A manufacturing process of C-shaped sealing ring

Through multi-step processes, including forming, cutting, rolling, welding and stress removal treatment, the problem of C-shaped seal ring manufacturing in high-temperature and high-pressure environments is solved, efficient and automated production is achieved, product quality and consistency is improved, and chemical industry is met Industry working conditions requirements.

CN114559214BActive Publication Date: 2024-11-22WUXI SMART AUTO CONTROL ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210158737.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-21
Publication Date
2024-11-22
Estimated Expiration
2042-02-21

AI Technical Summary

Technical Problem

The prior art is difficult to effectively manufacture C-shaped sealing rings in high temperature and high pressure environments, resulting in leakage of seals in the chemical industry under harsh working conditions and lack of efficient and automated manufacturing equipment.

Method used

Using forming and pressing devices, laser cutting equipment, automatic round rolling devices, laser welding equipment, heat treatment equipment and grinding and polishing equipment, a high-quality C-shaped sealing ring is formed through a multi-step process, including forming, cutting, round rolling, welding, and stress removal. Handle and polish to ensure that the sealing ring size and quality meet the requirements.

Benefits of technology

It realizes the manufacture of efficient and automated C-shaped sealing rings in high temperature and high pressure environments, improves product quality and consistency, reduces manufacturing difficulty and labor intensity, and meets the working conditions requirements of the chemical industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114559214B_ABST
    Figure CN114559214B_ABST
Patent Text Reader

Abstract

The present invention relates to a manufacturing process of a C-shaped sealing ring. The present invention includes forming a blank sheet into a C-shaped cross-section strip profile by a forming and pressing device; cutting the C-shaped cross-section strip profile into a C-shaped cross-section surface material of a preset length by a laser cutting device; rolling by an automatic rolling device; welding the cross-section of a circular C-shaped ring by a laser welding device to form a C-shaped ring; stress relief treatment of the welded C-shaped ring by a heat treatment device; grinding and polishing the circumferential weld of the C-shaped ring after the stress relief treatment by a grinding and polishing device to form a C-shaped sealing ring, and checking whether the roughness and size of the C-shaped sealing ring meet the requirements by a detection device. The present invention can be compatible with the production of C-shaped sealing rings of various specifications at the same time, realize automated production, reduce manufacturing difficulty, and improve production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal sealing rings for control valves, in particular to a manufacturing process of a C-shaped sealing ring. Background Art

[0002] Industrial control valves are indispensable control units in the chemical industry. Sleeve control valves, top-mounted ball valves, and two-way sealed butterfly valves in industrial control valves all have working conditions where C-shaped sealing rings are used. For example, the valve body and valve seat of a top-mounted ball valve are conical self-sealing structures. Usually, the valve seat and valve body seals use graphite, PTFE, etc. as sealing materials, but such materials can only be used in low-temperature or low-pressure working environments. Once there is a high-pressure and high-temperature working environment, the valve body and valve seat seal will fail and leak. Therefore, it is necessary to produce a C-shaped sealing ring that can be used in high-temperature and high-pressure environments as a seal on the back of the valve seat. Ball valves, butterfly valves, and sleeve control valves all have harsh working conditions such as high temperature, high pressure, and high corrosion. The C-shaped metal sealing ring will become an effective replacement for non-metallic seals in the chemical industry due to its excellent and reliable sealing ring performance.

[0003] Therefore, it is urgent to design a C-shaped sealing ring manufacturing equipment with high production efficiency, high degree of automation and guaranteed quality requirements, so as to solve the problems that plague manufacturers in the chemical industry. Summary of the invention

[0004] The object of the present invention is to overcome the above-mentioned shortcomings and thereby provide a device for manufacturing a C-shaped sealing ring, which can meet the size, quality and working condition requirements of the C-shaped sealing ring, reduce the manufacturing difficulty and improve the production efficiency.

[0005] In order to solve the above technical problems, the present invention provides a manufacturing process of a C-shaped sealing ring, comprising the following steps:

[0006] Step S1: forming the blank sheet into a C-shaped cross-section strip profile by a forming and pressing device, wherein the forming and pressing device comprises at least a pair of forming rollers, wherein the forming rollers comprise a concave wheel and a cam, and the concave wheel and the cam cooperate to rotate to drive the blank sheet forward;

[0007] Step S2: cutting the C-shaped cross-section strip into C-shaped cross-section surface materials of a preset length by laser cutting equipment;

[0008] Step S3: rolling the material by an automatic rolling device, the automatic rolling device comprising a first outer roller, a second outer roller, and an inner roller, the first outer roller, the second outer roller, and the inner roller are all concave rollers, the inner roller is arranged below between the first outer roller and the second outer roller, after the compression spring is filled in the C-shaped cavity of the C-shaped cut fabric material, and then the material is rolled in sequence between the first outer roller and the inner roller and between the second outer roller and the inner roller of the automatic rolling device to form a circular C-shaped ring filled with the compression spring;

[0009] Step S4: welding the cross-section of the circular C-shaped ring by laser welding equipment to form a welded C-shaped ring;

[0010] Step S5: performing stress relief treatment on the welded C-shaped ring through a heat treatment device;

[0011] Step S6: grinding and polishing the annular weld of the C-shaped ring after the stress relief treatment by means of a grinding and polishing device to form a C-shaped sealing ring, and inspecting whether the roughness and size of the C-shaped sealing ring meet the requirements by means of a testing device.

[0012] In one embodiment of the present invention, the blank plate is a fixed-width steel strip, using 316 plate with a thickness of 0.8-1 mm.

[0013] In one embodiment of the present invention, the number of the forming rollers is three pairs, and the three pairs of forming rollers are arranged along the same straight line.

[0014] In one embodiment of the present invention, the cutting power of the laser cutting equipment is 1000-1200w.

[0015] In one embodiment of the present invention, the concave shapes of the first outer roller, the second outer roller and the inner roller are arcs.

[0016] In one embodiment of the present invention, the welding power of the laser welding equipment is 500~550W.

[0017] In one embodiment of the present invention, the heat treatment temperature of the heat treatment equipment is 450±14°C, the heating rate is 100-200°C / h, and the holding time is 6-8h.

[0018] In one embodiment of the present invention, in step S6, the grinding and polishing equipment uses a molding grinding wheel for grinding and polishing, and uses 600# molding sand after 200# rough machining and wheel fine machining and polishing.

[0019] In one embodiment of the present invention, the roughness of the ring weld of the C-shaped ring after stress relief treatment is controlled to be less than 0.2 after grinding and polishing.

[0020] In one embodiment of the present invention, in step S6, the detection device implements free measurement through a wireless handheld probe, and detects whether the roughness of the sealing surface meets the requirements through a roughness measuring instrument.

[0021] The above technical solution of the present invention has the following advantages compared with the prior art:

[0022] The manufacturing process of a C-shaped sealing ring described in the present invention can be compatible with the production of C-shaped sealing rings of various specifications, improve product quality and product consistency, and realize automated production; the equipment can meet the size, quality and working condition requirements of the C-shaped sealing ring, reduce manufacturing difficulty, and improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein

[0024] Figure 1 It is a schematic diagram of the overall structure of the manufacturing equipment of the C-shaped sealing ring of the present invention.

[0025] Figure 2 It is a cross-sectional view of the first forming roller, the second forming roller, and the third forming roller.

[0026] Figure 3 This is a schematic diagram of the installation of the first forming roller, the second forming roller, and the third forming roller.

[0027] Figure 4 This is a schematic diagram of the installation of the outer roller and inner roller in the automatic rolling device.

[0028] Explanation of the reference numerals in the drawings in the specification: 1. first forming roller; 1a. first concave wheel; 1b. first cam; 2. second forming roller; 2a. second concave wheel; 2b. second cam; 3. third forming roller; 3a. third concave wheel; 3b. third cam; 3d. forming connecting shaft; 3e. forming bearing; 3f. forming bracket; 4. laser cutting equipment; 5. C-shaped cut surface material; 6. compression spring; 7. automatic rolling device; 7a. first outer roller; 7b. second outer roller; 7c. inner roller; 7d. rolling connecting shaft; 7e. rolling bearing; 7f. rolling bracket; 8. blank sheet material; 9. circular C-shaped ring; 10. laser welding equipment; 11. heat treatment equipment; 12. grinding and polishing equipment; 13. testing equipment. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0030] Reference Figure 1-3 As shown, the present invention provides a manufacturing process of a C-shaped sealing ring, comprising the following steps:

[0031] Step S1: forming the blank sheet 8 into a C-shaped cross-section strip profile by a forming and pressing device, wherein the forming and pressing device comprises at least a pair of forming rollers, wherein the forming rollers comprise a concave wheel and a cam, and the concave wheel and the cam cooperate to rotate to drive the blank sheet 8 forward;

[0032] Step S2: cutting the C-shaped cross-section strip into C-shaped cross-section material 5 of a preset length by laser cutting equipment 4;

[0033] Step S3: Rolling by the automatic rolling device 7, the automatic rolling device 7 comprises a first outer roller 7a, a second outer roller 7b, and an inner roller 7c, the first outer roller 7a, the second outer roller 7b, and the inner roller 7c are all concave rollers, the inner roller 7c is arranged below between the first outer roller 7a and the second outer roller 7b, after the compression spring 6 is filled in the C-shaped cavity of the C-shaped cut surface material 5, and then passes through the first outer roller 7a and the inner roller 7c of the automatic rolling device 7 and the second outer roller 7b and the inner roller 7c to form a round C-shaped ring 9 filled with the compression spring 6;

[0034] Step S4: welding the cross section of the circular C-shaped ring 9 by means of a laser welding device 10 to form a welded C-shaped ring;

[0035] Step S5: performing stress relief treatment on the welded C-shaped ring through a heat treatment device 11;

[0036] Step S6: The annular weld of the C-shaped ring after the stress relief treatment is ground and polished by a grinding and polishing device 12 to form a C-shaped sealing ring, and the roughness and size of the C-shaped sealing ring are checked by a testing device 13 to see if they meet the requirements.

[0037] Specifically, the blank plate 8 is a steel strip of fixed width, and is made of 316 plate with a thickness of 0.8-1 mm. In this embodiment, the thickness is 1 mm.

[0038] Specifically, the number of the forming rollers is three pairs, and the three pairs of forming rollers are arranged along the same straight line. The blank sheet 8 is a steel strip of fixed width; the forming and pressing device includes a first forming roller 1, a second forming roller 2 and a third forming roller 3, the first forming roller 1 includes a first concave wheel 1a and a first cam 1b; the second forming roller includes a second concave wheel 2a and a second cam 2b; the third forming roller 3 includes a third concave wheel 3a and a third cam 3b; the steel strip of fixed width is rolled by the first forming roller 1, the second forming roller 2 and the third forming roller 3 in sequence, and gradually forms a C-shaped ring cross-section shape as shown in the figure. Each concave wheel and cam in the first forming roller 1, the second forming roller 2 and the third forming roller 3 are installed on the forming bracket 3f through their respective forming connecting shafts 3d and forming bearings 3e. The forming and pressing device can select an 8-12 type spiral rib forming machine.

[0039] Specifically, the laser cutting device 4 is a model LB-3015-1500 laser cutting machine, and the cutting power of the laser cutting device is 1000-1200w. In this embodiment, the cutting power is selected to be 1200w. After the fixed-width steel strip is pressed out from the third forming rolling wheel, it is cut into a C-shaped cut surface material 5 by a rear laser cutter. The laser cutting machine can set cutting parameters to fix the cut material size and has a sensor to measure the cut length; the C-shaped cut surface material 5 is transferred by the feeder to the filled compression spring 6 into the outer groove cavity of the C-shaped ring.

[0040] Specifically, the concave shapes of the first outer roller 7a, the second outer roller 7b, and the inner roller 7c are circular arcs. The first outer roller 7a, the second outer roller 7b, and the inner roller 7c are all mounted on the rolling bracket 7f through their respective rolling connecting shafts 7d and rolling bearings 7e. After the compression spring 6 is filled in the C-shaped cavity of the C-shaped cut surface material 5, it can be wrapped and rolled in by the first outer roller 7a, the second outer roller 7b, and the inner roller 7c, and then formed into a circular ring shape by passing between the first outer roller 7a and the inner roller 7c, and between the second outer roller 7b and the inner roller 7c. The outer edge of the C-shaped ring is wrapped and folded into a circular arc to prevent the filled spring from falling out. The automatic rolling device 7 can use the Qingke QK-01 pipe rolling machine.

[0041] Specifically, the model of the laser welding equipment 10 is SUPHW1500+Fanuc M-20iD, and the welding power is 500~550 W. After the ring is rolled and formed, it is sent to the rear laser welding equipment 10 by the feeder. The tooling fixture fixes the ring, and the laser head can swing with the manipulator to weld the weld at the joint of the welding ring.

[0042] Specifically, the heat treatment equipment 11 is a car-type resistance furnace of model DT6-4511, and the ring is fixed with a tooling. The heat treatment temperature of the heat treatment equipment is 450±14°C, the heating rate is 100-200°C / h, and the insulation time is 6-8h. In this embodiment, the heat treatment temperature is set to 450°C, the heating rate is 200°C / h, and the insulation time is 6h.

[0043] Specifically, in step S6, a molding grinding wheel is used for grinding and polishing, and 600# molding sand is used for wheel fine machining and polishing after 200# rough machining, so that the roughness of the ring weld of the C-shaped ring after stress relief treatment is controlled below 0.2 after grinding and polishing.

[0044] Specifically, in step S6, the detection device 13 is a three-dimensional coordinate measuring machine WM-3000, which realizes free measurement through a wireless handheld probe, detects whether the roughness of the sealing surface meets the requirements through a roughness measuring instrument, and outputs a CAD drawing and a test report for archiving and customer acceptance. Through the above settings, the manufacturing equipment of the C-shaped ring can ensure quality, improve work efficiency, reduce labor intensity, and achieve the purpose of automated production.

[0045] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A manufacturing process for a C-shaped sealing ring, characterized in that: The steps include: Step S1: forming the blank sheet into a C-shaped cross-section strip profile by a forming and pressing device, wherein the forming and pressing device comprises at least a pair of forming rollers, wherein the forming rollers comprise a concave wheel and a cam, and the concave wheel and the cam cooperate to rotate to drive the blank sheet forward; Step S2: cutting the C-shaped cross-section strip into C-shaped cross-section surface materials of a preset length by laser cutting equipment; Step S3: rolling the material by an automatic rolling device, the automatic rolling device comprising a first outer roller, a second outer roller, and an inner roller, the first outer roller, the second outer roller, and the inner roller are all concave rollers, the inner roller is arranged below between the first outer roller and the second outer roller, after the compression spring is filled in the C-shaped cavity of the C-shaped cut fabric material, and then the material is rolled in sequence between the first outer roller and the inner roller and between the second outer roller and the inner roller of the automatic rolling device to form a circular C-shaped ring filled with the compression spring; Step S4: welding the cross-section of the circular C-shaped ring by laser welding equipment to form a welded C-shaped ring; Step S5: performing stress relief treatment on the welded C-shaped ring through a heat treatment device; Step S6: grinding and polishing the annular weld of the C-shaped ring after the stress relief treatment by a grinding and polishing device to form a C-shaped sealing ring, and inspecting whether the roughness and size of the C-shaped sealing ring meet the requirements by a testing device; The cutting power of the laser cutting equipment is 1000-1200w; The concave shapes of the first outer roller, the second outer roller and the inner roller are arcs; The welding power of the laser welding equipment is 500~550W; The heat treatment temperature of the heat treatment equipment is 450±14°C, the heating rate is 100-200°C / h, and the holding time is 6-8h; In step S6, the grinding and polishing equipment uses a molding grinding wheel for grinding and polishing, and uses 600# molding sand after 200# rough machining, and the wheel is used for fine machining and polishing; The roughness of the annular weld of the C-shaped ring after stress relief treatment is controlled below 0.2 after grinding and polishing.

2. A manufacturing process for a C-shaped sealing ring according to claim 1, characterized in that: The blank plate is a steel strip of fixed width, using 316 plate, and its thickness is 0.8-1mm.

3. A manufacturing process for a C-shaped sealing ring according to claim 1, characterized in that: The number of the forming rollers is three pairs, and the three pairs of forming rollers are arranged along the same straight line.

4. A manufacturing process for a C-shaped sealing ring as claimed in claim 1, characterized in that: In step S6, the detection device realizes free measurement through a wireless handheld probe, and detects whether the roughness of the sealing surface meets the requirements through a roughness measuring instrument.