Copper-based halide powders, scintillator films, preparation methods and applications
The preparation of scintillator films by combining copper-based halide powder and polymer composite materials solves the problems of low light yield and imaging artifacts in existing X-ray detectors, and achieves efficient X-ray imaging and irradiation stability .
Patent Information
- Application Number
- CN202410955362.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The scintillator materials (such as CsI: Tl, GOS: Tb) in existing X-ray detectors (such as CsI: Tl, GOS: Tb) have low light yield and long afterglow, which leads to high dose X-ray sources during the imaging process, and imaging artifacts exist. It is not possible to meet higher X-ray imaging requirements.
Copper-based halide powder is used to prepare copper-based halide powder by grinding method, and mixed with polymer composite material to prepare scintillator films. High-efficiency scintillator films are prepared by drop coating, scraping coating or spraying methods for radiation detection. utensil.
It improves the fluorescence quantum efficiency and radiation luminescence performance of the ray detector, reduces the non-radiative recombination path, enhances the luminescence efficiency, is suitable for efficient X-ray imaging, and maintains radiation stability under continuous igmoidation of gamma rays.
Smart Images

Figure CN118495577B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of indirect detection in radiation detection, and in particular to copper-based halide powder, a scintillator film, a method for preparing the copper-based halide powder, a method for preparing the scintillator film, and the application of the copper-based halide powder or the scintillator film in the field of ray detectors. Background Art
[0002] X-ray detectors are widely used in medical diagnosis, radiotherapy, safety inspection, geological exploration, deep space exploration, industrial non-destructive testing, environmental radiation monitoring, etc. Scintillators (such as CsI: Tl and GOS: Tb) are currently widely used in commercial X-ray flat panel detection. However, CsI: Tl crystals and GOS: Tb films are limited by low light yield and long afterglow. During the imaging process, the X-ray source needs to provide a higher dose. There are also problems such as imaging artifacts, which cannot meet the higher requirements of X-ray imaging. Summary of the invention
[0003] In order to achieve the above-mentioned object, the first aspect of the present invention provides a copper-based halide powder, the chemical constituent elements of which include alkali metal elements, copper elements and halogen elements; the copper-based halide powder is applied in the field of radiation detectors.
[0004] According to an embodiment of the present invention, the chemical composition formula of the copper-based halide powder includes: m Cu n X m+n ; Wherein, A represents an alkali metal element, X represents a halogen element, and m and n are both real numbers.
[0005] According to an embodiment of the present invention, the alkali metal element includes at least one of the following: Cs + 、Na + , K + , Rb + .
[0006] According to an embodiment of the present invention, the particle size of the copper-based halide powder is less than 1 μm.
[0007] A second aspect of the present invention provides a scintillator film, which is prepared by using copper-based halide powder, wherein the chemical constituent elements of the copper-based halide powder include alkali metal elements, copper elements and halogen elements.
[0008] The third aspect of the present invention provides a method for preparing a copper-based halide powder, comprising: grinding solid materials of AX and CuX by a grinding method to obtain a copper-based halide powder; wherein A represents an alkali metal element, and X represents a halogen element.
[0009] According to an embodiment of the present invention, the grinding time is 3 to 12 hours; the grinding speed is 500 to 2000 r / min; the molar ratio of AX to CuX is 0.5:1 to 1.7:1; and the grinding method includes dry grinding and / or wet grinding.
[0010] The fourth aspect of the present invention provides a method for preparing a scintillator film, comprising: mixing a copper-based halide powder, a polymer composite material and a dispersant to obtain a powder dispersion, wherein the chemical constituent elements of the copper-based halide powder include alkali metal elements, copper elements and halogen elements; and forming a film of the powder dispersion to obtain a scintillator film.
[0011] According to an embodiment of the present invention, the film-making method includes at least one of the following: drip coating, blade coating, and spray coating; the mass ratio of the copper-based halide powder to the polymer composite material is 1:1 to 500:1;
[0012] The polymer composite material includes at least one of the following: polymethyl methacrylate, polydimethylsiloxane, polyvinyl alcohol, polyvinyl butyral, and polystyrene; the dispersant includes at least one of the following: dimethylformamide, dimethyl sulfoxide, γ-hydroxybutyrolactone, β-mercaptoethanol, nitrogen methyl pyrrolidone, dimethylacetamide, anhydrous ethanol, and toluene.
[0013] The fifth aspect of the present invention provides an application of a copper-based halide powder or a scintillator film in the field of radiation detectors; wherein the copper-based halide powder is the above-mentioned copper-based halide powder or a copper-based halide powder prepared by the above-mentioned method for preparing the copper-based halide powder; the scintillator film is the above-mentioned scintillator film or a scintillator film prepared by the above-mentioned method for preparing the scintillator film. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1A A scanning electron microscope (SEM) image of the Cs3Cu2I5 copper-based halide powder obtained according to Example 1 of the present invention is shown;
[0015] Figure 1B The SEM image of the Cs3Cu2I5 copper-based halide powder obtained in Comparative Example 1 of the present invention is shown;
[0016] Figure 2A The photoluminescence quantum efficiency (PLQY) of the scintillator film obtained according to Example 1 of the present invention is shown;
[0017] Figure 2B The PLQY of the scintillator film obtained in Comparative Example 1 of the present invention is shown;
[0018] Figure 3The photoluminescence spectra of the scintillator thin film obtained in Example 1 and the scintillator thin film doped with different alkali metal elements obtained in Example 2 of the present invention are shown;
[0019] Figure 4A The radiant luminescence spectra of CsI: Tl crystal and Cs3Cu2I5 scintillator film obtained in Example 2 of the present invention under X-ray irradiation are shown;
[0020] Figure 4B The PLQY of the scintillator film doped with alkali metal elements obtained in Example 2 of the present invention is shown;
[0021] Figure 5 A photograph (a) of the alkali metal-doped flexible scintillator film obtained in Example 3 of the present invention and a photograph (b) of the flexible film after folding are shown;
[0022] Figure 6 The photoluminescence spectra of the copper-based halide scintillator films obtained with different molar ratios of CsI to CuI in Examples 1, 5 and 6 of the present invention are shown;
[0023] Figure 7 The photoluminescence spectra of the copper-based halide scintillator films obtained in Example 6 and Example 7 of the present invention are shown;
[0024] Fig. 8A The imaging photograph of the scintillator film doped with alkali metal elements obtained in Example 2 of the present invention on the lead wire to plate under X-ray irradiation is shown;
[0025] Figure 8B The figure shows the imaging photograph of the lead wire-to-plate by a commercial X-ray flat panel detector (the scintillator layer is a GOS film) under X-ray irradiation;
[0026] Fig. 9 The irradiation stability of the flexible scintillator film doped with alkali metal elements obtained in Example 3 of the present invention under continuous irradiation of gamma rays is shown. DETAILED DESCRIPTION
[0027] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0028] In the process of realizing the present invention, it was found that the scintillators of commercial X-ray flat-panel detectors are limited by low light yield and long afterglow, etc., and the X-ray source is required to provide a higher dose during the imaging process. At the same time, there are problems such as imaging artifacts, which cannot meet the higher requirements of X-ray imaging.
[0029] Metal halide perovskite materials contain elements with higher atomic numbers such as cesium, lead, and iodine, which can effectively absorb high-energy rays such as X-rays. They also have excellent optoelectronic properties such as adjustable emission wavelength, high defect tolerance, and short fluorescence decay lifetime, making them very suitable for indirect detection in radiation detection, that is, as scintillators. Although new metal halide perovskites, such as lead-based halide perovskites, have been widely studied in the field of X-ray imaging due to their excellent performance, lead-based halide perovskites have self-absorption problems, which limits their light yield and resolution. In addition, the development of lead-based halide perovskite scintillators also has problems such as poor stability and the presence of toxic elements.
[0030] In addition, although copper-based halide perovskites are also a new type of metal halide perovskites, typical copper-based halide perovskite bulk single crystals are not suitable for use in the field of X-ray imaging due to low resolution and other reasons. The method of synthesizing copper-based halide perovskite powder based on the anti-solvent method requires the use of large amounts of toxic solvents. Therefore, it is necessary to explore a new material that can be easily prepared and can meet the higher requirements of X-ray imaging.
[0031] Based on this, the present invention provides a copper-based halide powder, the chemical constituent elements of which include alkali metal elements, copper elements and halogen elements; the copper-based halide powder is applied in the field of ray detectors.
[0032] According to the embodiments of the present invention, the copper-based halide powder contains alkali metal elements, copper elements and halogen elements, but does not contain toxic elements, thereby improving safety. In addition, the copper-based halide powder has good fluorescence performance and high luminous efficiency, and is suitable for the field of ray detectors, especially the field of X-ray detectors.
[0033] According to an embodiment of the present invention, the chemical composition formula of the copper-based halide powder may include: m Cu n X m+n ; Wherein, A represents an alkali metal element, X represents a halogen element, and m and n are both real numbers.
[0034] According to the embodiments of the present invention, due to the presence of A-site doping of alkali metal elements in copper-based halides, the lattice constant of the copper-based halides can be adjusted without changing the lattice structure, making the lattice more adaptable, and at the same time passivating the A-site defects, reducing the non-radiative recombination paths of the copper-based halides, and making the luminescence efficiency higher.
[0035] According to an embodiment of the present invention, the alkali metal element may include at least one of the following: Cs + 、Na + , K + , Rb + .
[0036] According to an embodiment of the present invention, the copper-based halide powder may be a copper-based halide powder containing a single alkali metal element, or may be a copper-based halide powder doped with different alkali metal elements.
[0037] According to an embodiment of the present invention, the alkali metal element may include a first alkali metal element and a second alkali metal element. The first alkali metal element and the second alkali metal element are different. The molar amount of the second alkali metal element may be 5% to 80% of the molar amount of the first alkali metal element. The second alkali metal element is doped in the first alkali metal element in the manner of A-position doping.
[0038] For example, the chemical composition of the copper-based halide powder may include, but is not limited to, at least one of the following: Cs3Cu2I5, Cs3Cu2I5:NaI, Cs3Cu2I5:KI, Cs3Cu2I5:RbI, Cs3Cu2Br5, Cs3Cu2Br5:KBr, Cs3Cu2Br5:RbBr, Cs3Cu2Cl5, Cs3Cu2Cl5:KCl, Cs3Cu2Cl5:RbCl, CsCu2I 3. CsCu2I3:NaI, CsCu2I3:KI, CsCu2I3:RbI, Cs5Cu3I8, Cs5Cu3I8:NaI, Cs5Cu3I8:KI, Cs5Cu3I8: RbI, Cs5Cu3Cl6I2, Cs5Cu3Cl6I2:KI, Cs5Cu3Cl6I2:KCl, Cs5Cu3Cl6I2:RbCl, Cs5Cu3Cl6I2:RbI, etc.
[0039] According to an embodiment of the present invention, the halogen element may include at least one of the following: - Br - , Cl - .
[0040] According to an embodiment of the present invention, the particle size of the copper-based halide powder is less than 1 μm.
[0041] According to an embodiment of the present invention, the ray detector may include an X-ray flat panel detector or a gamma ray detector, but is not limited thereto.
[0042] According to an embodiment of the present invention, the copper-based halide powder does not contain toxic elements, has a small particle size, a high fluorescence quantum efficiency (for example, the fluorescence quantum efficiency may be greater than 90%), and a short fluorescence decay lifetime (for example, the fluorescence decay lifetime may be less than 1 μs), and can be used in radiation detectors.
[0043] According to an embodiment of the present invention, flexible scintillator films of various thicknesses and sizes can be prepared using copper-based halide powder, and can be applied to scenarios such as radiotherapy dose monitoring and industrial nondestructive testing.
[0044] In the process of realizing the inventive concept of the present application, it is also found that the preparation method of copper-based halide powder and the particle size of copper-based halide powder will affect the performance of the prepared scintillator film. Based on this, the present invention also provides a method for preparing copper-based halide powder, which may include: grinding solid materials of AX and CuX by grinding method to obtain copper-based halide powder; wherein A represents an alkali metal element and X represents a halogen element.
[0045] According to an embodiment of the present invention, the grinding time may be 3 to 12 hours. For example, the grinding time may include but is not limited to 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours.
[0046] According to the embodiment of the present invention, too short a grinding time may result in insufficient grinding, affecting the yield, particle size and purity of the copper-based halide powder, etc. Too long a grinding time may waste time costs.
[0047] According to an embodiment of the present invention, the grinding speed may be 500-2000 r / min. For example, the grinding speed may include but is not limited to 500 r / min, 750 r / min, 1000 r / min, 1250 r / min, 1500 r / min, 1750 r / min, and 2000 r / min.
[0048] According to the embodiment of the present invention, too low a grinding speed may affect the grinding efficiency and the particle size of the copper-based halide powder, while too high a grinding speed may damage the grinder and cause damage due to the centrifugal force and vibration, and parts splitting.
[0049] According to an embodiment of the present invention, the molar ratio of AX to CuX may be 0.5: 1 to 1.7: 1. Preferably, the molar ratio of AX to CuX may be 3:2.
[0050] According to an embodiment of the present invention, when the molar ratio of AX to CuX is too low, it will lead to disproportionation of cuprous ions and generation of halogen elements, and when the molar ratio of AX to CuX is too high, excessive AX powder that is difficult to clean will remain.
[0051] According to an embodiment of the present invention, AX may be a doped alkali metal halide.
[0052] Taking Cs3Cu2I5 prepared from CsI and CuI as an example, other alkali metal halides can be added to CsI and CuI, and the molar amount of other alkali metal halides can be 5% to 80% of the molar amount of CsI. For example, the molar ratio of RbI (or NaI or KI), CsI and CuI can be 0.15 to 2.4:3:2.
[0053] According to an embodiment of the present invention, the grinding method may include a dry grinding method and / or a wet grinding method.
[0054] For example, the dry grinding method may include directly adding solid materials of AX and CuX into a grinding jar, placing the jar in a physical grinder for grinding, and obtaining a copper-based halide powder.
[0055] The wet grinding method may include adding solid materials of AX and CuX together with a solvent insoluble in the solid materials into a grinding jar, placing the jar in a physical grinder for grinding, and obtaining a copper-based halide powder.
[0056] The solvent insoluble in the solid material may include, but is not limited to, at least one of the following: dimethylformamide (DMF), dimethyl sulfoxide (DMSO), γ-hydroxybutyrolactone (GBL), β-mercaptoethanol (2-ME), nitrogenmethylpyrrolidone (NMP), dimethylacetamide (DMAC), anhydrous ethanol and toluene.
[0057] According to an embodiment of the present invention, the grinding jar may include a ball mill jar, but is not limited thereto. Balls made of non-metallic materials may be placed in the ball mill jar, such as agate balls.
[0058] According to an embodiment of the present invention, after grinding, anhydrous ethanol or other solvents may be added to the ball mill to assist in dispersion, and the ultrasonic power may be 100-500 W. After ultrasonic dispersion, the dispersion is centrifuged, and the centrifugal rate may be 3000-7000 r / min. The precipitate is taken and dried, and the drying temperature may be 80 o C~150 o C, drying time can be longer than 5h.
[0059] The present invention also provides a scintillator film, which is prepared by using copper-based halide powder. The chemical constituent elements of the copper-based halide powder may include alkali metal elements, copper elements and halogen elements.
[0060] According to an embodiment of the present invention, the copper-based halide powder used to prepare the scintillator thin film may be the copper-based halide powder provided above or the copper-based halide powder prepared by the method for preparing the copper-based halide powder above.
[0061] In the process of implementing the present invention, it is also found that the scintillators (such as CsI:Tl, GOS:Tb) used in commercial X-ray flat panel detectors are prepared by thermal evaporation or sintering, which requires 1700 o The high temperature of around 30°C has disadvantages such as high energy consumption and long preparation cycle. Therefore, it is necessary to explore a new method that can meet the needs of scintillator preparation.
[0062] Based on this, the present invention also provides a method for preparing a scintillator thin film, which may include: mixing copper-based halide powder, polymer composite material and dispersant to obtain a powder dispersion liquid, and forming a film on the powder dispersion liquid to obtain a scintillator thin film.
[0063] According to an embodiment of the present invention, chemical constituent elements of the copper-based halide powder may include alkali metal elements, copper elements, and halogen elements.
[0064] According to an embodiment of the present invention, the mass ratio of the copper-based halide powder to the polymer composite material may be 1:1 to 500:1.
[0065] According to an embodiment of the present invention, a mass ratio of copper-based halide powder to polymer composite material that is too small will affect the radioluminescence performance and X-ray absorptivity of the scintillator film, while a mass ratio that is too large will lead to uneven dispersion of the dispersion liquid, making it difficult to prepare a uniform scintillator film.
[0066] According to an embodiment of the present invention, the polymer composite material may include at least one of the following: polymethyl methacrylate (PMMA), polydimethylsiloxane (PDMS), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), and polystyrene (PS).
[0067] According to an embodiment of the present invention, the mass ratio of different polymer composite materials to copper-based halide powder may range from different ranges. For example, the mass ratio of copper-based halide powder to PMMA may range from 1:1 to 2:1, the mass ratio of copper-based halide powder to PDMS may range from 1:1 to 10:1, the mass ratio of copper-based halide powder to PVB may range from 25:1 to 500:1, etc.
[0068] According to an embodiment of the present invention, the dispersant may include at least one of the following: dimethylformamide, dimethyl sulfoxide, γ-hydroxybutyrolactone, β-mercaptoethanol, nitrogen methyl pyrrolidone, dimethylacetamide, anhydrous ethanol and toluene.
[0069] According to an embodiment of the present invention, the copper-based halide powder, the polymer composite material and the dispersant can be fully stirred by a magnetic particle to obtain a powder dispersion. The stirring temperature can be 60 o C~80 o C, stirring time can be longer than 3h.
[0070] According to an embodiment of the present invention, the film forming method may include one of the following: drip coating, blade coating, and spray coating.
[0071] The drop coating method may include the following operations: preparing glass of a preset area, cleaning the glass and drying it, dropping a powder dispersion onto the dried glass, and slowly evaporating it in a glove box at room temperature to peel off the scintillator film.
[0072] The scraping method may include the following operations: preparing glass of a preset area, cleaning the glass and drying it, scraping the powder dispersion on the dried glass with a scraper, heating and curing it in the air, and then peeling off the scintillator film.
[0073] The spraying method may include the following operations: preparing a substrate of a preset area, cleaning the substrate and then drying it, spraying a powder dispersion on the dried substrate to obtain a composite thin film of the scintillator and the substrate.
[0074] According to the embodiments of the present invention, the prepared scintillator film has a lower synthesis temperature and a shorter preparation period than the scintillators currently widely used in commercial X-ray flat panel detection (such as CsI:Tl and GOS:Tb).
[0075] The following is a more specific example of copper-based halide powder, scintillator film, copper-based halide powder preparation method and scintillator film preparation method. It should be noted that the example is only a specific embodiment of the present invention and cannot limit the protection scope of the present invention.
[0076] Embodiment 1:
[0077] S1, placing 2 g of solid materials of CsI and CuI with a molar ratio of 3:2, 2 mL of anhydrous ethanol and agate balls in a ball mill with a volume of 50 mL, the mass ratio of agate balls to solid materials being 20:1, and evacuating the ball mill and placing it in a ball mill to prepare copper-based halide powder by wet grinding, the ball milling speed being 1000 r / min, and the ball milling time being 5 h;
[0078] S2, add 20mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer it to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge it at 120 o C and dried for 5 h, and the copper-based halide powder was collected;
[0079] S3, mixing the copper-based halide powder and PMMA at a mass ratio of 1:1, adding toluene, and stirring thoroughly to obtain a powder dispersion with a concentration of 75 mg / mL;
[0080] S4, preparation of scintillator thin film by drop coating: preparation area 3×3 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. 1.2 mL of the powder dispersion obtained in S3 was dropped on the dried glass and slowly evaporated in a glove box at room temperature to peel off the scintillator film.
[0081] Comparative Example 1:
[0082] The difference between this comparative example 1 and example 1 is that example 1 adopts a grinding method to prepare copper-based halide powder, while comparative example 1 adopts an anti-solvent method to prepare copper-based halide powder. The specific method is as follows:
[0083] S1, adding a solid material of CsI and CuI with a total mass of 2 g and a molar ratio of 3:2 to DMSO, adding a magnet, and stirring thoroughly to obtain a copper-based halide solution; then transferring the copper-based halide solution to a centrifuge tube, quickly adding methanol to the centrifuge tube, the volume ratio of methanol to the copper-based halide solution being 1:20, forming a precipitate, placing the centrifuge tube in a centrifuge, centrifuging at 5000 r / min for 5 minutes, discarding the supernatant and taking the precipitate, and obtaining a copper-based halide powder;
[0084] S2, add copper-based halide powder to 20 mL of methanol, centrifuge and take the precipitate, and heat the precipitate at 120 o C and dried for 5 h, and the copper-based halide powder was collected;
[0085] S3, mixing the copper-based halide powder and PMMA at a mass ratio of 1:1, adding toluene, and stirring thoroughly to obtain a powder dispersion with a concentration of 75 mg / mL;
[0086] S4, prepare the scintillator film by drop coating. The preparation area is 3×3 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. 1.2 mL of the powder dispersion obtained in S3 was dropped on the dried glass and slowly evaporated in a glove box at room temperature to peel off the scintillator film.
[0087] Figure 1A A scanning electron microscope (SEM) image of the Cs3Cu2I5 copper-based halide powder obtained according to Example 1 of the present invention is shown; Figure 1B The SEM image of the Cs3Cu2I5 copper-based halide powder obtained in Comparative Example 1 of the present invention is shown; Figure 2A The photoluminescence quantum efficiency (PLQY) of the scintillator film obtained according to Example 1 of the present invention is shown; Figure 2B The PLQY of the scintillator thin film obtained in Comparative Example 1 according to the present invention is shown.
[0088] The copper-based halide powder is prepared by the preparation method provided in the embodiment of the present invention, such as Figure 1A As shown in FIG. 1 , the particle size of the copper-based halide powder obtained in Example 1 is less than 1 μm. Figure 1BAs shown in FIG. 1 , the particle size of the copper-based halide powder obtained in this comparative example 1 is greater than 10 μm. It can be seen that the copper-based halide powder prepared by the grinding method has a smaller particle size. It is found that different methods for preparing copper-based halide powders not only affect the particle size of the copper-based halide powders, but also affect the optical properties of the scintillator film prepared therefrom. Figure 2A As shown in FIG. 1 , the photoluminescence quantum efficiency (PLQY) of the scintillator film obtained in Example 1 is about 89%. Figure 2B As shown, the PLQY of the scintillator film obtained in this comparative example 1 is about 70.7%. Since the scintillator film prepared by the copper-based halide powder with a particle size of less than 1 μm prepared by the grinding method has a higher PLQY, the copper-based halide powder prepared by the grinding method can be used to prepare a scintillator film with high photoluminescence quantum efficiency, which is conducive to meeting the higher requirements of X-ray imaging.
[0089] Embodiment 2:
[0090] The difference between Example 2 and Example 1 is that RbI or NaI or KI is doped into the copper-based halide powder. The specific method is as follows:
[0091] S1, placing 2 g of solid materials of RbI or NaI or KI, CsI and CuI with a molar ratio of 0.3:3:2, 2 mL of anhydrous ethanol and agate balls in a ball mill with a volume of 50 mL, the mass ratio of agate balls to powder is 20:1, and the ball mill is evacuated and placed in a ball mill to prepare copper-based halide powder by wet grinding, the ball mill speed is 1000 r / min, and the ball milling time is 5 h;
[0092] S2, add 20mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer it to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge it at 120 o C and dried for 5 h, and the copper-based halide powder was collected;
[0093] S3, mixing the copper-based halide powder and PMMA at a mass ratio of 1:1, adding toluene, and stirring thoroughly to obtain a powder dispersion with a concentration of 75 mg / mL;
[0094] S4, preparation of scintillator film by drop coating: cutting area 3×3 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. 1.2 mL of the powder dispersion obtained in S3 was dropped on the dried glass and slowly evaporated in a glove box at room temperature to peel off the scintillator film.
[0095] Figure 3The photoluminescence spectra of the scintillator thin film obtained in Example 1 and the scintillator thin film doped with different alkali metal elements obtained in Example 2 according to the present invention are shown.
[0096] like Figure 3 As shown, the photoluminescence intensity of the scintillator film prepared by using the copper-based halide powder doped with different alkali metal elements is higher than that of the scintillator film prepared by using the copper-based halide powder not doped with alkali metal elements, which is more conducive to the application in X-ray detectors.
[0097] Figure 4A The luminescence spectra of the CsI:Tl crystal and the scintillator film doped with alkali metal elements obtained in Example 2 of the present invention under X-ray irradiation are shown; Figure 4B The PLQY of the scintillator film doped with alkali metal elements obtained in Example 2 of the present invention is shown;
[0098] like Figure 4A As shown in the figure, under the irradiation of X-rays with a peak energy of 100 keV, the scintillator film prepared by using copper-based halide powder doped with alkali metal elements has enhanced radiation luminescence intensity compared with CsI:Tl crystal in existing X-ray detectors. The light yield of the scintillator film is about 1.5 times that of CsI:Tl crystal. Figure 4B As shown, the photoluminescence quantum efficiency of the scintillator film provided by the present invention can be as high as 97%. It should be noted that the ratio of the light yield of the scintillator film to the light yield of the CsI:Tl crystal is based on Figure 4A It is determined by the integration of the radiant luminescence spectra of the scintillator film and the CsI:Tl crystal.
[0099] Embodiment 3:
[0100] The difference between Example 3 and Example 2 is that the amount of raw materials is increased and the flexible scintillator film is prepared by a scraping method. The specific method is as follows:
[0101] S1, placing 20 mL of anhydrous ethanol and agate balls of solid materials of RbI, CsI and CuI with a total mass of 20 g and a molar ratio of 0.3:3:2 in a ball mill with a volume of 500 mL, and the mass ratio of agate balls to powder is 20:1, and the ball mill is evacuated and placed in a ball mill to prepare copper-based halide powder by wet grinding, the ball mill speed is 1000 r / min, and the ball milling time is 5 h;
[0102] S2, add 200mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer it to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge it at 120 o C and dried for 5 h, and the copper-based halide powder was collected;
[0103] S3, mixing the copper-based halide powder and PDMS in a mass ratio of 1:1, stirring thoroughly, and evacuating to remove bubbles to obtain a powder dispersion;
[0104] S4, preparation of flexible scintillator film by blade coating: preparation area 20 × 20 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. A release agent was sprayed on the dried glass, and 20 mL of the powder dispersion obtained in S3 was scraped on the glass with a scraper. Then, it was heated and cured at 120°C in air for 2 h, and the scintillator film could be peeled off.
[0105] Figure 5 A photograph (a) of the alkali metal-doped flexible scintillator film obtained in Example 3 of the present invention and a photograph (b) of the flexible film after folding are shown.
[0106] like Figure 5 As shown, according to Embodiment 3 of the present invention, a flexible scintillator thin film can be obtained.
[0107] Embodiment 4:
[0108] The difference between the present embodiment 4 and the embodiment 3 is that the composite film of the scintillator and the reflective film is prepared by the spraying method, and the specific method is as follows:
[0109] S1, placing 20 mL of anhydrous ethanol and agate balls of solid materials of RbI, CsI and CuI with a total mass of 20 g and a molar ratio of 0.3:3:2 in a ball mill with a volume of 500 mL, and the mass ratio of agate balls to powder is 20:1, and the ball mill is evacuated and placed in a ball mill to prepare copper-based halide powder by wet grinding, with a ball mill speed of 1000 r / min and a ball milling time of 5 h;
[0110] S2, add 200mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer the ball mill to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge at 120 o C and dried for 5 h, and the copper-based halide powder was collected;
[0111] S3, mixing the copper-based halide powder and PVB at a mass ratio of 25:1, adding anhydrous ethanol and stirring thoroughly to obtain a powder dispersion with a concentration of 200 mg / mL;
[0112] S4, preparation of scintillator film by spray coating: preparation area 5×5 cm 2The polyethylene terephthalate (PET) reflective film was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned PET reflective film was placed on the spraying substrate of the ultrasonic sprayer. The substrate heating temperature was 80°C, and 20 mL of the powder dispersion obtained in S3 was sprayed on the dried reflective film. The operating power of the ultrasonic nozzle was 3 W, and the liquid supply speed was 3 mL / min to obtain a composite film of the scintillator and the PET reflective film.
[0113] Embodiment 5:
[0114] The difference between this embodiment 5 and embodiments 1 to 4 is that the ratio of AX to CuX in the raw materials is reduced, and the specific method is as follows:
[0115] S1, placing 2 g of CsI and CuI solid materials with a molar ratio of 1:2, 2 mL of anhydrous ethanol and agate balls in a 50 mL ball mill, the mass ratio of agate balls to solid materials being 20:1, and evacuating the ball mill and placing it in a ball mill to prepare copper-based halide powder by wet grinding, the ball mill speed being 1000 r / min, and the ball milling time being 5 h;
[0116] S2, add 20mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer it to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge it at 120 o C and dried for 5 hours, and a copper-based halide powder is collected, wherein the component of the copper-based halide powder is CsCu2I3;
[0117] S3, mixing the copper-based halide powder and PMMA at a mass ratio of 1:1, adding toluene, and stirring thoroughly to obtain a powder dispersion with a concentration of 75 mg / mL;
[0118] S4, preparation of scintillator thin film by drop coating: preparation area 3×3 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. 1.2 mL of the powder dispersion obtained in S3 was dropped on the dried glass and slowly evaporated in a glove box at room temperature to peel off the scintillator film.
[0119] Embodiment 6:
[0120] The difference between this embodiment 6 and embodiments 1 to 4 is that the ratio of AX to CuX in the raw materials is increased, and the specific method is as follows:
[0121] S1, placing 2 g of solid materials of CsCl, CuCl and CuI with a molar ratio of 5:1:2, 2 mL of anhydrous ethanol and agate balls in a ball mill with a volume of 50 mL, the mass ratio of agate balls to solid materials being 20:1, and evacuating the ball mill and placing it in a ball mill to prepare copper-based halide powder by wet grinding, the ball mill speed being 1000 r / min, and the ball milling time being 5 h;
[0122] S2, add 20mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer it to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge it at 120 o C and dried for 5 hours, and a copper-based halide powder is collected, wherein the component of the copper-based halide powder is Cs5Cu3Cl6I2;
[0123] S3, mixing the copper-based halide powder and PMMA at a mass ratio of 1:1, adding toluene, and stirring thoroughly to obtain a powder dispersion with a concentration of 75 mg / mL;
[0124] S4, preparation of scintillator thin film by drop coating: preparation area 3×3 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. 1.2 mL of the powder dispersion obtained in S3 was dropped on the dried glass and slowly evaporated in a glove box at room temperature to peel off the scintillator film.
[0125] Figure 6 The photoluminescence spectra of the copper-based halide scintillator films obtained at different molar ratios of CsI to CuI in Examples 1, 5 and 6 of the present invention are shown.
[0126] like Figure 6 It is shown that the fluorescence efficiency of the copper-based halide scintillator film obtained when the molar ratio of CsI to CuI is 3:2 is the highest.
[0127] Embodiment 7:
[0128] The difference between Example 6 and Example 7 is that the ratio of AX to CuX in the raw materials is increased, and KI is doped in the copper-based halide. The specific method is as follows:
[0129] S1, placing solid materials of CsCl, CuCl, CuI and KI with a total mass of 2 g and a molar ratio of 5:1:2:0.5, 2 mL of anhydrous ethanol and agate balls in a ball mill with a volume of 50 mL, the mass ratio of agate balls to solid materials being 20:1, and the ball mill is evacuated and placed in a ball mill to prepare copper-based halide powder by wet grinding, the ball mill speed is 1000 r / min, and the ball milling time is 5 h;
[0130] S2, add 20mL of anhydrous ethanol to the ball mill, place the ball mill in an ultrasonic cleaner with an ultrasonic power of 400W, transfer it to a centrifuge tube for centrifugation, take the precipitate, and then centrifuge it at 120 o C and dried for 5 hours, and a copper-based halide powder is collected, wherein the composition of the copper-based halide powder is Cs5Cu3Cl6I2:KI;
[0131] S3, mixing the copper-based halide powder and PMMA at a mass ratio of 1:1, adding toluene, and stirring thoroughly to obtain a powder dispersion with a concentration of 75 mg / mL;
[0132] S4, preparation of scintillator thin film by drop coating: preparation area 3×3 cm 2 The glass was ultrasonically cleaned with detergent, deionized water and anhydrous ethanol respectively, and then the cleaned glass was stored in an oven at 70°C for drying. 1.2 mL of the powder dispersion obtained in S3 was dropped on the dried glass and slowly evaporated in a glove box at room temperature to peel off the scintillator film.
[0133] Figure 7 The photoluminescence spectra of the copper-based halide scintillator films obtained in Examples 6 and 7 of the present invention are shown.
[0134] like Figure 7 As shown, the photoluminescence intensity of the copper-based halide scintillator film obtained by using the copper-based halide powder doped with alkali metal is higher than that of the copper-based halide scintillator film obtained by using the copper-based halide powder not doped with alkali metal, which is also beneficial for application in X-ray detectors.
[0135] The present invention also provides an application of copper-based halide powder or scintillator film in the field of ray detectors.
[0136] According to an embodiment of the present invention, the copper-based halide powder may be the above-mentioned copper-based halide powder or a copper-based halide powder prepared by the above-mentioned method for preparing the copper-based halide powder; the scintillator film may be the above-mentioned scintillator film or a scintillator film prepared by the above-mentioned method for preparing the scintillator film.
[0137] According to an embodiment of the present invention, the radiation detector may include but is not limited to an X-ray flat panel detector or a gamma ray detector.
[0138] Fig. 8A The imaging photograph of the scintillator film doped with alkali metal elements obtained in Example 2 of the present invention on the lead wire to plate under X-ray irradiation is shown; Figure 8B The figure shows the imaging photograph of the lead wire-to-plate by a commercial X-ray flat panel detector (the scintillator layer is a GOS film) under X-ray irradiation; Fig. 9The irradiation stability of the flexible scintillator film doped with alkali metal elements obtained in Example 3 of the present invention under continuous irradiation of gamma rays is shown.
[0139] According to the embodiment of the present invention, the scintillator film provided by the present invention can be used to replace the GOS thin film scintillator layer of a commercial X-ray flat panel detector to obtain a new detector. By observing the imaging of the lead line to the plate of the new detector provided by the present invention and the commercial X-ray flat panel detector at the same spatial resolution, the imaging capabilities of the two can be compared. Fig. 8A As shown, the spatial resolution is up to 30lp mm -1 When the scintillator film provided by the present invention is used, the imaging of the lead wire on the plate is clearly visible. Figure 8B As shown, the spatial resolution is up to 30lp mm -1 Therefore, the imaging capability of the scintillator film provided by the present invention for the lead line to the board in the X-ray flat panel detector is significantly stronger than that of the commercial X-ray flat panel detector (the scintillator layer is the GOS film) for the lead line to the board, and the spatial resolution of the scintillator film provided by the present invention for the lead line to the board in the X-ray flat panel detector can be as high as 30lp mm -1 It can be understood that the GOS film is a Gadolinium Oxysulfide film.
[0140] In addition, the scintillator film provided by the present invention has a good response to X-rays and exhibits good irradiation stability under high-energy ray irradiation. Fig. 9 As shown, under continuous irradiation with γ-rays with an energy of 6 MeV (total dose of 50 Gyair), the fluorescence intensity can be retained by 96%.
[0141] The scintillator film provided by the present invention has a high photoluminescence quantum efficiency and can generate a high fluorescence signal. In addition, the scintillator film provided by the present invention is applied to a detector and has a high spatial resolution. The combination of the two makes it easier to detect the generated high fluorescence signal due to the high spatial resolution, thereby improving the signal-to-noise ratio of the detector measurement.
[0142] The above specific embodiments further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A scintillator film, characterized in that: The scintillator film is used in an X-ray flat panel detector. The scintillator film is obtained by film-forming a powder dispersion obtained by mixing copper-based halide powder, a polymer composite material and a dispersant. The particle size of the copper-based halide powder is less than 1 μm. The copper-based halide powder is obtained by grinding solid materials of RbI, CsI and CuI with a molar ratio of 0.3:3:2 and a solvent insoluble in the solid materials by wet grinding, wherein the Rb element in the RbI is doped in the Cs element in the CsI in an A-site doping manner.
2. The scintillator thin film according to claim 1, characterized in that: The grinding time is 3 to 12 hours; The grinding speed is 500-2000 r / min.
3. A method for preparing a scintillator thin film, characterized in that: The preparation method comprises: A solid material of RbI, CsI and CuI with a molar ratio of 0.3:3:2 and a solvent insoluble in the solid material are ground by a wet grinding method to obtain a copper-based halide powder, wherein the Rb element in the RbI is doped into the Cs element in the CsI in an A-site doping manner; The copper-based halide powder, the polymer composite material and the dispersant are mixed to obtain a powder dispersion, wherein the particle size of the copper-based halide powder is less than 1 μm; The powder dispersion is subjected to film formation to obtain the scintillator thin film used in an X-ray flat panel detector.
4. The preparation method according to claim 3, characterized in that: The film-making method includes at least one of the following: drip coating, blade coating, and spray coating; The mass ratio of the copper-based halide powder to the polymer composite material is 1:1 to 500:1; The polymer composite material comprises at least one of the following: polymethyl methacrylate, polydimethylsiloxane, polyvinyl alcohol, polyvinyl butyral, polystyrene; The dispersant includes at least one of the following: dimethylformamide, dimethyl sulfoxide, γ-hydroxybutyrolactone, β-mercaptoethanol, nitrogen methyl pyrrolidone, dimethylacetamide, anhydrous ethanol and toluene.
5. Application of copper-based halide powder or scintillator film in the field of radiation detectors; in, The copper-based halide powder is the copper-based halide powder according to any one of claims 1 to 2; The scintillator film is the scintillator film according to any one of claims 1 to 2 or a scintillator film prepared by the preparation method according to any one of claims 3 to 4.
Citation Information
Cited By
Copper-based halide powder, scintillator film, preparation method and application thereof