Cathode materials and their preparation methods, lithium-ion batteries
By forming a double coating layer of organic lithium salt and graphite-phase carbon nitride on the surface of high-nickel cathode material, the problems of Li/Ni mixing and residual alkali are solved, the structural stability of the material and battery performance are improved, and the production process is simplified.
Patent Information
- Application Number
- CN202210723085.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-24
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-06-24
AI Technical Summary
In existing technologies, high-nickel ternary cathode materials suffer from poor battery cycle life, rate capability, and thermal stability due to Li/Ni mixing and residual alkali on the surface. Furthermore, the multi-stage processing steps are time-consuming and labor-intensive, and the water washing process increases costs and reduces electrode performance.
A double coating layer is formed on the surface of a high-nickel cathode material, consisting of a first coating layer of organic lithium salt and a second coating layer of graphitic carbon nitride. This is achieved by heat treatment of a polymer solution in an oxygen-containing atmosphere, which simplifies the process and improves the stability of the material.
It improves the structural stability and charge transfer efficiency of high-nickel materials, reduces impedance, enhances coulombic efficiency and rate performance, avoids side reactions, and simplifies the production process.
Smart Images

Figure CN114937771B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to a cathode material and its preparation method, and a lithium-ion battery. Background Technology
[0002] Lithium-ion batteries are now the primary power source for portable electronic devices and are increasingly being used in electric vehicles and other large-scale applications due to their high energy density and long lifespan.
[0003] Cathode materials are key materials in lithium-ion batteries, exhibiting high differentiation, accounting for a significant portion of cost, and crucial to performance. Currently, the main cathode materials on the market are lithium cobalt oxide, lithium iron phosphate, and ternary cathode materials. Lithium cobalt oxide, as the first generation of commercially available lithium battery cathode materials, boasts advantages such as high tap density, stable charge and discharge, and high operating voltage, making it widely used in small batteries. However, lithium cobalt oxide is expensive and has poor cycle life and safety. Lithium iron phosphate is cheaper, more environmentally friendly, and offers better safety and high-temperature performance, making it a popular cathode material in the electric vehicle industry. However, it has lower energy density and poorer low-temperature performance. Ternary cathode materials are the next-generation upgrade of lithium iron phosphate, combining the advantages of lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide. They exhibit a significant synergistic effect, resulting in higher energy density, but also higher cost and stricter safety requirements.
[0004] Ternary cathode materials vary in capacity and cost depending on the nickel, cobalt, and manganese content, but their overall energy density is higher than that of lithium iron phosphate and lithium cobalt oxide. In ternary cathode materials, nickel is primarily used to improve battery energy density, manganese plays a stabilizing role in the structure, and cobalt can both stabilize the layered structure of the material and reduce cation mixing, which is beneficial to battery cycle performance. However, cobalt is the most expensive. Therefore, to reduce costs while increasing battery energy density, gradually increasing the nickel content is the trend in the development of ternary cathode materials. Medium-nickel ternary cathode materials (nickel ratio ≤ 5, such as NCM111 and NCM523 (N represents Ni, C represents Co, M represents Mn, and 523 represents the ratio of Ni, Co, and Mn respectively) and high-nickel ternary cathode materials (nickel ratio ≥ 6, such as NCM811 and NCM622) have emerged. High-nickel ternary cathode materials have high specific capacity and energy density, making them one of the most promising cathode materials.
[0005] However, due to Ni 2+ and Li + With similar radii, as the nickel content increases, the Ni content in high-nickel ternary cathode materials... 2+ Some of these substances will migrate into the Li layer, leading to severe Li / Ni mixing and increased surface residual alkali (LiOH, Li2CO3, etc.), which in turn worsens the battery's cycle life, rate capability, and thermal stability, and may induce gas bulging and other safety hazards.
[0006] Existing technologies primarily address the severe Li / Ni mixing problem in high-nickel ternary cathode materials through micro-size design and elemental doping coating, while also incorporating post-treatment processes such as water washing to reduce surface residual alkali. However, these multi-stage processing steps are not only time-consuming and labor-intensive, increasing production costs, but the water washing process also makes the surface of the high-nickel ternary cathode material more susceptible to side reactions and increases impedance, thereby reducing the electrode's reversible capacity, cycle life, and rate performance. Summary of the Invention
[0007] The purpose of this invention is to overcome the above-mentioned defects in the prior art and provide a cathode material and its preparation method, as well as a lithium-ion battery. This cathode material can improve the structural stability of the cathode material, promote the improvement of cycle performance, and promote the charge transfer process, reduce impedance, thereby improving coulombic efficiency and rate performance.
[0008] To achieve the above objectives, the technical solution of the present invention is as follows:
[0009] A cathode material includes a high-nickel cathode material and a coating layer formed on at least a portion of the surface of the high-nickel cathode material; the coating layer includes a first coating layer and a second coating layer located on the surface of the first coating layer, the first coating layer including an organolithium salt and the second coating layer including graphitic carbon nitride.
[0010] This invention also discloses a method for preparing the above-mentioned cathode material, comprising the following steps:
[0011] A polymer solution is obtained by mixing a mixture containing nitrogen-containing organic matter, acidic organic matter, and a solvent.
[0012] The polymer solution is mixed with a high-nickel cathode material and then coated to obtain a polymer-coated high-nickel cathode material; and
[0013] The polymer-coated high-nickel cathode material is subjected to heat treatment in an oxygen-containing atmosphere to obtain a cathode material; the cathode material includes a high-nickel cathode material and a coating layer formed on at least a portion of the surface of the high-nickel cathode material; the coating layer includes a first coating layer and a second coating layer located on the surface of the first coating layer, the first coating layer includes an organolithium salt, and the second coating layer includes graphitic carbon nitride.
[0014] The present invention also discloses a lithium-ion battery, comprising the above-described positive electrode material or the positive electrode material prepared by the above-described preparation method.
[0015] Implementing the embodiments of the present invention will have the following beneficial effects:
[0016] First, in this embodiment, the cathode material has a first coating layer formed on the surface of a high-nickel cathode material. This first coating layer includes an organolithium salt, and a second coating layer formed on the surface of the first coating layer. This second coating layer includes graphitic carbon nitride. The combined effect of the two coating layers improves the structural stability of the high-nickel material and promotes improved cycle performance. Specifically, the graphitic carbon nitride (g-C3N4) in the second coating layer forms a metallic Li-N / Ni-N highly conductive interface between the first coating layer containing the organolithium salt and the high-nickel cathode material. This facilitates charge transfer, reduces impedance, and improves the coulombic efficiency and rate performance of the high-nickel material. This cathode material with two coating layers reduces residual alkali and overcomes the problems of high impedance and irreversible capacity decay caused by residual alkali. Furthermore, it significantly improves the conductivity of the coating layers.
[0017] Secondly, this embodiment uses a polymer solution to provide the acidic organic compound. In the polymer solution, the acidic functional groups in the acidic organic compound act as electron acceptors, and the nitrogen atoms in the nitrogen-containing organic compound act as electron donors. The acidic organic compound and the nitrogen-containing organic compound reversibly polymerize to form a supramolecular polymer through intermolecular interactions (such as hydrogen bonds, host-guest interactions, charge transfer interactions, and π-π interactions). Since the polymerization reaction to form the supramolecular polymer is a reversible polymerization reaction, the monomers in the supramolecular polymer still retain their original functional roles. Due to the influence of the electron donors, the acidity of the acidic organic compound is greatly reduced. Because of the reduced acidity, the acidic organic compound not only effectively dissolves residual alkali but also avoids corrosion of the high-nickel cathode material. In addition, because the acidity of the acidic organic compound is reduced, the amount of solvent used can also be significantly reduced. When the solvent contains water, the amount of water used can be significantly reduced, avoiding the occurrence of side reactions on the surface of the high-nickel cathode material caused by a large amount of water, which generates NiOOH-like phase impurities, leading to increased internal resistance of the material and severe degradation of battery performance.
[0018] Third, this embodiment achieves one-step removal of surface residual alkali and in-situ generation of an organic lithium salt first coating layer and a graphite phase carbon nitride second coating layer on the surface of the high-nickel cathode material. The entire process has the advantages of being simple and easy to promote, having low energy consumption, short production cycle, and good product quality. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] in:
[0021] Figure 1This is a flowchart of a method for preparing a positive electrode material according to a specific embodiment of the present invention.
[0022] Figure 2 This is a high-magnification SEM image of the cathode material prepared in Example 1.
[0023] Figure 3 This is a high-magnification TEM image of the cathode material prepared in Example 1.
[0024] Figure 4 The high-resolution Ni alloys are the cathode material prepared in Example 1 and the salt-coated cathode material prepared in Comparative Example 3. 2p Spectrum and N 1s Spectrum.
[0025] Figure 5 These are high-resolution N1s spectra of the cathode material prepared in Example 1 and the g-C3N4-coated cathode material prepared in Comparative Example 2.
[0026] Figure 6 These are the electrochemical impedance spectroscopy spectra of the biphase layer coated cathode material prepared in Example 1, the g-C3N4 coated cathode material prepared in Comparative Example 2, and the salt coated cathode material prepared in Comparative Example 3.
[0027] Figure 7 This is a graph showing the capacity retention rate of the cathode material prepared in Example 1 after 100 cycles at 25°C and 55°C. Detailed Implementation
[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] One embodiment of the cathode material addresses the problems of deteriorated cycle life, rate capability, reversible capacity, and thermal stability in high-nickel cathode materials caused by Li / Ni mixing and residual alkalis (LiOH, Li2CO3, etc.) on the surface. Specifically, the cathode material of the present invention includes a high-nickel cathode material and a coating layer formed on at least a portion of the surface of the high-nickel cathode material; the coating layer includes a first coating layer and a second coating layer located on the surface of the first coating layer, the first coating layer comprising an organolithium salt, and the second coating layer comprising graphitic carbon nitride.
[0030] This embodiment forms a first coating layer containing an organolithium salt and a second coating layer containing graphitic carbon nitride. The combined effect of the first and second coating layers improves the structural stability of the high-nickel material and promotes enhanced cycle performance. Specifically, the graphitic carbon nitride (g-C3N4) in the second coating layer forms a metallic Li-N / Ni-N highly conductive interface between the first coating layer containing the organolithium salt and the high-nickel cathode material, which promotes charge transfer, reduces impedance, and improves the coulombic efficiency and rate performance of the high-nickel material. This cathode material with dual coating layers reduces residual alkali and overcomes the problems of high impedance and irreversible capacity decay caused by residual alkali, while significantly improving the conductivity of the coating layers.
[0031] In some embodiments, the chemical formula of the high-nickel cathode material can be LiNi. x Co y M (1x y) O2, where 0.6 < x < 1.0, 0 < y < 0.2, and M includes at least one of Mn and Al; of course, high-nickel cathode materials may also contain a small number of other doped atoms, such as Zr atoms.
[0032] Specifically, the value of x can be 0.65, 0.7, 0.76, 0.8, 0.83, 0.85, 0.88, 0.9, 0.92, 0.94, or 0.97, etc., and the value of y can be 0.01, 0.02, 0.03, 0.05, 0.08, 0.10, 0.12, 0.15, 0.17, or 0.18, etc., without any restrictions here.
[0033] In some embodiments, the thickness of the first coating layer is 1 nm to 5 nm. Specifically, the thickness of the first coating layer can be 1 nm, 1.5 nm, 2 nm, 2.3 nm, 2.5 nm, 3 nm, 3.5 nm, 4.5 nm, or 5 nm.
[0034] In some embodiments, the thickness of the second coating layer is 5 nm to 20 nm, which can provide better cycling, rate, coulombic efficiency, thermal stability and mechanical strength properties of the high-nickel cathode material. Specifically, the thickness of the second coating layer can be 5 nm, 6.5 nm, 7.5 nm, 10 nm, 12 nm, 15 nm, 17 nm, 18.5 nm or 20 nm.
[0035] In some embodiments, the organolithium salt contains acidic groups; the acidic functional groups in the acidic organic compounds of the organolithium salt act as electron acceptors, and the nitrogen atoms in the nitrogen-containing organic compounds act as electron donors. The acidic organic compounds and the nitrogen-containing organic compounds reversibly polymerize through intermolecular interactions (e.g., hydrogen bonds, host-guest interactions, charge transfer interactions, and π-π interactions) to form a polymer. Since the polymerization reaction that forms the supramolecular polymer is reversible, the monomers in the supramolecular polymer retain their original functional roles. Due to the influence of the electron donors, the acidity of the acidic organic compounds is greatly reduced. Because of this reduced acidity, the acidic organic compounds not only effectively dissolve residual alkali but also prevent corrosion of the high-nickel cathode material. Furthermore, since the acidity of the acidic organic matter is reduced, the amount of solvent used can be significantly reduced. When the solvent contains water, the amount of water used can be significantly reduced, avoiding the occurrence of side reactions on the surface of the high-nickel cathode material caused by a large amount of water, generating NiOOH-like phase impurities, which leads to increased internal resistance of the material and severe degradation of battery performance. Moreover, this organic lithium salt can form a metallic Li-N / Ni-N highly conductive interface with graphitic carbon nitride (g-C3N4) and the high-nickel cathode material, which can promote the charge transfer process, reduce impedance, and improve the coulombic efficiency and rate performance of the high-nickel material.
[0036] In some embodiments, the acidic groups include at least one of phosphate groups, carboxylic acid groups, and imide groups. The inventors have found that the organic lithium salts using the above-mentioned acidic groups can better form a metallic Li-N / Ni-N highly conductive interface with the graphitic carbon nitride (g-C3N4) of the second coating layer and the high-nickel cathode material, which can promote the charge transfer process, reduce impedance, improve the coulombic efficiency and rate performance of the high-nickel material, and is more conducive to improving the structural stability of the high-nickel material.
[0037] In some embodiments, the organolithium salt containing a phosphate group includes at least one of lithium phytate, lithium diphenyl phosphate, and lithium glycerophosphate.
[0038] In some embodiments, the organolithium salt containing a carboxylic acid group includes at least one of lithium phenylacetate, lithium ethylenediaminetetraacetate, and lithium barbiturate.
[0039] In some embodiments, the organolithium salt containing an imide group includes lithium phthalimide, lithium butyromide, and lithium maleimide.
[0040] The inventors have discovered that, compared to other organic lithium salts, the use of the aforementioned types of organic lithium salts is more conducive to promoting the charge transfer process, reducing impedance, improving the coulombic efficiency and rate performance of high-nickel materials, and is also more beneficial to improving the structural stability of high-nickel materials.
[0041] In some embodiments, the mass ratio of the organolithium salt to graphitic carbon nitride is 0.1 to 1:1. Within this mass ratio range, the graphitic carbon nitride in the second coating layer can better form metallic Li-N / Ni-N bonds with the organolithium salt in the first coating layer and the high-nickel cathode material, greatly improving the electron transport rate. When the mass ratio is less than 0.1, almost only a single layer of graphitic carbon nitride is formed on the surface of the high-nickel cathode material, which is not conducive to improving the stability of the cathode material. When the mass ratio is greater than 1, the first coating layer of organolithium salt formed on the surface of the high-nickel cathode material is too thick, which is not conducive to the formation of highly conductive Ni-N bonds between the graphitic carbon nitride in the second coating layer and the high-nickel cathode material. Specifically, the mass ratio of the organolithium salt to graphitic carbon nitride can be 0.1:1, 0.25:1, 0.5:1, 0.6:1, 0.75:1, 0.8:1, or 1:1.
[0042] In some embodiments, the morphology of the cathode material can be one or more of the following: agglomerated secondary particles, single-crystal particles, and large particles of quasi-single-crystal type. The aforementioned particles can be of any shape, such as spherical or quasi-spherical.
[0043] In some embodiments, the average particle size of the cathode material is 5 μm to 30 μm. Specifically, the particle size of the cathode material can be 5 μm, 6.5 μm, 7.5 μm, 10 μm, 12 μm, 15 μm, 17 μm, 18.5 μm, 20 μm, 22 μm, 23 μm, 25 μm, or 30 μm.
[0044] In one specific embodiment, the high-nickel cathode material adopts spherical agglomerate secondary particles with a particle size of 5μm to 30μm.
[0045] In some embodiments, the cathode material exhibits characteristic peaks representing Ni-N binding energy at 852.0–855.5 eV and 396.2–398.5 eV in the Ni2p XPS and N1s XPS spectra, and characteristic peaks representing Li-N binding energy at 398.6–400.5 eV in the N1s XPS spectra. This indicates that graphitic carbon nitride forms a metallic Li-N / Ni-N highly conductive interface between the first coating layer and the high-nickel cathode material, respectively, which promotes the charge transfer process and improves the coulombic efficiency and rate performance of the high-nickel cathode material. The reason why a metallic Ni-N / Li-N highly conductive interface can be formed between the first organic lithium salt coating layer and the high-nickel cathode material is that the high-nickel cathode material is coated and modified with a polymer solution containing acidic organic matter and nitrogen-containing organic matter. Since the acidic organic matter and nitrogen-containing organic matter are uniformly dispersed in the polymer solution, they are also uniformly distributed in the initial coating layer. Then, the first organic lithium salt coating layer and the second graphite phase carbon nitride coating layer are generated sequentially through in-situ reaction, so that Ni-N / Li-N bonds can be formed between the first organic lithium salt coating layer and the high-nickel cathode material.
[0046] In some embodiments, the residual alkali content of the cathode material is 100ppm to 2000ppm.
[0047] In some embodiments, the charge transfer resistance of the positive electrode material is less than 40Ω; specifically, the charge transfer resistance can be 20Ω, 22Ω, 25Ω, 28Ω, 30Ω, 32Ω, 36Ω, etc.
[0048] In some embodiments, the specific surface area of the positive electrode material is 1m². 2 / g~3m 2 / g. Specifically, the specific surface area of the cathode material is 1m². 2 / g, 1.2m 2 / g, 1.5m 2 / g、2m 2 / g, 2.5m 2 / g or 3m 2 / g.
[0049] refer to Figure 1 Another embodiment of the above-mentioned cathode material preparation method includes the following steps:
[0050] Step S1: Mix the mixture containing nitrogen-containing organic matter, acidic organic matter, and solvent to obtain a polymer solution.
[0051] In this embodiment, nitrogen-containing organic compounds and acidic organic compounds can form polymer solutions in solvents through intermolecular interactions (such as hydrogen bonds, host-guest interactions, charge transfer interactions, π-π interactions, etc.); host-guest interactions refer to selective binding through non-covalent interactions.
[0052] In some embodiments, acidic organic compounds include organic compounds containing acidic functional groups; specifically, the acidic functional groups may include at least one of phosphate groups, carboxylic acid groups, and imide groups.
[0053] In some embodiments, the acidic organic compound containing a phosphate group includes at least one of phytic acid, lithium diphenyl phosphate, and glycerophosphate.
[0054] In some embodiments, the acidic organic compound containing a carboxylic acid group includes at least one of phenylacetic acid, ethylenediaminetetraacetic acid, and barbituric acid.
[0055] In some embodiments, the acidic organic compound containing an imide group includes at least one of phthalimide, butyramide, and maleimide.
[0056] In some embodiments, nitrogen-containing organic compounds can undergo a polymerization reaction upon heating to generate graphitic carbon nitride. Specifically, in one embodiment, the nitrogen-containing organic compound may include melamine. formamide 1,3-Dimethylurea N,N-dimethylurea Aminourea Cucurbita And at least one of the derivatives of any of the above-mentioned organic compounds.
[0057] In some embodiments, the solvent may include at least one selected from water, ethanol, ethylene glycol, methanol, acetone, and N,N-dimethylformamide. A polar organic solvent is preferred, and water is avoided because it can lead to increased side reactions and surface structure remodeling on the surface of the high-nickel cathode material. In this invention, when the solvent includes water, a relatively small amount of water can be used to dissolve nitrogen-containing organic compounds and acidic organic compounds, thereby minimizing the side reactions and surface structure remodeling problems caused by water on the high-nickel cathode material.
[0058] In this embodiment, the acidic functional groups in the acidic organic compound act as electron acceptors, and the nitrogen atoms in the nitrogen-containing organic compound act as electron donors. The acidic organic compound and the nitrogen-containing organic compound reversibly polymerize to form a supramolecular polymer through intermolecular interactions (e.g., hydrogen bonds, host-guest interactions, charge transfer interactions, and π-π interactions). Since the polymerization reaction to form the supramolecular polymer is reversible, the monomers in the supramolecular polymer retain their original functional roles. Due to the influence of the electron donors, the acidity of the acidic organic compound is greatly reduced. This reduced acidity not only effectively dissolves residual alkali but also prevents corrosion of the high-nickel cathode material. Furthermore, the reduced acidity of the acidic organic compound significantly reduces the amount of solvent used. When the solvent contains water, the amount of water used can be significantly reduced, preventing large amounts of water from triggering side reactions on the surface of the high-nickel cathode material, generating NiOOH-like impurities, which would lead to increased internal resistance and severe performance degradation of the battery.
[0059] In some embodiments, the total mass of nitrogen-containing organic matter and acidic organic matter in the polymer solution can account for 20% to 50% of the mass of the solvent. Specifically, the total mass of nitrogen-containing organic matter and acidic organic matter can account for 20%, 22%, 25%, 30%, 35%, 40%, 45%, 46%, or 50% of the mass of the solvent.
[0060] In this invention, the acidic organic matter in the supramolecular polymer is used to dissolve the residual alkali (LiOH, Li2CO3, etc.) on the surface of the high-nickel cathode material and generate an organic lithium salt first coating layer covering the high-nickel cathode material; the nitrogen-containing organic matter in the supramolecular polymer is used to generate a graphitic carbon nitride (g-C3N4) second coating layer on the surface of the organic lithium salt first coating layer through a thermal polymerization reaction.
[0061] In some embodiments, the pH value of the polymer solution is 4-7. Specifically, the pH of the supramolecular polymer solution can be adjusted to 4-7 by adjusting the molar ratio of nitrogen-containing organic matter to acidic organic matter. Excessive acidity can easily corrode high-nickel cathode materials. Experimental data from this invention demonstrates that adjusting the pH of the supramolecular polymer solution to 4-7 can reduce the residual alkali content on the surface of the high-nickel cathode material to as low as 100ppm-2000ppm, significantly lower than that of existing technologies. This invention adjusts the pH value by adjusting the amount of acidic organic matter, unlike existing technologies that adjust the pH value by increasing the amount of water solvent to dilute the acid solution. This avoids the limitations of existing technologies that require changing the solution volume to adjust the pH value when using acid solutions to remove residual alkali, and also avoids problems such as increased side reactions and surface structure remodeling in high-nickel cathode materials due to adding too much water solvent to dilute the acid solution.
[0062] In some embodiments, the molar ratio of nitrogen-containing organic matter to acidic organic matter can be 0.5 to 4:1, which can effectively remove residual alkali and generate an organic lithium salt first coating layer and a graphite-phase carbon nitride second coating layer of appropriate thickness, respectively, providing the high-nickel cathode material with superior cycle life, rate capability, coulombic efficiency, and thermal stability. Specifically, the molar ratio of nitrogen-containing organic matter to acidic organic matter can be 0.5:1, 0.8:1, 1:1, 1.5:1, 2.1:1, 2.2:1, 2.5:1, 2.8:1, 3.2:1, or 4:1.
[0063] In some embodiments, the nitrogen-containing organic compounds and acidic organic compounds can be uniformly dispersed in a solvent by methods such as stirring or ultrasonic dispersion. The preferred temperature for the mixing and polymerization of the acidic organic compounds and nitrogen-containing organic compounds is 10°C to 120°C. Specifically, the temperature can be 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, or 120°C.
[0064] In some embodiments, the polymerization time of the mixture of acidic organic matter and nitrogen-containing organic matter is 2h to 48h.
[0065] In some embodiments, the stirring speed for mixing nitrogen-containing organic matter and acidic organic matter is 200 rpm to 1000 rpm.
[0066] In some embodiments, the stirring time for mixing nitrogen-containing organic matter and acidic organic matter is 2h to 48h.
[0067] In some embodiments, nitrogen-containing organic compounds and acidic organic compounds can be dispersed in a solvent to obtain a mixed solution. The mixed solution is then placed at a temperature of 10°C to 120°C and stirred at a stirring speed of 200 rpm to 1000 rpm for 2 h to 48 h. The acidic organic compounds and nitrogen-containing organic compounds polymerize to form a supramolecular polymer, resulting in a supramolecular polymer solution.
[0068] Step S2: The polymer solution is mixed with the high-nickel cathode material and coated to obtain a polymer-coated high-nickel cathode material. The acidic organic matter in the polymer dissolves the residual alkali (LiOH, Li2CO3, etc.) on the surface of the high-nickel cathode material and generates an organic lithium salt first coating layer that coats the high-nickel cathode material.
[0069] In some embodiments, the mass of the polymer solution is 5% to 15% of the mass of the high-nickel cathode material. Specifically, the mass of the polymer solution is 5%, 7%, 8.5%, 10%, 10.5%, 12%, 13.5%, or 15% of the mass of the high-nickel cathode material.
[0070] In some embodiments, the polymer solution is stirred and mixed with a high-nickel cathode material.
[0071] In some embodiments, the stirring time is 20 min to 40 min.
[0072] In some embodiments, the stirring speed is 500 rpm to 800 rpm.
[0073] In this step, the dissolution of residual alkali can be carried out at room temperature, or the mixture coated in step S2 can be heated to accelerate the dissolution rate. The temperature for dissolving residual alkali can be 10℃ to 120℃. Alternatively, the polymer solution can be heated first, and then the high-nickel cathode material can be added to the heated polymer solution.
[0074] Step S3: The polymer-coated high-nickel cathode material is heat-treated in an oxygen-containing atmosphere to obtain the cathode material.
[0075] The nitrogen-containing organic matter in the polymer undergoes a thermal polymerization reaction to form a second coating layer of graphite-phase carbon nitride on the surface of the first coating layer of the organolithium salt, thereby obtaining a cathode material. The cathode material includes a high-nickel cathode material and a coating layer formed on at least a portion of the surface of the high-nickel cathode material. The coating layer includes a first coating layer and a second coating layer located on the surface of the first coating layer. The first coating layer includes an organolithium salt, and the second coating layer includes graphite-phase carbon nitride.
[0076] In some embodiments, the heating rate of the heat treatment is 2°C / min to 10°C / min. Specifically, the heating rate can be 2°C / min, 2.5°C / min, 3.5°C / min, 5°C / min, 6.5°C / min, 7.8°C / min, or 10°C / min.
[0077] In some embodiments, the heat treatment temperature is 400°C to 600°C. Specifically, the heat treatment temperature is 400°C, 450°C, 480°C, 500°C, 530°C, 550°C, 580°C, or 600°C.
[0078] In some embodiments, the heat treatment time is 2h to 8h. Specifically, the heat treatment time can be 2h, 3h, 3.5h, 4h, 4.5h, 6h, 7.2h, 7.5h, 7.6h or 8h.
[0079] In some embodiments, the oxygen-containing atmosphere includes oxygen with a volume percentage of less than 25% and greater than 1%, i.e., the oxygen-containing atmosphere is a low-oxygen atmosphere. Adding a small amount of oxygen can further reduce Li / Ni mixing. If the oxygen content is too high, it can easily lead to the oxidation and combustion of organic compounds in the polymer.
[0080] Specifically, the oxygen-containing atmosphere can be dehydrated and decarbonized air (abbreviated as PSA atmosphere), or a mixture of oxygen and inert gases, etc.
[0081] The graphitic carbon nitride obtained in this heat treatment step is formed through in-situ thermal polymerization. Therefore, the graphitic carbon nitride has stronger atomic bonding with the high-nickel cathode material. Experiments show that the modified cathode material of this invention has characteristic peaks representing Ni-N binding energy at 852.0–855.5 eV and 396.2–398.5 eV in the Ni 2p XPS and N 1s XPS spectra, and characteristic peaks representing Li-N binding energy at 398.6–400.5 eV in the N 1s XPS spectrum. This indicates that the graphitic carbon nitride forms a metallic Li-N / Ni-N highly conductive interface between the first organic lithium salt coating layer and the high-nickel cathode material, promoting the charge transfer process and improving the coulombic efficiency and rate performance of the high-nickel cathode material. Furthermore, graphitic carbon nitride is also a two-dimensional layered structure material with high stability and high mechanical strength, which can greatly improve the thermal stability and cycle performance of the high-nickel cathode material.
[0082] In summary, this invention employs a one-step process, using gradient heating to remove residual alkali in one step and generate a biphase organic lithium salt first coating layer and a graphite-phase carbon nitride second coating layer in situ on the surface of the high-nickel cathode material. This not only simplifies the surface treatment process of the high-nickel cathode material and avoids the multi-stage processing steps of existing technologies, but also improves the cycle life, rate capability, coulombic efficiency, thermal stability, and mechanical strength of the high-nickel cathode material. It also avoids the problems of surface instability, increased impedance, and capacity decay of high-nickel cathode materials caused by the water washing process in existing technologies.
[0083] The organic lithium salt in the cathode material prepared by the above method is obtained by the acid-base reaction between the acidic organic matter in the polymer and the residual alkali. Specifically, the organic lithium salt may include one or more of lithium phytate, lithium phenylacetate, lithium ethylenediaminetetraacetate and lithium barbiturate. The organic lithium salt formed by dissolving the residual alkali (LiOH, Li2CO3, etc.) overcomes the problems of high impedance and irreversible capacity decay caused by the residual alkali.
[0084] The graphitic carbon nitride in the cathode material prepared by the above method is formed by in-situ conversion of nitrogen-containing organic matter in the polymer through heat treatment of the polymer-coated high-nickel cathode material. The graphitic carbon nitride formed forms a metallic Li-N / Ni-N highly conductive interface between the first organic lithium salt coating layer and the high-nickel cathode material, which promotes the charge transfer process and improves the coulombic efficiency and rate performance of the high-nickel cathode material.
[0085] The present invention also provides a lithium-ion battery comprising the above-described positive electrode material or the positive electrode material prepared by the above-described preparation method.
[0086] The following is a specific embodiment. (The room temperature in this embodiment refers to 25°C.)
[0087] Example 1
[0088] A method for preparing a cathode material includes the following steps:
[0089] 1) Melamine and phytic acid were dissolved in ethylene glycol at a molar ratio of 2:1 at room temperature and stirred at 350 rpm for 24 h. A white melamine-phytic acid supramolecular polymer solution was formed under the interaction of hydrogen bonding and charge transfer, with a pH value of 5. The mass of the melamine-phytic acid supramolecular polymer accounted for 30 wt% of the ethylene glycol solution.
[0090] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e. NCM811) and the supramolecular polymer solution obtained in step 1) are placed in a reactor and stirred and mixed. The amount of supramolecular polymer solution added accounts for 10 wt% of the mass of the high-nickel cathode material. The stirring time is 20 min and the stirring speed is 500 rpm.
[0091] 3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 550°C at a heating rate of 2°C / min and held at that temperature for 2 hours. After the reaction was completed, the positive electrode material was obtained.
[0092] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate and the second coating layer includes graphitic carbon nitride; the thickness of the first coating layer is 4 nm and the thickness of the second coating layer is 10 nm, the mass ratio of lithium phytate to graphitic carbon nitride is 0.45:1; the average particle size of the cathode material is 15 μm, denoted as biphase layer coated NCM.
[0093] Example 2
[0094] A method for preparing a cathode material includes the following steps:
[0095] 1) Melamine and phenylacetic acid were dissolved in ethylene glycol at a molar ratio of 3:1 at room temperature and stirred at 350 rpm for 36 h. A melamine-phenylacetic acid supramolecular polymer solution was formed under hydrogen bonding and π-π interaction. The pH value was 6.5 and the mass of the melamine-phenylacetic acid supramolecular polymer accounted for 25 wt% of the ethylene glycol solution.
[0096] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 20 μm.0.6 Co 0.2 Mn 0.2 O2 (i.e. NCM622) and melamine-phenylacetic acid supramolecular polymer solution were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 30 min and the stirring speed was 550 rpm.
[0097] 3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 580°C at a heating rate of 2°C / min and held at that temperature for 4 hours. After the reaction was completed, the positive electrode material was obtained.
[0098] Cathode materials include LiNi 0.6 Co 0.2 Mn 0.2 O2 and coated LiNi 0.6 Co 0.2 Mn 0.2 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phenylacetate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 3.5 nm, the thickness of the second coating layer is 10 nm, the mass ratio of lithium phenylacetate to graphitic carbon nitride is 0.4:1, and the average particle size of the cathode material is 20 μm.
[0099] Example 3
[0100] A method for preparing a cathode material includes the following steps:
[0101] 1) N,N-dimethylurea and barbituric acid were dissolved in water at a molar ratio of 2:1 at room temperature. The solution was heated to 120°C in a reaction vessel and stirred at 400 rpm for 6 hours. Under the action of hydrogen bonding and charge transfer, an N,N-dimethylurea-barbituric acid supramolecular polymer solution was formed with a pH of 5.5. The mass of the N,N-dimethylurea-barbituric acid supramolecular polymer accounted for 20 wt% of the aqueous solution.
[0102] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e., NCM811) and the N,N-dimethylurea-barbituric acid supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 15 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 550 rpm.
[0103] 3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 500°C at a heating rate of 5°C / min and held at that temperature for 3 hours. After the reaction was completed, the positive electrode material was obtained.
[0104] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium barbiturate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 3nm, the thickness of the second coating layer is 9nm, the mass ratio of lithium barbiturate to graphitic carbon nitride is 0.35:1, and the average particle size of the cathode material is 15μm.
[0105] Example 4
[0106] A method for preparing a cathode material includes the following steps:
[0107] 1) At room temperature, formamide and ethylenediaminetetraacetic acid were dissolved in water at a molar ratio of 1:1. The solution was heated to 120°C in a reaction vessel and stirred at 500 rpm for 4 hours. A formamide-ethylenediaminetetraacetic acid supramolecular polymer solution was formed under the action of hydrogen bonding and charge transfer. The pH value was 6, and the mass of the formamide-ethylenediaminetetraacetic acid supramolecular polymer accounted for 40 wt% of the aqueous solution.
[0108] 2) High-nickel cathode material LiNi with spherical agglomerates and secondary particles with an average particle size of 20 μm. 0.8 Co 0.15 Al 0.05 O2 (i.e., NCA) and the formamide-ethylenediaminetetraacetic acid supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 500 rpm.
[0109] (3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 500°C at a heating rate of 3°C / min and kept at a constant temperature for 2 hours. After the reaction was completed, the positive electrode material was obtained.
[0110] Cathode materials include LiNi 0.8 Co 0.15 Al 0.05 O2 and coated LiNi 0.8 Co 0.15 Al 0.05The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium ethylenediaminetetraacetate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 5 nm, the thickness of the second coating layer is 8 nm, the mass ratio of lithium ethylenediaminetetraacetate to graphitic carbon nitride is 0.65:1, and the average particle size of the cathode material is 20 μm.
[0111] Example 5
[0112] A method for preparing a cathode material includes the following steps:
[0113] 1) At room temperature, aminourea and phytic acid were dissolved in water at a molar ratio of 4:1. The solution was heated to 80°C in a reaction vessel and stirred at 450 rpm for 12 h. Under the action of hydrogen bonding and charge transfer, an aminourea-phytic acid supramolecular polymer solution was formed with a pH value of 5. The mass of the aminourea-phytic acid supramolecular polymer accounted for 30 wt% of the aqueous solution.
[0114] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e., NCM811) and the aminourea-phytic acid supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 500 rpm.
[0115] (3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 550°C at a heating rate of 5°C / min and kept at a constant temperature for 6 hours. After the reaction was completed, the positive electrode material was obtained.
[0116] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 3nm, the thickness of the second coating layer is 15nm, the mass ratio of lithium phytate to graphitic carbon nitride is 0.25:1, and the average particle size of the cathode material is 15μm.
[0117] Example 6
[0118] A method for preparing a cathode material includes the following steps:
[0119] 1) Dimethylurea, cucurbita, and phytic acid were dissolved in water at a molar ratio of 1:0.5:1 at room temperature. The solution was heated to 100°C in a reaction vessel and stirred at 500 rpm for 8 hours. Under the influence of hydrogen bonding, host-guest interaction, and charge transfer, a supramolecular polymer solution of dimethylurea-cucurbita-phytic acid was formed with a pH of 6. The mass of the dimethylurea-cucurbita-phytic acid supramolecular polymer accounted for 50 wt% of the aqueous solution.
[0120] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e., NCM811) and the dimethylurea-cucurbita-phytic acid supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 500 rpm.
[0121] (3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 600°C at a heating rate of 2°C / min and kept at a constant temperature for 6 hours. After the reaction was completed, the positive electrode material was obtained.
[0122] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 5nm, the thickness of the second coating layer is 18nm, the mass ratio of lithium phytate to graphitic carbon nitride is 0.2:1, and the average particle size of the cathode material is 15μm.
[0123] Example 7
[0124] A method for preparing a cathode material includes the following steps:
[0125] 1) Melamine and diphenylphosphoric acid were dissolved in ethylene glycol at a molar ratio of 2:1 at room temperature (25℃). The solution was heated to 80℃ in a reaction vessel and stirred at 600 rpm for 12 h. A melamine-diphenylphosphoric acid supramolecular polymer solution was formed under hydrogen bonding, charge transfer and π-π interaction. The pH value was 5.5 and the mass of the melamine-diphenylphosphoric acid supramolecular polymer accounted for 30 wt% of the ethylene glycol solution.
[0126] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.15Al 0.05 O2 (i.e., NCA) and the melamine-diphenylphosphate supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 500 rpm.
[0127] (3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 500°C at a heating rate of 3°C / min and kept at a constant temperature for 4 hours. After the reaction was completed, the positive electrode material was obtained.
[0128] Cathode materials include LiNi 0.8 Co 0.15 Al 0.05 O2 and coated LiNi 0.8 Co 0.15 Al 0.05 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium diphenyl phosphate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 5 nm, the thickness of the second coating layer is 10 nm, the mass ratio of lithium diphenyl phosphate to graphitic carbon nitride is 0.55:1, and the average particle size of the cathode material is 15 μm.
[0129] Example 8
[0130] A method for preparing a cathode material includes the following steps:
[0131] 1) At room temperature (25℃), aminourea and glycerophosphate were dissolved in water at a molar ratio of 3:1 and stirred at 800 rpm for 24 h. Under the action of hydrogen bonding and charge transfer, an aminourea-glycerophosphate supramolecular polymer solution was formed with a pH value of 5 and the mass of the aminourea-glycerophosphate supramolecular polymer accounted for 50 wt% of the aqueous solution.
[0132] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e., NCM811) and the aminourea-glycerophosphate supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 5 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 500 rpm.
[0133] 3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 500°C at a heating rate of 3°C / min and held at that temperature for 5 hours. After the reaction was completed, the positive electrode material was obtained.
[0134] Cathode materials include LiNi 0.8 Co0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium glycerol phosphate, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 3nm, the thickness of the second coating layer is 12nm, the mass ratio of lithium glycerol phosphate to graphitic carbon nitride is 0.3:1, and the average particle size of the cathode material is 15μm.
[0135] Example 9
[0136] A method for preparing a cathode material includes the following steps:
[0137] 1) Melamine and phthalimide were dissolved in pyridine at a molar ratio of 3:1 at room temperature (25℃) and stirred at 450 rpm for 24 h. A melamine-phthalimide supramolecular polymer solution was formed under hydrogen bonding, charge transfer and π-π interaction, with a pH of 5. The mass of the melamine-phthalimide supramolecular polymer accounted for 30 wt% of the pyridine solution.
[0138] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e. NCM811) and the supramolecular polymer solution obtained in step 1) are placed in a reactor and stirred and mixed. The amount of supramolecular polymer solution added accounts for 15 wt% of the mass of the high-nickel cathode material. The stirring time is 40 min and the stirring speed is 550 rpm.
[0139] 3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 550°C at a heating rate of 10°C / min and held at that temperature for 6 hours. After the reaction was completed, the positive electrode material was obtained.
[0140] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phthalimide and the second coating layer includes graphitic carbon nitride; the thickness of the first coating layer is 4 nm and the thickness of the second coating layer is 15 nm, the mass ratio of lithium phthalimide to graphitic carbon nitride is 0.4:1; the average particle size of the cathode material is 15 μm.
[0141] Example 10
[0142] A method for preparing a cathode material includes the following steps:
[0143] 1) At room temperature (25℃), aminourea and butyrylimide were dissolved in water at a molar ratio of 1:1 and stirred at 500 rpm for 24 h. Under the interaction of hydrogen bonding and charge transfer, an aminourea-butyrylimide supramolecular polymer solution was formed with a pH value of 6.5 and the mass of the aminourea-butyrylimide supramolecular polymer accounted for 45 wt% of the aqueous solution.
[0144] 2) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e. NCM811) and aminourea-butyrylimide supramolecular polymer solution were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 30 min and the stirring speed was 500 rpm.
[0145] 3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 500℃ at a heating rate of 2℃ / min and held at that temperature for 2 hours. After the reaction was completed, the positive electrode material was obtained.
[0146] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium butyrylimide, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 3.5 nm, the thickness of the second coating layer is 6 nm, the mass ratio of lithium butyrylimide to graphitic carbon nitride is 0.6:1, and the average particle size of the cathode material is 15 μm.
[0147] Example 11
[0148] A method for preparing a cathode material includes the following steps:
[0149] 1) At room temperature (25°C), formamide and maleimide were dissolved in water at a molar ratio of 2:1. The solution was heated to 60°C in a reaction vessel and stirred at 400 rpm for 6 hours. A formamide-maleimide supramolecular polymer solution was formed under the action of hydrogen bonding and charge transfer. The pH value was 6, and the mass of the formamide-maleimide supramolecular polymer accounted for 40 wt% of the aqueous solution.
[0150] 2) High-nickel cathode material LiNi with spherical agglomerates and secondary particles with an average particle size of 15 μm.0.8 Co 0.1 Mn 0.1 O2 (i.e., NCM811) and the formamide-maleimide supramolecular polymer solution obtained in step 1) were stirred and mixed in a reactor. The amount of supramolecular polymer solution added accounted for 10 wt% of the mass of the high-nickel cathode material. The stirring time was 30 min and the stirring speed was 550 rpm.
[0151] (3) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 500°C at a heating rate of 5°C / min and kept at a constant temperature for 4 hours. After the reaction was completed, the positive electrode material was obtained.
[0152] Cathode materials include LiNi 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium maleimide, the second coating layer includes graphitic carbon nitride, the thickness of the first coating layer is 4nm, the thickness of the second coating layer is 10nm, the mass ratio of lithium maleimide to graphitic carbon nitride is 0.5:1, and the average particle size of the cathode material is 15μm.
[0153] Example 12
[0154] The difference between this embodiment and Embodiment 1 is that the molar ratio of melamine to phytic acid is 0.5:1; the final cathode material includes LiNi. 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate and the second coating layer includes graphitic carbon nitride; the thickness of the first coating layer is 4 nm and the thickness of the second coating layer is 1.5 nm, the mass ratio of lithium phytate to graphitic carbon nitride is 2:1; the average particle size of the cathode material is 15 μm.
[0155] Example 13
[0156] The difference between this embodiment and Embodiment 1 is that the molar ratio of melamine to phytic acid is 4:1; the final cathode material includes LiNi. 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate and the second coating layer includes graphitic carbon nitride; the thickness of the first coating layer is 4 nm and the thickness of the second coating layer is 17 nm, the mass ratio of lithium phytate to graphitic carbon nitride is 0.3:1; the average particle size of the cathode material is 15 μm.
[0157] Example 14
[0158] The difference between this embodiment and Embodiment 1 is that the molar ratio of melamine to phytic acid is 6:1; the final cathode material includes LiNi. 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate and the second coating layer includes graphitic carbon nitride; the thickness of the first coating layer is 4 nm and the thickness of the second coating layer is 24 nm, the mass ratio of lithium phytate to graphitic carbon nitride is 0.15:1; the average particle size of the cathode material is 15 μm.
[0159] Example 15
[0160] The difference between this embodiment and Embodiment 1 is that the molar ratio of melamine to phytic acid is 8:1; the final cathode material includes LiNi. 0.8 Co 0.1 Mn 0.1 O2 and coated LiNi 0.8 Co 0.1 Mn 0.1 The first coating layer of O2 and the second coating layer located on the surface of the first coating layer, the first coating layer includes lithium phytate and the second coating layer includes graphitic carbon nitride; the thickness of the first coating layer is 4 nm and the thickness of the second coating layer is 35 nm, the mass ratio of lithium phytate to graphitic carbon nitride is 0.08:1; the average particle size of the cathode material is 15 μm.
[0161] Comparative Example 1
[0162] A method for preparing a positive electrode material is as follows:
[0163] 1) Ni high-nickel cathode material precursor with spherical secondary particles and an average particle size of 20 μm. 0.6 Co 0.3 Mn 0.1(OH)2, lithium hydroxide and additives are mixed evenly to obtain a mixture. The molar ratio of lithium element in lithium hydroxide to nickel, cobalt and manganese elements in high nickel cathode material precursor is 1.02. The additives include lithium sulfate and ammonium dihydrogen phosphate. The amount of lithium sulfate added accounts for 0.1 wt% of the mass of high nickel cathode material precursor, and the amount of ammonium dihydrogen phosphate added accounts for 0.4 wt% of the mass of high nickel cathode material precursor.
[0164] 2) The mixture is heated to 700℃ at a heating rate of 1℃ / min and held for 10h; then cooled to 200℃ at a cooling rate of 1℃ / min and held for 5h, and finally cooled with the furnace to obtain the sintered material.
[0165] 3) The sintering materials are crushed and ground sequentially. The particle size of the crushed and ground materials is 8μm. After passing through a 200-mesh sieve, the crushed and ground materials are used to obtain a high-nickel sintering product with low residual alkali.
[0166] Comparative Example 1 obtained a high-nickel cathode material with low residual alkali by gradient sintering a mixture of a high-nickel cathode material precursor, lithium salt, and weak acid salt additive. The principle behind this method is that the weak acid salt additive reacts with the residual alkali on the surface of the high-nickel cathode material after melting. However, this method has limitations: it requires high temperatures to melt the weak acid salt before reacting with the residual alkali on the high-nickel surface, and the weak acid salt is prone to agglomeration in the high-temperature molten state. The entire process is not only energy-intensive but also leads to incomplete removal of residual alkali. Furthermore, the method in Comparative Example 1 cannot form a graphitic carbon nitride coating layer with high stability, high mechanical strength, and high conductivity on the surface of the high-nickel cathode material, resulting in poor coulombic efficiency, cycle life, and rate performance.
[0167] Comparative Example 2
[0168] The only difference between Comparative Example 2 and Example 1 is that only melamine was used in the preparation of the supramolecular polymer solution, and phytic acid was not added to form a melamine-ethylene glycol solution. The melamine accounted for 30 wt% of the ethylene glycol solution and the melamine-ethylene glycol solution accounted for 10 wt% of the high-nickel cathode material. The remaining steps were the same as in Example 1. The final product obtained was graphite-phase carbon nitride coated high-nickel cathode material NCM811, denoted as g-C3N4 coated NCM.
[0169] Comparative Example 3
[0170] The only difference between Comparative Example 3 and Example 1 is that only phytic acid was used, and melamine was not added to form a phytic acid-ethylene glycol solution. Phytic acid accounted for 30 wt% of the ethylene glycol solution, and the phytic acid-ethylene glycol solution accounted for 10 wt% of the high-nickel cathode material. The pH of the phytic acid-ethylene glycol solution was 1. The high-nickel cathode material NCM811, which consists of spherical agglomerates with an average particle size of 15 μm, and the phytic acid-ethylene glycol solution were stirred and mixed in a reactor at a stirring speed of 500 rpm for 20 min to obtain lithium phytate-coated high-nickel cathode material NCM811, denoted as salt-coated NCM.
[0171] Comparative Example 4
[0172] Comparative Example 4 differs from Example 1 in that: phytic acid glycol solution and melamine glycol solution were prepared separately, and then the high-nickel cathode material was treated sequentially with phytic acid glycol solution and melamine glycol solution. Specifically, the preparation method is as follows:
[0173] 1) Dissolve phytic acid in ethylene glycol at room temperature and stir at 350 rpm for 24 h to obtain a phytic acid ethylene glycol solution with a pH of 1. The mass of phytic acid accounts for 10 wt% of the ethylene glycol solution.
[0174] 2) Melamine was dissolved in ethylene glycol at room temperature and stirred at 350 rpm for 24 h to obtain a melamine ethylene glycol solution, wherein the mass of melamine accounted for 20 wt% of the ethylene glycol solution.
[0175] 3) High-nickel cathode material LiNi, consisting of spherical agglomerates with an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e., NCM811) and the phytic acid solution obtained in step 1) are placed in a reaction vessel and stirred and mixed. The amount of phytic acid solution added accounts for 10 wt% of the mass of the high-nickel cathode material. The stirring time is 20 min and the stirring speed is 500 rpm.
[0176] 4) Add the melamine glycol solution obtained in step 2) into the reactor and continue to stir and mix at 500 rpm for 20 min. Then, under PSA atmosphere, heat the reactor from room temperature to 550℃ at a heating rate of 2℃ / min and keep it at the temperature for 2 h. After the reaction is completed, the positive electrode material is obtained.
[0177] Comparative Example 5
[0178] Comparative Example 5 differs from Example 1 in that oxalic acid and melamine solutions were prepared separately, and the high-nickel cathode material was then treated with oxalic acid and melamine solutions respectively. Specifically, the preparation methods are as follows:
[0179] 1) Dissolve oxalic acid in water at room temperature (25℃) and stir at 350 rpm for 10 min to obtain an oxalic acid solution with a pH of 1.3, wherein the mass of oxalic acid accounts for 1 wt% of the aqueous solution;
[0180] 2) Melamine was dissolved in ethylene glycol at room temperature (25℃) and stirred at 350 rpm for 2 hours to obtain a melamine ethylene glycol solution, wherein the mass of melamine accounted for 20 wt% of the ethylene glycol solution.
[0181] 3) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e. NCM811) and the oxalic acid solution obtained in step 1) are placed in a reaction vessel and stirred and mixed. The amount of oxalic acid solution added accounts for 60 wt% of the mass of the high-nickel cathode material. The stirring time is 20 min and the stirring speed is 500 rpm.
[0182] 4) After the reaction in step 3) is completed, the melamine glycol solution obtained in step 2) is placed in the reaction vessel in step 3) and stirred and mixed. The amount of melamine glycol solution added is 20 wt% of the mass of the high-nickel cathode material. The stirring time is 20 min and the stirring speed is 500 rpm.
[0183] 5) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 550°C at a heating rate of 2°C / min and held at that temperature for 2 hours. After the reaction was completed, the positive electrode material was obtained.
[0184] Comparative Example 5 involves first mixing a high-nickel cathode material with an oxalic acid solution, then adding a melamine solution and mixing further, finally sintering to obtain a cathode material coated with graphite-phase carbon nitride. This method removes residual alkali by adding oxalic acid solution. However, because oxalic acid cannot form supramolecular polymers, even at a mass fraction of 1 wt%, the acidity is still too strong and easily corrodes the surface structure of the high-nickel cathode material. Excessive water as a solvent can also trigger side reactions on the surface of the high-nickel cathode material, generating NiOOH-like phase impurities, leading to increased internal resistance and severe performance degradation of the battery.
[0185] Comparative Example 6
[0186] Comparative Example 6 differs from Example 1 in that acetic acid and melamine solutions were prepared separately, and then the high-nickel cathode material was treated with acetic acid and melamine solutions respectively. Specifically, the preparation methods are as follows:
[0187] 1) Dissolve acetic acid in water at room temperature (25℃) and stir at 350 rpm for 10 min to obtain an acetic acid solution with a pH of 2.8, wherein the mass of acetic acid accounts for 1 wt% of the aqueous solution;
[0188] 2) Melamine was dissolved in ethylene glycol at room temperature (25℃) and stirred at 350 rpm for 2 hours to obtain a melamine ethylene glycol solution, wherein the mass of melamine accounted for 20 wt% of the ethylene glycol solution.
[0189] 3) High-nickel cathode material LiNi with spherical secondary particles and an average particle size of 15 μm. 0.8 Co 0.1 Mn 0.1 O2 (i.e. NCM811) and the acetic acid solution obtained in step 1) were placed in a reaction vessel and stirred and mixed. The amount of acetic acid solution added accounted for 70 wt% of the mass of the high-nickel cathode material. The stirring time was 20 min and the stirring speed was 500 rpm.
[0190] 4) After the reaction in step 3) is completed, the melamine glycol solution obtained in step 2) is placed in the reaction vessel in step 3) and stirred and mixed. The amount of melamine glycol solution added is 20 wt% of the mass of the high-nickel cathode material. The stirring time is 20 min and the stirring speed is 500 rpm.
[0191] 5) Under a PSA atmosphere (oxygen content ≈ 21%), the reactor was heated from room temperature to 550°C at a heating rate of 2°C / min and held at that temperature for 2 hours. After the reaction was completed, the positive electrode material was obtained.
[0192] Test Example 1
[0193] Product morphology and composition analysis
[0194] The biphasic layer-coated NCM prepared in Example 1 was subjected to SEM and TEM imaging, respectively. Figure 2 and Figure 3 As shown. By Figure 2 As can be seen, the NCM811 particles exhibit a uniform coating layer on their surface. (From...) Figure 3 As can be seen, the NCM811 particles exhibit a dual-phase coating layer, consisting of an organolithium salt first coating layer and a graphite-phase carbon nitride second coating layer. The thickness of the organolithium salt first coating layer is approximately 4 nm, and the thickness of the graphite-phase carbon nitride second coating layer is approximately 10 nm.
[0195] refer to Figure 4 and Figure 5The figures show the high-resolution Ni2p and N1s spectra of the biphase layer-coated NCM obtained in Example 1. It can be seen that for the biphase layer-coated NCM, Ni-N peaks are fitted at 853.2 eV in the Ni2p spectrum and 398.4 eV in the N1s spectrum, while a Li-N peak is fitted at 398.9 eV in the N1s spectrum, with an error range of ±0.5 eV. This indicates that the positive electrode active material obtained in Example 1 has Ni-N peaks fitted at 852.0–855.5 eV in the Ni2p spectrum and 396.2–398.5 eV in the N1s spectrum, while a Li-N peak is fitted at 398.6–400.5 eV in the N1s spectrum. This demonstrates that a metallic Ni-N / Li-N highly conductive interface is formed between the first organic lithium salt coating layer and the high-nickel positive electrode material, which is beneficial for rapid charge transfer and reduces impedance. The Ni-N content of the salt-coated NCM... 2p The spectrum does not show Ni-N bonds, and the N in g-C3N4 is... 1s No Li-N / Ni-N bonds were detected in the spectrum. The reason why a metallic Ni-N / Li-N highly conductive interface can be formed between the organolithium salt first coating layer and the high-nickel cathode material should be that: the high-nickel cathode material is coated and modified with a polymer solution containing acidic organic matter and nitrogen-containing organic matter. Since the acidic organic matter and nitrogen-containing organic matter are uniformly dispersed in the polymer solution, they are also uniformly distributed in the initial coating layer. Then, the organolithium salt first coating layer and the graphite phase carbon nitride second coating layer are generated sequentially through in-situ reaction, so that Ni-N / Li-N bonds can be formed between the organolithium salt first coating layer and the high-nickel cathode material.
[0196] Test Example 2
[0197] Determination of specific surface area and residual alkali content of cathode materials.
[0198] The specific surface area of the cathode material was tested using a Microt Tristar 3020 specific surface area and pore size analyzer. A certain mass of powder was weighed and completely degassed under vacuum heating to remove surface adsorbates. The specific surface area of the particles was calculated by the amount of nitrogen adsorbed using the nitrogen adsorption method. The results are shown in Table 1.
[0199] The total amount of residual alkali on the surface of the cathode material was tested using a potentiometric titrator. Specifically, the residual alkali content was calculated by titrating with hydrochloric acid and then converting the amount of hydrochloric acid consumed. The results are shown in Table 1. The residual alkali content in Table 1 refers to the mass of residual alkali as a percentage of the mass of the cathode material in parts per million.
[0200] Table 1: Residual alkali content and specific surface area of the cathode materials obtained in each embodiment and comparative example
[0201]
[0202]
[0203] As can be seen from Table 1: (1) Referring to Comparative Example 2, only a graphite phase carbon nitride layer was generated, and the residual alkali was not removed. The residual alkali content was as high as 7245 ppm. Compared with Comparative Example 2, the residual alkali content of the method of the present invention was all lower than 1500 ppm, and the residual alkali removal rate was between 80% and 90%. It can be seen that the residual alkali was fully removed; (2) Referring to Comparative Example 3, the modifier used in Comparative Example 3 was phytic acid solution. Since a supramolecular polymer solution was not formed, the acidity of the phytic acid solution (pH 1) was stronger than that of the supramolecular polymer solution (pH 5). Therefore, the residual alkali content of the product obtained in Comparative Example 3 was lower than that of the present invention, which was 1053 ppm. However, the phytic acid solution obviously corroded the ternary cathode material, and etching marks appeared on the surface of the ternary cathode material; (3) Comparing Example 1 and Comparative Example 3, the only difference between Example 1 and Comparative Example 3 is that Example 1 used a supramolecular polymer solution. The residual alkali content of the product obtained in Example 1 was lower than that of the present invention. The residual alkali removal effect was 1153 ppm, which is comparable to that of Comparative Example 3 (1053 ppm). It can be seen that the supramolecular polymer solution of the present invention can fully remove the residual alkali, and there are no etching marks on the surface of the ternary cathode material; (4) Referring to Comparative Example 1, which is the existing method of removing residual alkali by melting weak acid salt, the residual alkali content was 4280 ppm. Compared with the method of the present invention, the weak alkali content was about 3 times higher. It can be seen that the method of the present invention significantly reduced the weak alkali content compared with the prior art; (5) Referring to Comparative Example 4, which is a double-layer coated cathode material prepared by phytic acid solution and melamine solution respectively. Although the residual alkali content was low, the specific surface area was large; Referring to Comparative Examples 5 and 6, which are two-phase coated cathode materials prepared by oxalic acid and acetic acid solutions with low mass fraction and high solvent content respectively. Although the residual alkali was low, the specific surface area was significantly increased. This is because the high nickel cathode interface was reorganized by the excessive proportion of aqueous solution treatment, which increased the specific surface area.
[0204] Compared with Comparative Examples 2, 3, and 4, Examples 1-15 are two-phase layer coated cathode materials, and the specific surface area of the products obtained in Examples 1-15 is less than 2.1 m². 2 / g, Comparative Examples 2 and 3 are cathode materials coated with monolayer graphitic carbon nitride and monolayer lithium phytate salt, respectively, with specific surface areas of 2.49 and 2.58 m², respectively. 2 / g, it can be seen that the specific surface area of the bilayer coated cathode material is lower than that of the monolayer coated cathode material. The lower specific surface area is beneficial to the material to obtain a high coulombic efficiency.
[0205] Test Example 3
[0206] Electrical performance testing
[0207] The electrochemical performance of the prepared positive electrode material was evaluated using a coin cell. The specific method is as follows: The positive electrode material, conductive carbon black Super P, and polyvinylidene fluoride (PVDF) were weighed at a mass ratio of 96:2:2. N-methyl-2-pyrrolidone (NMP) was added at a solid content of 50%, and the mixture was prepared into a viscous slurry using a high-speed disperser. This slurry was then uniformly coated onto aluminum foil using a scraper, dried in an oven at 80°C, and rolled to form a positive electrode sheet with a diameter of 14 mm. A 16 mm diameter lithium sheet was used as the negative electrode, a Celgard polypropylene (PP) membrane as the separator, and a 1 mol / L LiPF6 carbonate solution (diethyl carbonate (DEC) / ethylene carbonate (EC) volume ratio 1:1) as the electrolyte. The coin cell was assembled in an argon-filled glove box.
[0208] The coin cell half-cells prepared above were subjected to electrical performance tests on an AUTOLAB PGSTAT 302N electrochemical workstation and a LANDCT3002A. First, an AC impedance test was performed. The test method was as follows: after cycling the coin cell once, the test was conducted at an open-circuit voltage of 4.3V, with a test frequency range of 10 Hz. -2 ~10 5 Hz, amplitude voltage is 5mV. (Through) Figure 6 The equivalent circuit model was fitted to the measured AC impedance spectrum, and the charge transfer resistance was calculated. The results are shown in Table 2. Figure 6 Electrochemical impedance spectroscopy (EIS) of the biphase layer-coated NCM prepared in Example 1, the g-C3N4-coated NCM prepared in Comparative Example 2, and the salt-coated NCM prepared in Comparative Example 3.
[0209] Then, the coin cells were tested for capacity at 25℃ and 55℃, and at 3.0V to 4.3V, respectively. The reference capacity was set to 200mAh / g, and the current density corresponding to 1C was 200mA / g. The capacity retention rate after 100 cycles at 25℃ and 55℃ is shown in Table 2. Figure 7 The graph shows the capacity retention rate of the biphase layer coated NCM prepared in Example 1 after 100 cycles at 25°C and 55°C.
[0210] Table 2: Electrical performance indicators of the cathode materials obtained in each embodiment and comparative example
[0211]
[0212] Refer to Table 2, and combine with Figure 6As can be seen: 1) The charge transfer resistance (31Ω) of the battery prepared from the cathode material obtained in Example 1 is smaller than that of Comparative Examples 2-6 (39Ω-52Ω). This is mainly due to the formation of a metallic Li-N / Ni-N highly conductive interface in the cathode material of the present invention. 2) The cathode materials obtained in Examples 2-11 and 13-15 also have low charge transfer resistance (33Ω-36Ω). The charge transfer resistance of Example 12 is larger (45Ω). This is because the mass ratio of lithium phytate salt to graphite phase carbon nitride in Example 12 is too large (2:1), resulting in an excessively thick first coating layer of lithium phytate salt formed on the surface of the high-nickel cathode material. This is not conducive to the formation of highly conductive Ni-N bonds between the graphite phase carbon nitride in the second coating layer and the high-nickel cathode material, thus increasing the charge transfer resistance. The charge transfer resistance of the cathode materials prepared in Comparative Examples 5 and 6 increased significantly (>50Ω). This is because the addition of a high proportion of acid solution during the removal of residual alkali not only caused corrosion of the surface of the high-nickel cathode material, but also generated the NiOOH phase on the surface of the high-nickel cathode, which increased the charge transport resistance.
[0213] Refer to Table 2, and combine with Figure 7 As can be seen: 1) The battery prepared with the cathode material of Example 1 retains a capacity of 94.7% after 100 cycles at 25°C, which is higher than the 88.2% to 92.4% of the prior art documents 2 to 6, demonstrating the high cycle stability of the cathode material of the present invention; after 100 cycles at a high temperature of 55°C, the capacity retention is even higher, reaching 97.9%, which is higher than the 90.5% to 94.7% of the prior art documents 2 to 6, demonstrating the high thermal stability of the cathode material of the present invention. 2) The cathode materials prepared in Examples 2 to 11 and 13 to 14 also exhibit excellent cycle stability and thermal stability. The cycle stability of Example 15 is poor. This is because the mass ratio of lithium phytate salt to graphite phase carbon nitride in Example 15 is too small (0.8:1), resulting in almost only a single layer of graphite phase carbon nitride coating on the surface of the high-nickel cathode material, which is not conducive to improving the stability of the cathode material.
[0214] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.
Claims
1. A positive electrode material, characterized in that, The invention includes a high-nickel cathode material and a coating layer formed on at least a portion of the surface of the high-nickel cathode material; the coating layer includes a first coating layer and a second coating layer located on the surface of the first coating layer, the first coating layer including an organolithium salt, the organolithium salt including an organolithium salt containing acidic groups, the acidic groups of the organolithium salt including at least one of phosphate groups, carboxylic acid groups and imide groups, and the second coating layer including graphitic carbon nitride; The residual alkali content of the positive electrode material is 100ppm to 2000ppm, the charge transfer resistance of the positive electrode material is less than or equal to 36Ω, and the specific surface area of the positive electrode material is 1m². 2 / g~2.1m 2 / g; the cathode material exhibits Ni2pXPS and N1sXPS spectra at 852.0–855.5 eV and 396.2–398.5 eV, respectively. The characteristic peak of the N binding energy, located at 398.6–400.5 eV in the N1s XPS spectrum, indicates that Li The characteristic peak of N binding energy.
2. The cathode material according to claim 1, characterized in that, The chemical formula of the high-nickel cathode material is LiNi. x Co y M (1-x -y) O2, wherein 0.6 < x < 1.0, 0 < y < 0.2, and M includes at least one of Mn and Al.
3. The cathode material according to claim 1 or 2, characterized in that, It satisfies at least one of the following characteristics a to f: a. The organolithium salt containing a phosphate group includes at least one of lithium phytate, lithium diphenyl phosphate, and lithium glycerophosphate; b. The organolithium salt containing a carboxylic acid group includes at least one of lithium phenylacetate, lithium ethylenediaminetetraacetate, and lithium barbiturate; c. The organolithium salts containing imide groups include lithium phthalimide, lithium butyrylimide, and lithium maleimide; d. The thickness of the first coating layer is 1 nm to 5 nm; e. The thickness of the second coating layer is 5 nm to 20 nm; f. The mass ratio of the organic lithium salt to the graphitic carbon nitride is 0.1 to 1:
1.
4. The cathode material according to claim 1, characterized in that, It satisfies at least one of the following characteristics a to b: a. The positive electrode material has a spherical or near-spherical structure; b. The average particle size of the cathode material is 5 μm to 30 μm.
5. A method for preparing a positive electrode material, characterized in that, Includes the following steps: A mixture containing nitrogen-containing organic matter, acidic organic matter, and solvent is mixed to obtain a polymer solution. The acidic organic matter includes organic matter containing acidic groups, and the acidic groups in the acidic organic matter include at least one of phosphate groups, carboxylic acid groups, and imide groups. The polymer solution is mixed with a high-nickel cathode material and then coated to obtain a polymer-coated high-nickel cathode material; and The polymer-coated high-nickel cathode material was heat-treated in an oxygen-containing atmosphere to obtain the cathode material; The cathode material includes a high-nickel cathode material and a coating layer formed on at least a portion of the surface of the high-nickel cathode material; the coating layer includes a first coating layer and a second coating layer located on the surface of the first coating layer, the first coating layer including an organolithium salt and the second coating layer including graphitic carbon nitride.
6. The preparation method according to claim 5, characterized in that, It satisfies at least one of the following characteristics a to h: a. The nitrogen-containing organic compounds include melamine, formamide, 1,3-dimethylamine, and methylamine. Dimethylurea, N,N At least one of dimethylurea, aminourea, cucurbita, and derivatives of any of the above organic compounds; b. The acidic organic compound containing a phosphate group includes at least one of phytic acid, lithium diphenyl phosphate, and glycerophosphate; c. The acidic organic compound includes acidic organic compounds containing carboxylic acid groups, and the acidic organic compounds containing carboxylic acid groups include at least one of phenylacetic acid, ethylenediaminetetraacetic acid, and barbituric acid; d. The acidic organic compound containing an imide group includes at least one of phthalimide, butyrylimide, and maleimide; e. The solvent includes water, ethanol, ethylene glycol, methanol, acetone, pyridine, and N,N At least one of dimethylformamide; f. The molar ratio of the nitrogen-containing organic compound to the acidic organic compound is 0.5 to 4:1; g. The pH of the polymer solution is 4–7; h. In the polymer solution, the total mass of the nitrogen-containing organic matter and the acidic organic matter accounts for 20% to 50% of the mass of the solvent.
7. The preparation method according to claim 5 or 6, characterized in that, It satisfies at least one of the following characteristics a to c: a. The mixing temperature of the mixture is 10℃~120℃; b. The mixing speed of the mixture is 200 rpm to 1000 rpm; c. The mixing time of the mixture is 2h to 48h.
8. The preparation method according to any one of claims 5 to 7, characterized in that, It satisfies at least one of the following characteristics a to d: a. The polymer solution comprises 5 wt% to 15 wt% of the high-nickel material. b. The method of mixing the polymer solution with the high-nickel cathode material is stirring; c. The stirring time is 20 min to 40 min; d. The stirring speed is 500 rpm to 800 rpm.
9. The preparation method according to any one of claims 5 to 8, characterized in that, It satisfies at least one of the following characteristics a to d: a. The oxygen content of the oxygen-containing atmosphere is less than 25% and greater than 1% by volume; b. The heat treatment temperature is 400℃~600℃; c. The heating rate of the heat treatment is 2℃ / min to 10℃ / min; d. The heat treatment time is 2h to 8h.
10. A lithium-ion battery, characterized in that, The cathode material includes the cathode material according to any one of claims 1 to 4 or the cathode material prepared by the preparation method according to any one of claims 5 to 9.
Citation Information
Patent Citations
Surface coating modified lithium-ion battery laminar positive electrode material and preparation method thereof
CN106784618A
Lithium ion battery high-nickel ternary positive electrode material and preparation method thereof, and lithium ion battery
CN108206279A
Preparation method for N-doped carbon-covered positive electrode material
CN108682828A
High-nickel ternary positive electrode material and preparation method and application thereof
CN111092202A