Biodegradable particles, preparation method and application

By performing nitrogen-expanding modification and gaseous modification treatment on hollow titanium dioxide balls, combining the blending preparation of polylactic acid and thermoplastic acrylic resin, biodegradable particles with delayed degradation and good mechanical properties are formed, and existing degradable plastic materials are solved. The problem of degradation too fast.

CN118652530BActive Publication Date: 2024-11-19FUJIAN DELV NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411154619.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-19
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing biodegradable plastic materials degrade too quickly during normal use and cannot meet the normal use requirements of load-bearing and jab performance.

Method used

Hot air flow suspension treatment was performed by hollow titanium dioxide balls, modified by ammonia nitrogen expansion, combined with gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilicon propyl)amine, combined with polylactic acid and The melt blending preparation of thermoplastic acrylic resin forms biodegradable particles with controllable degradation.

Benefits of technology

The delayed degradation of plastics is achieved while maintaining good mechanical properties. The cavity structure of titanium dioxide reflects and refractions to light, prevents early excessive degradation, and reduces the physical cross-linking point of polylactic acid through modification treatment, enhancing the movement space of plastics .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a biodegradable particle, a preparation method and an application, and relates to the field of plastic technology. The present invention uses titanium dioxide as a raw material, performs nitrogen expansion modification, realizes the visible light catalytic performance of titanium dioxide, combines the hollow spherical structure of titanium dioxide itself, and adopts a post-addition method in the preparation process of plastic raw material melt blending, retains titanium dioxide itself and the external part of the cavity structure, thereby realizing the reflection and refraction of visible light, preventing early excessive degradation, and enabling more light to be injected into the interior of the plastic, thereby accelerating the degradation process; the titanium dioxide after nitrogen expansion modification is secondary modified by N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine, which can reduce the physical crosslinking points of polylactic acid, and due to the presence of a partial cavity structure, the space required for the movement of polylactic acid segments can be provided, producing a certain plasticizing effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, in particular to biodegradable particles, a preparation method and application thereof. Background Art

[0002] While plastic products bring convenience to people, the impact of white pollution on the environment is becoming increasingly serious. Therefore, the production and modification technology of degradable plastics will become a hot topic in the future. For a long time, the large-scale increase in non-degradable plastic waste around the world has caused serious environmental pollution. With the adjustment of national development plans and industrial policies, it is imperative to solve the problem of domestic waste and control the pollution caused by plastic waste to the ecological environment. Therefore, it is necessary to develop low-cost, superior performance, and market-recognized fully biodegradable materials.

[0003] However, the current biodegradable materials on the market generally have the problem of rapid degradation. For example, agricultural mulch materials have broken during use, and the performance of express bags and garbage bags has obviously decreased after being opened for a period of time. The load-bearing and puncture performance cannot meet the normal use requirements. Therefore, it is very necessary to provide a controllable fully biodegradable material to solve the problem of the rapid degradation of existing traditional materials during normal use. Summary of the invention

[0004] The purpose of the present invention is to provide a biodegradable particle, a preparation method and an application thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing biodegradable particles, comprising the following preparation steps:

[0006] (1) The hollow titanium dioxide balls are carried into the suspension furnace along with the hot air flow at a temperature of 300-400°C. The hot air flow ejector is turned on to suspend the hollow titanium dioxide balls. The heat is kept for 25-35 minutes to obtain nitrogen-doped titanium dioxide.

[0007] (2) The nitrogen-doped titanium dioxide is sent to the transmission pipeline from the discharge door on the other side of the suspension furnace under the action of gas propulsion. A vent is provided at 1 / 3 of the distance from the discharge door in the transmission pipeline. Argon gas at 200-300°C is introduced at a rate of 100-150 mL / min. After the nitrogen-doped titanium dioxide is sent to the reaction furnace, the furnace ventilation device is turned on and argon gas at 60-80°C is introduced at a rate of 150-250 mL / min. After the ammonia is exhausted, the furnace airflow ejector is turned on. The ejection speed of the airflow ejector is 20 ~30m / s, the air flow temperature is 60~80℃, the air flow is prepared by mixing a gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine mixture and argon gas in a volume ratio of 1:10, and after reacting for 2~3h, a modified nitrogen-doped titanium dioxide is obtained; the gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine mixture is obtained by bubbling a 1~20wt% N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine-ethanol solution through compressed air;

[0008] (3) 40-89 parts by weight of polylactic acid and 30-40 parts by weight of thermoplastic acrylic resin are melt-blended at 160-200°C for 25-40 minutes, 25-35 parts by weight of corn starch are added at 80 rpm, the rotation speed is adjusted to 1000 rpm, 4-10 parts by weight of modified nitrogen-doped titanium dioxide are added, and the mixture is stirred for 1-3 minutes. The melt-blended material is then extruded and granulated using a twin-screw extruder to obtain biodegradable particles.

[0009] Furthermore, the preparation method of the hollow titanium dioxide spheres in step (1) is as follows: 0.1-0.3 mass fractions of calcium carbonate, 0.9-1.1 mass fractions of butyl titanate, and 30-35 mass fractions of anhydrous ethanol are ultrasonically dispersed at 20-30 kHz for 30 min, stirred at 80-200 rpm for 12 h, spray granulated to a particle size of 60-150 mesh, and fed into a heating furnace for heat treatment to obtain hollow titanium dioxide spheres.

[0010] Furthermore, the calcium carbonate particle size is 50-70 nm.

[0011] Furthermore, the heat treatment is specifically as follows: heating to 250°C at 5°C / min, then heating to 550°C at 3°C / min, then heating to 800°C at 15°C / min, and keeping the temperature for 2h.

[0012] Furthermore, the hot gas flow in step (1) is all ammonia.

[0013] Furthermore, in step (1), the injection speed of the hot air flow injector is 20-30 m / s, and the hot air flow temperature used by the hot air flow injector is 800-1100°C.

[0014] Furthermore, the polylactic acid in step (3) is any one of L-type polylactic acid, D-type polylactic acid or LD mixed polylactic acid.

[0015] Furthermore, the thermoplastic acrylic resin in step (3) is NeoCry1 B-735 solid thermoplastic acrylic resin.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0017] The present invention uses titanium dioxide as a raw material, performs hot air flow suspension treatment, uses ammonia as an air flow, and promotes the high temperature generated by the ambient temperature and the friction between particles to promote the ammonia to nitrogen-expand titanium dioxide, thereby achieving the visible light catalytic performance of titanium dioxide. At the same time, the temperature and time are effectively adjusted to avoid the reaction time process, so that titanium dioxide is converted into titanium nitride, which affects the photodegradation performance of the plastic. In addition, the titanium dioxide of the present invention selects a hollow spherical structure, and in the process of melt blending and preparing the plastic raw materials, a post-addition method is adopted, and high-speed stirring is combined to achieve a rapid and efficient dispersion effect of titanium dioxide, and it can also avoid that the titanium dioxide particles are completely wrapped and infiltrated by the plastic, retaining the self- The body and the external part of the cavity structure can realize the reflection and refraction of visible light, prevent early excessive degradation, and enable more light to enter the interior of the plastic, thereby accelerating the degradation process; the nitrogen-expanded modified titanium dioxide is sent into the modification chamber with the ammonia gas flow, and the gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine and argon replace the ammonia as a new gas flow. The functional groups of the gaseous coupling agent molecules are attached to the surface of the titanium dioxide to obtain modified titanium dioxide. The terminal hydroxyl group can react with the carboxyl group in the polylactic acid, so that the physical cross-linking points of the polylactic acid are reduced, and due to the existence of the partial cavity structure, the space required for the movement of the polylactic acid chain segments can be provided, resulting in a certain plasticizing effect.

[0018] The raw materials of the present invention are biodegradable and green and environmentally friendly. The raw materials cooperate with each other so that the plastic particles are not only green and biodegradable, but also have good mechanical properties. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods of various indicators of the biodegradable particles prepared in the following examples:

[0021] Degradation rate: The materials obtained in the embodiments and comparative examples were sampled to obtain uniformly sized specimens with similar mass. Three specimens in each embodiment and comparative example were randomly selected, and the mass was recorded respectively to start the simulation experiment; a large rectangular container was made, 2 / 3 of the volume of soil was placed in it, the entire container was flattened, all the specimens were placed in the container in parallel in sequence, the specimens were spaced 30 cm apart, and the container was placed in a lighted room; the specimens in the container were sprayed with water, soil was sprinkled, rinsed with clean water, and blown with cold wind from a hair dryer to simulate the weather in nature every day. The time interval for each operation was fixed at 2 hours. The specimens were taken out every 60 days, rinsed with clean water, dried in an oven, and the mass was recorded: then the soil in the container was replaced repeatedly, and the specimens continued to perform a series of experiments simulating the natural conditions. The entire experimental measurement process was 3 months, and the degradation rate was recorded according to the mass obtained. Degradation rate = (original test mass before the test - test mass after the test) / test mass before the test.

[0022] Tensile strength: Tested in accordance with GB / T 1040.1.

[0023] Example 1; (1) 0.1 mass fraction of calcium carbonate with a particle size of 50-70 nm, 0.9 mass fraction of butyl titanate, and 31 mass fraction of anhydrous ethanol were ultrasonically dispersed at 30 kHz for 30 min, stirred at 100 rpm for 12 h, spray granulated, and the particle size was 60-150 mesh. The mixture was placed in a heating furnace and heated to 250°C at 5°C / min, then heated to 550°C at 3°C / min, and then heated to 800°C at 15°C / min. The mixture was kept warm for 2 h to obtain hollow titanium dioxide spheres.

[0024] (2) The hollow titanium dioxide balls are carried into the suspension furnace along with the hot air flow at a temperature of 350°C. The hot air flow ejector is turned on to suspend the hollow titanium dioxide balls. The ejection speed of the hot air flow ejector is 25 m / s. The hot air flow temperature used by the hot air flow ejector is 800°C. The hot air flow is kept at this temperature for 30 minutes to obtain nitrogen-doped titanium dioxide. The hot air flow is ammonia.

[0025] (3) The nitrogen-doped titanium dioxide is sent to the transmission pipeline from the discharge door on the other side of the suspension furnace under the action of gas propulsion. A vent is provided at a distance of 1 / 3 of the discharge door of the transmission pipeline. Argon at 200°C is introduced at 150 mL / min. After the nitrogen-doped titanium dioxide is sent to the reaction furnace, the ventilation device in the furnace is turned on, and argon at 60°C is introduced at 250 mL / min. After the ammonia is exhausted, the air flow injector in the furnace is turned on. The injection speed of the air flow injector is 25 m / s, and the air flow temperature is 60°C. The air flow is a mixture of gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine and argon in a volume ratio of 1:10. After reacting for 2 hours, modified nitrogen-doped titanium dioxide is obtained; the gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine mixture is obtained by bubbling 8wt% N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine-ethanol solution through compressed air;

[0026] (4) 40 parts by weight of L-type polylactic acid and 30 parts by weight of NeoCry1 B-735 solid thermoplastic acrylic resin were melt-blended at 180°C for 30 min, 25 parts by weight of corn starch were added at 80 rpm, the rotation speed was adjusted to 1000 rpm, 4 parts by weight of modified nitrogen-doped titanium dioxide were added, and the mixture was stirred for 1 min. The melt-blended material was then extruded and granulated using a twin-screw extruder to obtain biodegradable particles.

[0027] Example 2; (1) 0.1 mass fraction of calcium carbonate with a particle size of 60 nm, 0.9 mass fraction of butyl titanate, and 31 mass fraction of anhydrous ethanol were ultrasonically dispersed at 30 kHz for 30 min, stirred at 100 rpm for 12 h, spray granulated, and the particle size was 100 mesh. The mixture was sent into a heating furnace and heated to 250°C at 5°C / min, then heated to 550°C at 3°C / min, and then heated to 800°C at 15°C / min. The mixture was kept warm for 2 h to obtain hollow titanium dioxide spheres.

[0028] (2) The hollow titanium dioxide balls are carried into the suspension furnace along with the hot air flow at a temperature of 350°C. The hot air flow ejector is turned on to suspend the hollow titanium dioxide balls. The ejection speed of the hot air flow ejector is 25 m / s. The hot air flow temperature used by the hot air flow ejector is 1050°C. The temperature is kept for 30 minutes to obtain nitrogen-doped titanium dioxide. The hot air flow is ammonia.

[0029] (3) The nitrogen-doped titanium dioxide is sent to the transmission pipeline from the discharge door on the other side of the suspension furnace under the action of gas propulsion. A vent is provided at a distance of 1 / 3 of the discharge door of the transmission pipeline. Argon at 200°C is introduced at 150 mL / min. After the nitrogen-doped titanium dioxide is sent to the reaction furnace, the ventilation device in the furnace is turned on, and argon at 60°C is introduced at 250 mL / min. After the ammonia is exhausted, the air flow injector in the furnace is turned on. The injection speed of the air flow injector is 25 m / s, and the air flow temperature is 60°C. The air flow is a mixture of gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine and argon in a volume ratio of 1:10. After reacting for 2.5 hours, modified nitrogen-doped titanium dioxide is obtained; the gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine mixture is obtained by bubbling 12 wt% N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine-ethanol solution with compressed air;

[0030] (4) 65 parts by weight of D-type polylactic acid and 35 parts by weight of NeoCry1 B-735 solid thermoplastic acrylic resin were melt-blended at 180°C for 30 min, 20 parts by weight of corn starch were added at 80 rpm, the rotation speed was adjusted to 1000 rpm, 7 parts by weight of modified nitrogen-doped titanium dioxide were added, and the mixture was stirred for 1 min. The melt-blended material was then extruded and granulated using a twin-screw extruder to obtain biodegradable particles.

[0031] Example 3; (1) 0.1 mass fraction of calcium carbonate with a particle size of 70 nm, 0.9 mass fraction of butyl titanate, and 31 mass fraction of anhydrous ethanol were ultrasonically dispersed at 30 kHz for 30 min, stirred at 100 rpm for 12 h, spray granulated, and the particle size was 150 mesh. The mixture was sent into a heating furnace and heated to 250°C at 5°C / min, then heated to 550°C at 3°C / min, and then heated to 800°C at 15°C / min. The mixture was kept warm for 2 h to obtain hollow titanium dioxide spheres.

[0032] (2) The hollow titanium dioxide balls are carried into the suspension furnace along with the hot air flow at a temperature of 350°C. The hot air flow ejector is turned on to suspend the hollow titanium dioxide balls. The ejection speed of the hot air flow ejector is 25 m / s. The hot air flow temperature used by the hot air flow ejector is 1100°C. The hot air flow is kept at this temperature for 25 minutes to obtain nitrogen-doped titanium dioxide. The hot air flow is ammonia.

[0033] (3) The nitrogen-doped titanium dioxide is sent to the transmission pipeline from the discharge door on the other side of the suspension furnace under the action of gas propulsion. A vent is provided at 1 / 3 of the distance from the discharge door in the transmission pipeline. 200°C argon is introduced at 150 mL / min. After the nitrogen-doped titanium dioxide is sent to the reaction furnace, the ventilation device in the furnace is turned on, and 60°C argon is introduced at 250 mL / min. After the ammonia is exhausted, the air flow injector in the furnace is turned on. The injection speed of the air flow injector is 25 m / s, and the air flow temperature is 60°C. The air flow is a mixture of gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine and argon in a volume ratio of 1:10. After reacting for 3 hours, modified nitrogen-doped titanium dioxide is obtained; the gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine mixture is obtained by bubbling 20wt% N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine-ethanol solution with compressed air;

[0034] (4) 89 parts by weight of L-type polylactic acid and 40 parts by weight of NeoCry1 B-735 solid thermoplastic acrylic resin were melt-blended at 180°C for 30 min, 35 parts by weight of corn starch were added at 80 rpm, the rotation speed was adjusted to 1000 rpm, and 10 parts by weight of modified nitrogen-doped titanium dioxide were added. The mixture was stirred for 1 min, and the melt-blended material was extruded and granulated using a twin-screw extruder to obtain biodegradable particles.

[0035] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that no nitrogen expansion modification treatment is performed, and the remaining steps are the same as Example 2.

[0036] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (2) is different. Step (2) is changed to: the hollow titanium dioxide balls are carried into the suspension furnace with a hot air flow at a temperature of 350°C, and the hot air flow ejector is turned on to make the hollow titanium dioxide balls suspended. The ejection speed of the hot air flow ejector is 25m / s, the hot air flow temperature used by the hot air flow ejector is 1050°C, and the heat preservation is carried out for 40min to obtain nitrogen-doped titanium dioxide; the hot air flow is ammonia, and the remaining steps are the same as in Example 2.

[0037] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that there is no step (1), commercially available ordinary titanium dioxide is used as the raw material, and the remaining steps are the same as Example 2.

[0038] Comparative Example 4; The difference between Comparative Example 4 and Example 2 is that there is no gaseous N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine mixture modification, and the remaining steps are the same as Example 2.

[0039] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step (4) is different, and step (4) is changed to: 65 parts by weight of D-type polylactic acid, 35 parts by weight of NeoCry1 B-735 solid thermoplastic acrylic resin, 20 parts by weight of corn starch, and 7 parts by weight of modified nitrogen-doped titanium dioxide are melt-blended at 180° C. for 30 minutes, and then the material obtained after melt blending is extruded and granulated using a twin-screw extruder granulator to obtain biodegradable particles. The remaining steps are the same as in Example 2.

[0040] Effect example

[0041] Table 1 below shows the performance analysis results of the biodegradable particles of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.

[0042] Table 1

[0043]

[0044] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention uses titanium dioxide as a raw material, performs nitrogen expansion modification, realizes the visible light catalytic performance of titanium dioxide, and combines the hollow spherical structure of titanium dioxide itself. In the process of melt blending and preparation of plastic raw materials, a post-addition method is adopted to retain the titanium dioxide itself and the external part of the cavity structure, thereby realizing the reflection and refraction of visible light, preventing early excessive degradation, and allowing more light to enter the interior of the plastic, thereby accelerating the degradation process; the titanium dioxide after nitrogen expansion modification is secondary modified by N-(hydroxyethyl)-N,N-bis(trimethoxysilylpropyl)amine, which can reduce the physical cross-linking points of polylactic acid, and due to the presence of a partial cavity structure, it can provide the space required for the movement of polylactic acid segments, producing a certain plasticizing effect.

[0045] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing biodegradable particles, It is characterized in that The method comprises the following preparation steps: (1) The hollow titanium dioxide balls are carried into a suspension furnace along with a hot air flow at a temperature of 300-400°C, and a hot air flow ejector is turned on to suspend the hollow titanium dioxide balls. The hot air flow is kept warm for 25-35 minutes to obtain nitrogen-doped titanium dioxide; the hot air flow is ammonia; (2) The nitrogen-doped titanium dioxide is sent to the transmission pipeline from the discharge door on the other side of the suspension furnace under the action of gas propulsion. A vent is provided at 1 / 3 of the distance from the discharge door in the transmission pipeline. Argon gas at 200-300°C is introduced at a rate of 100-150 mL / min. After the nitrogen-doped titanium dioxide is sent to the reaction furnace, the furnace ventilation device is turned on and argon gas at 60-80°C is introduced at a rate of 150-250 mL / min. After the ammonia is exhausted, the furnace airflow ejector is turned on. The injection speed is 20-30 m / s, the air flow temperature is 60-80° C., the air flow is prepared by mixing a gaseous N-hydroxyethyl-N,N-bistrimethoxysilylpropylamine mixture and argon gas in a volume ratio of 1:10, and after reacting for 2-3 hours, the modified nitrogen-doped titanium dioxide is obtained; the gaseous N-hydroxyethyl-N,N-bistrimethoxysilylpropylamine mixture is obtained by bubbling a 1-20wt% N-hydroxyethyl-N,N-bistrimethoxysilylpropylamine-ethanol solution with compressed air; (3) 40-89 parts by weight of polylactic acid and 30-40 parts by weight of thermoplastic acrylic resin are melt-blended at 160-200°C for 25-40 minutes, 25-35 parts by weight of corn starch are added at 80 rpm, the rotation speed is adjusted to 1000 rpm, 4-10 parts by weight of modified nitrogen-doped titanium dioxide are added, and the mixture is stirred for 1-3 minutes. The melt-blended material is then extruded and granulated using a twin-screw extruder to obtain biodegradable particles.

2. A method for preparing biodegradable particles according to claim 1, It is characterized in that The preparation method of the hollow titanium dioxide spheres in step (1) is as follows: 0.1-0.3 mass fractions of calcium carbonate, 0.9-1.1 mass fractions of butyl titanate, and 30-35 mass fractions of anhydrous ethanol are ultrasonically dispersed at 20-30 kHz for 30 min, stirred at 80-200 rpm for 12 h, spray granulated to a particle size of 60-150 mesh, and fed into a heating furnace for heat treatment to obtain hollow titanium dioxide spheres.

3. A method for preparing biodegradable particles according to claim 2, It is characterized in that The calcium carbonate particle size is 50-70 nm.

4. A method for preparing biodegradable particles according to claim 2, It is characterized in that The heat treatment is specifically as follows: heating to 250°C at 5°C / min, then heating to 550°C at 3°C / min, then heating to 800°C at 15°C / min, and keeping the temperature for 2h.

5. The method for preparing biodegradable particles according to claim 1, It is characterized in that The injection speed of the hot air flow injector in step (1) is 20-30 m / s, and the hot air flow temperature used by the hot air flow injector is 800-1100°C.

6. A method for preparing biodegradable particles according to claim 1, It is characterized in that The polylactic acid in step (3) is any one of L-type polylactic acid, D-type polylactic acid or LD mixed polylactic acid.

7. The method for preparing biodegradable particles according to claim 1, It is characterized in that The thermoplastic acrylic resin in step (3) is NeoCry1 B-735 solid thermoplastic acrylic resin.

8. Use of the biodegradable particles prepared by the preparation method according to any one of claims 1 to 7 in plastic packaging.