. htps: / / doi.org / 10.1021 / acsami.2c06216.

[0170] (18) Koc. T.; Hallot, M.; Quemin, E.; Hennequart, B.; Dugas, R.;

[0171] Abakumov, A. M.; Lethien, C.; Tarascon, J.-M. Toward Optimization of the Chemical / Electrochemical Compatibility of Halide Solid Electrolytes in All-Solid-State Bateries. ACS Energy Let. 2022, 7 (9), 2979-2987.

[0172] htps : / / doi .org / 10.102 l / acsenergylet.2c01668.

[0173] (19) Chen, S.; Yu, C.; Chen, S.; Peng, L.; Liao, C.; Wei, C.; Wu, Z.; Cheng, S.; Xie, J. Enabling Ultrafast Lithium-Ion Conductivity of Li2ZrC16 by Indium Doping. Chinese Chemical Leters 2022, 33 (10), 4635-4639.

[0174] htps : / / do i .org / 10.1016 / j.cclet.2021.12.048.

[0175] (20) Zhou, L.; Kwok, C. Y.; Shyamsunder, A.; Zhang, Q.; Wu, X.; Nazar, L. F. A New Halospinel Superionic Conductor for High-Voltage All Solid StateLithium Batteries. Energy Environ. Sei. 2020, 13 (7), 2056-2063.

[0176] https : / / doi .org / 10.1039 / D0EE01017K.

[0177] (21) Samanta, S.; Bera, S.; Biswas, R. K.; Mondal, S.; Mandal, L.;

[0178] Banerjee, A. lonocovalency of the Central Metal Halide Bond-Dependent Chemical Compatibility of Halide Solid Electrolytes with Li 6 PS 5 Cl. ACS Energy Lett. 2024, 3683-3693. https: / / doi.org / 10.1021 / acsenergylett.4c01084.

[0179] (22) Panchai, A. A.; Pennebaker, T. N. T.; Sebti, E.; Li, Y.; Li, Y.;

[0180] Clement, R. J.; Canepa, P. Compatibility of Halide Bilayer Separators for All-Solid-State Batteries. ACS Energy Lett. 2024, 5935-5944. https: / / doi.org / 10.1021 / acsenergylett.4c02590.

[0181] (23) Song, Z.; Wang, T.; Yang, H.; Kan, W. H.; Chen, Y.; Yu, Q.; Wang, L.; Zhang, Y.; Dai, Y.; Chen, H.; Yin, W.; Honda, T.; Avdeev, M.; Xu, H.; Ma, J.; Huang, Y.; Luo, W. Promoting High-Voltage Stability through Local Lattice Distortion of Halide Solid Electrolytes. Nat Commun 2024, 15 (1), 1481. https: / / doi.org / 10.1038 / s41467-024-45864-l.

[0182] (24) Kim, Y.; Juarez-Yescas, C.; Liao, D. W.; Jangid, M. K.; Joshi, P.; Yang, H.; Zahiri, B.; Braun, P. V.; Dasgupta, N. P. Thin Tree-Standing Sulfide / Halide Bilayer Electrolytes for Solid-State Batteries Using Slurry Processing and Lamination. ACS Energy Lett. 2024, 9 (4), 1353-1360.

[0183] https : / / doi .org / 10.102 l / acsenergylett.4c00092.

[0184] (25) Kochetkov, I.; Zuo, T.-T.; Ruess, R.; Singh, B.; Zhou, L.; Kaup, K.; Janek, J.; Nazar, L. Different Interfacial Reactivity of Lithium Metal Chloride Electrolytes with High Voltage Cathodes Determines Solid-State Battery Performance. Energy Environ. Sci. 2022, 10.1039.D2EE00803C. https: / / doi.org / 10.1039 / D2EE00803C.

[0185] (26) Zhou, L.; Zuo, T.-T.; Kwok, C. Y.; Kim, S. Y.; Assoud, A.; Zhang, Q.; Janek, J.; Nazar, L. F. High Areal Capacity, Long Cycle Life 4 V Ceramic All-Solid-State Li-Ion Batteries Enabled by Chloride Solid Electrolytes. Nat Energy 2022, 7 (1), 83-93. https: / / doi.org / 10.1038 / s41560-021-00952-0.(27) Wang, S.; Bai, Q.; Nolan, A. M.; Liu, Y.; Gong, S.; Sun, Q.; Mo, Y. Lithium Chlorides and Bromides as Promising Solid-State Chemistries for Fast Ion Conductors with Good Electrochemical Stability. Angew. Chem. Int. Ed. 2019, 58 (24), 8039-8043. https: / / doi.org / 10.1002 / anie.201901938.

[0186] (28) Wenzel, S.; Sedlmaier, S. J.; Dietrich, C.; Zeier, W. G.; Janek, J. Interfacial Reactivity and Interphase Growth of Argyrodite Solid Electrolytes at Lithium Metal Electrodes. Solid State Ionics 2018, 318 (July 2017), 102-112. https: / / doi.Org / 10.1016 / j.ssi.2017.07.005.

[0187] (29) Wan, T. H.; Saccoccio, M.; Chen, C.; Ciucci, F. Influence of the Discretization Methods on the Distribution of Relaxation Times Deconvolution: Implementing Radial Basis Functions with DRTtools. Electrochimica Acta 2015, 184, 483-499. https: / / doi.Org / 10.1016 / j.electacta.2015.09.097.

[0188] (30) Irvine, J. T. S.; Sinclair, D. C.; West, A. R. Electroceramics:

[0189] Characterization by Impedance Spectroscopy. Advanced Materials 1990, 2 (3), 132— 138. https : / / doi .org / 10.1002 / adma.19900020304.

[0190] (31) Savina, A. A.; Abakumov, A. M. Benchmarking the Electrochemical Parameters of the LiNi0.8Mn0.lCo0.102 Positive Electrode Material for Li-Ion Batteries. Heliyon 2023, 9 (12), e21881. https: / / doi.Org / 10.1016 / j.heliyon.2023.e21881.

[0191] (32) Tan, D. H. S.; Chen, Y.-T.; Yang, H.; Bao, W.; Sreenarayanan, B.; Doux, J.-M.; Li, W.; Lu, B.; Ham, S.-Y.; Sayahpour, B.; Scharf, J.; Wu, E. A.;

[0192] Deysher, G.; Han, H. E.; Hah, H. J.; Jeong, H.; Lee, J. B.; Chen, Z.; Meng, Y. S. Carbon-Free High-Loading Silicon Anodes Enabled by Sulfide Solid Electrolytes. Science 2021, 373 (6562), 1494-1499. https: / / doi.org / 10.1126 / science.abg7217.

[0193] (33) Rajagopal, R.; Subramanian, Y.; Jung, Y. J.; Kang, S.; Ryu, K.-S. Rapid Synthesis of Highly Conductive Li6PS5Cl Argyrodite -Type Solid Electrolytes Using Pyridine Solvent. ACS Appl. Energy Mater. 2022, 5 (8), 9266-9272.

[0194] https: / / doi.org / 10.1021 / acsaem.2c01157.(34) Further information on one or more embodiments of the invention can be found in International Patent Application No. PCT / US24 / 55916 entitled “Li2ZrC16-Li6PS5Cl SOLID ELECTROLYTE PAIRING FOR DUAL SOLID ELECTROLYTE SOLID-STATE BATTERIES,” which application is incorporated by reference herein.

[0195] (35) JP published application No. JP-2023-21918 A (GS YUASA CORP) (36) US 2021 / 0005929 Al (HYUNDAI MOTOR COMPANY et al.

[0196] (37) Doux, J.-M.; Yang, Y.; Tan, D. H. S.; Nguyen, H.; Wu, E. A.; Wang, X.; Banerjee, A.; Meng, Y. S. Pressure Effects on Sulfide Electrolytes for All Solid-State Batteries. J. Mater. Chem. A 2020, 8 (10), 5049-5055.

[0197] https 7 / doi .org / 10.1039 / C9TA 12889A.

[0198] (38) Pennebaker, T., Sebti, E., Panchai, A., Huang, C-J., Trenikhina, Y ., Li, T., Li, Y ., Li, Y ., Kelly, S., Meng, Y. S., Canepa, P.*, Clement, R., Establishing the Compatibility of Anolytes and Catholytes in Dual Electrolyte Solid-State Batteries, under revision. DOI: 10.26434 / chemrxiv-2025-chtzv.

[0199] Conclusion

[0200] This concludes the description of the preferred embodiment of the present invention. The foregoing description of one or more embodiments of the invention has been presented for the purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Many modifications and variations are possible in light of the above teaching. It is intended that the scope of the invention be limited not by this detailed description, but rather by the claims appended hereto.

Claims

WHAT IS CLAIMED IS:

1. A device structure useful in a lithium-ion solid-state battery, comprising:a composite cathode layer comprising a mixture of a cathode active material, and an LZC compound comprising at least lithium, zirconium, and chlorine, wherein the LZC compound is a catholyte;an anolyte layer comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure, wherein:the composite cathode layer and the anolyte layer are in direct contact or coupled via a catholyte layer; andthe combination of the LZC compound and the LPSC compound is kinetically stabilized under normal operating conditions of an electrochemical cell comprising the device structure.

2. The device structure of claim 1, wherein the LZC compound has a trigonal structure (P-3ml) or a monoclinic structure (C2 / m).

3. The device structure of claim 1, wherein the LZC compound comprises Li2ZrClg and the LPSC compound comprises LigPSsCl.

4. The device structure of claim 1, wherein:the LZC compound comprises Li2-xZrC16-x(0 < x < 2) or Li2Zn-xC16-4X(0 < x < 1) or a variant thereof swapping out at least one of Li, Zr, or Cl by another element; andthe LPSC compound comprises Li6-xPS5-xCli+x(0 < x < 1).

5. The device structure of claim 1 further comprising the catholyte layer between and in direct contact with the anolyte layer and the composite cathode layer,wherein the LZC compound, the LPSC compound, and the cathode active material consist of chemical compositions resulting in a capacity retention of at least 90 % over 200 cycles and at least 83 % after 500 cycles, with each cycle comprising a charge and discharge of the cell under C / 3 conditions (charging over 3 hours and discharging over 3 hours) or at higher rates, when the electrochemical cell comprises the bilayer between and in contact with the anode and the composite cathode layer and a pressure of no more than 75 MPa is applied.

6. The device structure of claim 1, wherein the LZC compound and the LPSC compound have chemical compositions such that an LZC-LPSC phase boundary is conductive to Li, as characterized by measurement of a pellet comprising the LZC compound sandwiched between layers of the LPSC compound having an interfacial resistance of at most 9 Q / cm2.

7. The device structure of claim 1, wherein the LZC compound and the LPSC compound have chemical compositions such that a LZC-LPSC phase boundary is conductive to Li as characterized by measurement of a pellet comprising the LZC compound sandwiched between layers of the LPSC compound having an interfacial resistance accounting for at most 88 / cm2after the pellet is subjected to a 24-hour, 110 °C heat treatment under a uniaxial pressure of 75 MPa.

8. The device structure of claim 1, wherein:the catholyte layer and / or the composite cathode layer each comprise a first plurality of particles comprising the LZC compound and a first diameter D 1 in a range 10 nm < DI < 2 microns, andthe anolyte layer comprises a second plurality of particles comprising the LPSC compound and a second diameter D2 in a range of 10 nm < D2 < 10 microns.

9. A lithium-ion solid-state battery comprising the device structure of claim 1 comprising an anode and wherein the anolyte layer is between the anode and the catholyte layer.

10. The battery of claim 9, wherein the anode comprises Li, a Li -In alloy, Si, or a Li-Si alloy.

11. A lithium-ion solid-state battery system comprising the device structure of claim 1, comprising:an electrochemical cell comprising the anolyte layer between an anode layer and the composite cathode layer; anda circuit configured to charge and / or operate the electrochemical cell at an increased voltage ( > 3.6 V) applied across the anode and the composite cathode layer, through the use of the anolyte comprising the LPSC compound and the catholyte comprising the LZC compound, wherein the voltage is larger than that applied in an electrochemical cell comprising a single layer separating the anode and the composite cathode layer comprising either the LPSC compound without the LZC compound, or the LZC compound without the LPSC compound while still retaining at least 90% capacity after 200 cycles of charging and discharging.

12. An anode-less battery comprising the device structure of claim 1 comprising the anolyte layer between the composite cathode layer and a current collector such that lithium extracted from the composite cathode layer upon initial charging of the battery is plated directly onto the current collector to form an anode.

13. A battery comprising the device structure of claim 1, comprising the anolyte between the composite cathode layer and an anode, wherein the anolyte forms a passivating interface against the anode through decomposition into ionically conductive and electronically insulating products (comprising at least one of Li Cl, LisP, or Li2S).

14. The device structure of claim 1 wherein the cathode active material is LiNixMnyCoi-x-yCh (NMC) cathodes optionally with x > 0.8, LiNixCoi-x-yAlyCh (NCA)-type cathodes or “Li-rich” NMC cathodes, Lii+aNixMnyCoi-x-y-aCh, or spinel cathodes.

15. The device structure of claim 1 wherein the cathode active material is (NMC811 = LiNio.8Mno.1Coo.1O2).

16. The device structure of claim 1, wherein the cathode active material comprises a lithium transition metal compound and / or the anode comprises lithium metal, a lithium alloy, silicon, or a lithium-silicon alloy.

17. The device structure of claim 16, wherein the lithium transition metal compound comprises a lithium transition metal oxide, a lithium transition metal oxyfluoride, a lithium transition metal polyanionic compound, a lithium transition metal fluoride, or a lithium transition metal sulfide.

18. The device structure of claim 1, wherein the cathode active material is poly crystalline or single-crystalline.

19. The device structure of claim 1, wherein the composite cathode layer further comprises carbon fibers.

20. The device structure of claim 5, wherein the cycling is performed with the anode that does not include LPSC.

21. The device structure of claim 1, wherein the catholyte does not include indium.

22. The device structure of claim 1, wherein the electrified anolytecatholyte interface between the catholyte and the anolyte is practically stabilized bythe slow kinetics of decomposition reactions taking place between the LZC compound and the LPSC compound, such that the decomposition reactions do not contribute significantly to capacity degradation.

23. The device structure of claim 1, wherein the composite cathode layer comprises a carbon conductive additive.

24. A device structure useful in a lithium-ion solid state battery, comprising:a composite cathode layer comprising a mixture of a cathode active material, a carbon conductive additive, and an LZC compound comprising at least lithium, zirconium, and chlorine, wherein the LZC is a catholyte, wherein the cathode active material is coated and / or the carbon conductive additive is carbon fibers; andan anolyte layer comprising an LPSC compound comprising at least lithium, phosphorus, sulfur, and chlorine arranged in an argyrodite structure, wherein the composite cathode layer and the anolyte layer are in direct contact or coupled via a catholyte layer.

25. The device structure of claim 24, wherein the weight percentage of the carbon fibers is in a range of 0.2-5 wt.%.

26. The device structure of claim 24 or 25, wherein the cathode active material is coated with at least one of boron, aluminum, or LiNbO3.