Asymmetric catalyst of polymer-supported metal rhodium and synthesis method thereof
Through the design of asymmetric catalysts supported by polymer-supported metal rhodium, the problems of high cost and difficulty in recovery of homogeneous catalysts are solved, the catalytic efficiency and product purification are improved, and the application of single-atom catalysts in the field of asymmetric catalysis is realized.
Patent Information
- Application Number
- CN202310237055.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-12-24
- Estimated Expiration
- 2043-03-02
AI Technical Summary
Existing homogeneous catalysts are expensive in industrial applications and are difficult to recover. The subsequent separation and purification of reaction products are difficult, and single-atom catalysts are still in the exploration stage in the field of asymmetric catalysis.
A polymer-supported asymmetric catalyst of rhodium metal was developed, further with (4-vinyl group)-binaphthol monoesterification reaction of pivaloyl chloride, followed by bromine substitution and ester hydrolysis of liquid bromine, further with (4-vinyl group The coupling reaction of phenyl)boric acid and finally complex and copolymerize with (1,5-cyclooctadiene) rhodium chloride to produce a single-atom catalyst supported by polymer metal rhodium.
It improves the uniformity of the catalytic activity center, reduces the catalytic usage, prevents metal leaching, realizes continuous production, and simplifies the catalyst design and synthesis process.
Smart Images

Figure CN116284148B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic molecular catalysts, and in particular to an asymmetric catalyst of a polymer-loaded metal rhodium and a synthesis method thereof. Background Art
[0002] Transition metal asymmetric catalysis is one of the most important methods for constructing chiral molecules. With its many advantages such as high efficiency, excellent asymmetric selectivity, wide functional group tolerance and high scalability of products, it has become a research frontier and hotspot in the fields of chiral molecule synthesis and pharmaceutical research and development. However, most of the reactions reported so far are homogeneous catalytic systems. In their wider industrial applications, the chiral ligands of homogeneous catalysts are expensive and difficult to recycle; the subsequent separation and purification of reaction products are inconvenient (for example, catalyst metal residues and reduced product separation yield).
[0003] Single-atom catalysts combine the advantages of both homogeneous and heterogeneous catalysts and have become a research hotspot in synthetic chemistry. However, so far, single-atom catalysts are still in the exploratory stage in the field of asymmetric catalysis. Summary of the invention
[0004] In view of the prior art, the present invention develops an asymmetric catalyst of polymer-loaded metal rhodium and a synthesis method thereof.
[0005] Specifically, the present invention provides an asymmetric catalyst of a polymer-supported metal rhodium, characterized in that the structural formula of the asymmetric catalyst of a polymer-supported metal rhodium is:
[0006] Wherein, n1 is an integer from 10 to 100, n2 is an integer from 1 to 10, and n3 is 1.
[0007] Another object of the present invention is to provide a method for synthesizing an asymmetric catalyst of a polymer-supported metal rhodium, comprising at least the following steps:
[0008] Step 1, (S)-binaphthol and pivaloyl chloride undergo monoesterification reaction under the action of a basic catalyst to obtain an intermediate (S)-1;
[0009] Step 2, the intermediate (S)-1 reacts with liquid bromine to undergo bromine substitution reaction at the 6' position of another naphthol ring of the (S)-binaphthol, followed by quenching by adding an aqueous solution of NaHSO3. After quenching, the organic phase is extracted and concentrated, and the concentrate is subjected to an ester hydrolysis reaction to obtain the intermediate (S)-2;
[0010] Step 3, intermediate (S)-2 is further subjected to 4-vinylphenyl coupling reaction with (4-vinylphenyl)boronic acid at the 6'-bromine substituent position to obtain intermediate (S)-3;
[0011] Step 4, intermediate (S)-3, iminostilbene and phosphorus trichloride undergo a phosphoramidite reaction under the action of a basic catalyst to obtain monomer 1;
[0012] Step 5, monomer 1 and (1,5-cyclooctadiene)chlororhodium (I) dimer undergo complexation reaction, and the reaction solution after the reaction is filtered to obtain a monomer 2 solution;
[0013] Step 6, the monomer 2 solution undergoes copolymerization reaction with styrene and divinylbenzene under the action of a copolymerization catalyst and an initiator. After the reaction is completed, the reaction product is filtered, washed and dried to obtain the polymer-loaded metal rhodium asymmetric catalyst.
[0014] Furthermore, the process control of the monoesterification reaction is as follows: (S)-binaphthol and an alkaline catalyst are dissolved in a solvent, pivaloyl chloride is added dropwise at -5 to 5°C, and the temperature is raised to 20 to 30°C for reaction for 4 to 6 hours; wherein the molar ratio of (S)-binaphthol to pivaloyl chloride is 1:(1.0 to 1.01).
[0015] Furthermore, the process control of the bromine substitution reaction is as follows: dissolving the intermediate (S)-1 in a solvent, adding liquid bromine at -5 to 5°C, and keeping the reaction warm for 3 to 4 hours after the addition; wherein the molar ratio of the intermediate (S)-1 to the liquid bromine is 1:(1.8 to 2.2).
[0016] Furthermore, the process control of the ester hydrolysis reaction is as follows: adding a solvent and a strong alkaline solution to the concentrate, mixing, reacting at 20-30° C. for 2-3 hours, and then acidifying with a strong acid to a pH of 1-2.
[0017] Furthermore, the strong alkaline solution is at least one of potassium hydroxide, sodium hydroxide, sodium acetate, potassium acetate, sodium carbonate, sodium bicarbonate, and lithium hydroxide solution; and the concentration of the strong alkaline solution is 5-6 mol / L.
[0018] Furthermore, the strong acid solution is at least one of hydrochloric acid, sulfuric acid and nitric acid; and the concentration of the strong acid solution is 3 mol / L.
[0019] Furthermore, the process control of the coupling reaction is: the intermediate (S)-2, (4-vinylphenyl)boric acid, Pd(PPh3)4, K2CO3 and the solvent are evenly mixed, and heated to reflux for reaction for 10 to 14 hours under nitrogen protection; wherein the molar ratio of the intermediate (S)-2, (4-vinylphenyl)boric acid, K2CO3, and Pd(PPh3)4 is 1:(1.2 to 1.3):(2.5 to 3.5):0.03.
[0020] Furthermore, the process control of the phosphoramidation reaction is as follows: dissolve the alkaline catalyst and PCl3 in a solvent, add iminostilbene dropwise at -5 to 5°C, react at 20 to 30°C for 3 to 4 hours, then add the intermediate (S)-3 at -5 to 5°C, and react at 20 to 30°C for 18 to 20 hours; wherein the molar ratio of the intermediate (S)-3, iminostilbene, PCl3, and alkaline catalyst is 1:1:(1 to 1.05):(5 to 7).
[0021] Furthermore, the process control of the complex reaction is as follows: the solvent, monomer 1 and (1,5-cyclooctadiene)chlororhodium (I) dimer are uniformly mixed under nitrogen protection, and reacted at 20-30° C. for 2-3 hours to obtain a monomer 2 solution; wherein the molar ratio of monomer 1 to (1,5-cyclooctadiene)chlororhodium (I) dimer is 1:(0.5-0.52).
[0022] Furthermore, the process control of the copolymerization reaction is as follows: after the monomer 2 solution, divinylbenzene, azobisisobutyronitrile, styrene and solvent are uniformly mixed, the temperature is raised to 55-65° C., and the mixture is reacted for 36 hours under stirring at 500-700 rpm; wherein the molar ratio of monomer 2, divinylbenzene and styrene is 1:(1-10):(10-100), and the molar amount of azobisisobutyronitrile is 1-5% of the molar amount of monomer 2.
[0023] Furthermore, the alkaline catalyst is at least one of Et3N, N,N-diisopropylethylamine, pyridine and piperidine.
[0024] Furthermore, the solvent is at least one of acetonitrile, toluene, dichloromethane, tetrahydrofuran, acetone, ethyl acetate, methanol, ethanol, and petroleum ether.
[0025] In summary, the present invention has the following beneficial effects: the present invention synthesizes a polymer-supported metal rhodium single-atom asymmetric catalyst, designs and synthesizes a supported chiral catalyst based on the coordination characteristics of the metal and the ligand, fixes the coordination ratio of the metal and the supported ligand, improves the loading site, reduces the steric hindrance at the active center, and prevents the metal leaching problem caused by the extrusion between polymers. The uniformity of the catalytic active center of the single atom improves the catalytic efficiency, reduces the catalytic dosage, and realizes continuous production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0027] Figure 1 is the monomer 1 in Example 1 of the present invention 1 HNMR spectrum.
[0028] Figure 2 is the monomer 1 in Example 1 of the present invention 13 CNMR image.
[0029] Figure 3 is the monomer 1 in Example 1 of the present invention 31 PNMR diagram.
[0030] Figure 4 This is the IR graph of monomer 1 in Example 1 of the present invention.
[0031] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials and reagents used in the following examples are all commercially available unless otherwise specified. The quantitative tests in the following examples were performed in triplicate, and the data are the average or average ± standard deviation of the triplicate experiments.
[0034] In addition, the "and / or" in the full text includes three solutions. Taking A and / or B as an example, it includes technical solution A, technical solution B, and a technical solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.
[0035] Example 1
[0036] A method for synthesizing a polymer-supported asymmetric catalyst of metallic rhodium, the specific steps are as follows:
[0037] Step 1: (S)-binaphthol and pivaloyl chloride undergo a monoesterification reaction under the action of an alkaline catalyst to obtain an intermediate (S)-1, specifically:
[0038] To a solution of (S)-1,1'-bis(2-naphthol) (2.86 g, 10 mmol) and Et3N (3.03 g, 30 mmol) in acetonitrile (50 mL) was added pivaloyl chloride (1.22 g, 10.1 mmol) dropwise at 0°C, and the mixture was then warmed to 25°C and stirred for 5 hours.
[0039] After the reaction, the product was diluted with ether and washed with HCl aqueous solution (1 mol / L, 30 mL), saturated NaHCO3 (50 mL) and brine (50 mL) in sequence. The organic layer was dried over Na2SO4 and concentrated, and then purified by silica gel flash column chromatography to obtain intermediate (S)-1 as a white solid. The specific reaction equation is as follows:
[0040]
[0041] Step 2, the intermediate (S)-1 reacts with liquid bromine to undergo bromine substitution reaction at the 6' position of another naphthol ring of the (S)-binaphthol, and then NaHSO3 aqueous solution is added to quench, and after the quenching is completed, the organic phase is extracted and concentrated, and the concentrate is subjected to ester hydrolysis reaction to obtain the intermediate (S)-2, specifically:
[0042] At 0°C, liquid bromine (3.2 g, 20 mmol) was slowly added to a mixed solution of acetonitrile (MeCN) and toluene (toluene) containing intermediate (S)-1 (3.7 g, 10 mmol), and the volume of acetonitrile and toluene was 30 mL each; then the reaction mixture was stirred at 0°C for 3 h and quenched with an aqueous NaHSO3 solution (3 mol / L, 10 mL). After quenching, 100 mL of ether was added, and the organic phase was separated and concentrated.
[0043] Methanol (MeOH) (20 mL) and KOH solution (5 mol / L, 20 mL) were added to the residue obtained by concentration of the organic phase. The resulting mixture was stirred at 25° C. for 2 h and then acidified to pH=1 with 3 mol / L HCl.
[0044] After the reaction was completed, ethyl acetate (100 mL) was added to the product, and the organic phase was washed with saturated NaHCO3 and brine, dried over Na2SO4 and concentrated. The crude product was purified by silica gel flash column chromatography to obtain a white solid intermediate (S)-2. The reaction equation is as follows:
[0045]
[0046] Step 3, intermediate (S)-2 and (4-vinylphenyl)boronic acid further undergo 4-vinylphenyl coupling reaction at the 6'-bromine substituent position to obtain intermediate (S)-3, specifically:
[0047] A solution (20 mL) of (4-vinylphenyl)boric acid (1.22 g, 1.25 equiv.), Pd(PPh3)4 (227 mg, 3 mol%), intermediate (S)-2 (2.4 g, 6.57 mmol) and K2CO3 (1 mol / L) was added to a mixed solvent of tetrahydrofuran (THF) (96 mL) + H2O (20 mL), and refluxed at 85°C under nitrogen for 12 h; then cooled to room temperature, and the mixture was extracted three times with dichloromethane (40 mL).
[0048] The organic phases were combined, washed with brine, dried over magnesium sulfate and concentrated, and then purified by silica gel column chromatography to obtain intermediate (S)-3 as a white solid. The reaction equation is as follows:
[0049]
[0050] Step 4, intermediate (S)-3, iminostilbene, and phosphorus trichloride undergo a phosphoramidite reaction under the action of an alkaline catalyst to obtain monomer 1, specifically:
[0051] At 0°C, Et3N (5mmol) and PCl3 (1mmol) were dissolved in dichloromethane (37mL) and stirred evenly. A solution containing iminostilbene (1mmol) (solvent: dichloromethane) was added dropwise to the reaction mixture at 0°C, and the mixture was stirred at 25°C for 4h. Intermediate (S)-3 (1mmol) was slowly added to the reaction mixture at 0°C, and the suspension was stirred at room temperature for 18h; the suspension was then diluted in DCM (8mL) and filtered on neutral alumina, the solution was concentrated and purified by silica gel flash chromatography to obtain monomer 1 as a white solid, and the reaction equation is as follows:
[0052]
[0053] Characterization of Monomer 1:
[0054] Mp:127-130℃.
[0055] R f (n-pentane:ethyl acetate 20:1)=0.61.
[0056] 11H NMR (400 MHz, Chloroform-d) δ 8.35 - 8.10 (m, 2H), 8.00 (dd, J = 49.2, 8.1 Hz, 1H), 7.82 (dd, J = 20.3, 8.0 Hz, 3H), 7.70 - 7.48 (m, 7H), 7.39 (dt, J = 19.0, 8.7 Hz, 7H), 7.11 (q, J = 11.2 Hz, 4H), 6.92 (dt, J = 18.9, 9.9 Hz, 1H), 6.73 (dt, J = 14.1, 7.3 Hz, 1H), 5.96 (dd, J = 17.8, 8.0 Hz, 1H), 5.45 (dd, J = 11.1, 6.7 Hz, 1H). As Figure 1 shown.
[0057] 13 13C NMR (101 MHz, Chloroform-d) δ 150.37 (dd, J = 13.9, 7.9 Hz), 149.07 (d, J = 5.9 Hz), 143.24, 143.00, 142.71, 140.18 (d, J = 3.3 Hz), 137.20, 136.86 (d, J = 5.2 Hz), 136.78 - 136.34 (m), 135.45, 133.11, 132.37 (d, J = 8.5 Hz), 132.02, 131.77 (d, J = 6.0 Hz), 131.62, 130.95, 130.77, 130.49, 129.54 (d, J = 8.0 Hz), 129.32 (t, J = 7.1 Hz), 128.91 (d, J = 9.0 Hz), 128.62 (d, J = 9.6 Hz), 128.23, 127.97, 127.74, 127.61 - 127.24 (m), 126.52 (d, J = 6.1 Hz), 126.12 (d, J = 4.6 Hz), 125.73 (d, J = 9.5 Hz), 125.25 (d, J = 5.2 Hz), 124.70, 124.50 (t, J = 4.6 Hz), 122.91, 122.46, 122.25, 121.78, 121.35, 114.24. As Figure 2 shown.
[0058] 31 31P NMR (162 MHz, Chloroform-d) δ 137.91 (d, J = 9.1 Hz). As Figure 3 shown.
[0059] Infrared spectrum IR: v 2970.39, 1589.27, 1494.63, 1465.08, 1331.94, 1231.07, 1073.94, 948.02, 822.91, 779.75, 749.00, 696.29, 545.71. Figure 4 shown.
[0060] HRMS(ESI)calcd for C 42 H 29 NO2P+ + [(M+H) + ]610.1930, found 610.1932.
[0061] Step 5, monomer 1 and (1,5-cyclooctadiene)chlororhodium (I) dimer undergo complexation reaction, and the reaction solution after the reaction is filtered to obtain a monomer 2 solution, specifically:
[0062] Under nitrogen protection, monomer 1 (0.1 mmol) and (1,5-cyclooctadiene) rhodium chloride (I) dimer (0.05 mmol) were mixed evenly and reacted in toluene (3.5 mL) at 25°C for 2 h to obtain monomer 2 solution. The reaction equation is as follows:
[0063]
[0064] Step 6, the monomer 2 solution is copolymerized with styrene and divinylbenzene under the action of a copolymerization catalyst and an initiator. After the reaction is completed, the reaction product is filtered, washed and dried to obtain the polymer-supported metal rhodium asymmetric catalyst, specifically:
[0065] In a nitrogen environment, the monomer 2 solution obtained in step 5 was filtered, and deionized water (degassed for 3h under a nitrogen flow) (1.5mL), divinylbenzene (DVB) (5equiv), azobisisobutyronitrile (AIBN) (2mol%), and styrene (50equiv) were added; then, the mixture was stirred at room temperature for 30 minutes. The temperature was then raised to 60°C, and the reaction mixture was vigorously stirred at 600rpm for 36h. The resulting polymer was filtered and washed several times with hot water (50°C), then washed with methanol, ethanol and acetone, and then dried under reduced pressure at 40°C, and then further ground into powder with a mortar, and the powder was further washed several times with acetonitrile to obtain a yellow powder product, and the reaction equation is as follows.
[0066]
[0067] The product was tested twice in parallel by ICP-OES, and the results are as follows:
[0068] ICP-OES: Rh: 9913.07mg / kg,
[0069] ICP-OES: Rh: 9900.32mg / kg,
[0070] ICP-OES: Rh (average): 9906.7 mg / kg.
[0071] In summary, the present invention synthesizes a polymer-supported metal rhodium single-atom asymmetric catalyst, designs and synthesizes a supported chiral catalyst based on the coordination characteristics of the metal and the ligand, fixes the coordination ratio of the metal and the supported ligand, improves the loading site, reduces the steric hindrance at the active center, and prevents the metal leaching problem caused by the extrusion between polymers. The uniformity of the catalytic active center of the single atom improves the catalytic efficiency, reduces the catalytic dosage, and realizes continuous production.
[0072] Comparative Example 1
[0073] The difference between Comparative Example 1 and Example 1 is that the iminostilbene in step 4 is replaced by
[0074] Although the product prepared in Comparative Example 1 can load metal rhodium, the obtained polymer loaded with metal rhodium has no conversion rate in the same catalytic experiment, and therefore does not have catalytic performance.
[0075] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for synthesizing an asymmetric catalyst of a polymer-supported metal rhodium, characterized in that: At least the following steps are included: Step 1, (S)-binaphthol and pivaloyl chloride undergo monoesterification reaction under the action of a basic catalyst to obtain an intermediate (S)-1; Step 2, the intermediate (S)-1 reacts with liquid bromine to undergo bromine substitution reaction at the 6' position of another naphthol ring of the (S)-binaphthol, followed by quenching by adding an aqueous solution of NaHSO3. After quenching, the organic phase is extracted and concentrated, and the concentrate is subjected to an ester hydrolysis reaction to obtain the intermediate (S)-2; Step 3, intermediate (S)-2 is further subjected to 4-vinylphenyl coupling reaction with (4-vinylphenyl)boronic acid at the 6'-bromine substituent position to obtain intermediate (S)-3; Step 4, intermediate (S)-3, iminostilbene and phosphorus trichloride undergo a phosphoramidite reaction under the action of a basic catalyst to obtain monomer 1; Step 5, monomer 1 and (1,5-cyclooctadiene)chlororhodium (I) dimer undergo complexation reaction, and the reaction solution after the reaction is filtered to obtain a monomer 2 solution; Step 6, the monomer 2 solution is copolymerized with styrene and divinylbenzene under the action of a copolymerization catalyst and an initiator. After the reaction is completed, the reaction product is filtered, washed and dried to obtain the polymer-loaded metal rhodium asymmetric catalyst; The process control of the copolymerization reaction is as follows: after the monomer 2 solution, divinylbenzene, azobisisobutyronitrile, styrene and solvent are uniformly mixed, the temperature is raised to 55-65° C., and the mixture is stirred at 500-700 rpm for 36 hours; wherein the molar ratio of monomer 2, divinylbenzene and styrene is 1:(1-10):(10-100), and the molar amount of azobisisobutyronitrile is 1-5% of the molar amount of monomer 2; The alkaline catalyst is at least one of Et3N, N,N-diisopropylethylamine, pyridine and piperidine.
2. The method for synthesizing an asymmetric catalyst of a polymer-supported metal rhodium according to claim 1, characterized in that: The process control of the monoesterification reaction is as follows: (S)-binaphthol and an alkaline catalyst are dissolved in a solvent, pivaloyl chloride is added dropwise at -5 to 5°C, and the temperature is raised to 20 to 30°C for reaction for 4 to 6 hours after the addition is completed; wherein the molar ratio of (S)-binaphthol to pivaloyl chloride is 1:(1.0 to 1.01).
3. The method for synthesizing a polymer-supported asymmetric catalyst of metal rhodium according to claim 1, characterized in that: The process control of the bromine substitution reaction is as follows: dissolving the intermediate (S)-1 in a solvent, adding liquid bromine at -5 to 5°C, and keeping the reaction warm for 3 to 4 hours after the addition; wherein the molar ratio of the intermediate (S)-1 to the liquid bromine is 1:(1.8 to 2.2).
4. The method for synthesizing an asymmetric catalyst of a polymer-supported metal rhodium according to claim 1, characterized in that: The process control of the ester hydrolysis reaction is as follows: adding a solvent and a strong alkaline solution to the concentrate and mixing them evenly, reacting at 20-30° C. for 2-3 hours, and then acidifying with a strong acid to a pH of 1-2.
5. The method for synthesizing a polymer-supported asymmetric catalyst of metal rhodium according to claim 1, characterized in that: The process control of the coupling reaction is: the intermediate (S)-2, (4-vinylphenyl)boric acid, Pd(PPh3)4, K2CO3 and the solvent are mixed evenly, and heated to reflux for reaction for 10 to 14 hours under nitrogen protection; wherein the molar ratio of the intermediate (S)-2, (4-vinylphenyl)boric acid, K2CO3, and Pd(PPh3)4 is 1:(1.2 to 1.3):(2.5 to 3.5):0.
03.
6. The method for synthesizing a polymer-supported asymmetric catalyst of metal rhodium according to claim 1, characterized in that: The process control of the phosphoramidation reaction is as follows: dissolving the alkaline catalyst and PCl3 in a solvent, adding iminostilbene dropwise at -5 to 5°C, reacting at 20 to 30°C for 3 to 4 hours, then adding the intermediate (S)-3 at -5 to 5°C, reacting at 20 to 30°C for 18 to 20 hours; wherein the molar ratio of the intermediate (S)-3, iminostilbene, PCl3, and the alkaline catalyst is 1:1:(1 to 1.05):(5 to 7).
7. The method for synthesizing a polymer-supported rhodium asymmetric catalyst according to claim 1, characterized in that: The process control of the complex reaction is as follows: the solvent, monomer 1 and (1,5-cyclooctadiene)chlororhodium (I) dimer are uniformly mixed under nitrogen protection, and reacted at 20-30° C. for 2-3 hours to obtain a monomer 2 solution; wherein the molar ratio of monomer 1 to (1,5-cyclooctadiene)chlororhodium (I) dimer is 1:(0.5-0.52).
8. A polymer-supported asymmetric catalyst of metallic rhodium, characterized in that: The polymer-supported rhodium metal asymmetric catalyst is prepared by the synthesis method described in any one of claims 1-7.