A processing technology of coordination complex fluorine-free waterproof nylon fabric
Through the covalent bond reaction between fluorine-free waterproofing agents and acidic metal complex dyes, the environmental and human hazard problems caused by fluorine-containing waterproofing agents are solved, the safe production and excellent performance of fluorine-free waterproof nylon fabrics are realized, and the fabrics are ensured during use. safety and waterproof effect.
Patent Information
- Application Number
- CN202211101027.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-09-09
AI Technical Summary
In the existing technology, the use of fluorine-containing waterproofing agents to process textiles will produce toxic intermediates, endangering the environment and human health, and there are potential safety hazards during use.
The fluorine-free waterproofing agent and acidic metal complex dyes are used for covalent bond coordination reaction, and the fluorine-free waterproof nylon fabric is processed by double padding. The fluorine-free waterproof nylon fabric is combined with citric acid finishing liquid for drying and shaping to ensure that the fabric is in the production and use process. security in.
The production of perfluorooctanoic acid and perfluorooctane sulfonate is avoided during the production process. The fabric is safe and non-toxic, and has excellent waterproof performance and wet rubbing fastness.
Smart Images

Figure CN116289266B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printing and dyeing, and in particular to a processing technology of coordinated complex fluorine-free waterproof nylon fabric. Background Art
[0002] With the rapid development of global science and technology and the continuous improvement of living standards, people's demand for functional textiles is also increasing, including textiles with waterproof functions. In the existing technology, textiles with waterproof functions are all processed using waterproofing agents containing fluorine compounds. During the processing of fluorine-containing waterproof textiles, intermediates perfluorooctanoic acid and perfluorooctane sulfonic acid will appear. The intermediates are ecotoxic, and fluorine-containing waterproof textiles will also cause harm to the human body and the environment during use. Therefore, it is necessary to develop a fluorine-free waterproof textile. Summary of the invention
[0003] The technical problem to be solved by the present invention is to solve the deficiencies in the prior art and provide a processing technology for a coordination complex fluorine-free waterproof nylon fabric which is harmless to human body and environment.
[0004] The technical scheme adopted by the present invention is a processing technology of a coordination complex fluorine-free waterproof nylon fabric, which includes the following steps: Step 1: Material collection: Select nylon fabric made of 1D-20D nylon filaments, and perform quality inspection on the selected nylon fabric; Step 2: Tension-free desizing: Desizing the selected nylon fabric with a tension-free desizing machine; Step 3: Rolling, stacking and dyeing: The nylon fabric treated in step 2 is rolled up and stacked with a rolling machine, and the rolled and stacked fabric is dyed with a dyeing machine, and the dye in the dyeing machine is an acidic metal complex dye; Step 4: Fluorine-free cleaning and detection: The nylon fabric treated in step 3 is cleaned with a fluorine-free soap detergent to remove surface residues; The nylon fabric with the surface residue removed is checked with a magnifying glass with a magnification of 50-100 times to see whether the surface residues are removed. Clean; Step 5: Fluorine-free waterproof finishing: A drying machine with a front double dipping and rolling tank is used, the first rolling tank contains citric acid finishing liquid, the citric acid finishing liquid includes citric acid and the rest is water, the content of citric acid is 0.1-0.2g in 1000g water, the nylon fabric treated in step 4 is rolled through the first rolling tank, and the pH value of the citric acid finishing liquid in the first rolling tank is adjusted to 4-5 by citric acid and sodium citrate; the second rolling tank contains fluorine-free waterproof agent finishing liquid, the tank temperature is 40-50℃, the nylon fabric is rolled through the second rolling tank containing fluorine-free waterproof agent finishing liquid, the fluorine-free waterproof agent finishing liquid and the acidic metal complex dye undergo covalent bond coordination reaction; the nylon fabric passing through the second rolling tank is dried; Step 6: Setting: The nylon fabric treated in step 5 is set by a setting machine.
[0005] The nylon fabric in step 1 of the present invention is made of 7D-20D nylon filaments, and the gram weight of the nylon fabric does not exceed 40g / m 2 .
[0006] Step 2 of the present invention also includes a refining process: the nylon fabric after desizing treatment is put into a refining process, and the refining process adopts a refining finishing liquid for refining. 1000g of the refining finishing liquid includes 8g of a refining agent, 5g of a dispersant, 20g of liquid alkali with a concentration of 32%, and the rest is water.
[0007] The desizing in step 2 of the present invention is a degreasing process, wherein the degreasing process uses a degreasing finishing liquid for degreasing, and 1000 g of the degreasing finishing liquid includes 5 g of a degreasing agent, 5 g of soda ash, 8 g of a refining agent, and the rest is water.
[0008] In step three of the present invention, the stacking time is 16-24h, the moisture content of the fabric is 4-10%, the acid metal complex dye is a 1:1 type acid metal complex dye or a 1:2 type acid metal complex dye, the acid metal complex dye is a dye formed by complexing an acid dye with a metal ion, the metal ion is an iron ion or an aluminum ion or a chromium ion, and the acid dye is acid red G or acid mordant black T or weak acid brilliant blue RAW.
[0009] The residue in step 4 of the present invention includes slurry and spinning oil.
[0010] In step five of the present invention, 1000g of the fluorine-free waterproofing agent finishing liquid includes 20-60g of a fluorine-free waterproofing agent of model R3, 20-60g of a fluorine-free waterproofing agent of model PM-3705, 0-15g of a fluorine-free cross-linking agent, 1g of a penetrant, 0.1-1g of citric acid, and the rest is water. The speed of the padding mill is 30-50m / min, the drying temperature is 100-110°C, and the drying time is 2-3 minutes.
[0011] 1000g of the fluorine-free waterproofing agent finishing liquid of the present invention comprises 40g of the fluorine-free waterproofing agent with the model number R3 and 20g of the fluorine-free waterproofing agent with the model number PM-3705.
[0012] When the total amount of the acid dye in the present invention accounts for 0.5-3% of the mass of the nylon fabric, the fluorine-free crosslinking agent is 0.5-10g; when the total amount of the acid dye in the present invention accounts for ≤0.5% of the mass of the nylon fabric, the fluorine-free crosslinking agent is 10-15g.
[0013] In step six of the present invention, the setting temperature of the setting machine is 160-170° C., and the speed is 30-50 m / min.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1. Compared with the prior art using fluorine-containing waterproofing agents, the present invention uses fluorine-free waterproofing agent finishing liquid to impregnate nylon fabrics, so that no toxic intermediates such as perfluorooctanoic acid and perfluorooctane sulfonic acid are produced during the production process, thereby protecting the environment and making the fabrics safe and non-toxic during use. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a process flow chart of the present invention.
[0017] Figure 2 It is a schematic diagram of the covalent bond coordination reaction between the fluorine-free water repellent finishing liquid and the acidic metal complex dye in step five of the present invention. DETAILED DESCRIPTION
[0018] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0019] like Figure 1-2 As shown, the processing technology of a coordination complex fluorine-free waterproof nylon fabric described in this embodiment. Specific implementation method one:
[0021] The following steps are included: Step 1: Material: Select 7D nylon filament with a gram weight of 15g / m 2 The quality inspection items mainly include physical indicators such as appearance quality inspection, fabric strength, color difference, color fastness, etc.; chemical indicators such as pH value, odor, whether it contains heavy metals, whether it contains fluorescence, etc.; performance indicators such as touch feel, fabric smoothness, fluffiness, etc.
[0022] Step 2: tensionless desizing: the selected nylon fabric is desized by a tensionless desizing machine; the desizing is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing, 1000g of the degreasing finishing liquid includes 5g of degreasing agent, 5g of soda ash, 8g of refining agent, and the rest is water; it also includes a refining process, the nylon fabric after desizing treatment enters a refining process, the refining process uses a refining finishing liquid for refining, 1000g of the refining finishing liquid includes 8g of refining agent, 5g of a dispersant, 20g of liquid alkali with a concentration of 32%, and the rest is water, wherein the desizing is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing, 1000g of the degreasing finishing liquid includes 5g of degreasing agent, 5g of soda ash, 8g of refining agent, and the rest is water.
[0023] Step 3: Rolling, piling and dyeing: The nylon fabric treated in step 2 is rolled and piled up by a rolling machine, and the rolled and piled fabric is dyed by a dyeing machine, and the dye in the dyeing machine is an acid metal complex dye; the piling time is 16 hours, and the moisture content of the fabric is 4%, the acid metal complex dye is a 1:1 type acid metal complex dye, and the acid metal complex dye is a dye formed by complexing an acid dye with a metal ion, the metal ion is an iron ion, and the acid dye is acid red G. The concept of moisture content is the amount of water in the textile material measured under specified conditions, which is expressed as the percentage of the difference between the mass of the sample before drying and the mass after drying to the mass before drying.
[0024] Step 4: Fluorine-free cleaning and testing: Clean the nylon fabric treated in step 3 with a fluorine-free soap detergent to remove surface residues; the residues include slurry and spinning oil. Use a 50x magnifying glass to check whether the surface residues of the nylon fabric after removing the surface residues have been completely removed; since the fluorine-free waterproof finishing liquid requires a higher degree of cleanliness, a 50x magnifying glass is required to carefully check whether the residues have been removed.
[0025] Step 5: Fluorine-free waterproof finishing: A drying machine with a front double dipping and rolling tank is used, the first rolling tank contains citric acid finishing liquid, the citric acid finishing liquid includes citric acid, and the content of the citric acid is 0.1g in 1000g aqueous solution, the nylon fabric treated in step 4 is rolled through the first rolling tank, and the pH value of the citric acid finishing liquid in the first rolling tank is adjusted to 4 by using citric acid and sodium citrate; the second rolling tank contains fluorine-free waterproof agent finishing liquid, the tank temperature is 40°C, the nylon fabric is rolled in the second rolling tank containing fluorine-free waterproof agent finishing liquid, and the fluorine-free waterproof agent finishing liquid reacts with the acidic metal complex dye by covalent bond coordination; the nylon fabric after the second rolling tank is dried; wherein 1000g fluorine-free waterproof agent The finishing liquid includes 20g of fluorine-free waterproofing agent with model R3, 20g of fluorine-free waterproofing agent with model PM-3705, 0.1g of fluorine-free cross-linking agent, 1g of penetrant, 0.1g of citric acid, and the rest is water. The speed of the impregnation mill is 30m / min, the drying temperature is 100℃, and the drying time is 2 minutes; when the total amount of the acid dye and the mass ratio of the nylon fabric are between 0.5-3%, the fluorine-free cross-linking agent is 0.5g; when the total amount of the acid dye and the mass ratio of the nylon fabric are ≤0.5%, the fluorine-free cross-linking agent is 10g; the fluorine-free waterproofing agent R3 is Huntsman fluorine-free waterproofing agent R3; the brand of the fluorine-free waterproofing agent with model PM-3705 is 3M, and the production company is Shanghai Green Copper Materials Co., Ltd.
[0026] Step 6: Shaping: The nylon fabric treated in step 5 is shaped by a shaping machine; the shaping temperature of the shaping machine is 160°C and the speed is 30m / min, and the shaping effect is best at this time. Specific implementation method 2:
[0028] The following steps are included: Step 1: Material: Select 15D nylon filament with a gram weight of 30g / m 2 The quality inspection items mainly include physical indicators such as appearance quality inspection, fabric strength, color difference, color fastness, etc.; chemical indicators such as pH value, odor, whether it contains heavy metals, whether it contains fluorescence, etc.; performance indicators such as touch feel, fabric smoothness, fluffiness, etc.
[0029] Step 2: tensionless desizing: the selected nylon fabric is desized by a tensionless desizing machine; the desizing is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing, 1000g of the degreasing finishing liquid includes 5g of degreasing agent, 5g of soda ash, 8g of refining agent, and the rest is water; it also includes a refining process, the nylon fabric after desizing treatment enters a refining process, the refining process uses a refining finishing liquid for refining, 1000g of the refining finishing liquid includes 8g of refining agent, 5g of a dispersant, 20g of liquid alkali with a concentration of 32%, and the rest is water; wherein the desizing is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing, 1000g of the degreasing finishing liquid includes 5g of degreasing agent, 5g of soda ash, 8g of refining agent, and the rest is water.
[0030] Step 3: rolling, stacking and dyeing: the nylon fabric treated in step 2 is rolled up and stacked by a rolling machine, and the rolled and stacked fabric is dyed by a dyeing machine, and the dye in the dyeing machine is an acid metal complex dye; the stacking time is 24 hours, the moisture content of the fabric is 10%, the acid metal complex dye is a 1:2 type acid metal complex dye, the acid metal complex dye is a dye formed by complexing an acid dye with a metal ion, the metal ion is a chromium ion, and the acid dye is an acid mordant black T.
[0031] Step 4: Fluorine-free cleaning and testing: Clean the nylon fabric treated in step 3 with a fluorine-free soap detergent to remove surface residues; the residues include slurry and spinning oil. Use a 100x magnifying glass to check whether the surface residues have been completely removed from the nylon fabric after removing the surface residues; since the fluorine-free waterproof finishing liquid requires a higher degree of cleanliness, a 100x magnifying glass is needed to carefully check whether the residues have been removed.
[0032] Step 5: Fluorine-free waterproof finishing: A drying machine with a front double dipping and rolling tank is used, the first rolling tank contains citric acid finishing liquid, the citric acid finishing liquid includes citric acid and the rest is water, the content of the citric acid is 0.1-0.2g in 1000g water, the nylon fabric treated in step 4 is rolled through the first rolling tank, and the pH value of the citric acid finishing liquid in the first rolling tank is adjusted to 4-5 with citric acid and sodium citrate; the second rolling tank contains fluorine-free waterproof agent finishing liquid, the tank temperature is 40-50°C, the nylon fabric is rolled through the second rolling tank containing fluorine-free waterproof agent finishing liquid, and the fluorine-free waterproof agent finishing liquid and the acidic metal complex dye undergo a covalent bond coordination reaction; the nylon fabric passing through the second rolling tank is dried; wherein 1 000g fluorine-free waterproofing agent finishing liquid includes 60g fluorine-free waterproofing agent of model R3, 60g fluorine-free waterproofing agent of model PM-3705, 15g fluorine-free cross-linking agent, 1g penetrant, 1g citric acid, and the rest is water. The speed of the impregnation mill is 50m / min, the drying temperature is 110℃, and the drying time is 3 minutes; when the total amount of the acid dye and the mass ratio of the nylon fabric are between 0.5-3%, the fluorine-free cross-linking agent is 10g; when the total amount of the acid dye and the mass ratio of the nylon fabric are ≤0.5%, the fluorine-free cross-linking agent is 15g; wherein the fluorine-free waterproofing agent R3 is Huntsman fluorine-free waterproofing agent R3; the brand of the fluorine-free waterproofing of model PM-3705 is 3M, and the production company is Shanghai Green Copper Materials Co., Ltd.
[0033] Step 6: shaping: the nylon fabric treated in step 5 is shaped by a shaping machine; the shaping temperature of the shaping machine is 170°C and the speed is 50m / min, and the shaping effect is best at this time. Specific implementation method three:
[0035] The following steps are included: Step 1: Material: Select 20D nylon filament with a gram weight of 40g / m 2 The quality inspection items mainly include physical indicators such as appearance quality inspection, fabric strength, color difference, color fastness, etc.; chemical indicators such as pH value, odor, whether it contains heavy metals, whether it contains fluorescence, etc.; performance indicators such as touch feel, fabric smoothness, fluffiness, etc.
[0036] Step 2: tensionless desizing: the selected nylon fabric is desized by a tensionless desizing machine; the desizing is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing, 1000g of the degreasing finishing liquid includes 5g of degreasing agent, 5g of soda ash, 8g of refining agent, and the rest is water; it also includes a refining process, the nylon fabric after desizing treatment enters a refining process, the refining process uses a refining finishing liquid for refining, 1000g of the refining finishing liquid includes 8g of refining agent, 5g of a dispersant, 20g of liquid alkali with a concentration of 32%, and the rest is water; wherein the desizing is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing, 1000g of the degreasing finishing liquid includes 5g of degreasing agent, 5g of soda ash, 8g of refining agent, and the rest is water.
[0037] Step 3: rolling, stacking and dyeing: the nylon fabric treated in step 2 is rolled up and stacked by a rolling machine, and the rolled and stacked fabric is dyed by a dyeing machine, and the dye in the dyeing machine is an acid metal complex dye; the stacking time is 20 hours, the moisture content of the fabric is 8%, the acid metal complex dye is a 1:1 type acid metal complex dye, the acid metal complex dye is a dye formed by complexing an acid dye with a metal ion, the metal ion is an aluminum ion, and the acid dye is a weakly acid brilliant blue RAW.
[0038] Step 4: Fluorine-free cleaning and testing: Clean the nylon fabric treated in step 3 with a fluorine-free soap detergent to remove surface residues; the residues include slurry and spinning oil. Use an 80x magnifying glass to check whether the surface residues of the nylon fabric are completely removed; since the fluorine-free waterproof finishing liquid requires a higher degree of cleanliness, it is necessary to use an 80x magnifying glass to carefully check whether the residues are completely removed.
[0039] Step 5: Fluorine-free waterproof finishing: A drying machine with a front double dipping tank is used, the first rolling tank contains citric acid finishing liquid, the citric acid finishing liquid includes citric acid and the rest is water, the content of the citric acid is 0.1-0.2g in 1000g water, the nylon fabric treated in step 4 is rolled through the first rolling tank, and the pH value of the citric acid finishing liquid in the first rolling tank is adjusted to 4-5 with citric acid and sodium citrate; the second rolling tank contains fluorine-free waterproof agent finishing liquid, the tank temperature is 40-50°C, the nylon fabric is rolled through the second rolling tank containing fluorine-free waterproof agent finishing liquid, and the fluorine-free waterproof agent finishing liquid and the acidic metal complex dye undergo a covalent bond coordination reaction; the nylon fabric passing through the second rolling tank is dried; wherein 10 00g fluorine-free waterproofing agent finishing liquid includes 40g fluorine-free waterproofing agent of model R3, 20g fluorine-free waterproofing agent of model PM-3705, 7g fluorine-free cross-linking agent, 1g penetrant, 0.5g citric acid, and the rest is water. The speed of the impregnation mill is 40m / min, the drying temperature is 105℃, and the drying time is 205 minutes; when the total amount of the acid dye and the mass ratio of the nylon fabric are between 0.5-3%, the fluorine-free cross-linking agent is 5g; when the total amount of the acid dye and the mass ratio of the nylon fabric is ≤0.5%, the fluorine-free cross-linking agent is 13g; wherein the fluorine-free waterproofing agent R3 is Huntsman fluorine-free waterproofing agent R3; the brand of the fluorine-free waterproofing of model PM-3705 is 3M, and the production company is Shanghai Green Copper Materials Co., Ltd.
[0040] Step 6: Shaping: The nylon fabric treated in step 5 is shaped by a shaping machine; the shaping temperature of the shaping machine is 165°C and the speed is 40m / min, and the shaping effect is best at this time.
[0041] Comparative Example 1:
[0042] The specific steps of the processing technology of nylon fabrics using fluorine-containing waterproofing agent in the prior art are as follows: material collection: nylon fabrics are selected and quality inspection is performed on the selected nylon fabrics; step two: tension-free desizing: the selected nylon fabrics are desized using a tension-free desizing machine; step three: rolling, stacking and dyeing: the nylon fabrics treated in step two are rolled up and stacked by a rolling machine, and then dyed by a metal complex acid dye by a roller dyeing machine; step four: cleaning and testing: the nylon fabrics treated in step three are cleaned to remove surface residues; the nylon fabrics with surface residues removed are checked with a magnifying glass with a magnification of 100 times to see whether the surface residues are completely removed; step five: waterproof finishing: the fluorine-containing waterproofing agent is C6 waterproofing agent, and finally enters the dryer for drying; step six: shaping: the nylon fabrics treated in step five are shaped by a shaping machine.
[0043] Compared with the fabrics processed by fluorine-containing waterproofing agents in the prior art, the three fabrics processed by 3M fluorine-free waterproofing agent PM-3705 of the present invention have good effects in terms of shade drying, color difference, and hand scratches. In addition, the present invention does not produce toxic intermediates such as perfluorooctanoic acid and perfluorooctane sulfonic acid during the production process, and will not cause harm to the human body. The fabrics are safe and non-toxic during use.
[0044] Through tests respectively, it is concluded that the nylon fabric processed by the 3M fluorine-free waterproof agent PM-3705 of the present invention has excellent waterproof performance and wet friction fastness. Specifically, the test results are that the initial water splashing degree of the spray test reaches 95 points, the water splashing degree of the spray test after 25 washings and drying reaches 90 points, the water splashing degree of the spray test after 25 washings and drying reaches 80 points, and the wet friction fastness reaches level 4.
Claims
1. A processing technology for coordination complex fluorine-free waterproof nylon fabric, characterized in that: The following steps are involved: Step 1: Material: Select nylon fabric made of 1D-20D nylon filament and conduct quality inspection on the selected nylon fabric; Step 2: tension-free desizing: Desizing the selected nylon fabric using a tension-free desizing machine; Step 3: rolling, stacking and dyeing: the nylon fabric treated in step 2 is rolled up and stacked by a rolling machine, and the rolled and stacked fabric is dyed by a dyeing machine, and the dye in the dyeing machine is an acid metal complex dye; Step 4: Fluorine-free cleaning and testing: Clean the nylon fabric treated in step 3 with a fluorine-free soap detergent to remove surface residues; use a magnifying glass with a magnification of 50-100 times to check whether the surface residues of the nylon fabric after surface residues have been removed completely; Step 5: fluorine-free waterproof finishing: a dryer with a front double dipping tank is used, the first rolling tank contains citric acid finishing liquid, the citric acid finishing liquid includes citric acid and the rest is water, the content of the citric acid is 0.1-0.2g in 1000g water, the nylon fabric treated in step 4 is rolled through the first rolling tank, and the pH value of the citric acid finishing liquid in the first rolling tank is adjusted to 4-5 by using citric acid and sodium citrate; the second rolling tank contains fluorine-free waterproof agent finishing liquid, the tank temperature is 40-50°C, the nylon fabric is rolled through the second rolling tank containing fluorine-free waterproof agent finishing liquid, and the fluorine-free waterproof agent finishing liquid and the acidic metal complex dye undergo a covalent bond coordination reaction; the nylon fabric passing through the second rolling tank is dried; Step 6: shaping: the nylon fabric treated in step 5 is shaped using a shaping machine; In step 3, the stacking time is 16-24h, the moisture content of the fabric is 4-10%, the acid metal complex dye is a 1:1 type acid metal complex dye or a 1:2 type acid metal complex dye, the acid metal complex dye is a dye formed by complexing an acid dye with a metal ion, the metal ion is an iron ion or an aluminum ion or a chromium ion, and the acid dye is acid red G or acid mordant black T or weak acid brilliant blue RAW; In step 5, 1000g of the fluorine-free waterproofing agent finishing liquid includes 40g of a fluorine-free waterproofing agent of model R3, 20g of a fluorine-free waterproofing agent of model PM-3705, 0-15g of a fluorine-free crosslinking agent, 1g of a penetrant, 0.1-1g of citric acid, and the rest is water. The speed of the padding mill is 30-50m / min, the drying temperature is 100-110°C, and the drying time is 2-3 minutes; 2. The processing technology of the coordination complex fluorine-free waterproof nylon fabric according to claim 1 is characterized in that: The nylon fabric in step 1 is made of 7D-20D nylon filament, and the weight of the nylon fabric does not exceed 40g / m 2 .
3. The processing technology of the coordination complex fluorine-free waterproof nylon fabric according to claim 1 is characterized in that: The step 2 also includes a refining process: the nylon fabric after desizing is put into a refining process, and the refining process uses a refining finishing liquid for refining. 1000g of the refining finishing liquid includes 8g of a refining agent, 5g of a chelating dispersant, 20g of a liquid alkali with a concentration of 32%, and the rest is water.
4. The processing technology of the coordination complex fluorine-free waterproof nylon fabric according to claim 1 is characterized in that: The desizing in step 2 is a degreasing process, and the degreasing process uses a degreasing finishing liquid for degreasing. 1000g of the degreasing finishing liquid includes 5g of a degreasing agent, 5g of soda ash, 8g of a refining agent, and the rest is water.
5. The processing technology of the coordination complex fluorine-free waterproof nylon fabric according to claim 1 is characterized in that: The residues from step 4 include pulp and spinning oil.
6. The processing technology of the coordination complex fluorine-free waterproof nylon fabric according to claim 1 is characterized in that: When the total amount of the acid dye and the mass ratio of the nylon fabric are between 0.5-3%, the fluorine-free crosslinking agent is 0.5-10g; when the total amount of the acid dye and the mass ratio of the nylon fabric are ≤0.5%, the fluorine-free crosslinking agent is 10-15g.
7. The processing technology of the coordination complex fluorine-free waterproof nylon fabric according to claim 1 is characterized in that: In step six, the setting temperature of the setting machine is 160-170°C, and the speed is 30-50m / min.