A kind of high purity polyphenylene sulfide and preparation method thereof
Through the combination of solution polymerization method and nanomolecular sieve, the problem of removing oligomers and volatile impurities in polyphenylene sulfide is solved, and the preparation of high-purity polyphenylene sulfide is achieved, which meets the application needs in high-standard fields and reduces the Energy consumption and cost.
Patent Information
- Application Number
- CN202411096501.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The prior art is difficult to achieve the preparation of high-purity polyphenylene sulfides, especially in removing oligomers and volatile impurities inside the resin, resulting in limited application in the field of corrosion.
Using solution polymerization method, under the protection of inert gas, catalyst, sodium sulfide hydrated and alkali are used to perform dehydration reaction in organic solvents, nanomolecular sieve and para-dichlorobenzene are added, and ethylene carbonate, sulfolane and The mixed solvent of tetraethylene glycol is washed at high temperature, and the molecular sieve is adsorbed and removed impurities to improve the purity of polyphenylene sulfide.
The preparation of high-purity polyphenylene sulfide is achieved, which reduces energy consumption and operating costs, improves the purity of polyphenylene sulfide, and meets the use requirements in the fields of 3D printing, coatings and gas packaging.
Smart Images

Figure CN118620206B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to high-purity polyphenylene sulfide and a preparation method thereof, belonging to the technical field of high molecular polymer preparation. Background Art
[0002] Polyphenylene sulfide is abbreviated as PPS, and its full name is polyphenylene sulfide, also known as polyphenylene sulfide. It is a special engineering plastic that began industrial production in the United States in 1973. It has excellent heat resistance, chemical corrosion resistance, flame retardancy, and insulation. Its strength and hardness are both high, and its mechanical properties are excellent. The product has good dimensional stability and can be processed by a variety of processing methods, and can be precisely formed. Due to the good affinity of polyphenylene sulfide with inorganic fillers and reinforcing fibers and its good compatibility with other polymer materials, it can be made into different reinforced filling varieties and polymer alloys, and has a wide range of uses.
[0003] Polyphenylene sulfide can be processed by injection molding, pressing, sintering, calendering and other methods to obtain products. The related devices made of it can withstand the erosion of some corrosive media such as soldering liquid and cleaning agent, and do not need to add flame retardants, have low hygroscopicity and excellent electrical insulation. At the same time, polyphenylene sulfide has outstanding adhesion and can also be made into packaging materials for electronic components and integrated circuits with special requirements, such as resistors, capacitors, transistors, varistors and other devices. At the same time, the current automotive field is developing towards light weight and low cost. Polyphenylene sulfide can replace some metal materials due to its low density, light weight, heat resistance and stable size, and can be made into some parts in automobiles, such as water tank water chamber, carburetor, clutch, exhaust treatment device parts, lamp holder, oil pump, etc. Due to its excellent comprehensive performance, PPS plastic is made into an increasing number of parts for various purposes, and its application potential is very huge.
[0004] Polyphenylene sulfide is mainly used as an anti-corrosion material and can be used for plastic parts or coated parts. It is particularly widely used in the fields of 3D printing, coatings, and gas packaging. Polyphenylene sulfide prepared by existing technology cannot be directly used in the field of corrosion because the purity of polyphenylene sulfide cannot meet the use requirements. The main difficulty in purifying polyphenylene sulfide is that the general washing method can only remove the ions and oligomers on its surface, and is often powerless to remove impurities wrapped in the resin. Special methods must be studied and used to remove the oligomers and volatile impurities wrapped therein. Summary of the invention
[0005] In view of this, the present invention provides a high-purity polyphenylene sulfide and a preparation method thereof, which realizes the preparation of high-purity polyphenylene sulfide with lower energy consumption and safer operation process.
[0006] To achieve the above object, the present invention provides a method for preparing high-purity polyphenylene sulfide, comprising the following steps:
[0007] (1) Under the protection of inert gas, the catalyst, hydrated sodium sulfide and alkali are dispersed in an organic solvent, and an anhydrous sodium sulfide solution is obtained after dehydration reaction;
[0008] (2) After the solution is cooled, add p-dichlorobenzene and mix well; then heat to 220-240°C and react for 1-2 hours, add nano molecular sieves, and continue to react for 3-5 hours;
[0009] (3) End the reaction and cool to 130-160°C, add into 50-60°C warm water for precipitation, and obtain precipitated particles;
[0010] (4) adding the precipitated particles into a mixed solvent consisting of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 170-180° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: (5-8) mL: (2-4) mL: 1 mL;
[0011] (5) The product obtained in step (4) is washed with ethanol and deionized water respectively, and dried to obtain high-purity polyphenylene sulfide.
[0012] The present invention adopts a solution polymerization method to prepare polyphenylene sulfide. The nano molecular sieve added during the polymerization process has a siphon effect. The organic monomer particles are small and can pass freely; the high molecular polymer is large in volume and cannot be adsorbed by the molecular sieve; and small molecular impurities such as oligomers are easily adsorbed by the molecular sieve. That is, the molecular sieve can enhance the mechanical properties and adsorption. It can not only adsorb the polar water generated by the reaction, but more importantly, it can adsorb the impurities generated during the reaction to prevent the impurities from being coated inside by polyphenylene sulfide, which is not conducive to subsequent washing. After the polymerization reaction is completed, the polymer and the slurry need to be separated by precipitation. At the same time, other products generated during the reaction, such as solvents and a very small amount of unreacted monomers, are also attached to the polyphenylene sulfide resin. The solvent needs to be removed by washing, and there is also a very small amount of unreacted monomers, so that a relatively pure polyphenylene sulfide resin can be obtained. After the reaction of the present invention is completed, the polymer reduced to 130-160°C is directly put into warm water without cooling to room temperature to precipitate the polyphenylene sulfide. The residual heat of the polymer is used to heat the water, and the heat exchange process between the polymer and water is used to increase the porosity of the polymer particles, which is beneficial to the exposure of the molecular sieve and the subsequent washing process. Further, the solution is cooled to 140-150°C, which is conducive to sufficient washing with warm water and can form a certain temperature difference with warm water, so that cracks are formed in the polyphenylene sulfide during the quenching process, which is convenient for subsequent washing with organic solvents.
[0013] During the precipitation process, various salts and impurities on the surface of the polymer have been dissolved in water and separated. Subsequently, the precipitated particles are transferred to a mixed solvent consisting of ethylene carbonate, cyclopentane sulfone and tetraethylene glycol, and washed at 170-180°C. At this temperature, polyphenylene sulfide can fully swell, and the polyphenylene sulfide molecular chain slowly creeps and fully stretches out; in the presence of solvents, the activity space of the molecular chain becomes larger, and the molecular sieve wrapped by polyphenylene sulfide is more easily exposed due to its poor compatibility with the resin; thus, the organic impurities adsorbed by the molecular sieve are taken away from the polyphenylene sulfide matrix under the action of the solvent, and the molecular sieve undergoes desorption, thereby removing the impurities adsorbed by the molecular sieve in the polymer. Among them, ethylene carbonate, as a high-boiling point organic solvent, has good wettability with polyphenylene sulfide and can improve the washing effect; cyclopentane has good compatibility with the oligomers generated during the polymerization process, can reduce the amount of solvent used, and improve the filling factor of the purification device; and tetraethylene glycol is a straight-chain organic solvent containing polyhydroxyl groups, and the molecular chain has good flexibility, can be folded into holes of different sizes, easily enter the interior of the polymer and molecular sieve, and can play a role in phase transfer for impurities such as ions. The present invention uses ethylene carbonate, cyclopentane and tetraethylene glycol as mixed solvents, which can give full play to the role of each component, play a synergistic effect, and improve the washing effect. During the washing process, the washing temperature should be controlled to be 170-180°C; if the temperature is too low, the polymer cannot be fully swollen, and the motion performance of the polymer molecular chain and tetraethylene glycol molecules is reduced, which is not conducive to the full exposure and cleaning of the molecular sieve; if the temperature is too high, the washing effect is limited, and the stability of the polymer is affected under the action of the solvent.
[0014] Furthermore, in step (1), the inert gas is nitrogen.
[0015] Furthermore, in step (1), the catalyst is one or more of sodium formate, lithium formate, lithium carbonate, lithium acetate, lithium benzoate, and lithium chloride; the hydrated sodium sulfide is sodium sulfide nonahydrate; and the base is sodium hydroxide.
[0016] Furthermore, in step (1), the organic solvent is N-methylpyrrolidone.
[0017] Furthermore, the dehydration reaction temperature in step (1) is 170-190°C.
[0018] Furthermore, in step (2), the temperature is lowered to 120-130° C.; the nano molecular sieve is one or more of type A molecular sieve, type X molecular sieve, and type Y molecular sieve with a particle size of 50-200 nm.
[0019] Furthermore, the amounts of materials used in step (1) and step (2) are respectively: 8-12 parts by weight of catalyst, 120-140 parts by weight of hydrated sodium sulfide, 1-2 parts by weight of alkali, 250-300 parts by weight of organic solvent, 70-80 parts by weight of p-dichlorobenzene, and 5-10 parts by weight of molecular sieve.
[0020] Furthermore, the product in step (5) is washed with ethanol for 1-3 times and with deionized water for 3-5 times.
[0021] Furthermore, the drying in step (5) is carried out in a vacuum drying oven.
[0022] On the other hand, the present invention also provides a high-purity polyphenylene sulfide, which has high purity and corrosion resistance and can meet the use requirements in the fields of 3D printing, coatings, gas packaging, etc.
[0023] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0024] It can be seen from the synthesis method and process of polyphenylene sulfide resin that industrially synthesized polyphenylene sulfide resin contains a large amount of impurities and cannot be directly used in special fields. It is necessary to conduct systematic research on the purification of the resin so that commercial polyphenylene sulfide can be directly used in high-standard fields such as chemical industry. The nano molecular sieve added during the polymerization process has a siphon effect and can play an adsorption role; the impurities are adsorbed into the molecular sieve to prevent the impurities from being coated by the polymer molecular chain, which is not conducive to washing. After the reaction is completed, the present invention does not need to be cooled to room temperature, and the polymer reduced to 130-160°C is directly placed in warm water to precipitate polyphenylene sulfide. The water is heated by the residual temperature of the polymer, and the heat exchange process between the polymer and water is used to increase the porosity of the polymer particles, which is conducive to the exposure of the molecular sieve and the subsequent washing process. The present invention uses ethylene carbonate, cyclopentane sulfone and tetraethylene glycol as a mixed solvent, which can give full play to the role of each component, play a synergistic role, and improve the washing effect. During the washing process, the polymer is fully swollen, the molecular sieve is fully exposed, and the washing effect is greatly improved. The purified PPS resin has greatly reduced impurity content and is widely used in 3D printing, coatings, gas packaging and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings of the embodiment are briefly introduced below.
[0026] Figure 1 This is a scanning electron microscope image of the precipitated particles obtained by precipitation in warm water in Example 8. DETAILED DESCRIPTION
[0027] The above scheme is further described below in conjunction with specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0028] Unless otherwise specified in the following examples, all raw materials are commercially available or prepared by conventional methods in the art. The nano molecular sieve is a type A molecular sieve with a particle size of 100 nm, specifically a type 4A molecular sieve produced by the Catalyst Factory of Nankai University.
[0029] Example 1.
[0030] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0031] (1) Under nitrogen protection, the catalyst lithium carbonate, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 170°C;
[0032] (2) The solution was cooled to 120°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 220°C for reaction for 1 hour, nano molecular sieve was added, and the reaction was continued for 5 hours; the amounts of materials used in step (1) and step (2) were: 8 parts by weight of catalyst, 120 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 250 parts by weight of organic solvent, 70 parts by weight of p-dichlorobenzene, and 5 parts by weight of molecular sieve;
[0033] (3) End the reaction and cool to 140°C, add into 50°C warm water for precipitation, and obtain precipitated particles;
[0034] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 170°C; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 5 mL: 2 mL: 1 mL;
[0035] (5) The product obtained in step (4) is washed once with ethanol and five times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0036] Example 2
[0037] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0038] (1) Under nitrogen protection, the catalyst lithium acetate, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 190°C;
[0039] (2) The solution was cooled to 130°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 240°C for reaction for 2 hours, nano molecular sieve was added, and the reaction was continued for 5 hours; the amounts of materials used in step (1) and step (2) were: 12 parts by weight of catalyst, 140 parts by weight of hydrated sodium sulfide, 2 parts by weight of sodium hydroxide, 300 parts by weight of organic solvent, 80 parts by weight of p-dichlorobenzene, and 10 parts by weight of molecular sieve;
[0040] (3) End the reaction and cool to 150°C, add into 60°C warm water for precipitation, and obtain precipitated particles;
[0041] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 180° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 8 mL: 4 mL: 1 mL;
[0042] (5) The product obtained in step (4) was washed with ethanol for 3 times, deionized water for 3 times, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0043] Example 3
[0044] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0045] (1) Under nitrogen protection, the catalyst lithium benzoate, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 172°C;
[0046] (2) The solution was cooled to 130°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 220°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 5 hours; the amounts of materials used in step (1) and step (2) were: 8 parts by weight of catalyst, 140 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 250 parts by weight of organic solvent, 80 parts by weight of p-dichlorobenzene, and 10 parts by weight of molecular sieve;
[0047] (3) End the reaction and cool to 140°C, add into 60°C warm water for precipitation, and obtain precipitated particles;
[0048] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 170° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 8 mL: 2 mL: 1 mL;
[0049] (5) The product obtained in step (4) is washed once with ethanol and four times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0050] Example 4
[0051] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0052] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 190°C;
[0053] (2) The solution was cooled to 120°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 240°C for reaction for 1.2 hours, nano molecular sieve was added, and the reaction was continued for 3 hours; the amounts of materials used in step (1) and step (2) were: 12 parts by weight of catalyst, 120 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 300 parts by weight of organic solvent, 78 parts by weight of p-dichlorobenzene, and 5 parts by weight of molecular sieve;
[0054] (3) End the reaction and cool to 150°C, add into 50°C warm water for precipitation, and obtain precipitated particles;
[0055] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 180° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 5 mL: 4 mL: 1 mL;
[0056] (5) The product obtained in step (4) was washed with ethanol for 3 times, deionized water for 3 times, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0057] Example 5
[0058] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0059] (1) Under nitrogen protection, the catalyst lithium carbonate, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 178°C;
[0060] (2) The solution was cooled to 122°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 224°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 9 parts by weight of catalyst, 128 parts by weight of hydrated sodium sulfide, 1.2 parts by weight of sodium hydroxide, 280 parts by weight of organic solvent, 76 parts by weight of p-dichlorobenzene, and 6 parts by weight of molecular sieve;
[0061] (3) The reaction was terminated and the temperature was lowered to 142°C, and the mixture was added into 53°C warm water for precipitation to obtain precipitated particles;
[0062] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 172°C; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 2.5 mL: 1 mL;
[0063] (5) The product obtained in step (4) is washed twice with ethanol and five times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0064] Example 6
[0065] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0066] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 185°C;
[0067] (2) The solution was cooled to 127°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 236°C for reaction for 1.8h, nano-molecular sieve was added, and the reaction was continued for 3.5h; the amounts of materials used in step (1) and step (2) were: 11 parts by weight of catalyst, 133 parts by weight of hydrated sodium sulfide, 1.7 parts by weight of sodium hydroxide, 290 parts by weight of organic solvent, 76 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0068] (3) The reaction was terminated and the temperature was lowered to 148°C, and the mixture was added into 58°C warm water for precipitation to obtain precipitated particles;
[0069] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 177°C; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g:7 mL:3.8 mL:1 mL;
[0070] (5) The product obtained in step (4) was washed with ethanol for 3 times, deionized water for 5 times, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0071] Example 7
[0072] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0073] (1) Under nitrogen protection, the catalyst lithium benzoate, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 183°C;
[0074] (2) The solution was cooled to 128°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 232°C and the reaction was continued for 1.7 hours, and the nano molecular sieve was added and the reaction was continued for 4.5 hours; the amounts of materials used in step (1) and step (2) were: 11 parts by weight of catalyst, 132 parts by weight of hydrated sodium sulfide, 1.5 parts by weight of sodium hydroxide, 290 parts by weight of organic solvent, 77 parts by weight of p-dichlorobenzene, and 9 parts by weight of molecular sieve;
[0075] (3) The reaction was terminated and the temperature was lowered to 146°C, and the mixture was added into 54°C warm water for precipitation to obtain precipitated particles;
[0076] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 176°C; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g:5.8 mL:3.2 mL:1 mL;
[0077] (5) The product obtained in step (4) is washed once with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0078] Example 8
[0079] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0080] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0081] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0082] (3) End the reaction and cool to 145°C, add into 55°C warm water for precipitation, and obtain precipitated particles;
[0083] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 3 mL: 1 mL;
[0084] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0085] Example 9
[0086] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0087] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0088] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0089] (3) The reaction was terminated and the temperature was lowered to 130°C, and the mixture was added into 55°C warm water for precipitation to obtain precipitated particles;
[0090] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 3 mL: 1 mL;
[0091] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0092] Example 10
[0093] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0094] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0095] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0096] (3) The reaction was terminated and the temperature was lowered to 160°C, and the mixture was added into 55°C warm water for precipitation to obtain precipitated particles;
[0097] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 3 mL: 1 mL;
[0098] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0099] Comparative Example 1
[0100] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0101] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0102] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0103] (3) End the reaction and cool to 145°C, add into 55°C warm water for precipitation, and obtain precipitated particles;
[0104] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 0 mL: 4 mL;
[0105] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0106] Comparative Example 2
[0107] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0108] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0109] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0110] (3) End the reaction and cool to 145°C, add into 55°C warm water for precipitation, and obtain precipitated particles;
[0111] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 4 mL: 0 mL;
[0112] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0113] Comparative Example 3
[0114] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0115] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0116] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 0 parts by weight of molecular sieve;
[0117] (3) End the reaction and cool to 145°C, add into 55°C warm water for precipitation, and obtain precipitated particles;
[0118] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 3 mL: 1 mL;
[0119] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0120] Comparative Example 4
[0121] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0122] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0123] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0124] (3) End the reaction and cool to 145°C, add into 55°C warm water for precipitation, and obtain precipitated particles;
[0125] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 175° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 3 mL: 2 mL;
[0126] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0127] Comparative Example 5
[0128] A method for preparing high-purity polyphenylene sulfide comprises the following steps:
[0129] (1) Under nitrogen protection, the catalyst lithium chloride, sodium sulfide nonahydrate and sodium hydroxide are dispersed in an organic solvent N-methylpyrrolidone, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; the dehydration reaction temperature is 180°C;
[0130] (2) The solution was cooled to 126°C, p-dichlorobenzene was added, and the mixture was mixed evenly; the temperature was then raised to 230°C for reaction for 1.5 hours, nano molecular sieve was added, and the reaction was continued for 4 hours; the amounts of materials used in step (1) and step (2) were: 10 parts by weight of catalyst, 130 parts by weight of hydrated sodium sulfide, 1 part by weight of sodium hydroxide, 290 parts by weight of organic solvent, 75 parts by weight of p-dichlorobenzene, and 8 parts by weight of molecular sieve;
[0131] (3) End the reaction and cool to 145°C, add into 55°C warm water for precipitation, and obtain precipitated particles;
[0132] (4) adding the precipitated particles into a mixed solvent of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 160° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: 6 mL: 3 mL: 1 mL;
[0133] (5) The product obtained in step (4) is washed twice with ethanol and three times with deionized water, and dried in a vacuum drying oven to obtain high-purity polyphenylene sulfide.
[0134] The oligomer content (%) (chloroform solution extraction method) and volatile organic matter content (ppm) (high temperature degassing method) in the polyphenylene sulfide samples prepared in Examples 1-10 and Comparative Examples 1-5 were tested. The results are shown in Table 1-2 below.
[0135]
[0136]
[0137] As can be seen from Table 1-Table 2, the present invention adopts solution polymerization to prepare polyphenylene sulfide, and through the combination of solvent and process, the cost is greatly reduced and the purification process is simplified. The impurity content of the purified PPS resin is greatly reduced. As can be seen from Examples 1-7, 8-10, the solution is cooled to 140-150°C and then put into warm water. At this temperature, it is not only conducive to sufficient washing with warm water, but also can form a certain temperature difference with warm water, so that cracks are formed in the polyphenylene sulfide during the quenching process, which is convenient for subsequent washing with organic solvents. Figure 1 This is a scanning electron microscope image of the precipitated particles obtained by precipitation in warm water in Example 8. It can be seen that the surface of the precipitated particles is relatively loose and there are a large number of gaps, which is conducive to the subsequent immersion, swelling and washing processes of the organic solvent.
[0138] As can be seen from Comparative Examples 1-2, the present invention uses ethylene carbonate, cyclopentane sulfone and tetraethylene glycol as mixed solvents, which can give full play to the role of each component and play a synergistic effect. When the total amount remains unchanged, the washing effect is significantly reduced when one of them is missing. At the same time, Comparative Examples 3-4 show that without adding molecular sieves, impurities are easily wrapped by polyphenylene sulfide, and the removal effect of impurities is reduced; at the same time, due to the high viscosity of tetraethylene glycol, its dosage should not be too much, otherwise it is easy to cause the mixed organic solvent to not easily infiltrate the precipitated particles, and the technical effect of washing cannot be effectively achieved. Comparative Example 5 shows that during the washing process, the washing temperature should be controlled to 170-180°C; if the temperature is too low, the polymer cannot be fully swollen, and the motion performance of the polymer molecular chain and the tetraethylene glycol molecule is reduced, which is not conducive to cleaning; and if the temperature is too high, the washing effect is limited, which is not conducive to the cleaning of impurities, and the stability of the polymer is affected under the action of the solvent.
[0139] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0140] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A method for preparing high-purity polyphenylene sulfide, characterized in that: The following steps are involved: (1) Under the protection of inert gas, the catalyst, hydrated sodium sulfide and alkali are dispersed in an organic solvent, and an anhydrous sodium sulfide solution is obtained after dehydration reaction; (2) After the solution is cooled, add p-dichlorobenzene and mix well; then heat to 220-240°C and react for 1-2 hours, add nano molecular sieves, and continue to react for 3-5 hours; (3) End the reaction and cool to 140-150°C, add 50-60°C warm water for precipitation to obtain precipitated particles; (4) adding the precipitated particles into a mixed solvent consisting of ethylene carbonate, sulfolane and tetraethylene glycol, and washing them at 170-180° C.; the mass volume ratio of the precipitated particles to ethylene carbonate, sulfolane and tetraethylene glycol is 1 g: (5-8) mL: (2-4) mL: 1 mL; (5) The product obtained in step (4) is washed with ethanol and deionized water respectively, and dried to obtain high-purity polyphenylene sulfide.
2. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: In step (1), the inert gas is nitrogen.
3. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: In step (1), the catalyst is one or more of sodium formate, lithium formate, lithium carbonate, lithium acetate, lithium benzoate, and lithium chloride; the hydrated sodium sulfide is sodium sulfide nonahydrate; and the alkali is sodium hydroxide.
4. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: The organic solvent in step (1) is N-methylpyrrolidone.
5. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: The dehydration reaction temperature in step (1) is 170-190°C.
6. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: In step (2), the temperature is lowered to 120-130° C.; the nano molecular sieve is one or more of type A molecular sieve, type X molecular sieve, and type Y molecular sieve with a particle size of 50-200 nm.
7. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: The amounts of materials used in step (1) and step (2) are respectively: 8-12 parts by weight of catalyst, 120-140 parts by weight of hydrated sodium sulfide, 1-2 parts by weight of alkali, 250-300 parts by weight of organic solvent, 70-80 parts by weight of p-dichlorobenzene, and 5-10 parts by weight of nano molecular sieve.
8. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: The product in step (5) is washed with ethanol for 1-3 times and deionized water for 3-5 times.
9. The method for preparing high-purity polyphenylene sulfide according to claim 1, characterized in that: The drying in step (5) is carried out in a vacuum drying oven.
10. A high-purity polyphenylene sulfide, characterized in that: The high-purity polyphenylene sulfide is prepared by the preparation method of any one of claims 1 to 9.