Lead smelting method using oxygen-enriched top-blown furnace

By controlling the temperature and thickness of the foam slag in the oxygen-rich top blower, the problem of foam slag generated by changes in the slag viscosity in the Isa furnace is solved, and the stability and energy consumption of the lead smelting process are reduced, which is shortened. Smelting cycle.

CN115948661BActive Publication Date: 2024-11-22YUNNAN CHIHONG ZN & GE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211468735.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-11-22
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

During the lead smelting process, the existing Isa furnace produces foam slag due to changes in the slag viscosity, which affects the process stability and requires frequent adjustment of process parameters, resulting in a long smelting cycle, high energy consumption and safety and environmental protection risks.

Method used

Mix lead concentrate, lead oxide, lead sulfate slag, quartz sand and crushed coal and melt it in an oxygen-rich top blower. By controlling the temperature and thickness of the foam slag, the penetration rate of high-temperature reduction gas is suppressed and the heat utilization efficiency is improved. and the contact area between the reducing gas and the slag promotes the aggregation and precipitation of lead liquid.

Benefits of technology

The lead smelting cycle is shortened, the comprehensive energy consumption of smelting is reduced, and the process stability is improved, reducing the risk of foam slag being out of control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115948661B_ABST
    Figure CN115948661B_ABST
Patent Text Reader

Abstract

The present invention relates to a lead smelting method of an oxygen-enriched top-blown furnace, and belongs to the technical field of lead ore smelting. The present invention mixes lead concentrate, lead oxide ore, lead sulfate slag, quartz sand, and crushed coal, and continuously adds them into an oxygen-enriched top-blown furnace for smelting, forms foam slag on the lead slurry, controls the viscosity of the foam slag by controlling the temperature of the foam slag, and thus controls the height of the foam slag, so that (side blowing) after the foam is generated, the penetration speed of the high-temperature reducing gas is suppressed, the diffusion law of the airflow is disrupted, the heat utilization efficiency and the contact area between the reducing gas and the slag are improved, bubbles are formed in the molten pool, the condensation and precipitation of the reduced lead droplets are accelerated, the reduction speed is increased, the smelting cycle is shortened, and the comprehensive energy consumption of smelting is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lead ore smelting, and in particular relates to a lead smelting method using an oxygen-enriched top-blown furnace. Background Art

[0002] The Isa furnace is a fixed vertical cylindrical steel shell lined with magnesia-chrome bricks. A spray gun is installed on the top of the furnace. Materials are added to the furnace from the charging port on the top of the furnace. Smelting is a continuous process. Oxidation reaction takes place in the furnace, directly producing a portion of crude lead and the rest of the lead-rich slag. During the continuous production process, as materials are continuously added, the height of the slag pool continues to rise. After reaching a certain height, the discharge operation is carried out, and the height of the slag pool continues to decrease until it reaches the lowest point required by the process. In actual production practice, due to changes in raw material composition, temperature and other factors that affect the viscosity of the slag, it is necessary to frequently adjust the process control parameters to suppress the generation of foam slag to maintain normal production. In the process of adjusting the process control parameters, the properties of the slag will change, resulting in the generation of foam slag. In severe cases, measures must be taken to deal with it. If it is not handled in time, the foam slag will be out of control and overflow from the opening on the top of the furnace, causing serious safety and environmental problems. Therefore, the current process stabilizes the slag shape, adjusts the temperature, and suppresses the generation of foamy slag. During the production process, the addition of slag materials and lead oxide concentrate is stopped at any time to adjust the furnace temperature, resulting in low slag material processing capacity, long smelting cycle, and high comprehensive energy consumption of lead smelting. Summary of the invention

[0003] In order to solve the above problems, the present invention proposes a lead smelting method of an oxygen-enriched top-blown furnace. The present invention mixes lead concentrate, lead oxide ore, lead sulfate slag, quartz sand, and crushed coal, and continuously adds them into an oxygen-enriched top-blown furnace for smelting, forming foam slag on the lead slurry, and controlling the foam slag viscosity by controlling the foam slag temperature, thereby controlling the height of the foam slag, so that (side blowing) after the foam is generated, the penetration speed of the high-temperature reducing gas is suppressed, the diffusion law of the airflow is disrupted, the heat utilization efficiency and the contact area between the reducing gas and the slag are improved, bubbles are formed in the molten pool, the condensation and precipitation of the reduced lead droplets are accelerated, the reduction speed is increased, the smelting cycle is shortened, and the comprehensive energy consumption of smelting is reduced.

[0004] To achieve the above object, the present invention is implemented according to the following technical scheme:

[0005] The lead smelting method of the oxygen-enriched top-blown furnace specifically comprises the following steps:

[0006] 1) 10-30 t / h of lead concentrate, 10-15 t / h of lead oxide ore, 15-20 t / h of lead sulfate slag, 1.5-3 t / h of quartz sand and 1-2 t / h of crushed coal are mixed and continuously added into an oxygen-enriched top-blown furnace for smelting, and the addition of lead concentrate and quartz sand is stopped when 80% of the materials added in the smelting cycle, and lead slurry and foam slag floating on the lead slurry are formed in the oxygen-enriched top-blown furnace;

[0007] 2) Continue to add lead sulfate slag and lead oxide ore, and adjust the process air volume: 10800~11880Nm 3 / h, oxygen volume: 2300~3600Nm 3 / h, oxygen enrichment concentration: 29-36% and pulverized coal feed rate of 0.8-1.3t / h, control the furnace atmosphere and molten pool temperature at 900-950℃ for continuous smelting until all the lead sulfide in the lead concentrate is reacted;

[0008] 3) Control the temperature in the oxygen-enriched top-blown furnace at 900-950°C for continuous smelting, so that the unreacted materials in the molten pool can fully react, the lead metal can be reduced in the slag, and the low-melting-point raw materials can be gradually separated from the foam slag layer;

[0009] 4) Raise the temperature in the oxygen-enriched top-blown furnace to 950-1050°C, reduce the viscosity of the slag, and completely melt the foamy slag into metallurgical furnace slag;

[0010] 5) After clarification for 0.3-0.5 hours, lead-rich slag is discharged from the slag outlet of the oxygen-enriched top-blown furnace.

[0011] Preferably, in step 1), the lead concentrate, lead oxide ore, lead sulfate slag, quartz sand and crushed coal are put into a granulator, mixed and granulated, and then put into an oxygen-enriched top-blown furnace.

[0012] Preferably, in step 1), the Ca / Si ratio of the material entering the furnace is 0.35-0.45, and the Si / Fe ratio is 0.7-9.0.

[0013] Preferably, in step 2), crushed coal is continuously added to control the thickness of the foamed slag to be 1-1.5 m.

[0014] Preferably, in step 3), crushed coal is continuously added to control the thickness of the foamed slag to be 0.5-1 m.

[0015] Preferably, the particle size of the crushed coal is 100-300 mm.

[0016] Beneficial effects of the present invention:

[0017] The present invention mixes lead concentrate, lead oxide ore, lead sulfate slag, quartz sand and crushed coal, and continuously adds the mixture into an oxygen-enriched top-blown furnace for smelting, so as to form foam slag on the lead slurry. The foam slag viscosity is controlled by controlling the foam slag temperature, thereby controlling the height of the foam slag, so that after the foam is generated (side blowing), the penetration speed of the high-temperature reducing gas is suppressed, the diffusion law of the airflow is disrupted, the heat utilization efficiency and the contact area between the reducing gas and the slag are improved, bubbles are formed in the molten pool, the condensation and precipitation of the reduced lead droplets are accelerated, the reduction speed is improved, the smelting cycle is shortened, and the comprehensive energy consumption of smelting is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. It is obvious that the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0019] Figure 1 It is the material distribution in the top-blown furnace during smelting of the present invention; DETAILED DESCRIPTION

[0020] In order to make the objectives, technical solutions and beneficial effects of the present invention clearer, the preferred embodiments of the present invention will be described in detail below to facilitate understanding by technicians. Specific embodiment:

[0022] 10-30t / h of lead concentrate, 10-15t / h of lead oxide ore, 15-20t / h of lead sulfate slag, 1.5-3t / h of quartz sand, and 1-2t / h of crushed coal with a particle size of 100-300mm are mixed and continuously added into an oxygen-enriched top-blown furnace for smelting. When 80% of the materials added in the smelting cycle are reached, the addition of lead concentrate and quartz sand is stopped, and lead slurry and foam slag floating on the lead slurry are formed in the oxygen-enriched top-blown furnace. The oxygen-enriched top-blown furnace is an Isa furnace. The smelting of the Isa furnace is a molten pool smelting. The spray gun is inserted into the inside of the molten pool. The lead-rich slag in the molten pool is a PbO-CaO-SiO2-FeO-ZnO slag type. The reaction distribution of the materials in the furnace is as follows: Figure 1 As shown, zone 1: at the outlet of the spray gun, it belongs to the combustion oxidation zone; the fuel burns rapidly in this zone, the lead sulfide concentrate undergoes a violent oxidation reaction, and releases a large amount of heat. The foamy slag inhibits the airflow penetration speed and regularity during the reaction process, allowing the high-temperature gas in the main reaction zone to diffuse to the secondary reaction zone, avoiding insufficient reaction in the secondary reaction zone, resulting in the accumulation of added materials, causing partial freezing of the molten pool, and then carrying out material reduction and temperature increase treatment).

[0023] Zone 2: This zone is a secondary reaction zone. The added charge flows toward the furnace wall along with the melt, the charge is preheated and melted, and a small amount of oxidation reaction occurs with the diffused oxygen.

[0024] Zone 3: Circulation flow zone, the charge and a small amount of bubbles in the injected gas flow downward from zone 2 to form a reflux cycle, and the residual oxygen in the bubbles fully reacts with the concentrate and coal. When passing through zone 1, it encounters a large number of bubbles and a strong oxidation slagging reaction occurs again.

[0025] Zone 4: Relatively static zone, enriched with crude lead, which is conducive to the separation of slag and lead.

[0026] As a preferred embodiment, the Ca / Si ratio of the materials fed into the furnace is 0.35-0.45, and the Si / Fe ratio is 0.7-9.0. During the smelting process, the composition control mainly detects the contents of SiO2, CaO and Fe. Si / Fe is generally about 0.8, and Ca / Si is generally about 0.4. The melting point of the slag is stabilized, and the reaction speed and temperature of the reaction zone are controlled. The viscosity of the slag is controlled by temperature, the surface tension of the molten pool is increased, and the time for the reaction gas to penetrate the molten pool is suppressed, so that the slag is foamy; if the Si / Fe ratio is too high, the slag tends to vitrify, the viscosity of the slag increases, and the melting point rises. Because Isa furnace smelting is an intensive smelting with violent reactions, inappropriate Si:Fe will cause the Fe3O4 in the slag to increase sharply, and the viscosity of the slag will increase rapidly. In severe cases, the gas fed into the molten pool and the gas generated by the reaction cannot be released in time, and the suffocation will expand sharply to a certain extent. Although the molten pool is surging, the tumbling effect is poor, and finally a large amount of slag is sprayed out of the feeding port and the spray gun port, forming serious foamy slag.

[0027] Continuously add lead sulfate slag and lead oxide ore, and adjust the process air volume: 10800~11880Nm 3 / h, oxygen volume: 2300~3600Nm 3 / h, oxygen enrichment concentration: 29-36% and pulverized coal feed rate of 0.8-1.3t / h, control the furnace atmosphere and molten pool temperature at 900-950℃ for continuous smelting until all the lead sulfide in the lead concentrate is reacted; continue to add crushed coal to control the thickness of the foam slag at 1-1.5m, lead sulfate slag decomposes violently at 900℃, and the molten pool temperature and reaction conditions can be indirectly judged by online monitoring of flue gas SO2 concentration; through the endothermic reaction of lead oxide ore, the slag temperature is stabilized during the oxygen enrichment process, and at the same time, the lead slag and lead oxide ore are decomposition reactions to produce gas, increase the amount of gas in the molten pool, and maintain the height of the foam slag during the gradual temperature increase process to make the air flow in the molten pool penetrate more fully. The viscosity of the slag is controlled by controlling the slag temperature. After the foam is generated (side blowing), the penetration speed of the high-temperature reducing gas is suppressed, the diffusion law of the airflow is disrupted, the heat utilization efficiency and the contact area between the reducing gas and the slag are improved, bubbles are formed in the molten pool, the coagulation and precipitation of the reduced lead droplets are accelerated, the reduction speed is increased, the smelting cycle is shortened, and the comprehensive energy consumption of smelting is reduced.

[0028]

[0029]

[0030] The temperature in the oxygen-enriched top-blown furnace is controlled at 900-950℃ for continuous smelting, so that the unreacted materials in the molten pool can fully react, the lead metal can be reduced in the slag, and the low-melting-point raw materials can be gradually separated from the foam slag layer; crushed coal is continuously added to control the thickness of the foam slag to 0.5-1m;

[0031] Increase the temperature in the oxygen-enriched top-blown furnace to 950-1050°C, reduce the viscosity of the slag, and completely melt the foamy slag into metallurgical furnace slag; clarify for 0.3-0.5 hours, and discharge the lead-rich slag from the slag outlet of the oxygen-enriched top-blown furnace.

[0032] Table of relationship between foam slag height and temperature

[0033]

[0034] Comparison table of original process and current process

[0035] Bed capacity t / m2.d One-time lead slag material quantity Smoke rate (%) Original process 39.8 20 22.5 Current technology 50.6 30 18.5

[0036] Preferably, the particle size of the crushed coal is 100-300mm, which matches the existing Isa furnace body (11m high). If the particle size of the crushed coal is too small, it is easy to burn above the slag. If the particle size is large, it cannot be dispersed after entering the molten pool, resulting in a concentrated reaction at the falling point.

[0037] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A lead smelting method using an oxygen-enriched top-blown furnace, characterized in that: The specific steps include: 1) 10-30 t / h of lead concentrate, 10-15 t / h of lead oxide ore, 15-20 t / h of lead sulfate slag, 1.5-3 t / h of quartz sand and 1-2 t / h of crushed coal are mixed and continuously added into an oxygen-enriched top-blown furnace for smelting. When 80% of the materials added during the smelting cycle are reached, the addition of lead concentrate and quartz sand is stopped, and lead slurry and foam slag floating on the lead slurry are formed in the oxygen-enriched top-blown furnace; 2) Continuously add lead sulfate slag and lead oxide ore, and adjust the process air volume: 10800-11880 Nm3 / h, oxygen volume: 2300-3600 Nm3 / h, oxygen enrichment concentration: 29-36% and lance pulverized coal feed rate of 0.8-1.3t / h, control the furnace atmosphere and molten pool temperature at 900-950℃ for continuous smelting until all the lead sulfide in the lead concentrate is reacted; 3) Control the temperature in the oxygen-enriched top-blown furnace at 900-950℃ for continuous smelting, so that the unreacted materials in the molten pool can fully react, the lead metal can be reduced in the slag, and the low-melting-point raw materials can be gradually separated from the foamy slag layer; 4) Raise the temperature in the oxygen-enriched top-blown furnace to 950-1050°C, reduce the viscosity of the slag, and completely melt the foamy slag into metallurgical furnace slag; 5) After clarification for 0.3-0.5 hours, lead-rich slag is discharged from the slag outlet of the oxygen-enriched top-blown furnace.

2. The lead smelting method of an oxygen-enriched top-blown furnace according to claim 1, characterized in that: In step 1), lead concentrate, lead oxide ore, lead sulfate slag, quartz sand and crushed coal are put into a granulator, mixed and granulated, and then put into an oxygen-enriched top-blown furnace.

3. The lead smelting method of an oxygen-enriched top-blown furnace according to claim 1, characterized in that: In step 1), the Ca / Si ratio of the materials entering the furnace is 0.35-0.45, and the Si / Fe ratio is 0.7-9.

0.

4. The lead smelting method of an oxygen-enriched top-blown furnace according to claim 1, characterized in that: In step 2), crushed coal is continuously added to control the thickness of the foam slag to be 1-1.5 m.

5. The lead smelting method of an oxygen-enriched top-blown furnace according to claim 1, characterized in that: In step 3), crushed coal is continuously added to control the thickness of the foam slag to be 0.5-1m.

6. A lead smelting method using an oxygen-enriched top-blown furnace according to any one of claims 1, 2, 3, 4 or 5, characterized in that: The particle size of crushed coal is 100-300mm.