Metal element doped ZnO-based piezoelectric-photocatalytic material as well as preparation method and application thereof

By introducing specific metal elements into ZnO-based materials, adjusting the lattice structure, and combining ultrasonic and photocatalysis, the problem of insufficient piezoelectric and photocatalytic performance in the existing technology is solved, and efficient and safe bacterial killing and tooth antibacterial effects are achieved. .

CN118698533APending Publication Date: 2024-09-27SICHUAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410694982.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

It is difficult to enhance the piezoelectric and photocatalytic properties of existing ZnO-based piezoelectric-photocatalytic materials doped with metal elements during the synthesis process, and their application scenarios are limited by insufficient production of reactive oxygen species, short half-life, potential toxicity, and limited antibacterial equipment conditions. This results in low efficiency and difficulty in achieving efficient and safe bacterial killing under mild conditions.

Method used

By introducing alkali metals, lanthanides and actinides into ZnO-based materials, the lattice structure is adjusted to enhance the piezoelectric effect and photocatalytic performance, and a low-cost hydrothermal method is used to synthesize nanomorphological materials, combining ultrasonic and photocatalytic conditions , improve carrier migration efficiency and reactive oxygen species generation.

Benefits of technology

It achieves efficient and safe killing of bacteria and microorganisms and expands the application scenarios of the material, especially in the fields of medical wastewater and dental antibacterial, demonstrating excellent antibacterial performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698533A
    Figure CN118698533A
Patent Text Reader

Abstract

The invention relates to a metal-element-doped ZnO-based piezoelectric-photocatalytic material, a preparation method and application, and belongs to the technical fields of sewage treatment, wastewater sterilization, tooth whitening and antibiosis and the like. The main body of the metal-element-doped ZnO-based piezoelectric-photocatalytic material is a ZnO material with multiple catalytic effects; the doping element can be one or more of alkali metal elements, lanthanide elements and actinide elements. The preparation method comprises the following steps: (1) synthesizing different zincate types in a precursor solution through a water bath method; and (2) synthesizing the ZnO-based piezoelectric-photocatalytic material doped with different metal elements through a solvothermal method. As a catalytic antibacterial agent for microorganisms and bacteria in industrial wastewater or a medical environment, metal elements are introduced into ZnO crystal lattices, so that the light response range is expanded, the separation efficiency of photo-induced electron-hole pairs is improved, the photocatalytic performance of the material is improved, meanwhile, crystal lattice expansion and crystal lattice distortion are caused, and the photocatalytic performance of the material is improved. Therefore, the non-central symmetry of unit cells is enhanced, the piezoelectric effect is promoted, and the piezoelectric catalytic performance of the material is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical fields of sewage treatment, wastewater sterilization, and tooth whitening and antibacterial, and more specifically relates to a metal element-doped ZnO-based piezoelectric-photocatalytic material, a preparation method and an application thereof. Background Art

[0002] Directly converting solar energy into chemical energy through photocatalysis has become a research hotspot in the field of energy recycling, but its conversion efficiency is limited by the rapid recombination of electron-hole pairs. In order to improve the separation efficiency and migration rate of carriers in the photocatalytic process, the built-in electric field through the piezoelectric effect is used to promote the migration performance of carrier pairs, thereby coupling photocatalysis with the piezoelectric effect, that is, "piezoelectric-photosynergistic catalysis". Driven by ultrasound, polarized positive and negative charges are generated through the piezoelectric effect, which react chemically with components in the surrounding environment to generate reactive oxygen species (ROS, such as hydroxyl radicals, superoxide radicals, etc.); at the same time, the built-in electric field is constructed inside the material, which can extend the migration path of carrier pairs and enhance their separation efficiency, which is conducive to the migration of charges to the surface active centers to participate in various catalytic reactions. Piezoelectric potential can improve the separation efficiency of photogenerated electrons and holes, provide source power for photoinduced charges, promote separation and inhibit recombination, and achieve long-term enhanced piezoelectric-photosynergistic catalytic effect.

[0003] Piezoelectric catalysis and photocatalysis overcome the uncontrollable characteristics of traditional chemical oxidation. They capture mechanical energy and solar energy to drive surface catalytic chemical reactions to produce reactive oxygen species. Reactive oxygen species can enhance the oxidative properties of the reaction system, thereby destroying bacterial cell walls and denaturing bacterial proteins, thereby killing microorganisms and bacteria, thereby achieving the purpose of killing microorganisms and bacteria in industrial wastewater or medical environments.

[0004] However, there are many difficulties and challenges in the process of material synthesis and scene application. First, in the synthesis of metal-doped ZnO-based piezoelectric-photocatalytic materials, the doped metal components are mismatched with the ZnO lattice, making it difficult to successfully introduce the metal components into the ZnO lattice and enhance the piezoelectric and photocatalytic properties of ZnO. At the same time, the internal electric field plays a key role in promoting the separation of photogenerated carriers. One of the challenges is to construct an electric field inside the material and effectively stimulate the separation of the generated photogenerated electron-hole pairs.

[0005] Secondly, the current nanomaterials with coexisting piezoelectric and photocatalytic properties usually have poor light response, weak piezoelectric effect, insufficient production of reactive oxygen species due to hypoxic microenvironment, short half-life of reactive oxygen species, and most of them are potentially toxic, which limits their application scenarios. Therefore, it is one of the difficulties to synthesize piezoelectric photocatalytic materials with good biological safety, low cytotoxicity, high efficiency, flexible and changeable structure, and large property regulation space so that they can be applied in a variety of scenarios.

[0006] Finally, the equipment conditions used in antibacterial treatment are limited. In clinical, commercial and home applications, excessively high power of light source equipment can easily cause overheating damage to surrounding tissues, and cavitation caused by excessively high ultrasonic power can damage surrounding tissues, resulting in a significant reduction in equipment power; low ultrasonic power but high frequency (greater than 28kHz), long wavelength of the excitation light source (above the wavelength of visible light), and limited penetration depth, making it difficult for the material to achieve the desired therapeutic effect. How to achieve efficient and safe antibacterial treatment under mild conditions is also a major difficulty.

[0007] Based on the above analysis, designing and developing an efficient and safe piezoelectric photocatalytic material to use it as an antibacterial agent for microorganisms and bacteria in industrial wastewater or medical environments has important practical significance and clinical application value. Summary of the invention

[0008] The present invention provides a metal element doped ZnO-based piezoelectric-photocatalytic material, a preparation method and an application thereof, the main purpose of which is to simultaneously achieve the synthesis of safe and efficient nanomaterials and the piezoelectric-photocatalytic killing of bacteria and microorganisms.

[0009] In order to achieve the above-mentioned purpose, the present invention constructs an electric field inside the photocatalyst material by coordinating multiple catalytic mechanisms, promotes the migration of photogenerated carriers, and can effectively inhibit the recombination of carriers; at the same time, low-cost and highly biocompatible ZnO inorganic piezoelectric photocatalytic materials are used, and doping with metal elements reduces the gap width of the material on the one hand, and widens the light response range;

[0010] On the other hand, it causes lattice expansion and lattice distortion, thereby enhancing the non-central symmetry of the unit cell and strengthening the piezoelectric effect, and finally synthesizing metal element-doped ZnO piezoelectric photocatalytic materials. Under the conditions of ultrasound and light synergistic catalysis, the activity efficiency of piezoelectric photocatalysis in killing bacteria and microorganisms is greatly improved. The development of this piezoelectric photocatalytic material can bring social and economic value, and it is expected that this work will be further studied and widely used.

[0011] The specific technical solutions are:

[0012] Metal element doped ZnO-based piezoelectric-photocatalytic material, the main body is zinc oxide ZnO, and the doping element can be one or more of alkali metal elements, lanthanide elements and actinide elements;

[0013] The doped alkali metal element may be one or more of alkali metal elements such as lithium Li, sodium Na, potassium K, etc.; the lanthanide element may be one or more of lanthanide elements such as europium Eu, terbium Tb, thulium Tm, yttrium Yb, etc.; the actinide element may be one or more of actinide elements such as actinium Ac, thorium Th, protactinium Pa, uranium U, etc.;

[0014] The mass ratio of zinc oxide to the doped metal element is (0.02-2000):1;

[0015] The morphology of the synthetic material can be one or more of zero-dimensional morphology such as nanoparticles; one-dimensional morphology such as nanorods, nanowires, nanofibers; and two-dimensional morphology such as nanosheets.

[0016] The method for preparing the metal element doped ZnO-based piezoelectric-photocatalytic material comprises the following steps:

[0017] (1) Synthesizing different zincate species in the precursor solution by a water bath method;

[0018] (2) ZnO-based piezoelectric-photocatalytic materials doped with different metal elements were synthesized by solvothermal method.

[0019] Furthermore, the specific method of step (1) is:

[0020] a) gradually dissolving a salt containing a zinc source and a salt containing one or more metal element sources in a certain amount of water, and stirring with a magnetic force until a clear and transparent solution is formed;

[0021] b) stirring the mixed solution at a certain temperature (10-100° C.) for a period of time to fully form a zincate precursor;

[0022] The salt containing the zinc source described in step (1) may be one or more of zinc chloride, zinc nitrate, zinc sulfate, and zinc acetate; the salt containing the metal element source includes a salt containing an alkali metal element, such as a lithium salt which may be one or more of lithium carbonate, lithium chloride, and lithium bromide; a sodium salt which may be one or more of sodium carbonate, sodium chloride, and sodium bicarbonate; a potassium salt which may be one or more of dipotassium hydrogen phosphate, potassium carbonate, and potassium bicarbonate; a salt containing a lanthanide element may be one or more of a nitrate and a sulfate; and a salt containing an actinide element may be one or more of a nitrate and a perchlorate;

[0023] The concentration of the salt containing the zinc source in the mixed solution is 0.05 to 300 mg / mL;

[0024] The concentration of the salt containing the metal element source in the mixed solution is 0.05 to 1000 g / mL;

[0025] The specific method of step (2) is:

[0026] The precursor solution prepared in step (1) is reacted at a certain temperature for a period of time by a solvothermal synthesis method;

[0027] After the reaction is completed, the metal element-doped ZnO-based piezoelectric photocatalytic material is obtained through purification, washing and drying.

[0028] The reaction time is 1 to 72 hours, and the hydrothermal temperature is 60 to 500°C.

[0029] The metal element doped ZnO-based piezoelectric-photocatalytic material can be used as an antibacterial catalyst for various microorganisms and bacteria in industrial wastewater or medical environments, specifically for killing one or more of Escherichia coli, Streptococcus gordonii, and Staphylococcus aureus.

[0030] Zinc oxide (ZnO), as a new generation of semiconductor, has the advantages of wide sources, strong redox ability, simple preparation process, stable photochemical properties, high electron mobility, low cost and low toxicity. It can achieve ultraviolet laser emission at 25°C and has both piezoelectric and photoelectric properties.

[0031] Under the joint excitation of light source and mechanical force, the crystal deforms, causing relative displacement of positive and negative ions, generating polarized positive and negative charges to participate in the redox reaction; at the same time, the internal electric field is constructed to promote the separation of photogenerated electrons and holes, improve the photocatalytic efficiency, and generate reactive oxygen species, which can participate in the electron transport chain of bacterial metabolism. When the bacteria are subjected to a sufficient level of stress, membrane damage will occur, and toxic substances such as aldehydes and oxides will be produced in the bacteria. These products will destroy the internal proteins of the bacteria and kill the microorganisms and bacteria.

[0032] The metal-doped ZnO-based piezoelectric-photocatalytic materials are synthesized. The metal elements are introduced into the ZnO unit cell, which, on the one hand, causes lattice expansion and lattice distortion, thereby enhancing the non-central symmetry of the unit cell, promoting the piezoelectric effect, and strengthening the piezoelectric catalytic performance; on the other hand, the band structure of the semiconductor material is changed to expand the light response range, improve the separation efficiency of photogenerated electron-hole pairs, promote the photocatalytic effect, and enhance the photocatalytic performance.

[0033] Ultimately, it will be possible to achieve efficient piezoelectric-photocatalytic synergistic catalytic disinfection and sterilization of medical wastewater, or to utilize low-power vibration mechanical energy and low-power light sources such as luminous electric toothbrushes to excite catalysts to produce reactive oxygen species to kill bacteria and microorganisms, thereby achieving the goal of efficient and safe piezoelectric photocatalytic dental antibacterial treatment, and has broad application prospects in the fields of medical wastewater sterilization treatment and dental antibacterial technology.

[0034] The present invention synthesizes a metal element-doped ZnO-based piezoelectric-photocatalytic material, which has the small size effect and surface effect of nanomaterials, increases the specific surface area and thus provides more active sites; has excellent stability and electron transport properties, thereby improving the migration efficiency of carriers and effectively promoting rapid electron transport.

[0035] The present invention adjusts the amount of the salt containing the zinc source in the precursor solution, changes the content ratio of zinc (Zn) and the metal element and the pH value of the system, thereby adjusting the degree of conversion of zinc hydroxide (Zn(OH)2) into zincate, changes the type of precursor, successfully introduces the metal element, solves the lattice mismatch problem of the two components of ZnO and the doped metal element, and synthesizes the unique lattice forced matching structure of the metal element doped ZnO-based piezoelectric-photocatalytic material;

[0036] The present invention prepares the material by a hydrothermal method with low production cost, high reliability, good repeatability, simple process, minimum energy consumption and mild reaction conditions. In the process of synthesizing nano ZnO by the hydrothermal method, ZnO with different morphologies and sizes can be well obtained by controlling the concentration of reactants, and has better uniformity and catalytic performance.

[0037] When the present invention uses Na-ZnONWs material to perform piezoelectric-photosynergistic catalysis to kill bacteria and microorganisms, Streptococcus mutans is selected for experimentation. Streptococcus mutans is a common facultative anaerobic, Gram-positive coccus in the human oral cavity and is an important factor causing tooth decay.

[0038] Under the simultaneous action of low-power ultrasound and LED light, the Na-ZnONWs material achieved a sterilization rate of ~40% against Streptococcus mutans after 5 minutes; the sterilization rate of Na-ZnONWs synergistically with low-concentration hydrogen peroxide against Streptococcus mutans reached ~100%, showing excellent antibacterial properties.

[0039] This shows that by introducing sodium elements into the ZnO lattice, not only the light response range is expanded and the separation efficiency of photogenerated electron-hole pairs is improved, but also significant lattice expansion and lattice distortion are brought about, which stimulates the non-central symmetry of the unit cell and strengthens the piezoelectric effect. This verifies that the material has excellent piezoelectric-optical properties and indicates that the material is expected to achieve high-efficiency antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a transmission electron microscope image of the final product Li-ZnONPs material of Example 1;

[0041] Figure 2 This is a transmission electron microscope image of the final product Na-ZnONWs material of Example 2;

[0042] Figure 3 This is a transmission electron microscope image of the final product K-ZnONRs material of Example 3;

[0043] Figure 4 This is the element distribution energy spectrum of the final product Na-Tb-ZnONWs material of Example 4;

[0044] Figure 5This is the element distribution energy spectrum of the final product Na-Yb-ZnONWs material of Example 5;

[0045] Figure 6 This is the element distribution energy spectrum of the final product Na-Ag-ZnONWs material of Example 6;

[0046] Figure 7 X-ray diffraction patterns of the final product Na-Tb-ZnONWs of Example 4 and the final product Na-Yb-ZnONWs of Example 5;

[0047] Figure 8 The antibacterial activity graphs against Streptococcus mutans under four conditions: adding only the final product Na-ZnONWs catalytic material of Example 2, adding only sterile water, adding only hydrogen peroxide, and adding the final product Na-ZnONWs catalytic material of Example 2 and hydrogen peroxide; DETAILED DESCRIPTION

[0048] The present invention is further described below in conjunction with embodiments, which are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, other embodiments obtained by ordinary technicians in the field without creative work are all within the scope of protection of the present invention.

[0049] Example 1

[0050] (1) 1-3 g zinc chloride (ZnCl2) and 20-80 g lithium carbonate (Li2CO3) are gradually dissolved in 100-250 mL water, and magnetically stirred until a clear transparent solution is formed. The solution is naturally cooled to room temperature, and the mixed solution is transferred to a three-necked flask and magnetically stirred at 30-50°C for 10-36 hours.

[0051] (2) The prepared precursor solution is transferred to a hydrothermal autoclave containing 25-200 mL of polytetrafluoroethylene lining, and hydrothermaled at 110-160° C. for 4-10 hours; after being allowed to stand and naturally cool to room temperature, ultrapure water is used as a precipitant and purifier, and the obtained mixed solution is washed and centrifuged multiple times by a selective precipitation method to purify the sample; finally, the mixture is vacuum dried at 60-100° C. for 10-24 hours, and the Li-ZnO NPs piezoelectric photocatalytic material is obtained after grinding.

[0052] Example 2

[0053] (1) 1-5 g zinc chloride (ZnCl2) and 50-100 g sodium carbonate (Na2CO3) are gradually dissolved in 100-250 mL water, and magnetically stirred until a clear transparent solution is formed. The solution is naturally cooled to room temperature, and the mixed solution is transferred to a three-necked flask and magnetically stirred at 30-50°C for 2-36 hours.

[0054] (2) The prepared precursor solution is transferred to a hydrothermal autoclave containing 25-200 mL of polytetrafluoroethylene lining, and hydrothermaled at 100-180° C. for 4-10 hours; after being allowed to stand and naturally cool to room temperature, ultrapure water is used as a precipitant and purifier, and the obtained mixed solution is washed and centrifuged multiple times by a selective precipitation method to purify the sample; finally, the mixture is vacuum dried at 60-100° C. for 10-24 hours, and the Na-ZnO NWs piezoelectric photocatalytic material is obtained after grinding.

[0055] Example 3

[0056] (1) 0.8-5.5 g zinc chloride (ZnCl2) and 150-200 g potassium carbonate (K2CO3) are gradually dissolved in 100-250 mL water, and magnetically stirred until a clear transparent solution is formed. The solution is naturally cooled to room temperature, and the mixed solution is transferred to a three-necked flask and magnetically stirred at 30-50°C for 6-48 hours.

[0057] (2) The obtained precursor solution is transferred to a hydrothermal autoclave containing 25-200 mL of polytetrafluoroethylene lining, and hydrothermaled at 120-200° C. for 4-10 hours; after being allowed to stand and naturally cool to room temperature, ultrapure water is used as a precipitant and purifier, and the obtained mixed solution is washed and centrifuged multiple times by a selective precipitation method to purify the sample; finally, the mixture is vacuum dried at 60-100° C. for 10-24 hours, and the K-ZnO NRs piezoelectric photocatalytic material is obtained after grinding.

[0058] Example 4

[0059] (1) 0.8-3.5 g zinc chloride (ZnCl2), 50-100 g sodium carbonate (Na2CO3) and 0.01-0.4 g terbium nitrate hexahydrate (Tb(NO3)3·6H2O) are gradually dissolved in 100-250 mL water, and magnetically stirred until a clear transparent solution is formed. The solution is naturally cooled to room temperature, and the mixed solution is transferred to a three-necked flask and magnetically stirred at 30-50°C for 5-42 hours.

[0060] (2) The prepared precursor solution is transferred to a hydrothermal autoclave containing 25-200 mL of polytetrafluoroethylene lining, and hydrothermaled at 120-200° C. for 4-10 hours; after being allowed to stand and naturally cool to room temperature, ultrapure water is used as a precipitant and purifier, and the obtained mixed solution is washed and centrifuged multiple times by a selective precipitation method to purify the sample; finally, the mixture is vacuum dried at 60-100° C. for 10-24 hours, and the Na-Tb-ZnO NWs piezoelectric photocatalytic material is obtained after grinding.

[0061] Example 5

[0062] (1) 1-5 g zinc chloride (ZnCl2), 50-100 g sodium carbonate (Na2CO3) and 0.02-0.4 g yttrium nitrate hexahydrate (Yb(NO3)3·6H2O) are gradually dissolved in 100-250 mL water, and magnetically stirred until a clear transparent solution is formed. The solution is naturally cooled to room temperature, and the mixed solution is transferred to a three-necked flask and magnetically stirred at 30-50°C for 4-30 hours.

[0063] (2) The prepared precursor solution is transferred to a hydrothermal autoclave containing 25-200 mL of polytetrafluoroethylene lining, and hydrothermaled at 100-180° C. for 4-10 hours; after being allowed to stand and naturally cool to room temperature, ultrapure water is used as a precipitant and purifier, and the obtained mixed solution is washed and centrifuged multiple times by a selective precipitation method to purify the sample; finally, the mixture is vacuum dried at 60-100° C. for 10-24 hours, and the Na-Yb-ZnO NWs piezoelectric photocatalytic material is obtained after grinding.

[0064] The X-ray diffraction patterns of the final product Na-Tb-ZnONWs of Example 4 and the final product Na-Yb-ZnONWs of Example 5 are shown in Figure 7 .

[0065] Example 6

[0066] (1) 1-5 g zinc chloride (ZnCl2), 50-100 g sodium carbonate (Na2CO3) and 0.2-1.4 g silver nitrate (AgNO3) are gradually dissolved in 100-250 mL water, and magnetically stirred until a clear transparent solution is formed. The solution is naturally cooled to room temperature, and the mixed solution is transferred to a three-necked flask and magnetically stirred at 25-45°C for 5-28 hours.

[0067] (2) The prepared precursor solution is transferred to a hydrothermal autoclave containing 25-200 mL of polytetrafluoroethylene lining, and hydrothermaled at 100-180° C. for 3-12 hours; after being allowed to stand and naturally cool to room temperature, ultrapure water is used as a precipitant and purifier, and the obtained mixed solution is washed and centrifuged multiple times by a selective precipitation method to purify the sample; finally, the mixture is vacuum dried at 60-100° C. for 10-24 hours, and the Na-Ag-ZnO NWs piezoelectric photocatalytic material is obtained after grinding.

[0068] Product analysis:

[0069] The final product Li-ZnO NPs synthesized in Example 1, the final product Na-ZnO NWs synthesized in Example 2, and the final product K-ZnO NRs piezoelectric photocatalytic materials synthesized in Example 3 were analyzed by transmission electron microscopy. Figure 1 , Figure 2 and Figure 3High-magnification electron microscopy images show that Li-doped ZnO nanoparticles, Na-doped ZnO nanowires and K-doped ZnO nanorods were successfully prepared.

[0070] The final product Na-Tb-ZnO NWs synthesized in Example 4, the final product Na-Yb-ZnO NWs synthesized in Example 5, and the final product Na-Ag-ZnO NWs piezoelectric photocatalytic material synthesized in Example 6 were subjected to elemental energy spectrum analysis. Figure 4 , Figure 5 and Figure 6 The figure shows that the main body of the material is ZnO, and it is successfully doped with corresponding elements, and the elements are distributed relatively evenly in the material.

[0071] The final product Na-Tb-ZnO NWs synthesized in Example 4 and the final product Na-Yb-ZnONWs piezoelectric photocatalytic material synthesized in Example 5 were analyzed by X-ray diffractometer. In the XRD spectrum between 20°-80°, the XRD diffraction peaks of the synthesized samples were basically consistent with the diffraction peaks of the standard PDF card of ZnO (JCPDS NO.70-8072), showing sharp diffraction peaks with high peak intensity, indicating that a material with ZnO as the main component was successfully synthesized, and the crystallization performance of each component in the material was good and the purity was high.

[0072] At the same time, it can be observed that in addition to the peaks of the corresponding crystal planes at ZnO, the synthesized samples also have other diffraction peaks, indicating that other elements have been successfully introduced into the ZnO unit cell, and ZnO-based piezoelectric photocatalytic materials doped with one or more metal elements have been successfully synthesized. The introduction of one or more metal elements into the ZnO unit cell can effectively broaden the absorption and utilization range of light wavelengths and enhance the photocatalytic performance of the material; on the other hand, it causes lattice expansion and lattice distortion, enhances the non-central symmetry of the structure, and increases the center misalignment of positive and negative charges under the action of external mechanical stress, changes the polarization state, and easily accumulates charges to generate potential differences, strengthens the piezoelectric effect, and enhances the piezoelectric properties of the material. Based on the above analysis, ZnO-based materials doped with metal elements have been successfully prepared.

[0073] Example 7

[0074] Weigh 6 mg of the final product Na-ZnO NWs piezoelectric photocatalytic material catalyst synthesized in Example 1, ultrasonically disperse it into 3 mL of sterilized water, and sterilize the above material solution in a biological operation table for 1 hour to kill the bacteria in the catalyst; then, measure 750 μL of material solution (the control group is sterilized water, hydrogen peroxide solution, and a mixture of material and hydrogen peroxide) and 750 μL of bacterial culture solution for mixing, and transfer the above mixed solution to low-power ultrasound and LED illumination conditions for piezoelectric photocatalytic anti-mutant Streptococcus activity test, maintain the reaction temperature at about 25 ° C, take 10 μL of the mixed solution after the reaction at intervals, dilute the solution 10000 times with sterilized water, and then take 20 μL and evenly apply it on a 1 / 3LB agar plate, repeat the above operation 3 times, and cover the entire culture plate. Subsequently, the plate was placed in a 37 ° C constant temperature incubator for 24 hours, and the colonies were photographed with a camera after the colonies were stable, and the colonies were counted with Image J to calculate the antibacterial rate.

[0075] Result analysis: The experimental results are as follows Figure 8 As shown, under the simultaneous action of low-power ultrasound and LED illumination, the bacterial mortality rate is 8.9%, indicating that the reaction conditions are not the cause of large-scale bacterial death. After adding Na-ZnO NWs material or H2O2 for 5 minutes during the reaction, the bacterial mortality rates were 40% and 45%, respectively. Among them, H2O2, as an active oxygen species, still showed certain antibacterial properties. Na-ZnO NWs also showed good piezoelectric-photocatalytic bactericidal performance in a short time, which was attributed to the fact that the inorganic nanomaterial can be excited under the combined action of low-power ultrasound (80W) and LED (10W), and piezoelectric-photosynergistic catalysis produces active oxygen species for antibacterial. Under the same reaction conditions, when Na-ZnO NWs cooperated with 1% H2O2 to act on Streptococcus mutans, the bacterial removal rate exceeded 90%, further indicating that the Na-ZnO NWs material effectively activated the conversion of H2O2 through catalysis, released a large number of active oxygen species to act on bacteria, resulting in their efficient killing, indicating that the material has good antibacterial properties under low-power ultrasound illumination conditions.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A metal element doped ZnO-based piezoelectric-photocatalytic material, characterized in that: The main body is ZnO material with multiple catalytic effects, and the doping elements are alkali metal elements, lanthanide elements and actinide elements.

2. The metal element doped ZnO-based piezoelectric-photocatalytic material according to claim 1, characterized in that: The doped alkali metal elements are one or more of lithium, sodium, potassium, and rubidium alkali metal elements; the lanthanide elements are one or more of europium, terbium, thulium, and yttrium lanthanide elements; and the actinide elements are one or more of actinium, thorium, protactinium, and uranium actinide elements.

3. The metal element doped ZnO-based piezoelectric-photocatalytic material according to claim 1, characterized in that: The mass ratio of zinc oxide to the doped metal element is (0.001-3000):

1.

4. The metal element doped ZnO-based piezoelectric-photocatalytic material according to claim 1, characterized in that: The synthesized metal element doped ZnO-based piezoelectric-photocatalytic material has a variety of morphologies: one or more of nanoparticles, nanorods, nanowires, nanofibers, and nanosheets.

5. The method for preparing the metal element doped ZnO-based piezoelectric-photocatalytic material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Regulating the type of zincate in the precursor by water bath method; (2) Prepare metal element doped ZnO-based piezoelectric-photocatalytic materials by solvent thermal synthesis.

6. The method for preparing the metal element doped ZnO-based piezoelectric-photocatalytic material according to claim 5, characterized in that: The specific method of step (1) is: a) gradually dissolving a salt containing a zinc source and a salt containing a metal element source in a certain amount of water, stirring with a magnetic force until a clear and transparent solution is formed, and the temperature of the solution is naturally cooled down to room temperature; b) stirring the mixed solution magnetically at 5-100°C for a period of time.

7. The method for preparing the metal element doped ZnO-based piezoelectric-photocatalytic material according to claim 6, characterized in that: The salt containing the zinc source described in step (1) is one or more of zinc chloride, zinc nitrate, zinc sulfate, and zinc acetate; the salt containing the metal element source includes a salt containing an alkali metal element, wherein the lithium salt is one or more of lithium carbonate, lithium chloride, and lithium bromide; the sodium salt is one or more of sodium carbonate, sodium chloride, and sodium bicarbonate; the potassium salt is one or more of dipotassium hydrogen phosphate, potassium carbonate, and potassium bicarbonate; the salt containing lanthanide elements can be one or more of nitrates and sulfates; and the salt containing actinide elements can be one or more of nitrates and perchlorates.

8. The method for preparing the metal element doped ZnO-based piezoelectric-photocatalytic material according to claim 5, characterized in that: The specific method of step (2) is: The precursor solution prepared in step (1) is transferred and reacted for a period of time by a solvent thermal synthesis method; after the reaction is completed, it is allowed to stand and naturally cool to room temperature; after multiple washing, separation, purification and drying, a metal element-doped ZnO-based piezoelectric-photocatalytic material is obtained.

9. Application of metal element doped ZnO-based piezoelectric-photocatalytic materials, characterized in that: As an antimicrobial agent against microorganisms and bacteria in industrial wastewater or medical environments.

Citation Information

Cited By

  • Piezoelectric photocatalytic composite material as well as preparation method and application thereof

    CN121266582A

  • Sulfur-doped zinc oxide nano material with broad-spectrum piezoelectric photocatalytic degradation characteristic as well as preparation method and application of sulfur-doped zinc oxide nano material

    CN121775869A