Heat treatment method for passivated contact solar cell, heat treatment device, preparation method and passivated contact solar cell

Through a multi-stage heating and cooling heat treatment method, hydrogen ions are allowed to enter the polysilicon layer and silicon matrix of the passivation contact solar cell, which solves the problem of hydrogen ion escape during a single heating and cooling process, significantly improves the cell efficiency and reduces the attenuation phenomenon.

CN115642198BActive Publication Date: 2024-10-29TRINA SOLAR CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202110812245.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-19
Publication Date
2024-10-29
Estimated Expiration
2041-07-19

AI Technical Summary

Technical Problem

In the existing heat treatment method for passivating contact solar cells, a single heating and cooling process causes hydrogen ions to escape, which makes it impossible to effectively passivate defects in crystalline silicon cells, leading to photo-induced attenuation and thermal-assisted attenuation problems.

Method used

Using a multi-stage heating and cooling heat treatment method, the peak temperature of each stage of heating and cooling gradually decreases. Through multiple heating and cooling, hydrogen ions enter the polysilicon layer and the silicon matrix to achieve the hydrogen passivation effect, replacing the traditional hydrogen passivation treatment.

Benefits of technology

It significantly improves the efficiency of passivated contact cells, increases short-circuit current and open-circuit voltage, reduces photo-induced attenuation and heat-assisted photo-induced attenuation, and completely replaces hydrogen passivation treatment in conventional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003168809190000111
    Figure BDA0003168809190000111
  • Figure BDA0003168809190000121
    Figure BDA0003168809190000121
Patent Text Reader

Abstract

The present invention provides a heat treatment method, a heat treatment device, a preparation method and a passivated contact solar cell, wherein the heat treatment method comprises: performing heating and cooling heat treatments on the cell alternately in sequence, and the peak temperature of each heating and cooling heat treatment is gradually reduced. The present invention achieves a hydrogen passivation effect through continuous heating and cooling, can increase short-circuit current and open-circuit voltage, greatly improve the efficiency of the passivated contact cell, and reduce photo-induced degradation and heat-assisted photo-induced degradation, and can completely replace the hydrogen passivation treatment in conventional processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar energy, and relates to a heat treatment method and a preparation method of a passivated contact solar cell and a passivated contact solar cell. Background Art

[0002] Light Induced Degradation (LID), also known as light decay, refers to the power decay phenomenon caused by solar cells and modules during illumination. By passivating solar cells under certain process conditions, the internal defects of crystalline silicon cells can be passivated, and the recombination center can be reduced, which can effectively improve the conversion efficiency of photovoltaic cells, effectively reduce the light-induced decay and heat-assisted decay of crystalline silicon cells, and increase the power generation of photovoltaic systems during their life cycle, which ultimately helps to reduce the investment in photovoltaic systems.

[0003] On the other hand, with the continuous advancement of industrial technology and the demand for affordable access to the Internet, people are constantly exploring and developing various types of high-efficiency crystalline silicon cell technologies. Among them, TOPCon (Tunnel Oxide Passivating Contacts) cells are recognized by the industry as one of the most efficient solar cells. They form a very thin silicon oxide layer on the back of the silicon wafer, and form a microcrystalline amorphous mixed Si film after phosphorus doping. After high-temperature annealing and activation, an excellent passivation contact structure is formed.

[0004] CN111987182A discloses a TOPCon solar cell and a method for manufacturing the same, the method comprising the following steps: (a) providing an N-type silicon wafer for a TOPCon solar cell; (b) texturing the silicon wafer and diffusing it on a first surface thereof to form a PN junction; (c) sequentially forming a silicon oxide layer, a microcrystalline silicon seed crystal layer, a doped amorphous silicon layer or a doped microcrystalline silicon layer on a second surface of the silicon wafer opposite to the first surface; (d) performing a crystallization annealing treatment on the silicon wafer to crystallize the microcrystalline silicon and / or amorphous silicon into polycrystalline silicon; (e) forming a first anti-reflection passivation film and a second anti-reflection passivation film on the first surface and the second surface of the silicon wafer, respectively; and (f) forming a first electrode and a second electrode on the first surface and the second surface of the silicon wafer, respectively.

[0005] CN110459469A discloses a sintering method, a preparation method, a solar cell and a sintering furnace for a solar cell. The sintering method for a solar cell includes: performing a first heating treatment on the front surface of a silicon wafer; performing a second heating treatment on the front surface of the silicon wafer that has been subjected to the first heating treatment; performing a heat preservation treatment on the front surface of the silicon wafer that has been subjected to the second heating treatment; performing a temperature reduction treatment on the front surface of the silicon wafer that has been subjected to the heat preservation treatment, so as to form a solar cell; wherein the heating rate of the front surface of the silicon wafer in the first heating treatment is greater than the heating rate of the front surface of the silicon wafer in the second heating treatment.

[0006] CN107863417A discloses a method for preparing an n-type solar cell, comprising the following steps: 1. texturing and cleaning the surface of an n-type silicon substrate; 2. preparing an emitter on the front side of the silicon substrate; 3. performing insulation treatment; 4. preparing a back surface field and a back passivation layer; 5. preparing a front passivation and anti-reflection film; 6. patterning an electrode slurry layer containing a conductive component on the front and back sides; 7. performing a first heat treatment process; and 8. performing a second heat treatment process.

[0007] CN108039374A discloses a method for preparing an n-type bifacial solar cell, which includes removing a damage layer or texturing treatment and cleaning treatment on an n-type silicon substrate; preparing an emitter on the back of the silicon substrate; performing insulation treatment; preparing a front surface field on the front of the silicon substrate; preparing a passivation and anti-reflection film on the light-receiving surface, and preparing a back passivation layer; patterning an electrode slurry layer containing a conductive component on the front and back surfaces; performing a first heat treatment process; and performing a second heat treatment process. Summary of the invention

[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a heat treatment method, a heat treatment device, a preparation method and a passivated contact solar cell. The present invention achieves a hydrogen passivation effect through continuous heating and cooling, which can increase the short-circuit current and open-circuit voltage, greatly improve the efficiency of the passivated contact cell and reduce photoinduced degradation and heat-assisted photoinduced degradation, and can completely replace the hydrogen passivation treatment in conventional processes.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a heat treatment method for a passivated contact solar cell, the heat treatment method comprising: performing alternating heating and cooling heat treatments on the cell pieces, wherein the peak temperature of each heating heat treatment stepwise decreases.

[0011] The present invention achieves hydrogen passivation effect through continuous heating and cooling. The traditional sintering process includes a heating and cooling process with only one temperature peak. However, during a heating process, hydrogen ions in the passivated contact solar cell escape due to the influence of high temperature, and the passivation effect that can be played is limited. Therefore, the present invention performs multi-stage heating and cooling heat treatment on the basis of a single heating and cooling process. The peak temperature of each subsequent heating and cooling heat treatment is lower than that of the previous stage. Under this heat treatment method, hydrogen ions in the hydrogen-rich silicon nitride layer on the back of the passivated contact structure battery can enter the polysilicon layer to further passivate the defects in the polysilicon layer. At the same time, part of the hydrogen ions enter the silicon substrate through the polysilicon layer and the tunneling layer to further passivate the defects of the silicon substrate, thereby achieving the hydrogen passivation effect, increasing the short-circuit current and the open-circuit voltage, greatly improving the efficiency of the passivated contact battery, and reducing photoinduced degradation and heat-assisted photoinduced degradation. The present invention can completely replace the hydrogen passivation treatment in the conventional process.

[0012] It should be noted that the heat treatment process provided by the present invention has no holding time, that is, the temperature of the entire process changes continuously, and multiple peaks of the heating heat treatment process and multiple peaks of the cooling heat treatment process will appear on the temperature change curve.

[0013] As a preferred technical solution of the present invention, the heat treatment method specifically includes: performing a first heating heat treatment, a first cooling heat treatment and a second heating heat treatment on the battery cell in sequence and then cooling to room temperature.

[0014] It should be noted that room temperature is a concept well known to those skilled in the art, that is, 20 to 30°C.

[0015] The present invention replaces the hydrogen passivation of the original scheme with a multi-stage heat treatment. The first heating plays a role in slurry sintering (similar to the sintering in the original preparation process), so that the slurry forms a good ohmic contact with the silicon wafer. At the same time, under the first peak temperature condition, the hydrogen ions in the passivated contact solar cell escape due to the influence of high temperature. In the process of the first cooling heat treatment, since a certain temperature condition is still retained, the remaining hydrogen ions in the matrix are redistributed, which has a certain passivation effect on the defects in the body. However, since the first peak temperature is too high, a large number of hydrogen ions escape. The passivation effect is limited; at the same time, since the polysilicon structure in the passivation contact structure is formed by amorphous silicon crystallization through high-temperature annealing, the amorphous state and the crystalline state coexist in its structure, and the temperature after cooling is not enough to allow hydrogen ions to enter the polysilicon layer to passivate the defects in the layer; based on this, the present invention proposes a second heating process, which can allow the hydrogen ions in the hydrogen-rich silicon nitride layer on the back of the passivation contact structure battery to enter the polysilicon layer, further passivating the defects in the polysilicon layer, and at the same time, some hydrogen ions enter the silicon substrate through the polysilicon layer and the tunneling layer, further passivating the defects in the silicon substrate. The second cooling heat treatment process causes the hydrogen ions in the silicon substrate and the polysilicon layer to be redistributed for the second time.

[0016] As a preferred technical solution of the present invention, the peak temperature of the first temperature increase heat treatment is higher than the peak temperature of the second temperature increase heat treatment.

[0017] As a preferred technical solution of the present invention, the peak temperature of the first temperature increase heat treatment is 760-800°C, for example, it can be 760°C, 765°C, 770°C, 775°C, 780°C, 785°C, 790°C, 795°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] As a preferred technical solution of the present invention, the peak temperature zone of the first cooling heat treatment is 200-600°C, for example, it can be 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 350-450°C.

[0019] As a preferred technical solution of the present invention, the peak temperature of the second temperature increase heat treatment is 550-650°C, for example, it can be 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C or 650°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 590-610°C.

[0020] In a second aspect, the present invention provides a heat treatment device for performing the heat treatment method described in the first aspect, wherein the heat treatment device comprises a sintering furnace.

[0021] In a third aspect, the present invention provides a method for preparing a passivated contact solar cell, the preparation method comprising:

[0022] (1) Texturing the surface of the silicon wafer, diffusing boron on the surface of the silicon wafer and removing the borosilicate glass on the back;

[0023] (2) depositing a back tunneling oxide layer and a back doped polysilicon layer on the back side of the silicon wafer in sequence;

[0024] (3) Clean the front side of the silicon wafer to remove the phosphorus silicon glass and polysilicon coating on the front side;

[0025] (4) depositing a front passivation film and a front anti-reflection layer on the front side of the silicon wafer in sequence;

[0026] (5) depositing a back anti-reflection layer on the back side of the silicon wafer;

[0027] (6) forming metal grid lines on the surface of the back anti-reflection layer and the front anti-reflection layer by screen printing to obtain a solar cell;

[0028] (7) Heat-treating the cell piece to obtain the passivated contact solar cell.

[0029] Wherein, the heat treatment in step (7) adopts the heat treatment method described in the first aspect.

[0030] The conventional preparation process of the passivated contact solar cell is: cleaning and texturing - boron diffusion - back cleaning, removal of back borosilicate glass - oxidation - deposition of N-type polysilicon - wet cleaning - front and back surface dielectric film passivation and anti-reflection film deposition - screen printing - sintering - hydrogen passivation; while the preparation process provided by the present invention is: cleaning and texturing - boron diffusion - back cleaning to remove back borosilicate glass - oxidation - deposition of N-type polysilicon - wet cleaning - front and back surface deposition of passivation film and anti-reflection layer - screen printing - heat treatment. It can be seen from this that the difference between the present invention and the conventional preparation process is that the hydrogen passivation process in the traditional process is eliminated, a new temperature control is performed at the sintering end, the temperature field is processed by heat treatment, and the hydrogen passivation process is completed by using sintering equipment, which reduces one process and saves hydrogen passivation equipment.

[0031] It should be noted that the present invention uses multi-stage heat treatment in the preparation process of passivated contact solar cells, replacing the hydrogen passivation operation in the original preparation process. Its role and effect are the same as hydrogen passivation, and it can also increase short-circuit current and open-circuit voltage, greatly improve the efficiency of passivated contact cells, and reduce light-induced degradation and heat-assisted light-induced degradation. In order to better illustrate the advantages of replacing hydrogen passivation with multi-stage heat treatment in the present invention, the working principle of hydrogen passivation is particularly explained:

[0032] Defects in silicon crystals include intrinsic point defects, especially grain boundaries, dislocations, and silicon dangling bonds on the surface of the crystal, etc. These impurities and defects become "killers" of photogenerated electrons and holes, significantly reducing the lifetime of minority carriers and thus reducing the conversion efficiency of solar cells.

[0033] The hydrogen element in crystalline silicon plays an important role in solar cells. The hydrogen atoms in silicon have strong reactivity. They can react with light element impurities and their complexes, with doping atoms such as boron and phosphorus, with transition metal impurities, and with silicon dangling bonds, and are enriched on the crystal surface, grain boundaries, and dislocation regions; they can even react with other hydrogen atoms to form hydrogen molecules. Therefore, the reaction of hydrogen atoms with other impurities and defects can be used to passivate the recombination activity of these recombination centers and increase the lifespan of minority carriers in silicon crystals. Therefore, after hydrogen passivation treatment, the short-circuit current and open-circuit voltage can be increased, the efficiency of the passivated contact cell can be greatly improved, and the photoinduced degradation and thermally assisted photoinduced degradation can be reduced.

[0034] The hydrogen passivation process refers to the process of promoting the movement of hydrogen enriched in the passivation layer of the solar cell under high temperature conditions. The hydrogen atoms will react with the defect states in the solar cell body to form hydrogen molecules, passivating the composite properties of the defect states and greatly improving the photoelectric conversion efficiency of the solar cell.

[0035] The present invention replaces the hydrogen passivation of the original scheme with a multi-stage heat treatment. The first heating plays a role in slurry sintering (similar to the sintering in the original preparation process), so that the slurry forms a good ohmic contact with the silicon wafer. At the same time, under the first peak temperature condition, the hydrogen ions in the passivated contact solar cell escape due to the influence of high temperature. In the process of the first cooling heat treatment, since a certain temperature condition is still retained, the remaining hydrogen ions in the matrix are redistributed, which has a certain passivation effect on the defects in the body. However, since the first peak temperature is too high, a large number of hydrogen ions escape. The passivation effect is limited; at the same time, since the polysilicon structure in the passivation contact structure is formed by amorphous silicon crystallization through high-temperature annealing, the amorphous state and the crystalline state coexist in its structure, and the temperature after cooling is not enough to allow hydrogen ions to enter the polysilicon layer to passivate the defects in the layer; based on this, the present invention proposes a second heating process, which can allow the hydrogen ions in the hydrogen-rich silicon nitride layer on the back of the passivation contact structure battery to enter the polysilicon layer, further passivating the defects in the polysilicon layer, and at the same time, some hydrogen ions enter the silicon substrate through the polysilicon layer and the tunneling layer, further passivating the defects in the silicon substrate. The second cooling heat treatment process causes the hydrogen ions in the silicon substrate and the polysilicon layer to be redistributed for the second time.

[0036] Therefore, the two-stage heat treatment operation provided by the present invention can completely replace the original hydrogen passivation treatment, and also replace the original sintering process. In this way, not only the hydrogen passivation equipment is saved, but also the heat treatment can be achieved by only appropriate modification on the basis of the existing sintering furnace, the equipment modification project is small, and the modification cost is low.

[0037] In a fourth aspect, the present invention provides a passivated contact solar cell, which is prepared by the preparation method described in the third aspect.

[0038] As a preferred technical solution of the present invention, the solar cell includes a silicon wafer, and the back side of the silicon wafer is sequentially stacked with a back tunneling oxide layer, a back doped polysilicon layer, a back anti-reflection layer and a back metal grid line, and the back metal grid line is in passivation contact with a back passivation film.

[0039] As a preferred technical solution of the present invention, a boron diffusion layer, a front passivation film, a front anti-reflection layer and a front metal grid line are sequentially stacked on the front side of the silicon wafer.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The present invention achieves hydrogen passivation effect through continuous heating and cooling. The traditional sintering process includes a heating and cooling process with only one temperature peak. However, during a heating process, hydrogen ions in the passivated contact solar cell escape due to the influence of high temperature, and the passivation effect that can be played is limited. Therefore, the present invention performs multi-stage heating and cooling heat treatment on the basis of a single heating and cooling process. The peak temperature of each subsequent heating and cooling heat treatment is lower than that of the previous stage. Under this heat treatment method, hydrogen ions in the hydrogen-rich silicon nitride layer on the back of the passivated contact structure battery can enter the polysilicon layer to further passivate the defects in the polysilicon layer. At the same time, part of the hydrogen ions enter the silicon substrate through the polysilicon layer and the tunneling layer to further passivate the defects of the silicon substrate, thereby achieving the hydrogen passivation effect, increasing the short-circuit current and the open-circuit voltage, greatly improving the efficiency of the passivated contact battery, and reducing photoinduced degradation and heat-assisted photoinduced degradation. The present invention can completely replace the hydrogen passivation treatment in the conventional process. DETAILED DESCRIPTION

[0042] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0043] Example 1

[0044] This embodiment provides a method for preparing a battery cell, and the method specifically comprises the following steps:

[0045] (1) KOH and a texturing additive were used to texturize an N-type single crystal silicon wafer with a thickness of 170 μm, and then RCA cleaning was performed to form a pyramid-structured texture surface with a texture reflectivity of 12%;

[0046] (2) preparing a boron diffusion layer on the surface of the silicon wafer by high-temperature diffusion, and the sheet resistance of the boron diffusion layer is 120Ω / □;

[0047] (3) The borosilicate glass formed on the back and the excess boron diffusion layer on the edge are etched away using a mixed pickling solution of HF and HNO3, leaving the boron diffusion layer on the front side of the silicon wafer;

[0048] (4) A 1.5 nm thick SiO2 layer and a 120 nm thick n-type polysilicon layer are deposited and grown on the back of the silicon wafer using an LPVCD device;

[0049] (5) cleaning to remove the excess n-type polysilicon layer and performing RCA cleaning;

[0050] (6) growing a 10 nm thick aluminum oxide passivation layer on the surface of the boron diffusion layer using the ALD method;

[0051] (7) depositing a 70 nm thick front silicon nitride layer on the surface of the aluminum oxide passivation layer by a PECVD method;

[0052] (8) depositing a 75 nm thick back silicon nitride layer on the surface of the p-type polysilicon layer by using a PECVD method;

[0053] (9) Back metal grid lines and front metal grid lines are formed on the surface of the back silicon nitride layer and the front silicon nitride layer respectively by screen printing, wherein the width of the main grid line in the front metal grid line is 0.6 mm, the number of the main grid lines is 9, the width of the secondary grid line is 35 μm, and the number of the secondary grid lines is 100; the width of the main grid line in the back metal grid line is 0.6 mm, the number of the main grid lines is 9, the width of the secondary grid line is 35 μm, and the number of the secondary grid lines is 110.

[0054] Example 2

[0055] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 760°C, then cooled to 200°C, heated again to 550°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0056] Example 3

[0057] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 770°C, then cooled to 250°C, heated again to 570°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0058] Example 4

[0059] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 780°C, then cooled to 300°C, heated again to 600°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0060] Example 5

[0061] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 785°C, then cooled to 350°C, heated again to 630°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0062] Example 6

[0063] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 790°C, then cooled to 400°C, heated again to 590°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0064] Example 7

[0065] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 800°C, then cooled to 600°C, heated again to 650°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0066] Example 8

[0067] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 760°C, then cooled to 620°C, heated again to 650°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0068] Example 9

[0069] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 760°C, then cooled to 180°C, heated again to 550°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0070] Example 10

[0071] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 760°C, then cooled to 200°C, heated again to 600°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0072] Embodiment 11

[0073] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 760°C, then cooled to 200°C, heated again to 500°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0074] Comparative Example 1

[0075] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is heated to 760°C, then cooled to 200°C, heated again to 900°C and then cooled to room temperature to obtain a passivated contact solar cell.

[0076] Comparative Example 2

[0077] This embodiment provides a heat treatment method for a passivated contact solar cell. The cell prepared in Example 1 is sintered. The sintering process includes: placing the cell into a sintering furnace, heating it to 760° C. and then cooling it down to room temperature to obtain a passivated contact solar cell.

[0078] Comparative Example 3

[0079] The present embodiment provides a heat treatment method for a passivated contact solar cell, wherein the cell prepared in Example 1 is sintered and hydrogen passivated to obtain the passivated contact solar cell, wherein the sintering process comprises: placing the cell into a sintering furnace, heating it to 760°C and then cooling it down to room temperature; the hydrogen passivation process comprises performing three stages of electrical injection on the cell at one time, wherein the first stage: the electrical injection current is 10-12A, and the electrical injection time is 300-450s; the second stage: the electrical injection current is 16-18A, the electrical injection temperature is 260-285°C, and the electrical injection time is 1500-2250s; the third stage: the electrical injection current is 14-16A, the electrical injection temperature is 240-275°C, and the electrical injection time is 600-900s.

[0080] The passivated contact solar cells prepared in Examples 1-11 and Comparative Examples 1-3 were tested, and the corresponding IV detection graphs were drawn. The short-circuit current density, open-circuit voltage and photoelectric conversion efficiency of the cells were calculated from the graphs. Specific data are shown in Table 1.

[0081] Table 1

[0082]

[0083]

[0084] From the data in Table 1, we can see that:

[0085] (1) Example 8 and Example 9 adjusted the temperature of the first cooling heat treatment, wherein Example 8 exceeded the upper limit of the preferred range of the present application, while Example 9 exceeded the lower limit of the preferred range of the present invention. According to the data in Table 1, it can be seen that compared with Example 2, the short-circuit current density, open-circuit voltage and photoelectric conversion efficiency of Example 8 and Example 9 are lower. This is because, during the first cooling heat treatment, since certain temperature conditions are still retained, the remaining hydrogen ions in the matrix are redistributed, which has a certain passivation effect on the defects in the body. However, the temperature of the first cooling heat treatment cannot be too high, otherwise it will cause a large amount of hydrogen to escape and will not enter the polysilicon layer or the silicon matrix; the temperature of the first cooling heat treatment cannot be too low, otherwise it will affect the passivation effect of the second heating heat treatment.

[0086] (2) Example 10 and Example 11 adjusted the temperature of the second heating heat treatment, wherein Example 10 exceeded the upper limit of the preferred range of the present application, while Example 11 exceeded the lower limit of the preferred range of the present invention. According to the data in Table 1, it can be seen that compared with Example 2, the short-circuit current density, open-circuit voltage and photoelectric conversion efficiency of Example 10 and Example 11 are lower. This is because the second heating heat treatment can allow the hydrogen ions in the hydrogen-rich silicon nitride layer on the back of the passivated contact structure battery to enter the polysilicon layer, further passivating the defects in the polysilicon layer. At the same time, some hydrogen ions enter the silicon substrate through the polysilicon layer and the tunneling layer, further passivating the defects in the silicon substrate. However, if the temperature is too high, hydrogen will escape instead of entering the polysilicon layer. If the temperature is too low, the amount of hydrogen will be insufficient, and the passivation effect cannot be achieved.

[0087] (3) The difference between Comparative Example 1 and Example 2 is that the peak temperature of the second temperature increase heat treatment in Comparative Example 1 is higher than the peak temperature of the first temperature increase heat treatment, which causes the short-circuit current density, open-circuit voltage and photoelectric conversion efficiency of the prepared passivated contact solar cell to be significantly reduced. This is because the peak temperature of the first temperature increase heat treatment is too high, a large number of hydrogen ions escape, and the passivation effect is limited. Therefore, the temperature needs to be controlled during the second temperature increase heat treatment. The temperature cannot be too high, otherwise the hydrogen ions will further escape and the passivation effect cannot be achieved.

[0088] (4) The difference between Comparative Example 2 and Example 2 is that Comparative Example 2 only uses one heating and cooling sintering process, while Example 2 uses two staged heat treatments, which results in a significant reduction in the short-circuit current density, open-circuit voltage and photoelectric conversion efficiency of the prepared passivated contact solar cell. The first heating and cooling heat treatment process in Example 2 is the same as the sintering process of Comparative Example 2, and a second heating and cooling heat treatment process is added on this basis. Through the second heating and cooling heat treatment process, the hydrogen ions in the hydrogen-rich silicon nitride layer on the back of the passivated contact structure battery can enter the polysilicon layer, further passivating the defects in the polysilicon layer, and at the same time, some hydrogen ions enter the silicon substrate through the polysilicon layer and the tunneling layer, further passivating the defects in the silicon substrate. During the second cooling heat treatment process, the hydrogen ions in the silicon substrate and the polysilicon layer are redistributed for a second time.

[0089] (5) The difference between Comparative Example 3 and Example 2 is that Comparative Example 3 adopts the conventional sintering + hydrogen passivation treatment scheme, while Example 2 adopts two staged heat treatments instead of "sintering + hydrogen passivation". It can be seen from the data in Table 1 that the various properties of the passivated contact solar cells prepared by these two preparation schemes are not much different. Therefore, it can be considered that the use of staged heat treatment can replace the conventional hydrogen passivation treatment.

[0090] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A heat treatment method for passivated contact solar cells, characterized in that: The heat treatment method comprises: performing a heating treatment and a cooling treatment on the battery cells alternately in sequence, wherein the peak temperature of each heating treatment step is gradually reduced; The heat treatment method specifically comprises: performing a first heating treatment, a first cooling treatment and a second heating treatment on the battery cell in sequence and then cooling the temperature to room temperature; The peak temperature of the first heating treatment is higher than the peak temperature of the second heating treatment; The peak temperature of the first heating treatment is 760-800°C; The peak temperature of the first cooling heat treatment is 200-600°C; The peak temperature of the second heating treatment is 550-650°C.

2. The heat treatment method according to claim 1, characterized in that The peak temperature of the first cooling heat treatment is 350-450°C.

3. The heat treatment method according to claim 1, characterized in that: The peak temperature of the second heating treatment is 590-610°C.

4. A heat treatment device for performing the heat treatment method according to any one of claims 1 to 3, characterized in that: The heat treatment device comprises a sintering furnace.

5. A method for preparing a passivated contact solar cell, characterized in that: The preparation method comprises: (1) Texturing the surface of the silicon wafer, diffusing boron on the surface of the silicon wafer and removing the borosilicate glass on the back; (2) Depositing a back tunneling oxide layer and a back doped polysilicon layer on the back of the silicon wafer in sequence; (3) Clean the front side of the silicon wafer on one side to remove the phosphorus silicon glass and polysilicon coating on the front side; (4) Depositing a front passivation film and a front anti-reflection layer on the front side of the silicon wafer in sequence; (5) Depositing a back anti-reflection layer on the back of the silicon wafer; (6) Forming metal grid lines on the surface of the back anti-reflection layer and the front anti-reflection layer by screen printing to obtain a solar cell; (7) heat treating the cell to obtain the passivated contact solar cell; The heat treatment in step (7) adopts the heat treatment method described in any one of claims 1 to 3.

6. A passivated contact solar cell, characterized in that: The passivated contact solar cell is prepared by the preparation method described in claim 5.

7. The passivated contact solar cell according to claim 6, characterized in that: The solar cell comprises a silicon wafer, the back side of which is sequentially stacked with a back tunneling oxide layer, a back doped polysilicon layer, a back anti-reflection layer and a back metal grid line, and the back metal grid line is in passivation contact with a back passivation film.

8. The passivated contact solar cell according to claim 7, characterized in that: The front side of the silicon wafer is sequentially stacked with a boron diffusion layer, a front side passivation film, a front side anti-reflection layer and a front side metal grid line.

Citation Information

Patent Citations

  • Fabrication method of n-type solar cell

    CN107863417A

  • Preparation method of n-shaped double-surface solar cell

    CN108039374A

  • Solar cell sintering method and preparation method, solar cell and sintering furnace

    CN110459469A

  • TOPCon solar cell and manufacturing method thereof

    CN111987182A

  • Preparation method of passivated emitter and rear side cell (PERC) and passivated emitter and rear total diffused (PERT) solar cells

    CN105097961A