Platinum-rhodium hollow nanorod with high peroxidase-like activity and preparation method of platinum-rhodium hollow nanorod
By using the substitution reaction of telluride-selenide nanorods with polyvinylpyrrolidone, rhodium and platinum in the preparation of platinum-rhodium hollow nanorods, the problem of insufficient activity of existing platinum-based nanomaterials is solved, and a new product with high peroxidase-like activity is solved. Platinum-rhodium hollow nanorods are suitable for a variety of applications.
Patent Information
- Application Number
- CN202410770329.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
The catalytic activity of existing platinum-based nanomaterials is worse than that of natural horseradish peroxidase, and the preparation process is cumbersome and time-consuming, and the catalytic activity is low.
Telluride-selenium nanorods are used as substrates, and platinum-rhodium hollow nanorods with high peroxidase-like activity are prepared through displacement reaction with polyvinylpyrrolidone solution and rhodium and platinum precursors, and the Kirkendall effect is used to regulate their activity. Morphology and catalytic activity.
The high peroxidase-like activity of platinum-rhodium hollow nanorods is achieved, and the activity is equivalent to that of natural horseradish peroxidase. It is suitable for detection, medical treatment, environmental protection and other fields.
Smart Images

Figure CN118720124A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of nanomaterials, and more specifically, relates to a platinum-rhodium hollow nanorod with high peroxidase-like activity and a preparation method thereof. Background Art
[0002] Platinum group metals have good catalytic activity, especially platinum-based nanomaterials, which show broad application prospects in the field of catalysis. Platinum-based bimetallic nanomaterials can form new structures such as core-shell structures, heterostructures and alloy structures through interface engineering, which have been widely proven to have better physical and chemical properties than single metals. However, the specific activity of natural horseradish peroxidase (1305U mg -1 )There are few reports on comparable nanozymes.
[0003] Although the existing technology provides many methods for improving the activity of platinum-based nanozymes, there are still problems such as complicated catalyst preparation process, long time consumption and low catalytic activity. Taking Pt-Sn nanoparticles as an example, the existing technology proposes to first mix the platinum precursor, tin precursor and polyvinyl pyrrolidone solution in a stainless steel autoclave, heat it at 180°C for 12 hours, and then use ultrapure water and ethanol to wash and centrifuge to prepare Pt-Sn nanomaterials. After the enzyme catalytic performance test, its optimal specific activity is 345.3U mg -1 , this value is still far behind that of natural horseradish peroxidase. Summary of the invention
[0004] In view of the defects of the prior art, the present application provides a platinum-rhodium hollow nanorod with high peroxidase-like activity and a preparation method thereof, aiming to solve the problem that the activity of existing platinum-based nanomaterials is far inferior to that of natural horseradish peroxidase.
[0005] According to one aspect of the present application, a method for preparing platinum-rhodium hollow nanorods with high peroxidase-like activity is provided, specifically:
[0006] S1 uses tellurium precursor and selenium precursor to prepare tellurium selenide nanorods;
[0007] S2 disperses the tellurium selenide nanorods obtained in step S1 in an aqueous solution, adds a polyvinyl pyrrolidone solution and reacts for a preset time, then adds a rhodium precursor and continues to react for a preset time, and finally adds a platinum precursor and reacts for a preset time. After the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby obtaining platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0008] Through the above technical scheme conceived in the present application, compared with the prior art, polyvinyl pyrrolidone can be used to regulate the morphology of platinum-rhodium hollow nanorods and achieve excellent results in peroxidase-like specific activity.
[0009] As a further preferred embodiment, step S1 is specifically as follows: adding a tellurium precursor and a selenium precursor to a solution containing a reducing agent and reacting for a preset time, adding a solution containing a surfactant after the reaction is completed and stirring sufficiently, and finally performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods.
[0010] As further preferred, in step S1, the tellurium precursor is one or more of tellurium dioxide, tellurous acid and tellurite, the selenium precursor is selenous acid and / or selenite, the reducing agent is hydrazine hydrate, and the surfactant is sodium dodecyl sulfate.
[0011] As further preferred, in step S1, the reaction temperature is 30°C to 50°C, and the reaction time after adding the tellurium precursor and the selenium precursor is 15min to 20min.
[0012] As further preferred, in step S2, the concentration of the polyvinyl pyrrolidone solution is 1 μg / mL to 1500 μg / mL.
[0013] As further preferred, the rhodium precursor is one or more of rhodium trichloride, ammonium chlororhodate, rhodium nitrate, and rhodium sulfate, and the platinum precursor is one or more of chloroplatinic acid, ammonium chloroplatinate, platinum dichloride, platinum tetrachloride, and platinum nitrate.
[0014] As further preferred, in step S2, the molar ratio of the rhodium precursor to the platinum precursor is 8:3-8:10, and the molar ratio of the tellurium selenide nanorods to the platinum precursor is 4:1-2:1.
[0015] As further preferred, in step S2, the reaction temperature is 15°C to 30°C, the reaction time after adding the polyvinyl pyrrolidone solution is 5min to 30min, the reaction time after adding the rhodium precursor is 20min to 50min, and the reaction time after adding the platinum precursor is 10min to 30min.
[0016] According to another aspect of the present application, provided are platinum-rhodium hollow nanorods with high peroxidase-like activity obtained by the above-mentioned preparation method.
[0017] As further preferred, the length of the platinum-rhodium hollow nanorods with high peroxidase-like activity is 90 nm to 110 nm, and the diameter is 30 nm to 50 nm.
[0018] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:
[0019] 1. The present application proposes to add a polyvinyl pyrrolidone solution to a tellurium selenide nanorod solution to stabilize the tellurium selenide nanorods, and then successively add a rhodium precursor and a platinum precursor, and utilize a displacement substitution reaction and a Kirkendall effect to obtain platinum-rhodium hollow nanorods with high peroxidase-like activity;
[0020] 2. In particular, the present application can achieve differentiated control of the structure of platinum-rhodium hollow nanorods by optimizing the concentration of the polyvinyl pyrrolidone solution;
[0021] 3. The platinum-rhodium hollow nanorods with high peroxidase-like activity prepared in the present application not only have the property of adjustable morphology, but also have excellent peroxidase-like activity, which is equivalent to the activity of natural horseradish peroxidase. Therefore, they can be used as peroxidase-like enzymes in detection, medical treatment, environmental protection and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a flow chart for preparing platinum-rhodium hollow nanorods with high peroxidase-like activity provided by a preferred embodiment of the present invention;
[0023] Figure 2 TEM images of platinum-rhodium hollow nanorods with high peroxidase-like activity of different morphologies prepared in the preferred embodiments of the present invention, wherein A is the platinum-rhodium hollow nanorods prepared in Example 9, B is the platinum-rhodium hollow nanorods prepared in Example 4, and C is the platinum-rhodium hollow nanorods prepared in Example 1. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0025] like Figure 1 As shown, the present application provides a method for preparing platinum-rhodium hollow nanorods with high peroxidase-like activity, specifically:
[0026] S1: adding a tellurium precursor and a selenium precursor to a solution containing a reducing agent, stirring the mixture for 15 to 20 minutes at a temperature of 30 to 50°C, adding a solution containing a surfactant after the reaction is completed and stirring the mixture, and finally performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0027] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 15°C to 30°C, adding a polyvinyl pyrrolidone solution and reacting for 5min to 30min, then adding a rhodium precursor and continuing the reaction for 20min to 50min, and finally adding a platinum precursor and continuing the reaction for 10min to 30min. After the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby obtaining platinum-rhodium hollow nanorods (Pt-on-Rh hollow nanorods) with high peroxidase-like activity.
[0028] Furthermore, in step S1, the tellurium precursor is one or more of tellurium dioxide, tellurous acid and tellurite, the selenium precursor is selenous acid and / or selenite, the reducing agent is hydrazine hydrate, and the surfactant is sodium dodecyl sulfate. The molar ratio of the tellurium precursor to the selenium precursor is 17.86:1 to 178.6:1.
[0029] Further, in step S2, the rhodium precursor is one or more of rhodium trichloride, ammonium chlororhodiumate, rhodium nitrate, and rhodium sulfate, and the platinum precursor is one or more of chloroplatinic acid, ammonium chloroplatinate, platinum dichloride, platinum tetrachloride, and platinum nitrate. The concentration of the polyvinyl pyrrolidone solution is 1 μg / mL to 1500 μg / mL. The structure of the hollow nanorods can be regulated by adjusting the concentration of the polyvinyl pyrrolidone solution. When the concentration of the polyvinyl pyrrolidone solution is too low, the morphology of the prepared platinum-rhodium hollow nanorods is as follows: Figure 2 As shown in A, the surface of the material presents large and dense particles. When the concentration of the polyvinyl pyrrolidone solution is too high, the morphology of the prepared platinum-rhodium hollow nanorods is as follows: Figure 2 As shown in C, the surface of the material shows small and dispersed particles.
[0030] Furthermore, in step S2, the molar ratio of the rhodium precursor to the platinum precursor is 8:3-8:10, and the molar ratio of the tellurium selenide nanorods to the platinum precursor is 4:1-2:1. When the above ratios are too high or too low, the morphology of the prepared platinum-rhodium hollow nanorods is poor.
[0031] According to another aspect of the present application, a platinum-rhodium hollow nanorod with high peroxidase activity prepared by the above method is provided, wherein the length of the platinum-rhodium hollow nanorod is 90nm to 110nm and the diameter is 30nm to 50nm. The platinum-rhodium hollow nanorod with high peroxidase activity prepared by the method provided by the present application comprises shell particles and a hollow region formed by coating the shell particles, and the diameter of the hollow region is about two-thirds of the total diameter of the platinum-rhodium hollow nanorod with high peroxidase activity.
[0032] The platinum-rhodium hollow nanorods with high peroxidase-like activity prepared in the present application have excellent peroxidase-like activity and are suitable for use as enzyme catalysts in the fields of detection, medical treatment, and environmental protection. At the same time, the platinum-rhodium hollow nanorods can be used in small molecule detection, tumor diagnosis and treatment, organic matter degradation, or pesticide detection.
[0033] The technical solution provided by this application is further described below based on specific embodiments.
[0034] Example 1
[0035] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution thoroughly at 30°C for 15 minutes, wherein the molar ratio of tellurium dioxide to selenious acid is 89.3:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution thoroughly, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0036] S2: dispersing the tellurium selenide nanorods obtained in step S2 in an aqueous solution at 20°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 10 minutes, then adding rhodium trichloride and continuing the reaction for 30 minutes, and finally adding chloroplatinic acid and continuing the reaction for 20 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 3:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 8:5, wherein the concentration of the polyvinyl pyrrolidone solution is about 500 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0037] Example 2
[0038] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution at 40°C for 15 minutes, wherein the molar ratio of tellurium dioxide to selenious acid is 44.65:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution sufficiently, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0039] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 30°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 15 minutes, then adding ammonium chlororhodate and continuing the reaction for 20 minutes, and finally adding ammonium chloroplatinate and continuing the reaction for 10 minutes, wherein the molar ratio of tellurium selenide nanorods to ammonium chloroplatinate is 2:1, and the molar ratio of ammonium chlororhodate and ammonium chloroplatinate is 8:3, wherein the concentration of the polyvinyl pyrrolidone solution is about 100 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0040] Example 3
[0041] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution at 40°C for 15 minutes, wherein the molar ratio of tellurium dioxide to selenious acid is 44.65:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution sufficiently, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0042] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 25°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 20 minutes, then adding rhodium nitrate and continuing the reaction for 40 minutes, and finally adding platinum dichloride and continuing the reaction for 30 minutes, wherein the molar ratio of tellurium selenide nanorods to platinum dichloride is 3:1, and the molar ratio of rhodium nitrate to platinum dichloride is 1:1, wherein the concentration of the polyvinyl pyrrolidone solution is about 100 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0043] Example 4
[0044] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution thoroughly for 15 minutes at 35°C, wherein the molar ratio of tellurium dioxide to selenious acid is 125:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution thoroughly, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0045] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 25°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 30 minutes, then adding rhodium trichloride and continuing the reaction for 40 minutes, and finally adding chloroplatinic acid and continuing the reaction for 20 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 4:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 1:1, wherein the concentration of the polyvinyl pyrrolidone solution is about 50 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0046] Example 5
[0047] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution thoroughly for 15 minutes at 35°C, wherein the molar ratio of tellurium dioxide to selenious acid is 125:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution thoroughly, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0048] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 25°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 30 minutes, then adding rhodium trichloride and continuing the reaction for 50 minutes, and finally adding chloroplatinic acid and continuing the reaction for 20 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 4:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 1:1, wherein the concentration of the polyvinyl pyrrolidone solution is about 1500 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0049] Example 6
[0050] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution at 35°C for 25 minutes, wherein the molar ratio of tellurium dioxide to selenious acid is 107:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution sufficiently, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0051] S2: Disperse the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 20°C, add polyvinyl pyrrolidone solution and stir to react for 5 minutes, then add rhodium trichloride and continue to react for 10 minutes, and finally add chloroplatinic acid and continue to react for 10 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 3:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 8:10, wherein the concentration of polyvinyl pyrrolidone solution is about 200 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0052] Example 7
[0053] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution fully for 20 minutes at 35°C, wherein the molar ratio of tellurium dioxide to selenious acid is 107:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution fully, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0054] S2: Disperse the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 30°C, add polyvinyl pyrrolidone solution and stir to react for 12 minutes, then add rhodium trichloride and continue to react for 45 minutes, and finally add chloroplatinic acid and continue to react for 15 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 4:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 8:5, wherein the concentration of the polyvinyl pyrrolidone solution is about 1000 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0055] Example 8
[0056] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution fully for 20 minutes at 35°C, wherein the molar ratio of tellurium dioxide to selenious acid is 107:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution fully, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0057] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 15°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 15 minutes, then adding rhodium trichloride and continuing the reaction for 50 minutes, and finally adding chloroplatinic acid and continuing the reaction for 30 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 2:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 8:7, wherein the concentration of the polyvinyl pyrrolidone solution is about 20 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0058] Example 9
[0059] S1: adding tellurium dioxide and selenious acid to a hydrazine hydrate solution, stirring the solution thoroughly at 30°C for 15 minutes, wherein the molar ratio of tellurium dioxide to selenious acid is 89.3:1. After the reaction is completed, diluting the reaction solution in a solution containing sodium dodecyl sulfate, stirring the solution thoroughly, and performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods;
[0060] S2: dispersing the tellurium selenide nanorods obtained in step S1 in an aqueous solution at 25°C, adding polyvinyl pyrrolidone solution and stirring the reaction for 25 minutes, then adding rhodium trichloride and continuing the reaction for 20 minutes, and finally adding chloroplatinic acid and continuing the reaction for 10 minutes, wherein the molar ratio of tellurium selenide nanorods to chloroplatinic acid is 4:1, and the molar ratio of rhodium trichloride to chloroplatinic acid is 2:1, wherein the concentration of the polyvinyl pyrrolidone solution is about 1 μg / mL, and after the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby preparing platinum-rhodium hollow nanorods with high peroxidase-like activity.
[0061] Figure 2 A is a TEM image of the platinum-rhodium hollow nanorods with high peroxidase-like activity prepared in Example 9, i.e., when the concentration of the polyvinyl pyrrolidone solution is 1 μg / mL, Figure 2 B is a TEM image of the platinum-rhodium hollow nanorods with high peroxidase-like activity prepared in Example 4, i.e., when the concentration of the polyvinyl pyrrolidone solution is 50 μg / mL, Figure 2C is a TEM image of the high peroxidase-like activity platinum rhodium hollow nanorods prepared in Example 1 when the concentration of the polyvinyl pyrrolidone solution is 500 μg / mL. The high peroxidase-like activity platinum rhodium hollow nanorods prepared by the method provided in this application have similar microscopic morphology, including shell particles and hollow areas formed by the shell particles, with an average length of about 105 nm and an average diameter of about 40 nm. . From Figure 2 It can be seen that when the concentration of the polyvinyl pyrrolidone solution is low, the Pt particles distributed on the Rh metal layer are large and concentrated. When the concentration of the polyvinyl pyrrolidone solution is high, the Pt particles distributed on the Rh metal layer are small and dispersed. When the concentration of polyvinyl pyrrolidone is greater than 500μg / mL and less than 1500μg / mL, the product has the same Figure 2 The morphology is similar to that of the Pt / Rh hollow nanorods in C.
[0062] When the concentration of polyvinyl pyrrolidone solution was 1 μg / mL to 1500 μg / mL, the prepared highly active Pt-on-Rh hollow nanorods had intrinsic excellent peroxidase-like activity, with a specific activity of 607 U mg -1 ~1352U mg -1 , which is equivalent to the activity of natural horseradish peroxidase. The specific activity test scheme is tested according to the specific activity standardization method.
[0063] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A method for preparing platinum-rhodium hollow nanorods with high peroxidase-like activity, characterized in that: The preparation method is: S1 uses tellurium precursor and selenium precursor to prepare tellurium selenide nanorods; S2 disperses the tellurium selenide nanorods obtained in step S1 in an aqueous solution, adds a polyvinyl pyrrolidone solution and reacts for a preset time, then adds a rhodium precursor and continues to react for a preset time, and finally adds a platinum precursor and reacts for a preset time. After the reaction is completed, solid-liquid separation is performed to obtain a precipitate, thereby obtaining platinum-rhodium hollow nanorods with high peroxidase-like activity.
2. The preparation method according to claim 1, characterized in that Step S1 specifically includes: adding a tellurium precursor and a selenium precursor to a solution containing a reducing agent and reacting for a preset time, adding a solution containing a surfactant after the reaction is completed and stirring sufficiently, and finally performing solid-liquid separation to obtain a precipitate, thereby preparing tellurium selenium nanorods.
3. The preparation method according to claim 2, characterized in that: In step S1, the tellurium precursor is one or more of tellurium dioxide, tellurous acid and tellurite, the selenium precursor is selenous acid and / or selenite, the reducing agent is hydrazine hydrate, and the surfactant is sodium dodecyl sulfate.
4. The preparation method according to claim 2, characterized in that: In step S1, the reaction temperature is 30°C to 50°C, and the reaction time after adding the tellurium precursor and the selenium precursor is 15min to 20min.
5. The preparation method according to claim 1, characterized in that: In step S2, the concentration of the polyvinyl pyrrolidone solution is 1 μg / mL to 1500 μg / mL.
6. The preparation method according to claim 1, characterized in that: The rhodium precursor is one or more of rhodium trichloride, ammonium chlororhodate, rhodium nitrate, and rhodium sulfate; the platinum precursor is one or more of chloroplatinic acid, ammonium chloroplatinate, platinum dichloride, platinum tetrachloride, and platinum nitrate.
7. The preparation method according to claim 1, characterized in that: In step S2, the molar ratio of the rhodium precursor to the platinum precursor is 8:3-8:10, and the molar ratio of the tellurium selenide nanorods to the platinum precursor is 4:1-2:
1.
8. The preparation method according to claim 1, characterized in that: In step S2, the reaction temperature is 15°C to 30°C, the reaction time after adding the polyvinyl pyrrolidone solution is 5min to 30min, the reaction time after adding the rhodium precursor is 20min to 50min, and the reaction time after adding the platinum precursor is 10min to 30min.
9. Platinum-rhodium hollow nanorods with high peroxidase-like activity obtained by the preparation method according to any one of claims 1 to 8.
10. The platinum-rhodium hollow nanorods with high peroxidase-like activity as claimed in claim 9, characterized in that: The length of the high peroxidase-like activity platinum-rhodium hollow nanorod is 90nm-110nm, and the diameter is 30nm-50nm.
Citation Information
Cited By
Platinum-based hollow nanorod with ultra-thin wall thickness as well as preparation method and application of platinum-based hollow nanorod
CN120619382A
Preparation method of platinum-doped hollow gold nanorod with high photo-thermal stability
CN120755340A
Preparation method and application of high-activity nano enzyme with rich gold nano islands
CN121797363A
Preparation method and application of high-activity nanoscale enzyme with rich gold nanometer islands
CN121797363B