Crystalline boron nitride deposition
A PECVD process using dual RF sources deposits boron nitride with high thermal conductivity and dielectric properties, addressing the heat dissipation challenge in semiconductor devices by enhancing the thermal management of advanced devices.
Patent Information
- Application Number
- PCT/US2026/026977
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-06
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional dielectric materials used in semiconductor fabrication, such as silicon oxides and silicon nitrides, fail to adequately dissipate the high heat generated in advanced devices due to their low thermal conductivity, necessitating the development of materials with high thermal conductivity and electrical insulation properties.
A plasma enhanced chemical vapor deposition (PECVD) process using dual RF sources to deposit boron nitride at temperatures below 400°C, employing high and low frequency powers to achieve a hexagonal crystal structure with high thermal conductivity and dielectric properties.
The process produces boron nitride with a thermal conductivity of at least 2 W/m-K and a dielectric constant of at most 6, effectively dissipating heat while maintaining electrical insulation, suitable for intermetal and interlayer dielectric layers in semiconductor devices.
Smart Images

Figure US2026026977_12112026_PF_FP_ABST
Abstract
Description
Atorney Docket No. LAM1P135 WO- 12202-1 WO CRYSTALLINE BORON NITRIDE DEPOSITIONINCORPORATION BY REFERENCE
[0000] A PCT Request Form is filed concurrently with this specification as part of the present application. Each application that the present application claims benefit of or priority to as identified in the concurrently filed PCT Request Form is incorporated by reference herein in their entireties and for all purposes.BACKGROUND
[0001] In semiconductor fabrication, a dielectric material is incorporated into a device to provide insulating properties between features such as current carrying lines or devices while efficiently dissipating the heat generated during device operation. Such requirements are commonly specified for logic devices.
[0002] The background provided herein is for the purposes of generally presenting the context of the disclosure. Work of the presently named inventors, to the extent that it is described in this background or presented as contextual information in the description, that may not otherwise qualify as prior art at the time of filing, is neither expressly nor impliedly admitted as prior art against the present disclosure.SUMMARY
[0003] Disclosed herein are methods of depositing boron nitride on a substrate, which methods may be characterized by the following operations:(a) receiving the substrate in a plasma reactor;(b) delivering a process gas to the plasma reactor, wherein the process gas comprises: a boron precursor, a nitrogen source comprising ammonia or molecular nitrogen, and a carrier gas; and(c) applying a low frequency power to a first electrode, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz.
[0004] Also disclosed herein are methods of depositing boron nitride on a substrate, which methods may be characterized by the following operations:Atorney Docket No. LAM1P135 WO- 12202-1 WO (a) receiving the substrate in a plasma reactor;(b) delivering a process gas to the plasma reactor, wherein the process gas comprises: a boron precursor, a nitrogen source comprising ammonia or molecular nitrogen, and a carrier gas;(c) applying a high frequency power to a first electrode in the plasma reactor, wherein the high frequency power is at least about 400 W at a frequency of between about 13-60 MHz; and (d) applying a low frequency power to a second electrode, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz.
[0005] In some embodiments, a method disclosed herein may further comprise applying a high frequency power to a second electrode in the plasma reactor, wherein the high frequency power is at a frequency of about 13-60 MHz.
[0006] In some embodiments, the high frequency power is about 0.1 to 2000 W at a frequency of about 13-60 MHz. In some embodiments, the high frequency power is at least about 400 W at a frequency of about 13-60 MHz.
[0007] In some embodiments, the low frequency power is about 2,000 to 5.000 W at a frequency of about 400 kHz and 1MHz.
[0008] In some embodiments, the resulting boron nitride has a substantially hexagonal crystal structure, a purity of at least about 97 mol%, athermal conductivity of at least about 2 W / m-K, a dielectric constant of at most about 6, or any combination of these features. In some embodiments, the boron nitride has a substantially cubic crystal structure. In some embodiments, the boron nitride comprises a mixture of hexagonal and cubic crystal structures.
[0009] The first and second electrodes may have various structures, orientations, relative arrangements, and configurations. In some embodiments, the first and second electrodes are different. In some embodiments, the second electrode comprises or is integrated in a substrate support.
[0010] The substrate may be made from any of various materials. In some embodiments, the substrate comprises a single crystal silicon wafer.
[0011] The boron nitride may be used in any of many different structures, some of which form part of an electrical device. In some embodiments, the boron nitride forms at least part of an intermetal dielectric layer on the substrate. In some embodiments, the boron nitride forms at leastAtorney Docket No. LAM1P135 WO- 12202-1 WO part of a packaging structure. As an example, the packaging structure may comprise a bond film for bonding to a carrier substrate.[00121 In some embodiments, the boron nitride has a dielectric constant ranging from about 4 to about 6. In some embodiments, the boron nitride exhibits a leakage current of at most about 6.5 *10'4A / cm2at an electric field of 4 MV / cm, or at most about 2.5 *10'9A / cm2at the electric field of 2 MV / cm. In some embodiments, the boron nitride has a thermal conductivity ranging from about 2 to about 25 W / m-K. In some embodiments, the boron nitride has a grain size ranging from about 3 to about 9.5 nm. In some embodiments, the boron nitride has an impurity ranging from about 0 to about 3 mol%. In some embodiments, the boron nitride has a density ranging from about 1.5 to about 2.3 g / cc.
[0013] In certain embodiments, the boron precursor comprises diborane (EhHe), borazine, Ammonia Borane complex (AB), 1, 3, 5-Tri(methyl)borazine (TMBZ), B-tris(dimethylamino) borazine [N-dimethyl TMBZ], Tris(dimethylamino) borane (TDMAB), boron chloride (BCls), boron fluoride (BF3), or any combination thereof.
[0014] In certain embodiments, the process gas comprises the boron precursor in a concentration of about 0.01 mol% to 0.3 mol%, the nitrogen source in a concentration of about 50 mol% to 90 mol%, and the carrier gas in a concentration of about 9 mol% to about 50 mol%.
[0015] In certain embodiments, the process gas further comprises a fluorine source. In some embodiments, the fluorine source is nitrogen trifluoride (NF3), molecular fluorine (F2), sulfur hexafluoride (SFs), or boron trifluoride (BF3), or any combination thereof.
[0016] In certain embodiments, the high frequency power is about 400 and 4,000 W at a frequency of between about 13-60 MHz. In certain embodiments, such as one where the HF power is about 400 and 4,000 W. the low frequency power is about 400 and 4,000 W at a frequency of between about 400 kHz and 1MHz.
[0017] In certain embodiments, operations (b)-(c) are performed at a pressure of about 0.5 to about 6.5 Torr. In certain embodiments, operations (b)-(c) are performed at a temperature of about 350°C to about 450°C. In certain embodiments, operations (b)-(d) are performed at a pressure of about 0.5 to about 6.5 Torr. In certain embodiments, operations (b)-(d) are performed at a temperature of about 350°C to about 450°C.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0018] In certain embodiments, the boron nitride has an atomic ratio between boron and nitrogen of about 1: 1.01 to about 1: 1.25. In certain embodiments, the boron nitride has a compressive stress relative to the substrate of about -300 to about -3200 GPa.
[0019] Aspects of this disclosure pertain to systems for producing boron nitride, which systems may be characterized by a plasma enhanced chemical vapor deposition reactor and a controller. The plasma enhanced chemical vapor deposition reaction includes (a) at least two electrodes with one configured to produce high frequency RF energy for generating a plasma and another configured to produce low frequency RF energy for driving ions from the plasma to a surface of the substrate, and (b) a process gas inlet. The controller may be configured to cause concurrently: (i) delivery7of a process gas to the plasma enhanced chemical vapor deposition reactor via the process gas inlet, wherein the process gas comprises: a boron precursor, a nitrogen source comprising ammonia or molecular nitrogen, and a carrier gas. (ii) application of a low frequency power to a first one of the at least two electrodes, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz, and (iv) a pressure within the plasma enhanced chemical vapor deposition reactor to be between about 0.5 and 5 Torr.
[0020] Aspects of this disclosure additionally pertain to systems for producing boron nitride, which systems may be characterized by a plasma enhanced chemical vapor deposition reactor and a controller. The plasma enhanced chemical vapor deposition reaction includes (a) at least two electrodes with one configured to produce high frequency RF energy for generating a plasma and another configured to produce low frequency RF energy’ for driving ions from the plasma to a surface of the substrate, and (b) a process gas inlet. The controller may be configured to cause concurrently: (i) delivery7of a process gas to the plasma enhanced chemical vapor deposition reactor via the process gas inlet, wherein the process gas comprises: a boron precursor, a nitrogen comprises ammonia or molecular nitrogen, and a carrier gas, (ii) application of a high frequency power to a first one of the at least two electrodes, wherein the high frequency power is at least about 400 W at a frequency of between about 13-60 MHz, (iii) application of a low frequency power to a second one of the at least two electrodes, wherein the low frequency pow er is at least about 400 W at a frequency of between about 400 kHz and 1MHz, and (iv) a pressure within the plasma enhanced chemical vapor deposition reactor to be between about 0.5 and 5 Torr.
[0021] In some embodiments, the controller of a system described herein may be additionally configured to cause application of a high frequency power to a second one of the at least two electrodes, wherein the high frequency power is at a frequency of between about 13-60 MHz. In some embodiments, the high frequency power is about 0.1 to 2000 W at a frequency of betweenAtorney Docket No. LAM1P135 WO- 12202-1 WO about 13-60 MHz. In some embodiments, the high frequency power is at least about 400 W at a frequency of about 13-60 MHz.
[0022] The first and second electrodes may have various structures, orientations, relative arrangements, and configurations. In some embodiments, the first and second electrodes are different from each other. In some embodiments, the second electrode comprises or is integrated in a substrate support.
[0023] The substrate may be made from any of various materials. In some embodiments, the substrate comprises a single crystal silicon wafer.
[0024] The boron nitride produced by the system may be used in any of many different structures, some of which form part of an electrical device. In some embodiments, the boron nitride forms at least part of an intermetal dielectric layer on the substrate. In some embodiments, the boron nitride forms at least part of a packaging structure. As an example, the packaging structure may comprise a bond film for bonding to a carrier substrate.
[0025] In some embodiments, the system can produce boron nitride having a dielectric constant ranging from about 4 to about 6. In some embodiments, the system can produce boron nitride exhibiting a leakage current of at most about 6.5 / 1 O'4A / cm2at an electric field of 4 MV / cm, or at most about 2.5 / I O'9A / cm2at the electric field of 2 MV / cm. In some embodiments, the system can produce boron nitride having a thermal conductivity of about 2 to about 25 W / m-K. In some embodiments, In some embodiments, the system can produce boron nitride having a grain size of about 3 to about 9.5 nm. In some embodiments, the system can produce boron nitride having an impurity level of about 0 to about 3 mol%. In some embodiments, In some embodiments, the system can produce boron nitride having a density of about 1.5 to about 2.3 g / cc.
[0026] In certain embodiments, the boron precursor employed by the system comprises diborane (B2H5), borazine, Ammonia Borane complex (AB), 1, 3, 5-Tri(methyl)borazine (TMBZ), B-tris(di ethylamino) borazine [N-dimethyl TMBZ], Tris(dimethylamino) borane (TDMAB), boron chloride (BCh), boron fluoride (BF3), or any combination thereof.
[0027] In certain embodiments, the process gas used in the system comprises the boron precursor in a concentration of about 0.01 mol% to 0.3 mol%, the nitrogen source in a concentration of about 50 mol% to 90 mol%, and the carrier gas in a concentration of about 9 mol% to about 50 mol%.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0028] In certain embodiments, the controller is configured to cause the high frequency power to be about 400 and 4,000 W at a frequency of between about 13-60 MHz. In certain embodiments, such as one where the HF power is about 400 and 4.000 W, the controller is configured to cause the low frequency power to be about 400 and 4,000 W at a frequency of between about 400 kHz and 1MHz. In certain embodiments, the controller is configured to cause the low frequency power to be about 2,000 to 5,000 W at a frequency of about 400 kHz to 1MHz.
[0029] In certain embodiments, the controller is configured to cause the pressure within the plasma enhanced chemical vapor deposition reactor to be about 0.5 to about 6.5 Torr. In certain embodiments, the controller is configured to cause a temperature within the plasma enhanced chemical vapor deposition reactor to be about 350°C to about 450°C.
[0030] In certain embodiments, the boron nitride produced by the system has an atomic ratio between boron and nitrogen of about 1:1.01 to about 1:1.25. In certain embodiments, the boron nitride has a compressive stress relative to the substrate of about -300 to about -3200 GPa.These and other features of the disclosure will be described in more detail below, sometimes with reference to figures.BRIEF DESCRIPTION OF THE DRAWINGS
[0031] FIG. 1 depicts thermal conductivity and band gap (Eg) for various metals, dielectric, and semiconductor materials.
[0032] FIG. 2 depicts a process station that may be used to carry out the disclosed method.
[0033] FIG. 3 depicts a multi-station apparatus that may be used to cany7out the disclosed method.
[0034] FIG. 4 depicts a multi-chamber processing tool that may be used to carry7out the disclosed methods.
[0035] FIG. 5 describes a normalized relationship between thermal conductivity and gran size for a hexagonal boron nitride (h-BN) layers according to some embodiments.
[0036] FIG. 6 depicts the variation of a grain size as a function of a low frequency (LF) RF power.DETAILED DESCRIPTIONContext and Overview
[0037] Films with high thermal conductivity and high electrical resistance are needed for heat management in modem devices, particularly logic devices in which many closely packed metalAtorney Docket No. LAM1P135 WO- 12202-1 WO lines simultaneously carry current. The thermal and electrical requirements become additionally stringent in the advanced devices as more heat is generated in a given volume. Much of the generated heat needs to be effectively and immediately dissipated to prevent device malfunction. Conventionally used dielectric materials such as silicon oxides and silicon nitrides have thermal conductivities that cannot adequately dissipate heat generated with advanced devices. Therefore, there is a need for new dielectric films that efficiently dissipate heat while maintaining good electrical insulation. Boron nitride is one possible material due to its high band gap (about 5.9 to 6.0 eV for hexagonal crystalline boron nitride (h-BN)) and high thermal conductivity. Unfortunately, it is very difficult to grow a good crystalline boron nitride at temperatures appropriate for device manufacturing, e.g., below about 400°C.
[0038] Disclosed are plasma enhanced chemical vapor deposition (PECVD) processes for depositing boron nitride at a temperature of at most about 400°C using, e.g.. two RF sources. In some implementations, the disclosed PECVD processes can grow near stoichiometric 1 :1 crystalline boron nitride films with high thermal conductivity and adequate leakage properties.
[0039] In some embodiments, boron nitride is deposited by exposing a process gas comprising a boron precursor, a nitrogen source such ammonia or molecular nitrogen, and a carrier gas to a plasma formed from a combination of (a) high frequency power of at least about 400 W at a frequency of between about 13-60 MHz and (b) a low frequency power of at least about 400 W at a frequency of between about 400 kHz and 1MHz. The boron nitride can have a substantially hexagonal crystal structure, a purity of at least about 97 mol%, a thermal conductivity of at least about 2 W / m-K, and a dielectric constant of at most about 6.Boron Nitride Film Properties
[0040] FIG. 1 shows thermal conductivity and band gap for various metal, dielectric, and semiconducting materials. For semiconductor devices such as those including an intermetal dielectric (IMD) or interlayer dielectric (ILD), where high thermal conduction with no electrical leakage is ideal, it is desirable to use a dielectric material having a high thermal conductivity and a high electrical resistance (e.g., low leakage current). It is known that the band gap of a material correlates to the electrical resistance of the material and that a high band gap corresponds to a high electrical resistance. As illustrated in FIG. 1, silicon oxide has a high band gap but its thermal conductivity is relatively low. In another example, graphite has a high thermal conductivity but offers no band gap. On the other hand, diamond, hexagonal boron nitride (h-BN), and aluminum nitride (AIN) (all presented in the right, upper portion of FIG. 1) have both a high thermal conductivity and a large band gap higher, notably in comparison to most metal, dielectric, andAtorney Docket No. LAM1P135 WO- 12202-1 WO semiconducting materials. Therefore, it is reasonable to assume that diamond, h-BN, and AIN may be suitable for applications that require high thermal conductivity and a low leakage current. The present disclosure focuses on h-BN deposited by a dual RF CVD process. Such material may serve as, e.g., a dielectric layer in a logic device having stacked conductors.
[0041] The stoichiometry of deposited h-BN is one of the characteristics that may correlate with the quality of a h-BN film in an electrical device. According to some embodiments, the atomic ratio between boron (B) and nitrogen (N) in a h-BN may range from about 1 : 1 to about 1 : 1.25 or from about 1:1.01 to about 1:1.08.
[0042] A deposited h-BN material may include a certain amount of one or more impurities such as carbon, oxygen, hydrogen, or any combination thereof. Impurities may be provided from a boron precursor, a nitrogen source, and / or a carrier gas. To form a good quality h-BN material, the amount of impurity may be limited to at most a defined amount. A h-BN material formed according to some embodiments may include an impurity having a concentration of about 0 to about 3 mol% or about 0.03 to about 3 mol%.
[0043] Depending on one or more process parameters, the crystal structure of a BN (boron nitride) layer may be determined. A h-BN layer, as disclosed herein, may include substantially a boron nitride in the hexagonal crystalline structure. In some embodiments, a h-BN layer may include at least about 95 mol% or at least about 97 mol% of the boron nitride in the hexagonal crystalline structure. The remaining portion of the BN may include boron nitride in another crystalline form, e.g., cubic form. In another embodiment, a BN layer, as disclosed herein, may include boron nitride substantially in the cubic crystalline structure. In some embodiments, a crystalline BN layer, as disclosed herein, may include a mixture of hexagonal and cubic crystalline structures. In some embodiments, the cubic cry stalline structure may comprise about 1 to 100 mol% of the BN layer. In some embodiments, the cubic crystalline structure may comprise about 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 100 mol% ofthe BN layer. In some embodiments, the hexagonal crystalline structure may comprise about 1 to 100 mol% of the BN layer. In some embodiments, the hexagonal crystalline structure may comprise about 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85. 90. 95 or 100 mol% ofthe BN layer.
[0044] The grain size of the h-BN layer may be controlled by one or more deposition parameters. The deposition parameters may include a deposition temperature, deposition pressure, type of precursor etc. In some embodiments, the average grain size of the deposited h-BN is about 3 and 10 nm or about 7.9 to 9.5 nm. In some embodiments, the grain size may vary with the value of low frequency (LF) power applied during deposition. During deposition, the h-BN may preferentiallyAtorney Docket No. LAM1P135 WO- 12202-1 WO grow in a defined direction. After or concurrent with nucleation, h-BN may grow and / or elongate in a direction substantially vertical to the substrate, which is referred to as c-axis direction, or in a direction substantially parallel to the substrate, which is referred to as a- axis. In some embodiments, h-BN may grow in random directions without any preferred growth direction.
[0045] The grain size and / or growth direction (e.g., elongating direction) may impact the thermal conductivity' of the h-BN. Generally, greater grain sizes of h-BN correlate with lower density of grain boundaries, and higher thermal conductivity. The direction of grain growth may be correlated with the direction of thermal conduction. The h-BN grains preferentially elongated in the c-axis direction have a higher thermal conductivity in the c-axis direction, thereby dissipating more thermal energy' in the c-axis direction compared to other directions. The h-BN grains grown in random orientation would have similar thermal conductivities in different directions. The grain size of a h-BN layer can be determined by using, for example. X-ray diffraction (XRD) or electron microscopy, e.g., scanning electron microscopy (SEM) or transmission electron microscopy (TEM)
[0046] In some embodiments, deposited h-BN material has a dielectric constant of at most about 6, our about 4 to about 6. The dielectric constant may be measured by any of various accepted techniques such as by using a mercury probe at a frequency of, e.g.. about 5 kHz and / or 100 kHz.
[0047] In some embodiments, values of the thermal conductivity of a h-BN layer are about 2 W / m-Kto about 25 W / m-K. The thermal conductivity may be measured by any of various accepted techniques such as by a Time Domain Thermoreflectance (TDTR) technique. The thermal conductivity of the h-BN may depend on and controlled by at least one of the grain orientations, grain size, purity, density, the amount of hexagonal cry stal structure in the h-BN, or a combination thereof. In some cases, the thermal conductivity of a h-BN increases as the average grain size in the h-BN also increases.
[0048] In some embodiments, the leakage current of a h-BN layer such as one formed according to the process described herein is at most about 6.5><10'4A / cm2at an electric field of 4 MV / cm, or at most about 2.5xl0‘9A / cm2at an electric field of 2 MV / cm. The leakage current of a h-BN layer may be determined by any of various accepted techniques such as using a mercury probe under application of an electric field of defined magnitude to the h-BN layer.
[0049] The density of a h-BN layer such as one formed according to the process described herein may be about 1.5 g / cc to about 2.3 g / cc or about 2.1 g / cc to about 2.3 g / cc. The density of a h-BN layer may be measured by any of various accepted techniques such as by X-ray reflectometry (XRR).Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0050] While this disclosure focuses on boron nitride having a hexagonal crystal form, the disclosed embodiments naturally extent to other forms of boron nitride such as those having other crystal structures (e.g., cubic or wurtzite) or mixed crystal structures.Process Conditions
[0051] A hexagonal boron nitride (h-BN) layer may be deposited on a substrate using plasma-enhanced chemical vapor deposition (PECVD), chemical vapor deposition (CVD), atomic layer deposition (ALD). plasma enhanced atomic layer deposition (PEALD). high-density plasma chemical vapor deposition (HDPCVD), an epitaxial growth process, or another process. In some embodiments, a high-quality7h-BN layer is deposited by using one or more boron precursors, a nitrogen precursor, and a carrier gas. As an example, such gases may be employed in a PECVD process. In depositing a high-quality h-BN layer using PECVD, two separate RF sources may be employed. Together, these sources may control plasma conditions appropriate for forming the h-BN layer. The sources may be controlled independently, so that different levels of power and frequency are applied, optionally simultaneously, during the PECVD process. In some embodiments, one source applies RF power at a high-frequency and the second source applies RF power at a lower-frequency. This dual-frequency approach is sometimes referred to as a dual RF CVD
[0052] In some embodiments, two RF sources, i.e., a high-frequency (e.g., 13.56-60 MHz) RF source and a low-frequency (e.g., 400 kHz-1 MHz) RF source are employed to produce a goodquality h-BN layer. A high-frequency (HF) power may be applied to a first electrode, e.g., coil or plate electrode, to generate and / or sustain a plasma from a source gas. The source gas may include an inert gas. In some embodiments, plasma may be generated in a portion of the process chamber that is opposite to (or above) the substrate. By modulating the HF power, the density of the plasma may be controlled, which varies the density7of the ions or reaction species that impinge on the substrate during deposition. In some embodiments, the plasma is a high-density7plasma (HDP). A low-frequency (LF) powder may be applied to a second electrode, which is different from the first electrode. In some embodiments, the second electrode may be near to or actually in a substrate holder (e.g., in susceptor on which a substrate is supported). The LF power may control a bombardment of ions or reaction species generated in the plasma to the substrate. In some cases, the kinetic energy of the ions or reaction species traveling to the substrate is controlled by the LF pow er. In some cases, high LF power is controlled to enhance the grow th of h-BN grains, resulting in elongated grain growth in a c-axis direction.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0053] The conditions described in the remainder of this “Process Conditions” section may be employed any combination, including combinations employing one or more sub-ranges identified below. In some embodiments, a combination of process conditions results in a deposition process that deposits h-BN at a rate of at least about 50 A / min, e.g., about 80 to 400A / min.
[0054] During a h-BN deposition process, a process gas is supplied to a process chamber. The process gas has a composition that may be appropriate for any of various types of deposition process such as PECVD. PEALD, or other deposition process. The process gas may include one or more boron precursors, one or more nitrogen source gases, and a carrier gas. One or more boron precursors according to this disclosure may include diborane (B2H6), borazine, Ammonia Borane complex (AB), 1, 3, 5-Tri(methyl)borazine (TMBZ), B-tris(dimethylamino) borazine [N-dimethyl TMBZ], Tris(dimethylamino) borane (TDMAB), boron chloride (BCh). and boron fluoride (BFs), or any combination thereof. For nitrogen sources, ammonia (NH3). molecular nitrogen (N2). or a mixture of N2 and H2 may be used for example. Nitrogen (N2) or argon (Ar) may be used as a carrier gas. In one example, the reaction of a process gas, including the starting precursor such as diborane (B2H6), nitrogen source, and carrier gas, to form a boron nitride may proceed as follows.B2H6 + N2 + H2 + He (inert) -> BN + N2 + NH3 + He (inert)
[0055] In some embodiments, a process gas for forming a h-BN layer may include a boron precursor in a concentration of about 0.01 mol% to about 0.3 mol% (e.g., 0.017 mol% to about 0.26 mol%), a nitrogen source in a concentration of about 50 mol% to about 90 mol% (e.g., about 54.2 mol% to about 88.8 mol%), and the carrier gas in a concentration of about 9 mol% to about 50 mol% (e.g., about 9.7 mol% to about 44.7 mol%). In some embodiments, the boron precursor may be delivered at a flow rate of about 0.5 to 300 seem. In some embodiments, the nitrogen source may be delivered at a flow rate of about 50 to 2500 seem.
[0056] In some embodiments, the process gas further includes one or more fluorine sources. The fluorine source may act as a hydrogen scavenger and / or a co-etchant of low-quality' boron nitride. In some embodiments, the fluorine source may include nitrogen trifluoride (NF3), molecular fluorine (F2), sulfur hexafluoride (SFe), or boron trifluoride (BF3), or any combination thereof. In some embodiments, the fluorine source may be delivered at a flow rate of about 0.25 to 75 seem.
[0057] As explained, in some embodiments, both high-frequency (HF) power and low-frequency (LF) power are applied during a deposition process to form a h-BN layer. In some embodiments, the HF source has a frequency between about 13 MHz and about 60 MHz, which may be applied to a coil or other electrode to generate and / or sustain plasma from a gas source. The gas source forAtorney Docket No. LAM1P135 WO- 12202-1 WO generating or maintaining a plasma may include an inert gas, e.g., nitrogen. The applied HF power may be about 0 to 2000 Watts at, e.g., 13.56 MHz, or about 400 to 1000 Watts at, e.g., 13.56 MHz, or about 1200 to 4000 Watts at, e.g., 13.56 MHz. The HF power may be applied in the process chamber such that it produces a plasma in a space that is opposite to or above the substrate. In some implementations, the HF power and process chamber are configured such that the plasma comes in direct contact with the substrate. Alternately, the plasma may be remotely generated in a region separate from the space where h-BN is deposited (e.g., the plasma is generated at a location remote from the substrate).
[0058] In a dual RF CVD process and associated apparatus as described herein, an LF power source is separate from the HF power source that is employed to generate plasma in the process chamber. The LF power source may be configured to control ion bombardments on the substrate. In some embodiments, the LF power is applied through a susceptor (e.g.. substrate holder) to a substrate supported on the susceptor. As an example, the LF pulse may have a frequency of about 400 kHz to about 1 MHz. In some implementations, the applied LF power is about 400 to about 1000 Watts at, e.g., 400 kHz, or about 1500 to about 3000 Watts at, e g., 400kHZ, or about 2,000 to 5,000 Watts at. e.g., 400 kHz.
[0059] In some embodiments, the pressure during deposition of a h-BN layer is about 0.5 Torr to about 6.5 Torr or about 0.5 Torr to about 5 Torr.
[0060] The substrate temperature during the deposition of a h-BN layer in the process chamber may be limited to about 450°C or less, or about 400°C or less, or about 350°C or less, or from about 300°C to about 450°C. The substrate temperature may be configured to be substantially the same as the chamber wall temperature. In some embodiments, the temperature is limited to a maximum value at which it is safe to produce electronic devices in a particular process chamber. For example, the materials of construction used in the process chamber (e.g., aluminum) may be damaged if the deposition process chamber temperature remains above the maximum value. Additionally or alternatively, a device (or devices) being fabricated on a substrate may be damaged if the deposition process chamber temperature remains above the maximum value.
[0061] The substrate on which a h-BN material is deposited, according to the disclosure, may include a semiconductor wafer (e.g., a single crystal silicon (Si) wafer or gallium arsenide wafer); a dielectric support such as a ceramic or glass of any composition (e.g., silica glass); a layer or layers on such support or wafer (e.g., a layer of poly crystalline silicon (doped or undoped), silicon oxide, nitrogen-doped silicon oxide, silicon nitride, aluminum axide, hafnium oxide, carbon, or any combination thereof); a metal; etc. In some cases, h-BN grain growth may vary depending onAtorney Docket No. LAM1P135 WO- 12202-1 WO the substrate composition or morphology, particularly of the material on which the h-BN material is directly deposited. On a silicon oxide or carbon surface, for example, a h-BN layer may be grown without forming a substantial interfacial layer between a h-BN and the underlying oxide or carbon. A h-BN material deposited on a silicon layer may, for example, employ an interfacial layer having a defined thickness on which the h-BN material is directly deposited.Applications
[0062] The h-BN layer described herein may be employed in various applications. Some such applications include those requiring a device such as an electronic device formed on, e.g., a semiconductor substrate. A h-BN layer may be well-suited for such applications because, as described herein, h-BN has superior electrical and thermal properties. Due to its large band gap, h-BN is a good electrical insulator exhibiting low leakage current. The h-BN material, according to some embodiments, may be formed by a dual RF PECVD, where the deposition rate is about 80 to 400A / min, which is faster than other processes, such as ALD. The high deposition rate is beneficial in high volume manufacturing (HVM) and is also suitable for forming devices having features with high aspect ratios.
[0063] Increasingly, logic devices demand dielectric materials having both strongly electrical insulating properties and superior thermal management, i.e., fast heat dissipation. Modem logic devices generate so much heat in a small volume that the dielectric material must quickly dissipate thermal energy accumulated within the device during operation. Replacing a conventional oxide or nitride insulating layer with a h-BN layer advantageously accelerates heat dissipation while keeping the metal lines insulated from each other.
[0064] A h-BN layer as described herein may be beneficial as an intermetal dielectric (IMD) to insulate the devices from the first metallization layer or to electrically isolates metal features on a single level packing. In modem devices of any type, the IMD may require a dielectric having high thermal conductivity as well as insulating properties. A boron nitride material as disclosed herein may amply fill this need.
[0065] Modem devices of any ty pe may also require highly insulating and thermally conductive interlayer dielectrics (ILDs). A h-BN material, as described herein, may be used in an ILD for electrically separating different layers including metalization layers and other structural layers in a device.
[0066] A h-BN may be employed in packaging and bonding applications. In modem device packages, thermal management is becoming more important. Further, some bonding processesAtorney Docket No. LAM1P135 WO- 12202-1 WO such as bonding a die having a plurality of devices to a carrier wafer for thinning or die bonding, require very good heat dissipation. A h-BN insulating material may allow effective bonding operations.
[0067] More generally, a h-BN layer may be employed to replace any dielectric layer currently employed in a device such as a logic or memory device. Materials currently in use for dielectric layers, e.g., silicon oxide and silicon nitride, have relatively poor thermal conductivity7, unsuitable for advanced device designs. In addition to its higher thermal conductivity. h-BN has a dielectric constant comparable to or higher than that of silicon oxide or silicon nitride, and therefore may be suitable as a replacement for any device application.Apparatus
[0068] FIG. 2 schematically shows an embodiment of a process station 200 that may be used to deposit h-BN material using chemical vapor deposition (CVD) or atomic layer deposition (ALD), either of which may be plasma enhanced. For simplicity, the process station 200 is depicted as a standalone process station having a process chamber body 202 for maintaining a low-pressure environment. However, it will be appreciated that a plurality of process stations 200 may be included in a common process tool environment. Further, it will be appreciated that, in some embodiments, one or more operating parameters of process station 200, including those discussed in detail below, may be adjusted programmatically by one or more computer controllers.
[0069] Process station 200 is configured to receive boron precursors and / or other process gas components by any suitable mechanism from any suitable source. For example, in the depicted embodiment, process station 200 is fluidly communicates with reactant delivery7system 201 for delivering process gases to a distribution showerhead 206. The process gases may include one or more boron precursors, one or more nitrogen source gases, and a carrier gas. Reactant delivery system 201 includes a mixing vessel 204 for blending and / or conditioning process gases for delivery' to showerhead 206. One or more mixing vessel inlet valves 220 may control the introduction of process gases to mixing vessel 204. Similarly, a showerhead inlet valve 205 may control the introduction of process gasses to the showerhead 206.
[0070] Some reactants, such as certain boron precursors, may be stored in liquid or solid form prior to vaporization at and subsequent delivery to the process station. For example, the embodiment of FIG. 2 includes a vaporization point 203 for vaporizing liquid reactant to be supplied to mixing vessel 204. In some embodiments, vaporization point 203 may be a heated vaporizer. The reactant vapor produced from such vaporizers may condense in downstreamAtorney Docket No. LAM1P135 WO- 12202-1 WO delivery piping. Exposure of incompatible gases to the condensed reactant may create small particles. These small particles may clog piping, impede valve operation, contaminate substrates, etc. Some approaches to addressing these issues involve sweeping and / or evacuating the delivery piping to remove residual reactant. However, sweeping the delivery piping may increase process station cycle time, degrading process station throughput. Thus, in some embodiments, delivery piping downstream of vaporization point 203 may be heat traced. In some examples, mixing vessel 204 may also be heat traced. In one non-limiting example, piping downstream of vaporization point 203 has an increasing temperature profile extending from approximately 100°C to approximately 150°C at mixing vessel 204.
[0071] In some embodiments, reactant liquid may be vaporized at a liquid injector. For example, a liquid injector may inject pulses of a liquid reactant into a carrier gas stream upstream of the mixing vessel. In one scenario, a liquid injector may vaporize reactant by flashing the liquid from a higher pressure to a lower pressure. In another scenario, a liquid injector may atomize the liquid into dispersed microdroplets that are subsequently vaporized in a heated delivery pipe. It will be appreciated that smaller droplets may vaporize faster than larger droplets, reducing a delay between liquid injection and complete vaporization. Faster vaporization may reduce a length of piping downstream from vaporization point 203. In one scenario, a liquid injector may be mounted directly to mixing vessel 204. In another scenario, a liquid injector may be mounted directly to showerhead 206.
[0072] In some embodiments, a liquid flow controller upstream of vaporization point 203 may be provided for controlling a mass flow of liquid for vaporization and delivery' to process station 200. For example, the liquid flow controller (LFC) may include a thermal mass flow meter (MFM) located downstream of the LFC. A plunger valve of the LFC may then be adjusted to be responsive to feedback control signals provided by a proportional-integral-derivative (PID) controller in electrical communication with the MFM. However, it may take one second or more to stabilize liquid flow using feedback control. This may extend a time for dosing a liquid reactant. Thus, in some embodiments, the LFC may be dynamically switched between a feedback control mode and a direct control mode. In some embodiments, the LFC may be dynamically switched from a feedback control mode to a direct control mode by disabling a sense tube of the LFC and the PID controller.
[0073] Showerhead 206 distributes process gases toward substrate 212. In the embodiment shown in FIG. 2, substrate 212 is located beneath showerhead 206, and is shown resting on a pedestal 208. It will be appreciated that showerhead 206 may have any suitable shape, and mayAtorney Docket No. LAM1P135 WO- 12202-1 WO have any suitable number and arrangement of ports for distributing processes gases to substrate 212.
[0074] In some embodiments, a microvolume 207 for confining the deposition reaction is defined beneath showerhead 206. Performing an ALD and / or CVD process in a microvolume rather than in the entire interior volume of a process station may reduce reactant exposure and sweep times, may reduce times for altering process conditions (e.g., pressure, temperature, etc.), may limit an exposure of process station robotics to process gases, etc. Example microvolume sizes include, but are not limited to, volumes between 0.1 liter and 2 liters. This microvolume also impacts productivity throughput. While deposition rate at the substrate may drop, the overall cycle time actually reduces. In certain cases, the effect of the latter is dramatic enough to improve overall throughput of the module for a given target thickness of film.
[0075] In some embodiments, pedestal 208 may be raised or lowered to expose substrate 212 to microvolume 207 and / or to vary a volume of microvolume 207. For example, in a substrate transfer phase, pedestal 208 may be lowered to allow substrate 212 to be loaded onto pedestal 208. During a deposition process phase, pedestal 208 may be raised to position substrate 212 within microvolume 207. In some embodiments, microvolume 207 may completely enclose substrate 212 as well as a portion of pedestal 208 to create a region of high flow impedance during a deposition process.
[0076] Optionally, pedestal 208 may be lowered and / or raised during portions the deposition process to modulate process pressure, reactant concentration, etc., within microvolume 207. In one scenario where process chamber body 202 remains at a base pressure during the deposition process, lowering pedestal 208 may allow microvolume 207 to be evacuated. Example ratios of microvolume to process chamber volume include, but are not limited to, volume ratios between 1 :200 and 1 : 10. It will be appreciated that, in some embodiments, pedestal height may be adjusted programmatically by a suitable computer controller.
[0077] In another scenario, adjusting a height of pedestal 208 may allow a plasma density to be varied during plasma activation and / or treatment cycles included in the deposition process. At the conclusion of the deposition process phase, pedestal 208 may be lowered during another substrate transfer phase to allow removal of substrate 212 from pedestal 208.
[0078] While the example microvolume variations described herein refer to a height-adjustable pedestal, it will be appreciated that, in some embodiments, a position of showerhead 206 may be adjusted relative to pedestal 208 to vary a volume of microvolume 207. Further, it will beAtorney Docket No. LAM1P135 WO- 12202-1 WO appreciated that a vertical position of pedestal 208 and / or showerhead 206 may be varied by any suitable mechanism within the scope of the present disclosure. In some embodiments, pedestal 208 may include a rotational axis for rotating an orientation of substrate 212. It will be appreciated that, in some embodiments, one or more of these example adjustments may be performed programmatically by one or more suitable computer controllers.
[0079] Returning to the embodiment shown in FIG. 2, showerhead 206 and pedestal 208 electrically communicate with RF power supply 214 and matching network 216 for powering a plasma. In some embodiments, the plasma energy may be controlled by controlling one or more of a process station pressure, a gas concentration, an RF source power, an RF source frequency, and a plasma power pulse timing. For example, RF power supply 214 and matching network 216 may be operated at any suitable power to form a plasma having a desired composition of radical species. Examples of suitable powers are included above. Likewise, RF power supply 214 may provide RF power of any suitable frequency. In some embodiments, as indicated above, RF power supply 214 may be configured to control high- and low-frequency RF power sources independently of one another. Example low-frequency RF frequencies may include, but are not limited to, frequencies of about 50 kHz to 1 MHz; e.g., about 50 kHz to 200 kHz, or about 400 kHz to 1 MHz. Example high-frequency RF frequencies may include, but are not limited to, frequencies of about 1.8 MHz to 2.45 GHz or about 13 MHz to 60 MHz. It will be appreciated that any suitable parameters may be modulated discretely or continuously to provide plasma energy for the surface reactions. In one non-limiting example, the plasma power may be intermittently pulsed to reduce ion bombardment with the substrate surface relative to continuously powered plasmas.
[0080] In some embodiments, the plasma may be monitored in-situ by one or more plasma monitors. In one scenario, plasma power may be monitored by one or more voltage, current sensors (e.g., VI probes). In another scenario, plasma density and / or process gas concentration may be measured by one or more optical emission spectroscopy sensors (OES). In some embodiments, one or more plasma parameters may be programmatically adjusted based on measurements from such in-situ plasma monitors. For example, an OES sensor may be used in a feedback loop for providing programmatic control of plasma power. It will be appreciated that, in some embodiments, other monitors may be used to monitor the plasma and other process characteristics. Such monitors may include, but are not limited to, infrared (IR) monitors, acoustic monitors, and pressure transducers.
[0081] In some embodiments, the plasma may be controlled via input / output control (IOC) sequencing instructions. In one example, the instructions for setting plasma conditions for a plasmaAtorney Docket No. LAM1P135 WO- 12202-1 WO process phase may be included in a corresponding plasma activation recipe phase of a deposition process recipe. In some cases, process recipe phases may be sequentially arranged, so that all instructions for a deposition process phase are executed concurrently with that process phase. In some embodiments, instructions for setting one or more plasma parameters may be included in a recipe phase preceding a plasma process phase. For example, a first recipe phase may include instructions for setting a flow rate of an inert and / or a reactant gas, instructions for setting a plasma generator to a power set point, and time delay instructions for the first recipe phase. A second, subsequent recipe phase may include instructions for enabling the plasma generator and time delay instructions for the second recipe phase. A third recipe phase may include instructions for disabling the plasma generator and time delay instructions for the third recipe phase. It will be appreciated that these recipe phases may be further subdivided and / or iterated in any suitable way within the scope of the present disclosure.
[0082] In some deposition processes, plasma strikes last on the order of a few seconds or more in duration. In certain implementations, much shorter plasma strikes may be used. These may be on the order of 10 ms to 1 second, typically, about 20 to 80 ms. with 50 ms being a specific example. Such very short RF plasma strikes require extremely quick stabilization of the plasma. To accomplish this, the plasma generator may be configured such that the impedance match is set preset to a particular voltage, while the frequency is allowed to float. Conventionally, high-frequency plasmas are generated at an RF frequency at about 13.56 MHz or between about 13 MHz and about 60 MHz. In various embodiments disclosed herein, the frequency is allowed to float to a value that is different from this standard value. By permitting the frequency to float while fixing the impedance match to a predetermined voltage, the plasma can stabilize much more quickly, a result which may be important when using the very short plasma strikes associated with some types of deposition cycles.
[0083] In some embodiments, pedestal 208 may be temperature controlled via heater 210. Further, in some embodiments, pressure control for deposition process station 200 may be provided by butterfly valve 218. As shown in the embodiment of FIG. 2, butterfly valve 218 throttles a vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, pressure control of process station 200 may also be adjusted by varying a flow rate of one or more gases introduced to process station 200.
[0084] FIG. 3 shows a schematic view of an embodiment of a multi-station processing tool 300 with an inbound load lock 302 and an outbound load lock 304, either or both of which may comprise a remote plasma source. A robot 306, at atmospheric pressure, is configured to moveAtorney Docket No. LAM1P135 WO- 12202-1 WO wafers from a cassette loaded through a pod 308 into inbound load lock 302 via an atmospheric port 310. A wafer is placed by the robot 306 on a pedestal 312 in the inbound load lock 302, the atmospheric port 310 is closed, and the load lock is pumped down. Where the inbound load lock 302 comprises a remote plasma source, the wafer may be exposed to a remote plasma treatment in the load lock prior to being introduced into a processing chamber 314. Further, the wafer also may be heated in the inbound load lock 302 as well, for example, to remove moisture and adsorbed gases. Next, a chamber transport port 316 to processing chamber 314 is opened, and another robot (not shown) places the wafer into the reactor on a pedestal of a first station shown in the reactor for processing. While the embodiment depicted in FIG. 3 includes load locks, it will be appreciated that, in some embodiments, direct entry of a wafer into a process station may be provided.
[0085] The depicted processing chamber 314 comprises four process stations, numbered from 1 to 4 in the embodiment shown in FIG. 3. Each station has a heated pedestal (shown at 318 for station 1), and gas line inlets. It will be appreciated that in some embodiments, each process station may have different or multiple purposes. While the depicted processing chamber 314 comprises four stations, it will be understood that a processing chamber according to the present disclosure may have any suitable number of stations. For example, in some embodiments, a processing chamber may have five or more stations, while in other embodiments a processing chamber may have three or fewer stations.
[0086] FIG. 3 also depicts an embodiment of a wafer handling system 390 for transferring wafers within processing chamber 314. In some embodiments, wafer handling system 390 may transfer wafers betw een various process stations and / or betw een a process station and a load lock. It will be appreciated that any suitable wafer handling system may be employed. Non-limiting examples include wafer carousels and wafer handling robots. FIG. 3 also depicts an embodiment of a system controller 350 employed to control process conditions and hardware states of process tool 300. System controller 350 may include one or more memory devices 356, one or more mass storage devices 354, and one or more processors 352. Processor 352 may include a CPU or computer, analog and / or digital input / output connections, stepper motor controller boards, etc.
[0087] In some embodiments, system controller 350 controls all of the activities of process tool 300. System controller 350 executes system control software 358 stored in mass storage device 354, loaded into memory device 356. and executed on processor 352. System control software 358 may include instructions for controlling the timing, mixture of gases, chamber and / or station pressure, chamber and / or station temperature, purge conditions and timing, wafer temperature, RF pow er levels, RF frequencies, substrate, pedestal, chuck and / or susceptor position, and otherAtorney Docket No. LAM1P135 WO- 12202-1 WO parameters of a particular process performed by process tool 300. System control software 358 may be configured in any suitable way. For example, various process tool component subroutines or control objects may be written to control operation of the process tool components necessary to carry out various process tool processes in accordance with the disclosed methods. System control software 358 may be coded in any suitable computer readable programming language.
[0088] In some embodiments, system control software 358 may include input / output control (IOC) sequencing instructions for controlling the various parameters described above. For example, each phase of a PEALD / PECVD process may include one or more instructions for execution by system controller 350. The instructions for setting process conditions for a PEALD / PECVD process phase may be included in a corresponding PEALD recipe phase. In some embodiments, the PEALD / PECVD recipe phases may be sequentially arranged, so that all instructions for a PEALD / PECVD process phase are executed concurrently with that process phase.
[0089] Other computer software and / or programs stored on mass storage device 354 and / or memory device 356 associated with system controller 350 may be employed in some embodiments. Examples of programs or sections of programs for this purpose include a substrate positioning program, a process gas control program, a pressure control program, a heater control program, and a plasma control program.
[0090] A substrate positioning program may include program code for process tool components that are used to load the substrate onto pedestal 318 and to control the spacing between the substrate and other parts of process tool 300.
[0091] A process gas control program may include code for controlling gas composition and flow rates and optionally for flowing gas into one or more process stations prior to deposition in order to stabilize the pressure in the process station. The process gas control program may include code for controlling gas composition and flow rates within any of the disclosed ranges. A pressure control program may include code for controlling the pressure in the process station by regulating, for example, a throttle valve in the exhaust system of the process station, a gas flow into the process station, etc. The pressure control program may include code for maintaining the pressure in the process station within any of the disclosed pressure ranges.
[0092] A heater control program may include code for controlling the current to a heating unit that is used to heat the substrate. Alternatively, the heater control program may control delivery of a heat transfer gas (such as helium) to the substrate. The heater control program may includeAtorney Docket No. LAM1P135 WO- 12202-1 WO instructions to maintain the temperature of the substrate within any of the disclosed ranges.
[0093] A plasma control program may include code for setting RF power levels and frequencies applied to the process electrodes in one or more process stations, for example using any of the RF power levels disclosed herein. The plasma control program may also include code for controlling the duration of each plasma exposure.
[0094] In some embodiments, there may be a user interface associated with system controller 350. The user interface may include a display screen, graphical software displays of the apparatus and / or process conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc.
[0095] In some embodiments, parameters adjusted by system controller 350 may relate to process conditions. Non-limiting examples include process gas composition and flow rates, temperature, pressure, plasma conditions (such as RF power levels, frequency, and exposure time), etc. These parameters may be provided to the user in the form of a recipe, which may be entered utilizing the user interface.
[0096] Signals for monitoring the process may be provided by analog and / or digital input connections of system controller 350 from various process tool sensors. The signals for controlling the process may be output on the analog and digital output connections of process tool 300. Nonlimiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (such as manometers), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain process conditions.
[0097] Any suitable chamber may be used to implement the disclosed embodiments. Example deposition apparatuses include, but are not limited to, apparatus from the ALTUS® product family, the VECTOR® product family, and / or the SPEED® product family, each available from Lam Research Corp., of Fremont, California, or any of a variety of other commercially available processing systems. Two or more of the stations may perform the same functions. Similarly, two or more stations may perform different functions. Each station can be designed / configured to perform a particular function / method as desired.
[0098] FIG. 4 is a block diagram of a processing system suitable for conducting thin film deposition processes in accordance with certain embodiments. A system 400 includes a transfer module 403. The transfer module 403 provides a clean, pressurized environment to minimize risk of contamination of substrates being processed as they are moved between various reactorAtorney Docket No. LAM1P135 WO- 12202-1 WO modules. Mounted on the transfer module 403 are two multi-station reactors 409 and 410, each capable of performing atomic layer deposition (ALD) and / or chemical vapor deposition (CVD) according to certain embodiments. Reactors 409 and 410 may include multiple stations 411, 413, 415, and 417 that may sequentially or non-sequentially perform operations in accordance with disclosed embodiments. The stations may include a heated pedestal or substrate support, one or more gas inlets or showerhead or dispersion plate.
[0099] Also mounted on the transfer module 403 may be one or more single or multi-station modules 407 capable of performing plasma or chemical (non-plasma) pre-cleans, or any other processes described in relation to the disclosed methods. The module 407 may in some cases be used for various treatments to, for example, prepare a substrate for a deposition process. The module 407 may also be designed / configured to perform various other processes such as etching or polishing. The system 400 also includes one or more wafer source modules 401, where wafers are stored before and after processing. An atmospheric robot (not shown) in the atmospheric transfer chamber 419 may first remove wafers from the source modules 401 to loadlocks 421. A wafer transfer device (generally a robot arm unit) in the transfer module 403 moves the wafers from loadlocks 421 to and among the modules mounted on the transfer module 403.
[0100] In various embodiments, a system controller 429 is employed to control process conditions during deposition. The controller 429 will typically include one or more memory devices and one or more processors. A processor may include a CPU or computer, analog and / or digital input / output connections, stepper motor controller boards, etc.
[0101] The controller 429 may control all of the activities of the deposition apparatus. The system controller 429 executes system control software, including sets of instructions for controlling the timing, mixture of gases, chamber pressure, chamber temperature, wafer temperature, radio frequency (RF) power levels, wafer chuck or pedestal position, and other parameters of a particular process. Other computer programs stored on memory devices associated with the controller 429 may be employed in some embodiments.
[0102] Typically there will be a user interface associated with the controller 429. The user interface may include a display screen, graphical software displays of the apparatus and / or process conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc.
[0103] System control logic may be configured in any suitable way. In general, the logic can be designed or configured in hardware and / or software. The instructions for controlling the driveAtorney Docket No. LAM1P135 WO- 12202-1 WO circuitry may be hard coded or provided as software. The instructions may be provided by “programming.” Such programming is understood to include logic of any form, including hard coded logic in digital signal processors, application-specific integrated circuits, and other devices which have specific algorithms implemented as hardware. Programming is also understood to include software or firmware instructions that may be executed on a general purpose processor. System control software may be coded in any suitable computer readable programming language.
[0104] The computer program code for controlling the germamum-containing reducing agent pulses, hydrogen flow, and tungsten-containing precursor pulses, and other processes in a process sequence can be written in any conventional computer readable programming language: for example, assembly language, C, C++, Pascal, Fortran, or others. Compiled object code or script is executed by the processor to perform the tasks identified in the program. Also as indicated, the program code may be hard coded.
[0105] The controller parameters relate to process conditions, such as, for example, process gas composition and flow rates, temperature, pressure, cooling gas pressure, substrate temperature, and chamber wall temperature. These parameters are provided to the user in the form of a recipe, and may be entered utilizing the user interface. Signals for monitoring the process may be provided by analog and / or digital input connections of the system controller 429. The signals for controlling the process are output on the analog and digital output connections of the deposition system 400.
[0106] The system software may be designed or configured in many different ways. For example, various chamber component subroutines or control objects may be written to control operation of the chamber components necessary to carry out the deposition processes (and other processes, in some cases) in accordance with the disclosed embodiments. Examples of programs or sections of programs for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.
[0107] In some implementations, controller 429 is part of a system, which may be part of the above-described examples. Such systems can include semiconductor processing equipment, including a processing tool or tools, chamber or chambers, a platform or platforms for processing, and / or specific processing components (a wafer pedestal, a gas flow7system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after processing of a semiconductor wafer or substrate. The electronics may be referred to as the “controller,” which may control various components or subparts of the system or systems. Controller 429, depending on the processing requirements and / or the type of system, may be programmed to control any of the processes disclosed herein, including the delivery of processingAtorney Docket No. LAM1P135 WO- 12202-1 WO gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings in some systems, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, positional and operation settings, wafer transfers into and out of a tool and other transfer tools and / or load locks connected to or interfaced with a specific system.
[0108] Broadly speaking, the controller may be defined as electronics having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operation, enable cleaning operations, enable endpoint measurements, and the like. The integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors, or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions communicated to the controller in the form of various individual settings (or program files), defining operational parameters for carrying out a particular process on or for a semiconductor wafer or to a system. The operational parameters may, in some embodiments, be part of a recipe defined by process engineers to accomplish one or more processing steps during the fabrication of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.
[0109] The controller, in some implementations, may be a part of or coupled to a computer that is integrated with, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the controller may be in the “cloud” or all or a part of a fab host computer system, which can allow for remote access of the wafer processing. The computer may enable remote access to the system to monitor current progress of fabrication operations, examine a history of past fabrication operations, examine trends or performance metrics from a plurality of fabrication operations, to change parameters of current processing, to set processing steps to follow a current processing, or to start a new process. In some examples, a remote computer (e.g. a server) can provide process recipes to a system over a network, which may include a local network or the Internet. The remote computer may include a user interface that enables entry or programming of parameters and / or settings, which are then communicated to the system from the remote computer. In some examples, the controller receives instructions in the form of data, which specify parameters for each of the processing steps to be performed during one or more operations. It should be understood that the parameters may be specific to the type of process to be performed and the ty pe of tool that the controller is configured to interface with or control. Thus as described above, the controller may be distributed, such as by comprising one or more discrete controllers that are networked together and working towards a common purpose, such as the processes andAtorney Docket No. LAM1P135 WO- 12202-1 WO controls described herein. An example of a distributed controller for such purposes would be one or more integrated circuits on a chamber in communication with one or more integrated circuits located remotely (such as at the platform level or as part of a remote computer) that combine to control a process on the chamber.
[0110] Without limitation, example systems may include a plasma etch chamber or module, a deposition chamber or module, a spin-rinse chamber or module, a metal plating chamber or module, a clean chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an atomic layer deposition (ALD) chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, and any other semiconductor processing systems that may be associated or used in the fabrication and / or manufacturing of semiconductor wafers.
[0111] As noted above, depending on the process step or steps to be performed by the tool, the controller might communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout a factory, a main computer, another controller, or tools used in material transport that bring containers of wafers to and from tool locations and / or load ports in a semiconductor manufacturing factory.ExperimentalExperiment 1
[0112] FIG. 5 presents a normalized relationship between thermal conductivity and grain size for a h-BN layer formed according to some embodiments. The thermal conductivity of the h-BN layer shows a proportional relationship with respect to the grain size. Without wishing to be bound by any particular theory, the larger the grain size, the less the grain boundary' density in the h-BN. The diffusion of phonons through the larger grains (i.e., smaller grain boundary’ density) in the h-BN grains may be less hindered compared to the smaller grains having more grain boundaries (i.e., high grain boundary density); thereby, higher thermal conductivity may7be achieved for the h-BN layer having larger grains.Experiment 2
[0113] FIG. 6 shows the variation of the grain sizes of h-BN layers with respect to low-frequency (LF) RF deposition power for the h-BN layers deposited under different deposition conditions (i.e., process regimes). The horizontal axis of FIG. 6 represents the LF RF power applied to the substrate susceptor during the depositions. The vertical axis represents the average grain size of the h-BNAtorney Docket No. LAM1P135 WO- 12202-1 WO layers formed according to the different process regimes. Both the LF RF power in the x-axis and the grain size in the y-axis are normalized. FIG. 6 includes four separate data sets, including the black square set, black circle set, blank square set, and blank circle set, each set representing the grain sizes of h-BN layers deposited at the same processing conditions while varying the LF RF power. For each data set, the gran size initially increases as the LF RF power increases up to a certain point, where the maximum grain size was obtained. Then, further increasing the LF RF power decreases the grain size. The initial increase in the grain size in each data set may be attributed to the increased ion bombardments to the substrate, which facilitates efficient cross linking andgrain growth. During deposition, a h-BN layer may grow in a certain direction. For example, during deposition, the grain may be elongated in the c-axis direction. Further increasing the LF RF power above the level where the maximum grain size was observed resulted in the decreased grain size. Without wishing to be bound by any particular theory, this decrease may have been caused by too much ion bombardment on the h-BN formed on the substrate leading to grain growth disruption. Above a certain threshold, the energy' of the ions bombarding the h-BN may be high enough to sputter the h-BN already formed into smaller sizes.Clauses / Embodiments
[0114] In some aspects, the techniques described herein relate to a method of depositing boron nitride on a substrate, the method including: (a) receiving the substrate in a plasma reactor; (b) delivering a process gas to the plasma reactor, wherein the process gas includes: a boron precursor, a nitrogen source including ammonia or molecular nitrogen, and a carrier gas; and (c) applying a low frequency power to a first electrode, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz, wherein the boron nitride has a thermal conductivity7of at least about 2 W / m-K.
[0115] In some aspects, the techniques described herein relate to a method, further including applying a high frequency power to a second electrode in the plasma reactor, wherein the high frequency power is at a frequency of about 13-60 MHz.
[0116] In some aspects, the techniques described herein relate to a method, wherein the high frequency power is about 0.1 to 2000 W at a frequency of about 13-60 MHz.
[0117] In some aspects, the techniques described herein relate to a method, wherein the low frequency power is about 2,000 to 5,000 W at a frequency of about 400 kHz and 1MHz.
[0118] In some aspects, the techniques described herein relate to a method, wherein the first and second electrodes are different.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0119] In some aspects, the techniques described herein relate to a method, wherein the second electrode includes or is incorporated in a substrate support.
[0120] In some aspects, the techniques described herein relate to a method, wherein the substrate includes a single crystal silicon wafer.
[0121] In some aspects, the techniques described herein relate to a method, wherein the boron nitride forms at least part of an intermetal dielectric layer on the substrate.
[0122] In some aspects, the techniques described herein relate to a method, wherein the boron nitride forms at least part of a packaging structure.
[0123] In some aspects, the techniques described herein relate to a method, wherein the packaging structure includes a bond film for bonding to a carrier substrate.
[0124] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a dielectric constant of at most about 6.
[0125] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a leakage current of at most about 6.5 xlO’4A / cm2 at an electric field of 4 MV / cm. or at most about 2.5x 10'9A / cm2 at the electric field of 2 MV / cm.
[0126] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a thermal conductivity' of about 2 to about 25 W / m-K.
[0127] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a grain size of about 3 to about 9.5 nm.
[0128] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has an impurity of about 0 to about 3 mol%.
[0129] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a density of about 1.5 to about 2.3 g / cc.
[0130] In some aspects, the techniques described herein relate to a method, wherein the boron precursor includes diborane (EhHe). borazine, Ammonia Borane complex (AB). 1, 3, 5-Tri(methyl)borazine (TMBZ), B-tris(dimethylamino) borazine [N-dimethyl TMBZ], Tris(dimethylamino) borane (TDMAB), boron chloride (BCh), and boron fluoride (BFs), or any combination thereof.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0131] In some aspects, the techniques described herein relate to a method, wherein the process gas includes the boron precursor in a concentration of about 0.01 mol% to 0.3 mol%, the nitrogen source in a concentration of about 50 mol% to 90 mol%, and the carrier gas in a concentration of about 9 mol% to about 50 mol%.
[0132] In some aspects, the techniques described herein relate to a method, wherein the process gas further includes a fluorine source.
[0133] In some aspects, the techniques described herein relate to a method, wherein the process gas further includes a fluorine source including nitrogen trifluoride (NFs), molecular fluorine (F2), sulfur hexafluoride (SFe), or boron trifluoride (BF3), or any combination thereof.
[0134] In some aspects, the techniques described herein relate to a method, wherein the high frequency power is about 400 to 4.000 W at a frequency of between about 13-60 MHz.
[0135] In some aspects, the techniques described herein relate to a method, wherein the low frequency pow er is about 400 to 4,000 W at a frequency of between about 400 kHz and 1MHz.
[0136] In some aspects, the techniques described herein relate to a method, wherein operations (b)-(c) are performed at a pressure of about 0.5 to about 6.5 Torr.
[0137] In some aspects, the techniques described herein relate to a method, wherein operations (b)-(c) are performed at a temperature of about 350°C to about 450°C.
[0138] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has an atomic ratio between boron and nitrogen of about 1:1.01 to about 1:1.25.
[0139] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a compressive stress relative to the substrate of about -300 to about -3200 GPa.
[0140] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a substantially hexagonal crystal structure.
[0141] In some aspects, the techniques described herein relate to a method, wherein the boron nitride has a substantially cubic crystal structure.
[0142] In some aspects, the techniques described herein relate to a method, wherein the boron nitride includes a mixture of hexagonal and cubic crystal structures.
[0143] In some aspects, the techniques described herein relate to a method, the boron nitride has a purity of at least about 97 mol% and a dielectric constant of about 4 to about 6.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0144] In some aspects, the techniques described herein relate to a system configured to produce boron nitride, the system including: a plasma enhanced chemical vapor deposition reactor including (a) at least two electrodes configured to produce high frequency RF energy’ for generating a plasma and low frequency RF energy for driving ions from the plasma to a surface of a substrate, and (b) a process gas inlet; and a controller configured to cause concurrently: delivery of a process gas to the plasma enhanced chemical vapor deposition reactor via the process gas inlet, wherein the process gas includes: a boron precursor, a nitrogen source including ammonia or molecular nitrogen, and a carrier gas, application of a low frequency power to a first one of the at least two electrodes, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz, and a pressure within the plasma enhanced chemical vapor deposition reactor to be between about 0.5 and 10 Torr.
[0145] In some aspects, the techniques described herein relate to a system, wherein the controller is additionally configured to cause application of a high frequency power to a second one of the at least two electrodes, wherein the high frequency power is at a frequency of about 13-60 MHz.
[0146] In some aspects, the techniques described herein relate to a system, wherein the high frequency power is about 0.1 to 2000 W at a frequency of about 13-60 MHz.
[0147] In some aspects, the techniques described herein relate to a system, wherein the low frequency power is about 2,000 to 5,000 W at a frequency of about 400 kHz to 1MHz.
[0148] In some aspects, the techniques described herein relate to a system, wherein the first and second electrodes are different from each other.
[0149] In some aspects, the techniques described herein relate to a system, wherein the second electrode includes or is integrated in a substrate support.
[0150] In some aspects, the techniques described herein relate to a system, wherein the substrate includes a single crystal silicon wafer.
[0151] In some aspects, the techniques described herein relate to a system, wherein the boron nitride forms at least part of an intermetal dielectric layer on the substrate.
[0152] In some aspects, the techniques described herein relate to a system, wherein the boron nitride forms at least part of a packaging structure.
[0153] In some aspects, the techniques described herein relate to a system, wherein the packaging structure includes a bond film for bonding to a carrier substrate.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0154] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has a dielectric constant of at most about 6.
[0155] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has a leakage current of at most about 6.5x1 O'4A / cm2 at an electric field of 4 MV / cm, or at most about 2.1 x 10'4A / cm2 at the electric field of 2 MV / cm.
[0156] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has a thermal conductivity of about 2 to about 25 W / m-K.
[0157] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has a grain size of about 3 to about 9.5 nm.
[0158] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has an impurity of about 0 to about 3 mol%.
[0159] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has a density of about 1.5 to about 2.3 g / cc.
[0160] In some aspects, the techniques described herein relate to a system, wherein the boron precursor includes diborane (BeHs), borazine, Ammonia Borane complex (AB), 1, 3, 5-Tri(methyl)borazine (TMBZ), B-tris(dimethylamino) borazine [N-dimethyl TMBZ], Tris(dimethylamino) borane (TDMAB), boron chloride (BCh), and boron fluoride (BF3), or any combination thereof.
[0161] In some aspects, the techniques described herein relate to a system, wherein the process gas includes the boron precursor in a concentration of about 0.01 mol% to 0.3 mol%, the nitrogen source in a concentration of about 50 mol% to 90 mol%, and the carrier gas in a concentration of about 9 mol% to about 50 mol%.
[0162] In some aspects, the techniques described herein relate to a system, wherein the high frequency power is about 400 to about 4,000 W at a frequency of between about 13-60 MHz.
[0163] In some aspects, the techniques described herein relate to a system, wherein the low frequency power is about 400 to about 4.000 W at a frequency of between about 400 kHz and 1MHz.
[0164] In some aspects, the techniques described herein relate to a system, wherein the controller is configured to cause the pressure within the plasma enhanced chemical vapor deposition reactor to be about 0.5 to 6.5 Torr.Atorney Docket No. LAM1P135 WO- 12202-1 WO
[0165] In some aspects, the techniques described herein relate to a system, wherein the controller is configured to cause a temperature within the plasma enhanced chemical vapor deposition reactor to be about 350 to 450 °C.
[0166] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has an atomic ratio between boron and nitrogen of about 1:1.01 to about 1:1.25.
[0167] In some aspects, the techniques described herein relate to a system, wherein the boron nitride has a compressive stress relative to the substrate of about -300 to about -3200 GPa.Conclusion
[0168] In the foregoing description, numerous specific details are set forth to provide a thorough understanding of the presented embodiments. The disclosed embodiments may be practiced without some or all these specific details. In other instances, well-known process operations have not been described in detail to not unnecessarily obscure the disclosed embodiments. While the disclosed embodiments are described in conjunction with the specific embodiments, it will be understood that it is not intended to limit the disclosed embodiments.
[0169] Although the foregoing embodiments have been described in some detail for purposes of clarity of understanding, it will be apparent that certain changes and modifications may be practiced within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the processes, structures, systems, and apparatus of the present embodiments. Accordingly, the present embodiments are to be considered as illustrative and not restrictive, and the embodiments are not to be limited to the details given herein.
Claims
Atorney Docket No. LAM1P135 WO- 12202-1 WO CLAIMSWhat is claimed is:
1. A method of depositing boron nitride on a substrate, the method comprising:(a) receiving the substrate in a plasma reactor;(b) delivering a process gas to the plasma reactor, wherein the process gas comprises: a boron precursor, a nitrogen source comprising ammonia or molecular nitrogen, and a carrier gas; and(c) applying a low frequency power to a first electrode, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz,wherein the boron nitride has a thermal conductivity of at least about 2 W / m-K.
2. The method of claim 1 , further comprising applying a high frequency power to a second electrode in the plasma reactor, wherein the high frequency power is at a frequency of about 13-60 MHz.
3. The method of claim 2. wherein the high frequency power is about 0.1 to 2000 W at a frequency of about 13-60 MHz.
4. The method of claim 1, wherein the low frequency power is about 2,000 to 5,000 W at a frequency of about 400 kHz and 1MHz.
5. The method of claim 2, wherein the first and second electrodes are different.
6. The method of claim 2, wherein the second electrode comprises or is incorporated in a substrate support.
7. The method of claim 1. wherein the boron nitride has a grain size of about 3 to about 9.5 nm.
8. The method of claim 1, wherein the boron nitride has an impurity of about 0 to about 3 mol%.
9. The method of claim 1. wherein the boron nitride has a density of about 1.5 to about 2.3 g / cc.
10. The method of claim 1, wherein the boron precursor comprises diborane (EhHe), borazine, Ammonia Borane complex (AB), 1, 3, 5-Tri(methyl)borazine (TMBZ), B-Atorney Docket No. LAM1P135 WO- 12202-1 WO tris(dimethylamino) borazine [N-dimethyl TMBZ], Tris(di methylamino) borane (TDMAB), boron chloride (BCh), and boron fluoride (BF3), or any combination thereof.
11. The method of claim 1. wherein the process gas comprises the boron precursor in a concentration of about 0.01 mol% to 0.3 mol%, the nitrogen source in a concentration of about 50 mol% to 90 mol%, and the carrier gas in a concentration of about 9 mol% to about 50 mol%.
12. The method of claim 1, wherein the process gas further comprises a fluorine source comprising nitrogen trifluoride (NF3), molecular fluorine (F2), sulfur hexafluoride (SFe), or boron trifluoride (BF3), or any combination thereof.
13. The method of claim 2, wherein the high frequency power is about 400 to 4,000 W at a frequency of between about 13-60 MHz.
14. The method of claim 1. wherein the low frequency power is about 400 to 4.000 W at a frequency of between about 400 kHz and 1MHz.
15. The method of claim 1, wherein operations (b)-(c) are performed at a pressure of about 0.5 to about 6.5 Torr.
16. The method of claim 1, wherein operations (b)-(c) are performed at a temperature of about 350°C to about 450°C.
17. The method of claim 1, wherein the boron nitride has an atomic ratio between boron and nitrogen of about 1:1.01 to about 1:1.25.
18. A system configured to produce boron nitride, the system comprising:a plasma enhanced chemical vapor deposition reactor comprising (a) at least two electrodes configured to produce high frequency RF energy for generating a plasma and low frequency RF energy for driving ions from the plasma to a surface of a substrate, and (b) a process gas inlet; anda controller configured to cause concurrently:delivery of a process gas to the plasma enhanced chemical vapor deposition reactor via the process gas inlet, wherein the process gas comprises: a boron precursor, a nitrogen source comprising ammonia or molecular nitrogen, and a carrier gas.Atorney Docket No. LAM1P135 WO- 12202-1 WO application of a low frequency power to a first one of the at least two electrodes, wherein the low frequency power is at least about 400 W at a frequency of between about 400 kHz and 1MHz, anda pressure within the plasma enhanced chemical vapor deposition reactor to be between about 0.5 and 10 Torr.
19. The system of claim 18, wherein the controller is additionally configured to cause application of a high frequency power to a second one of the at least two electrodes, wherein the high frequency power is at a frequency of about 13-60 MHz.
20. The system of claim 19, wherein the high frequency power is about 0.1 to 2000 W at a frequency of about 13-60 MHz.
21. The system of claim 18, wherein the low frequency power is about 2,000 to 5,000 W at a frequency of about 400 kHz to 1 MHz.
22. The system of claim 19, wherein the first and second electrodes are different from each other.
23. The system of claim 19, wherein the second electrode comprises or is integrated in a substrate support.
24. The system of claim 18, wherein the boron precursor comprises diborane (EhHe). borazine, Ammonia Borane complex (AB), 1, 3, 5-Tri(methyl)borazine (TMBZ), B-tris(dimethylamino) borazine [N-dimethyl TMBZ], Tns(dimethylammo) borane (TDMAB), boron chloride (BCk), and boron fluoride (BF3), or any combination thereof.
25. The system of claim 18, wherein the process gas comprises the boron precursor in a concentration of about 0.01 mol% to 0.3 mol%, the nitrogen source in a concentration of about 50 mol% to 90 mol%, and the carrier gas in a concentration of about 9 mol% to about 50 mol%.
26. The system of claim 18, wherein the high frequency power is about 400 to about 4,000 W at a frequency of between about 13-60 MHz.
27. The system of claim 18, wherein the low frequency power is about 400 to about 4,000 W at a frequency of between about 400 kHz and 1MHz.
28. The system of claim 18, wherein the controller is configured to cause the pressure within the plasma enhanced chemical vapor deposition reactor to be about 0.5 to 6.5 Torr.Atorney Docket No. LAM1P135 WO- 12202-1 WO 29. The system of claim 18, wherein the controller is configured to cause a temperature within the plasma enhanced chemical vapor deposition reactor to be about 350 to 450 °C.
30. The system of claim 18, wherein the boron nitride has an atomic ratio between boron and nitrogen of about 1:1.01 to about 1:1.25.