A toughened high barrier plastic particle and preparation method thereof

By adding modified EVOH and modified magnesium hydroxide to medical polyethylene materials, the problems of insufficient brittleness, high temperature resistance and flame retardancy of the materials are solved, and high temperature resistance, high flame retardancy and toughening are prepared. High barrier plastic particles, suitable for medical packaging materials.

CN118599206BActive Publication Date: 2024-11-22QINGDAO SHENGDEHAISI MEDICAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410827575.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-22
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

Existing medical polyethylene materials have problems such as brittleness, poor high temperature resistance and poor flame retardancy, which is difficult to meet the needs of medical packaging materials for toughening, high temperature resistance and high flame retardancy.

Method used

High-density polyethylene is used as the main component, combined with modified EVOH, composite filler and dispersant, and modified treatment is carried out by graphene oxide, 4-methoxybenzene diazotetrafluoroborate, aniline and cypress lactone. Improve the barrier, heat resistance and mechanical properties of the material, and improve flame retardant and toughness by modifying magnesium hydroxide with palmitic acid and melamine-formaldehyde resin.

Benefits of technology

Toughened high-barrier plastic particles with high temperature resistance, high flame retardancy, good toughening and high barrier properties were prepared. They are suitable for the field of medical polymer materials, significantly improving the durability and commercial application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910955850000081
    Figure BDA0004910955850000081
Patent Text Reader

Abstract

The present invention provides a toughened high-barrier plastic particle and a preparation method thereof. The toughened high-barrier plastic particle includes the following raw materials, by weight: 70-80 parts of PE, 4-10 parts of modified EVOH, 5-10 parts of composite filler, 1-3 parts of dispersant, 0.5-2 parts of antioxidant, and 0.5-2 parts of lubricant. The plastic particles provided by the present invention have high temperature resistance, high flame retardancy, good toughening and high barrier properties, can be widely used in the field of medical polymer materials, and have good commercial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of medical polymer materials, and in particular to toughened high-barrier plastic particles and a preparation method thereof. Background Art

[0002] The barrier property of a material refers to its ability to prevent the penetration of small molecules, including water molecules, oxygen, nitrogen, carbon dioxide, etc., which can play a good protective role. Materials with barrier properties can be widely used in food, medical, cosmetics and other packaging fields. In the medical field, with the continuous development of my country's medical level, people have put forward higher requirements for the barrier properties of packaging materials, which not only need to have good barrier properties, but also need to have functional properties such as toughening and high temperature resistance.

[0003] In the medical field, PE (polyethylene) is favored by people because of its light weight, high strength, good chemical stability and good barrier properties. However, PE still has some unresolved defects. For example, PE has a certain brittleness, which leads to a decrease in toughness after long-term use or storage; PE has a low melting point and is easily affected by high temperature environment, and has poor high temperature resistance. In addition, PE itself does not have flame-retardant functional groups and properties, resulting in its poor flame retardancy.

[0004] Patent CN 111635603A discloses a high-barrier medical composite material and a preparation method thereof. The high-barrier medical composite material prepared in this application includes components such as nano-titanium dioxide, citric acid, and polyvinylidene chloride, and has good oxygen and water barrier properties, as well as good antibacterial properties. However, it does not mention the improvement of the toughness and high-temperature resistance of the prepared high-barrier medical composite material, which results in certain limitations in its use. Patent CN 101768302B discloses a preparation method for a high-barrier polyethylene / nylon 6 in-situ nanocomposite material. This application is prepared from raw materials such as polyethylene, caprolactam, montmorillonite, and a compatibilizer, and has excellent barrier properties to air, hydrocarbon solvents, and moisture. However, it does not solve the problems of poor flame retardancy and poor high-temperature resistance of polyethylene, and has the defect of insufficient durability.

[0005] Therefore, there is an urgent need in the market for a high-barrier plastic particle with high temperature resistance, high flame retardancy and good toughness. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention selects PE as the main component, and then adds modified EVOH, composite fillers and dispersants to prepare a toughened high-barrier plastic particle, which has the advantages of high temperature resistance, high flame retardancy, good toughness and high barrier.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] On one hand, the present invention provides a toughened high-barrier plastic particle. The toughened high-barrier plastic particle includes the following raw materials, calculated by weight: 70-80 parts of PE, 4-10 parts of modified EVOH, 5-10 parts of composite filler, 1-3 parts of dispersant, 0.5-2 parts of antioxidant, and 0.5-2 parts of lubricant.

[0009] In some embodiments of the present invention, the PE is high-density polyethylene with a density of 0.941-0.965 g / cm 3 .

[0010] The applicant selected a density of 0.941-0.965 g / cm 3 High-density polyethylene, as the main component of toughened high-barrier plastic particles, has good mechanical properties, heat resistance and chemical stability, and its density is higher than that of ordinary polyethylene, which makes it have a higher degree of crystallinity and thus has good barrier properties.

[0011] In some embodiments of the present invention, the method for preparing the modified EVOH comprises the following steps:

[0012] (1) adding graphene oxide to an aqueous solution of sodium dodecyl sulfate, stirring, ultrasonicating, heating, adding hydrazine hydrate, stirring, adding 4-methoxybenzenediazonium tetrafluoroborate, stirring, filtering, washing, drying, and grinding to obtain a solid 1 for standby use;

[0013] (2) taking the solid 1 of step (1), adding deionized water, and ultrasonicating to obtain solution 1 for use; adding EVOH to the acetic acid solution, heating, and stirring to obtain solution 2 for use; adding aniline and ammonium persulfate to the hydrochloric acid solution, and ultrasonicating to obtain solution 3 for use;

[0014] (3) adding solution 1 of step (2) to solution 2, adding dilute hydrochloric acid, stirring, adding solution 3 dropwise, stirring, washing, filtering, and drying to obtain solid 2 for later use;

[0015] (4) The solid 2 of step (3) and triphenylphosphine are dissolved in tetrahydrofuran, stirred, dalbergia lactone is added, stirred, diethyl azodicarboxylate and 3,5-di-tert-butyl-4-hydroxytoluene are added, stirred, methanol is added, filtered, and dried to obtain modified EVOH.

[0016] Among them, the ethylene content of EVOH is 35-40%.

[0017] The present invention does not impose any special restrictions on the source of the EVOH, which can be purchased from commercial sources, including but not limited to Dongguan Changping Pingzhi Plastic Raw Materials Trading Company.

[0018] In some embodiments of the present invention, in step (1), the mass ratio of graphene oxide to 4-methoxybenzenediazonium tetrafluoroborate is 1:(72-74); in step (4), the mass ratio of solid 2 to dalbergia lactone is 1:(0.2-0.6).

[0019] Preferably, in step (1), the mass ratio of graphene oxide to 4-methoxybenzenediazonium tetrafluoroborate is 1:73; in step (4), the mass ratio of solid 2 to dalbergia lactone is 1:0.4.

[0020] EVOH (ethylene-vinyl alcohol copolymer) is a chain-like structure formed by alternating ethylene and vinyl alcohol. The presence of vinyl alcohol units makes EVOH hydrophilic to a certain extent, while ethylene units make it hydrophobic to a certain extent. This alternating structure makes EVOH highly transparent and has excellent gas barrier properties, and is widely used in packaging materials, medical materials, etc. However, since EVOH molecules contain hydroxyl groups, which make them highly hydrophilic and hygroscopic, the barrier properties of EVOH will decrease significantly after absorbing moisture, and the vinyl alcohol units in EVOH make it poorly heat-resistant.

[0021] On the one hand, the applicant selected graphene oxide with a lamellar structure to modify EVOH. Graphene oxide has a good barrier effect on oxygen and the like due to its large specific surface area and good mechanical strength. The applicant also used 4-methoxybenzenediazonium tetrafluoroborate to covalently modify graphene oxide. While ensuring the integrity of the graphene oxide nanosheet structure, the applicant introduced benzyloxy and fluorine groups, thereby improving the thermal stability and hydrophobicity of graphene oxide, and improving the barrier effect of graphene oxide on moisture, thereby improving the barrier effect of EVOH. On the other hand, the applicant also introduced aniline to modify E VOH is modified, and the introduction of benzene ring makes EVOH have better heat resistance and mechanical properties. Furthermore, NB coordination bond is formed between amino group and 4-methoxybenzenediazonium tetrafluoroborate, which improves the stability of EVOH and thus improves the heat resistance of EVOH. On the other hand, the applicant introduces dalbergia lactone to modify EVOH, and introduces the coumarin functional group in dalbergia lactone into the side chain of EVOH, which has antibacterial, anti-ultraviolet absorption and antioxidant properties, and the applicant forms a stable CO-aryl chemical bond by controlling the reaction conditions, thereby improving the mechanical properties and heat resistance of EVOH.

[0022] In some embodiments of the present invention, the composite filler is a mixture of silicon dioxide and modified magnesium hydroxide in a mass ratio of 1:(3-5).

[0023] Preferably, the mass ratio of the silicon dioxide to the modified magnesium hydroxide is 1:4.

[0024] Silica has the characteristics of high temperature resistance and high strength, which can effectively improve the toughness of PE. Silica also has good hydrophobicity, which can improve the barrier properties of plastic particles. Silica and magnesium hydroxide can work together to improve the flame retardant properties of composite fillers.

[0025] In some embodiments of the present invention, the method for preparing the modified magnesium hydroxide comprises the following steps:

[0026] 1) Mix formaldehyde, melamine and deionized water, add alkali solution to adjust pH to 8-10, heat to 65-75° C., and stir to obtain a mixed solution for use;

[0027] 2) Take the mixed solution of step 1), add magnesium hydroxide, palmitic acid and anhydrous ethanol, heat to 90-100° C., stir, filter and dry to obtain modified magnesium hydroxide.

[0028] In some embodiments of the present invention, in step 2), the mass ratio of magnesium hydroxide to palmitic acid is 1:(0.015-0.025).

[0029] Preferably, in step 2), the mass ratio of magnesium hydroxide to palmitic acid is 1:0.02.

[0030] Magnesium hydroxide is a non-toxic and environmentally friendly flame retardant commonly used in PE materials. However, due to its strong surface polarity, its compatibility with PE is poor. On the one hand, the applicant uses palmitic acid with a long alkyl chain to modify magnesium hydroxide. A stable chemical bond is formed between the carboxyl group of palmitic acid and the hydroxyl group of magnesium hydroxide. The tail chain of palmitic acid is fixed to the PE matrix through physical entanglement and van der Waals force, thereby improving the compatibility of magnesium hydroxide and PE. At the same time, the long-chain alkyl group can make the modified magnesium hydroxide have good mechanical properties, so that magnesium hydroxide can have a toughening effect in plastic particles. Effect; on the other hand, the applicant uses formaldehyde and melamine to synthesize melamine-formaldehyde resin to modify magnesium hydroxide. Melamine-formaldehyde resin has good flame retardancy and higher compatibility with PE, thereby improving the flame retardancy of the modified magnesium hydroxide and its compatibility with PE. At the same time, the amino group in melamine and the hydroxyl group in magnesium hydroxide produce hydrogen bonds, thereby improving the stability of the modified magnesium hydroxide and thereby improving the toughness of the plastic particles; further, hydrogen bonding occurs between melamine and palmitic acid, thereby improving the stability of the modified magnesium hydroxide and improving the toughness of the plastic particles.

[0031] In some embodiments of the present invention, the dispersant is a polyacrylic acid type dispersant.

[0032] In some embodiments of the present invention, the antioxidant 1010 or the antioxidant 168.

[0033] In some embodiments of the present invention, the lubricant is calcium stearate or zinc stearate.

[0034] Another aspect of the present invention further provides a method for preparing the toughened high barrier plastic particles described in the above technical solution, comprising the following steps:

[0035] S1. Add PE, modified EVOH, composite filler, dispersant, antioxidant and lubricant into a reaction kettle, heat to 130-150° C., stir for 20-40 min, and obtain a mixture for standby use;

[0036] S2. Extruding the mixture obtained in step S1 at 160-180° C., cooling, pelletizing, sieving, and drying to obtain toughened high-barrier plastic particles.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The present invention uses PE as the main component, and then adds modified EVOH, composite fillers and dispersants to prepare a toughened high-barrier plastic particle. Through the synergistic effect of the components, the plastic particle has the characteristics of high temperature resistance, high flame retardancy, good toughness and high barrier.

[0039] (2) The present invention uses EVOH as a barrier material, modifies it with graphene oxide and dalbergia lactone, and modifies the graphene oxide with 4-methoxybenzenediazonium tetrafluoroborate, thereby improving the barrier effect, heat resistance and moisture resistance of EVOH, thereby improving the barrier properties and toughness of the plastic particles.

[0040] (3) The present invention introduces palmitic acid and melamine-formaldehyde resin to modify magnesium hydroxide with good flame retardancy, thereby improving the compatibility of magnesium hydroxide with PE and the stability of magnesium hydroxide, thereby playing a toughening role on plastic particles.

[0041] (4) The plastic particles prepared by the present invention have high temperature resistance, high flame retardancy, good toughness and high barrier properties, can be widely used in the field of medical polymer materials, and have good commercial application value. DETAILED DESCRIPTION

[0042] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0043] In the following examples and comparative examples, except for modified EVOH and modified magnesium hydroxide, the other compound monomers and related reagents used can be purchased from the market. Among them, the density of PE is 0.960 g / cm3 , purchased from Langfang Wanfu Insulation Materials Co., Ltd.; the ethylene content of EVOH is 38%, purchased from Dongguan Changping Pingzhi Plastic Raw Materials Trading Co., Ltd.; the particle size of silicon dioxide is 50nm, purchased from Xi'an Qiyue Biotechnology Co., Ltd.; the particle size of magnesium hydroxide is 3μm, purchased from Wuhan Kemik Biomedical Technology Co., Ltd.; melamine was purchased from Wujiang Huaxu Chemical Technology Co., Ltd.; the model of polyacrylic acid type dispersant is kpl-030201, purchased from Shandong Kepler Biotechnology Co., Ltd.

[0044] Preparation Example 1

[0045] The synthesis method of modified EVOH-1 comprises the following steps:

[0046] (1) 30 mg of graphene oxide was added to 30 ml of 1 wt% sodium dodecyl sulfate aqueous solution, stirred for 1 h, ultrasonicated for 10 min, heated to 80° C., 1 ml of hydrazine hydrate was added, stirred for 24 h, 2.2 g of 4-methoxybenzenediazonium tetrafluoroborate was added, stirred for 30 min, filtered, washed with deionized water 3 times, dried at 60° C. for 12 h, and ground to obtain solid 1 for later use;

[0047] (2) Take 20 mg of the solid 1 of step (1), add 20 ml of deionized water, and ultrasonicate for 30 min to obtain solution 1 for use; add 30 g of EVOH to 200 ml of 30 wt% acetic acid solution, heat to 70° C., and stir for 30 min to obtain solution 2 for use; add 125 mg of aniline and 100 g of ammonium persulfate to 10 ml of 1 mol / L hydrochloric acid solution, and ultrasonicate for 15 min to obtain solution 3 for use;

[0048] (3) Add solution 1 of step (2) to solution 2, add 10 ml of 1 mol / L dilute hydrochloric acid, stir for 30 min, add solution 3 dropwise, stir for 12 h, wash with anhydrous ethanol and deionized water three times respectively, filter, and dry in vacuo at -40 ° C for 24 h to obtain solid 2 for standby use;

[0049] (4) Dissolve 10 g of the solid 2 obtained in step (3) and 3.9 g of triphenylphosphine in 50 ml of tetrahydrofuran, stir for 10 min, add 4 g of dalbergia lactone, stir for 15 min, add 2.6 g of diethyl azodicarboxylate and 0.5 g of 3,5-di-tert-butyl-4-hydroxytoluene, stir for 12 h, add 30 ml of methanol, filter, and dry at 60 ° C for 24 h to obtain modified EVOH-1.

[0050] Preparation Example 2

[0051] The specific implementation method of modified EVOH-2 is the same as that of modified EVOH-1, except that in step (1), the mass of 4-methoxybenzenediazonium tetrafluoroborate is replaced with 1.4 g.

[0052] Preparation Example 3

[0053] The specific implementation method of modified EVOH-3 is the same as that of modified EVOH-1, except that in step (4), the mass of dalbergia lactone is replaced with 1.5 g.

[0054] Preparation Example 4

[0055] The synthetic method of modified magnesium hydroxide A comprises the following steps:

[0056] 1) 0.3 mol formaldehyde, 0.1 mol melamine and 50 ml deionized water were mixed, 1 mol / L NaOH solution was added to adjust the pH to 9, heated to 70° C., and stirred for 1 h to obtain a mixed solution for use;

[0057] 2) 10 g of magnesium hydroxide, 0.2 g of palmitic acid and 40 ml of anhydrous ethanol were added to the mixed solution of step 1), heated to 95° C., stirred for 30 min, filtered, and dried at 60° C. for 12 h to obtain modified magnesium hydroxide A.

[0058] Preparation Example 5

[0059] The specific implementation manner of modified magnesium hydroxide B is the same as that of modified magnesium hydroxide A, except that in step 2), the mass of palmitic acid is replaced with 0.1 g.

[0060] Example 1

[0061] A toughened high-barrier plastic particle. The toughened high-barrier plastic particle includes the following raw materials by weight: 75 parts of PE, 7 parts of modified EVOH-1, 7.5 parts of composite filler, 12 parts of polyacrylic acid type dispersant kpl-03020, 1.25 parts of antioxidant 1010, and 1.25 parts of calcium stearate.

[0062] The composite filler is a mixture of silicon dioxide and modified magnesium hydroxide A, with a mass ratio of 1:4.

[0063] The preparation method of toughened high barrier plastic particles in this embodiment comprises the following steps:

[0064] S1, adding PE, modified EVOH-1, composite filler, polyacrylic acid type dispersant kpl-030201, antioxidant 1010 and calcium stearate into a reaction kettle, heating to 140°C, stirring for 30 minutes, and obtaining a mixture for use;

[0065] S2. Extruding the mixture obtained in step S1 at 170° C., cooling to room temperature, pelletizing, sieving, removing pellets larger than 5 mm, and drying at 80° C. for 12 h to obtain toughened high-barrier plastic pellets.

[0066] Example 2

[0067] A toughened high-barrier plastic particle. The toughened high-barrier plastic particle includes the following raw materials by weight: 70 parts of PE, 17 parts of modified EVOH, 5 parts of composite filler, 11 parts of polyacrylic acid type dispersant kpl-03020, 1680.5 parts of antioxidant, and 0.5 parts of zinc stearate.

[0068] The composite filler is a mixture of silicon dioxide and modified magnesium hydroxide A, with a mass ratio of 1:3.

[0069] The preparation method of toughened high barrier plastic particles in this embodiment comprises the following steps:

[0070] S1, adding PE, modified EVOH-1, composite filler, polyacrylic acid type dispersant kpl-030201, antioxidant 168 and zinc stearate into a reaction kettle, heating to 130°C, stirring for 20 minutes, and obtaining a mixture for use;

[0071] S2. Extruding the mixture obtained in step S1 at 160° C., cooling to room temperature, pelletizing, sieving, removing pellets larger than 5 mm, and drying at 80° C. for 12 h to obtain toughened high-barrier plastic particles.

[0072] Example 3

[0073] A toughened high-barrier plastic particle. The toughened high-barrier plastic particle includes the following raw materials by weight: 80 parts of PE, 17 parts of modified EVOH-1, 10 parts of composite filler, 2013 parts of polyacrylic acid type dispersant kpl-030, 10102 parts of antioxidant, and 2 parts of calcium stearate.

[0074] The composite filler is a mixture of silicon dioxide and modified magnesium hydroxide A, with a mass ratio of 1:5.

[0075] The preparation method of toughened high barrier plastic particles in this embodiment comprises the following steps:

[0076] S1, adding PE, modified EVOH-1, composite filler, polyacrylic acid type dispersant kpl-030201, antioxidant 1010 and calcium stearate into a reaction kettle, heating to 150°C, stirring for 40 minutes, and obtaining a mixture for standby use;

[0077] S2. Extruding the mixture obtained in step S1 at 180° C., cooling to room temperature, pelletizing, sieving, removing pellets larger than 5 mm, and drying at 80° C. for 12 h to obtain toughened high-barrier plastic particles.

[0078] Example 4

[0079] A toughened high-barrier plastic particle. The toughened high-barrier plastic particle includes the following raw materials, calculated by weight: 72 parts of PE, 14 parts of modified EVOH-1, 6 parts of composite filler, 11.5 parts of polyacrylic acid type dispersant kpl-03020, 10101 parts of antioxidant, and 1 part of calcium stearate.

[0080] The composite filler is a mixture of silicon dioxide and modified magnesium hydroxide A, with a mass ratio of 1:4.

[0081] The preparation method of the toughened high barrier plastic particles in this embodiment is the same as that in Example 1.

[0082] Example 5

[0083] A toughened high-barrier plastic particle. The toughened high-barrier plastic particle includes the following raw materials by weight: 78 parts of PE, 10 parts of modified EVOH-1, 9 parts of composite filler, 12.5 parts of polyacrylic acid type dispersant kpl-03020, 1.5 parts of antioxidant 1010, and 1.5 parts of calcium stearate.

[0084] The composite filler is a mixture of silicon dioxide and modified magnesium hydroxide A, with a mass ratio of 1:4.

[0085] The preparation method of the toughened high barrier plastic particles in this embodiment is the same as that in Example 1.

[0086] Example 6

[0087] This embodiment provides a toughened high-barrier plastic particle and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified EVOH-2 replaces the modified EVOH-1 in equal amounts.

[0088] Example 7

[0089] This embodiment provides a toughened high-barrier plastic particle and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified EVOH-3 replaces the modified EVOH-1 in equal amounts.

[0090] Example 8

[0091] This embodiment provides a toughened high-barrier plastic particle and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that modified magnesium hydroxide B replaces modified magnesium hydroxide A in equal amounts.

[0092] Comparative Example 1

[0093] This comparative example provides a toughened high-barrier plastic particle and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that EVOH is used instead of modified EVOH-1.

[0094] Comparative Example 2

[0095] This comparative example provides a toughened high-barrier plastic particle and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that magnesium hydroxide is used instead of modified magnesium hydroxide A.

[0096] Performance Testing

[0097] The plastic particles of the above Examples 1-8 and Comparative Examples 1-2 were made into films to test their toughness and barrier properties. The test results are shown in Table 1.

[0098] The process of making plastic granules into film is as follows:

[0099] The plastic particles are melted and extruded to obtain a film with a melting temperature of 190° C. and a thickness of 0.2 mm.

[0100] (1) Toughness

[0101] The toughness is determined by testing the tensile strength of the film, referring to the standard GB / T 1040-2006.

[0102] (2) Barrier properties

[0103] ① Water barrier property: Test the water vapor permeability of the film, refer to the standard GB / T 21529-2008;

[0104] ② Oxygen barrier property: Test the oxygen permeability of the film, refer to the standard GB / T 1038-2000.

[0105] Table 1

[0106]

[0107] It can be seen from the data in Table 1 that the plastic particles in Examples 1-5 of the present invention have relatively high tensile strength, water vapor permeability and oxygen permeability as a whole, that is, they have good toughness and barrier properties. Among them, Examples 6-7 changed the modification ratio of 4-methoxybenzenediazo tetrafluoroborate to graphene oxide in the modified EVOH and the modification ratio of dalbergia lactone to EVOH, so that the high temperature resistance and moisture resistance of EVOH were not well improved, and the stability and mechanical properties were not well improved, resulting in the reduction of the toughness and barrier properties of the film made of plastic particles; Example 8 changed the ratio between magnesium hydroxide and palmitic acid in the modified magnesium hydroxide, so that the compatibility of magnesium hydroxide and PE was not well improved and the introduction ratio of long-chain alkanes in palmitic acid was insufficient, resulting in the reduction of the toughness and barrier properties of the film made of plastic particles; Comparative Examples 1-2 respectively selected EVOH and magnesium hydroxide to replace modified EVOH-1 and modified magnesium hydroxide A, and the test found that the toughness and barrier properties of the film prepared by plastic particles showed poor results.

[0108] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A toughened high barrier plastic particle, It is characterized in that The toughened high barrier plastic particles include the following raw materials in parts by weight: 70-80 parts of PE, 4-10 parts of modified EVOH, 5-10 parts of composite filler, 1-3 parts of dispersant, 0.5-2 parts of antioxidant, and 0.5-2 parts of lubricant; The preparation method of the modified EVOH comprises the following steps: (1) adding graphene oxide to an aqueous solution of sodium dodecyl sulfate, stirring, ultrasonicating, heating, adding hydrazine hydrate, stirring, adding 4-methoxybenzenediazonium tetrafluoroborate, stirring, filtering, washing, drying, and grinding to obtain a solid 1 for later use; (2) Take the solid 1 of step (1), add deionized water, and ultrasonicate to obtain solution 1 for use; add EVOH to the acetic acid solution, heat, and stir to obtain solution 2 for use; add aniline and ammonium persulfate to the hydrochloric acid solution, and ultrasonicate to obtain solution 3 for use; (3) adding solution 1 of step (2) into solution 2, adding dilute hydrochloric acid, stirring, adding solution 3 dropwise, stirring, washing, filtering, and drying to obtain solid 2 for later use; (4) dissolving the solid 2 obtained in step (3) and triphenylphosphine in tetrahydrofuran, stirring, adding dalbergia lactone, stirring, adding diethyl azodicarboxylate and 3,5-di-tert-butyl-4-hydroxytoluene, stirring, adding methanol, filtering, and drying to obtain modified EVOH; In the step (1), the mass ratio of graphene oxide to 4-methoxybenzenediazonium tetrafluoroborate is 1:(72-74); in the step (4), the mass ratio of solid 2 to dalbergia lactone is 1:(0.2-0.6); The composite filler is a mixture of silicon dioxide and modified magnesium hydroxide, with a mass ratio of 1:(3-5); The preparation method of the modified magnesium hydroxide comprises the following steps: 1) Mix formaldehyde, melamine and deionized water, add alkali solution to adjust pH to 8-10, heat to 65-75℃, stir to obtain a mixed solution for use; 2) taking the mixed solution of step 1), adding magnesium hydroxide, palmitic acid and anhydrous ethanol, heating to 90-100° C., stirring, filtering and drying to obtain modified magnesium hydroxide; In the step 2), the mass ratio of magnesium hydroxide to palmitic acid is 1:(0.015-0.025).

2. The toughened high barrier plastic particles according to claim 1, It is characterized in that The PE is high-density polyethylene with a density of 0.941-0.965 g / cm 3 .

3. The toughened high barrier plastic particles according to claim 1, It is characterized in that The dispersant is a polyacrylic acid type dispersant.

4. The toughened high barrier plastic particles according to claim 1, It is characterized in that The lubricant is calcium stearate or zinc stearate.

5. A method for preparing the toughened high barrier plastic particles according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1. Add PE, modified EVOH, composite filler, dispersant, antioxidant and lubricant into a reaction kettle, heat to 130-150° C., stir for 20-40 min, and obtain a mixture for standby use; S2. Extruding the mixture obtained in step S1 at 160-180° C., cooling, pelletizing, sieving, and drying to obtain toughened high-barrier plastic particles.