A high-performance solid waste-based cementitious material and preparation method thereof
By using solid waste raw materials such as slag and steel slag in solid waste-based gelling materials, the aluminate hydration reaction and metal ion dissolution is solved, and the problem of low strength of solid waste-based gelling materials in the early stage in the low temperature environment is achieved. Premature strength effect and resource utilization at low temperatures.
Patent Information
- Application Number
- CN202311168675.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-09-12
AI Technical Summary
The existing solid waste-based gelling materials have low early strength and slow hydration rates in low temperature environments, which limits their application in low temperature environments.
The solid waste raw materials such as slag, steel slag, industrial by-product gypsum, photovoltaic silicon sludge, aluminate cement clinker and electrolytic waste slag are used to react calcium aluminate and sulfate in aluminate cement clinker to form C-A-S-H gel, and Adjusting alkalinity and diethanolamine through steel slag promotes the dissolution and hydration of metal ions, increasing the early strength of the gelled material.
It significantly improves the early strength and hydration speed of solid waste-based gelling materials, shortens the gelling time, is suitable for low-temperature environments, reduces production costs, and realizes the resource utilization of solid waste.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cementitious materials, and in particular relates to a high-performance solid waste-based cementitious material and a preparation method thereof. Background Art
[0002] Solid waste-based cementitious materials are made entirely of industrial solid waste from the metallurgical and coal-fired power industries, such as steel slag, slag, and desulfurized gypsum. They do not consume natural mineral resources, do not require high-temperature calcination, do not decompose carbonate raw materials, and do not use alkali excitation. They have similar cementitious properties to traditional cement. Compared with traditional cement clinker, each ton of solid waste-based cementitious materials can reduce CO2 emissions by more than 0.5 tons, and production energy consumption can be reduced by more than 75%, with significant advantages in energy conservation and emission reduction. However, solid waste-based cementitious materials in the prior art face the performance defects of low early strength and slow hydration rate, especially in low-temperature environments, which increases the complexity of construction in low-temperature environments and limits the application of low-carbon cementitious materials in low-temperature environments.
[0003] Therefore, how to improve the early strength and other mechanical properties of solid waste-based cementitious materials and expand their scope of application is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes an early-strength high-performance solid waste-based cementitious material that can be used in a low-temperature environment and a preparation method thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A high-performance solid waste-based cementitious material comprises the following raw materials in parts by weight: 55-65 parts of slag, 10-15 parts of steel slag, 20-30 parts of industrial by-product gypsum, 5-8 parts of photovoltaic silicon mud, 10-20 parts of aluminate cement clinker, 1-3 parts of electrolytic waste residue and 0.02-0.05 parts of diethanolamine.
[0007] Preferably, the raw materials include the following parts by weight: 65 parts of slag, 13 parts of steel slag, 25 parts of industrial by-product gypsum, 7 parts of photovoltaic silicon mud, 15 parts of aluminate cement clinker, 2 parts of electrolytic waste residue and 0.04 parts of diethanolamine.
[0008] Beneficial effects: After the solid waste-based cementitious material is mixed with water, the calcium aluminate in the aluminate cement clinker reacts rapidly with sulfate to form CASH gel, which can ensure the early strength of the solid waste-based cementitious material. At the same time, the steel slag in the present invention has the function of adjusting the alkalinity. Only when an appropriate amount of steel slag is added can the alkalinity and sulfate content be appropriate, thereby allowing the system to generate hydrated alumina gel, which plays a role in filling and compacting the hydration product, further improving the strength of the hardened body. Secondly, the addition of diethanolamine in the present invention can promote the dissolution of RO phase Fe ions in steel slag and aluminum, iron and other metal ions in photovoltaic silicon mud, release the silicon oxygen tetrahedron and aluminum oxygen tetrahedron wrapped by the RO phase and participate in the hydration reaction, and allow the CASH gel to adsorb the metal ions, thereby improving the early strength of the obtained cementitious material. In addition, the photovoltaic silicon mud in the present invention contains a large amount of silicon powder and silicon oxide, which can provide sufficient silicon elements for the cementitious material, thereby further improving the strength of the cementitious material.
[0009] Preferably, the slag is granulated blast furnace slag;
[0010] The steel slag is hot-splashed steel slag from a steel plant;
[0011] The industrial by-product gypsum is wet desulfurized gypsum.
[0012] Preferably, the electrolytic waste slag is fluorine-containing waste slag from electrolytic aluminum.
[0013] Beneficial effects: The electrolytic waste slag in the present invention contains a large amount of fluorine element, which can realize the rapid coagulation and hardening of cement clinker. At the same time, the diethanolamine in the present invention can simultaneously dissolve the RO phase in the electrolytic waste slag and interact with other solid waste raw materials, thereby greatly improving the early strength of the cementitious material and reducing the influence of the fluorine element in the electrolytic waste slag on the early strength of the cementitious material.
[0014] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0015] After the photovoltaic silicon mud is dried and pretreated, the slag, steel slag, industrial by-product gypsum, photovoltaic silicon mud, aluminate cement clinker and electrolytic waste residue are ground separately and then evenly mixed with the diethanolamine to obtain the high-performance solid waste-based cementitious material.
[0016] Preferably, the separate grinding is specifically: grinding the slag, steel slag, industrial by-product gypsum, photovoltaic silicon mud, aluminate cement clinker and electrolytic waste residue to a specific surface area of 350-550m 2 / kg.
[0017] More preferably, the separate grinding is specifically:
[0018] The slag is ground to a specific surface area of 450-550m 2 / kg;
[0019] The steel slag is ground to a specific surface area of 400-500m 2 / kg;
[0020] Grind the industrial by-product gypsum to a specific surface area of 350-400m 2 / kg;
[0021] The aluminate cement clinker is ground to a specific surface area of 400-450m 2 / kg;
[0022] The photovoltaic silicon mud is ground to a specific surface area of 400-550m 2 / kg;
[0023] Grind the electrolytic waste slag to a specific surface area of 400-450m 2 / kg.
[0024] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0025] The photovoltaic silicon mud is dried and pre-treated, and then mixed and ground with other raw materials to obtain the high-performance solid waste-based gelling material.
[0026] Preferably, the grinding is grinding to a specific surface area of 560-600m 2 / kg.
[0027] Preferably, the above drying pretreatment of photovoltaic silicon mud comprises the following steps:
[0028] The photovoltaic silicon mud collected from the photovoltaic plant is dried at 50-60°C, and then washed 3-5 times with clean water, and then dried.
[0029] Beneficial effects: Through the above pretreatment process, harmful volatile substances such as organic solvents in photovoltaic silicon mud can be removed, while retaining silicon oxides and other solid components therein, further improving its activity, and avoiding the harm of volatile substances contained in concrete to the human body. In addition, the solid fineness in the photovoltaic silicon mud raw material is about 5 microns. The photovoltaic silicon mud in the present invention can partially restore the original fineness during the application process, thereby increasing the specific surface area of the cementitious material, promoting hydration, further shortening the initial setting time of the cementitious material, and improving the early strength of the product.
[0030] The present invention discloses a high-performance solid waste-based cementitious material and a preparation method thereof. The present invention prepares the cementitious material by using solid waste raw materials such as slag, copper slag, photovoltaic silicon mud and electrolytic waste slag, so that the obtained cementitious material product can achieve early strength effect under low-temperature curing, greatly reducing the gelling time of the cementitious material, and improving the early strength of the cementitious material, and can replace conventional cement used in low-temperature environments. At the same time, the present invention recycles industrial solid waste, greatly reducing production costs, and provides new ideas and approaches for the resource utilization of solid waste. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.
[0033] An embodiment of the present invention provides a high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight: 55-65 parts of slag, 10-15 parts of steel slag, 20-30 parts of industrial by-product gypsum, 5-8 parts of photovoltaic silicon mud, 10-20 parts of aluminate cement clinker, 1-3 parts of electrolytic waste residue and 0.02-0.05 parts of diethanolamine.
[0034] In a further preferred embodiment, the raw materials are included in the following weight proportions: 65 parts of slag, 13 parts of steel slag, 25 parts of industrial by-product gypsum, 7 parts of photovoltaic silicon mud, 15 parts of aluminate cement clinker, 2 parts of electrolytic waste residue and 0.04 parts of diethanolamine.
[0035] In a further preferred embodiment, the slag is granulated blast furnace slag.
[0036] In a further preferred embodiment, the steel slag is hot-splashed steel slag from a steel plant.
[0037] In a further preferred embodiment, the industrial by-product gypsum is wet desulfurization gypsum.
[0038] In a further preferred embodiment, the electrolytic waste slag is fluorine-containing waste slag from electrolytic aluminum.
[0039] The embodiment of the present invention also provides a method for preparing a high-performance solid waste-based cementitious material, comprising the following steps:
[0040] After the photovoltaic silicon mud is dried and pretreated, the slag, steel slag, industrial by-product gypsum, photovoltaic silicon mud, aluminate cement clinker and electrolytic waste residue are ground separately and then evenly mixed with the diethanolamine to obtain the high-performance solid waste-based cementitious material.
[0041] In a further preferred embodiment, the separate grinding specifically comprises: grinding the slag, steel slag, industrial by-product gypsum, photovoltaic silicon mud, aluminate cement clinker and electrolytic waste residue to a specific surface area of 350-550m 2 / kg.
[0042] In a further preferred embodiment, the separate grinding specifically comprises:
[0043] The slag is ground to a specific surface area of 450-550m 2 / kg;
[0044] The steel slag is ground to a specific surface area of 400-500m 2 / kg;
[0045] Grind the industrial by-product gypsum to a specific surface area of 350-400m 2 / kg;
[0046] The aluminate cement clinker is ground to a specific surface area of 400-450m 2 / kg;
[0047] The photovoltaic silicon mud is ground to a specific surface area of 400-550m 2 / kg;
[0048] Grind the electrolytic waste slag to a specific surface area of 400-450m 2 / kg.
[0049] In some other preferred embodiments, the present invention also provides a method for preparing a high-performance solid waste-based cementitious material, comprising the following steps:
[0050] The photovoltaic silicon mud is dried and pre-treated, and then mixed and ground with other raw materials to obtain the high-performance solid waste-based gelling material.
[0051] In a further preferred embodiment, the grinding is grinding to a specific surface area of 560-600m 2 / kg.
[0052] In a further preferred embodiment, the photovoltaic silicon mud is dried and pretreated, comprising the following steps:
[0053] The photovoltaic silicon mud collected from the photovoltaic plant is dried at 50-60°C, and then washed 3-5 times with clean water, and then dried.
[0054] The slag in the embodiment of the present invention is s95 grade granulated blast furnace slag, and the steel slag is hot-sprayed steel slag from a steel plant, both of which were purchased from Anshan Iron and Steel Green Resources Technology Co., Ltd.
[0055] The industrial by-product gypsum is wet desulfurization gypsum, which was purchased from Weifang Shengchuan Chemical Co., Ltd.
[0056] The electrolytic waste slag is fluorine-containing waste slag of electrolytic aluminum, which was purchased from Guizhou Aluminum City Aluminum Raw Materials Research and Development Co., Ltd.;
[0057] Photovoltaic silicon mud was purchased from Hongguang Enamel Factory in Anci District, Langfang City.
[0058] Example 1
[0059] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0060] 65 parts of slag, 15 parts of steel slag, 20 parts of industrial by-product gypsum, 5 parts of photovoltaic silicon mud, 12 parts of aluminate cement clinker, 3 parts of electrolytic waste residue and 0.03 parts of diethanolamine.
[0061] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0062] (1) The photovoltaic silicon mud collected from the photovoltaic plant is dried at 50-60°C, and then the dried photovoltaic silicon mud is washed 4 times with clean water and then dried;
[0063] (2) Grind the slag to a specific surface area of 500m 2 / kg;
[0064] Grind the steel slag to a specific surface area of 450m 2 / kg;
[0065] Grind industrial by-product gypsum to a specific surface area of 370m 2 / kg;
[0066] Grind aluminate cement clinker to a specific surface area of 430m 2 / kg;
[0067] Grind photovoltaic silicon mud to a specific surface area of 500m 2 / kg;
[0068] Grind the electrolytic waste slag to a specific surface area of 430m 2 / kg;
[0069] (3) The ground raw materials are mixed evenly with diethanolamine to obtain a high-performance solid waste-based cementitious material.
[0070] Example 2
[0071] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0072] 65 parts of slag, 13 parts of steel slag, 25 parts of industrial by-product gypsum, 7 parts of photovoltaic silicon mud, 15 parts of aluminate cement clinker, 2 parts of electrolytic waste residue and 0.04 parts of diethanolamine.
[0073] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0074] (1) The photovoltaic silicon mud collected from the photovoltaic plant is dried at 50-60°C, and then the dried photovoltaic silicon mud is washed three times with clean water and then dried;
[0075] (2) Grind the slag to a specific surface area of 450m 2 / kg;
[0076] Grind the steel slag to a specific surface area of 500m 2 / kg;
[0077] Grind industrial by-product gypsum to a specific surface area of 400m 2 / kg;
[0078] Grind aluminate cement clinker to a specific surface area of 450m 2 / kg;
[0079] Grind photovoltaic silicon mud to a specific surface area of 530m 2 / kg;
[0080] Grind the electrolytic waste slag to a specific surface area of 410m 2 / kg;
[0081] (3) The ground raw materials are mixed evenly with diethanolamine to obtain a high-performance solid waste-based cementitious material.
[0082] Example 3
[0083] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0084] 57 parts of slag, 10 parts of steel slag, 23 parts of industrial by-product gypsum, 6 parts of photovoltaic silicon mud, 20 parts of aluminate cement clinker, 1 part of electrolytic waste residue and 0.03 parts of diethanolamine.
[0085] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0086] (1) The photovoltaic silicon mud collected from the photovoltaic plant is dried at 50-60°C, and then the dried photovoltaic silicon mud is washed 4 times with clean water and then dried;
[0087] (2) Grind the slag to a specific surface area of 550m 2 / kg;
[0088] Grind the steel slag to a specific surface area of 400m 2 / kg;
[0089] Grind industrial by-product gypsum to a specific surface area of 350m 2 / kg;
[0090] Grind aluminate cement clinker to a specific surface area of 410m 2 / kg;
[0091] Grind photovoltaic silicon mud to a specific surface area of 400m 2 / kg;
[0092] Grind the electrolytic waste slag to a specific surface area of 450m 2 / kg;
[0093] (3) The ground raw materials are mixed evenly with diethanolamine to obtain a high-performance solid waste-based cementitious material.
[0094] Example 4
[0095] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0096] 55 parts of slag, 11 parts of steel slag, 27 parts of industrial by-product gypsum, 8 parts of photovoltaic silicon mud, 18 parts of aluminate cement clinker, 2.5 parts of electrolytic waste residue and 0.05 parts of diethanolamine.
[0097] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0098] The photovoltaic silicon mud collected from the photovoltaic plant was dried at 50-60°C, then washed three times with clean water, and then dried. The dried pre-treated photovoltaic silicon mud was mixed with other raw materials and ground to a specific surface area of 600kg / m 2 , that is, high-performance solid waste-based cementitious materials are obtained.
[0099] Example 5
[0100] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0101] 63 parts of slag, 14 parts of steel slag, 30 parts of industrial by-product gypsum, 7 parts of photovoltaic silicon mud, 10 parts of aluminate cement clinker, 1.5 parts of electrolytic waste residue and 0.02 parts of diethanolamine.
[0102] A method for preparing a high-performance solid waste-based cementitious material comprises the following steps:
[0103] The photovoltaic silicon mud collected from the photovoltaic plant was dried at 50-60°C, then washed 5 times with clean water, and then dried. The dried pre-treated photovoltaic silicon mud was mixed with other raw materials and ground to a specific surface area of 560kg / m 2 , that is, high-performance solid waste-based cementitious materials are obtained.
[0104] Comparative Example 1
[0105] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0106] 65 parts of slag, 15 parts of steel slag, and 20 parts of industrial by-product gypsum.
[0107] A method for preparing a high-performance solid waste-based cementitious material is the same as that in Example 1.
[0108] Comparative Example 2
[0109] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0110] 65 parts of slag, 15 parts of steel slag, 20 parts of industrial by-product gypsum, 3 parts of electrolytic waste residue, and 12 parts of aluminate cement clinker.
[0111] A method for preparing a high-performance solid waste-based cementitious material is the same as that in Example 1.
[0112] Comparative Example 3
[0113] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0114] 65 parts of slag, 40 parts of steel slag, 20 parts of industrial by-product gypsum, 5 parts of photovoltaic silicon mud, 12 parts of aluminate cement clinker, 3 parts of electrolytic waste residue and 0.03 parts of diethanolamine.
[0115] A method for preparing a high-performance solid waste-based cementitious material is the same as that in Example 1.
[0116] Comparative Example 4
[0117] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0118] 65 parts of slag, 5 parts of steel slag, 20 parts of industrial by-product gypsum, 5 parts of photovoltaic silicon mud, 12 parts of aluminate cement clinker, 3 parts of electrolytic waste residue and 0.03 parts of diethanolamine.
[0119] A method for preparing a high-performance solid waste-based cementitious material is the same as that in Example 1.
[0120] Comparative Example 5
[0121] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0122] 65 parts of slag, 15 parts of steel slag, 20 parts of industrial by-product gypsum, 12 parts of aluminate cement clinker, 3 parts of electrolytic waste residue and 0.03 parts of diethanolamine.
[0123] A method for preparing a high-performance solid waste-based cementitious material is the same as that in Example 1.
[0124] Comparative Example 6
[0125] A high-performance solid waste-based cementitious material, comprising the following raw materials in parts by weight:
[0126] 65 parts of slag, 15 parts of steel slag, 20 parts of industrial by-product gypsum, 5 parts of photovoltaic silicon mud, 12 parts of aluminate cement clinker and 0.03 parts of diethanolamine.
[0127] A method for preparing a high-performance solid waste-based cementitious material is the same as that in Example 1.
[0128] Technical effects:
[0129] The setting time was measured according to the standard "GBT1346 Cement Standard Consistency Water Consumption, Setting Time, and Stability Test Method", and the preparation and curing quality inspection were carried out according to the standard "GB 17671 Cement Mortar Strength Test Method (ISO Method)", and the compressive strength at 1d and 3d was measured. The results are shown in Table 1:
[0130] Table 1
[0131]
[0132] As can be seen from Table 1, the high-performance solid waste-based cementitious material provided by the present invention greatly shortens the initial setting and final setting time of the product. Even under low-temperature curing at 5°C, the initial setting effect can still be achieved within 7.7 hours and the final setting can be achieved within 9.3 hours. At the same time, by comparing with Comparative Examples 1-5, it can be seen that the raw materials in the present invention have a certain synergistic effect, which can jointly improve the early compressive strength of the cementitious material, and the strength can meet the needs of roads or buildings.
[0133] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A high-performance solid waste-based cementitious material, characterized in that: The invention comprises the following raw materials in parts by weight: 55-65 parts of slag, 10-15 parts of steel slag, 20-30 parts of industrial by-product gypsum, 5-8 parts of photovoltaic silicon mud, 10-20 parts of aluminate cement clinker, 1-3 parts of electrolytic waste residue and 0.02-0.05 parts of diethanolamine.
2. A high-performance solid waste-based cementitious material according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 65 parts of slag, 13 parts of steel slag, 25 parts of industrial by-product gypsum, 7 parts of photovoltaic silicon mud, 15 parts of aluminate cement clinker, 2 parts of electrolytic waste residue and 0.04 parts of diethanolamine.
3. A high-performance solid waste-based cementitious material according to claim 2, characterized in that: The slag is granulated blast furnace slag.
4. A high-performance solid waste-based cementitious material according to claim 2, characterized in that: The steel slag is hot-splashed steel slag from a steel plant.
5. The high-performance solid waste-based cementitious material according to claim 2, characterized in that: The industrial by-product gypsum is wet desulfurized gypsum.
6. A high-performance solid waste-based cementitious material according to claim 2, characterized in that: The electrolytic waste slag is fluorine-containing waste slag from electrolytic aluminum.
7. A method for preparing a high-performance solid waste-based cementitious material according to any one of claims 1 to 6, characterized in that: The following steps are involved: After the photovoltaic silicon mud is dried and pretreated, the slag, steel slag, industrial by-product gypsum, photovoltaic silicon mud, aluminate cement clinker and electrolytic waste residue are ground separately and then evenly mixed with the diethanolamine to obtain the high-performance solid waste-based cementitious material.
8. The method for preparing a high-performance solid waste-based cementitious material according to claim 7, characterized in that: The separate grinding specifically comprises: grinding the slag, steel slag, industrial by-product gypsum, photovoltaic silicon mud, aluminate cement clinker and electrolytic waste slag to a specific surface area of 350-550m 2 / kg.
9. A method for preparing a high-performance solid waste-based cementitious material according to any one of claims 1 to 6, characterized in that: The following steps are involved: The photovoltaic silicon mud is dried and pre-treated, and then mixed and ground with other raw materials to obtain the high-performance solid waste-based gelling material.
10. The method for preparing a high-performance solid waste-based cementitious material according to claim 9, characterized in that: The grinding is grinding to a specific surface area of 560-600m 2 / kg.
Citation Information
Cited By
Solid waste-based cementing material with high interface bonding strength and preparation method of solid waste-based cementing material
CN120736813A
Solid waste-based cementitious material with high interfacial bonding strength and preparation method thereof
CN120736813B