Adaptive polymer electrolytes and methods of making and use thereof
Adaptive polymer electrolytes with conductive particles in a polymer matrix address the interface stability issue in lithium-metal solid-state batteries by expanding under an electric field to maintain contact, improving battery performance.
Patent Information
- Application Number
- PCT/US2026/027251
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
The stability of the interface between the lithium-metal anode and the solid-state electrolyte in lithium-metal solid-state batteries is limited by the formation of voids due to non-uniform lithium plating/stripping, leading to discontinuous contact during cycling.
Adaptive polymer electrolytes comprising conductive polymer particles dispersed in a continuous polymer electrolyte matrix, which exhibit an expansion response under an applied electric field to maintain continuous contact and stabilize the lithium-metal interface.
The adaptive polymer electrolytes provide stable lithium-metal interfaces, maintaining contact over multiple cycles and enhancing the performance of lithium-metal solid-state batteries.
Smart Images

Figure US2026027251_12112026_PF_FP_ABST
Abstract
Description
[0001] ADAPTIVE POLYMER ELECTROLYTES
[0002] AND METHODS OF MAKING AND USE THEREOF
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to U.S. Provisional Application No.
[0004] 63 / 802,802 filed May 9, 2025, which is hereby incorporated herein by reference in its entirety.
[0005] BACKGROUND
[0006] The energy density and safety of lithium -metal solid-state batteries (LIMSSBs) are limited by the stability of the interface between the lithium-metal anode and the solid-state electrolyte. Traditional approaches using static interlayers or coatings often fail to maintain continuous contact during cycling, particularly when voids form due to non-uniform lithium plating / stripping. Improved interlayers are needed. The compositions, methods, and systems described herein address this and other needs.
[0007] SUMMARY
[0008] In accordance with the purposes of the disclosed compositions, methods, and systems as embodied and broadly described herein, the disclosed subject matter relates to adaptive polymer electrolytes and methods of making and use thereof. For example, the disclosed subject matter relates to thin adaptive polymer interlayer for stabilizing lithium-metal interfaces in solid state batteries.
[0009] For example, disclosed herein are adaptive polymer electrolytes comprising: a plurality of conductive polymer particles dispersed throughout a continuous polymer electrolyte matrix; wherein the adaptive polymer electrolyte exhibits an expansion response at room temperature under an applied electric field.
[0010] In some examples, the plurality of conductive polymer particles exhibit electrorheological properties under an electric field.
[0011] In some examples, the plurality of conductive polymer particles are provided in an amount below the percolation threshold.
[0012] In some examples, the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 5 wt.% (relative to the amount of main and additional monomers in the matrix).
[0013] In some examples, the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
[0014] In some examples, the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 30 vol%, such as from greater than 0 to 15 vol%, of theadaptive polymer electrolyte.
[0015] In some examples, the plurality of conductive polymer particles comprise polypyrrole. In some examples, the plurality of conductive polymer particles comprise polypyrrole doped with a dopant. In some examples, the plurality of conductive polymer particles comprise polypyrrole doped with dodecylbenzenesulfonate.
[0016] In some examples, the plurality of conductive polymer particles comprise polypyrrole doped with dodecylbenzenesulfonate and the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
[0017] In some examples, the continuous polymer electrolyte matrix is derived from a main chain polymer, such as polyethylene oxide (e.g., PEO with a molecular weight of 100,000).
[0018] In some examples, the continuous polymer electrolyte matrix is further derived from a cross-linking monomer, such as tetraethylene glycol dimethacrylate (TEGDMA).
[0019] In some examples, the continuous polymer electrolyte matrix is further derived from one or more salts, such as one or more lithium salts. In some examples, the lithium salts comprise lithium bis(trifluoromethane)sulfonamide (LiTFSI), lithium bis(oxalate)borate (LiBoB), or a combination thereof.
[0020] In some examples, the continuous polymer electrolyte matrix is further derived from a plasticizer, such as tetraethylene glycol dimethyl ether (TEGDME).
[0021] In some examples, the continuous polymer electrolyte matrix is further derived from a photoinitiator, such as a UV-photoinitiator, such as methylbenzophenone (MBP).
[0022] In some examples, the continuous polymer electrolyte matrix is derived from: 20-40 wt.% (e.g., 30.3 wt.%) main chain polymer (e.g. PEO); 10-20 wt.% (e.g., 15.1 wt.%) crosslinking monomer (e.g., TEGDMA); 15-25 wt.% (e.g., 21.3 wt.%) Li Salt (e.g., 17.8 wt.% LITFSI and 3.5 wt.% LiBoB); 20-40 wt.% (e.g., 30.3 wt.%) plasticizer (e.g., TEGDME); and 1-5 wt.% (e.g., 3.0 wt.%) photoinitiator (e.g., MBP); wherein the sum adds to 100%.
[0023] In some examples, the continuous polymer electrolyte matrix is derived from: 20-40 wt.% (e.g., 30.3 wt.%) PEO; 10-20 wt.% (e.g., 15.1 wt.%) TEGDMA; 15-25 wt.% (e.g., 21.3 wt.%) Li Salt (e.g., 17.8 wt.% LITFSI and 3.5 wt.% LiBoB); 20-40 wt.% (e.g., 30.3 wt.%) TEGDME; and 1-5 wt.% (e.g., 3.0 wt.%) MBP; wherein the sum adds to 100%.
[0024] In some examples, the continuous polymer electrolyte matrix is derived from: 30.3 wt.% PEO; 15.1 wt.% TEGDMA; 17.8 wt.% LITFSI; 3.5 wt.% LiBoB; 30.3 wt.% TEGDME; and 3.0 wt.% MBP.
[0025] In some examples, the adaptive polymer electrolyte has an ionic conductivity of from 0.1to 0.5 mS cm'1, such as 0.1 to 0.25 mS cm'1(e.g., 0.11-0.16 mS cm'1), at 25°C.
[0026] In some examples, the adaptive polymer electrolyte exhibits an expansion response of greater than 0% to 10% strain (e.g., 6%) at room temperature and an electric field strength of 0.3 V pm'1.
[0027] In some examples, the adaptive polymer electrolyte is a free-standing film.
[0028] In some examples, the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 50 micrometers. In some examples, the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 25 micrometers, such as from 50 nanometers to 10 micrometers or from 50 nanometers to 5 micrometers.
[0029] In some examples, the adaptive polymer electrolyte is substantially stable over 5 or more cycles (e.g., 50 or more cycles, or 100 or more cycles).
[0030] Also disclosed herein are methods of use of any of the adaptive polymer electrolytes disclosed herein. In some examples,
[0031] the method comprises using the adaptive polymer electrolyte as an interlayer between lithium-metal electrode (e.g., Li-metal anode) and solid electrolyte in a lithium metal solid-state battery.
[0032] Also disclosed herein are articles of manufacture comprising any of the adaptive polymer electrolytes disclosed herein. In some examples, the article comprises a lithium metal solid-state battery.
[0033] Also disclosed herein are methods of making any of the adaptive polymer electrolytes disclosed herein. In some examples, the method comprises: combining the continuous polymer electrolyte matrix precursors and the plurality of conductive polymer particles to form a mixture; stirring the mixture for 4 -24 hours (e.g., 8-12 hours or overnight) at room temperature; subsequently ultrasonicating the mixture for 1 minute to 30 minutes (e.g., 10 minutes); subsequently hot pressing the mixture (e.g., 80°C, 4.4 bar, 10 minutes); and subsequently UV-polymerizing the mixture (e.g., 150 mW / cm2, 10 minutes). In some examples, the methods further comprise subsequently vacuum drying the UV-polymerized mixture (e.g., 40°C, overnight). In some examples, the methods further comprise making the plurality of conductive polymer particles.
[0034] Additional advantages of the disclosed compositions, systems, and methods will be set forth in part in the description which follows, and in part will be obvious from the description. The advantages of the disclosed compositions, systems, and methods will be realized and attained by means of the elements and combinations particularly pointed out in the appended claims. It is to be understood that both the foregoing general description and the followingdetailed description are exemplary and explanatory only and are not restrictive of the disclosed compositions, systems, and methods, as claimed.
[0035] The details of one or more embodiments of the invention are set forth in the accompanying drawings and the description below. Other features, objects, and advantages of the invention will be apparent from the description and drawings, and from the claims.
[0036] BRIEF DESCRIPTION OF DRAWINGS FIG. 1 shows the concept of a self-adaptive interlayer applied between a Li-metal anode and ceramic solid electrolyte. The self-adaptive interlayer (SAI) is shown as a polymer electrolyte matrix in blue with black CP particles dispersed in the matrix, which would try to align along an electric field (AT) to expand and re-establish interface contact. Li-ion transfer is shown to occur primarily through the polymer electrolyte matrix.
[0037] FIG. 2 shows a summary of the polymer electrolyte components and the synthesis process used.
[0038] FIGs. 3A-3B show the (FIG. 3 A) schematic of AFM sample setup for the A-PE and (FIG. 3B) picture of a sample with the area used for AFM characterizations indicated by the dotted line box (grid size 5 mm).
[0039] FIGs. 4A-4D show the physical characterizations of the polymer electrolytes. (FIG. 4A) Insoluble fraction measurements with markers indicating average values and error bars indicating standard deviations. Markers are offset horizontally for visibility. Inset shows appearance of films with different amounts of PPy(DBS) (grid size 5 mm). (FIG. 4B) XRD patterns (FIG. 4C) DSC profiles, and (FIG. 4D) DMA tan delta thermograms, a.u. denotes arbitrary units. XRD, DSC, and DMA curves are offset vertically for visibility.
[0040] FIGs. 5A-5F show the AFM continuous point measurement of polymer film under 0.3 V / pm followed by 0 V / pm electric field strength for (FIG. 5A) 0 wt% PPy(DBS), (FIG. 5B) 0.25 wt% PPy(DBS), (FIG. 5C) 0.5 wt% PPy(DBS), and (FIG. 5D) 1 wt% PPy(DBS). (FIG. 5E) Film strain at the end of each excitation and relaxation and (FIG. 5F) excitation and relaxation time constants with markers indicating median values and error bars indicating standard deviations.
[0041] FIGs. 6A-6H show the surface of 50 nm gold coated 1 wt% PPy(DBS) film (FIG. 6A) SEM micrograph, (FIGs. 6B-6D) AFM topography maps of 10 pm x 10 pm area (FIG. 6B) at initial rest, (FIG. 6C) after the first excitation for 10 min, and (FIG. 6D) after the first relaxation for 10 min. Zoomed-out (FIG. 6E) SEM micrograph, (FIGs. 6F-6H) AFM topography maps of 30 pm x 30 pm area (FIG. 6F) at initial rest, (FIG. 6G) after the first excitation for 10 min, and (FIG. 6H) after the first relaxation for 10 min. SEM micrographs were obtained with secondary electron mode at an accelerating voltage of 5 kV and beam current of 0.20 nA.FIGs. 7A-7B show the (FIG. 7 A) schematic of block force setup for the A-PE and (FIG.
[0042] 7B) force response measurements under different electric field strengths. Markers indicate average values, and the shaded area indicates the region below the detection limit of the force sensor.
[0043] FIGs. 8A-8D show a summary of polymer electrolyte electrochemical characterizations at 25 °C. (FIG. 8A) Ionic conductivity from EIS and (FIG. 8B) interfacial impedance from EIS after 50 Li symmetric cycles with markers indicating median values (corresponding to an actual coin cell) and error bars indicating standard deviations. (FIG. 8C) EIS spectra of representative Li / polymer / Li coin cells after 50 Li symmetric cycles for 0-1 wt% PPy(DBS) with markers indicating measured values and solid lines representing the equivalent circuit fit. Equivalent circuit elements consist of series resistance (Rs), solid electrolyte interphase resistance (RSEI), charge transfer resistance (Ret), and constant phase elements (CPEi, CPE2). (FIG. 8D) ESW from CV and LSV.
[0044] FIG. 9 shows the SEM cross-section of thin polymer film (targeting ~10 pm thick) between indium tin oxide (ITO) coated polyethylene terephthalate (PET) sheets. Cross-section obtained by shearing with titanium coated blade. SEM micrograph obtained with backscatter electron mode at an accelerating voltage of 2 kV and beam current of 13 pA.
[0045] FIG. 10 shows the coin cell stack used for electrochemical impedance spectroscopy and Li symmetric cycling experiments.
[0046] FIGs. 11A-11B show the coin cell stack used for electrochemical stability window experiments with Li-metal as the counter / reference electrode (CE / RE) for (FIG. 11 A) anodic scan with 304SS as the working electrode (WE) and (FIG. 11B) cathodic scan with Cu as the WE.
[0047] FIGs. 12A-12C show images demonstrating the as produced free-standing polymer electrolyte film for 0 wt% PPy(DBS) composition. (FIG. 12 A) Unstretched film, (FIG. 12B) stretching the film and (FIG. 12C) bending the film. Grid size 5 mm.
[0048] FIG. 13 shows the electrical conductivity measurements of the polymer films with varying amounts of PPy(DBS). Markers indicate average values and error bars indicate standard deviations.
[0049] FIGs. 14A-14D show the DMA storage (G’) and loss modulus (G”) profiles for (FIG.
[0050] 14A) 0 wt% PPy(DBS), (FIG. 14B) 0.25 wt% PPy(DBS), (FIG. 14C) 0.5 wt% PPy(DBS), and (FIG. 14D) 1 wt% PPy(DBS).
[0051] FIGs. 15A-15C show the AFM continuous point measurement of polymer film under 0.1-0.2 V / pm followed by 0 V / pm electric field strength for (FIG. 15A) 1 wt% PPy(DBS) with0.2 V / pm excitations, (FIG. 15B) 0.5 wt% PPy(DBS) with 0.2 V / pm excitations, and (FIG. 15C) 1 wt% PPy(DBS) with 0.1 V / pm excitations.
[0052] FIG. 16 shows the Li symmetric cycling overpotentials for a representative Li / polymer / Li coin cell from each composition at 25 °C under ± 0.1 mA / cm2for 30 min each direction with 30 min rests for 50 cycles.
[0053] FIGs. 17A-17D show the EIS spectra at 25 °C of representative Li / polymer / Li coin cells after 0, 25, and 50 Li symmetric cycles for (FIG. 17A) 0 wt% PPy(DBS), (FIG. 17B) 0.25 wt% PPy(DBS), (FIG. 17C) 0.5 wt% PPy(DBS), and (FIG. 17D) 1 wt% PPy(DBS). Markers indicate measured values and solid lines represent the equivalent circuit fit. Equivalent circuit elements consist of series resistance (Rs), solid electrolyte interphase resistance (RSEI), charge transfer resistance (Ret), and constant phase elements (CPEi, CPE2).
[0054] FIGs. 18A-18B show zoomed-in plots of (FIG. 18A) the cathodic CVs and (FIG. 18B) the anodic LSV for determining ESW of the polymer electrolyte compositions with 0-1 wt% PPy(DBS).
[0055] FIG. 19 shows the LIMSSB interface degradation after cycling for (top) no modifications and (bottom) contemporary solutions such as a polymer interlayer to provide good initial contact and flexibility to accommodate some volume changes.
[0056] FIGs. 20A-20D show the (top) surface modification without and with atomic layer deposition of AI2O3 [B22] and (bottom) without and with acid-salt treatment [B23 ] .
[0057] FIGs. 21A-21B show the (left) composite SSE [B24] and (right) polymer interlayers [B25],
[0058] FIGs. 22A-22B show the chemical structure of CPs (FIG. 22A) polypyrrole doped with dodecylbenzenesulfonate [B43] and (FIG. 22B) polyaniline [B44],
[0059] FIGs. 23A-23B shown the (FIG. 23 A) flow curve of PPy -based ER fluid and (FIG. 23B) light microscopy image of fluid under electric field of 3 kV / mm [B3],
[0060] FIGs. 24A-24B show the concept of an adaptive polymer interlayer applied between a Li-metal anode and ceramic solid electrolyte. The zoomed-in views show the interlayer with the battery circuit open at rest and the interlayer expanding due to the electric field when the battery circuit is closed during charging or discharging. (FIG. 24A) A CP film applied as the interlayer. (FIG. 24B) A composite of CP particles in a polymer electrolyte matrix applied as the interlayer with the zoomed-in view showing the particles within the polymer electrolyte matrix trying to align when polarized under the electric field causing the interlayer to expand. Li-ion transfer is shown to occur primarily through the polymer electrolyte matrix.
[0061] FIGs. 25A-25B show the Electrochemically delaminated films from (FIG. 25A) 304SSand (FIG. 25B) EBPVD gold substrate. Grid size 5 mm.
[0062] FIGs. 26A-26B show the representative SEM cross-sections of electrochemically delaminated free-standing PPy(DBS) films from (FIG. 26A) 304SS with electropolymerization charge densities of 1.0 C / cm2and (FIG. 26B) EBPVD gold with electropolymerization charge densities of 0.1 C / cm2.
[0063] FIG. 27 shows the custom Swagelok pressure cell setup. A Swagelok cell containing the solid-state battery stack between two metal plungers is pressurized between plates of a pressure retention jig on the left. An in-line load cell monitors the stack pressure when the pressure is applied uniaxially with a hydraulic press on the right.
[0064] FIG. 28 shows the summary of solvent cast synthesis process for PEO based polymer electrolyte.
[0065] FIGs. 29A-29B show the XRD measurements comparing the crystallinity of films without and with SN plasticizer (FIG. 29A) in this work compared to (FIG. 29B) literature.
[0066] FIGs. 30A-30C show the Li / polymer / Li Swagelok cell at room temperature (FIG. 30 A) Li cycling under ±0.1 mA / cm2, (FIG. 30B) operating stack pressure, and (FIG. 30C) intermittent EIS spectra.
[0067] FIG. 31 shows the periodic EIS measurements of coin cell over 24 hr rest at 70 °C. FIG. 32 shows the Li cycling at ±0.1 mA / cm2and intermittent EIS of coin cell at 50 °C. FIG. 33 shows the summary of UV polymerization synthesis process for PEO based polymer electrolyte replicated as closely as possible to literature process [B66], PET -polyethylene terephthalate.
[0068] FIG. 34 shows the summary of UV polymerization synthesis process for PEO based polymer electrolyte adapted from literature process [B67],
[0069] FIGs. 35A-35B show the (FIG. 35 A) graphic adapted from [B67] showing how the film is prepared prior to dissolving the soluble components and (FIG. 35B) insoluble fraction results for compositions adapted from [B66, B67],
[0070] FIGs. 36A-36B show the XRD spectra of polymer electrolyte film with TEGDMA from (FIG. 36A) this work and (FIG. 36B) reported by literature [B67],
[0071] FIG. 37 shows the intermittent EIS spectra over Li cycling at ±0.1 mA / cm2at 25 °C of middle performing Li symmetric coin cell with the final polymer electrolyte composition.
[0072] FIGs. 38A-38F show the SEM micrographs of LLZTO pellet cross-sections for (FIG. 38Aand 38B) commercially purchased pellets, (FIG. 38C and 38D) lab-made oven sintered pellets from commercially purchased nm-powder, and (FIG. 38E and 38F) lab-made oven sintered pellets from commercially purchased pm-powder. SEM micrographs were obtained withsecondary electron mode at an accelerating voltage of 2 kV and beam current of 25 pA.
[0073] FIG. 39 shows the Nyquist plot obtained from EIS measurements on three samples of 50 nm gold blocking electrode / LLZTO / 50 nm gold blocking electrode for oven sintered LLZTO pellets pressed from commercial nm-powder and covered with commercial pm-powder during sintering.
[0074] FIG. 40 shows the modified process for synthesizing the polymer interlayer directly on the Li-metal surface.
[0075] FIG. 41 shows the interfacial impedance of Li / polymer interlayer (synthesized directly on Li-metal) / Li coin cells over a few days at rest at 25 °C.
[0076] FIG. 42 shows the adapted process for synthesizing the polymer interlayer directly on the LLZTO ceramic solid electrolyte surface.
[0077] FIG. 43 shows the LLZTO pellet with 5 mg / cm2of polymer solution hot-pressed and UV cured on it, followed by peeling off the top PET film and an SEM cross-section of areas with the polymer remaining on the LLZTO pellet.
[0078] FIG. 44 shows the modified synthesis process of polymer interlayer on LLZTO ceramic solid electrolyte surface.
[0079] FIG. 45 shows the LLZTO pellet with 3 mg / cm2of polymer solution hot-pressed and UV cured on it, followed by peeling off the top FEP film which left the polymer interlayer fully intact on the LLZTO surface.
[0080] FIG. 46 shows the SEM cross-sections of 3 mg / cm2polymer interlayer on LLZTO ceramic electrolyte pellet, with the approximate locations indicated on the image of the coated pellet.
[0081] FIG. 47 shows the LLZTO / polymer interlayer incorporated in symmetric Li coin cell with a free-standing polymer electrolyte on the other side to measure the electrochemical stability of the polymer interlayer after synthesis.
[0082] FIG. 48 shows the interfacial impedance of LLZTO / polymer interlayer in symmetric Li coin cells over several days resting at 25 °C.
[0083] FIG. 49 shows the diagram of pseudo-solid LIMSSB to focus on the Li / polymer interlayer / LLZTO side of the cell. Liquid is added to improve the interface on the cathode side of the cell.
[0084] FIG. 50 shows the pseudo-solid LIMSSB coin cell setup.
[0085] FIG. 51 shows the assembly process of pseudo-solid LIMSSB coin cell, pictured with the baseline polymer interlayer, with Cu foil then placed on top of the Li chip followed by the top (smaller) coin cell case, then the coin cell is crimped closed.FIGs. 52A-52B show the specific capacity of pseudo-solid full cells with number of cycles at areal current density of 0.3 mA / cm2with respect to (FIG. 52A) the active material mass of the NMC622 cathode or (FIG. 52B) the total mass of the internal cell stack. Charge cycles are represented with solid markers and discharge cycles are represented with hollow markers on the plot. The vertical dotted lines indicate when EIS is performed on the cells.
[0086] FIGs. 53A-53B show the specific capacity of pseudo-solid full cells with number of cycles at areal current density of 0.5 mA / cm2with respect to (FIG. 53 A) the active material mass of the NMC622 cathode or (FIG. 53B) the total mass of the internal cell stack. Charge cycles are represented with solid markers and discharge cycles are represented with hollow markers on the plot. The vertical dotted lines indicate when EIS is performed on the cells.
[0087] FIGs. 54A-54B show the capacity retention of pseudo-solid full cells with number of cycles at areal current density of (FIG. 54A) 0.3 mA / cm2and (FIG. 54B) 0.5 mA / cm2.
[0088] FIGs. 55A-55D show the (FIG. 55A) Nyquist plot and (FIG. 55B) DRT analysis for a symmetric Li / SPE / Li coin cell disclosed in the examples. (FIG. 55C) Nyquist plot and (FIG. 55D) DRT analysis for Li / Interlayer / LLZTO / SPE / Li coin cells.
[0089] FIGs. 56A-56D show the EIS results from the first batch of pseudo-solid full cells. (FIG.
[0090] 56A) Nyquist plot and (FIG. 56B) DRT analysis for the cell that appeared completely dry on the cathode side in FIG. 62A. (FIG. 56C) Nyquist plot and (FIG. 56D) DRT analysis for the cell that still appeared partially wetted on the cathode side in FIG. 62B.
[0091] FIGs. 57A-57D show the EIS results from a representative pseudo-solid full cell of each composition with the updated assembly process, cycled at areal current density of 0.5 mA / cm2. (FIG. 57A) Nyquist plot and (FIG. 57B) DRT analysis for 0 wt% PPy(DBS) - Cell 1. (FIG. 57C) Nyquist plot and (FIG. 57D) DRT analysis for 1 wt% PPy(DBS) - Cell 2.
[0092] FIG. 58 shows the 3 -electrode pseudo-solid full cell assembly with a RE inserted between a free-standing polymer electrolyte layer and the LLZTO ceramic electrolyte.
[0093] FIG. 59 shows the lithiation of the gold wire RE and the potential stability of the RE during rest after the lithiation.
[0094] FIG. 60 shows the RE measurements of 3 -electrode pseudo-solid full cell under various charging and discharging current densities.
[0095] FIGs. 61A-61B show the disassembled pseudo-solid full cells from the first batch where 10 pL of high concentrated electrolyte was used on the cathode side of the cell for (FIG. 61 A) one cell that appeared completely dry on the cathode side and (FIG. 6 IB) one cell that was ly dry on the cathode side.
[0096] FIGs. 62A-62B show the disassembled pseudo-solid full cells from the first batchshowing the Li-metal anode stuck to the coin cell case upon disassembly for (FIG. 62A) cell with 0 wt% PPy(DBS) polymer interlayer and (FIG. 62B) cell with 1 wt% PPy(DBS) polymer interlayer.
[0097] FIGs. 63A-63B show the disassembled pseudo-solid full cells from the updated assembly process with 30 pL of high concentrated electrolyte used on the cathode side of the cell. (FIG. 63 A) NMC622 cathode side and Celgard separator still appears fully wetted. (FIG.
[0098] 63B) Li-metal anode still came off with coin cell case, even with Cu foil in between.
[0099] FIGs. 64A-64C show the disassembled pseudo-solid full cells from the updated assembly process with Cu foil in between the Li-metal anode and coin cell case showing (FIG.
[0100] 64A) the Cu foil / Li-metal anode was barely stuck to coin cell case and easily removed, (FIG.
[0101] 64B) Li-metal side, and (FIG. 64C) Cu foil side showing the Cu foil fully covered the Li-metal, separating the Li-metal from the coin cell case.
[0102] FIGs. 65A-65B show the coulombic efficiencies of pseudo-solid full cells with number of cycles at areal current density of (FIG. 65A) 0.3 mA / cm2and (FIG. 65B) 0.5 mA / cm2.
[0103] FIGs. 66A-66D show the EIS results from pseudo-solid full cell of each composition with the updated assembly process, cycled at areal current density of 0.3 mA / cm2. (FIG. 66A) Nyquist plot and (FIG. 66B) DRT analysis for 0 wt% PPy(DBS) - Cell 1. (FIG. 66C) Nyquist plot and (FIG. 66D) DRT analysis for 1 wt% PPy(DBS) - Cell 1.
[0104] FIGs. 67A-67D show the EIS results from pseudo-solid full cell of each composition with the updated assembly process, cycled at areal current density of 0.3 mA / cm2. (FIG. 67A) Nyquist plot and (FIG. 67B) DRT analysis for 0 wt% PPy(DBS) - Cell 2. (FIG. 67C) Nyquist plot and (FIG. 67D) DRT analysis for 1 wt% PPy(DBS) - Cell 2.
[0105] FIGs. 68A-68D show the EIS results from pseudo-solid full cell of each composition with the updated assembly process, cycled at areal current density of 0.3 mA / cm2. (FIG. 68A) Nyquist plot and (FIG. 68B) DRT analysis for 0 wt% PPy(DBS) - Cell 3. (FIG. 68C) Nyquist plot and (FIG. 68D) DRT analysis for 1 wt% PPy(DBS) - Cell 3.
[0106] FIGs. 69A-69D show the EIS results from pseudo-solid full cell of each composition with the updated assembly process, cycled at areal current density of 0.5 mA / cm2. (FIG. 69A) Nyquist plot and (FIG. 69B) DRT analysis for 0 wt% PPy(DBS) - Cell 2. (FIG. 69C) Nyquist plot and (FIG. 69D) DRT analysis for 1 wt% PPy(DBS) - Cell 1.
[0107] FIGs. 70A-70D show the EIS results from pseudo-solid full cell of each composition with the updated assembly process, cycled at areal current density of 0.5 mA / cm2. (FIG. 70A) Nyquist plot and (FIG. 70B) DRT analysis for 0 wt% PPy(DBS) - Cell 3. (FIG. 70C) Nyquist plot and (FIG. 70D) DRT analysis for 1 wt% PPy(DBS) - Cell 3.FIG. 71 provides a schematic of HIL experimental setup.
[0108] FIG. 72 provides the current profile for training.
[0109] FIG. 73 provides the battery model state cse pprediction training set.
[0110] FIG. 74 provides the battery model state cse pprediction under a section of training and validation sets.
[0111] FIG. 75 provides the RL-HIL experimental data for knidentification.
[0112] FIG. 76 provides the drive cycle verification of the calibrated model with identified knusing RL-HIL experiment and 1C, 5C and RCID conventional tests.
[0113] DETAILED DESCRIPTION
[0114] Before the present compositions, methods, and systems are disclosed and described, it is to be understood that the aspects described below are not limited to specific synthetic methods or specific reagents, as such may, of course, vary. It is also to be understood that the terminology used herein is for the purpose of describing particular aspects only and is not intended to be limiting.
[0115] Also, throughout this specification, various publications are referenced. The disclosures of these publications in their entireties are hereby incorporated by reference into this application in order to more fully describe the state of the art to which the disclosed matter pertains. The references disclosed are also individually and specifically incorporated by reference herein for the material contained in them that is discussed in the sentence in which the reference is relied upon.
[0116] In this specification and in the claims that follow, reference will be made to a number of terms, which shall be defined to have the following meanings.
[0117] Throughout the description and claims of this specification the word “comprise” and other forms of the word, such as “comprising” and “comprises,” means including but not limited to, and is not intended to exclude, for example, other additives, components, integers, or steps.
[0118] As used in the description and the appended claims, the singular forms “a,” “an,” and “the” include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to “a composition” includes mixtures of two or more such compositions, reference to “an agent” includes mixtures of two or more such agents, reference to “the component” includes mixtures of two or more such components, and the like.
[0119] “Optional” or “optionally” means that the subsequently described event or circumstance can or cannot occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.
[0120] Ranges can be expressed herein as from “about” one particular value, and / or to “about”another particular value. By “about” is meant within 5% of the value, e.g., within 4, 3, 2, or 1% of the value. When such a range is expressed, another aspect includes from the one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, by use of the antecedent “about,” it will be understood that the particular value forms another aspect. It will be further understood that the endpoints of each of the ranges are significant both in relation to the other endpoint, and independently of the other endpoint.
[0121] “Exemplary” means “an example of’ and is not intended to convey an indication of a preferred or ideal embodiment. “Such as” is not used in a restrictive sense, but for explanatory purposes.
[0122] Values can be expressed herein as an “average” value. “Average” generally refers to the statistical mean value.
[0123] By “substantially” is meant within 5%, e.g., within 4%, 3%, 2%, or 1%.
[0124] It is understood that throughout this specification the identifiers “first” and “second” are used solely to aid in distinguishing the various components and steps of the disclosed subject matter. The identifiers “first” and “second” are not intended to imply any particular order, amount, preference, or importance to the components or steps modified by these terms.
[0125] References in the specification and concluding claims to parts by weight of a particular element or component in a composition denotes the weight relationship between the element or component and any other elements or components in the composition or article for which a part by weight is expressed. Thus, in a compound containing 2 parts by weight of component X and 5 parts by weight component Y, X and Y are present at a weight ratio of 2:5, and are present in such ratio regardless of whether additional components are contained in the compound.
[0126] A weight percent (wt. %) of a component, unless specifically stated to the contrary, is based on the total weight of the formulation or composition in which the component is included.
[0127] A volume percent (vol%) of a component, unless specifically stated to the contrary, is based on the total volume of the formulation or composition in which the component is included.
[0128] The term “or combinations thereof’ as used herein refers to all permutations and combinations of the listed items preceding the term. For example, “A, B, C, or combinations thereof’ is intended to include at least one of: A, B, C, AB, AC, BC, or ABC, and if order is important in a particular context, also BA, CA, CB, CBA, BCA, ACB, BAC, or CAB.
[0129] Continuing with this example, expressly included are combinations that contain repeats of one or more item or term, such as BB, AAA, AB, BBC, AAABCCCC, CBBAAA, CAB ABB, and so forth. The skilled artisan will understand that typically there is no limit on the number of items or terms in any combination, unless otherwise apparent from the context.The expressions “ambient temperature” and “room temperature” as used herein are understood in the art and refer generally to a temperature from about 20°C to about 35°C.
[0130] “Phase,” as used herein, generally refers to a region of a material having a substantially uniform composition which is a distinct and physically separate portion of a heterogeneous system. The term “phase” does not imply that the material making up a phase is a chemically pure substance, but merely that the chemical and / or physical properties of the material making up the phase are essentially uniform throughout the material, and that these chemical and / or physical properties differ significantly from the chemical and / or physical properties of another phase within the material. Examples of physical properties include density, thickness, aspect ratio, specific surface area, porosity, and dimensionality. Examples of chemical properties include chemical composition.
[0131] By “continuous” it is meant a phase such that all points within the phase are directly connected, so that for any two points within a continuous phase there exists a path which connects the two points and does not leave the phase.
[0132] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0133] Compositions, Systems, and Methods
[0134] Disclosed herein are compositions, systems, and methods. For example, disclosed herein are compositions, systems, and methods for adaptive polymer electrolytes. For example, the disclosed subject matter relates to thin adaptive polymer interlayer for stabilizing lithium-metal interfaces in solid state batteries.
[0135] For example, described herein are adaptive polymer electrolytes comprising: a plurality of conductive polymer particles dispersed throughout a continuous polymer electrolyte matrix; wherein the adaptive polymer electrolyte exhibits an expansion response at room temperature under an applied electric field.
[0136] In some examples, the plurality of conductive polymer particles exhibit electrorheological properties under an electric field.
[0137] In some examples, the plurality of conductive polymer particles are provided in an amount below the percolation threshold.
[0138] In some examples, the plurality of conductive polymer particles are provided in an amount of greater than 0 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.1 wt.% or more, 0.25 wt.% or more, 0.5 wt.% or more, 0.75 wt.% or more, 1 wt.% or more, 1.25 wt.% or more, 1.5 wt.% or more, 1.75 wt.% or more, 2 wt.% or more, 2.5wt.% or more, 3 wt.% or more, 3.5 wt.% or more, or 4 wt.% or more). In some examples, the plurality of conductive polymer particles are provided in an amount of 5 wt.% or less (relative to the amount of main and additional monomers in the matrix) (e.g., 4.5 wt.% or less, 4 wt.% or less, 3.5 wt.% or less, 3 wt.% or less, 2.5 wt.% or less, 2 wt.% or less, 1.75 wt.% or less, 1.5 wt.% or less, 1.25 wt.% or less, 1 wt.% or less, 0.75 wt.% or less, 0.5 wt.% or less, or 0.25 wt.% or less). The amount of conductive polymer particles can range from any of the minimum values described above to any of the maximum values described above. For example, the plurality of conductive polymer particles can be provided in an amount of from greater than 0 to 5 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., from greater than 0 to 2.5 wt.%, from 2.5 to 5 wt.%, from greater than 0 to 1 wt.%, from 1 to 2 wt.%, from 2 to 3 wt.%, from 3 to 4 wt.%, from 4 to 5 wt.%, from greater than 0 to 4 wt.%, from greater than 0 to 3 wt.%, from greater than 0 to 2 wt.%, from 0.1 to 5 wt.%, from 0.25 to 5 wt.%, from 0.5 to 5 wt.%, from 1 to 5 wt.%, from 2 to 5 wt.%, from 3 to 5 wt.%, from 0.1 to 4 wt.%, or from 0.25 to 2 wt.%). In some examples, the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
[0139] In some examples, the plurality of conductive polymer particles are provided in an amount of greater than 0 vol% of the adaptive polymer electrolyte (e.g., 0.1 vol% or more, 0.5 vol% or more, 1 vol% or more, 1.5 vol% or more, 2 vol% or more, 2.5 vol% or more, 3 vol% or more, 3.5 vol% or more, 4 vol% or more, 4.5 vol% or more, 5 vol% or more, 6 vol% or more, 7 vol% or more, 9 vol% or more, 10 vol% or more, 11 vol% or more, 12 vol% or more, 13 vol% or more, 14 vol% or more, 15 vol% or more, 16 vol% or more, 17 vol% or more, 18 vol% or more, 19 vol% or more, 20 vol% or more, 21 vol% or more, 22 vol% or more, 23 vol% or more, 24 vol% or more, 25 vol% or more, 26 vol% or more, 27 vol% or more, or 28 vol% or more). In some examples, the plurality of conductive polymer particles are provided in an amount of 30 vol% or less of the adaptive polymer electrolyte (e.g., 29 vol% or less, 28 vol% or less, 27 vol% or less, 26 vol% or less, 25 vol% or less, 24 vol% or less, 23 vol% or less, 22 vol% or less, 21 vol% or less, 20 vol% or less, 19 vol% or less, 18 vol% or less, 17 vol% or less, 16 vol% or less, 15 vol% or less, 14 vol% or less, 13 vol% or less, 12 vol% or less, 11 vol% or less, 10 vol% or less, 9 vol% or less, 8 vol% or less, 7 vol% or less, 6 vol% or less, 5 vol% or less, 4.5 vol% or less, 4 vol% or less, 3.5 vol% or less, 3 vol% or less, 2.5 vol% or less, 2 vol% or less, 1.5 vol% or less, 1 vol% or less, or 0.5 vol% or less). The amount of conductive polymer particles in the adaptive polymer electrolyte can range from any of the minimum values described above to any of the maximum values described above. For example, the plurality of conductive polymerparticles are provided in an amount of from greater than 0 to 30 vol% of the adaptive polymer electrolyte (e.g., from greater than 0 to 15 vol%, from 15 to 30 vol%, from greater than 0 to 10 vol%, from 10 to 20 vol%, from 20 to 30 vol%, from greater than 0 to 25 vol%, from greater than 0 to 20 vol%, from greater than 0 to 5 vol%, from 0.1 to 30 vol%, from 1 to 30 vol%, from 5 to 30 vol%, from 10 to 30 vol%, from 0.1 to 25 vol%, from 0.5 to 20 vol%, or from 1 to 15 vol%). In some examples, the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 15 vol% of the adaptive polymer electrolyte.
[0140] In some examples, the plurality of conductive polymer particles comprise polypyrrole, polyaniline (PANI), poly(3,4-ethylenedi oxythiophene) (PEDOT), derivatives thereof, or combinations thereof. In some examples, the plurality of conductive polymer particles comprise polypyrrole. In some examples, the plurality of conductive polymer particles comprise polypyrrole doped with a dopant. In some examples, the plurality of conductive polymer particles comprise polypyrrole doped with dodecylbenzenesulfonate.
[0141] In some examples, the plurality of conductive polymer particles comprise polypyrrole doped with dodecylbenzenesulfonate and the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
[0142] In some examples, the continuous polymer electrolyte matrix is derived from a main chain polymer. Examples of main chain polymers include, but are not limited to polyethylene oxide (PEO), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), derivatives thereof, and combinations thereof. In some examples, the continuous polymer electrolyte matrix is derived from a main chain polymer comprising polyethylene oxide (e.g., PEO with a molecular weight of 100,000).
[0143] In some examples, the continuous polymer electrolyte matrix is further derived from a cross-linking monomer. Examples of cross-linking monomers include, but are not limited to, polyethylene glycol diacrylate (PEGDA) and tetraethyleneglycol diacrylate (TEGDA), tetraethylene glycol dimethacrylate (TEGDMA), derivatives thereof, and combinations thereon. In some examples, the continuous polymer electrolyte matrix is further derived from a crosslinking monomer comprising tetraethylene glycol dimethacrylate (TEGDMA).
[0144] In some examples, the continuous polymer electrolyte matrix is further derived from one or more salts, such as one or more lithium salts. Examples of lithium salts include, but are not limited to lithium bis(trifluoromethane)sulfonamide (LiTFSI), lithium bis(oxalate)borate (LiBoB), lithium hexafluorophosphate (LiPFe), lithium perchlorate (LiCIC ), lithiumtetrafluoroborate (LiBFfl, lithium nitrate (LiNCh), derivatives thereof, and combinations thereof. In some examples, the lithium salts comprise lithium bis(trifluoromethane)sulfonamide (LiTFSI), lithium bis(oxalate)borate (LiBoB), or a combination thereof.
[0145] In some examples, the continuous polymer electrolyte matrix is further derived from a plasticizer. Examples of plasticizers include, but are not limited to tetraethylene glycol dimethyl ether (TEGDME), succinonitrile (SN), derivatives thereof, and combinations thereof. In some examples, the continuous polymer electrolyte matrix is further derived from a plasticizer comprising tetraethylene glycol dimethyl ether (TEGDME).
[0146] In some examples, the continuous polymer electrolyte matrix is further derived from a photoinitiator, such as a UV-photoinitiator. Examples of photoinitiators include, but are not limited to, methylbenzophenone (MBP), methyl benzoylformate (MBF), 2,2-dimethoxy-2-phenyl acetophenone (DMPA), 2-hydroxy-2-methylpropiophenone (HMPP), derivatives thereof, and combinations thereof. In some examples, the continuous polymer electrolyte matrix is further derived from a photoinitiator comprising methylbenzophenone (MBP).
[0147] In some examples, the continuous polymer electrolyte matrix is derived from:
[0148] 20-40 wt.% (e.g., 30.3 wt.%) main chain polymer (e.g. PEO);
[0149] 10-20 wt.% (e.g., 15.1 wt.%) cross-linking monomer (e.g., TEGDMA);
[0150] 15-25 wt.% (e.g., 21.3 wt.%) Li Salt (e.g., 17.8 wt.% LITFSI and 3.5 wt.% LiBoB); 20-40 wt.% (e.g., 30.3 wt.%) plasticizer (e.g., TEGDME); and
[0151] 1-5 wt.% (e.g., 3.0 wt.%) photoinitiator (e.g., MBP);
[0152] wherein the sum adds to 100%.
[0153] In some examples, the continuous polymer electrolyte matrix is derived from:
[0154] 20-40 wt.% (e.g., 30.3 wt.%) PEO;
[0155] 10-20 wt.% (e.g., 15.1 wt.%) TEGDMA;
[0156] 15-25 wt.% (e.g., 21.3 wt.%) Li Salt (e.g., 17.8 wt.% LITFSI and 3.5 wt.% LiBoB); 20-40 wt.% (e.g., 30.3 wt.%) TEGDME; and
[0157] 1-5 wt.% (e.g., 3.0 wt.%) MBP;
[0158] wherein the sum adds to 100%.
[0159] In some examples, the continuous polymer electrolyte matrix is derived from: 30.3 wt.% PEO; 15.1 wt.% TEGDMA; 17.8 wt.% LITFSI; 3.5 wt.% LiBoB; 30.3 wt.% TEGDME; and 3.0 wt.% MBP.
[0160] In some examples, the adaptive polymer electrolyte has an ionic conductivity of 0.1 mS cm’1or more at 25°C (e.g., 0.15 mS cm’1or more, 0.2 mS cm’1or more, 0.25 mS cm’1or more, 0.3 mS cm’1or more, 0.35 mS cm’1or more, or 0.4 mS cm’1or more). In some examples, theadaptive polymer electrolyte has an ionic conductivity of 0.5 mS cm’1or less at 25°C (e.g., 0.45 mS cm’1or less, 0.4 mS cm’1or less, 0.35 mS cm’1or less, 0.3 mS cm’1or less, 0.25 mS cm’1or less, or 0.2 mS cm’1or less). The ionic conductivity of the adaptive polymer electrolyte can range from any of the minimum values described above to any of the maximum values described above. For example, the adaptive polymer electrolyte can have an ionic conductivity of 0.1 to 0.5 mS cm’1at25°C (e.g., from 0.1 to 0.3 mS cm’1, from 0.3 to 0.5 mS cm’1, from 0.1 to 0.2 mS cm’ from 0.2 to 0.3 mS cm’1, from 0.3 to 0.4 mS cm’1, from 0.4 to 0.5 mS cm’1, from 0.1 to 0.45 mS cm’1, from 0.1 to 0.4 mS cm’1, from 0.1 to 0.25 mS cm’1, from 0.15 to 0.5 mS cm’1, from 0.2 to 0.5 mS cm’1, from 0.25 to 0.5 mS cm’1, or from 0.15 to 0.45 mS cm’1). In some examples, the adaptive polymer electrolyte has an ionic conductivity of 0.1 to 0.25 mS cm’1(e.g., 0.11-0.16 mS cm’1) at 25°C.
[0161] In some examples, the adaptive polymer electrolyte exhibits an expansion response of greater than 0% strain at room temperature and an electric field strength of 0.3 V pm'1(e.g., 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, 3.5% or more, 4% or more, 4.5% or more, 5% or more, 5.5% or more, 6% or more, 6.5% or more, 7% or more, 7.5% or more, 8% or more, 8.5% or more, or 9% or more). In some examples, the adaptive polymer electrolyte exhibits an expansion response of 10% strain or less at room temperature and an electric field strength of 0.3 V pm'1(e.g., 9.5% or less, 9% or less, 8.5% or less, 8% or less, 7.5% or less, 7% or less, 6.5% or less, 6% or less, 5.5% or less, 5% or less, 4.5% or less, 4% or less, 3.5% or less, 3% or less, 2.5% or less, 2% or less, 1.5% or less, 1% or less, or 0.5% or less). The expansion response of the adaptive polymer electrolyte can range from any of the minimum values described above to any of the maximum values described above. For example, the adaptive polymer electrolyte can exhibit an expansion response of greater than 0% to 10% strain at room temperature and an electric field strength of 0.3 V pm'1(e.g., from greater than 0 to 5%, from 5 to 10%, from greater than 0 to 2%, from 2 to 4%, from 4 to 6%, from 6 to 8%, from 8 to 10%, from greater than 0 to 8%, from greater than 0 to 6%, from greater than 0 to 4%, from 0.1 to 10%, from 1 to 10%, from 2 to 10%, from 4 to 10%, from 6 to 10%, from 0.1 to 9.5%, from 1 to 9%, or from 2 to 8%). In some examples the adaptive polymer electrolyte exhibits an expansion response of 6% strain at room temperature and an electric field strength of 0.3 V pm'1
[0162] In some examples, the adaptive polymer electrolyte is a free-standing film.
[0163] In some examples, the adaptive polymer electrolyte has an average thickness of 50 nanometers or more (e.g., 75 nanometers or more, 100 nanometers or more, 125 nanometers or more, 150 nanometers or more, 200 nanometers or more, 250 nanometers or more, 300nanometers or more, 350 nanometers or more, 400 nanometers or more, 450 nanometers or more, 500 nanometers or more, 600 nanometers or more, 700 nanometers or more, 800 nanometers or more, 900 nanometers or more, 1 micrometer or more, 2 micrometers or more, 3 micrometers or more, 4 micrometers or more, 5 micrometers or more, 6 micrometers or more, 7 micrometers or more, 8 micrometers or more, 9 micrometers or more, 10 micrometers or more, 15 micrometers or more, 20 micrometers or more, 25 micrometers or more, 30 micrometers or more, 35 micrometers or more, 40 micrometers or more, or 45 micrometers or more). In some examples, the adaptive polymer electrolyte has an average thickness of 50 micrometers or less (e.g., 45 micrometers or less, 40 micrometers or less, 35 micrometers or less, 30 micrometers or less, 25 micrometers or less, 20 micrometers or less, 15 micrometers or less, 10 micrometers or less, 9 micrometers or less, 8 micrometers or less, 7 micrometers or less, 6 micrometers or less, 5 micrometers or less, 4 micrometers or less, 3 micrometers or less, 2 micrometers or less, 1 micrometer or less, 900 nanometers or less, 800 nanometers or less, 700 nanometers or less, 600 nanometers or less, 500 nanometers or less, 450 nanometers or less, 400 nanometers or less, 350 nanometers or less, 300 nanometers or less, 250 nanometers or less, 200 nanometers or less, 150 nanometers or less, 125 nanometers or less, or 100 nanometers or less). The average thickness of the adaptive polymer electrolyte can range from any of the minimum values described above to any of the maximum values described above. For example, the adaptive polymer electrolyte can have an average thickness of from 50 nanometers to 50 micrometers (e.g., from 50 nanometers to 500 nanometers, from 500 nanometers to 5 micrometers, from 5 micrometers to 50 micrometers, from 50 nanometers to 25 micrometers, from 50 nanometers to 10 micrometers, from 50 nanometers to 10 micrometers, or from 50 nanometers to 5 micrometers). In some examples, the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 25 micrometers. In some examples, the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 10 micrometers. In some examples, the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 5 micrometers.
[0164] In some examples, the adaptive polymer electrolyte is substantially stable over 5 or more cycles (e.g., 50 or more cycles, or 100 or more cycles).
[0165] Also disclosed herein are methods of use of any of the adaptive polymer electrolytes disclosed herein. In some examples, the method comprises using the adaptive polymer electrolyte as an interlayer between lithium-metal electrode (e.g., Li-metal anode) and solid electrolyte in a lithium metal solid-state battery.
[0166] Also disclosed herein are articles of manufacture comprising any of the adaptive polymer electrolytes disclosed herein. In some examples, the article comprises a lithium metal solid-statebattery.
[0167] Also disclosed herein are methods of making any of the adaptive polymer electrolytes disclosed herein. In some examples, the method comprises:
[0168] combining the continuous polymer electrolyte matrix precursors and the plurality of conductive polymer particles to form a mixture;
[0169] stirring the mixture for 4 -24 hours (e.g., 8-12 hours or overnight) at room temperature; subsequently ultrasonicating the mixture for 1 minute to 30 minutes (e.g., 10 minutes); subsequently hot pressing the mixture (e.g., 80°C, 4.4 bar, 10 minutes); and subsequently UV-polymerizing the mixture (e.g., 150 mW / cm2, 10 minutes).
[0170] In some examples, the method further comprises subsequently vacuum drying the UV-polymerized mixture (e.g., 40°C, overnight).
[0171] In some examples, the method further comprises making the plurality of conductive polymer particles.
[0172] A number of embodiments of the invention have been described. Nevertheless, it will be understood that various modifications may be made without departing from the spirit and scope of the invention. Accordingly, other embodiments are within the scope of the following claims.
[0173] The examples below are intended to further illustrate certain aspects of the systems and methods described herein, and are not intended to limit the scope of the claims.
[0174] EXAMPLES
[0175] The following examples are set forth below to illustrate the methods and results according to the disclosed subject matter. These examples are not intended to be inclusive of all aspects of the subject matter disclosed herein, but rather to illustrate representative methods and results. These examples are not intended to exclude equivalents and variations of the present invention which are apparent to one skilled in the art.
[0176] Efforts have been made to ensure accuracy with respect to numbers (e.g., amounts, temperature, etc.) but some errors and deviations should be accounted for. Unless indicated otherwise, parts are parts by weight, temperature is in °C or is at ambient temperature, and pressure is at or near atmospheric. There are numerous variations and combinations of measurement conditions, e.g., component concentrations, temperatures, pressures and other measurement ranges and conditions that can be used to optimize the described process.
[0177] Example 1 - Thin Adaptive Polymer Interlayer for Stabilizing Lithium-Metal Interfaces in Solid State Batteries
[0178] The energy density and safety of lithium-metal solid-state batteries (LIMSSBs) are limited by the stability of the interface between the lithium-metal anode and the solid-stateelectrolyte. Traditional approaches using static interlayers or coatings often fail to maintain continuous contact during cycling, particularly when voids form due to non-uniform lithium plating / stripping.
[0179] A previous advancement (M. Newman et al. “Design and Characterization of an Adaptive Polymer Electrolyte for Lithium Metal Solid-State Battery Applications”. Journal of Materials Chemistry A, 13, 7914-7928 (2025). DOI: 10.1039 / d4ta08556f), introduced an adaptive polymer electrolyte that exhibits expansion under relatively low electric field strengths (-0.1-0.3 V / pm), attributed to the polarization and alignment of conducting polymer (CP) particles (specifically PPy(DBS)) within an insulating and ion-conducting polymer matrix. That work, however, focused on bulk, free-standing films (-125 pm), unsuitable for practical integration in battery cells due to their thickness and mechanical limitations.
[0180] The interlayers described herein build upon the prior adaptive polymer electrolyte by developing a thin, conformal adaptive polymer interlayer (<10 pm). This interlayer:
[0181] 1. Retains the adaptive behavior — expansion under an electric field via conducting polymer particle polarization.
[0182] 2. Minimizes thickness to reduce impedance and preserve energy density.
[0183] 3. Ensures strong interfacial adhesion to ceramic electrolytes via an innovative synthesis process.
[0184] The thin polymer film is synthesized directly on bulk ceramic solid electrolyte via hot-pressing the polymer precursor solution followed by UV polymerization. An important aspect to achieve the thin polymer film on the ceramic solid electrolyte comprises replacing the polyethylene terephthalate (PET) cover sheet during synthesis with a fluorinated ethylene propylene (FEP) cover sheet. This FEP cover sheet enabled synthesis of a thin polymer film (<10 pm) on the ceramic solid electrolyte without the film being delaminated during removal of the cover sheet following UV polymerization.
[0185] This new approach enables successful integration of the adaptive interlayer into prototype LIMSSB cells, achieving average thicknesses as low as 5 pm and maintaining mechanical stability during synthesis and assembly.
[0186] Example 2 - Real-Time Optimal Design of Experiment for Parameter Identification of Li-Ion Cell Electrochemical Model
[0187] Abstract. Accurately identifying the parameters of electrochemical models of Li-ion battery (LiB) cells is a critical task for enhancing the fidelity and predictive ability. Traditional parameter identification methods often require extensive data collection experiments and lack adaptability in dynamic environments. This paper describes a Reinforcement Learning (RL)based approach that dynamically tailors the current profile applied to a LiB cell to optimize the parameters identifiability of the electrochemical model. The proposed framework is implemented in real-time using a Hardware-in-the-Loop (HIL) setup, which serves as a reliable testbed for evaluating the RL-based design strategy. The HIL validation confirms that the RL-based experimental design outperforms conventional test protocols used for parameter identification in terms of both reducing the modeling errors on a verification test and minimizing the duration of the experiment used for parameter identification.
[0188] Introduction. Lithium-ion batteries (LiBs) have become indispensable across diverse industrial sectors, being the energy storage solution of choice for applications spanning consumer electronics, electric vehicles, and grid-level energy storage. Accurate modeling and testing of LiBs are critical for optimizing their performance, ensuring safety, and extending their operational life. Historically, research in this domain has prioritized the development of physicsbased electrochemical models and estimation algorithms. However, recent studies underscore the importance of parameter identification and model calibration, including the design of appropriate experiments, data collection and post-processing to facilitate such tasks (Andersson et al., 2022).
[0189] Among emerging methodologies in this field, Optimal Experimental Design (OED) has gained prominence for its ability to enhance parameter identifiability by maximizing Fisher Information (FI) for specific parameters over a defined time horizon (Huang et al., 2023b). OED provides a systematic framework to identify operating conditions and excitation inputs that yield the most informative data for parameter calibration. As shown by (Lopez C et al., 2016) only a small number of parameters can be identified from conventional characterization tests such as constant discharge experiments while parameters like the rate constant in the anode are left unidentifiable. OED addresses these limitations by tailoring input profiles to ensure maximum informativeness for parameter estimation.
[0190] Despite its advantages, conventional OED methods face several challenges. For instance, input profiles are often selected from predefined libraries, which may exclude truly optimal designs. Convex programming approaches, as described in (Park et al., 2018), optimize FI but are limited by the constraints of the predefined library, potentially overlooking profiles that excite the battery in conditions most conducive to parameter identifiability. Iterative optimization schemes, such as those proposed by (Pozzi et al., 2019), risk failing to converge to an optimal design due to computational limits. The widely used D-optimal design approach maximizes the determinant of the FI matrix but assumes linearity (Mathieu et al., 2017), a limitation when dealing with the nonlinear behavior of high-fidelity electrochemical models (Chhajer and Roy,To address these gaps, reinforcement learning (RL) has emerged as a promising tool for designing adaptive excitation policies that optimize data collection in real-time (Huang et al., 2023a). By dynamically tailoring input profiles during experimentation, RL-based OED can improve parameter identifiability while reducing the computational burden and duration of the identification process. However, most studies to date have been confined to simulations, limiting their applicability to real-world scenarios (Taylor et al., 2019).
[0191] An RL framework was integrated into a hardware-in-the-loop (HIL) environment to perform online OED. The experimental procedure to estimate a rate constant parameter in a LiB electrochemical model is described. Unlike conventional characterization methods, such as constant-current discharges or relaxation current interrupt discharge (RCID) tests, the proposed approach dynamically adapts the input excitation to maximize the informativeness of collected data. This innovation enables improved parameter identifiability while reducing the duration and computational burden of the identification process.
[0192] HIL validation was leveraged to bridge the gap between simulation and real-world experimentation. While simulations offer valuable insights, they often fail to fully account for real-world factors such as manufacturing inconsistencies, degradation mechanisms, or measurement errors (Taylor et al., 2019). By implementing OED in a physical HIL environment, a robust evaluation platform for LiB parameter identification methods is provided, supporting applications ranging from state of charge (SOC) estimation (Guo et al., 2019) to battery management system (BMS) verification (Bui et al., 2019).
[0193] A reduced-order enhanced single-particle model (ESPM) is used to guide the OED process, serving as a benchmark against which experimental results are evaluated (Seals et al., 2022). By comparing RL-based OED with conventional testing protocols, the potential for significant improvements in both parameter identifiability and experimental efficiency is demonstrated.
[0194] Experimental Setup. The HIL environment for online OED validation was configured using Math Works and dSPACE tools in conjunction with an Elektro Automatik (EA) Cycler. More specifically, Simulink was used to initialize the test procedure which was ran through dSPACE ControlDesk. The analog signals defining the set and measured voltage and current values were used to control charge and discharge current of the cycler. A schematic of this flow of information can be seen in FIG. 71, where Power Commands represented the voltage and current commands delivered to the cell cycler, EA Data Acquisition included the measured current values, Power Cable indicated the current supply to the battery, and Voltage Measurement was applied directly at the battery tabs to increase resolution and minimize sourcesof error. The measured voltage and current was fed into a data-driven State Estimator in Simulink. The estimator provided the normalized lithium surface concentration in the cathode cSe,p, which was required by the RL agent along with the measured terminal voltage.
[0195] Problem Formulation. Consider a nonlinear, single-input, single-output discrete time system:
[0196] Xk+1 = fk(Xk'Uk,&) (El)
[0197] yk= gk(xk>uk> ®) (2.1)
[0198] where xkdenotes the states, ukis the input, ykthe voltage output, and 0 = {91, 92, 93, ..., 9m} the entire set of model parameters, including known parameters and parameters that need to be identified. Without loss of generality, consider the case of single parameter identification, 0 = 9. The objective of OED is to define the input sequence
[0199]
[0200] u2, . . . , uNover a finite time horizon N that maximizes the information content of the parameter 9 on the output yk, which is achieved by optimizing the FI (Scharf and McWhorter, 1993):
[0201] 2
[0202] (3.1)
[0203]
[0204] Uy \ OXj /
[0205] where < y denotes the variance of the output measurement noise. In the context of LiB cell model calibration, maximizing FI implies optimizing the input current profile to enhance the sensitivity of the voltage output to the parameter (Huang et al., 2922). The OED problem can be formulated as:
[0206] N2
[0207] max y / dyk\
[0208] u-1, a2, . . . , \ dQ J
[0209]
[0210] k=l
[0211] s.t. Xk+1= fk(xk,uk, 0) (4.1)
[0212] yk= gk(xk,uk, Q)
[0213] The OED problem required the physics-based LiB model to compute the states, output and sensitivity of the voltage output ykto the target parameter 9.
[0214] Overview of Li-ion Cell Model Equation. The electrochemical model of a 39 Ah NMC-graphite cell was leveraged for automotive applications. A reduced-order electrochemical equivalent circuit model (E-ECM) was previously developed and compared against a high-fidelity physics-based model of the same cell (Seals et al., 2922). The benefit to utilizing the E-ECM compared to other electrochemical models is that it reduces the computation time for simulation.
[0215] A summary of the governing equations for the E-ECM is provided below, while a more in-depth study of the framework can be found in (Seals et al., 2922). The terminal voltage V of the E-ECM comprises seven terms:V(t) Up^CSetpr se,n> (5-1)
[0216]
[0217] "I" Y]n\C se,n>f) + <Pdiff(7) + 0 ion (t) - / (t) / ?cthe first two terms, Upand Un, are the half-cell open circuit potentials of the cathode and anode, which are nonlinear functions of the lithium surface concentration, cse i, i =p, / / , in each electrode. The terms, i]j, define the kinetic overpotential of each electrode at the solid-electrolyte interface, computed through a linearized Butler- Volmer reaction kinetic equation. The overpotentials in the electrolyte due to diffusion and ionic conductivity are represented by the terms (paiff and ton, respectively. The Rcrepresents the contact resistance at the current collectors. Last, the surface concentration dynamics (6.1) was predicted by a linear system, obtained via Pade approximation of the diffusion partial differential equations (PDEs) describing the transport of lithium in the solid phase (Seals et al., 2022):
[0218] —^-se,iO T \Gb(7) T Gd(s)JAI(s) (6 1)
[0219] 3 5£>j
[0220] Gb(s) = Gd(s) = (7.1)
[0221]
[0222] where Gbs) represents the bulk concentration dynamics and Gd(s)the diffusion dynamics, A) is the particle radius and
[0223]
[0224] denotes the diffusion coefficient, a parameter assumed known.
[0225] Calculation of Parameter Sensitivity. Because the Li-ion cell model is physics-based, hence described fully by analytical equations, the sensitivity of the terminal voltage in (5.1) to a given parameter was assessed by symbolically computing the first-order partial derivative with respect to that parameter. The parameter considered as a case study to illustrate the OED procedure was the anode rate constant (fcn). This parameter is useful for accurately capturing the dynamic behavior of the electrochemical model (Dangwal and Canova, 2021). The sensitivity of the cell voltage to the parameter knis given by:
[0226]
[0227] \ 3 k, / \ 3 k, / \ 3kj / \ 3k, / \ 3k, / \ 3k; / \ 3k; / \ / which, after simplification, becomes:
[0228] dVXt) _ dT]n(t) dion(t) . .
[0229]
[0230] 3kndi-on 3kn
[0231] where rji represents the kinetic overpotential and ioidenotes the exchange current density. See (Seals et al., 2022) for the definitions of rji and ioi. Substituting the analytical expressions for each PDE the sensitivity to kncan be expressed as:
[0232]
[0233] / Wh=(RTMtp ((J. _ 1_E^\ r 7 _ X \\n nk 3k„ J Fi^nP[ \TrefT(t) R JrylCse,n^max,n he.nh H O
[0234]
[0235] where Jnrepresents the intercalation current density at the anode, Eo^denotes the activation energy associated with the anode, cmax nis the maximum surface concentration in the anode, ceindicates the electrolyte concentration, and Tref specifies the reference temperature.
[0236] Optimal experimental design with reinforcement learning. The Twin Delayed Deep Deterministic Policy Gradient (TD3) algorithm, an advanced actor-critic Deep RL (DRL) method, was employed to optimize input excitation in LiBs. TD3, an enhancement of the Deep Deterministic Policy Gradient (DDPG) algorithm, was chosen for its improved stability and effectiveness in continuous action spaces, making it useful for this application (Fujimoto et al., 2018). The problem of generating optimal input excitation is modeled as a Markov Decision Process (MDP), where the states (5) are defined by measurable or estimable quantities. The measured cell terminal voltage (F) and the estimated normalized lithium surface concentration in the cathode (cse p) were assumed as the states for the model. The goal was to determine an optimal control policy, 7t( |A> that maximizes the reward function ( / ), mapping states s to action (a), where a represents the electrical current. RL learns this policy by exploring the state-action space and solving the Bellman Equation. The Bellman Equation evaluates the value of a state 5 by combining immediate rewards with discounted future rewards, guiding the optimization process. The Q-function is defined as:
[0237] Q(s|a) = ^5|^[rt + S”=iKfcrt+fc| st+1,at+1], (11.1)
[0238]
[0239] evaluates the joint desirability of a state-action pair under a given policy 7t(5|a), where y is the discount factor and rt+krepresents the reward at time t + k.
[0240] The TD3’s actor-critic structure consists of two networks: the actor network, which learns the policy 7t(5|a), and the critic network, which estimates Q-values. The reward function is designed with two components. The first term maximizes the normalized FI for the selected parameter, while the second term penalizes any constraint violation on the cell voltage. The single-step reward is given as:
[0241] (dvklc\2
[0242] r
[0243]
[0244] k={M,kn n' , normal condition (12.1)
[0245] constraint violation.
[0246] Each training episode begins at 100% SOC and either concludes after 1800 steps or terminates early if constraints are violated. A step size of 1 second was applied, with training conducted over 1,000 to 5,000 episodes.
[0247] The TD3 algorithm was trained using MATLAB’s RL toolbox. Table 1 details the operating conditions of the simulated battery system and penalties for constraint violations.Table 1. TD3 model parameters and settings.
[0248] Parameter Value
[0249] Current Input Range [-2C, -5C]
[0250] Voltage Output Range [2.8 V, 4.2 V]
[0251] Penalty for Constraint Violation M -5
[0252] Simulation Length and Time Step 1800 s and 1 s
[0253]
[0254] Data-driven state estimator. A data-driven identification approach was used to create an estimator of the normalized lithium surface concentration in the cathode cse p, which is required as a state by the RL agent. This approach was warranted by the need to achieve a generally applicable procedure that could be applied even if the plant model is unknown. The method used to synthesize the data-driven model was based on a sparse identification of nonlinear dynamics with control (SINDYc) (Brunton et al., 2016), which constructs a dynamic model as follows:
[0255] C
[0256]
[0257] se,p[k +!] = (13-1)
[0258] where 0 E Rnxmrepresents the basis functions of the predicted model, and S, G Rmis the sparse coefficient vector. The S, vector is determined by a sequentially thresholded ridge (STRidge) regression technique (14), where i and Aa represent the regularization parameter and sparsification knob, respectively. The selection of these hyperparameters and the library functions 0 was achieved through a hybrid sparse learning approach, as outlined in (da Silva et al., 2024).
[0259] = arg 11 cse p[k + 1] - 0(cseip[fc],V[fc],I[fc]X||2
[0260]
[0261] +^IIKII2s
[0262]
[0263] .t.: |£| < A2(14.1) The current profile used in the training dataset is shown in FIG. 72. This profile was generated by simulating the battery cell under various current cycles. To avoid over discharge, a constant charging current was applied between each cycle. Validation of the model was performed by using current-voltage data corresponding to the regulatory UDDS, HWFET, US06 and WLTC driving cycles. FIG. 73 illustrates the model’s performance on the training dataset, achieving an R2 value of 0.9987 and a mean squared error (MSE) of 1.16 / IO4Similarly, as shown in FIG.
[0264] 74, the model effectively captures the cse pdynamics during validation, with an R2 value of 0.9951 and an MSE of 4.28 / IO4. As detailed in the following section, the data-driven estimator closes the loop in the HIL framework by providing the state estimate cse pthat is fed back to the RL agent.Implementation, results and analysis. As mentioned above, the focus of this study is to demonstrate the process of OED for the parameter kn, facilitated through an RL agent that makes decisions in real-time through a HIL framework with a battery cell in the loop.
[0265] FIG. 75 illustrates the results of the experimental test, including the input current, battery SOC (calculated via Coulomb counting) and measured cell terminal voltage, which were useful for understanding the system’s behavior under the designed conditions. In the high SOC region, the lithium concentration within the anode was significant, nearing its upper boundary as the SOC approaches 100%. This results in increased voltage sensitivity to variations in kn, making this region highly informative for calibrating kn. The RL agent identifies this high-sensitivity operating condition from and guides the battery to operate predominantly in this region. The resulting excitation, as evident from the applied current and corresponding voltage fluctuations in the figure, was designed to extract the maximum information relevant to kn.
[0266] Parameter identification analysis. After collecting the data using the HIL setup, an offline parameter identification process was conducted to compare the current profile generated via the RL-based OED to a set of conventional test cycles commonly used in battery testing, including 1C and 5C constant current discharging tests and RCID (Hu et al., 2011). The problem of parameter identification was addressed as a model-free constrained optimization, where a Bayesian optimization method (Pi et al., 2024) was applied to minimize the squared error between experimental voltage measurements and the E-ECM voltage output starting from an arbitrary initial value of the parameter kn. The optimization problem is expressed as follows:
[0267] e; = ■ Vt(et,ik))2(15 1)
[0268]
[0269] The constraint set 0 for knwas defined as [2 1011, 1 x 10x] and the evenly distributed ten initial guesses for knfrom this set were considered in the optimization process.
[0270] To validate the effectiveness of the identification process, a drive cycle from (Pi et al., 2024) was considered as the verification test. This involves using the identified parameter knfrom each experimental design to predict the battery’s voltage response under a realistic drive cycle. The predicted voltage was then compared against the experimental voltage measurements, and the median of the prediction errors across the drive cycle was calculated.
[0271] To illustrate the results, FIG. 76 shows a box plot computing the prediction errors across all tests, providing an overview of the variability and consistency in the prediction errors for each experimental design. The variation in errors was minimal across all tests, indicating that the Bayesian optimization process consistently converges to the same value regardless of the initial guesses. This consistency demonstrates the robustness of the Bayesian optimization method inparameter identification. The median values of these verification errors, as derived from the box plot, are listed in Table 2 for a more detailed comparison.
[0272] The results in Table 2 highlight the effectiveness of different current profiles for parameter identification, with the profile obtained from the RL-based OED demonstrating a strong balance between accuracy and test duration. The lowest drive cycle verification error (12.32 mV) was achieved, along with a high FI of 0.08 V2, all within a short experiment duration of 1800 s. This reflects the ability of the RL-based OED to effectively excite the parameter knwhile being time-efficient. The RCID profile, while requiring a much longer experiment duration (~ 28 hrs), achieved the highest FI (0.42 V2) and a similarly low verification error (13.33 mV), making it a robust but time-intensive approach. Traditional fixed profiles, such as 1C and 5C Discharge, exhibited higher verification errors (47.98 mV and 47.31 mV, respectively) and lower FI values (0.01 V2and 0.05 V2), demonstrating their limitations in sufficiently exciting fcn., thereby producing data set that were less useful for accurate parameter identification. These results underscore the RL-HIL’s capability to deliver highly accurate parameter identification in a time-efficient manner while also showing that RCID remains a strong method for scenarios where experiment duration is less critical.
[0273] Conclusion. The importance of optimizing the input excitation to generating data sets for parameter identification was demonstrated by the favorable results of the RL agent’s OED. By maximizing the FI for a specific parameter over the duration of a 1800-second experiment, an optimal experiment design can be generated online by the reinforcement learning agent in real time. In a 30-minute experiment, the RL-based OED produced data containing high levels of parameter identifiability.
[0274] This result was confirmed by utilizing the generated data set for parameter identification via minimization of the output error. The results indicate that the test profile generated by the RL-based OED leads to significantly lower voltage RMSE than conventional constant current discharge tests and is on par with the efficacy of a 28 hr RCID test. By utilizing optimal experimental design, accurate parameter estimation can be achieved in a fraction of the time it would normally take to get values that result in such low errors. As an extension, the proposed framework can be applied to generate OEDs for other model parameters or groups of parameters altogether.Table 2. Parameter identification results for various experimental designs, showing the FI, drive cycle verification error (median), and experiment length for each test.
[0275] Current FI Drive Cycle Verification Error (Median) Experiment Length Profile [V2] [mV] [s]
[0276] 1C Discharge 0.01 47.98 3781
[0277] 5C Discharge 0.05 47.31 701
[0278] RCID 0.42 13.33 103333
[0279] RL-HIL 0.08 12.32 1800
[0280]
[0281] References
[0282] Andersson, M. et al. (2022). Parametrization of physics-based battery models from input-output data: A review of methodology and current research. Journal of Power Sources, 521, 230859.
[0283] Brunton, S.L. et al. (2016). Sparse identification of nonlinear dynamics with control (SINDYc). IFAC-PapersOnLine, 49(18), 710-715. 10th IFAC Symposium on Nonlinear Control Systems NOLCOS 2016.
[0284] Bui, T.M.N. et al. (2019). An advanced hardware-in-the-loop battery simulation platform for the experimental testing of battery management system. In 201923rd International Conference on Mechatronics Technology (ICMT), 1-6.
[0285] Chhajer, H. and Roy, R. (2024). Rationalised experiment design for parameter estimation with sensitivity clustering. Scientific Reports, 14(1).
[0286] da Silva, S.F. et al. (2024). Improving low-fidelity models of li-ion batteries via hybrid sparse identification of nonlinear dynamics. arXiv preprint.
[0287] Dangwal, C. and Canova, M. (2021). Parameter identification for electrochemical models of lithium-ion batteries using sensitivity analysis. ASME Letters in Dynamic Systems and Control, 1(4), 041014.
[0288] Fujimoto, S. et al. (2018). Addressing function approximation error in actor-critic methods. In International conference on machine learning, 1587- 1596. PMLR.
[0289] Guo, L. et al. (2019). Lithium-ion battery soc estimation and hardware-in-the-loop simulation based on ekf. Energy Procedia, 158, 2599-2604. Innovative Solutions for Energy Transitions.
[0290] Hu, Y. et al. (2011). Electro-thermal battery model identification for automotive applications. Journal of Power Sources, 196(1), 449-457.
[0291] Huang, R. et al. (2022). Input excitation optimization for estimating batteryelectrochemical parameters using reinforcement learning. In 2022 IEEE Vehicle Power and Propulsion Conference (VPPC), 1-6.
[0292] Huang, R. et al. (2023a). Reinforcement learning of optimal input excitation for parameter estimation with application to li-ion battery. IEEE Transactions on Industrial Informatics, 19(11), 11160- 11170.
[0293] Huang, R. et al. (2023b). Excitation optimization for estimating battery health parameters using reinforcement learning considering information content and bias. In 2023 American Control Conference (ACC), 3093-3098. IEEE.
[0294] Lopez C et al. (2016). A computational framework for identifiability and ill-conditioning analysis of lithium-ion battery models. Industrial & Engineering Chemistry Research, 55(11), 3026-3042.
[0295] Mathieu, R. et al. (2017). D-optimal design of experiments applied to lithium battery for ageing model calibration. Energy, 141, 2108-2119.
[0296] Park, S. et al. (2018). Optimal experimental design for parameterization of an electrochemical lithium-ion battery model. Journal of The Electrochemical Society, 165(7), A1309.
[0297] Pi, J. et al. (2024). Parameter identification for electrochemical models of lithium-ion batteries using bayesian optimization. arXiv preprint arXiv:2405.10750.
[0298] Pozzi, A. et al. (2019). Optimal design of experiments for a lithium-ion cell: Parameters identification of an isothermal single particle model with electrolyte dynamics. Industrial & Engineering Chemistry Research, 58(3), 1286-1299.
[0299] Scharf, L.L. and McWhorter, L.T. (1993). Geometry of the cramer-rao bound. Signal Processing, 31(3), 301-311.
[0300] Seals, D. et al. (2022). Physics-based equivalent circuit model for lithium-ion cells via reduction and approximation of electrochemical model. SAE International Journal of Advances and Current Practices in Mobility, 4(2022-01- 0701), 1154-1165.
[0301] Taylor, J. et al. (2019). An insight into the errors and uncertainty of the lithium-ion battery characterisation experiments. Journal of Energy Storage, 24, 100761.
[0302] Example 3 - Design and characterization of an adaptive polymer electrolyte for lithium metal solid-state battery applications
[0303] Abstract. A challenge for Li-metal solid-state batteries (LIMSSBs) lies in the mechanical degradation of the solid interface between Li-metal and the solid electrolyte. This work focuses on the synthesis and electrochemomechanical characterization of an adaptive polymer electrolyte (A-PE) that could potentially be applied as an interlayer to stabilize theinterfacial contact between the lithium metal anode and the solid electrolyte, mitigating the effects of void formation leading to contact loss. The A-PE operates based on the principle of utilizing the polarization of conducting polymer particles, polypyrrole doped with dodecylbenzenesulfonate (PPy(DBS)), to impart adaptive properties to a polymer electrolyte matrix. The A-PE was synthesized via hot pressing and subsequent UV polymerization resulting in free-standing films with various amounts of PPy(DBS) and ionic conductivities in the range of 0.11-0.16 mS / cm at 25 °C. Film characterizations included insoluble fraction, mechanical response under electric field, and Li symmetric cycling with intermittent electrochemical impedance spectroscopy (EIS). The measured mechanical responses of the film were expansion with atomic force microscopy (AFM) and block force response by exciting the film with electric field of variable strength. The results obtained suggest that the addition of PPy(DBS) particles provides adaptive capability in polymer electrolytes at room temperature (20-25 °C), with an expansion response of up to 6% strain with 1 wt% PPy(DBS) at an electric field strength of 0.3 V / pm. The results indicate that the A-PE shows promise for application as an interlayer in LIMSSBs, with the potential to reduce mechanical degradation at the lithium metal-solid electrolyte interface and enhance durability by expanding to maintain contact with the lithium metal anode.
[0304] Introduction. With the rising demand for high energy density Li-ion batteries for electric vehicles and grid storage applications, solid-state electrolytes offer improved safety due to their non-flammability and the opportunity to enable the use of a lithium anode in Li-metal solid-state batteries (LIMSSBs). This technology could result in gravimetric and volumetric energy density gains of up to 40% and 70%, respectively, compared to conventional Li-ion batteries [Al], On the other hand, the solid-solid anode-electrolyte interface in LIMSSBs has been recognized as one of the limiting factors for the performance and durability, due to various mechanical and electrochemical challenges [A1-A6], Mechanically, a rigid lithium metal-solid electrolyte interface cannot maintain sufficient contact due to the large volume and morphology change of the Li-metal anode from repeated Li stripping and plating during cell operation. Contact loss and Li filament growth has been shown to short the cell, except in cases of unrealistically high stack pressure forcing the interface to maintain contact [A3, A6-A10], Electrochemically, ceramic solid electrolytes are not stable at the low potential conditions that occur when direct contact with Li-metal is established, which can necessitate the use of a protective layer or interlayer [A4, A5],
[0305] To address these challenges, solutions such as engineered interfaces, polymer / ceramic composite solid electrolytes, or polymer interlayers have been proposed to improve the initialinterface, provide flexibility to accommodate some of the volume change of the Li-metal anode, and increase the electrochemical stability [Al 1-A20], Composite solid electrolytes may compromise on ionic conductivity through the entire separator thickness as the polymer electrolyte component typically has lower ionic conductivity than ceramic solid electrolytes [A14-A17], Polymer interlayers can offer similar benefits of flexibility and electrochemical stability without compromising on ionic conductivity through the whole separator thickness but instead through a thin interlayer thickness [A18-A20], However, these solutions have limited ability to maintain the interfacial contact in the event of non-uniform Li stripping and plating, and long-term stability is not guaranteed as contact loss can cause the cell to eventually fail.
[0306] An adaptive polymer electrolyte (A-PE) was designed to offer self-adaptive capabilities at room temperature (20-25 °C). The A-PE is envisioned as an interlayer between the Li-metal anode and the solid electrolyte, where it could help maintain interfacial contact in the event of partial contact loss. A conceptual representation of the A-PE working principles and its potential future role as an interlayer is shown in FIG. 1. It is suggested that the A-PE could expand under an electric field present in a battery to maintain interfacial contact with the anode. As long as some contact is maintained, the electric field across the interlayer would induce expansion to restore interfacial integrity. This approach could improve durability and safety of the battery. This adaptive behavior is imparted by the polarization of conducting polymer (CP) particles, which exhibit electrorheological (ER) properties under an electric field. The mobility of electrons in CPs allow the particles to polarize and align along the field at relatively low electric field strengths [A21-A25], While ER properties are well studied in fluids, research on ER polymers or elastomers has focused on the change in storage modulus under an electric field rather than on deformation or expansion responses [A26-A29], A comprehensive electrochemomechanical characterization is described of an A-PE envisioned for application in Li-metal solid-state batteries. Unlike traditional approaches to enhancing lithium metal solid-state batteries, the A-PE uniquely leverages the polarization of CP particles in a solid polymer matrix, providing a mechanical response under relatively low electric field strengths.
[0307] An experimental evaluation was conducted of the A-PE's physical, electrochemical, and mechanical properties. Physical characterizations include insoluble fraction and electrical conductivity measurements, X-ray diffraction (XRD), differential scanning calorimetry (DSC), and dynamic mechanical analysis (DMA). Mechanical response characterizations are conducted using atomic force microscopy (AFM) and block force measurements to demonstrate the adaptive property through expansion and force response under applied electric fields.
[0308] Electrochemical characterizations encompass electrochemical impedance spectroscopy (EIS),Li-Li symmetric cycling, and electrochemical stability window (ESW) measurements. These results establish the A-PE’s potential as a promising interlayer material for LIMSSB, with the possibility of mitigating interfacial degradation and enhancing battery performance.
[0309] Adaptive Polymer Electrolyte Synthesis Process. Polypyrrole doped with dodecylbenzenesulfonate (PPy(DBS)) is the CP used in this example for its polarization under an electric field in the polymer electrolyte. While other types of CPs can exhibit similar properties, polypyrrole (PPy) was chosen for this work because PPy-based materials have been reported to respond to low electric field strengths of 0.1 V / pm or less [A22, A24, A26], Doping PPy can increase the mobility of electrons for polarization of the particles. Dodecylbenzenesulfonate (DBS') was used as a large, immobile dopant (compared to smaller dopants that can migrate from the CP) and has also been shown to improve stability of PPy [A30, A31], However, a limitation with the addition of CPs is the electrical conductivity that provides CPs (such as PPy(DBS)) this property can make a composite (with an insulative matrix) electrically conductive at a high enough CP filler loading, known as the percolation threshold. The percolation threshold widely varies depending on the properties of the electrically conductive filler (such as size, morphology, aspect ratio), insulative matrix, and the mixing method [A32-A34], Thus, the electrical conductivity of composites should be measured for any new compositions. The amount of PPy(DBS) added in a polymer electrolyte or polymer interlayer for LIMSSBs should stay below the percolation threshold, otherwise, the cell could electrically short, Li could plate on the opposite side of the interlayer, and no appreciable electric field strength could be maintained across the polymer interlayer. With the amount of PPy(DBS) below the percolation threshold, the ionic conduction mechanism of the polymer electrolyte, through the segmental motion of polymer chains and Li-ions in the polymer electrolyte matrix, will remain relatively unchanged.
[0310] A polymer electrolyte that can operate near room temperature (25 °C) is desirable for more equivalent comparisons between the characterization techniques. Thus, a polyethylene oxide (PEO) based polymer electrolyte [A35] was used as the polymer electrolyte matrix in which the CP particles are dispersed. PEO based polymer electrolytes are widely studied and show adequate room temperature ionic conductivity (> 0.1 mS / cm at 25 °C) if the crystallinity can be inhibited. PEO (M.W. 100,000) as the main long chain polymer gives a balance between mechanical properties and potential for lower crystallinity [A35, A36], Tetraethylene glycol dimethacrylate (TEGDMA) as an additional cross-linking short chain monomer can inhibit crystallinity and improve interfacial contact [A35], Tetraethylene glycol dimethyl ether (TEGDME) as a cross-linking plasticizer can further reduce crystallinity and reduce thecoordination of Li-ions with EO in long chain PEO. Lithium bis(trifluoromethane)sulfonimide (LiTFSI) as the main Li salt was the salt of choice in most polymer electrolytes, showing relatively high ionic conductivity and the TFSI' anion can have a plasticizing effect [A35, A36], Lithium bis(oxalato)borate (LiBoB) as an additional Li salt has lower ionic conductivity than LiTFSI but used in small amounts can improve the interface stability with Li-metal [A37], 4-methylbenzophenone (MBP) is a hydrogen abstraction photoinitiator used to generate free radical chains from the methylene groups in PEO, TEGDMA, and TEGDME for UV-polymerization. Photopolymerization is a rapid process and does not require volatile solvents as compared to thermal polymerization or solvent evaporation synthesis methods [A35-A36], Materials. All chemicals were used as received. Iron (III) sulfate (F 62(804)3) pentahydrate (97%) and PEO (M.W. 100,000) were purchased from Thermo Scientific. Pyrrole (reagent grade 98%), sodium dodecylbenzenesulfonate (NaDBS, technical grade), TEGDMA (>90% technical grade), TEGDME (>99%), LiTFSI (99.95% trace metals basis), LiBoB, MBP (99%), and indium tin oxide (ITO) coated polyethylene terephthalate (PET) sheets (ITO-PET, 130 nm thick ITO coating on one side of 178 pm thick PET, surface resistivity 60 Q / sq) were purchased from Sigma- Aldrich. Clear PET film (127 pm thick) and copper tape with conductive adhesive were purchased from McMaster-Carr. Li-metal chips (0.6 mm thick) were purchased from MTI.
[0311] Chemical polymerization of CP particles. PPy(DBS) was chemically polymerized as described previously, reported to have an electrical conductivity of approximately 21.7 S / cm and molecular weight per residue of approximately 138.4 g / mol [A31], In brief, a polymerization solution of 0.375M pyrrole monomer, 0.030M NaDBS for DBS' dopant, and 0.100M F 62(804)3 chemical oxidant was prepared in 200 mL of deionized (DI) water. One half solution of pyrrole and NaDBS was stirred in 100 mL of DI water, and the other half solution of Fe2(SO4)3 was stirred in a separate 100 mL of DI water. The solution with Fe2(SO4)3 was slowly poured into the solution with pyrrole and NaDBS until fully combined, and the polymerization reaction was allowed to proceed for 16h at room temperature (20-25 °C) under slow magnetic stirring. The solution was then poured through 0.8 pm filter paper, rinsed with DI water until the filtrate is neutral pH, rinsed with ethanol several times, dried at 40 °C under vacuum (gauge pressure -0.95 bar) for 24h, and manually grinded with a mortar and pestle. The reaction yielded 2.1g of PPy(DBS) particles (approximately 13.6 mL loosely packed).
[0312] Polymer electrolyte preparation. The synthesis process of the polymer electrolyte film is summarized in FIG. 2. The polymer electrolyte was composed of 30.3 wt% PEO (approximate 100,000 M.W.) as the main long chain polymer, 15.1 wt% TEGDMA as an additional cross-linking short chain monomer, 30.3 wt% TEGDME as cross-linking plasticizer, 17.8 wt% LiTFSI as the main Li salt, 3.5 wt% LiBoB as additional Li salt (20% of LiTFSI amount), and 3.0 wt% MBP as photoinitiator. PPy(DBS) CP particles were added as an additional 0-2 wt% of PEO and TEGDMA amounts (0-0.9 wt% of total components, -0-15 vol% of final polymer electrolyte film) for their properties of polarizing and trying to align under an electric field. The PPy(DBS) particles are insoluble in the polymer electrolyte solution and will remain as particles dispersed in the cured polymer electrolyte matrix. PPy(DBS) added as up to 0.9 wt% of the total components is well below the percolation threshold reported for roughly spherical PPy particles of at least 3-5 wt% [A33, A34], The components were combined in an argon-filled glovebox, magnetic stirred overnight (at room temperature, 20-25 °C, in a sealed vial) to form a viscous liquid mixture, then ultrasonicated for 10 min prior to hot-pressing. In ambient air, the mixture was hot-pressed between PET sheets at 80 °C under 4.4 bar of pressure for 10 min (film thickness set to around 125 pm with a spacer). The film was polymerized for 10-20 min under UV light with 150 mW / cm2intensity at the film surface (main wavenumber 365 nm), flipping the film over halfway through the UV curing process, to obtain the polymer electrolyte. The polymer electrolyte film was vacuum dried (gauge pressure -0.95 bar) overnight at 40 °C to try to remove residual moisture prior to further characterizations. Hereafter, the amount of PPy(DBS) is referred to as the wt% of PEO and TEGDMA amounts in the compositions (0-2 wt% of the polymer and monomer).
[0313] Procedures for Characterization of Adaptive Polymer Electrolyte. The polymer electrolyte films were characterized with a combination of physical, mechanical, and electrochemical tests. Physical characterizations consisted of insoluble fraction, electrical conductivity, XRD, DSC, and DMA. Mechanical response characterizations included block force response and AFM. Electrochemical characterizations consisted ofEIS, Li-Li symmetric cycling, and ESW.
[0314] Physical characterizations. Insoluble fraction measurements were performed by taking the initial dry weight of the film (14.3 mm dia.), sandwiching the film between 304 stainless steel mesh, soaking in acetonitrile overnight at room temperature (20-25 °C) to dissolve the soluble (non-cross-linked) components [A35, A36], vacuum drying (gauge pressure -0.95 bar) overnight at 40 °C, and taking the final dry weight of the film. Electrical conductivity measurements were performed with the polymer film between copper foil contacts, using an Extech EX330 multimeter to obtain the electrical resistance.
[0315] XRD was collected at room temperature (20-25 °C) from 10° to 40° 29 with a Rigaku MiniFlex 600 with a Cu K-a radiation source (k = 1.5406A) at 40 kV voltage and 15 mA current.DSC was performed with a TA Instruments DSC 2500 (TA Instruments-Waters LLC, New Castle, DE). Samples between 2.5 mg to 7.5 mg were used in Tzero hermetic aluminum pans. Samples were cooled from room temperature to -90 °C at 10 °C / min, then heated to 120 °C at 5 °C / min. This process was repeated for a second scan to remove any thermal history. In the DSC analysis, the glass transition temperature (Tg) was determined from the inflection point in the slope towards the middle of the glass transition step. The DSC slope of heat flow after the glass transition was determined by performing a linear regression of the slope from -20 °C to 120 °C. DMA was performed with a TA Instruments Q800 (TA Instruments-Waters LLC, New Castle, DE) equipped with a tension clamp and Thermal Advantage Q Series version 5.5.22 software. The DMA was operated under tension analysis (0. IN preload) on polymer films with sample dimensions of 20 mm L (±1 mm) x 10.5 mm W (±0.6 mm) x 0.28 mm T (±0.2 mm) from -120 °C to 150 °C at a 3 °C / min heating rate and a 1 Hz frequency. Thicker films for DMA were obtained by using thicker spacers in the synthesis process.
[0316] Mechanical response characterizations. AFM was used to measure the expansion response of polymer electrolyte films under an applied electric field at room temperature (20-25 °C) in air. A schematic of the AFM sample setup and picture of a sample are shown in FIGs. 3 A-3B. Small alterations were made to the polymer synthesis process for producing ~10 pm thick polymer film samples. Polymer solution was poured onto an ITO-PET sheet (ITO side facing up) to form a 15 mm dia. pool of solution, then hot-pressed between another ITO-PET sheet (ITO side facing polymer solution) without any spacer. After curing, one of the ITO-PET sheets is peeled off and 1 cm x 2 cm samples of 10 pm thick polymer on ITO-PET are cut out. A 50 nm thick layer of gold is sputtered on top of the polymer using a 20 mA sputter current with an EMS150R ES sputter coater (Electron Microscopy Sciences / Quorum). The outer edges of the sample are cut off then a section of polymer film is removed on one end, and copper tape attached to the ITO-PET for the bottom electrical contact. Another copper tape is attached to the gold coating as the top electrical contact, with insulative tape between the top and bottom copper tapes to prevent electrical shorting. The sample is attached to a glass slide using double-sided tape then loaded into an MFP-3D Infinity AFM system (Oxford Instrument, Asylum Research). The cross-section and gold-coated surface morphology were investigated with a Thermo Scientific Apreo scanning electron microscope (SEM). The thicknesses of the films were confirmed to be approximately 10 pm thick by measuring with a micrometer and with cross-sectional SEM (FIG. 9).
[0317] Continuous point measurement with the AFM probe in contact with the sample surface was used to measure the displacement of the film over time. The displacement of the filmsurface (expansion and contraction) was obtained from the Z-piezo movement required to maintain a constant cantilever deflection. A commercial AFM cantilever was used for continuous point measurements (Olympus AC160-R3, nominal spring constant 4 N / m, nominal tip radius 7 nm, and nominal resonant frequency 300 kHz). An NI USB-6008 multifunction I / O data acquisition module (National Instruments) was used with Lab VIEW to apply a voltage for different electric field strengths across the polymer film for periods of 10 min excitations (voltage applied) followed by 10 min relaxations (no voltage applied). Additionally, topography maps were obtained using tapping mode using a commercial AFM cantilever (Olympus AC240-R3, nominal spring constant 2 N / m, nominal tip radius 7 nm, and nominal resonant frequency 70 kHz).
[0318] A block force setup was utilized to measure the force response of polymer electrolyte films under an applied electric field at room temperature (20-25 °C) in air. The film (14.3 mm dia., 125 pm thick) was sandwiched between 304 stainless steel (304SS) spacers (15.5 mm dia.) with conductive adhesive copper tape attached to each 304SS spacer for electrical connection. A calibrated MF01 A-N-221-A04 membrane force sensor (Alpha Taiwan) was used to measure the force. A polytetrafluoroethylene (PTFE) spacer (9.5 mm dia., 1.0 mm thick) was used between the membrane force sensor and the 304 SS / polymer electrolyte / 304SS stack to ensure the force was applied in the membrane force sensor active area (10.2 mm dia.) and for electrical isolation. This stack was clamped between insulated surfaces of a small vice mounted on a vibration isolation table. A programmable DC power supply (Tektronix PWS4305) connected with a linear amplifier (Piezo Systems, Inc. model EPA-104) was used to apply a voltage for different electric field strengths across the polymer electrolyte film. Deviations in the membrane force sensor readings from a stable ~1N clamp force were monitored to determine the force response of the polymer electrolyte.
[0319] Electrochemical characterizations. CR2032 coin cells were used for all electrochemical testing at 25 °C in a Thermo Scientific Heratherm Refrigerated Incubator. Li-metal chips were polished with a nylon brush to remove any oxide layer prior to coin cell assembly in an argon-filled glovebox. For EIS and Li-Li symmetric cycling, cells with 304SS spacer (15.5 mm dia.) / Li-metal (14.3 mm dia.) / polymer electrolyte (14.3 mm dia.) / Li-metal (11.1 mm dia.) / 304SS spacer (15.5 mm dia.) were used (as shown in FIG. 10). EIS was performed with a Gamry Instruments Reference 600+ potentiostat / galvanostat / ZRA at 25 °C from 5 MHz to 0.1 Hz with a 10 mV AC amplitude applied around the open-circuit voltage (OCV). Gamry Echem Analyst was used for fitting EIS spectra with equivalent circuits using the Simplex method and excluding data points after the end of the semicircle on the low frequency side (right side of the Nyquistplots). Li symmetric cell cycling was performed with an Arbin LBT21084 at 25 °C and a current density of ±0.1 mA / cm2(based on the area set by the 11.1 mm dia. Li-metal) for 30 min each direction with 30 min rests.
[0320] The ESW was determined by linear sweep voltammetry (LSV) and cyclic voltammetry (CV) at 25 °C with an Arbin LBT20084. Separate cells were used for anodic LSV and cathodic CV scans. For anodic LSV scans (OCV to 7V vs. Li / Li+at 0.1 mV / s scan rate), cells with the polymer electrolyte film (14.3 mm dia.) sandwiched between 304SS (15.5 mm dia.) as the working electrode (WE) and Li-metal (11.1 mm dia.) as the counter / reference electrode (CE / RE) were used (shown in FIG. 11 A). For cathodic CV scans (OCV to -0.2V vs. Li / Li+at 0.1 mV / s scan rate), cells with the polymer electrolyte film (14.3 mm dia.) sandwiched between Cu foil (14.3 mm dia.) as the WE and Li-metal (11.1 mm dia.) as the CE / RE were used (shown in FIG.
[0321] 11B).
[0322] Results and Discussion: Physical characterizations. As produced, the polymer electrolytes were free-standing films (shown for 0 wt% PPy(DBS) composition in FIGs. 12A-12C) that could be peeled off the PET sheet and were non-tacky. The cross-linked fraction of the polymer electrolytes was determined through insoluble fraction measurements, as the crosslinked components of the film remain after soaking in acetonitrile [A35, A36], The results in FIG. 4A show the insoluble fractions of compositions with various amounts of PPy(DBS). The target insoluble fraction of > 50 wt% was selected based on the similar polymer electrolyte composition from previous reports [A35] and above this threshold the films were free-standing. For a given UV curing time, as the amount of PPy(DBS) in the composition increased the insoluble fraction typically decreased and the variability in insoluble fraction between samples from the same film increased. With longer UV curing times for each composition, the insoluble fraction increased and the variability decreased. The PPy(DBS) particles are opaque, black particles that reduced UV transmittance through the thickness of the film (inhibiting UV curing), resulting in lower insoluble fractions and higher variability. The optical appearance of the films with increasing amounts of PPy(DBS) are shown in the inset in FIG. 4 A. The 0 wt% PPy(DBS) film was optically clear, becoming darker with more PPy(DBS) until appearing almost completely opaque at 2.0 wt% PPy(DBS). The 2.0 wt% PPy(DBS) film eventually reached the target insoluble fraction after 20 min UV curing time but resulted in a brittle film (possibly due to overcuring in areas of the film the UV transmittance was less obstructed by PPy(DBS) particles). The 2.0 wt% PPy(DBS) films did not reach full solidification below this curing time and the insoluble fraction could not be measured.
[0323] Electrical conductivities obtained from 5 samples of each composition are shown in FIG.13. The electrical conductivities (uezeC) were calculated using the resistance values measured with the multimeter (R), thickness of the film ( / ) and contact area (A) in the following equation: ^elec =A(1 2) Materials with an electrical conductivity below 10'8S / cm are typically considered electrical insulators, with the transition to electrical semiconductors for conductivities above 10'8S / cm [A38-A39], Films with 0 wt% through 2.0 wt% PPy(DBS) showed a minor increase in electrical conductivity from 4.6-6.3 x 10'9S / cm, confirming the compositions are below the percolation threshold (where a sharp increase in electrical conductivity of multiple orders of magnitude would be observed). Thus, the upper limit on the amount of PPy(DBS) that can be added to these compositions is due to the UV curing process, not the percolation threshold. For subsequent experiments, only 0 wt% through 1.0 wt% PPy(DBS) films from 10 min UV curing time were used. These films were selected to avoid potential effects from overcuring at longer UV cure times. The average insoluble fractions were above the target fraction for these films, even though the films with increasing amounts of PPy(DBS) had lower insoluble fractions.
[0324] XRD scans of polymer electrolyte films containing 0 wt% through 1.0 wt% PPy(DBS) particles (with background signal from the glass slide removed) are shown in FIG. 4B. There are no sharp crystalline peaks present in the XRD pattern - only a broad amorphous peak centered around 29 of 19.5° is present, indicating highly amorphous films. The amorphous peak appears to broaden with increasing amounts of PPy(DBS), suggesting the addition of PPy(DBS) may lead to increasingly disordered films.
[0325] DSC profiles from the second heating scan of the different polymer electrolyte compositions are shown in FIG. 4C with results summarized in Table 3. During DSC heating scans, thermal transitions such as the glass transition, melting, and crystallization can be observed. The glass transition occurs within the amorphous phase of PEO as the material changes from a rigid glassy state to a more mobile rubbery state due to heating. It presents itself as an endothermic step change in heat flow within the DSC heat scan. The polymer samples in this study showed Tgvalues between -37 °C and -41 °C, in order of increasing PPy(DBS). With Tgvalues well below room temperature, the polymer will exhibit a highly mobile rubbery structure around room temperature. The polymer samples did not display any distinct melting peaks in the DSC data up to 120 °C. This suggests the films are highly amorphous, as confirmed by XRD data, compared to the semi-crystalline behavior typically observed in similar PEO based polymer electrolytes [A35, A36], Li-ion transport in PEO based polymer electrolytes is typically considered to occur through segmental motion of polymer chains in amorphous regions and the subsequent Li-ion hopping along and between the polymer chains [A40], Thus, a highlyamorphous structure enhances segmental motion mechanisms for increasing ionic conductivity because there are no crystalline lattice structures to inhibit the movement of the polymer chains and lithium ions. As expected from literature on other filler particles incorporated in PEO lowering Tg(such as SiCh, SnCh, and TiCh) [A41-A43], incorporating increasing amounts of PPy(DBS) shifts the Tgto slightly lower temperatures. This could be caused by PPy(DBS) particles physically disrupting and interfering with the packing of PEO chains allowing the glass transition to occur at lower temperatures. The slope of the heat flow after the glass transition in FIG. 4C increased with the addition of PPy(DBS) from 20.1 mW7(g °C) to 85.9-115.0 mW / (g °C), summarized in Table 3. This increase in slope of the heat flow suggests an increase in specific heat capacity (requiring additional heat flow to maintain the same heating rate). This difference is not expected from the heat capacity of PPy(DBS), which is typically lower than the heat capacity of PEO. Instead, the increasingly mobile rubbery structures (as indicated by decreasing Tg) may cause the increase in specific heat capacity [A44-A47],
[0326] DMA tan delta thermograms are shown in FIG. 4D, with storage and loss modulus profiles shown in FIGs. 14A-14D. Results are only shown to 20 °C as the films became too soft above this temperature and broke or the measurement signal became unstable. The peak of the tan delta curve (when the material demonstrates the most viscous response to deformations) was used to determine Tgof the films from DMA in this analysis with the results summarized in Table 3. There are multiple methods to determine Tgfrom DMA, with the tan delta peak typically giving the highest value of Tg[A48], This is a conservative determination with respect to enhanced segmental motion of polymer chains for increased ionic conductivity in PEO based electrolytes. DMA results show Tgvalues between -43 °C and -57 °C in good agreement with the trend of Tggenerally decreasing with increasing amounts of PPy(DBS), as observed with DSC. The obtained values of Tgdiffered between DSC and DMA, which is not uncommon as glass transition is a region of behavior with values often differing by 10-25 °C between the techniques [A48], The difference in Tgbetween techniques can be attributed to the different property changes related to the glass transition region observed with DSC and DMA (measurement parameters can also affect the values obtained). Changes in heat flow due to the change in heat capacity of the polymer during its transition from a rigid glassy state to a mobile rubbery state are observed with DSC, whereas the change in mechanical properties are observed with DMA. These Tgvalues from DSC and DMA are within the range of similar PEO based polymer electrolytes with reported Tgvalues between -34 °C and -78 °C [A35, A36], The storage and loss moduli did not show a consistent trend with increasing amounts of PPy(DBS). If the addition of PPy(DBS) particles affected the storage and loss moduli, increasing or decreasing values withincreasing amounts of PPy(DBS) would be expected but no such trend is observed. The variability between the storage and loss moduli for the different compositions could obscure any effect from PPy(DBS).
[0327] Mechanical response characterizations. FIGs. 5A-5F shows the AFM continuous point measurements for the films under an electric field strength of 0.3 V / pm for 10 min followed by 0 V / pm for 10 min for 5 representative excitations and relaxations. The 0 wt% PPy(DBS) film (FIG. 5 A) does not show any appreciable response beyond the measurement uncertainty and noise. The 0.25-1 wt% PPy(DBS) films (FIGs. 5B-5D) show a clear expansion response up to 0.6 pm (corresponding to 6% strain for the approximately 10 pm thick films) under an electric field strength of 0.3 V / pm followed by a relaxation when the electric field is removed (0 V / pm). This response is attributed to the polarization of the PPy(DBS) particles in the polymer film. The PPy(DBS) particles are polarized under an electric field and would try to align, causing the film to expand. The expansion response increases from an average expansion of 0.44 pm for 0.25 wt% PPy(DBS) to 0.56 pm for 1 wt% PPy(DBS) and appears to be repeatable over several cycles. The expansion response decreases with decreasing electric field strength as shown in FIGs. 15A-15C, where the film does not produce an appreciable response below 0.2 V / pm regardless of the concentration of PPy(DBS).
[0328] The films not returning to zero displacement at the end of the relaxations suggests there is a residual expansion left in the films. This could be due to an irreversibility such as plastic deformation or an irreversible rearrangement of PPy(DBS) particles and polymer matrix chains during the initial excitation. This behavior is also seen to some extent in the storage modulus response for PPy -based and other ER elastomers [A26-A28], The strain of the films at the end of excitations and relaxations (sexcitation and 8relaxation, corresponding to expansion and residual expansion, respectively) were calculated from the displacement compared to the beginning of the excitation (taken as zero) divided by the film thickness (approximately 10 pm). The results are shown in FIG. 5E with 0 wt% PPy(DBS) included for comparison, even though it did not display a clear expansion and relaxation response. For the 0.25-1 wt% PPy(DBS) films, Sexcitation increased from -4-6% with increasing PPy(DBS) whereas 8relaxation did not display a clear trend.
[0329] The temporal characteristics of the response were investigated with the time constant for expansion and relaxation (Texcitation and relaxation, respectively). Texcitation was determined from the time taken for the excitation to reach 1-1 / e (63.2%) of the final value, relaxation was determined from the time taken for the relaxation to decay to 1 / e (36.8%) of the final excitation value compared to the final relaxation value. The results are shown in FIG. 5F, with the response times a similar magnitude to those of storage modulus for a PPy -based ER elastomer [A26], There wasno trend for the time constants with different amounts of PPy(DBS). However, Treiaxation was lower than Texcitation by about 1 min for each case. This suggests the polymer starts to return to its relaxed state faster than the excitation. This is seen in the storage modulus response for a PPy-based ER elastomer as well [A26], The storage modulus quantifies the elastic response of the polymer when it is subjected to a deformation. The energy is stored elastically when undergoing deformation and can be released once the stress is removed. This energy is required to rearrange the polymer chain entanglements and cross links in response to the stress (in this case, in response to the PPy(DBS) particles polarizing and trying to align in the polymer matrix under an electric field). However, this elastic energy can allow the polymer chains in the matrix to return to the relaxed state very fast, which could result in Treiaxation being lower than Texcitation. Also, the films do not return to zero displacement during the relaxation, which may contribute to the lower time constant.
[0330] Note that, while the AFM measurements were generally reliable, they were subject to uncertainties such as thermal drift over the long timescale of the polymer response. Some sharp increases or decreases were noted during the transitions between excited and relaxed states. These variations are possibly attributable to measurement artifacts, as the direction of these changes was inconsistent across similar transitions. Despite these uncertainties, the results indicate the 0.25-1 wt% PPy(DBS) films produced a significant expansion strain response during excitation (4.2-5.9%) and residual strain following relaxation (1.1-2.5%) compared to the 0 wt% PPy(DBS) control (with strains of 0.2% ± 0.3% and 0.1% ± 0.4%, respectively).
[0331] The surface morphology of gold coated 1 wt% PPy(DBS) film is shown in FIGs. 6A-6H. SEM micrographs (FIGs. 6A and 6E) of the pristine film showed relatively flat surfaces with a few raised areas. AFM topography maps were used to investigate the uniformity of the polymer film expansion in local regions. The AFM topography maps of the film at rest (FIGs. 6B and 6F), after the first excitation at 0.3 V / pm (FIGs. 6C and 6G), and after the first relaxation (FIGs. 6D and 6H) did not show any significant changes in the surface locally, suggesting the expansion response was relatively uniform across the surface of the film.
[0332] A simplified schematic of the block force setup (insulative layers between electrically conductive components not shown) used for measuring the force response of the polymer electrolyte compositions under an electric field is shown in FIG. 7A. The polymer electrolyte film was sandwiched between electrical contacts that were connected to a voltage source to apply an electric field across the film. A membrane force sensor was used in-line to measure force applied from the film (as deviations from the ~1N clamp force) with the entire stack clamped in a small vise. This setup roughly corresponds to the polymer electrolyte as an interlayer sandwichedbetween a Li-metal anode and ceramic solid electrolyte, however, the clamp force used here is lower than the stack pressure would be in a solid-state battery due to resolution limitations of force sensors with higher load capacities.
[0333] The resulting force response measurements are shown in FIG. 7B. For films with PPy(DBS), the force response increased with increasing wt% of PPy(DBS) (from 0.25 wt% to 1 wt%) and increasing electric field strength (from 0.1 V / pm to 0.3 V / pm). This force response trend is associated to the polarization of PPy(DBS) under an electric field as the particles may try to align, since this response of CP particles such as PPy(DBS) has typically been shown to increase with increased CP loading and electric field strength [A21-A29], Since the film is mechanically compressed under the clamp, changes in stiffness of the film under electric field may partially contribute to the measured response, implying that the force required to maintain the same level of compression would increase [A26-A29],
[0334] It is noteworthy that the 0 wt% PPy(DBS) films showed a non-zero response (FIG. 7B) that, however, did not indicate any appreciable relationship with the applied electric field strength. Polarization of ions within the film under an electric field could contributed to the response. The film responses in FIG. 7B are reported for the first actuation to mitigate possible effects on the response from decomposition of the films (as the applied voltages are above the ESW of around 4.5 V in FIG. 8D). However, these results still suggest a desirable force response due to the polarization of the PPy(DBS) particles as the responses of films with PPy(DBS) were significantly larger than the responses in the 0 wt% PPy(DBS) films, increasing with increasing electric field strength and amount of PPy(DBS) (and the ESW is similar between all compositions).
[0335] Electrochemical characterizations. The electrochemical characterizations of the polymer electrolyte compositions were all performed at 25 °C to investigate the performance around room temperature. Symmetric Li / polymer / Li coin cells were used to compare the polymer electrolyte performance of the compositions with PPy(DBS) to the 0 wt% PPy(DBS) composition. For symmetric cycling (30 min cycles at ±0.1 mA / cm2) and EIS, > 10 coin cells were tested for each composition. Results based on the 5 middle performing coin cells are reported in this work.
[0336] A summary of the measured ionic conductivities for the 5 middle performing coin cells at 25 °C are shown in FIG. 8A. The ionic conductivities (pion) were calculated using Rsfrom the equivalent circuit as the bulk polymer electrolyte impedance (Rb), thickness of the electrolyte ( / ) and contact area (A) in the following equation:
[0337] (Ron ~ r,A(2-2)
[0338]
[0339] The results indicate no trend for ionic conductivity between the compositions when considering the variability, with ionic conductivities between 0.11-0.16 mS / cm.
[0340] Out of the 5 middle performing coin cells for each composition the Li symmetric cycling overpotentials are shown in FIG. 16 and the Nyquist plots obtained from EIS are shown in FIGs.
[0341] 17A-17D for 0-50 cycles of the representative cells. Equivalent circuit model parameter fitting was performed with a series resistor (Rs) to model the bulk impedance of the polymer electrolyte and two sets of parallel resistors (RSEI, Ret) with constant phase elements (CPEi, CPE2) to model the solid electrolyte interphase and charge transfer of the Li / polymer interfaces, respectively. The total interfacial impedance was taken as the combination of RSEI and Ret of both Li / polymer interfaces, assuming the interfaces are nearly identical. CPEs were used to account for non-ideal capacitive behavior. The equivalent circuit model parameters for the representative cells are summarized in Table 4. The bulk impedance (which can be approximated as the left-side intersection of semicircle with the real impedance Z’ axis) remained relatively stable over 50 cycles. The interfacial impedance (can be approximated as the right-side intersection of semicircle with the real impedance Z’ axis) varied between the cells over 50 cycles with interfacial impedance decreasing (suggesting the interface is still stabilizing), increasing, a combination of the two, or remaining stable. Thus, the cells were compared after 50 cycles when there was less variability between the 5 cells with the interfacial impedances shown in FIG. 8B and Nyquist plots from EIS for representative cells shown in FIG. 8C.
[0342] As with the ionic conductivity, no trend in interfacial impedances was observed among the compositions with increasing amounts of PPy(DBS) when considering the variability of the 5 cells of each composition in FIG. 8B. One difference was the variability between the 0 wt% PPy(DBS) composition cells was higher than each of the compositions with PPy(DBS). The use of wave springs in the coin cells could contribute to increased variability in interfacial impedance, due to uneven pressure applied by wave springs [A49-A51], The total interfacial impedances of the cells were on the order of 4 kQ cm2. This value is higher than comparable PEO based polymer electrolytes [A35, A36] of -500-700 cm2which could be due to some experimental processing limitations in this work such as: hot-pressing and UV-curing the films in ambient air (possibility of moisture contamination that vacuum drying may not fully remove), hot-pressing under lower pressure, greater amount of photoinitiator used (evidenced by reaching target insoluble fraction in a shorter curing time compared to previous reports [A35] where photoinitiator amount was not specified), and differences in coin cell configuration (total spacer thickness and type of spring will affect stack pressure and thus interfacial impedance, which were not specified [A35, A36]). Excess photoinitiator could cause increased interfacialimpedance due to increased storage modulus [A52] or premature termination and incomplete cure of the polymer matrix [A53] . During polymerization, excess photoinitiator could cause more polymer chains to become crosslinked leading to a higher crosslink density. An increased storage modulus could result from the higher crosslink density due to less mobility within the polymer chains and the polymer would not be able to conform as easily to the Li-metal surface, increasing the interfacial impedance. An incomplete cure could lead to less crosslinks in the matrix than expected or inhomogeneous crosslinking. Regions of lower crosslinking could have higher mobility and leaching of non-crosslinked moi eties and regions of higher crosslinking could have more defects resulting in cracks or voids in the interface.
[0343] Although some polymer electrolytes have achieved sufficient ionic conductivities at 25 °C, high interfacial impedances > 100 Q cm2limit the commercial viability of polymer electrolytes in LIMSSBs for applications such as electric vehicles and consumer electronics (apart from semi-solid gel polymer electrolytes that can pose safety concerns). Further advancements are needed to lower interfacial impedance at 25 °C such as developments with in-situ polymerization or single ion conducting polymer electrolytes [A54-A57], The incorporation of PPy(DBS) particles and resulting properties presented in this work are expected to be applicable for other polymer electrolyte compositions.
[0344] The ESW at 25 °C with Li-metal of each polymer electrolyte composition was determined with cathodic CVs and anodic LSV shown in FIG. 8D (with zoomed-in plots shown in FIG. 18A and FIG. 18B, respectively). For the cathodic sweep, a small peak was initially seen around 1.5 V vs. Li / Li+that may be attributed to the decomposition of some polymer electrolyte components to form a passivation layer with Li-metal [A58], as many polymer electrolytes are not stable with Li-metal but form a stable passivation layer or interphase [A6, A20, A35, A36], This peak was present in all compositions, suggesting components in the 0 wt% PPy(DBS) composition were responsible, not PPy(DBS). Reversible Li plating and stripping on the Cu surface was seen from -0.2V to 0.3 V vs. Li / Li+, as Li will plate on the Cu WE when its potential goes below 0V vs. Li / Li+then strip after the potential increased above 0V vs. Li / Li+again. From the anodic sweep, the oxidative stability was conservatively determined as when the current density surpassed 1 pA / cm2giving a stability up to 4.5V vs. Li / Li+for all compositions.
[0345] Conclusions. The adaptive behavior of a polymer electrolyte at room temperature (20-25 °C) by incorporating conducting polymer particles was demonstrated, with the aim of investigating its potential for application as an interlayer to enhance the performance and durability of lithium metal solid-state batteries (LIMSSBs). The adaptive polymer electrolyte (A-PE) comprised of a polyethylene oxide based polymer electrolyte containing polypyrroledoped with dodecylbenzene sulfonate (PPy(DBS)) conducting polymer particles. The incorporation of PPy(DBS) particles imparted adaptive properties to a polymer electrolyte matrix, allowing for force and expansion responses under electric fields through the polarization of PPy(DBS) particles.
[0346] Experimental results confirmed the A-PE's adaptive behavior. Atomic force microscopy (AFM) measurements revealed an expansion response of films of up to 6% strain under a field of 0.3 V / pm, repeatable over several cycles, with reduced expansion observed at lower electric field strengths. Block force response measurements showed a corresponding increase in force with higher electric field (starting from 0.1 V / pm) and greater PPy(DBS) loading. These findings are consistent with the adaptive response being driven by the polarization of PPy(DBS) particles, a behavior commonly observed in electrorheological fluids and elastomers [A21-A29],
[0347] The incorporation of PPy(DBS) particles affected the polymer matrix by inhibiting UV curing, lowering the insoluble fraction of the film and restricting the PPy(DBS) particle amount to ~1 wt% of polymer and monomer content (equivalent to -0.45 wt% or -8 vol% of final film). Despite this, the films remained electrical insulators with no increase in electrical conductivity, indicating that the percolation threshold was not reached. Furthermore, no substantial trends were observed in the electrochemical performance of the polymer electrolytes at 25 °C with increasing amounts of PPy(DBS). The amorphous structure of the films showed minor changes with the amounts of PPy(DBS) incorporated.
[0348] Beyond LIMSSBs, this adaptive polymer concept shows promise for other applications, such as low voltage soft actuators. Exploring synthesis methods that allow for the addition of more PPy(DBS) is also of interest to determine if there is an optimal amount before the films become electrically conductive. Additionally, evaluating the performance of the A-PE as a thin interlayer (ideally < 10 pm thick) between the lithium metal anode and ceramic solid electrolyte in full LIMSSBs will be useful to understanding its potential to mitigate interfacial changes upon lithiation / delithiation, and its effects on battery durability.Table 3. Summary of properties from DSC and DMA. Tgfrom DSC obtained from the inflection point in the slope of the glass transition step, DSC slope of heat flow after glass transition obtained from a linear regression from -20 °C to 120 °C, and Tgfrom DMA obtained from the peak of the tan delta thermograms.
[0349] Tgfrom DSC DSC slope of heat flow after Tgfrom DMA tan Sample
[0350] [°C] glass transition [mW / (g °C)] delta [°C]
[0351] 0 wt% PPy(DBS) -37.4 20.1 -43.2
[0352] 0.25 wt% PPy(DBS) -38.8 88.6 -53.7
[0353] 0.5 wt% PPy(DBS) -39.9 115.0 -53.6
[0354] 1 wt% PPy(DBS) -40.9 85.9 -56.6
[0355]
[0356] Table 4. Equivalent circuit model parameters from EIS fitting of the representative cells in FIGs.
[0357] 17A-17D. Parameters are series resistance (Rs), solid electrolyte interphase resistance (RSEI), charge transfer resistance (Ret), constant phase elements (CPEi, CPE2), and exponent of the CPEs to account for the non-ideal capacitive behavior (a), a < 1 for non-ideal capacitive behavior, a = 1 for ideal capacitor.
[0358] Representative
[0359] 0 wt%PPy(DBS) 0.25 wt%PPy (DBS) 0.5 wt%PPy(DBS) 1 wt%PPy(DBS) Coin Cell
[0360] Cycles 0 25 50 0 25 50 0 25 50 0 25 50 Rs [Q] 76 79 83 92 108 102 99 107 109 78 82 82 RSEI [£2] 760 710 966 973 1088 1054 1164 866 800 1232 966 962
[0361] 3.07 4.30 4.98 2.75 4.85 6.25 1.95 4.81 6.77 2.42 5.38 6.55 CPEi [S*s“] * * * * * * * * * * * * IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6ai 0.79 0.76 0.74 0.80 0.73 0.71 0.81 0.72 0.69 0.77 0.69 0.68 Ret I | 2494 2402 3080 2667 2637 2147 4128 3274 2790 2463 2817 2626
[0362] 3.11 3.13 3.06 2.49 3.27 3.56 2.07 2.79 2.97 3.34 2.78 2.68 CPE2[S*S“] * * * * * * * * * * * * IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6IO'6a 0.89 0.88 0.87 0.90 0.88 0.88 0.87 0.85 0.85 0.88 0.86 0.88
[0363]
[0364] 2
[0365] References
[0366] Al J. Janek and W. G. Zeier, A solid future for battery development, Nature Energy, 2016, 1, 16141.
[0367] A2 K. J. Kim et al. Solid-State Li-Metal Batteries: Challenges and Horizons of Oxide and Sulfide Solid Electrolytes and Their Interfaces, Advanced Energy Materials, 2021, 11, 2002689.
[0368] A3 D. H. S. Tan et al. From nanoscale interface characterization to sustainable energy storage using all-solid-state batteries, Nature Nanotechnology, 2020, 15, 170-180.A4 Y. Zhu, X. He and Y. Mo, Origin of Outstanding Stability in the Lithium Solid Electrolyte Materials: Insights from Thermodynamic Analyses Based on First-Principles Calculations, ACS Applied Materials & Interfaces, 2015, 7, 23685-23693.
[0369] A5 F. Han et al. Electrochemical Stability of Li io GeP 2 S 12 and Li 7 La 3 Zr 2 O 12 Solid Electrolytes, Advanced Energy Materials, 2016, 6, 1501590.
[0370] A6 S. Sen et al. The role of polymers in lithium solid-state batteries with inorganic solid electrolytes, Journal of Materials Chemistry A, 2021, 9, 18701-18732.
[0371] A7 M. Nagao et al. In situ SEM study of a lithium deposition and dissolution mechanism in a bulk-type solid-state cell with a Li2S-P2S5 solid electrolyte, Phys. Chem.
[0372] Chem. Phys., 2013, 15, 18600.
[0373] A8 Y. Ren et al. Direct observation of lithium dendrites inside garnet-type lithium-ion solid electrolyte, Electrochemistry Communications, 2015, 57, 27-30.
[0374] A9 T. Krauskopf et al. Toward a Fundamental Understanding of the Lithium Metal Anode in Solid-State Batteries - An Electrochemo-Mechanical Study on the Garnet- Type Solid Electrolyte Li 6.25 Al 0.25 La 3 Zr 2 O 12, ACS Applied Materials and Interfaces, 2019, 11, 14463-14477.
[0375] A10 X. Zhang et al. Pressure-Driven Interface Evolution in Solid-State Lithium Metal Batteries, Cell Reports Physical Science, DOI: 10.1016 / j.xcrp.2019.100012.
[0376] All X. Han et al. Negating interfacial impedance in garnet-based solid-state Li metal batteries, Nature Materials, 2017, 16, 572-579.
[0377] A12 Y. Ruan et al. A 3D Cross-Linking Lithiophilic and Electronically Insulating Interfacial Engineering for Garnet-Type Solid-State Lithium Batteries, Advanced Functional Materials, 2021, 31, 2007815.
[0378] A13 W. Zhang et al. LivLasZrcOn Ceramic Nanofiber-Incorporated Solid Polymer Electrolytes for Flexible Lithium Batteries, ACSAppL Energy Mater. , 2020, 3, 5238-5246.
[0379] A14 J. Zhang et al. Flexible and ion-conducting membrane electrolytes for solid-state lithium batteries: Dispersion of garnet nanoparticles in insulating polyethylene oxide, Nano Energy, 2016, 28, 447-454.
[0380] Al 5 K. Liu et al. Polyoxyethylene (PEO)|PEO-Perovskite|PEO Composite Electrolyte for All-Solid-State Lithium Metal Batteries, ACS Applied Materials and Interfaces, 2019, 11, 46930-46937.
[0381] A16 J. Zheng et al. Interface-Enabled Ion Conduction in LiioGeP2Si2 -Poly(ethylene Oxide) Hybrid Electrolytes, ACSAppL Energy Mater, 2019, 2, 1452-1459.
[0382] A17 S. Wang et al. High-conductivity free-standing Li6PS5Cl / poly(vinylidenedifluoride) composite solid electrolyte membranes for lithium-ion batteries, Journal of Maleriomics, 2020, 6, 70-76.
[0383] Al 8 Z. Yang et al. Facile interfacial adhesion enabled LATP-based solid-state lithium metal battery, Chemical Engineering Journal, 2020, 392, 123650.
[0384] A19 H. Duan et al. Dendrite-Free Li-Metal Battery Enabled by a Thin Asymmetric Solid Electrolyte with Engineered Layers, Journal of the American Chemical Society, 2018, 140, 82-85.
[0385] A20 F. J. Simon et al. Properties of the Interphase Formed between Argyrodite-Type Li 6 PS 5 Cl and Polymer-Based PEO io:LiTFSI, ACSAppMat & Interf, 2019, 11, 42186-42196.
[0386] A21 D. S. Jang et al. Polypyrrole-wrapped halloysite nanocomposite and its rheological response under electric fields, Journal of Materials Science, 2014, 49, 7309-7316.
[0387] A22 G. C. Teare and N. M. Ratcliffe, Electrorheological properties of polypyrrole prepared by the action of mineral acids on pyrrole, Journal of Materials Chemistry, 1996, 6, 301.
[0388] A23 D.-H. Kim and Y. D. Kim, Electrorheological Properties of Polypyrrole and its Composite ER Fluids, Journal of Industrial and Engineering Chemistry, 2007, 13, 879-894.
[0389] A24 F. F. Fang et al. Electrorheological and magnetorheological response of polypyrrole / magnetite nanocomposite particles, Colloid and Polymer Science, 2013, 291, 1781— 1786.
[0390] A25 P. Chen et al. Fabrication of dual-coated graphene oxide nanosheets by polypyrrole and poly(ionic liquid) and their enhanced electrorheological responses, Journal of Industrial and Engineering Chemistry, 2019, 69, 106-115.
[0391] A26 P. Ludeelerd et al. Effect of elastomer matrix type on electromechanical response of conductive polypyrrol e / elastomer blends, Journal of Physics and Chemistry of Solids, 2010, 71, 1243-1250.
[0392] A27 W. Wichiansee and A. Sirivat, Electrorheological properties of poly(dimethylsiloxane) and poly(3,4-ethylenedioxy thiophene) / poly(stylene sulfonic acid) / ethylene glycol blends, Materials Science and Engineering: C, 2009, 29, 78-84.
[0393] A28 X. Yuan et al. A stable high-performance isotropic electrorheological elastomer towards controllable and reversible circular motion, Composites Part B: Engineering, 2020, 193, 107988.
[0394] A29 N. Ma et al. Properties and mechanical model of a stiffness tunable viscoelastic damper based on electrorheological elastomers, Smart Mater. Struct., 2020, 29, 045041.
[0395] A30 N. Aydemir et al. Electrolyte and solvent effects in PPy / DBS linear actuators, Sensors and Actuators, B: Chemical, 2015, 216, 24-32.A31 Y. Kudoh, Properties of polypyrrole prepared by chemical polymerization using aqueous solution containing Fe2(SC>4)3 and anionic surfactant, Synthetic Metals, 1996, 79, 17-22.
[0396] A32 G. Kaur et al. Electrically conductive polymers and composites for biomedical applications, RSC Adv., 2015, 5, 37553-37567.
[0397] A33 C. Cassignol et al. Microstructure-conductivity relationship in conducting polypyrrole / epoxy composites, Polymer, 1999, 40, 1139-1151.
[0398] A34 P. C. Vargas et al. Conductive Composites Based on Polyurethane and Nanostructured Conductive Filler of Montmorillonite / Polypyrrole for Electromagnetic Shielding Applications, Mat. Res., DOI:10.1590 / 1980-5373-mr-2018-0014.
[0399] A35 Y. Zhang et al. Cross-linking network based on Poly(ethylene oxide): Solid polymer electrolyte for room temperature lithium battery, Journal of Power Sources, 2019, 420, 63-72.
[0400] A36 L. Porcarelli et al. Super Soft All-Ethylene Oxide Polymer Electrolyte for Safe All-Solid Lithium Batteries, Scientific Reports, 2016, 6, 19892.
[0401] A37 R. He et al. Chemical and electrochemical stability enhancement of lithium bis(oxalato)borate (LiBOB)-modified solid polymer electrolyte membrane in lithium ion halfcells, Electrochimica Acta, 2017, 246, 123-134.
[0402] A38 M. Chanda, in Science of Engineering Materials, Macmillan Education UK, London, 1980, pp. 61-126.
[0403] A39 L. A. Fielding et al. Space science applications for conducting polymer particles: synthetic mimics for cosmic dust and micrometeorites, Chem. Commun., 2015, 51, 16886-16899.
[0404] A40 Z. Xue et al. Poly(ethylene oxide)-based electrolytes for lithium-ion batteries, J. Mater. Chem. A, 2015, 3, 19218-19253.
[0405] A41 K.-S. Ji et al. Role of functional nano-sized inorganic fillers in poly(ethylene) oxide-based polymer electrolytes, Journal of Power Sources, 2003, 117, 124-130.
[0406] A42 A. K. Thakur and S. A. Hashmi, Polymer matrix-filler interaction mechanism for modified ion transport and glass transition temperature in the polymer electrolyte composites, Solid State Ionics, 2010, 181, 1270-1278.
[0407] A43 K. Vignarooban et al. Effect of TiO2 nano-filler and EC plasticizer on electrical and thermal properties of poly(ethylene oxide) (PEO) based solid polymer electrolytes, Solid State Ionics, 2014, 266, 25-28.
[0408] A44 B. A. Lunn et al. Determination of the thermal conductivity of polypyrrole over the temperature range 280-335 K, Journal Of Materials Science, 1993, 28, 5092-5098.A45 A T. H. Gilani, Evidence for Metal-like Electronic Contribution in Low- Temperature Heat Capacity of Polypyrrole, J. Phys. Chem. B, 2005, 109, 19204-19207.
[0409] A46 T. Albrecht et al. Dynamics of Surface Crystallization and Melting in Polyethylene and Poly(ethylene oxide) Studied by Temperature-Modulated DSC and HeatWave Spectroscopy, Macromolecules , 2001, 34, 8456-8467.
[0410] A47 K. Pielichowski and K. Flejtuch, Phase Behavior of Poly(Ethylene Oxide) Studied by Modulated-Temperature DSC — Influence of the Molecular Weight, Journal of Macromolecular Science, Part B, 2004, 43, 459-470.
[0411] A48 K. P. Menard and N. Menard, Dynamic mechanical analysis, Taylor and Francis, Boca Raton, 3rd edn., 2020.
[0412] A49 J. S. Okasinski et al. In situ X-ray spatial profiling reveals uneven compression of electrode assemblies and steep lateral gradients in lithium-ion coin cells, Phys. Chem. Chem. Phys., 2020, 22, 21977-21987.
[0413] A50 F. C. Strobridge et al. Mapping the Inhomogeneous Electrochemical Reaction Through Porous LiFePO 4 -Electrodes in a Standard Coin Cell Battery, Chem. Mater., 2015, 27, 2374-2386.
[0414] A51 F. Dai and M. Cai, Best practices in lithium battery cell preparation and evaluation, Commun Mater , 2022, 3, 64.
[0415] A52 B. Steyrer et al. Visible Light Photoinitiator for 3D-Printing of Tough Methacrylate Resins, Materials, 2017, 10, 1445.
[0416] A53 K. Wang et al. Optimal photoinitiator concentration for light-cured dental resins, Polymer Testing, 2021, 94, 107039.
[0417] A54 Y. An et al. Progress in Solid Polymer Electrolytes for Lithium-Ion Batteries and Beyond, Small, 2022, 18, 2103617.
[0418] A55 P. Lennartz et al. Practical considerations for enabling Li|polymer electrolyte batteries, Joule, 2023, 7, 1471-1495.
[0419] A56 Q. Zhao et al. Solid-state polymer electrolytes with in-built fast interfacial transport for secondary lithium batteries, Nat Energy, 2019, 4, 365-373.
[0420] A57 H. Zhang et al. Suppressed Mobility of Negative Charges in Polymer Electrolytes with an Ether-Functionalized Anion, Angew Chem Int Ed, 2019, 58, 12070-12075.
[0421] A58 G. Lingua et al. Unique Carbonate-Based Single Ion Conducting Block Copolymers Enabling High-Voltage, All-Solid-State Lithium Metal Batteries, Macromolecules, 2021, 54, 6911-6924.Example 4 - Development and Characterization of Adaptive Polymer Interlayer for All-Solid-State Batteries with Lithium Metal Anodes
[0422] Abstract. Li-ion battery use continues to become increasingly prevalent across sectors from consumer electronics to electric vehicles. However, current Li-ion battery technology can pose safety concerns due to the flammable liquid electrolyte and are reaching their limit in achievable energy density. With this increasing demand for improved safety and energy density of batteries for widespread electrification, there is interest in solid-state batteries, especially Limetai solid-state batteries (LIMSSBs). LIMSSBs can improve safety by using a non-flammable solid electrolyte and improve energy density using a pure Li-metal anode. However, the unstable Li-metal / solid electrolyte interface, both mechanically and electrochemically, is one the main challenges that needs to be addressed to enable safe and durable LIMSSBs.
[0423] An adaptive polymer interlayer was investigated that could expand to reversibly maintain contact between the Li-metal anode and ceramic solid electrolyte during cycling. This adaptive property occurs through the polarization of conducting polymer (CP) particles that try to align along an electric field, causing the adaptive polymer to expand. The synthesis process and composition for the adaptive polymer interlayer including a pure CP film, solvent cast, and UV polymerization methods are compared and optimized before further characterization of the adaptive polymer interlayer. The adaptive property was successfully demonstrated with a UV polymerized adaptive polymer electrolyte comprising of CP particles in a polymer electrolyte matrix that exhibited appreciable expansion under relatively low electric field strengths. The adaptive polymer electrolyte was incorporated as an adaptive polymer interlayer in a pseudosolid full cell to compare the degradation to a baseline polymer interlayer, but thus far no difference in degradation was observed. Both polymer interlayers reduced the degradation compared to a bare Li-metal / ceramic electrolyte interface, but there may be insufficient electric field strength across the adaptive polymer interlayer to induce the adaptive property. A new adaptive property was demonstrated through the expansion of an adaptive polymer electrolyte under relatively low electric field strengths and set the groundwork for proving the feasibility of the adaptive property in an adaptive polymer interlayer incorporated in a solid-state cell between the Li-metal anode and ceramic solid electrolyte.
[0424] 1.1 Current State of Battery Technology. Since the commercialization of the rechargeable Li-ion battery in the 1990s, its use has become increasingly prevalent in the last few decades in everything from consumer electronics such as laptops and cellphones, grid energy storage, and electric vehicles. Li-ion battery technology has enabled the development of electric vehicles due to their greater specific energy and longer cycle life compared to otherrechargeable battery technologies such as lead-acid, nickel-cadmium, and nickel-metal hydride. However, current Li-ion batteries pose safety concerns due to the flammable liquid electrolyte and are reaching their limit in achievable energy density (amount of energy stored in a mass or volume). For ground-based electric vehicles alone, the demand for batteries is estimated to reach 245 GWh in 2030 [Bl, B2], With this rising demand for safe, high energy density batteries for electric vehicles and other applications such as grid storage and consumer electronics, solid-state electrolytes (SSE) have garnered interest. SSEs can offer improved safety due to less flammability and higher temperature operating range and have the potential to enable a Li-metal anode for higher energy density. In the commercial space, companies including Panasonic, Samsung SDI, QuantumScape, and Solid Power have been invested in trying to commercialize solid-state battery technology [B3 ] .
[0425] 1.2 Promise and Challenges of Solid-State Batteries. While a solid-state battery using conventional intercalation-based electrodes (those comm used in current liquid Li-ion batteries) can provide improved safety, the energy density of the battery can decrease due to the greater mass density and thus weight of SSEs, even if the thickness remains approximately the same. Therefore, the benefit of SSEs is with the use of a pure Li-metal anode, which can result in gravimetric (with respect to mass) and volumetric (with respect to volume) energy density gains of up to 40% and 70%, respectively. This is due to the anode being composed entirely of lithium, compared to conventional Li-ion batteries with anodes such as graphite where a limited amount of lithium intercalates and de-intercalates in the anode during cycling. These reasons motivate the interest in Li-metal solid-state batteries (LIMSSBs) [B4],
[0426] Solid-state batteries still face several challenges that currently prevent their commercialization and deployment at large scale including lower room temperature ionic conductivity compared to their liquid counterparts (although some recent compositions have matched or even exceeded that of liquid electrolytes [B5-B7]), processability of SSEs, and for LIMSSBs the solid interface with Li-metal both mechanically and electrochemically [B8-B13], Low ionic conductivity limits the Li-ion transfer capability of the SSE and reduces the rate at which the battery can charge or discharge [B8, B14, B 15] . For the Li-metal anode, a difference in its operation, compared to conventional intercalation anodes such as graphite (where Li-ions are removed or inserted within the structure during discharging and charging respectively), is that Li atoms are physically removed from (Li-metal to Li+ions) or deposited on (Li+ions to Li-metal) the Li-metal surface. This Li stripping and plating process, during discharging and charging respectively (typically an undesired and irreversible process for conventional anodes), is the reversible process by which Li-metal anodes operate. The volume and surface morphologyof the Li-metal anode directly changes with Li stripping / plating during operation [Bl 6, Bl 7], For the relatively rigid solid-solid contact between Li-metal and SSE, the Li-metal morphology change during cycling can quickly degrade the interface, resulting in non-uniform stripping and plating that ultimately causes the battery to fail [BIO, B18-B21], This is shown in FIG. 19, where a LIMSSB with no modifications can undergo interface degradation due to uneven Li stripping / plating causing contact loss and subsequent Li filament growth during plating.
[0427] Electrochemically, many SSE compositions, especially the high ionic conductivity sulfide ceramic SSEs, are not stable at the low potential in direct contact with Li-metal. SSEs can decompose into different products at the potential of Li / Li+, resulting in an interphase forming from these products. In some cases, such as for Li3PS4, the decomposition products (electrically insulative but ionically conductive) successfully passivate the interface to prevent further decomposition and allow operation. However, for other SSEs, such as LiioGeP2Si2, the decomposition products are electrically conductive and do not successfully passivate the interface, which results in the decomposition process continuing through the bulk of the SSE [B12, B 13] . This interface instability necessitates the use of an interlayer.
[0428] To mitigate the aforementioned issues, several solutions have been proposed in literature [B22-B28], Among others, polymer interlayers (as shown in FIG. 19) have been adopted to improve the initial contact at the interface to accommodate some of the volume changes due to Li stripping / plating. However, all these solutions do not guarantee long-term stability and reversibility of the interface contact, as these solutions have limited ability to maintain the interfacial contact in the event of uneven Li stripping / plating, eventually leading to the formation of voids or filaments.
[0429] 1.3 State of the Art for Solid-State Batteries. The solid-solid Li-metal and SSE interface in LIMSSBs has been recognized as a limiting factor for the performance and durability of LIMSSBs [B4, B8, B20, B21], Poor mechanical contact due to the rigid interface between the Li-metal anode and the ceramic SSE causes high interfacial resistance and uneven Li stripping and plating, which eventually leads to the growth of lithium filaments through the SSE. Due to the ductility and low density of Li-metal, these filaments are able to grow even through the dense SSE along the grain boundaries and cause the cell to short [B18, B19, B29], The straightforward method employed to improve the interfacial contact is to apply higher stack pressures, but the stack pressures required for stable cycling are often upwards of 10 MPa, which is not feasible for practical applications [B9, Bll], Other methods include engineered interfaces to provide better contact, as discussed below. Many ceramic solid electrolyte compositions (including the higher ionic conductivity compositions such as LiioGeP2Si2) suffer from narrowelectrochemical stability windows and are not directly stable with Li-metal [B8, B12, B13, B30], which necessitates the use of interphases or stable interlayers, such as the polymer interlayers discussed in below.
[0430] 1.3.1 Ceramic Solid Electrolytes. Comm studied ceramic SSE compositions can be grouped into oxides (such as LivLasZnOn based compositions) or sulfides (such as LiioGeP2Si2 or the Li2S-P2S5family including Li3PS4). Oxides typically have good stability, including with Li-metal, and sufficient ionic conductivities at room temperature, but can require high temperature sintering and have poor mechanical contact due to rigidity. Sulfides can exhibit high ionic conductivities at room temperature, upwards of 10 mS / cm, and their mechanical softness allows for cold pressing at room temperature and better interfacial contact. However, they often have lower stability with Li-metal, oxidation, and exposure to air generates toxic H2S gas [B8, B12, B13],
[0431] 1.3.2 Engineered Interfaces. Interfacial engineering to improve the contact between Li-metal and ceramic SSE generally employ techniques to make a lithiophilic surface on the ceramic SSE followed by melting Li on the surface. These techniques include atomic layer deposition or chemical treatment of the surface [B22, B23], The increased wettability with Li-metal results in initially good interfacial contact, as shown in FIGs. 20A-20D.
[0432] With atomic layer deposition of AI2O3, the interfacial impedance between Li-metal and Li7La2.75Cao.25Zn.75Nbo.250i2 ceramic SSE decreased from 1,710 cm2to 34 cm2. ALi symmetric cell showed stable cycling at room temperature for 90 hr at 0.2 mA / cm2(30 min each direction with 30 min rests in between), and a full cell with Li2FeMn30s cathode underwent 50 cycles at 0.1C [B22], The acid-salt treatment of the Li?La3Zr20i2 ceramic SSE decreased the interfacial impedance with Li-metal from 981.4 cm2to 11.6 cm2. ALi symmetric cell showed stable cycling at room temperature over 1000 hr at 0.5 mA / cm2(30 min each direction), and a full cell with LiNio.6Coo.2Mno.2O2 cathode underwent 100 cycles at 0.2 mA / cm2[B23] .
[0433] 1.3.3 Polymer Composite Solid Electrolytes and Interlayers. To address poor interfacial contact due to the rigid interface, accommodate some of the volume change of Li-metal stripping and plating, and improve the electrochemical stability of the SSE with the Li-metal anode, polymer composite SSEs or polymer interlayers have been studied with representative graphics shown in FIGs. 21 A-21B On the left in FIGs. 21A-21B is a composite SSE composed of Li?La3Zr20i2 nanofibers dispersed in a poly(vinylidenefluorideco-hexafluoropropylene) / ionic liquid matrix. At room temperature, a Li symmetric cell showed stable cycling for 800 hr at 0.2 mA / cm2(30 min each direction), and a full cell with LiMisOn cathode demonstrated 1000 cycles at 0.5C [B24], On the right in FIGs. 21 A-21B is apolyethylene oxide (PEO) based polymer interlayer with Lii.3Alo.3Tii.7(P04)3 ceramic SSE. The polymer interlayer decreased the interfacial impedance with Li-metal from 2491 cm2to 243 cm2. At 60 °C, a Li symmetric cell showed stable cycling for 200 hr at 0.1 mA / cm2(30 min each direction), and a full cell with LiFePCU cathode demonstrated 100 cycles at 0.3C [B25], Challenges for applying solid polymer electrolytes (SPE) alone in a LIMSSB include lower room-temperature ionic conductivity and insufficient strength to prevent Li filament growth through the entire separator [B21, B31, B32],
[0434] Composite SSEs combine the high ionic conductivity of ceramic SSEs with the flexibility and electrochemical stability of SPEs. These composites comm comprise of infiltration of a ceramic SSE template with an SPE, or ceramic SSE particles added as a filler to an SPE. While composites combine the benefits of both classes of electrolytes, the synthesis processes involved are often complex. In some instances, the resulting ionic conductivity is higher than the bulk ceramic filler, such as previous findings reporting 6.5 x 10'3S / cm for the composite at room temperature (compared to ~1.0 x 10'3S / cm for the bulk ceramic SSE, although the composite also contained ionic liquid) [B24], but often is a compromise between the ceramic SSE and the SPE conductivities [B26, B33-B35], Polymer interlayers can offer similar benefits by utilizing a ceramic SSE as the separator thickness with a thin SPE layer in between the Li-metal anode and ceramic SSE to provide the flexibility and electrochemical stability [B25, B27, B28], Synthesis processes for polymer interlayers are often simpler, and the separator thickness does not have to compromise on ionic conductivity (as with composite SSEs). Many of the currently reported applications of composite SSEs or polymer interlayers have been demonstrated at elevated temperature due to low room temperature ionic conductivity of the polymer component [B25-B28, B33-B35],
[0435] 1.4 Contribution and Structure of this Example. In summary, using solid electrolytes with a Li-metal anode can address the energy density and safety concerns of conventional liquid electrolyte Li-ion batteries, but the unstable Li-metal / solid electrolyte interface is one of the challenges that should be addressed for the realization of LIMSSBs. While some current methods improve the Li-metal interface, they have limited ability to maintain the interface in the event of non-uniform Li stripping and plating and cannot reversibly maintain the interface to assure long-term stability.
[0436] A new concept of polymer interlayer is disclosed that, under the influence of an applied electrical field, is able to expand and maintain the interface contact reversibly with the Li-metal anode as a LIMSSB is cycled, hence compensating for the inherent void formation mechanism. This concept involves the incorporation of a conducting polymer (CP) in the polymer interlayer.CPs are polarized and can try to align along an electric field, comm studied as an electrorheological (ER) property [B36-B42], The polarization of the CP could enable the interlayer to dynamically maintain the anode-SSE interface as the CP is polarized and tries to align along the electric field present in the battery. The objectives of this research are to synthesize, demonstrate and characterize the properties of an adaptive polymer electrolyte that expands under relatively low electric field strengths by exploiting the polarization of CPs. This is intended to be the first step for determining the feasibility of this electrolyte applied as an adaptive interlayer to maintain the interface with Li-metal anodes. This technology’s potential impact on the battery industry is a step toward enabling stable, long-lasting LIMSSBs through addressing the interfacial stability issue with Li-metal anodes, bringing LIMSSBs closer to commercial realization.
[0437] Optimizing the composition and synthesis process for the adaptive polymer interlayer by characterizing a pure CP film, solvent cast polymer electrolyte, and UV polymerized polymer electrolyte is disclosed. The final composition as discussed below can be characterized with additional physical, mechanical (adaptive response), and electrochemical characterizations. These characterizations verify the adaptive capability of the polymer and compare the physical and electrochemical properties to a baseline, non-adaptive composition. The ceramic solid electrolyte utilized with the polymer interlayer, synthesis of a thin polymer interlayer, and comparing the performance of LIMSSB cells with an adaptive polymer interlayer to cells with a baseline, non-adaptive polymer interlayer through electrochemical testing is discussed below. The contribution of this work and outlines of future directions is discussed.
[0438] Section 2: Selection of Adaptive Polymer Interlayer Composition. This section explores the concept of an adaptive polymer interlayer that, through its expansion under an electric field, could reversibly maintain interfacial contact with the Li-metal anode. The conducting polymer trying to align as it is polarized under an electric field is utilized for the adaptive property. This section focuses on selecting and optimizing the synthesis process for the adaptive polymer interlayer. First, a pure conducting polymer film was synthesized to produce a thin, free-standing film to apply as the interlayer. Next, compositions of a polymer electrolyte matrix for a composite film, which can comprise of conducting polymer particles in a polymer electrolyte matrix, were synthesized. These included solvent cast or UV polymerized polymer electrolyte compositions. The compositions were compared physically, mechanically, and electrochemically. Qualitative physical and mechanical comparisons were how viscous or spreadable the uncured polymer solution is, the film forming ability, and strength and flexibility of the cured polymer film. Electrochemically, the ability of the films to transfer Li-ions werecompared for their prospect of application as interlayers.
[0439] 2.1 Conducting Polymers and Electrorheological Properties. Conducting polymers (CPs) such as polypyrrole doped with dodecylbenzenesulfonate (PPy(DBS)) and polyaniline (PANI) with their chemical structures illustrated in FIGs. 22A-22B exhibit electrorheological (ER) properties, where CP particles dispersed in an insulative matrix align along an applied electric field. This phenomenon is due to the mobility of electrons in the CPs, which allows the particles to be polarized under an electric field.
[0440] The ER behavior of CPs is typically studied in ER fluids such as CP particles dispersed in silicone oil [B36-B40]. In ER fluids, the ER response can be measured with the increase in shear stress of the fluid under an applied electric field (shown in FIG. 23 A) as the particles align and increase the apparent viscosity of the fluid. FIG. 23B shows a light microscopy image where the particles align under an applied electric field.
[0441] While ER properties are well studied in fluids, research on ER polymers or elastomers has focused on the change in storage modulus under an electric field rather than on deformation or expansion responses [B41, B42, B45, B46], PPy -based composites have displayed this response under electric fields as low as 0.1-0.2 V / pm [B36, B37, B39, B41], In this research, the CP PPy(DBS) was synthesized and investigated for an adaptive polymer interlayer, which is the first known application where a volume change (expansion / contraction) of a solid material (polymer) is induced using the polarization of CP particles under an electric field.
[0442] The adaptive polymer interlayer is envisioned for application to all-solid-state lithium-ion cells, specifically as a protective layer between the Li-metal anode and the ceramic solid electrolyte that is engineered to preserve interfacial contact and mitigate dendrite formation. A conceptual representation of the adaptive polymer interlayer’s working principles is shown in FIGs. 24A-24B as a bulk CP film or composite film of CP particles in a polymer electrolyte matrix. It is hypothesized that the adaptive polymer interlayer could expand under an electric field present in a battery to maintain interfacial contact with the anode. As long as some contact is maintained, the electric field across the interlayer would induce expansion to restore interfacial integrity. Although this approach may result in a slight reduction in energy density due to the presence of the interlayer as an inert material (unable to store lithium) in the battery cell, the expected benefits include improved durability and safety.
[0443] 2.2 Conducting Polymer Film for the Adaptive Polymer Interlayer. One of the challenges in synthesizing the adaptive polymer interlayer for use in a Li-metal solid-state battery (LIMSSB) is to minimize the thickness. Achieving this target can minimize the impact on energy density of the cell, the bulk impedance, and result in a greater electric field strengthacross the interlayer for the given potential difference.
[0444] A common method for polymerizing CP films is by electropolymerization on an inactive, electrically conductive substrate (such as steel or gold) with the CP film being on the substrate in its final application. This method could be advantageous for some specific applications, for example utilizing the CP film as a corrosion-protective coating of the substrate or utilizing the CP film as a sensor layer with the substrate to provide an electrical connection to external circuitry [B47, B48], Improving the adhesion of the CP for these applications through methods such as increased surface roughness is desirable [B49, B50], However, for other applications, a free-standing CP film is desirable, such as flexible electrodes for energy storage devices, bilayer actuators, artificial muscles [B51-B53] or as an interlayer in this work. These films are typically prepared thick enough (10-15 pm or thicker) to be mechanically peeled off the substrate [B51, B52, B54, B55], Chemical polymerization methods such as interfacial polymerization at an air / liquid or liquid / liquid interface have been shown to produce ultrathin free-standing CP films (tens to hundreds of nanometers thick). However, the film growth can be slow (hours to days) in many cases [B56-B59],
[0445] Electrochemical delamination of polypyrrole doped with dodecylbenzene sulfonate (PPy(DBS)) was investigated for this work for quickly obtaining electropolymerized freestanding CP films that are thinner than mechanical peeling. Electropolymerization is advantageous because it can provide better control of film thickness and morphology [B51], relatively fast polymerization, superior electrochemical characteristics [B60], and no chemical oxidant is needed. The processes of electropolymerization, electrochemical delamination, and resulting free-standing PPy(DBS) films have been developed and investigated as part of prior work, and described in [B61 ]. In this study, conductive substrates for electropolymerization were prepared by mechanical polishing with aluminum oxide polishing paper for the 304 stainless steel chip (304SS, 15.5 mm dia.) down to 1 pm grit size, then both the 304SS and electron beam physical vapor deposited (EBPVD, 5 mm dia.) gold substrates were rinsed with ethanol, deionized (DI) water, and air-dried. The electropolymerization area was set by a polytetrafluoroethylene (PTFE) O-ring for the 304SS or by insulative and chemically inert silicon nitride coating for the EBPVD gold. The substrates were then electrochemically cleaned by performing cyclic voltammogram sweeps from -0.2V to 1.2V vs. Ag / AgCl at a scan rate of 50 mV / s in 50 mM NaOH aqueous solution until the current response was repeatable then rinsed thoroughly with DI water. For electropolymerization, an aqueous electropolymerization solution of 100 mMNaDBS and 200 mM pyrrole was used. PPy(DBS) films were electropolymerized with square waves at potentials of -100 mV vs. Ag / AgCl for 3s followed by 775 mV vs.Ag / AgCl for 10s until reaching the desired electropolymerization charge density at the end of an oxidation step (to prevent oxygen attack from air exposure upon removing film from solution) then rinsed thoroughly with DI water. Square wave electropolymerization has been reported to produce films with low adhesion to the substrate suitable for removal due to the intermediate oxidized state of the film [B52, B54], For electrochemical delamination of the PPy(DBS) film, an aqueous cycling solution of 100 mM NaDBS was used. The film underwent up to 50 cyclic voltammogram oxidation - reduction sweeps between 0.5 V and -1.5 V vs. Ag / AgCl at a scan rate of 50 mV / s.
[0446] Electrochemical delamination resulted in intact, free-standing PPy(DBS) films shown in FIGs. 25A-25B Cross-sectional views show films were obtainable down to 7.2 pm thick from 304SS substrate in FIG. 26A and 0.8 pm thick from EBPVD gold substrate in FIG. 26B.
[0447] For initial testing, solid-state Li-metal symmetric cells (Li / interlayer / ceramic / interlayer / Li) with bulk PPy(DBS) films as the interlayers were assembled in a custom Swagelok pressure cell shown in FIG. 27 under 1 MPa stack pressure at room temperature (20-25 °C). Commercial Li6.4La3Zn.4Tao.6O12 pellets were used as the ceramic solid-state electrolyte. However, the cells could not be cycled and did not display Li-ion transfer capability. Li cycling tests at ±0.1 mA / cm2immediately reached cutoff voltages (±3V) when attempting to cycle, and EIS measurements showed practically infinite impedances supporting the conclusion that there was a lack of Li-ion transfer through the bulk PPy(DBS) film in solid-state. The bulk PPy(DBS) film could not be investigated in Li / PPy(DBS) / Li symmetric cells, as the high electrical conductivity of the films (>10 S / cm) would electrically short the cell. Also, even if the bulk PPy(DBS) film were to allow cycling, the electrical conductivity might inhibit polarization and expansion of the interlayer as an appreciable electric field across the interlayer may be difficult to maintain.
[0448] The lack of Li-ion transfer could be in part due to the porosity of the bulk PPy(DBS) film being incompatible with a solid-state system. Li-ion transfer through bulk CP film has typically been demonstrated in liquid cells where liquid electrolyte may infiltrate the porous film [B62] . In the solid-state system, the electrolyte is not infiltrated into the pores of the film and is contacting the surface, which may lead to limited Li-ion transfer through the CP film. If the Li-ions are transported through the liquid electrolyte (Li-ion transfer occurring through the pores of the CP film), not through the bulk of the CP film, then no Li-ion transfer would occur.
[0449] 2.3 Composite Film of Conducting Polymer Particles in a Polymer Matrix. To overcome the limitations of applying a bulk CP film as the adaptive polymer interlayer, composite films with PPy(DBS) CP particles dispersed in a polymer electrolyte matrix wereinvestigated. PPy(DBS) particles were chemically polymerized as described previously, reported to have an electrical conductivity of approximately 21.7 S / cm and molecular weight per residue of approximately 138.4 g / mol [B63], Details of the synthesis process are described below.
[0450] For the polymer electrolyte matrix to disperse the PPy(DBS) particles in, a polymer electrolyte that can operate near room temperature (25 °C) is desirable for more equivalent comparisons between the electrochemical, physical, and mechanical (adaptive response) characterization techniques used in this work. Polyethylene oxide (PEO) based polymer electrolytes are widely studied and can achieve adequate room temperature ionic conductivity (>0.1 mS / cm at 25 °C) if the crystallinity can be inhibited [B64-B67], Thus, a PEO based polymer electrolyte was used as the polymer electrolyte matrix in which the PPy(DBS) particles were dispersed. Two common methods to synthesize a PEO polymer electrolyte are solvent casting [B64, B65] or UV polymerization [B66, B67], Solvent casting involves dispersing the components of the polymer electrolyte in a volatile solvent, spreading the mixture into a layer, then evaporating the solvent under elevated temperature and vacuum leaving behind a polymer film. UV polymerization involves mixing the components of the polymer electrolyte, spreading the mixture into a layer, then cross-linking the polymer chains under UV irradiation resulting in a polymer film.
[0451] 2.3.1 Solvent Cast Synthesis. For solvent cast PEO based polymer electrolyte, compositions previously adapted [B64] were investigated. One method for inhibiting the crystallinity and improving the ionic conductivity of the polymer electrolyte is the addition of a plasticizer, such as succinonitrile (SN) [B64, B65], PEO with 600k molecular weight (MW) was used in the composition. Lithium bis(trifluoromethane)sulfonimide (LiTFSI) was used as the Li salt, of which increasing amounts can increase the ionic conductivity due to increased availability of Li-ions in the polymer electrolyte and the Li salt exhibits a plasticizing effect. The synthesis process is summarized in FIG. 28 and compositions summarized in Table 5, with ionic conductivities obtained from electrochemical impedance spectroscopy (EIS) measurements of polymer electrolyte film sandwiched between stainless steel blocking electrodes.Table 5: Solvent cast PEO based polymer electrolyte compositions.
[0452] Li+:EO ratio SN (wt% of PEO) Ionic conductivity at 25 °C (S / cm2) 1:32 0 1.6 x IO’6
[0453] 1:32 45 3.2 x IO’6
[0454] 1:14 5 4.0 x 10’5
[0455] 1:12 5 5.2 x 10’5
[0456] 1:10 0 4.0 x 10’5
[0457] 1:10 5 1.1 x IO’4
[0458] 1:10 15 2.2 x IO’4
[0459] 1:8 0 1.8 x IO’4
[0460]
[0461] The addition of large amounts of SN with low Li salt was not found to reduce the crystallinity of the film and improve the ionic conductivity as much as reported. The actual reduction in crystallinity measured with X-ray diffraction (XRD) compared to the expected reduction is shown in FIGs. 29A-29B. The two sharp peaks between 18 - 25° 29 indicate crystalline content of the film by strongly diffracting the incident X-rays, producing a large signal. In this work, the first peak intensity slightly decreases and the second peak res about the same, whereas previous reports showed slight decrease in the first peak and a drastic decrease in the second peak [B64], For increasing Li salt amounts going down the table (from 1 : 14 to 1:8 Li+:EO ratio), adding >10 wt% of SN or too much Li salt can degrade the mechanical properties of the film. The 1 : 14 Li+:EO with 5 wt% SN composition was selected to pursue for additional experiments as it showed a suitable balance of properties.
[0462] Another advantage of investigating a composite film for the adaptive polymer interlayer is the polymer electrolyte matrix is electrically insulative and can be tested as a standalone electrolyte in Li-metal symmetric cells (Li / polymer / Li) without the additional variable of the ceramic solid electrolyte. If the polymer electrolyte matrix displays suitable performance, a composite with PPy(DBS) CP particles can also be tested as a standalone electrolyte prior to incorporation as an interlayer with ceramic solid electrolyte. The 1 : 14 Li+:EO with 5 wt% SN composition was first tested in Li / polymer / Li configuration in the Swagelok pressure cell shown in FIG. 27 under 1 MPa stack pressure at room temperature. A factor for the cells was the time required for the interphase to form between PEO-based polymer electrolyte and Li-metal, as PEO-based polymer electrolytes are not stable with Li-metal but form a stable interphase. Atroom temperature, the formation of the interphase is slow and can take several days, although the process can be accelerated by heating the cells (such as at 80 °C overnight [B66]).
[0463] For the Li / polymer / Li cell in the Swagelok setup, after letting the interfacial impedance stabilize over a few days, the Li cycling and intermittent EIS results are shown in FIGs. 30A-30C. While Li cycling at a current density of 0.1 mA / cm2, the overpotential between electrodes started at around 0.75 V at ambient temperature. The total impedances ranged from 10-50 k cm2, which are high compared to literature showing 600-3000 cm2at room temperature [B25, B33, B66, B67], These high overpotentials and impedances suggest this polymer electrolyte composition may not be suitable for room temperature operation. Also, the lab room temperature had large fluctuations and dropped between 13 °C and 20 °C during this testing, which had an effect on the electrochemical testing as polymer electrolytes are sensitive to lower temperatures. This is supported by the fluctuations in overpotentials and impedances over time, even though stack pressure fluctuations would also have an effect. However, both the interfacial impedance (approximately the diameter of semicircle) and bulk electrolyte impedance (approximately the left intercept of semicircle) vary between cycles, as shown in the intermittent EIS spectra. The bulk electrolyte impedance should not change much with cycling, indicating that temperature changes affect the polymer electrolyte bulk ionic conductivity.
[0464] For additional tests, Li / polymer / Li cells were assembled and sealed in CR2032 coin cells to allow for controlled heating and temperature of the cells in a thermal chamber, outside a glovebox. The cell stack configuration inside the coin cell is shown in FIG. 10. The controlled heating can accelerate the Li / polymer electrolyte interphase formation after assembly, and controlling the temperature enables more consistent electrochemical testing. Furthermore, building coin cells can allow for multiple samples to be tested simultaneously, compared to the single Swagelok cell setup. On the other hand, coin cell testing offers limited ability to control the stack pressure.
[0465] After assembly, the cell was placed in an environmental chamber at 70 °C for 24 hr (70 °C used due to temperature limits of potentiostat wiring and coin cell holders), with periodic EIS measurements performed on the cell, as shown in FIG. 31. The interface appeared to stabilize in about 12 hr. While elevated temperatures accelerate the interface stabilization process, the polymer electrolyte impedance at 25 °C was still exceedingly high. The Li cycling overpotentials and impedances at 50 °C shown in FIG. 32 were more acceptable, but the elevated temperature for electrochemical testing would prohibit equivalent comparison to physical and mechanical (adaptive response) characterizations that are not readily performed at elevated temperatures. As a conclusion of this experiment, alternative compositions for the PEO based polymer electrolytehad to be developed using UV polymerization synthesis, as illustrated in the following section.
[0466] 2.3.2 UV Polymerization Synthesis. Alternative PEO based polymer electrolyte compositions were synthesized using UV polymerization, in an attempt to improve the electrochemical performance at room temperature. Additional advantages of UV polymerization compared to methods such as slow thermal polymerization or solvent evaporation synthesis include the rapid polymerization process and no use of volatile solvents [B66, B67], The relatively simple PEO based polymer electrolyte from previous reports [B66] was replicated first to determine if the resulting polymer displays adequate performance at room temperature. The synthesis process is summarized in FIG. 33. While the process was replicated as closely as possible, parameters that could not be replicated due to equipment limitations were pressure of the hot-press limited to 4.4 bar (compared to 20 bar [B66]) and the hot-pressing was done in ambient air instead of a dry -room.
[0467] As replicated from previous reports (apart from the mentioned parameters), the UV polymerized PEO based polymer electrolyte performed better than the solvent cast synthesis with an ionic conductivity of 0.10 mS / cm at 25 °C (compared to 0.04 mS / cm for 1 : 14 Li+:EO with 5 wt% SN solvent cast composition) and total impedance in Li symmetric coin cells of ~10 kQ cm2(compared to 10-50 kQ cm2). However, the total impedance was still larger than the -700 Q cm2reported by literature [B66] . Also, the polymer solution prior to hot pressing is a paste-like consistency, which would make it more difficult to achieve a thin interlayer with this composition between Li-metal and ceramic solid electrolyte. Thus, the UV polymerization composition and process is further refined in the next section.
[0468] 2.4 Refinement of UV Polymerization Process. Refining the UV polymerization composition and process summarized in FIG. 34, the composition was first adapted from previous reports [B67] with the addition of tetraethylene glycol dimethacrylate (TEGDMA) as a cross-linking short chain monomer that can inhibit crystallinity and improve interfacial contact with Li-metal. Also, their composition resulted in a polymer solution that is a viscous, pourable liquid prior to hot-pressing and UV curing, which could enable a thinner interlayer between Li-metal and ceramic solid electrolyte. Increasing amounts of TEGDMA were reported to increase the brittleness and rigidity of the polymer film. A 1 :2 TEGDMA:PEO w: w ratio was reported to provide a balance between improved interfacial adhesion and inhibited crystallinity without the film becoming too brittle or rigid.
[0469] PEO (MW 100k) as the long chain polymer gives a balance between mechanical properties and potential for lower crystallinity. Higher molecular weights of PEO can improve mechanical strength but can result in more rigid films and inhibit the transfer of Li-ions,decreasing the ionic conductivity. Lower molecular weights of PEO can become increasingly flexible but reduce mechanical strength and may not produce cohesive films. Tetraethylene glycol dimethyl ether (TEGDME) is a cross-linking plasticizer that can further reduce crystallinity and reduce the coordination of Li-ions with EO in long chain PEO, improving the ionic conductivity. However, too much TEGDME can reduce the mechanical strength and prevent cohesive films from forming. LiTFSI as the Li salt is the salt of choice in polymer electrolytes, showing relatively high ionic conductivity and the TFST anion can have a plasticizing effect further reducing crystallinity of the polymer electrolyte. Increasing amounts of LiTFSI typically increase the ionic conductivity to a limit but can weaken the film and at too high amounts, preventing a cohesive film from forming. Excessive Li from too much LiTFSI can also inhibit Li-ion transfer, eventually resulting in lower ionic conductivity.
[0470] 4-methylbenzophenone (MBP) is a hydrogen abstraction photoinitiator used to generate free radical chains from the methylene groups in PEO, TEGDMA, and TEGDME for UV-polymerization. Decreasing the amount of MBP can result in longer UV curing times and could potentially result in an uneven cure with too little photoinitiator, causing some areas of the film to be overcured by the time the film has finished curing overall. Conversely, excess photoinitiator could cause increased interfacial impedance due to increased storage modulus [B68] or premature termination and incomplete cure of the polymer matrix [B69] . During polymerization, excess photoinitiator could cause more polymer chains to become crosslinked leading to a higher crosslink density. An increased storage modulus could result from the higher crosslink density due to less mobility within the polymer chains and the polymer would not be able to conform as easily to the Li-metal surface, increasing the interfacial impedance. An incomplete cure could lead to less crosslinks in the matrix than expected or inhomogeneous crosslinking. Regions of lower crosslinking could have higher mobility and leaching of noncrosslinked moi eties and regions of higher crosslinking could have more defects resulting in cracks or voids in the interface.
[0471] Literature did not report the amount of MBP photoinitiator used [B67] so the same amount as the previous composition attempted (from Porcarelli and coworkers [B66]) of 7.5 wt% was used first. At 25 °C, the resulting polymer electrolyte had approximately the same ionic conductivity, but the total impedance in Li symmetric coin cells (Li / polymer / Li) was reduced by about half (-5000 Q cm2compared to -10 kQ cm2). However, this amount of MBP is not likely needed, as both the UV intensity (150 mW / cm2compared to 40 mW / cm2) and UV curing time (15 min compared to 6 min) were greater. In addition to the aforementioned reasons, excess photoinitiator may result in more unreacted free radicals remaining after polymerization that caninduce undesirable side reactions with Li-metal [B31], To better compare the curing between different compositions and amounts of MBP photoinitiator, insoluble fraction measurements were performed. The insoluble fraction is a measure of the cross-linking percentage of the film as the non-cross-linked components can still be soluble in an applicable solvent. To perform the insoluble fraction measurement, 14.3 mm dia. samples (n = 5 samples for each composition) were punched out from a UV cured film. Each sample was sandwiched between two stainless steel meshes as shown graphically in FIG. 35 A, the corners were bent to hold the sample, and the sample was soaked in acetonitrile overnight to remove the soluble components. After soaking, the films were vacuum dried at 40 °C overnight, then the final weights of the films are divided by the initial weights to obtain the insoluble fraction (as wt% of initial film weight). The results are shown in FIG. 35B. The film using the composition from literature [B66] was above the target 40% insoluble fraction reported, but the various samples from the film showed a large variability. This could indicate non-uniform curing across the film which could be due in part to the high amount of MBP photoinitiator (7.5 wt%) and short curing time. The adapted composition from literature [B67] with 7.5 wt% MBP was above the target 50% insoluble fraction reported, even when reducing the curing time to 10 min. The variability from the samples across the film was much smaller, suggesting the longer cure time or addition of TEGDMA cross-linking monomer results in a more uniform cure. The insoluble fraction did not change much with the reduced curing time of 10 min, suggesting the film is already fully cured before that point and is likely being overcured. Thus, the amount of MBP photoinitiator can be reduced. The amount of MBP was reduced to 3 wt% (according to the amount the group uses in a different UV cured polymer composition [B70]) and cured at 10 min or 15 min. The insoluble fraction slightly decreased compared to 7.5 wt% MBP but was still above 50% insoluble fraction and low variability.
[0472] The composition adapted from [B67] with 3 wt% MBP showed a similar interfacial impedance while the ionic conductivity slightly increased from ~0.10 mS / cm to ~0.14 mS / cm at 25 °C. However, the impedance would still take several days to stabilize. While resting at elevated temperature can accelerate the stabilization, it can also induce undesirable side reactions. Adding lithium bis(oxalato)borate (LiBoB) as an additional Li salt has lower ionic conductivity than LiTFSI but used in small amounts can improve the interface stability with Li-metal [B71], Too much LiBoB can decrease the overall ionic conductivity of the polymer electrolyte, but too little can be insufficient to help stabilize the interface with Li-metal. Adding LiBoB to the composition as 20 wt% of the LiTFSI amount did not change the insoluble fraction, impedance, or ionic conductivity, but the impedance was stable after ~2 days resting at25 °C. XRD was performed to compare the crystallinity of this composition the original composition found in literature [B67], as shown in FIGs. 36A-36B. Both this composition and that reported in [B67] (labeled as PTT-SPE) appear almost entirely amorphous as no sharp crystalline peaks are displayed in the XRD spectra.
[0473] Proceeding with this polymer electrolyte composition and synthesis process, greater than 10 Li symmetric coin cells (Li / polymer / Li) were made for electrochemical testing as the baseline polymer electrolyte matrix (with no CP PPy(DBS) particles). The intermittent EIS spectra of a middle performing cell during Li cycling is shown in FIG. 37. For all the cells, the ionic conductivity of the polymer electrolyte was between 0.13-0.16 mS / cm and interfacial impedance between 2.5-5.5 kQ cm2. Additional characterizations of this baseline polymer electrolyte matrix and varying amounts of Ppy(DBS) CP particles are discussed in the following section.
[0474] 2.5 Summary. The rationale and steps taken to optimize the synthesis process for the adaptive polymer interlayer were described, which can be characterized and applied in the remainder of this example. First, a pure PPy(DBS) conducting polymer film was tested.
[0475] However, a lack of ion-transfer through the conducting polymer film was observed when incorporated in a solid-state cell, suggesting its incompatibility. The electrical conductivity of a pure conducting polymer film could also prevent an appreciable electric field being maintained across the interlayer.
[0476] Next, two different synthesis methods of a polymer electrolyte matrix were investigated for a composite film that would comprise of conducting polymer particles in the polymer electrolyte matrix - solvent cast or UV polymerization. The polymer electrolyte matrix should exhibit adequate electrochemical performance at room temperature to allow more equivalent comparison between electrochemical, physical, and mechanical (adaptive response) characterization techniques in this work that cannot readily be performed at elevated temperatures. A low viscosity was also desirable to enable synthesis of a thin interlayer when incorporated with a ceramic solid electrolyte. PEO based polymer electrolytes were investigated as they are widely studied and can achieve sufficient performance at room temperature if the crystallinity can be inhibited.
[0477] For the solvent cast synthesis method, while the viscosity can be easily adjusted with the amount of solvent, the compositions tested that achieved an ionic conductivity greater than 0.1 mS / cm at 25 °C had poor mechanical properties. The composition with a balance of mechanical and electrochemical properties had an ionic conductivity of 0.04 mS / cm at 25 °C and total impedance ranged from 10-50 kQ cm2. Swagelok cells were initially used for precisely controlling the stack pressure of the cell, but the polymer electrolyte was susceptible to lab roomtemperature fluctuations affecting the electrochemical performance. Thus, testing was transitioned to CR2032 coin cells to allow for controlled temperature of the cells in an environmental chamber, at the cost of limited ability to control the stack pressure. The solvent cast polymer electrolyte composition had adequate electrochemical performance at elevated temperature (50 °C), so alternative compositions had to be investigated using UV polymerization.
[0478] In addition to attempting to improve the electrochemical performance at room temperature, UV polymerization also has the advantage of a rapid synthesis process and no use of volatile solvents. The first UV polymerized composition, replicated from [B66], possessed sufficient electrochemical properties at 25 °C (ionic conductivity of 0.10 mS / cm and total impedance of approximately 10 kQ cm2) but was a paste-like consistency prior to polymerization, which would not readily enable synthesis of a thin interlayer. The composition was modified and the addition of a cross-linking short chain monomer (TEGDMA) from [B67], adjustment of photoinitiator amount, and additional Li salt (LiBoB) resulted in a final composition that had a viscous but pourable liquid consistency, ionic conductivity between 0.13 and 0.16 mS / cm, and interfacial impedance between 2.5 and 5.5 k cm225 °C. The synthesis process of the final composition is also described below.
[0479] Section 3: Characterization of Adaptive Polymer Electrolyte. The results of additional physical, mechanical (adaptive response), and electrochemical characterizations on the final UV polymerized composition of the baseline polymer electrolyte matrix discussed above and composites with varying amounts of polypyrrole doped with dodecylbenzenesulfonate (PPy(DBS)) conducting polymer (CP) particles in this polymer electrolyte matrix, also described in [B72] are presented. This baseline polymer electrolyte synthesis process and composition is summarized below in FIG. 2 and further detailed below. The composition comprised of 30.3 wt% polyethylene oxide (PEO, 100,000 MW), 15.1 wt% tetraethylene glycol dimethacrylate (TEGDMA), 30.3 wt% tetraethylene glycol dimethyl ether (TEGDME), 17.8 wt% lithium bis(trifluoromethane)sulfonimide (LiTFSI), 3.5 wt% lithium bis(oxalato)borate (LiBoB), and 3.0 wt% 4-methylbenzophenone (MBP). PPy(DBS) CP particles were added as an additional 0-2 wt% of the PEO and TEGDMA amounts (0-0.9 wt% of total components, approximately 0-15 vol% of final polymer electrolyte film) for their properties of polarizing and trying to align under an electric field making an adaptive polymer electrolyte (A-PE) composite. The PPy(DBS) particles are insoluble in the polymer electrolyte solution and can remain as particles dispersed in the cured polymer electrolyte matrix. PPy(DBS) added as up to 0.9 wt% of the total components is well below the percolation threshold reported for roughly spherical PPy particlesof at least 3-5 wt% [B73, B74], Hereafter, the amount of PPy(DBS) is referred to as the wt% of PEO and TEGDMA amounts in the compositions (0-2 wt% of the polymer and monomer). The thickness of the film was set to around 125 pm with the spacer and pressed to a final 6 cm x 10 cm area. Compositions with 0, 0.25, 0.5, 1.0, and 2.0 wt% PPy(DBS) were characterized.
[0480] 3.1 Procedures for Characterization of Adaptive Polymer Electrolyte. The polymer electrolyte films were characterized with a combination of physical, mechanical, and electrochemical tests. Physical characterizations comprised of insoluble fraction, electrical conductivity, X-ray diffraction (XRD), differential scanning calorimetry (DSC), and dynamic mechanical analysis (DMA). Mechanical response characterizations included block force response and atomic force microscopy (AFM). Electrochemical characterizations comprised of electrochemical impedance spectroscopy (EIS), Li-Li symmetric cycling, and electrochemical stability window (ESW).
[0481] 3.1.1 Physical Characterizations. The insoluble fraction measurements were performed by taking the initial dry weight of the film (14.3 mm dia.), sandwiching the film between 304 stainless steel mesh, soaking in acetonitrile overnight at room temperature (20-25 °C) to dissolve the soluble (non-cross-linked) components [B66, B67], vacuum drying (gauge pressure -0.95 bar) overnight at 40 °C, and taking the final dry weight of the film. Electrical conductivity measurements were performed with the polymer film between copper foil contacts, using an Extech EX330 multimeter to obtain the electrical resistance.
[0482] XRD was collected at room temperature (20-25 °C) from 10° to 40° 29 with a Rigaku MiniFlex 600 with a Cu K-a radiation source (k = 1.5406A) at 40 kV voltage and 15 mA current. DSC was performed with a TA Instruments DSC 2500 (TA Instruments-Waters LLC, New Castle, DE). Samples between 2.5 mg to 7.5 mg were used in Tzero hermetic aluminum pans. Samples were cooled from room temperature to -90 °C at 10 °C / min, then heated to 120 °C at 5 °C / min. This process was repeated for a second scan to remove any thermal history. In the DSC analysis, the glass transition temperature (Tg) was determined from the inflection point in the slope towards the middle of the glass transition step. The DSC slope of heat flow after the glass transition was determined by performing a linear regression of the slope from -20 °C to 120 °C. DMA was performed with a TA Instruments Q800 (TA Instruments-Waters LLC, New Castle, DE) equipped with a tension clamp and Thermal Advantage Q Series version 5.5.22 software. The DMA was operated under tension analysis (0. IN preload) on polymer films with sample dimensions of 20 mm L (±1 mm) x 10.5 mm W (±0.6 mm) x 0.28 mm T (±0.2 mm) from -120 °C to 150 °C at a 3 °C / min heating rate and a 1 Hz frequency. Thicker films for DMA were obtained by using thicker spacers in the synthesis process.3.1.2 Mechanical Response Characterizations. AFM was used to measure the expansion response of polymer electrolyte films under an applied electric field at room temperature (20-25 °C) in air. A schematic of the AFM sample setup and picture of a sample are shown in FIG. 3 A and FIG. 3B, respectively. Small alterations were made to the polymer synthesis process for producing ~10 pm thick polymer film samples. Polymer solution was poured onto an indium tin oxide (ITO) coated PET sheet (ITO-PET, 130 nm thick ITO coating on one side of 178 pm thick PET, surface resistivity 60 Q / sq, Sigma-Aldrich) with the ITO side facing up to form a 15 mm dia. pool of solution, then hot-pressed between another ITO-PET sheet (ITO side facing polymer solution) without any spacer. After curing, one of the ITO-PET sheets was peeled off and 1 cm x 2 cm samples of 10 pm thick polymer on ITO-PET were cut out. A 50 nm thick layer of gold was sputtered on top of the polymer using a 20 mA sputter current with an EMS150R ES sputter coater (Electron Microscopy Sciences / Quorum). The outer edges of the sample were cut off then a section of polymer film was removed on one end, and copper tape attached to the ITO-PET for the bottom electrical contact. Another copper tape was attached to the gold coating as the top electrical contact, with insulative tape between the top and bottom copper tapes to prevent electrical shorting. The sample was attached to a glass slide using double-sided tape then loaded into an MFP-3D Infinity AFM system (Oxford Instrument, Asylum Research). The cross-section and gold-coated surface morphology were investigated with a Thermo Scientific Apreo scanning electron microscope (SEM). The thicknesses of the films were confirmed to be approximately 10 pm thick by measuring with a micrometer and with cross-sectional SEM shown in FIG. 9.
[0483] Continuous point measurement with the AFM probe in contact with the sample surface was used to measure the displacement of the film over time. The displacement of the film surface (expansion and contraction) was obtained from the Z-piezo movement required to maintain a constant cantilever deflection. A commercial AFM cantilever was used for continuous point measurements (Olympus AC160-R3, nominal spring constant 4 N / m, nominal tip radius 7 nm, and nominal resonant frequency 300 kHz). An NI USB-6008 multifunction I / O data acquisition module (National Instruments) was used with Lab VIEW to apply a voltage for different electric field strengths across the polymer film for periods of 10 min excitations (voltage applied) followed by 10 min relaxations (no voltage applied). Additionally, topography maps were obtained using tapping mode using a commercial AFM cantilever (Olympus AC240-R3, nominal spring constant 2 N / m, nominal tip radius 7 nm, and nominal resonant frequency 70 kHz).
[0484] A simplified schematic of the block force setup (insulative layers between electricallyconductive components not shown) used for measuring the force response of the polymer electrolyte compositions under an electric field at room temperature (20-25 °C) in air is shown in FIG. 7A. The film (14.3 mm dia., 125 pm thick) was sandwiched between 304 stainless steel (304SS) spacers (15.5 mm dia.) with conductive adhesive copper tape attached to each 304SS spacer for electrical connection. A calibrated MF01 A-N-221-A04 membrane force sensor (Alpha Taiwan) was used to measure the force. A polytetrafluoroethylene (PTFE) spacer (9.5 mm dia., 1.0 mm thick) was used between the membrane force sensor and the 304SS / polymer electrolyte / 304SS stack to ensure the force was applied in the membrane force sensor active area (10.2 mm dia.) and for electrical isolation. This stack was clamped between insulated surfaces of a small vice mounted on a vibration isolation table. A programmable DC power supply (Tektronix PWS4305) connected with a linear amplifier (Piezo Systems, Inc. model EPA-104) was used to apply a voltage for different electric field strengths across the polymer electrolyte film. Deviations in the membrane force sensor readings from a stable ~1N clamp force were monitored to determine the force response of the polymer electrolyte. This setup roughly corresponds to the polymer electrolyte as an interlayer sandwiched between a Li-metal anode and ceramic solid electrolyte, however, the clamp force used here is lower than the stack pressure would be in a solid-state battery due to resolution limitations of force sensors with higher load capacities.
[0485] 3.1.3 Electrochemical Characterizations. CR2032 coin cells were used for all electrochemical testing at 25 °C in a Thermo Scientific Heratherm Refrigerated Incubator. Li-metal chips (0.6 mm thick, MTI) were punched to size and polished with a nylon brush to remove any oxide layer prior to coin cell assembly in an argon-filled glovebox. For EIS and Li-Li symmetric cycling, cells with 304SS spacer (15.5 mm dia.) / Li-metal (14.3 mm dia.) / polymer electrolyte (14.3 mm dia.) / Li-metal (11.1 mm dia.) / 304SS spacer (15.5 mm dia.) were used (as shown in FIG. 10). EIS was performed with a Gamry Instruments Reference 600+ potentiostat / galvanostat / ZRA at 25 °C from 5 MHz to 0.1 Hz with a 10 mV AC amplitude applied around the open-circuit voltage (OCV). Gamry Echem Analyst was used for fitting EIS spectra with equivalent circuits using the Simplex method and excluding data points after the end of the semicircle on the low frequency side (right side of the Nyquist plots). Li symmetric cell cycling was performed with an Arbin LBT21084 at 25 °C and a current density of ±0.1 mA / cm2(based on the area set by the 11.1 mm dia. Li-metal) for 30 min each direction with 30 min rests.
[0486] The ESW was determined by linear sweep voltammetry (LSV) and cyclic voltammetry (CV) at 25 °C with an Arbin LBT20084. Separate cells were used for anodic LSV and cathodicCV scans. For anodic LSV scans (OCV to 7V vs. Li / Li+at 0.1 mV / s scan rate), cells with the polymer electrolyte film (14.3 mm dia.) sandwiched between 304SS (15.5 mm dia.) as the working electrode (WE) and Li-metal (11.1 mm dia.) as the counter / reference electrode (CE / RE) were used (shown in FIG. 11 A). For cathodic CV scans (OCV to -0.2V vs. Li / Li+at 0.1 mV / s scan rate), cells with the polymer electrolyte film (14.3 mm dia.) sandwiched between Cu foil (14.3 mm dia.) as the WE and Li-metal (11.1 mm dia.) as the CE / RE were used (shown in FIG.
[0487] 11B).
[0488] 3.2.1 Physical Characterizations. After synthesis, the polymer electrolytes were freestanding films (shown for 0 wt% PPy(DBS) composition in FIGs. 12A-12C) that could be peeled off the PET sheet and were non-tacky. The cross-linked fraction of the polymer electrolytes was determined through insoluble fraction measurements, as the cross-linked components of the film re after soaking in acetonitrile [B66, B67], The results in FIG. 4A show the insoluble fractions of compositions with various amounts of PPy(DBS). The target insoluble fraction of greater or equal to 50 wt% was selected based on the similar polymer electrolyte composition from Zhang and coworkers [B67] and above this threshold the films were free-standing and flexible. For a given UV curing time, as the amount of PPy(DBS) in the composition increased the insoluble fraction typically decreased and the variability in insoluble fraction between samples from the same film increased. With longer UV curing times for each composition, the insoluble fraction increased and the variability decreased. The PPy(DBS) particles are opaque, black particles that reduced UV transmittance through the thickness of the film (inhibiting UV curing), resulting in lower insoluble fractions and higher variability. The optical appearance of the films with increasing amounts of PPy(DBS) are shown in the inset in FIG. 4 A. The 0 wt% PPy(DBS) film was optically clear, becoming darker with more PPy(DBS) until appearing al completely opaque at 2.0 wt% PPy(DBS). The 2.0 wt% PPy(DBS) film eventually reached the target insoluble fraction after 20 min UV curing time but resulted in a brittle film (likely due to overcuring in areas of the film the UV transmittance was less obstructed by PPy(DBS) particles). The 2.0 wt% PPy(DBS) films did not reach full solidification below this curing time and the insoluble fraction could not be measured.
[0489] Electrical conductivities obtained from 5 samples of each composition are shown in FIG.
[0490] 13. The electrical conductivities (uezeC) were calculated using the resistance values measured with the multimeter (R), thickness of the film ( / ) and contact area (A) in the following equation:
[0491] ^elec =A(1 3) Materials with an electrical conductivity below 10'8S / cm are typically considered electrical insulators, with the transition to electrical semiconductors for conductivities above 10'8S / cm [B75, B76], Films with 0 wt% through 2.0 wt% PPy(DBS) showed a minor increase in electrical conductivity from 4.6-6.3 x 10'9S / cm, confirming the compositions are below the percolation threshold (where a sharp increase in electrical conductivity of multiple orders of magnitude would be observed). Thus, the upper limit on the amount of PPy(DBS) that can be added to these compositions is due to the UV curing process, not the percolation threshold. For subsequent experiments, 0 wt% through 1.0 wt% PPy(DBS) films from 10 min UV curing time were used. These films were selected to avoid potential effects from overcuring at longer UV cure times. The average insoluble fractions were above the target fraction for these films, even though the films with increasing amounts of PPy(DBS) had lower insoluble fractions.
[0492] XRD scans of the different polymer electrolyte films containing 0 wt% through 1.0 wt% PPy(DBS) particles (with background signal from the glass slide removed) are shown in FIG.
[0493] 4B. There are no sharp crystalline peaks present in the XRD pattern - a broad amorphous peak centered around 29 of 19.5° is present, indicating highly amorphous films. The amorphous peak appears to broaden with increasing amounts of PPy(DBS), suggesting the addition of PPy(DBS) may lead to increasingly disordered films.
[0494] DSC profiles from the second heating scan of the different polymer electrolyte compositions are shown in FIG. 4C with results summarized in Table 3. During DSC heating scans, thermal transitions such as the glass transition, melting, and crystallization can be observed. The glass transition occurs within the amorphous phase of PEO as the material changes from a rigid glassy state to a more mobile rubbery state due to heating. It presents itself as an endothermic step change in heat flow within the DSC heat scan. The polymer samples in this study showed Tgvalues between -37 °C and -41 °C, in order of increasing PPy(DBS). With Tgvalues well below room temperature, the polymer can exhibit a highly mobile rubbery structure around room temperature. The polymer samples do not display any distinct melting peaks in the DSC data up to 120 °C. This suggests the films are highly amorphous, as confirmed by XRD data, compared to the semi-crystalline behavior typically observed in similar PEO based polymer electrolytes [B66, B67], Li-ion transport in PEO based polymer electrolytes is typically considered to occur through segmental motion of polymer chains in amorphous regions and the subsequent Li-ion hopping along and between the polymer chains [B77] . Thus, a highly amorphous structure enhances segmental motion mechanisms for increasing ionic conductivity in PEO based electrolytes because there are no crystalline lattice structures to inhibit the movement of the polymer chains and lithium ions. As expected from literature on other filler particles incorporated in PEO lowering Tg(such as SiO2, SnO2, and TiO2) [B78-B80], incorporating increasing amounts of PPy(DBS) shifts the Tgto slightly lower temperatures. Thiscould be caused by PPy(DBS) particles physically disrupting and interfering with the packing of PEO chains allowing the glass transition to occur at lower temperatures. This trend has been observed with other filler particles incorporated in PEO such as SiO2, SnO2, and TiO2. The slope of the heat flow after the glass transition in FIG. 4C increased with the addition of PPy(DBS) from 20.1 mW7(g °C) to 85.9-115.0 mW / (g °C), summarized in Table 3. This increase in slope of the heat flow suggests an increase in specific heat capacity (requiring additional heat flow to maintain the same heating rate). This difference is not expected from the heat capacity of PPy(DBS), which is typically lower than the heat capacity of PEO. Instead, the increasingly mobile rubbery structures (as indicated by decreasing Tg) may cause the increase in specific heat capacity [B81-B84],
[0495] DMA tan delta thermograms are shown in FIG. 4D, with storage and loss modulus profiles shown in FIGs. 14A-14D. Results are shown to 20 °C as the films became too soft above this temperature and broke or the measurement signal became unstable. The peak of the tan delta curve (when the material demonstrates the viscous response to deformations) was used to determine Tgof the films from DMA in this analysis with the results summarized in Table 3. There are multiple methods to determine Tgfrom DMA, with the tan delta peak typically giving the highest value of Tg[B85] . This is a conservative determination with respect to enhanced segmental motion of polymer chains for increased ionic conductivity in PEO based electrolytes. DMA results show Tgvalues between -43 °C and -57 °C in good agreement with the trend of Tggenerally decreasing with increasing amounts of PPy(DBS), as observed with DSC. The obtained values of Tgdiffered between DSC and DMA, which is not uncommon as glass transition is a region of behavior with values often differing by 10-25 °C between the techniques [B85] . The difference in Tgbetween techniques can be attributed to the different property changes related to the glass transition region observed with DSC and DMA (measurement parameters can also affect the values obtained). Changes in heat flow due to the change in heat capacity of the polymer during its transition from a rigid glassy state to a mobile rubbery state are observed with DSC, whereas the change in mechanical properties are observed with DMA. These Tgvalues from DSC and DMA are within the range of similar PEO based polymer electrolytes with reported Tgvalues between -34 °C and -78 °C [B66, B67], The storage and loss moduli did not show a consistent trend with increasing amounts of PPy(DBS). If the addition of PPy(DBS) particles affected the storage and loss moduli, increasing or decreasing values with increasing amounts of PPy(DBS) would be expected but no such trend is observed. The variability between the storage and loss moduli for the different compositions could obscure any effect from PPy(DBS).3.2.2 Mechanical Response Characterizations. FIGs. 5A-5D shows the AFM continuous point measurements for the films under an electric field strength of 0.3 V / pm for 10 min followed by 0 V / pm for 10 min for 5 representative excitations and relaxations. The 0 wt% PPy(DBS) film (FIG. 5 A) does not show any appreciable response beyond the measurement uncertainty and noise. The 0.25-1 wt% PPy(DBS) films (FIGs. 5B-5D) show a clear expansion response up to 0.6 pm (corresponding to 6% strain for the approximately 10 pm thick films) under an electric field strength of 0.3 V / pm followed by a relaxation when the electric field is removed (0 V / pm). This response is attributed to the polarization of the PPy(DBS) particles in the polymer film. The PPy(DBS) particles are polarized under an electric field and try to align, causing the film to expand. The expansion response increases from an average expansion of 0.44 pm for 0.25 wt% PPy(DBS) to 0.56 pm for 1 wt% PPy(DBS) and appears to be repeatable over several cycles. The expansion response decreases with decreasing electric field strength as shown in FIGs. 15A-15C, where the film does not produce an appreciable response below 0.2 V / pm regardless of the concentration of PPy(DBS).
[0496] The films not returning to zero displacement at the end of the relaxations suggests there is a residual expansion left in the films. This could be due to an irreversibility such as plastic deformation or an irreversible rearrangement of PPy(DBS) particles and polymer matrix chains during the initial excitation. This behavior is also seen to some extent in the storage modulus response for PPy -based and other ER elastomers [B41, B42, B45], The strain of the films at the end of excitations and relaxations (sexcitation and 8relaxation, corresponding to expansion and residual expansion, respectively) were calculated from the displacement compared to the beginning of the excitation (taken as zero) divided by the film thickness (approximately 10 pm). The results are shown in FIG. 5E with 0 wt% PPy(DBS) included for comparison, even though it did not display a clear expansion and relaxation response. For the 0.25-1 wt% PPy(DBS) films, Sexcitation increased from -4-6% with increasing PPy(DBS) whereas 8relaxation did not display a clear trend. Further characterization can be used to fully elucidate the relaxation behavior.
[0497] The temporal characteristics of the response were investigated with the time constant for expansion and relaxation (Texcitation and relaxation, respectively). Texcitation was determined from the time taken for the excitation to reach 1-1 / e (63.2%) of the final value, relaxation was determined from the time taken for the relaxation to decay to 1 / e (36.8%) of the final excitation value compared to the final relaxation value. The results are shown in FIG. 5F, with the response times a similar magnitude to those of storage modulus for a PPy -based ER elastomer [B41 ] . There was no trend for the time constants with different amounts of PPy(DBS). However, relaxation was lower than Texcitation by about 1 min for each case. This suggests the polymer starts to return to itsrelaxed state faster than the excitation. This is seen in the storage modulus response for a PPy-based ER elastomer as well [B41], The storage modulus quantifies the elastic response of the polymer when it is subjected to a deformation. The energy is stored elastically when undergoing deformation and can be released once the stress is removed. This energy is required to rearrange the polymer chain entanglements and cross links in response to the stress (in this case, in response to the PPy(DBS) particles polarizing and trying to align in the polymer matrix under an electric field). However, this elastic energy can allow the polymer chains in the matrix to return to the relaxed state fast, which could result in Trelaxation being lower than Texcitation. Also, the films do not return to zero displacement during relaxation, which may contribute to the lower time constant.
[0498] Note that, while the AFM measurements were generally reliable, they were subject to uncertainties such as thermal drift over the long timescale of the polymer response. Some sharp increases or decreases were noted during the transitions between excited and relaxed states. These variations are likely attributable to measurement artifacts, as the direction of these changes was inconsistent across similar transitions. Despite these uncertainties, the results indicate the 0.25-1 wt% PPy(DBS) films produce an expansion strain response during excitation (4.2-5.9%) and residual strain following relaxation (1.1-2.5%) compared to the 0 wt% PPy(DBS) control (with strains of 0.2% ± 0.3% and 0.1% ± 0.4%, respectively).
[0499] The surface morphology of gold coated 1 wt% PPy(DBS) film is shown in FIGs. 6A-6H. SEM micrographs (FIGs. 6A, 6E) of the pristine film showed relatively flat surfaces apart from a few raised areas. AFM topography maps were used to investigate the uniformity of the polymer film expansion in local regions. The AFM topography maps of the film at rest (FIGs. 6B, 6F), after the first excitation at 0.3 V / pm (FIGs. 6C, 6G), and after the first relaxation (FIGs. 6D, 6H) did not show any changes in the surface locally, suggesting the expansion response was relatively uniform across the surface of the film.
[0500] The block force response measurements are shown in FIG. 7B. For films with PPy(DBS), the force response increased with increasing wt% of PPy(DBS) (from 0.25 wt% to 1 wt%) and increasing electric field strength (from 0.1 V / pm to 0.3 V / pm). This force response trend is associated to the polarization of PPy(DBS) under an electric field as the particles may try to align, since this response of CP particles such as PPy(DBS) has typically been shown to increase with increased CP loading and electric field strength [B36-B42, B45, B46], Since the film is mechanically compressed under the clamp, changes in stiffness of the film under electric field may partially contribute to the measured response, implying that the force required to maintain the same level of compression would increase [B41, B42, B45, B46],It is worth noting that the 0 wt% PPy(DBS) films showed a non-zero response in FIG. 7B that, however, did not indicate any appreciable relationship with the applied electric field strength. Polarization of ions within the film under an electric field could contribute to the response. The film responses in FIG. 7B are reported for the first actuation to mitigate possible effects on the response from decomposition of the films (as the applied voltages are above the ESW of around 4.5 V in FIGs. 18A-18B). However, these results still suggest a desirable force response due to the polarization of the PPy(DBS) particles as the responses of films with PPy(DBS) are larger than the responses in the 0 wt% PPy(DBS) films, increasing with increasing electric field strength and amount of PPy(DBS) (and the ESW is similar between all compositions).
[0501] 3.2.3 Electrochemical Characterizations. The electrochemical characterizations of the polymer electrolyte compositions were all performed at 25 °C to investigate the performance around room temperature. Symmetric Li / polymer / Li coin cells were used to compare the polymer electrolyte performance of the compositions with PPy(DBS) to the 0 wt% PPy(DBS) composition. For symmetric cycling (30 min cycles at ±0.1 mA / cm2) and EIS, at least 10 coin cells were tested for each composition. Results based on the 5 middle performing coin cells are reported in this work.
[0502] A summary of the measured ionic conductivities for the 5 middle performing coin cells at 25 °C are shown in FIG. 8A. The ionic conductivities (pion) were calculated using Rsfrom the equivalent circuit as the bulk polymer electrolyte impedance (Rb), thickness of the electrolyte ( / ) and contact area (A) in the following equation:
[0503] A
[0504]
[0505] ION =RM The results indicate no trend for ionic conductivity between the compositions when considering the variability, with ionic conductivities between 0.11-0.16 mS / cm.
[0506] As with the ionic conductivity, no trend in interfacial impedances was observed among the compositions with increasing amounts of PPy(DBS) when considering the variability of the 5 cells of each composition. The cells are compared after 50 cycles when there was less variability between the 5 cells with the interfacial impedances shown in FIG. 8B and Nyquist plots from EIS for representative cells are shown in FIG. 8C. One notable difference was the variability between the 0 wt% PPy(DBS) composition cells was higher than each of the compositions with PPy(DBS). The use of wave springs in the coin cells could contribute to increased variability in interfacial impedance, due to uneven pressure applied by wave springs [B86-B88], Overall, the total interfacial impedances of the cells were on the order of 4 kQ cm2. This value is higher than comparable PEO based polymer electrolytes [B66, B67] of -500-700 Q cm2which could be dueto some experimental processing limitations in this work such as: hot-pressing and UV-curing the films in ambient air (possibility of moisture contamination that vacuum drying may not fully remove), hot-pressing under lower pressure, greater amount of photoinitiator used (evidenced by reaching target insoluble fraction in a shorter curing time compared to literature [B67] where photoinitiator amount was not specified), and differences in coin cell configuration (total spacer thickness and type of spring can affect stack pressure and thus interfacial impedance, which were not specified [B66, B67]). In particular, excess photoinitiator could cause increased interfacial impedance due to increased storage modulus [B68] or premature termination and incomplete cure of the polymer matrix [B69] . During polymerization, excess photoinitiator could cause more polymer chains to become crosslinked leading to a higher crosslink density. An increased storage modulus could result from the higher crosslink density due to less mobility within the polymer chains and the polymer would not be able to conform as easily to the Li-metal surface, increasing the interfacial impedance. An incomplete cure could lead to less crosslinks in the matrix than expected or inhomogeneous crosslinking. Regions of lower crosslinking could have higher mobility and leaching of non-crosslinked moi eties and regions of higher crosslinking could have more defects resulting in cracks or voids in the interface.
[0507] Out of the 5 middle performing coin cells for each composition, for representative cells the Li symmetric cycling overpotentials are shown in FIG. 16 and the Nyquist plots obtained from EIS are shown in FIGs. 17A-17D for 0-50 cycles of the representative cells. Equivalent circuit model parameter fitting was performed with a series resistor (Rs) to model the bulk impedance of the polymer electrolyte and two sets of parallel resistors (RSEI, Ret) with constant phase elements (CPEi, CPE2) to model the solid electrolyte interphase (SEI) and charge transfer of the Li / polymer interfaces, respectively. The total interfacial impedance is taken as the combination of RSEI and Ret of both Li / polymer interfaces, assuming the interfaces are nearly identical. CPEs are used to account for non-ideal capacitive behavior. The equivalent circuit model parameters for the representative cells are summarized in Table 4. The bulk impedance (which can be approximated as the left-side intersection of semicircle with the real impedance Z’ axis) remained relatively stable over 50 cycles. The interfacial impedance (can be approximated as the right-side intersection of semicircle with the real impedance Z’ axis) varied between the cells over 50 cycles with interfacial impedance decreasing (suggesting the interface is still stabilizing), increasing, a combination of the two, or remaining stable.
[0508] Although some polymer electrolytes have achieved sufficient ionic conductivities at 25 °C, high interfacial impedances > 100 Q cm2limit the commercial viability of polymer electrolytes in LIMSSBs for applications such as electric vehicles and consumer electronics(apart from semi-solid gel polymer electrolytes that can pose safety concerns). Further advancements are needed to lower interfacial impedance at 25 °C such as developments with in-situ polymerization or single ion conducting polymer electrolytes [B89-B92], The incorporation of PPy(DBS) particles and resulting properties presented in this work are expected to be applicable for other polymer electrolyte compositions.
[0509] The ESW at 25 °C with Li-metal of each polymer electrolyte composition was determined with anodic LSV and cathodic CVs shown in FIG. 8D. For the cathodic sweep, a small peak is initially seen around 1.5 V vs. Li / Li+that may be attributed to the decomposition of some polymer electrolyte components to form a passivation layer with Li-metal [B93], as many polymer electrolytes are not stable with Li-metal but form a stable passivation layer or interphase [B21, B28, B66, B67], This peak is present in all compositions, suggesting components in the 0 wt% PPy(DBS) composition are responsible, not PPy(DBS). Reversible Li plating and stripping on the Cu surface is seen from -0.2V to 0.3 V vs. Li / Li+, as Li can plate on the Cu WE when its potential goes below 0V vs. Li / Li+then strip after the potential increases above 0V vs. Li / Li+again. From the anodic sweep, the oxidative stability is conservatively determined as when the current density surpasses 1 pA / cm2giving a stability up to 4.5V vs. Li / Li+for all compositions.
[0510] 3.3 Summary. An experimental characterization activity demonstrating the adaptive behavior at room temperature (20-25 °C) of a polymer electrolyte that incorporates conducting polymer particles was summarized. The objective of this investigation was to evaluate the potential of this material for application as an interlayer to enhance the performance and durability of lithium metal solid-state batteries (LIMSSBs). The adaptive polymer electrolyte comprised of a PEO based polymer containing PPy(DBS) conducting polymer particles that impart adaptive properties to the polymer electrolyte, enabling force and expansion responses under electric fields through polarization of the PPy(DBS) particles.
[0511] Experimental results confirmed the adaptive polymer electrolyte’s adaptive behavior. AFM measurements revealed an expansion response of films of up to 6% strain under a field of 0.3 V / pm, repeatable over several cycles, with reduced expansion observed at lower electric field strengths. Block force response measurements showed a corresponding increase in force with higher electric field (starting from 0.1 V / pm) and greater PPy(DBS) loading. These findings are consistent with the hypothesis that the adaptive response is driven by the polarization of PPy(DBS) particles, a behavior observed in electrorheological fluids and elastomers [B36-B42, B45, B46], However, the alignment of PPy(DBS) particles in solid films was not directly observed and res an area for further exploration.The incorporation of PPy(DBS) particles affected the polymer matrix by inhibiting UV curing, lowering the insoluble fraction of the film and restricting the PPy(DBS) particle amount to ~1 wt% of polymer and monomer content (equivalent to -0.45 wt% or -8 vol% of final film). Despite these constraints during the synthesis process, the films remained electrical insulators with no increase in electrical conductivity, indicating that the percolation threshold was not reached. Furthermore, no substantial trends were observed in the electrochemical performance of the polymer electrolytes at 25 °C with increasing amounts of PPy(DBS). The amorphous structure of the films showed minor changes with the amounts of PPy(DBS) incorporated.
[0512] Further research could focus on characterizing the reversibility of the adaptive response, residual expansion upon relaxation, and direct observation of PPy(DBS) particle alignment in solid films. Exploring synthesis methods that allow for the addition of more PPy(DBS) could also be of interest to determine if there is an optimal amount before the films become electrically conductive. In the following sections, evaluating the performance of the adaptive polymer electrolyte as an interlayer in LIMSSBs (ideally less than 10 pm thick) can be useful to understanding its potential to mitigate interfacial changes upon lithiation / delithiation, and its effects on battery durability.
[0513] Section 4: Adaptive Polymer Interlayer. The steps to transition the adaptive polymer electrolyte (A-PE) from above to an adaptive polymer interlayer are presented. The polymer interlayer was incorporated between the Li-metal anode and ceramic solid electrolyte. To enable a thin polymer interlayer, synthesizing the interlayer directly on the Li-metal anode or ceramic solid electrolyte was investigated. Finally, the interlayer was incorporated in prototype LIMSSB coin cells that underwent electrochemical testing to investigate if the adaptive property occurred under the present electric field strength in the cell, and whether degradation of the Li-metal anode / polymer interlayer interface could be reduced with the adaptive polymer interlayer compared to a baseline polymer interlayer.
[0514] 4.1 Ceramic Solid Electrolyte Synthesis. A well understood ceramic solid electrolyte composition is desired for testing the proposed polymer interlayers in this research. The solid electrolyte should have adequate room temperature ionic conductivity (at least 0.1 mS / cm) and commercial availability or relatively straightforward synthesis of the solid electrolyte powder or resultant pelletized separators. A widely studied type of ceramic solid electrolyte meeting these requirements is the oxide composed of Li, La, Zr, O, doped with Ta to improve stability of the high ionic conductivity cubic phase [B94-B96] such as the commercially available Li6.4La3Zn.4Tao.6O12 (LLZTO) pellets or powder from MSE Supplies.
[0515] For synthesis of pellets from commercial powder, two methods were explored - usingpowder with pm-sized particles or nm-sized particles. The synthesis of pellets from powder with pm-sized particles was adapted from [Bl 3, B97] but using commercially purchased LLZTO powder (MSE Supplies, Li6.4La3Zn.4Tao.6O12, average particle size 5 pm). The synthesis of pellets from powder with nm-sized particles was adapted from literature [B96] but using commercially purchased LLZTO powder (MSE Supplies, Li6.4La3Zn.4Tao.6O12, average particle size 500 nm). The syntheses are described below. Commercially purchased LLZTO pellets (MSE Supplies, 700 pm thick, 97% relative density, 0.4-1.0 mS / cm bulk ionic conductivity) were also investigated.
[0516] Cross-sectional scanning electron microscopy (SEM) was used to examine the densification of the oven sintered pellets from commercially purchased powder and the commercially purchased pellets shown in FIGs. 38A-38F. All three types of pellets exhibit a dense grain structure locally in the cross-sections (shown in FIGs. 38 A, 38C, 38E), but the oven sintered pellets have a few sizeable pores throughout the cross-section (shown in FIGs. 38D, 38F) leading to a lower overall relative density of approximately 75% measured using the geometric method (volume from thickness and diameter measurements combined with weight to calculate actual pellet density, compared to LLZTO theoretical density of 5.5 g / cm3), whereas the commercially purchased pellets (shown in FIG. 38B) are more uniformly dense. The pores in the oven-sintered pellets could be due to the excess Li (in the form of Li OH) in the pellets that decomposes first during sintering, leaving pores filled with gas in its place [B98] . The commercially purchased pellets were likely synthesized with simultaneous pressing and sintering with a high temperature pellet press, not requiring excess Li and resulting in more uniformly dense pellets.
[0517] While the commercially purchased pellets are of good quality and readily useable, the cost is prohibitively expensive for a sufficient number of samples for the experiments in the following sections (approximately $350 per 14mm diameter pellet at the time of this writing). The oven sintered pellets from commercially purchased pm-powder or nm-powder, while some pores throughout the pellet are not ideal, are of adequate quality. The dense grain structure locally can provide sufficient ionic conductivity, and the pores are dispersed and not interconnected. As described below, oven sintered pellets from pm-powder required a higher temperature and longer sintering time (1250 °C for 12 hr) to be densified, compared to pellets from nm-powder (1210 °C for 3 hr). This is expected as smaller particles tend to sinter faster than larger particles, due to the shorter distance required for solid-state diffusion of the compounds during sintering [B99, B100], Also, sintering pellets from pm-powder was inconsistent as pellets in some batches were not properly densified during the sintering process.Thus, oven sintered pellets from commercially purchased nm-powder were used for the experiments described herein.
[0518] The ionic conductivity of the oven sintered LLZTO pellets from commercially purchased nm-powder was measured by sputter coating 50 nm thick gold on both sides of the LLZTO pellet as blocking electrodes, using 20 mA sputter current with an EMS150R ES sputter coater (Electron Microscopy Sciences / Quorum). Electrochemical impedance spectroscopy (EIS) was then performed on three samples of 50 nm gold / LLZTO / 50 nm gold with a Gamry Instruments Reference 600+ potentiostat / galvanostat / ZRA at 25 °C from 5 MHz to 100 Hz with a 10 mV AC amplitude applied around the open-circuit voltage (OCV) with the resulting Nyquist plot shown below in FIG. 39. The ionic conductivity (pion) of the LLZTO pellet was calculated using the electrolyte impedance from the EIS Nyquist plot intersecting with the real axis (Reiec), thickness of the electrolyte ( / ), and contact area (A) in equation:
[0519]
[0520] resulting in an average ionic conductivity of 0.49 ± 0.04 mS / cm from 3 samples of oven sintered LLZTO pellets pressed from commercial nm-powder and covered with commercial pm-powder during sintering. The thickness of each of the 3 pellets was between 1.1 -1.5 mm for the EIS measurements.
[0521] 4.2 Thin Polymer Interlayer Synthesis. The electric field strength across the polymer interlayer in V / pm can be closely related to the thickness of the polymer interlayer. Thus, a thin polymer interlayer less than 10 pm thick is targeted. To achieve this thickness or below, the polymer must be synthesized directly on the Li-metal anode or ceramic solid electrolyte as a free-standing polymer can require a greater thickness. The polymer interlayer synthesized on Li-metal or ceramic solid electrolyte is investigated in the following sections.
[0522] 4.2.1 Polymer Interlayer on Li-metal. For the polymer interlayer synthesized directly on the Li-metal anode, the process from above was first adapted as closely as possible but with the polymer solution on top of a Li-metal chip instead of a polyethylene terephthalate (PET) bottom film and pressed in a 12.7 mm diameter heated die inside an Ar-filled glovebox, instead of a large format hot press in air. However, the pliability of the Li-metal chip prevented the top PET cover film from being removed without bending or damaging the Li-metal chip after UV curing the polymer. The synthesis process was modified as shown in FIG. 40 using a polytetrafluoroethylene (PTFE) spacer to keep the thickness similar to the free-standing polymer electrolyte for impedance measurements (to determine if there are side reactions with the polymer synthesized directly on Li-metal) and PTFE top cover film in place of PET for lower adhesion to the polymer after UV curing. The top PTFE was removed after hot pressing andbefore UV curing. The cured polymer on Li-metal appeared optically clear with no discoloration that would initially indicate side reactions.
[0523] The Li / polymer interlayer was incorporated into a symmetric Li coin cell as shown in FIG. 40 to measure the impedance using EIS. The total interfacial impedance should be less than or equal to the interfacial impedance of Li / free-standing polymer electrolyte / Li unless there are side reactions or instabilities from the polymer being UV cured directly on the Li-metal surface [B101-B104], The interfacial impedance of the Li / free-standing polymer electrolyte / Li cells discussed above were typically around 4 kQ cm2with some outlier cells up to 10 kQ cm2. Thus, the interfacial impedance with the polymer interlayer synthesized directly on Li-metal should be no more than 10 k cm2marked with the dashed line in FIG. 41. While some of the cells shown in FIG. 41 were initially below 10 kQ cm2, the interfacial impedances continually increased over a few days of rest and surpassed 10 kQ cm2. This indicates instability or continual side reactions between the polymer and Li-metal when synthesized directly on Li-metal, which has been reported especially in the case of acrylate and methacrylate monomers and oligomers [Bl 03, Bl 04], Since the synthesis of this polymer electrolyte composition directly on Li-metal does not appear to be stable, synthesizing the polymer interlayer directly on the oxide LLZTO ceramic solid electrolyte, which should be much less reactive than Li-metal, is tested in the following section.
[0524] 4.2.2 Polymer Interlayer on Ceramic Solid Electrolyte. For the polymer interlayer directly on the LLZTO ceramic solid electrolyte, the synthesis process described above was first adapted as closely as possible but with the polymer solution on top of an LLZTO pellet instead of a polyethylene terephthalate (PET) bottom film and pressed in a 12.7 mm diameter heated die inside an Ar-filled glovebox instead of a large format hot press in air. The adapted synthesis process is shown in FIG. 42. To minimize the thickness of the polymer interlayer, no spacer was used between the top PET film and the LLZTO pellet. The amount of polymer solution added to the LLZTO pellet surface affects the final thickness of the polymer interlayer and was measured as areal mass loading in mg / cm2. Using the same areal mass loading helps reduce variability between multiple samples when targeting the same thickness.
[0525] The rigid LLZTO pellet allows for the top PET film to be peeled off compared to the pliable Li-metal that resulted in damage, as discussed herein. However, the polymer interlayer adhered more to the PET film than the LLZTO surface and was delaminated when the PET film was peeled off, shown in FIG. 43 for an areal mass loading of 5 mg / cm2. The polymer interlayer remained on the LLZTO surface in a few areas outlined in blue with an SEM cross-section from one of the areas. In this region, the thickness of the polymer interlayer of approximately 9 pmmeets the target thickness of less than 10 gm, so a greater areal mass loading of the polymer would not be desirable (even if this reduced the area of the polymer removed with the PET film).
[0526] For these reasons, the synthesis process was modified to prevent the polymer interlayer from being delaminated. The process is shown in FIG. 44 with the modifications outlined in red. To address the delamination of the polymer interlayer when the top cover film is peeled off after UV curing, the PET top film was replaced with a polymer that is stiff enough to provide a smooth top surface of the polymer interlayer when hot-pressed and subject to high UV transmission for curing, but with a lower adhesion surface. Fluorinated ethylene propylene (FEP, McMaster-Carr) was chosen with a similar thickness of 127 pm as the PET film. Additional modifications to improve the uniformity of the coating were pre-heating the LLZTO pellet at 80 °C with the polymer mixture on it (to reduce the viscosity of the polymer solution and allow for easier spreading) and using a PTFE scraper to spread the polymer solution prior to hot-pressing.
[0527] The modified synthesis process allowed for an areal mass loading down to approximately 3 mg / cm2spread on the LLZTO pellet surface. The FEP top sheet stayed on after hot-pressing to help provide a flat top surface for the polymer interlayer coating during UV curing. As shown in FIG. 45, the FEP sheet was easily removed after UV curing and the polymer interlayer did not delaminate at all from the LLZTO surface.
[0528] SEM cross-sections of the polymer interlayer on the LLZTO ceramic electrolyte pellet are shown in FIG. 46. With the improvements to the synthesis process, the polymer interlayer still ranged from 1 pm to 10 pm thick across the pellet with an average thickness of 5 ± 3 pm (obtained from 14 SEM images along the cross-section).
[0529] The LLZTO / polymer interlayer was incorporated into the symmetric Li coin cell shown in FIG. 47 to measure the impedance using EIS. The impedance was measured to determine if the polymerization directly on LLZTO was stable. If the impedance continually increases over time, that would suggest instability as observed for polymerization on Li-metal in Section 4.2.2. Layers of Ni foam (MSE Supplies, 97% porosity, initial thickness 0.3 mm) were used in place of standard coin cell springs to provide more uniform stack pressure to mitigate cracking the LLZTO ceramic solid electrolyte pellet during assembly.
[0530] The interfacial impedance of the LLZTO / polymer interlayer in symmetric Li coin cells is shown in FIG. 48 over several days of resting at 25 °C. The interfacial impedance shows an increase in the first day, which is to be expected from interphase formation between the freestanding polymer electrolyte / Li and the polymer interlay er / Li. Stack pressure relaxation following assembly of the coin cell is also possible, as the components may undergo some plastic deformation resulting in a slight decrease of the stack pressure. After the first day of rest,the interfacial impedance remains stable over several days.
[0531] These results indicate the polymer electrolyte composition is stable when synthesized as a polymer interlayer directly on the LLZTO ceramic solid electrolyte pellet and achieves the target thickness of 10 pm or less. This polymer interlayer synthesis method was adopted to build the prototype coin cells that were used to compare the performance of a standard polymer interlayer and an adaptive polymer interlayer.
[0532] 4.3 Pseudo-Solid Full Cells with Adaptive Polymer Interlayer. The ceramic solid electrolyte and polymer interlayer were integrated into prototype coin cells to perform a comparative study of the adaptive polymer interlayer (1 wt% PPy(DBS)) against the baseline polymer interlayer (0 wt% PPy(DBS)). The working hypothesis motivating these experiments is that the adaptive polymer interlayer may stabilize the interface of the Li-metal anode during cycling by expanding to maintain contact. The tests performed included comparisons to a baseline polymer interlayer, analyzing capacity retention and impedance growth over several consecutive cycles.
[0533] 4.3.1 Setup of Pseudo-Solid Full Cells. The LIMSSB coin cells were designed with the stack illustrated in FIG. 49, which features multiple interfaces (Li anode / polymer interlayer / ceramic LLZTO / cathode). To minimize the impedance and degradation of the cathode side of the cell, a small amount of liquid electrolyte was added to wet the interface. To prevent liquid electrolyte from traveling to the polymer interlayer side of the cell, a viscous high concentrated electrolyte was used. Adapted from [Bl 05], the viscous electrolyte comprises of 3M LiPFe Li salt in fluoroethylene carbonate (FEC): dimethyl carbonate (DMC) co-solvents with l,l,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) as diluent. A conventional Celgard separator was also used to help contain the electrolyte on the cathode side of the cell and to ensure separation of the LLZTO ceramic solid electrolyte from the cathode (as LLZTO can be unstable with higher voltages [B12]). LiNio.6Mno.2Coo.2O2 (NMC622) was used as the cathode, with the synthesis process further detailed below.
[0534] The setup for the pseudo-solid LIMSSB coin cells is shown in FIG. 50. Two layers of Ni foam were found to be sufficient in place of a spring for providing more uniform stack pressure and to mitigate cracking of the LLZTO ceramic solid electrolyte pellet during assembly. A few prior cells were made with three layers of Ni foam but upon disassembly some of the LLZTO pellets were found cracked. This was attributed to the additional stack pressure resulting from adding more Ni foam. Polyimide tape and PTFE were used to help align the stack during assembly. The polyimide tape helps align the NMC622 cathode with the stainless steel spacer, with the PTFE helping to align the LLZTO / polymer interlayer, Li chip, and top Cu foil. Siliconeadhesive (McMaster-Carr, high-temperature glue-on-a-roll silicone adhesive, 25 pm thick) was used to adhere the PTFE to the polyimide tape. 10 pL of high concentrated electrolyte between NMC622 and LLZTO was initially used but was insufficient to soak the NMC622, Celgard separator, and bottom side of the LLZTO in addition to free volume in the coin cell as the interface dried up over time (shown in FIGs. 61 A-61B), so the amount was increased to 30 pL. Cu foil was added between the Li-metal chip and coin cell case to try to prevent the Li chip sticking to the coin cell case during disassembly (shown in FIGs. 62A-62B), which is undesirable as the Li / polymer interface needs to be maintained for imaging. The initial batch of cells demonstrated that the setup was successful in keeping the battery stack aligned during assembly and the LLZTO pellets remaining intact during assembly and disassembly. For the updated assembly process with 30 pL of high concentrated electrolyte, the cathode remained fully wetted as shown in FIG. 63 A. Even with Cu foil between the Li-metal anode and coin cell case, it still came off with the coin cell case during disassembly, as shown in FIG. 63B.
[0535] However, the Li-metal anode and Cu foil barely adhered to the coin cell case and were easily removed, as shown in FIGs. 64A-64C, suggesting weak adherence between the Li-metal and the polymer interlayer.
[0536] The assembly process of the pseudo-solid LIMSSB coin cell is shown in FIG. 51. The gasket was inserted in the bottom (larger) coin cell case followed by the Ni foams (initial thickness of 0.3 mm each). The stainless steel spacer (1 mm thick) with the polyimide tape (40 pm thick) and PTFE (1.02 mm thick) was placed next, followed by the cathode (total 65 pm thick, 50 pm cathode layer on 15 pm foil). 30 pL of high concentrated electrolyte was added between the cathode and LLZTO ceramic solid electrolyte, with half of the high concentrated electrolyte added on the cathode, Celgard separator placed on top, then the other half of the high concentrated electrolyte. The LLZTO (approximately 700 pm thick) with polymer interlayer (approximately 5 pm thick) facing up was placed next, followed by the Li chip (approximately 600 pm thick), Cu foil (10 pm thick), then the top (smaller) coin cell case and the coin cell was crimped together.
[0537] 4.3.2 Electrochemical Testing of Pseudo-Solid Full Cells. After assembly, the cells were rested for at least one day at 25 °C to allow time for interphase formation prior to cycling. The electrochemical testing was also performed at 25 °C. While NMC622 can be cycled to high voltages, the material can be subject to more severe degradation above 4.3 V [B 106], For this reason, cycling of the cells was performed with an Arbin LBT21084 between cutoff voltages of 3.0-4.3V.
[0538] For the formation cycle, the cells underwent one slow charge and discharge cycle at 0.03mA / cm2, corresponding to a C-rate of approximately C / 50 based on the cathode nominal capacity. EIS from 5 MHz to 20 mHz with 10 points per decade and an excitation amplitude of 10 mV was then used to measure the impedance at the discharged state. Separate sets of 3 cells (for both 0 wt% PPy(DBS) and 1 wt% PPy(DBS) polymer interlayers) were then cycled at different areal current densities: 0.3 mA / cm2(C-rate of approximately C / 5 based on cathode capacity) or 0.5 mA / cm2(approximately C / 3). EIS was initially performed at the discharged state after every 5 charge / discharge cycles. However, due to large differences in impedance results after the cells were cycled at the higher current density (likely due to different SOCs at the ‘discharged’ state), an additional EIS was performed on subsequent cells after the first higher current density cycle (followed by EIS every 5thcharge / discharge cycle).
[0539] The specific capacities of the cells at each cycle are shown in FIGs. 52A-52B and FIGs.
[0540] 53 A-53B for current densities of 0.3 mA / cm2and 0.5 mA / cm2, respectively. Figure 52A and FIG. 53 A plot the specific capacity computed with respect to the mass of the cathode, while FIG.
[0541] 52B and FIG. 53B consider the total mass of the internal cell stack (including cathode, high concentrated liquid electrolyte, Celgard separator, LLZTO ceramic solid electrolyte, polymer interlayer, and Li-metal anode). The specific capacities with respect to the cathode mass are slightly below 100 mAh / g, compared to the theoretical capacity for NMC 622 in ideal fully liquid electrolyte cells that is approximately equal to 175 mAh / g [B106, B107] in the same voltage range of 3.0-4.3 V. This lower capacity is to be expected, considering all the components in the LIMSSB cell stack shown in FIG. 50. Compared to an ideal cell comprising of just the cathode, liquid electrolyte with Celgard separator, and anode, the additional impedance introduced from the thick LLZTO ceramic solid electrolyte and the polymer interlayer indirectly reduces the lithiation range of the NMC622 cathode between the cutoff voltages of 3.0-4.3 V. The higher impedances (also discussed in the prior sections) cause higher overpotentials, leading to the cell reaching the cutoff voltages sooner. Thus, the specific capacities with respect to the total mass of the internal cell stack in FIG. 52B and FIG. 53B are more indicative of the components involved.
[0542] To compare the capacity degradation and account for any differences in the initial discharge capacities between the cells, FIGs. 54A-54B compares the capacity retention (normalized as a percentage of the first measured discharge capacity) of the cells with number of cycles. While a bare ceramic solid electrolyte / Li-metal interface can experience degradation and result in cells shorting within a few cycles or less than a day of cycling [Bl 8, B25, Bl 08, Bl 09], the inclusion of a polymer interlayer in these cells inhibits the degradation of the Li-metal interface [B25, B108, B109], without showing appreciable degradation after 30 cycles. Due tolimitations in the cell setup, such as the thick ceramic solid electrolyte, the potential drop across the layers in the cell prior to the polymer interlayer is expected to be significant [Bl 8, Bl 08, Bl 09], This could result in insufficient electric field strength across the polymer interlayer, which could in turn not induce the adaptive property that, as shown above, is evident at electric field strength values above 0.1-0.2 V / pm. This assumption is motivated by the fact that no clear difference is observed in the trends for the baseline (0 wt% PPy(DBS)) polymer interlayer versus adaptive (1 wt% PPy(DBS)) polymer interlayer cells for 30 cycles at 0.3 mA / cm2or 0.5 mA / cm2. The coulombic efficiencies (ratio of discharge capacity to charge capacity each cycle) are also compared in FIGs. 65A-65B and stayed around 100% for all the cells over cycling.
[0543] Impedance analysis was performed using EIS and distribution of relaxation times (DRT), which can help differentiate between the sources of impedance in the cell and potentially detect changes or trends in these impedances before the effect is visible in cycling results. DRT is a method for the analysis of impedance data that can further deconvolute impedance contributions in complex EIS data that may not be otherwise differentiated from Nyquist plots [B110-B112], DRT converts the EIS data into peaks separated based on time constants and peak intensities from the corresponding impedance. As the physical impedance sources typically have different relaxation times and corresponding characteristic time constants, DRT can better separate these sources. DRT analysis is performed on the EIS data using the DRTtools MATLAB code developed by literature [Bl 10],
[0544] Li symmetric cells with the solid polymer electrolyte (SPE) from above were first analyzed to determine the contributions from Li-metal, SPE, and the interface between them. The Nyquist plot from EIS in FIG. 55A and the corresponding DRT in FIG. 55B display two major peaks labeled as Pl and P2. Peak Pl, occurring at high frequency (around 104Hz), is attributed to the impedance from the solid electrolyte interphase (SEI) formed between the Li-metal anode and the SPE. Peak P2 (around 103Hz) is attributed to the interfacial impedance (physical contact) between the Li-metal anode and the SPE. These peak associations agree with the DRT of cells with Li-metal from [Bill, Bl 12], The LLZTO / polymer interlayer was next incorporated in the Li symmetric cells, with the resulting Nyquist plot shown in FIG. 55C and the corresponding DRT in FIG. 55D, to determine any changes or additional peaks due to the addition of the ceramic electrolyte. The results indicate that no new peaks appear in the DRT, suggesting that any additional impedance contribution from the solid-state electrolyte and the LLZTO / polymer interlayer interface are included in peaks Pl and P2.
[0545] EIS and DRT are also analyzed from the first batch of coin cells, to determine the additional contributions from the inclusion of the NMC622 cathode with high concentratedelectrolyte and Celgard separator (FIGs. 56A-56D). Contributions to the DRT from degradation of the cathode interface can also be determined as the cells had fully or partially dried up at the cathode interface due to insufficient high concentrated electrolyte (FIGs. 56A, 56B and FIGs. 56C, 56D, respectively). With the inclusion of the cathode, an additional major peak labeled P3 (around 10° Hz) appears in the DRT. This peak is attributed to the charge transfer impedance of the cathode, which is in agreement with the findings for an NMC / solid electrolyte cell from [Bill], The contribution of any cathode-electrolyte interphase that formed would be included in peak Pl. The peaks P2 and P3 increasing with the number of cycles are attributed to the degradation of the cathode side of the cell, due to the viscous electrolyte drying up at the cathode interface over cycling. This shows P2 is a combination of the interfacial impedance (physical contact) for both the Li-metal anode (as P2 was present in the Li symmetric cells) and the NMC622 cathode. Thus, an observed increase in the magnitude of both P2 and P3 would suggest degradation at the NMC622 cathode interface, whereas an increase in just P2 would suggest degradation at the Li-metal anode interface.
[0546] For a representative LIMSSB cell of each composition from the updated assembly process (with sufficient amount of high concentrated electrolyte on the cathode side) cycled at an areal current density of 0.5 mA / cm2, the Nyquist plots from EIS are shown in FIGs. 57A, 57C and the corresponding DRT in FIGs. 57B, 57D. The major peaks P1-P3 are present in the DRT, as expected from the prior results, with an additional major peak P4 (around 10'1Hz) appearing that was not present in the cells with a cathode interface drying up. Based on the frequency P4 appears at and as suggested in [Bill], P4 can likely be attributed to Li-ion diffusion in the NMC622 cathode. The P4 peak may not have been present in the cells that dried up at the cathode interface, as insufficient electrolyte to wet the cathode may have resulted in negligible Li-ion diffusion through the bulk of the cathode.
[0547] Overall, the EIS and DRT results indicate a decrease in impedances during cycling and do not show a clear increase that would indicate sources of impedance resulting from degradation or damage to the cell components. A clear increase in peak P2 over cycling would be expected if there was appreciable degradation at the Li-metal anode interface. Also, peak P2 increasing over cycling more for the 0 wt% PPy(DBS) polymer interlayer (baseline polymer interlayer) compared to the 1 wt% PPy(DBS) polymer interlayer (adaptive polymer interlayer) would suggest the adaptive polymer interlayer is able to stabilize the Li-metal interface, however this trend is not observed in the data obtained from the experiments. The EIS and DRT results are similar for the rest of the cells, shown in FIGs. 66A-66D through FIGs. 70A-70D.
[0548] Inconsistences in the impedances over cycling could partially be due to variations in the state ofcharge (SOC) of the LIMSSB cells in the ‘discharged’ state over cycling. As the cycling rates are relatively high for these types of cells with large overpotentials, consistent SOCs after cycling cannot easily be achieved without prematurely reaching the cutoff voltages. Using a lower current to reach a targeted SOC would not be desirable as the lower current could partially heal any degradation present at the Li-metal anode interface.
[0549] The EIS and DRT results obtained from this set of experimental tests further support the hypothesis that the adaptive property of the 1 wt% PPy(DBS) polymer interlayer is not currently taking effect. The impedances have not clearly increased over the number of cycles, suggesting there has not yet been significant degradation of the interfaces. The high impedances of the cells overall (due to all the components in the stack in FIG. 50) can prevent sufficient electric field strength across the polymer interlayer to induce the adaptive response.
[0550] 4.3.3 Reference Electrode in Pseudo-Solid Full Cell. To obtain a rough estimate of the potential drop across the polymer layer in the cells, a 3-electrode LIMSSB cell was assembled with a reference electrode (RE) inserted between the LLZTO ceramic electrolyte and a freestanding polymer electrolyte layer. The design of this cell is shown in FIG. 58. A 25 pm diameter wire RE was used to minimize disturbance in the cell while still allowing the wire to be handled during assembly [Bl 13], Gold wire was used as it can be Li-alloyed in-situ after assembly in the cell, resulting in a Li-alloyed gold wire RE (REHAU) that has been shown to be a suitable RE with a stable reference potential of approximately 0.32V vs. Li / Li+[Bl 14], A small amount of high concentrated electrolyte was added between the RE wire and LLZTO for improving contact. Without the liquid, the contact was found too rigid and the RE could not measure any potential. The method of routing the RE wire out of the coin cell while still allowing the coin cell to be crimped and sealed was adapted from [Bl 15], For the battery tester connectors to achieve sufficient electrical connection with the RE wire outside of the cell, the wire was adhered to copper tape using silver paste then the battery tester connectors were connected to the copper tape. A BioLogic VMP3 Potentiostat was used for the electrochemical tests of the 3-electrode cell.
[0551] The in-situ lithiation of the RE and subsequent potential stability are shown in FIG. 59. The gold wire is Li-alloyed at a current of -0.5 pAfor 10 hr with the gold wire connected as the working electrode and Li-metal as the counter / reference electrode. The subsequent potential of the RE at rest was stable at approximately 0.32V vs. Li / Li+.
[0552] The potential drop across the polymer layer was estimated based on the RE measurements while the cell was charging or discharging at different current densities compared to a condition at rest, as shown in FIG. 60. The estimated potential drops were up to 0.14V at thecurrent densities tested. While the actual potential drop in the tests described herein may be a bit higher due to the higher current densities tested at (0.3-0.5 mA / cm2) and the RE may not include potential drop across the LLZTO / polymer interlayer interface, these results support the hypothesis that the potential drop across the polymer interlayer is too small for a sufficient electric field strength to induce the adaptive response. The average thickness of the polymer interlayers was approximately 5 pm (varied from 1-10 pm across a cross-section), so an electric field strength of 0.1-0.2 V / pm for the adaptive response would require a potential drop across the interlayer of 0.5-1 V in the current setup.
[0553] 4.4 Summary. The steps for transitioning an adaptive polymer electrolyte to an adaptive polymer interlayer that was then incorporated in prototype LIMSSB cells between the Li-metal anode and ceramic solid electrolyte were presented. LLZTO ceramic solid electrolyte pellets for use in the full cells were successfully synthesized using commercially purchased LLZTO nm-powder in pressed pellets with commercially purchased LLZTO pm-powder used for covering the pellets during high-temperature sintering. These oven-sintered pellets with an average ionic conductivity of approximately 0.49 mS / cm were found to be an adequate replacement for the prohibitively expensive commercially purchased LLZTO pellets. To obtain a thin polymer interlayer, coating the polymer directly on the Li-metal anode or LLZTO pellet was tested.
[0554] Results of coating the polymer directly on Li-metal suggested the polymer composition used in this work was not stable when polymerizing directly on Li-metal. However, the results of coating the polymer directly on LLZTO showed the polymerization directly on the LLZTO surface was stable. The process of coating the polymer interlayer on LLZTO was further improved by replacing the PET cover sheet with a lower adhesion FEP cover sheet to prevent delamination of the polymer interlayer from the LLZTO surface after UV polymerization. A polymer interlayer coating on the LLZTO surface with an average thickness of 5 pm was achieved.
[0555] By incorporating the adaptive polymer interlayer in prototype LIMSSB cells, the feasibility of the adaptive property occurring in a full cell configuration was investigated. As the degradation on the Li-metal interface side of the cell was of interest, a viscous liquid electrolyte (high concentrated electrolyte) was added on the cathode side of the cell to try to minimize the impedance and degradation of the cathode interface. Electrochemical testing including cycling, EIS, and DRT of the cells with a baseline polymer interlayer (0 wt% PPy(DBS)) and an adaptive polymer interlayer (1 wt% PPy(DBS)) was performed to determine if the adaptive polymer interlayer reduced degradation of the Li-metal anode interface compared to a baseline polymer interlayer. Thus far for 20 cycles at 0.3 mA / cm2or 0.5 mA / cm2there was no appreciable degradation, which can be expected for the polymer interlayer already reducing the degradationcompared to a bare Li-metal / ceramic solid electrolyte interface that would quickly degrade and lead to cell failure. No clear difference in the trends for the baseline (0 wt% PPy(DBS)) polymer interlayer versus adaptive (1 wt% PPy(DBS)) polymer interlayer cells suggested there may be insufficient electric field strength across the interlayer to induce the adaptive property. This was further supported with the relatively high impedances shown in the EIS and DRT results due to limitations in the cell setup (such as the thick ceramic solid electrolyte layer). The results indicated that there was no observable trend in the impedances attributed to the Li-metal interface between the baseline and adaptive polymer interlayer cells.
[0556] The results obtained were confirmed by incorporating a reference electrode into a 3-electrode LIMSSB cell to estimate the potential drop across the polymer layer. Results from cycling tests at different current densities corroborated the hypothesis that there may be insufficient electric field strength across the polymer interlayer.
[0557] The results from the tests described herein indicate the next steps that could be taken to prove the feasibility of the adaptive polymer, including alternate methods to analyze mechanical degradation at the Li-metal interface or improvements in the cell design to increase the electric field strength across the polymer interlayer. To investigate any differences in the mechanical degradation at the Li-metal anode for the baseline versus adaptive polymer interlayer cells after cycling, the surface morphology of the Li-metal anode that was in contact with the polymer interlayer can be investigated with SEM imaging (as the Li-metal comes detached from the polymer interlayer during disassembly). Alternatively, to preserve the Li-metal / polymer interlayer interface, a hole could be drilled in the coin cell case and the cell flooded with epoxy, followed by cutting the cell in haff to image the cross-section. Non-destructive imaging techniques are another option such as X-ray computed tomography (CT), but this solution requires a micro-CT or nano-CT with sufficient sub-pm resolution.
[0558] A potential path to improve the cell design would be to reduce the thickness of the ceramic solid electrolyte, which would allow for a greater potential drop across the polymer interlayer. However, achieving thinner ceramic solid electrolytes is still an active area of research. Cathode-supported thin ceramic solid electrolytes could be pursued, but the interface between the cathode and ceramic solid electrolyte might remain a challenge. A sheet of ceramic solid electrolyte with more consistent thickness could also enable a thinner and more uniform polymer interlayer coating on the ceramic electrolyte through methods such as doctor blade coating.
[0559] 5.1 Summary and Contributions. With the increasing demand for improved safety and energy density of batteries for widespread electrification, there is interest in solid-state batteries,especially Li-metal solid-state batteries (LIMSSBs). However, achieving stability in the Li-metal / solid electrolyte interface, both mechanically and electrochemically, is one of the crucial challenges that needs addressed to enable safe and reliable LIMSSB technology.
[0560] This example experimentally investigates an adaptive polymer interlayer that is able to expand upon being exposed to an electric field. The morphing ability of the interlayer makes it a potential candidate to stabilize the Li-metal / solid electrolyte interface, namely by reversibly maintaining contact with the Li-metal anode during cycling through polarization of conducting polymer (CP) particles, preventing the formation of dendrites.
[0561] The synthesis process and composition of the polymer interlayer was optimized before further characterizations of the adaptive property were performed. Initially, a pure polypyrrole doped with dodecylbenzensulfonate (PPy(DBS)) CP film was tested for the interlayer.
[0562] Electrochemical testing results indicated a lack of Li-ion transfer through the pure Ppy(DBS) in the solid-state system and the electrical conductivity of the film would inhibit any electric field strength across the interlayer. Thus, different polymer electrolyte compositions were investigated for further use as composite films for the adaptive polymer comprising of CP particles in an electrically insulative and ionically conductive polymer electrolyte matrix. A UV polymerized polymer electrolyte was synthesized with adequate electrochemical performance at room temperature, which was desirable for equivalent comparisons between additional characterizations, and a thin enough consistency of the uncured polymer solution to enable a thinner polymer interlayer between Li-metal and ceramic solid electrolyte.
[0563] The adaptive polymer, comprising of Ppy(DBS) particles in a polymer electrolyte matrix, was characterized as an adaptive polymer electrolyte to demonstrate the adaptive behavior.
[0564] Atomic force microscopy (AFM) and block force measurements confirmed the adaptive property, showing an expansion up to 6% strain under an electric field strength of 0.3 V / pm, repeatable over several actuations. The adaptive property was determined to occur under minimum electric field strengths of 0.1-0.2 V / pm. Electrochemical and physical characterizations of the adaptive polymer electrolyte showed the appreciable difference in other properties from the inclusion of Ppy(DBS) particles was slightly inhibiting the UV curing and lowering the insoluble fraction of the films. Otherwise, the adaptive polymer electrolyte performed similarly as the control polymer electrolyte, with the addition of the adaptive property.
[0565] After successful completion of the characterization experiments, the polymer electrolyte was integrated into a prototype LIMSSB coin cell to test its operation as an interlayer with a solid electrolyte. ALi6.4La3Zn.4Tao.6O12 (LLZTO) ceramic solid electrolyte was synthesizedfrom commercially purchased powder with adequate performance using oven-sintering, for use in solid-state cells. The current polymer interlayer composition was found to be incompatible with coating directly on the Li-metal anode but was compatible coating directly on the LLZTO ceramic solid electrolyte. After testing different synthesis methods, a polymer interlayer coating on LLZTO with an average thickness of approximately 5 pm was achieved. Electrochemical testing of pseudo-solid full cells with polymer interlayers did not exhibit much degradation thus far, showing an expected improvement over bare ceramic solid electrolyte / Li-metal interface that has been reported to fail within a few cycles or less than a day. However, the data did not show clear differences in the trends for the (0 wt% Ppy(DBS)) polymer interlayer versus the adaptive (1 wt% Ppy(DBS)) polymer interlayer cells. The results suggested that there may be insufficient electric field strength across the polymer interlayer to induce the desired adaptive property, due to the potential drop caused by the thick ceramic electrolyte. This finding was further supported by conducting electrochemical impedance spectroscopy (EIS) and distribution of relaxation times (DRT), which indicated impedance from bulk resistance of the ceramic electrolyte and overpotential at the anode-electrolyte interface. A confirmation test was also conducted by constructing a 3 -electrode cell, which allowed for estimating the potential drop across the polymer layer.
[0566] 5.2 Future Directions. This work demonstrated the adaptive property of an adaptive polymer electrolyte expanding under relatively low electric field strengths due to the inclusion of CP particles in a polymer electrolyte matrix. The research documented in this herein lays the groundwork for proving the feasibility of the adaptive property in an adaptive polymer interlayer in a solid-state cell between the Li-metal anode and ceramic solid electrolyte. As discussed herein, the next steps could include improving upon the limitations in the current cell design, such as reducing the thickness of the ceramic electrolyte with methods such as tape casting or cathode supported ceramic solid electrolyte.
[0567] Further research could focus on direct observation of CP particle alignment in a polymer matrix under an electric field, or improvements in the adaptive polymer electrolyte and interlayer. The adaptive property could be improved by achieving a higher loading of CP in a polymer matrix or even through different types of CP or other similarly polarizable particles. To maintain the advantages of UV polymerization while increasing CP loading, co-polymerization of CP from monomer with the polymer matrix may be investigated. Alternatively, other polymer film synthesis methods such as thermal polymerization or solvent casting could be explored where the CP particles inhibiting UV curing through blocking UV transmittance would not be a factor, although maintaining dispersion and preventing agglomeration of CP particles over thelonger synthesis time may be a challenge. These alternate synthesis methods could also support transitioning the polymer interlayer to larger manufacturing scale, such as casting in-line in a roll-to-roll manufacturing process. Otherwise, to transition the current synthesis method of hot-pressing and subsequent UV curing, alterations to the process would need to be made such as enabling a transfer film process to apply the cured (or partially cured) interlayer to the Li-metal anode or ceramic solid electrolyte. Reducing the baseline impedance of the polymer interlayer would also be of interest through improved compositions with lower interfacial impedance and developing an even thinner interlayer. For thin interlayers approaching 1 pm thick or sub-pm, further reducing CP particle size down to nanoparticle size would be a useful factor, as the interlayer would need to be as thick as at least a few particles or agglomerates of particles. To determine if the expansion is a constant strain value that scales with the polymer thickness and would be reduced with reduced polymer thickness, the relationship between the expansion amount through the adaptive property and polymer thickness should be explored.
[0568] Chemical polymerization of polypyrrole doped with dodecylbenzenesulfonate (PPy(DBS)) particles. A polymerization solution of 0.375M pyrrole (reagent grade 98%, Sigma-Aldrich) monomer, 0.030MNaDBS (technical grade, Sigma-Aldrich) for DBS' dopant, and 0.100M Fe2(SC>4)3 (97%, Thermo Scientific) chemical oxidant was prepared in 200 mL of deionized (DI) water. One half solution of pyrrole and NaDBS was stirred in 100 mL of DI water, and the other half solution of Fe2(SO4)3 was stirred in a separate 100 mL of DI water. The solution with Fe2(SO4)3 was slowly poured into the solution with pyrrole and NaDBS until fully combined, and the polymerization reaction was allowed to proceed for 16h at room temperature (20-25 °C) under slow magnetic stirring. The solution was then poured through 0.8 pm filter paper, rinsed with DI water until the filtrate is neutral pH, rinsed with ethanol several times, dried at 40 °C under vacuum (gauge pressure -0.95 bar) for 24h, and manually grinded with a mortar and pestle. The reaction yielded 2.1g of PPy(DBS) particles (approximately 13.6 mL loosely packed).
[0569] UV polymerization of polymer electrolyte matrix - final composition. The UV polymerized polymer electrolyte was composed of 30.3 wt% PEO (approximate 100,000 MW, Thermo Scientific) as the main long chain polymer, 15.1 wt% TEGDMA (>90% technical grade, Sigma-Aldrich) as an additional cross-linking short chain monomer, 30.3 wt% TEGDME (>99%, Sigma-Aldrich) as cross-linking plasticizer, 17.8 wt% LiTFSI (99.95% trace metals basis, Sigma-Aldrich) as the main Li salt, 3.5 wt% LiBoB (Sigma- Aldrich) as additional Li salt (20% of LiTFSI amount), and 3.0 wt% MBP (99%, Sigma-Aldrich) as photoinitiator. The components were combined in an argon-filled glovebox, magnetic stirred overnight (at roomtemperature, 20-25 °C, in a sealed vial) to form a viscous liquid mixture, then ultrasonicated for 10 min prior to hot-pressing. In ambient air, the mixture was hot-pressed between PET sheets (McMaster-Carr) at 80 °C under 4.4 bar of pressure for 10 min (film thickness set to around 125 pm with a spacer). The film was polymerized for 10-20 min under UV light with 150 mW / cm2intensity at the film surface (main wavenumber 365 nm), flipping the film over halfway through the UV curing process, to obtain the polymer electrolyte. The polymer electrolyte film was vacuum dried (gauge pressure -0.95 bar) overnight at 40 °C to try to remove residual moisture prior to further characterizations.
[0570] Synthesis of ceramic LLZTO pellets from commercial powder. To obtain properly densified Li6.4La3Zn.4Tao.6O12 (LLZTO) pellets from the commercially purchased powder as-is, access to a high-temperature (>1000 °C) high-pressure (30-40 MPa) pellet press would be needed, where the pellet can be densified in approximately 1 hr [Bl 16], Alternatively, if access to this equipment is not available, the powder should be cold-pressed into pellets at high pressure followed by sintering in a high-temperature furnace for several hours. Since the pellet is at high temperatures for a longer period in a more open configuration, excess Li must be added to account for Li loss during the oven sintering process.
[0571] The commercial LLZTO powder (pm-sized or nm-sized) was first manually mixed with 10 wt% Li OH (anhydrous laboratory grade from Thermo Scientific, dried at 200 °C overnight before use) to provide excess Li in a mortar and pestle, then 1g of the resulting powder was added to a lubricated 14.85 mm diameter pressing die (pressing die from MTI Corporation, and the inside of the pressing die is manually lubricated with a small amount of stearic acid mixed in acetone) and cold-pressed (at room temperature) uniaxially at 200 MPa for 3 min (Carver 3851-0 hydraulic press) to obtain a ceramic electrolyte green pellet. Next, the green pellet was removed from the die and placed on top of a small amount of pm-sized commercial LLZTO powder (for both types of pellets from pm-sized powder or nm-sized powder) in a MgO crucible then the pellets were covered with more pm-sized commercial LLZTO powder. The MgO crucible was covered with a loose fitting MgO lid prior to placing in the oven (KSL-1700X high temperature box furnace from MTI Corporation) for sintering. The pellets from pm-sized powder were sintered at 1250 °C for 12 hr with a 5 °C / min heating and cooling rate. The pellets from nm-sized powder were sintered at 1210 °C for 3 hr with a 2 °C / min heating rate and 5 °C / min cooling rate. After allowing the pellets to cool, they were roughly polished on a rotary polisher at 200 rpm (UNIPOL-810 precision lapping / polishing machine from MTI Corporation) using ethanol as a lubricant to approximately 700 pm thickness. The pellets were then transferred to an argon-filled glovebox for a final dry-polishing performed manually with 400-grit followed by800-grit SiC sandpaper (McMaster-Carr). After polishing, the pellets were wiped with a small amount of dimethyl carbonate (DMC) to remove polishing dust and allowed to dry in the glovebox prior to use.
[0572] Synthesis of NMC622 cathode sheets. A 90:5:5 (active material :binder:conductive additive) LiNio.6Mno.2Coo.2O2 (NMC622) cathode slurry for coating current collector sheet is made by mixing ultra-high molecular weight polyvinylidene fluoride (PVDF, Kynar HSV 900) as binder, Super P conductive carbon black (from MSE Supplies) as electrically conductive additive, and NMC622 powder (from MSE Supplies, D50 particle size 9-14 pm) as the cathode active material in N-methyl-2-pyrrolidone (NMP, 99.5+% from Thermo Scientific) as the solvent. 0.1g of PVDF and 2.5g of NMP were combined in a 12 mL Thinky mixer container with 2 zirconia mixer beads, then mixed for 8-10 min at 2000 rpm in a planetary centrifugal mixer (Thinky Mixer ARE-310) until the PVDF particles were no longer visible. Next, 0.1g of Super P was added to the container and mixed for an additional 2-3 min until a homogeneous, viscous black gel. Last, 1.8g of NMC622 powder was added and mixed for an additional 2-3 min until a less viscous, homogeneous black gel.
[0573] The resulting cathode slurry was coated 225 pm thick using a doctor blade onto carbon coated Al foil current collector (15 pm thick) sheet. The slurry coated foil was then dried in an oven on a glass plate at 90 °C for 30 min to evaporate most of the NMP solvent. Next, with a bare Al foil sheet on the bottom and the cathode coated foil on top (with cathode material facing down towards the bare Al foil), the cathode sheet was hot calendared (using MSK-HRP-1 A hot rolling press from MTI Corporation) with the rollers at 85 °C. The calendaring passes were started at the initial thickness of the foils and cathode layer and gradually decreasing the calendaring thickness with each pass until achieving a final cathode layer thickness of approximately 50 pm. The areal active material loading of the resulting cathode sheet was approximately 10 mg / cm2. Lastly, with the cathode layer facing up a polyethylene coated weighing paper was placed on top, and 9.5 mm diameter disc electrodes were punched out of the cathode sheet for use in coin cells.
[0574] References
[0575] [Bl] Zubi G et al. The lithium-ion battery: State of the art and future perspectives. Renewable and Sustainable Energy Reviews 2018;89:292-308.
[0576] [B2] Ghafari A. Current and future prospects of Li-ion batteries: A review. J NanoSci Tec 2023. doi:10.52319 / j.nanoscitec.2023.21.
[0577] [B3] Schmaltz T, Hartmann F, Wicke T, Weymann L, Neef C, Janek J. A Roadmap for Solid-State Batteries. Advanced Energy Materials 2023;13(43):2301886.[B4] Janek J, Zeier WG. A solid future for battery development. Nature Energy 2016; 1(9): 16141.
[0578] [B5] KamayaN et al. Alithium superionic conductor. Nature Mater 2011;10(9):682-686.
[0579] [B6] Seino Y et al. A sulphide lithium super ion conductor is superior to liquid ion conductors for use in rechargeable batteries. Energy Environ Sci 2014;7(2):627— 631.
[0580] [B7] Kato Y et al. High-power all-solid-state batteries using sulfide superionic conductors. Nat Energy 2016;l(4):16030.
[0581] [B8] Kim KJ et al. Solid-State Li-Metal Batteries: Challenges and Horizons of Oxide and Sulfide Solid Electrolytes and Their Interfaces. Advanced Energy Materials 2021;ll(l):2002689.
[0582] [B9] Krauskopf T et al. Toward a Fundamental Understanding of the Lithium Metal Anode in Solid-State Batteries - An Electrochemo-Mechanical Study on the Garnet- Type Solid Electrolyte Li6.25Alo.25La3Zr20i2. ACS Applied Materials and Interfaces 2019; 11(15): 14463— 14477.
[0583] [BIO] Kerman K et al. Review — Practical Challenges Hindering the Development of Solid State Li Ion Batteries. Journal of The Electrochemical Society 2017; 164(7): A1731-A1744.
[0584] [B 11 ] Zhang X et al. Pressure-Driven Interface Evolution in Solid-State Lithium Metal Batteries. Cell Reports Physical Science 2020; 1(2). doi: 10.1016 / j.xcrp.2019.100012.
[0585] [B12] Zhu Y et al. Origin of Outstanding Stability in the Lithium Solid Electrolyte Materials: Insights from Thermodynamic Analyses Based on First-Principles Calculations. ACS Applied Materials & Interfaces 2015;7(42):23685-23693.
[0586] [Bl 3] Han F et al. Electrochemical Stability of Li io GeP 2 S 12 and Li 7 La 3 Zr 2 O 12 Solid Electrolytes. Advanced Energy Materials 2016;6(8): 1501590.
[0587] [B14] Ohno S et al. Materials design of ionic conductors for solid state batteries.
[0588] Progress in Energy 2020;2(2): 022001.
[0589] [B15] Weiss M et al. Fast Charging of Lithium-Ion Batteries: AReview of Materials Aspects. Advanced Energy Materials 2021 ; 11(33):2101126.
[0590] [Bl 6] Lin D et al. Reviving the lithium metal anode for high-energy batteries. Nature Nanotech 2017; 12(3): 194-206.
[0591] [B17] Sanchez AJ et al. Lithium stripping: anisotropic evolution and faceting of pits revealed byoperando3-D microscopy. J Mat ChemA 2021;9(37):21013-21023.
[0592] [Bl 8] Ren Y et al. Direct observation of lithium dendrites inside garnet-type lithium-ion solid electrolyte. Electrochemistry Communications 2015;57:27-30.[B 19] Nagao M et al. In situ SEM study of a lithium deposition and dissolution mechanism in a bulk-type solid-state cell with a Li2S-P2S5 solid electrolyte. Phys Chem Chem / zys2013;15(42):18600.
[0593] [B20] Tan DHS et al. From nanoscale interface characterization to sustainable energy storage using all-solid-state batteries. Nature Nanotechnology 2020;15(3):170-180.
[0594] [B21] Sen S et al. The role of polymers in lithium solid-state batteries with inorganic solid electrolytes. Journal of Materials Chemistry A 2021;9(35): 18701-18732.
[0595] [B22] Han X et al. Negating interfacial impedance in garnet-based solid-state Li metal batteries. Nature Materials 2017;16(5):572-579.
[0596] [B23] Ruan Y et al. A 3D Cross-Linking Lithiophilic and Electronically Insulating Interfacial Engineering for Garnet-Type Solid-State Lithium Batteries. Advanced Functional Materials 2021;31(5):2007815.
[0597] [B24] Zhang W et al. LivLasZnOn Ceramic Nanofiber-Incorporated Solid Polymer Electrolytes for Flexible Lithium Batteries. ACSAppl Energy Mater 2020;3(6):5238-5246.
[0598] [B25] Yang Z et al. Facile interfacial adhesion enabled LATP -based solid-state lithium metal battery. Chemical Engineering Journal 2020;392: 123650.
[0599] [B26] Zhang J et al. Flexible and ion-conducting membrane electrolytes for solid-state lithium batteries: Dispersion of garnet nanoparticles in insulating polyethylene oxide. Nano Energy 2016;28:447-454.
[0600] [B27] Duan H et al. Dendrite-Free Li-Metal Battery Enabled by a Thin Asymmetric Solid Electrolyte with Engineered Layers. Journal of the American Chemical Society 2018;140(l):82-85.
[0601] [B28] Simon FJ et al. Properties of the Interphase Formed between Argyrodite-Type Li 6 PS 5 Cl and Polymer-Based PEO io :LiTFSI. ACS Applied Materials & Interfaces 2019;ll(45):42186-42196.
[0602] [B29] Han F et al. High electronic conductivity as the origin of lithium dendrite formation within solid electrolytes. Nature Energy 2019;4(3): 187-196.
[0603] [B30] Dietrich C et al. Lithium ion conductivity in Li 2 S-P 2 S 5 glasses - building units and local structure evolution during the crystallization of superionic conductors LLPS-r LivPsSi 1 and Li4P2S7. Journal of Materials Chemistry A 2017;5(34): 18111— 18119.
[0604] [B31] Wang H et al. Reviewing the current status and development of polymer electrolytes for solid-state lithium batteries. Energy Storage Materials 2020;33:188-215.
[0605] [B32] Nair JR et al. Lithium Metal Polymer Electrolyte Batteries: Opportunities and Challenges. Electrochem Soc Interface 2019;28(2):55-61.[B33] Liu K et al. Polyoxyethylene (PEO)|PEO-Perovskite|PEO Composite Electrolyte for All-Solid-State Lithium Metal Batteries. ACS Applied Materials and Interfaces 2019;ll(50):46930-46937.
[0606] [B34] Zheng J et al. Interface-Enabled Ion Conduction in LiioGeP2Si2 -Poly(ethylene Oxide) Hybrid Electrolytes. ACSAppl Energy Mater 2019;2(2): 1452-1459.
[0607] [B35] Wang S et al. High-conductivity free-standing Li6PS5Cl / poly(vinylidene difluoride) composite solid electrolyte membranes for lithium-ion batteries. Journal of Materiomics 2020;6(l):70-76.
[0608] [B36] Jang DS et al. Polypyrrole-wrapped halloysite nanocomposite and its rheological response under electric fields. Journal of Materials Science 2014;49(20):7309-7316.
[0609] [B37] Teare GC, Ratcliffe NM. Electrorheological properties of polypyrrole prepared by the action of mineral acids on pyrrole. Journal of Materials Chemistry 1996;6(3):301.
[0610] [B38] Kim D-H, Kim YD. Electrorheological Properties of Polypyrrole and its Composite ER Fluids. Journal of Industrial and Engineering Chemistry 2007;13(6):879-894.
[0611] [B39] Fang FF, Liu YD, Choi HJ. Electrorheological and magnetorheological response of polypyrrol e / magnetite nanocomposite particles. Colloid and Polymer Science 2013;291(7):1781-1786.
[0612] [B40] Chen P et al. Fabrication of dual-coated graphene oxide nanosheets by polypyrrole and poly(ionic liquid) and their enhanced electrorheological responses. Journal of Industrial and Engineering Chemistry 2019;69:106-115.
[0613] [B41] Ludeelerd P et al. Effect of elastomer matrix type on electromechanical response of conductive polypyrrol e / elastomer blends. Journal of Physics and Chemistry of Solids 2010;71(9):1243-1250.
[0614] [B42] Wichiansee W, Sirivat A. Electrorheological properties of poly(dimethylsiloxane) and poly(3,4-ethylenedioxy thiophene) / poly(stylene sulfonic acid) / ethylene glycol blends.
[0615] Materials Science and Engineering: C 2009;29(l):78-84.
[0616] [B43] Lundin V et al. Control of Neural Stem Cell Survival by Electroactive Polymer Substrates. PLoS ONE 2011;6(4):el8624.
[0617] [B44] Pyarasani RD et al. Polyaniline-based conducting hydrogels. J Mater Sci 2019;54(2):974-996.
[0618] [B45] Yuan X et al. A stable high-performance isotropic electrorheological elastomer towards controllable and reversible circular motion. Composites Part B: Engineering 2020;193:107988.
[0619] [B46] Ma N et al. Properties and mechanical model of a stiffness tunable viscoelasticdamper based on electrorheological elastomers. Smart Mater Struct 2020 29(4) :045041.
[0620] [B47] Teh K-S, Lin L. MEMS sensor material based on polypyrrole-carbon nanotube nanocomposite: film deposition and characterization. Journal of Micromechanics and Microengineering 2005;15(ll):2019-2027.
[0621] [B48] Garcia B et al. Oxi de / Poly pyrrole Composite Films for Corrosion Protection of Iron. Journal of The Electrochemical Society 2002; 149(12):B560.
[0622] [B49] Cui X, Martin DC. Fuzzy gold electrodes for lowering impedance and improving adhesion with electrodeposited conducting polymer films. Sensors and Actuators A: Physical 2003;103(3):384-394.
[0623] [B50] Pyo M et al. Direct strain measurement of polypyrrole actuators controlled by the polymer / gold interface. Chemistry of Materials 2003; 15(4): 916-922.
[0624] [B51] Wang Y, Northwood DO. An investigation into the nucleation and growth of an electropolymerized polypyrrole coating on a 316L stainless steel surface. Thin Solid Films 2008;516(21):7427-7432.
[0625] [B52] Otero TF et al. Electrochemomechanical properties from a bilayer: polypyrrole / non-conducting and flexible material — artificial muscle. Journal of Electroanalytical Chemistry 1992;341(1— 2):369— 375.
[0626] [B53] Ikushima K et al. A practical multilayered conducting polymer actuator with scalable work output. Smart Materials and Structures 2009;18(9):095022.
[0627] [B54] Otero TF et al. Mechanical characterization of free-standing polypyrrole film. Materials Science and Engineering C 2007;27(l): 18-22.
[0628] [B55] Hara S et al. Free-standing polypyrrole actuators with response rate of 10.8% s -1. Synthetic Metals 2005; 149(2-3): 199-201.
[0629] [B56] Wang D et al. Spontaneous growth of free-standing polypyrrole films at an air / ionic liquid interface. Langmuir 2010;26(18): 14405-14408.
[0630] [B57] Qi G et al. Highly conductive and semitransparent free-standing polypyrrole films prepared by chemical interfacial polymerization. Journal of Materials Chemistry C 2013;l(42):7102-7110.
[0631] [B58] Jha P et al. Growth of Free-Standing Polypyrrole Nanosheets at Air / Liquid Interface Using J-Aggregate of Porphyrin Derivative as in-Situ Template. Macromolecules 2011;44(12):4583-4585.
[0632] [B59] Jha P et al. Incorporation of non-conjugated polymer chain in conjugated polymer matrix: Anew single step strategy for free standing non-volatile polymer memory. Organic Electronics 2013 ; 14( 11 ) : 2896-2901.[B60] Budi S et al. Specific capacitance and impedance of electrodeposited polyaniline, polypyrrole and polyaniline / polypyrrole composite films. Journal of Physics: Conference Series 2019;1402(6):066015.
[0633] [B61] Newman M, Doan-Nguyen V. Electrochemical Delamination for Free-Standing Polypyrrole Doped with Dodecylbenzenesulfonate Films and the Effect of Substrate. J Electrochem Soc 2024;171(5):055503.
[0634] [B62] Hery T, Sundaresan V-B. Ionic redox transistor from pore-spanning PPy(DBS) membranes. Energy & Environmental Science 2016;9(8):2555-2562.
[0635] [B63] Kudoh Y. Properties of polypyrrole prepared by chemical polymerization using aqueous solution containing Fe2(SO4)3 and anionic surfactant. Synthetic Metals 1996;79(1):17-22.
[0636] [B64] Xu S et al. Homogeneous and Fast Ion Conduction of PEO-Based Solid-State Electrolyte at Low Temperature. Advanced Functional Materials 2020;30(51):2007172.
[0637] [B65] Wang J et al. Synergistic Effects of Plasticizer and 3D Framework toward High-Performance Solid Polymer Electrolyte for Room-Temperature Solid-State Lithium Batteries. ACS Applied Energy Materials 2021 ;4(4) : 4129-4137.
[0638] [B66] Porcarelli L et al. Super Soft All-Ethylene Oxide Polymer Electrolyte for Safe All-Solid Lithium Batteries. Scientific Reports 2016;6(l): 19892.
[0639] [B67] Zhang Y et al. Cross-linking network based on Polyethylene oxide): Solid polymer electrolyte for room temperature lithium battery. Journal of Power Sources 2019;420:63-72.
[0640] [B68] Steyrer B et al. Visible Light Photoinitiator for 3D-Printing of Tough Methacrylate Resins. Materials 2017; 10(12): 1445.
[0641] [B69] Wang K et al. Optimal photoinitiator concentration for light-cured dental resins. Polymer Testing 2021 ; 94 : 107039.
[0642] [B70] Fu F et al. A Dual-Salt PEO-based polymer electrolyte with Cross-Linked polymer network for High-Voltage lithium metal batteries. Chemical Engineering Journal 2022;450: 137776.
[0643] [B71] He R et al. Chemical and electrochemical stability enhancement of lithium bis(oxalato)borate (LiBOB)-modified solid polymer electrolyte membrane in lithium ion halfcells. Electrochimica Acta 2017;246:123-134.
[0644] [B72] Newman M et al. Design and characterization of an adaptive polymer electrolyte for lithium metal solid-state battery applications. J Mater ChemA 2025; 13(11):7914-7928.
[0645] [B73] Cassignol C et al. Microstructure-conductivity relationship in conductingpolypyrrole / epoxy composites. Polymer 1999;40(5): 1139— 1151.
[0646] [B74] Vargas PC et al. Conductive Composites Based on Polyurethane and Nanostructured Conductive Filler of Montmorillonite / Polypyrrole for Electromagnetic Shielding Applications. Mat Res 2018;21(5). doi:10.1590 / 1980-5373-mr-2018-0014.
[0647] [B75] Chanda M. Electrical, Electronic and Optical Properties. In: Science of Engineering Materials. Macmillan Education UK: London, 1980: 61-126.
[0648] [B76] Fielding LA et al. Space science applications for conducting polymer particles: synthetic mimics for cosmic dust and micrometeorites. Chem Commun 2015;51 (95): 16886- 16899.
[0649] [B77] Xue Z, He D, Xie X. Poly(ethylene oxide)-based electrolytes for lithium-ion batteries. J Mater Chem A 2015;3(38): 19218-19253.
[0650] [B78] Ji K-S et al. Role of functional nano-sized inorganic fillers in poly(ethylene) oxide-based polymer electrolytes. Journal of Power Sources 2003; 117(1-2): 124-130.
[0651] [B79] Thakur AK, Hashmi SA. Polymer matrix-filler interaction mechanism for modified ion transport and glass transition temperature in the polymer electrolyte composites. Solid State Ionics 2010; 181(27-28): 1270-1278.
[0652] [B80] Vignarooban K et al. Effect of TiO2 nano-filler and EC plasticizer on electrical and thermal properties of poly(ethylene oxide) (PEO) based solid polymer electrolytes. Solid State Ionics 2014;266:25-28.
[0653] [B81] Lunn BA et al. Determination of the thermal conductivity of polypyrrole over the temperature range 280-335 K. Journal Of Materials Science 1993;28(18):5092-5098.
[0654] [B82] Gilani TH. Evidence for Metal-like Electronic Contribution in Low-Temperature Heat Capacity of Polypyrrole. J Phys Chem B 2005; 109(41): 19204-19207.
[0655] [B83] Albrecht T et al. Dynamics of Surface Crystallization and Melting in Polyethylene and Poly(ethylene oxide) Studied by Temperature-Modulated DSC and HeatWave Spectroscopy. Macromolecules 2001;34(24): 8456-8467.
[0656] [B84] Pielichowski K, Flejtuch K. Phase Behavior of Poly(Ethylene Oxide) Studied by Modulated-Temperature DSC — Influence of the Molecular Weight. Journal of Macromolecular Science, Part B 2004;43(2):459-470.
[0657] [B85] Menard KP, Menard N. Dynamic mechanical analysis. 3rd ed. Taylor and Francis: Boca Raton, 2020 https: / / doi.org / 10.1201 / 9780429190308.
[0658] [B86] Okasinski JS et al. In situ X-ray spatial profiling reveals uneven compression of electrode assemblies and steep lateral gradients in lithium-ion coin cells. Phys Chem Chem Phys 2020;22(38):21977-21987.[B87] Strobridge FC et al. Mapping the Inhomogeneous Electrochemical Reaction Through Porous LiFePO 4 -Electrodes in a Standard Coin Cell Battery. Chem Mater 2015;27(7):2374-2386.
[0659] [B88] Dai F, Cai M. practices in lithium battery cell preparation and evaluation.
[0660] Commun Mater 2022;3(l):64.
[0661] [B89] An Y et al. Progress in Solid Polymer Electrolytes for Lithium-Ion Batteries and Beyond. A7w / / 2O22; I8(3):2IO36I7.
[0662] [B90] Lennartz P et al. Practical considerations for enabling Li|polymer electrolyte batteries. Joule 2023;7(7): 1471-1495.
[0663] [B91] Zhao Q et al. Solid-state polymer electrolytes with in-built fast interfacial transport for secondary lithium batteries. Nat Energy 2019;4(5):365-373.
[0664] [B92] Zhang H et al. Suppressed Mobility of Negative Charges in Polymer Electrolytes with an Ether-Functionalized Anion. Angew Chem Int Ed 2019;58(35): 12070-12075.
[0665] [B93] Lingua G et al. Unique Carbonate-Based Single Ion Conducting Block Copolymers Enabling High-Voltage, All-Solid-State Lithium Metal Batteries. Macromolecules 2021;54(14):6911-6924.
[0666] [B94] Raju MM et al. Crystal Structure and Preparation of Li7La3Zr2O12 (LLZO) Solid-State Electrolyte and Doping Impacts on the Conductivity: An Overview. Electrochem 2021;2(3):390-414.
[0667] [B95] Li Y et al. Densification and ionic-conduction improvement of lithium garnet solid electrolytes by flowing oxygen sintering. Journal of Power Sources 2014;248:642-646.
[0668] [B96] Li X. Reducing Interfacial Resistance in Garnet-Structured Solid-State Lithium-Ion Batteries . 2020. http: / / hdl.handle.net / 1811 / 91644.
[0669] [B97] Sakamoto Y et al. Sintering-free preparation of Li7La3Zr2O12-LiBH4-based solid-state electrolytes and their electrical conductivities. Electrochimica Acta 2023;457: 142488.
[0670] [B98] Shen F et al. A Simple and Highly Efficient Method toward High-Density Garnet-Type LLZTO Solid-State Electrolyte. ACS Appl Mater Interfaces 2020; 12(27): 30313-30319.
[0671] [B99] Weller JM et al. Observation of Elemental Inhomogeneity and Its Impact on Ionic Conductivity in Li-Conducting Garnets Prepared with Different Synthesis Methods. Adv Energy and Sustain Res 2021;2(5):2000109.
[0672] [B100] Wood M et al. Exploring the relationship between solvent-assisted ball milling, particle size, and sintering temperature in garnet-type solid electrolytes. Journal of Power Sources 2021;484:229252.
[0673] [B 101 ] Choi N-S et al. Protective layer with oligo(ethylene glycol) borate anion receptorfor lithium metal electrode stabilization. Electrochem Commun 2004;6(12): 1238-1242.
[0674] [Bl 02] Li S et al. A multifunctional artificial protective layer for producing an ultrastable lithium metal anode in a commercial carbonate electrolyte. J Mater Chem A 2021;9(12):7667-7674.
[0675] [Bl 03] Vijayakumar V et al. In situ polymerization process: an essential design tool for lithium polymer batteries. Energy Environ Sci 2021;14(5):2708-2788.
[0676] [B104] Sun M et al. In-situ Polymerization Methods for Polymer-based Solid-State Lithium Batteries. Batteries & Supercaps 2022;5(12):e202200338.
[0677] [B105] Wang T et al. Dual-Salts Localized High-Concentration Electrolyte for Li- and Mn-Rich High-Voltage Cathodes in Lithium Metal Batteries. Small 2024;20(42):2401364.
[0678] [Bl 06] Quilty CD et al. Probing Sources of Capacity Fade in LiNio.6Mno.2Coo.2O2 (NMC622): An Operando XRD Study of Li / NMC622 Batteries during Extended Cycling. J Phys Chem C 2020;124(15):8119-8128.
[0679] [Bl 07] Longhini M et al. Enabling a non-flammable methyl(2,2,2-trifluoroethyl) carbonate electrolyte in NMC622-graphite Li-ion cells by electrode pre-passivation. Energy Adv 2024;3(5): 1087-1091.
[0680] [Bl 08] Shi Y et al. In-situ cross-linked multifunctional polymer electrolyte buffer layers for high-performance garnet solid-state lithium metal batteries. Journal of Colloid and Interface Science 2023;641:470-478.
[0681] [Bl 09] Zhou W et al. Polymer lithium-garnet interphase for an all-solid-state rechargeable battery. Nano Energy 2018;53:926-931.
[0682] [B110] Wan TH et al. Influence of the Discretization Methods on the Distribution of Relaxation Times Deconvolution: Implementing Radial Basis Functions with DRTtools.
[0683] Electrochimica Acta 2015;184:483-499.
[0684] [Bill] Yu C-Y et al. Time-resolved impedance spectroscopy analysis of aging in sulfide-based all-solid-state battery full-cells using distribution of relaxation times technique. Journal of Power Sources 2024;597:234116.
[0685] [Bl 12] Pan K et al. Comprehensive electrochemical impedance spectroscopy study of Si-Based anodes using distribution of relaxation times analysis. Journal of Power Sources 2020;479:229083.
[0686] [B113] Simon FJ et al. Development of a Wire Reference Electrode for Lithium All-Solid-State Batteries with Polymer Electrolyte: FEM Simulation and Experiment. J Electrochem Soc 2018;165(7):A1363-A1371.
[0687] [Bl 14] Solchenbach S et al. A Gold Micro-Reference Electrode for Impedance andPotential Measurements in Lithium Ion Batteries. J Electrochem Soc 2016; 163(10): A2265-A2272.
[0688] [B 115] Seok J et al. Understanding the Impacts of Li Stripping Overpotentials at the Counter Electrode by Three-Electrode Coin Cell Measurements. Anal Chem 2021;93(46): 15459-15467.
[0689] [B 116] Xu R et al. A Morphologically Stable Li / Electrolyte Interface for All-Solid-State Batteries Enabled by 3D-Micropattemed Garnet. Advanced Materials 2021;33(49):2104009.
[0690] EXEMPLARY ASPECTS
[0691] In view of the described compositions, devices, systems, and methods, herein below are described certain more particularly described aspects of the inventions. The particularly recited aspects should not, however, be interpreted to have any limiting effect on any different claims containing different or more general teachings described herein or that the “particular” aspects are somehow limited in some way other than the inherent meanings of the language and formulas literally used therein.
[0692] Example 1: An adaptive polymer electrolyte comprising: a plurality of conductive polymer particles dispersed throughout a continuous polymer electrolyte matrix; wherein the adaptive polymer electrolyte exhibits an expansion response at room temperature under an applied electric field.
[0693] Example 2: The adaptive polymer electrolyte of any example herein, particularly example 1, wherein the plurality of conductive polymer particles exhibit electrorheological properties under an electric field.
[0694] Example 3 : The adaptive polymer electrolyte of any example herein, particularly example 1 or example 2, wherein the plurality of conductive polymer particles are provided in an amount below the percolation threshold.
[0695] Example 4: The adaptive polymer electrolyte of any example herein, particularly examples 1-3, wherein the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 5 wt.% (relative to the amount of main and additional monomers in the matrix).
[0696] Example 5: The adaptive polymer electrolyte of any example herein, particularly examples 1-4, wherein the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
[0697] Example 6: The adaptive polymer electrolyte of any example herein, particularly examples 1-5, wherein the plurality of conductive polymer particles are provided in an amountof from greater than 0 to 30 vol%, such as from greater than 0 to 15 vol%, of the adaptive polymer electrolyte.
[0698] Example 7: The adaptive polymer electrolyte of any example herein, particularly examples 1-6, wherein the plurality of conductive polymer particles comprise polypyrrole.
[0699] Example 8: The adaptive polymer electrolyte of any example herein, particularly examples 1-7, wherein the plurality of conductive polymer particles comprise polypyrrole doped with a dopant.
[0700] Example 9: The adaptive polymer electrolyte of any example herein, particularly examples 1-8, wherein the plurality of conductive polymer particles ...
Claims
CLAIMSWhat is claimed:
1. An adaptive polymer electrolyte comprising:a plurality of conductive polymer particles dispersed throughout a continuous polymer electrolyte matrix;wherein the adaptive polymer electrolyte exhibits an expansion response at room temperature under an applied electric field.
2. The adaptive polymer electrolyte of claim 1, wherein the plurality of conductive polymer particles exhibit electrorheological properties under an electric field.
3. The adaptive polymer electrolyte of claim 1 or claim 2, wherein the plurality of conductive polymer particles are provided in an amount below the percolation threshold.
4. The adaptive polymer electrolyte of any one of claims 1-3, wherein the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 5 wt.% (relative to the amount of main and additional monomers in the matrix).
5. The adaptive polymer electrolyte of any one of claims 1-4, wherein the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
6. The adaptive polymer electrolyte of any one of claims 1-5, wherein the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 30 vol%, such as from greater than 0 to 15 vol%, of the adaptive polymer electrolyte.
7. The adaptive polymer electrolyte of any one of claims 1-6, wherein the plurality of conductive polymer particles comprise polypyrrole.
8. The adaptive polymer electrolyte of any one of claims 1-7, wherein the plurality of conductive polymer particles comprise polypyrrole doped with a dopant.
9. The adaptive polymer electrolyte of any one of claims 1-8, wherein the plurality of conductive polymer particles comprise polypyrrole doped with dodecylbenzenesulfonate.
10. The adaptive polymer electrolyte of any one of claims 1-9, wherein the plurality of conductive polymer particles comprise polypyrrole doped with dodecylbenzenesulfonate and the plurality of conductive polymer particles are provided in an amount of from greater than 0 to 2 wt.% (relative to the amount of main and additional monomers in the matrix) (e.g., 0.25, 0.5, 1, or 2 wt.%).
11. The adaptive polymer electrolyte of any one of claims 1-10, wherein the continuous polymer electrolyte matrix is derived from a main chain polymer, such as polyethylene oxide (e.g., PEO with a molecular weight of 100,000).
12. The adaptive polymer electrolyte of claim 11, wherein the continuous polymer electrolyte matrix is further derived from a cross-linking monomer, such as tetraethylene glycol dimethacrylate (TEGDMA).
13. The adaptive polymer electrolyte of claim 11 or claim 12, wherein the continuous polymer electrolyte matrix is further derived from one or more salts, such as one or more lithium salts.
14. The adaptive polymer electrolyte of claim 13, wherein the lithium salts comprise lithium bis(trifluoromethane)sulfonamide (LiTFSI), lithium bis(oxalate)borate (LiBoB), or a combination thereof.
15. The adaptive polymer electrolyte of any one of claims 11-14, wherein the continuous polymer electrolyte matrix is further derived from a plasticizer, such as tetraethylene glycol dimethyl ether (TEGDME).
16. The adaptive polymer electrolyte of any one of claims 11-15, wherein the continuous polymer electrolyte matrix is further derived from a photoinitiator, such as a UV-photoinitiator, such as methylbenzophenone (MBP).
17. The adaptive polymer electrolyte of any one of claims 11-16, wherein the continuous polymer electrolyte matrix is derived from:20-40 wt.% (e.g., 30.3 wt.%) main chain polymer (e.g. PEO);10-20 wt.% (e.g., 15.1 wt.%) cross-linking monomer (e.g., TEGDMA);15-25 wt.% (e.g., 21.3 wt.%) Li Salt (e.g., 17.8 wt.% LITFSI and 3.5 wt.% LiBoB); 20-40 wt.% (e.g., 30.3 wt.%) plasticizer (e.g., TEGDME); and1-5 wt.% (e.g., 3.0 wt.%) photoinitiator (e.g., MBP);wherein the sum adds to 100%.
18. The adaptive polymer electrolyte of any one of claims 11-17, wherein the continuous polymer electrolyte matrix is derived from:20-40 wt.% (e.g., 30.3 wt.%) PEO;10-20 wt.% (e.g., 15.1 wt.%) TEGDMA;15-25 wt.% (e.g., 21.3 wt.%) Li Salt (e.g., 17.8 wt.% LITFSI and 3.5 wt.% LiBoB); 20-40 wt.% (e.g., 30.3 wt.%) TEGDME; and1-5 wt.% (e.g., 3.0 wt.%) MBP;wherein the sum adds to 100%.
19. The adaptive polymer electrolyte of any one of claims 11-18, wherein the continuous polymer electrolyte matrix is derived from:30.3 wt.% PEO;15.1 wt.% TEGDMA;17.8 wt.% LITFSI;3.5 wt.% LiBoB;30.3 wt.% TEGDME; and3.0 wt.% MBP.
20. The adaptive polymer electrolyte of any one of claims 1-19, wherein the adaptive polymer electrolyte has an ionic conductivity of from 0.1 to 0.5 mS cm’1, such as 0.1 to 0.25 mS cm’1(e.g., 0.11-0.16 mS cm’1), at 25°C.
21. The adaptive polymer electrolyte of any one of claims 1-20, wherein the adaptive polymer electrolyte exhibits an expansion response of greater than 0% to 10% strain (e.g., 6%) at room temperature and an electric field strength of 0.3 V pm'1.
22. The adaptive polymer electrolyte of any one of claims 1-21, wherein the adaptive polymer electrolyte is a free-standing film.
23. The adaptive polymer electrolyte of any one of claims 1-22, wherein the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 50 micrometers.
24. The adaptive polymer electrolyte of any one of claims 1-23, wherein the adaptive polymer electrolyte has an average thickness of from 50 nanometers to 25 micrometers, such as from 50 nanometers to 10 micrometers or from 50 nanometers to 5 micrometers.
25. The adaptive polymer electrolyte of any one of claims 1-24, wherein the adaptive polymer electrolyte is substantially stable over 5 or more cycles (e.g., 50 or more cycles, or 100 or more cycles).
26. A method of use of the adaptive polymer electrolyte of any one of claims 1-25.
27. The method of claim 26, wherein the method comprises using the adaptive polymer electrolyte as an interlayer between lithium-metal electrode (e.g., Li-metal anode) and solid electrolyte in a lithium metal solid-state battery.
28. An article of manufacture comprising the adaptive polymer electrolyte of any one of claims 1-25.
29. The article of claim 28, wherein the article comprises a lithium metal solid-state battery.
30. A method of making the adaptive polymer electrolyte of any one of claims 1-25.
31. The method of claim 30, wherein the method comprises:combining the continuous polymer electrolyte matrix precursors and the plurality of conductive polymer particles to form a mixture;stirring the mixture for 4 -24 hours (e.g., 8-12 hours or overnight) at room temperature; subsequently ultrasonicating the mixture for 1 minute to 30 minutes (e.g., 10 minutes); subsequently hot pressing the mixture (e.g., 80°C, 4.4 bar, 10 minutes); and subsequently UV-polymerizing the mixture (e.g., 150 mW / cm2, 10 minutes).
32. The method of claim 31, further comprising subsequently vacuum drying the UV-polymerized mixture (e.g., 40°C, overnight).