Method for preparing conductive forward osmosis membrane for algae-water separation and conductive forward osmosis membrane thereof
By depositing negatively charged electrochemical polymers and dopants on conductive porous carbon paper, a conductive forward osmosis membrane is formed, which solves the problem of dirt layer formation in algae water separation, achieves efficient separation and stable operation, and reduces costs.
Patent Information
- Application Number
- CN202410795384.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing conductive forward osmosis membranes easily form a fouling layer during the algae water separation process, resulting in unstable water flux, shortened membrane life, and increased operating costs. Moreover, the conductivity and stability of traditional conductive membranes are insufficient.
Conductive porous carbon paper is used as the supporting layer, and a negatively charged conductive intermediate layer and cortex are prepared through electrochemical polymer deposition and interfacial polymerization to form a conductive forward osmosis membrane with good conductivity and chemical stability.
It improves the efficiency of algae water separation and the anti-pollution ability of the membrane, extends the service life of the membrane, reduces operating costs, and maintains efficient water treatment capacity and stability.
Smart Images

Figure CN118751071A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of membrane technology, in particular to the field of membrane material technology applied to the field of algae water treatment technology, and specifically to a method for preparing a conductive forward osmosis membrane for algae water separation and a conductive forward osmosis membrane thereof. Background Art
[0002] In recent decades, forward osmosis (FO) technology driven by osmotic pressure has attracted widespread attention in algae-water separation due to its high separation efficiency, low membrane fouling tendency, high water recovery rate and relatively low energy consumption. During the dehydration process of microalgae, algae cells and gel-like soluble algae products (SAP) will form a fouling layer on the membrane surface, which seriously affects the water flux stability, membrane life and increases the operating cost. Currently, conductive forward osmosis membranes that control membrane fouling by means of conductive modification of the support layer have attracted more and more attention.
[0003] The support layer of traditional conductive membranes is mostly coated with conductive materials on a substrate or polyamide (PA) layer, such as the existing Chinese patent CN112473372B, which proposes a method of depositing a two-dimensional material MXene on a polymer membrane support layer, and then preparing a conductive forward osmosis membrane through interfacial polymerization. However, since the support layer is a non-conductive material, it not only has a relatively high resistivity, but also gradually decreases in membrane performance due to the loss of conductive additives during long-term operation. Therefore, it is very meaningful to prepare a forward osmosis membrane with both good conductivity and stability. Summary of the invention
[0004] To solve the above technical problems, the present invention provides a method for preparing a conductive forward osmosis membrane for algae-water separation and a conductive forward osmosis membrane thereof, which has good conductivity and chemical stability, and can achieve the effect of efficiently separating pollutants and alleviating membrane pollution in the field of algae-water separation.
[0005] In a first aspect, the present application provides a method for preparing a conductive forward osmosis membrane for algae-water separation, comprising the following steps:
[0006] 1) obtaining a conductive porous substrate of suitable size and performing a neutral treatment on the conductive porous substrate;
[0007] 2) depositing an electrochemical polymer on the conductive porous substrate in step 1) to prepare a conductive intermediate layer and obtain a conductive base film, wherein the electrochemical polymer contains a negatively charged electrochemical material and a negatively charged dopant;
[0008] 3) An interfacial polymerization reaction is performed on the conductive intermediate layer of the conductive base membrane to prepare a skin layer, thereby obtaining the conductive forward osmosis membrane for algae-water separation.
[0009] Furthermore, the conductive porous substrate is conductive porous carbon paper; the electrochemical polymer is a mixture of pyrrole and H2SO4, and the dopant is sodium dodecyl sulfate (SDBS).
[0010] Furthermore, the pyrrole concentration of the electrochemical polymer is 0.1 mol / L-0.2 mol / L.
[0011] Furthermore, the electrochemical polymer is obtained by the following method: a certain concentration and an appropriate amount of pyrrole solution, ethylene glycol, oxalic acid, and sodium dodecyl sulfate (SDBS) are fully dissolved in a certain amount of deionized water to obtain a first solution; a certain concentration of concentrated sulfuric acid is completely dissolved in a certain amount of deionized water to obtain a second solution, and finally the first and second solutions are mixed in a reactor for polymerization.
[0012] Furthermore, the electrochemical polymer is obtained by the following method: 10.35 mL of pyrrole solution, 3.0 mL of ethylene glycol, 3.0 mL of oxalic acid, and 13.40 g of sodium dodecyl sulfate (SDBS) are fully dissolved in 500 mL of deionized water to obtain a first solution; 16.1 mL of 98% concentrated sulfuric acid is completely dissolved in 500 mL of deionized water to obtain a second solution, and finally the first and second solutions are mixed in a reactor for polymerization.
[0013] Furthermore, when preparing the conductive intermediate layer, deposition is performed by a three-phase electrode method.
[0014] Furthermore, 50-800 cycles of electrochemical polymer are deposited on the porous conductive substrate.
[0015] Furthermore, the pyrrole concentration of the electrochemical polymer is 0.15 mol / L; and 600 cycles of the electrochemical polymer are deposited on the porous conductive substrate.
[0016] Furthermore, the porous conductive substrate is neutralized by soaking the porous conductive base film in 0.2 mol / L NaOH solution in a culture dish for 2 hours to enhance the bonding ability between the polypyrrole intermediate layer and the base film, and then soaking and rinsing with deionized water until neutralization after the soaking is completed.
[0017] In the second aspect, the present application provides a conductive forward osmosis membrane for algae-water separation, comprising a support layer, an intermediate layer and a skin layer, characterized in that the support layer is a porous conductive substrate, the intermediate layer is a negatively charged conductive intermediate layer, and the conductive forward osmosis membrane for algae-water separation is prepared by the method described in the first aspect above.
[0018] The beneficial effects of this application are:
[0019] The present application uses a conductive porous substrate as a support layer, and then electrochemically deposits an electrochemical material on the conductive porous substrate after neutral treatment to physically modify the substrate to obtain a conductive intermediate layer; interfacial polymerization is performed on the conductive intermediate layer to obtain a filterable skin layer to obtain a conductive forward osmosis membrane suitable for algae-water separation. The conductive forward osmosis membrane used for algae-water separation in the present application is used as an algae-water and algae liquid treatment membrane, and has good conductivity, anti-fouling and stability, which improves the performance and treatment efficiency of the overall algae-water separation system.
[0020] In the present application, negatively charged electrochemical polymers and dopants are deposited on conductive porous carbon paper, thereby enhancing the conductivity and hydrophilicity of the conductive intermediate layer, as well as the conductivity, strength and anti-fouling properties of the overall conductive forward osmosis membrane in the separation of algae water and algae liquid; at the same time, the negative electrons of the dopant further strengthen the connection between the filter cortex and the conductive base membrane, further strengthening the strength of the conductive forward osmosis membrane.
[0021] In addition, the present application forms a conductive base membrane including a conductive porous substrate support layer and a conductive material polymer layer by electrochemical material deposition on a conductive porous substrate. The conductive base membrane has low resistivity. At the same time, its porous permeability, excellent conductivity, low contact resistance, and good mechanical strength greatly improve the water treatment capacity stability and fouling resistance of the conductive forward osmosis membrane when applied to algae water treatment.
[0022] The present application enhances the adhesion of the electrochemical material to the conductive porous substrate by first performing a neutral treatment on the conductive porous substrate and then depositing the electrochemical material, thereby improving the overall strength and stability of the base membrane and its forward osmosis membrane.
[0023] At the same time, the present application enhances the conductivity, surface structure smoothness and nano-scale filtration performance of the conductive forward osmosis membrane by obtaining a forward osmosis membrane through interfacial polymerization of the cortex on the conductive base membrane.
[0024] At the same time, the present application provides a conductive forward osmosis membrane with strong conductivity and stability. When applied to algae water with different media and pollutants, under the condition of applied voltage, the anti-pollution effect of the membrane is enhanced, the removal efficiency of pollutants in algae water by forward osmosis filtration is improved, and the stability of the membrane is ensured.
[0025] The conductive forward osmosis membrane preparation method and forward osmosis membrane provided by the present application have strong conductivity and stability, and the anti-pollution effect of the membrane is enhanced under the condition of applying voltage. The conductive forward osmosis membrane prepared by the present invention is applied to the study of algae-water separation. Under the condition of an applied electric field, algae metabolites such as algae toxins, geosmin and dimethyl isoborneol can be removed to a high degree, and membrane pollution is alleviated to a certain extent. Under long-term operation, the removal efficiency of the main pollutants in algae water is still maintained at a very high effect, and stable chemical properties and forward osmosis performance are maintained, and the physical and chemical properties and performance of the conductive forward osmosis membrane will not be damaged, and it has strong chemical practicality and excellent water treatment stability.
[0026] In addition, the conductive base membrane of the conductive forward osmosis membrane of the present application has strong conductivity and stability and can be reused. After removing the contaminated skin layer, the filter skin layer can be repolymerized to obtain a new regenerated conductive forward osmosis membrane, which can reduce costs and reduce pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1a A flow chart of a method for preparing a conductive forward osmosis membrane for algae-water separation provided in this application;
[0028] Figure 1b This is a flow chart of preparing a conductive forward osmosis membrane for algae-water separation using conductive carbon paper as a substrate in an embodiment of the present application;
[0029] Figure 2a-2o Shown are scanning electron microscope images of the surface of the conductive porous carbon paper-based membrane obtained by depositing different concentrations of electrochemical polymer polypyrrole on a pure conductive porous carbon paper substrate at different deposition cycle numbers (200, 400, 500, 600, 700) in different embodiments of the present application;
[0030] Figure 3 It is a schematic diagram of the permeability performance experiment of the comparison base film of pure conductive porous carbon paper substrate and the conductive porous carbon paper base film at different polypyrrole deposition concentrations in different embodiments of the present application;
[0031] Figure 4 It is an experimental schematic diagram of the square resistance of a comparative base film of a pure conductive porous carbon paper base film and a conductive porous carbon paper base film at different polypyrrole deposition concentrations in different embodiments of the present application;
[0032] Figure 5 It is an experimental schematic diagram of the contact angle of a comparison base film of a pure conductive porous carbon paper substrate and a conductive porous carbon paper base film under different polypyrrole deposition circles in different embodiments of the present application;
[0033] Figure 6Schematic diagram of the Zeta potential experiment of the comparison base film of pure conductive porous carbon paper substrate and the conductive porous carbon paper base film under different polypyrrole deposition circle numbers in different embodiments of the present application;
[0034] Figure 7a-7f Schematic diagram of an atomic force microscope (AFM) experiment of a comparison base film of a pure conductive porous carbon paper substrate and a conductive porous carbon paper base film with different polypyrrole deposition circles in different embodiments of the present application;
[0035] Figure 8a1-Figure 8a6 , Figure 9b1-Figure 9b6 Schematic diagram of the surface scanning electron microscope of the conductive forward osmosis membrane formed on the pure conductive porous carbon paper substrate to compare the conductive forward osmosis membrane obtained after adding the intermediate layer of different concentrations of polypyrrole in different embodiments of the present application;
[0036] Figure 9c1-Figure 9c6 A schematic cross-sectional scanning electron microscope diagram of a conductive forward osmosis membrane formed on a pure conductive porous carbon paper substrate is provided to compare the conductive forward osmosis membrane obtained after adding an intermediate layer of polypyrrole with different deposition layers in different embodiments of the present application;
[0037] Figure 10a-10f Schematic diagram of the surface atomic force microscopy of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper substrate and a forward osmosis membrane obtained after adding an intermediate layer of polypyrrole deposited at the same concentration but at different cycles in different embodiments of the present application;
[0038] Fig.11 It is a schematic diagram showing the contact angle of the forward osmosis membrane formed on the pure conductive porous carbon paper substrate and the forward osmosis membrane obtained after adding the polypyrrole intermediate layer deposited at the same concentration but with different number of cycles in different embodiments of the present application;
[0039] Fig.12 Schematic diagram of X-ray photoelectron spectroscopy (XPS) of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper substrate and a forward osmosis membrane obtained after adding an intermediate layer of polypyrrole deposited at the same concentration but at different cycles in different embodiments of the present application;
[0040] Fig.13 Schematic diagram of cyclic voltammetry of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper substrate and a forward osmosis membrane obtained after adding a polypyrrole intermediate layer deposited at the same concentration but at different cycle numbers in different embodiments of the present application;
[0041] Fig.14 Schematic diagram of electrochemical impedance of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper substrate and a forward osmosis membrane obtained after adding a polypyrrole intermediate layer deposited at the same concentration but at different cycle times in different embodiments of the present application;
[0042] Fig.15A diagram of a cross-flow forward osmosis (FO) device for testing the permeation selectivity of a forward osmosis membrane;
[0043] Fig.16a , Fig.16b Schematic diagram of the performance of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper substrate and a forward osmosis membrane obtained after adding an intermediate layer of polypyrrole deposited at the same concentration but at different cycles in different embodiments of the present application in the FO mode (polyamide layer facing the raw material liquid) and in the PRO mode (polyamide layer facing the draw liquid);
[0044] Fig.17a Schematic diagram of water permeability coefficient (A value) and salt permeability coefficient (B value) of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper-based membrane and a forward osmosis membrane obtained after adding an intermediate layer of polypyrrole deposited at the same concentration but at different cycle numbers in different embodiments of the present application;
[0045] Fig.17b A schematic diagram of salt rejection of a comparative forward osmosis membrane formed on a pure conductive porous carbon paper-based membrane and a forward osmosis membrane obtained after adding an intermediate layer of polypyrrole deposited at the same concentration but at different cycle numbers in different embodiments of the present application;
[0046] Fig.18a , Fig.18b They are respectively a schematic diagram of the comparison of water flux and a schematic diagram of the comparison of salt return flux of a conductive forward osmosis membrane with a polypyrrole deposition concentration of 600 cycles at different draw solution concentrations;
[0047] Figure 19a-19b It is a schematic diagram showing the change of membrane flux of the conductive forward osmosis membrane in the application example of the present application under different voltages;
[0048] Figure 20a-20g It is a schematic diagram showing the thickness of the filter cake layer in the cross section of the conductive forward osmosis membrane in the application example of the present application under different applied voltages;
[0049] Figure 21a-Figure 21d It is a schematic diagram showing the effect of applying different voltages on the performance of the conductive forward osmosis membrane in the application example of the present application under the conditions of single and mixed algae water components;
[0050] Fig.22a , Figure 22a1-Figure 22g1 , Figure 22a2-Figure 22g2 , Figure 22a1'-Figure 22g1' , Figure 22a2'-Figure 22g2' Shown is a schematic diagram of a scanning electron microscope of a conductive forward osmosis membrane in an embodiment of the present application under different algae water components when different voltages are applied;
[0051] Figure 23a-23eIt is a schematic diagram showing the effect of applying different voltages on the performance of the conductive forward osmosis membrane in the application example of the present application in the algae water with added Ca2+;
[0052] Figure 24a-Figure 24e It is a schematic diagram showing the effect of applying different voltages on the performance of the conductive forward osmosis membrane in algae water in which HA coexists in the algae water in the application example of the present application;
[0053] Figure 25a-Figure 25e It is a schematic diagram showing the effect of applying different voltages on the performance of the conductive forward osmosis membrane in the algae water containing Kaolinite as a coexisting substance in the application example of the present application;
[0054] Fig.26a , 26b Schematic diagrams showing the membrane flux changes of the forward osmosis membrane CPFO of the embodiment of the present application and the regenerated forward osmosis CPFO-C membrane after stripping under long-term operation and the spectrum of the middle layer after stripping the CPFO membrane skin layer;
[0055] Figure 27a-27f This is a SEM image of the conductive forward osmosis membrane before and after peeling in the examples of the present application. DETAILED DESCRIPTION
[0056] In order to make the technical means, creative features, objectives and effects achieved by this application easy to understand, the application is further explained below with reference to specific diagrams and tables.
[0057] like Figure 1a As shown, the present application provides a method for preparing a conductive forward osmosis membrane for algae-water separation, comprising the following steps:
[0058] 1) obtaining a conductive porous substrate of suitable size and performing a neutral treatment on the conductive porous substrate;
[0059] 2) depositing an electrochemical polymer on the conductive porous substrate in step 1) to prepare a conductive intermediate layer and obtain a conductive base film, wherein the electrochemical polymer contains a negatively charged electrochemical material and a negatively charged dopant;
[0060] 3) An interfacial polymerization reaction is performed on the conductive intermediate layer of the conductive base membrane to prepare a skin layer, thereby obtaining the conductive forward osmosis membrane for algae-water separation.
[0061] Furthermore, the conductive porous substrate is conductive porous carbon paper; the electrochemical polymer is a mixture of pyrrole and H2SO4, and the dopant is sodium dodecyl sulfate (SDBS).
[0062] Furthermore, the pyrrole concentration of the electrochemical polymer is 0.1 mol / L-0.2 mol / L.
[0063] Furthermore, the electrochemical polymer is obtained by the following method: a certain concentration and an appropriate amount of pyrrole solution, ethylene glycol, oxalic acid, and sodium dodecyl sulfate (SDBS) are fully dissolved in a certain amount of deionized water to obtain a first solution; a certain concentration of concentrated sulfuric acid is completely dissolved in a certain amount of deionized water to obtain a second solution, and finally the first and second solutions are mixed in a reactor for polymerization.
[0064] Furthermore, the electrochemical polymer is obtained by the following method: 10.35 mL of pyrrole solution, 3.0 mL of ethylene glycol, 3.0 mL of oxalic acid, and 13.40 g of sodium dodecyl sulfate (SDBS) are fully dissolved in 500 mL of deionized water to obtain a first solution; 16.1 mL of 98% concentrated sulfuric acid is completely dissolved in 500 mL of deionized water to obtain a second solution, and finally the first and second solutions are mixed in a reactor for polymerization.
[0065] Furthermore, when preparing the conductive intermediate layer, deposition is performed by a three-phase electrode method.
[0066] Furthermore, 50-800 cycles of electrochemical polymer are deposited on the porous conductive substrate.
[0067] Furthermore, the pyrrole concentration of the electrochemical polymer is 0.15 mol / L; and 600 cycles of the electrochemical polymer are deposited on the porous conductive substrate.
[0068] Furthermore, the porous conductive substrate is neutralized by soaking the porous conductive base film in 0.2 mol / L NaOH solution in a culture dish for 2 hours to enhance the bonding ability between the polypyrrole intermediate layer and the base film, and then soaking and rinsing with deionized water until neutralization after the soaking is completed.
[0069] In the second aspect, the present application provides a conductive forward osmosis membrane for algae-water separation, comprising a support layer, an intermediate layer and a skin layer, characterized in that the support layer is a porous conductive substrate, the intermediate layer is a negatively charged conductive intermediate layer, and the conductive forward osmosis membrane for algae-water separation is prepared by the method described in the first aspect above.
[0070] Furthermore, the conductive porous substrate is conductive porous carbon paper or conductive carbon material, which is porous and conductive; preferably conductive porous carbon paper.
[0071] Furthermore, the conductive middle layer is made of polypyrrole material; and the skin layer is a polyamide layer.
[0072] Furthermore, the polypyrrole is deposited on the conductive porous carbon paper by electrochemical deposition of an electrochemical polymer material containing pyrrole.
[0073] Furthermore, the skin layer formed on the conductive intermediate layer has a smooth, spine-like shape; the forward osmosis membrane has a square resistance of 156.4 mΩ / sq to 300 mΩ / sq, preferably 156.4 mΩ / sq to 209.3 mΩ / sq.
[0074] Furthermore, the average water flux of the conductive forward osmosis membrane in FO / PRO mode is 9.09-33.96 L / (m2h), and the salt return flux is 3.38-21.48 g / (m2h), and the average water flux is 9.09-22.09 L / (m2h), or 21.76-33.96 L / (m2h); the salt return flux is 3.38-11.40 g / (m2h) or 5.48-21.48 g / (m2h); and the average water flux is 21.09 / 33.96 L / (m2h), and the average salt return flux is 4.61 and 5.48 g / (m2h).
[0075] The following further describes in detail the conductive forward osmosis membrane for algae-water separation and its preparation method provided by the present application:
[0076] Furthermore, the neutral treatment of the conductive porous substrate is performed in the following manner: obtaining a conductive porous substrate of a suitable size, placing the conductive porous substrate of a suitable size in a culture dish and soaking it, and then performing a neutral treatment on the substrate.
[0077] Furthermore, the pretreatment of the conductive porous substrate is performed in the following manner: a conductive porous substrate of a suitable size is placed in a culture dish and soaked in a 0.2 mol / L sodium hydroxide (NaOH) solution for a period of time, and then soaked and rinsed in deionized water until neutral.
[0078] Furthermore, the method for preparing the cortex is as follows: immersing the conductive base membrane in an aqueous solution of a certain concentration of a polyamine compound, and after being completely immersed for a certain period of time, removing excess aqueous solution to obtain a pretreated membrane; surface treating the pretreated membrane; pouring an organic solution containing a polyacyl chloride compound on the treated pretreated membrane to perform an interfacial polymerization reaction, and removing excess organic solution after a second specified time to obtain a cortex conductive forward osmosis membrane with a polyamide layer.
[0079] Furthermore, the method for preparing the polyamide layer is as follows: 25 ml of an aqueous solution containing a metaphenylenediamine compound (MPD) is slowly poured on the base membrane and allowed to soak therein, and the complete immersion is maintained for 180 seconds; then, excess aqueous solution is poured off, and a rubber roller is used to gently roll over the membrane surface to evenly disperse the aqueous solution on the membrane surface to obtain the pretreated membrane; then, 25 ml of an organic solution of a trimesoyl chloride compound (TMC) is poured on the pretreated membrane, and after reacting for 90 seconds, excess organic solution is poured off to obtain a nascent forward osmosis membrane; the prepared nascent forward osmosis membrane is air-dried for 60 seconds and then dried and cured for 300 seconds to obtain a selectively permeable cortex on the membrane surface.
[0080] Furthermore, the aqueous phase solution is configured as follows: a solution of a m-phenylenediamine compound with a concentration of 1.0wt%-6.0wt% is prepared with water as a solvent and dissolved in an opaque or semi-transparent container; the organic phase solution is configured as follows: a solution of a trimesoyl chloride compound with a concentration of 0.05wt%-0.5wt% is dissolved in a container with n-hexane as a solvent.
[0081] The original conductive porous carbon paper has high porosity and ultra-large pore structure, with the porosity and average pore size reaching 41.1% and 280μm. After depositing the polypyrrole intermediate layer, the defects of the large pores of the base membrane are compensated, the surface pore size is 1.08±3.4μm, and the porosity is 34.6±1.7%. The conductive porous carbon paper base membrane also obtains high hydrophilicity, and the base membrane is successfully modified.
[0082] The polyamide layer formed on the original conductive porous carbon paper substrate is smooth, but not spine-like; after the deposition of the intermediate layer, the defects of the rough large pores of the conductive porous carbon paper-based membrane are compensated, and a series of physical and chemical properties such as the hydrophilicity, roughness, pore size, and electrochemical properties of the membrane surface are changed, forming a new substrate morphology, which affects the morphology and performance of the polyamide layer. High hydrophilicity, reasonable small pore size, and uniform roughness provide greater reactivity and contact area for the interfacial polymerization reaction, resulting in a higher degree of cross-linking and excellent forward osmosis performance.
[0083] Please also see Figure 1b With respect to the conductive forward osmosis membrane for algae-water separation and the preparation method thereof of the first and second aspects, an embodiment of the present application provides a preparation method of the conductive forward osmosis membrane using conductive porous carbon paper as a supporting substrate, specifically comprising:
[0084] S1: pre-treating the conductive porous carbon paper substrate;
[0085] S2: electrochemically depositing a conductive intermediate layer on a conductive porous carbon paper substrate to obtain a conductive porous carbon paper-based membrane (CP); further, depositing an electrochemical polymer on the conductive porous carbon paper to obtain the conductive intermediate layer; further, the conductive intermediate layer of the electrochemical polymer is a polypyrrole intermediate layer;
[0086] S3: placing the conductive porous carbon paper base membrane on a flat plate with the conductive intermediate layer facing upward, and performing interfacial polymerization reaction on the conductive intermediate layer on the base membrane to obtain a conductive forward osmosis membrane with selective permeability.
[0087] The following is a further detailed description of the method for preparing the conductive forward osmosis membrane provided in the embodiment of the present application:
[0088] In the step S1: a conductive porous carbon paper substrate of a suitable size, such as 10×10 cm, is cut into a suitable size, such as 5×10 cm with a utility knife, and is soaked in a culture dish for a certain time, such as 2 hours, in a sodium hydroxide solution of a certain concentration, such as 0.2 mol / L NaOH solution, to enhance the bonding ability between the electrochemical polymer, such as the polypyrrole intermediate layer, and the conductive porous carbon paper substrate. After the soaking is completed, it is then soaked and rinsed with deionized water until it is neutral.
[0089] In the step S2: preparing a conductive porous carbon paper-based membrane with a polypyrrole intermediate layer: electrochemically polymerizing polypyrrole through a three-electrode system, first preparing an electrochemical polymerization solution, i.e., a mixture of pyrrole and H2SO4, mixing the two solutions in a reactor for polymerization. The reactor is placed in a magnetic stirrer, the stirring speed and the temperature around the reactor are set, the electrochemical polymerization mode is set to cyclic voltammetry (cyclic voltammetry), a fixed voltage scanning range, scanning rate and number of cycles are set, and the CP membranes deposited with polypyrrole are named -CP-n according to the number of cycles.
[0090] In the step S3, the conductive forward osmosis membrane obtained by interfacial polymerization on the base film is a conductive forward osmosis membrane having a polyamide layer obtained by interfacial polymerization on the base film deposited with the intermediate layer, comprising the following steps:
[0091] S4: soaking the base film in an aqueous solution containing a polyamine compound, and removing excess aqueous solution on the base film after a first specified time to obtain a pretreated film;
[0092] S5: performing surface treatment on the pre-treated film;
[0093] S6: pouring the organic phase solution containing the polyacyl chloride compound onto the pretreated membrane treated in step S5 to perform an interfacial polymerization reaction, and removing excess organic phase solution after a second specified time to obtain a conductive forward osmosis membrane having a polyamide layer.
[0094] In the step S3: the base film is placed flatly on a smooth flat plate with the base film facing upward. In the embodiment of the present application, the smooth flat plate is a smooth glass plate, and further includes a rubber ring and a stainless steel frame of a customized size; the rubber ring and the stainless steel frame are fixed on the glass plate, and further include a mounting fixing device and a leak-proof device.
[0095] The method also includes steps of preparing an aqueous solution and an organic solution respectively.
[0096] Furthermore, the aqueous phase solution is an aqueous phase solution of a polyamine compound, and the organic phase solution is an organic phase solution of a polyacyl chloride compound; in an embodiment of the present application, the aqueous phase solution is an aqueous phase solution of m-phenylenediamine, and the organic phase solution is an organic phase solution of trimesoyl chloride.
[0097] Furthermore, the step S4 is to pour an aqueous solution into the frame to soak the base film, remove excess aqueous solution after a first specified time, and remove the fixing device and the leak-proof device to obtain a pretreated film having an amine monomer aqueous solution on the surface.
[0098] Furthermore, the step S5 is to use a collecting roller to roll over the surface of the pre-treated membrane to evenly distribute the aqueous solution containing the amine monomer on the membrane surface, making the membrane smoother. In the embodiment of the present application, the collecting roller is made of rubber.
[0099] Furthermore, the step S6 is to pour the organic phase solution into the frame for reaction, and pour out the excess organic phase solution after the second specified time; since the two-phase solutions are incompatible with each other, the amine monomers in the aqueous phase diffuse into the organic phase solution, and the monomers in the two-phase solution can only contact and react at the interface between the two phases. In addition, the reaction rate between the monomers is extremely fast, so a polyamide layer can be formed on the surface of the intermediate layer of the conductive porous base membrane in a very short time.
[0100] The method further comprises the following step S7: curing the prepared conductive forward osmosis membrane after naturally drying it in the air, and obtaining a conductive forward osmosis membrane having a polyamide layer after a third specified time;
[0101] S8: The conductive forward osmosis membrane having a polyamide layer is stored in deionized water until testing; further stored in the deionized water at a temperature of 4°C.
[0102] In a further embodiment, the process flow for preparing the aqueous phase solution is to dissolve m-phenylenediamine in deionized water in a light-proof container such as a brown container, and then ultrasonicate for 10 min to 50 min.
[0103] In a further embodiment, the process flow for preparing the organic phase solution is to dissolve 1,3,5-benzenetricarboxylic acid chloride (TMC) in n-hexane solvent, and then ultrasonicate for 10min-50min. Further, in the embodiment of the present application, 1,3,5-benzenetricarboxylic acid chloride (TMC) with a concentration of 0.15wt% is dissolved in 50ml of n-hexane solution and ultrasonicate for 30 minutes to completely dissolve it.
[0104] In a further embodiment, the mass percentage of the interphenylenediamine in the aqueous solution is 1.0wt%-6.0wt%, and more preferably 3wt%; the mass percentage of trimesoyl chloride in the organic solution is 0.05wt%-0.5wt%, and more preferably 0.15wt%.
[0105] In a further embodiment, the first designated time is 3-7 minutes, more preferably 5 minutes; the second designated time is 1-6 minutes, more preferably 2 minutes; the third designated time is 30-90 seconds, more preferably 60 seconds.
[0106] In the description of the embodiments of the present application, including the accompanying drawings, the following terms are expressed as described if there is no special explanation: the conductive porous carbon paper-based membrane (CP) means a conductive porous carbon paper-based membrane after electrochemical deposition on a conductive porous carbon paper substrate, the conductive forward osmosis membrane is a conductive forward osmosis membrane prepared by an interfacial polymerization reaction process on a conductive porous carbon paper-based membrane, and the conductive forward osmosis membrane prepared by the interfacial polymerization reaction process of the conductive porous carbon paper-based membrane CP-0, CP-200, CP-400, CP-500, CP-600, and CP-700 according to the number of cycles of polypyrrole deposition are named CPFO0 membrane, CPFO200 membrane, CPFO400 membrane, CPFO500 membrane, CPFO600 membrane, and CPFO700 membrane, respectively. The experiments, tests, parameter descriptions, etc. of each embodiment in this embodiment, if there are corresponding expressions, are all carried out for the above-mentioned body. The skin layer is a polyamide layer, Drawconcentration means the draw liquid concentration, Water flux means the water flux, and Reverse salt flux means the reverse salt flux.
[0107] In the embodiments of the present application, the electrochemical polymer polypyrrole deposition concentration is 0.1mol / L-0.2mol / L, and the number of cycles is 200-700, especially 200, 400, 500, 600, and 700. Preferably, a further scheme of the embodiments of the present application is that the electrochemical polymer polypyrrole deposition concentration is 0.15mol / L, and the number of cycles is 600.
[0108] Preferably, the preparation process of the polypyrrole intermediate layer in step S2 is as follows: 10.35 mL (0.1-0.2 mol / L) of pyrrole solution, 3.0 mL of ethylene glycol, 3.0 mL of oxalic acid, and 13.40 g of sodium dodecyl sulfate are fully dissolved in 500 mL of deionized water, and 16.1 mL of concentrated sulfuric acid (98%) is measured with a measuring cylinder and completely dissolved in 500 mL of deionized water, and finally the two solutions are mixed in a reactor and polymerized immediately. The reactor is placed in a magnetic stirrer, the stirring speed and the temperature around the reactor are set, the electrochemical polymerization mode is set to cyclic voltammetry (CV), a fixed voltage scanning range, scanning rate and number of cycles are set, and the CP film deposited by polypyrrole is named -CP-n according to the number of cycles.
[0109] Preferably, the optimal pyrrole solution concentration is 0.15 mol / L.
[0110] Preferably, a three-electrode system is used in step S2, the working electrode is a treated conductive porous carbon paper-based membrane, the auxiliary electrodes are two titanium meshes with the same area as the conductive porous carbon paper-based membrane, the working electrode is placed between the two auxiliary electrodes, and the reference electrode is a saturated calomel electrode (SCE).
[0111] Preferably, the spacing between the electrodes is 1.5 cm, the stirring speed is 50 RPM, and the reactor temperature is maintained at about 5°C; the system voltage scanning range is -0.2-0.9V, the scanning rate is 0.03-0.06V / S, and the number of cycles is set to 0, 200, 400, 500, 600, and 700, respectively.
[0112] Preferably, the process flow for preparing the aqueous phase solution is to dissolve m-phenylenediamine in deionized water and then ultrasonicate for 10 min-50 min; the process flow for preparing the organic phase solution is to dissolve trimesoyl chloride in n-hexane solvent and then ultrasonicate for 10 min-50 min.
[0113] Preferably, the mass percentage of m-phenylenediamine (m-phenylenediamine) in the aqueous phase solution is 1.0wt%-6.0wt%, and the mass percentage of trimesoyl chloride in the organic phase solution is 0.05wt%-0.5wt%.
[0114] Preferably, the first designated time is 3-7 minutes, and the second designated time is 1-6 minutes, more preferably 2 minutes;
[0115] Furthermore, after obtaining the polyamide skin layer in step (c-3), the method further includes step (d): curing the prepared membrane after natural drying in air, and obtaining a conductive forward osmosis membrane with a polyamide layer after a third specified time.
[0116] Preferably, the third designated time is 30-90 seconds.
[0117] like Figure 2a-2o The following are scanning electron microscope images of the conductive porous carbon paper-based membrane surface with different concentrations of electrochemical polymer polypyrrole at different deposition cycle numbers (200, 400, 500, 600, 700), where: Figure 2a-2e The electrochemical polymer polypyrrole used was 0.1 mol / L polypyrrole deposition concentration. Figure 2f-2j The electrochemical polymer polypyrrole used was 0.15 mol / L polypyrrole deposition concentration. Figure 2k-Figure 2o The electrochemical polymer polypyrrole used has a polypyrrole deposition concentration of 0.2 mol / L. From the electron microscope image, it can be seen that the conductive porous carbon paper-based membrane formed after deposition at a lower polypyrrole deposition concentration of 0.1 mol / L has a large pore size; the conductive porous carbon paper-based membrane formed after deposition at a higher polypyrrole deposition concentration of 0.2 mol / L has a small pore size. Figure 2f-2j It can be seen from the figure that the pore size of the conductive porous carbon paper-based membrane formed after the deposition of polypyrrole at a concentration of 0.15 mol / L is relatively uniform. Polypyrrole can well cover the macroporous structure of the bottom surface of the conductive porous carbon paper substrate and has a relatively smooth surface structure.
[0118] Table 1 shows the porosity and average pore size of the conductive porous carbon paper-based membranes obtained under different layers of CP-0, CP-200, CP-400, CP-500, CP-600, and CP-700 at a deposition concentration of 0.15 mol / L of electrochemical polymer polypyrrole. Among them, CP-0, which is the original conductive porous carbon paper substrate, has a high porosity and ultra-large pore structure, and the porosity and average pore size reach 41.1% and 280 μm. With the increase of the number of polypyrrole intermediate layer cycles, the porosity and average pore size of CP-200, CP-400, CP-500, CP-600, and CP-700 decrease, and the porosity and average pore size reach 30.4% and 0.93 μm. This is because the intermediate layer formed by the deposition and coverage of polypyrrole causes the porosity and average pore size to decrease. The skin layer generated by interfacial polymerization reaction on the base membrane containing the intermediate layer in the embodiment of the present application floats on the surface of the conductive porous carbon paper base membrane and will not penetrate into the base membrane or the penetration of the skin layer into the base membrane is greatly reduced, thereby improving the performance of the forward osmosis membrane.
[0119] Table 1 Porosity and average pore size of base film
[0120]
[0121] The permeation properties of the conductive porous carbon paper-based membranes obtained with different initial deposition concentrations, e.g. Figure 3As shown, the permeability of the conductive porous carbon paper-based membrane can be adjusted by changing the number of cycles to achieve a filter with a nanoscale pore size.
[0122] like Figure 4 As shown, it is a schematic diagram of the resistance of the conductive porous carbon paper-based membrane obtained under different pyrrole deposition concentrations and different deposition cycles. As an important criterion for evaluating conductivity, resistance and the conductivity of an object show an inversely proportional relationship. It can be seen from the figure that at a low initial concentration (0.1mol / L), as the number of cycles increases, the resistance of the conductive porous carbon paper-based membrane gradually decreases. This is because the macroporous structure of the original conductive porous carbon paper-based membrane is not conducive to the transfer of electrons. With the deposition of polypyrrole, the specific surface area is increased, the ion embedding distance is reduced to the nanometer range, and the charge transfer is promoted to reduce the resistance. The deposition concentration of 0.15mol / L shows an excellent trend of enhanced conductivity. Further in the embodiment of the present application, the preferred concentration of deposited polypyrrole on the conductive porous carbon paper-based membrane is 0.15mol / L. At this time, the conductive porous carbon paper-based membrane shows excellent conductivity, and at the same time, its scanning electron microscope image and permeability both show excellent performance. The contact angle of a substrate is an indicator used to characterize whether a surface structure or coating is hydrophilic or hydrophobic. It indicates the force between solid and liquid molecules, that is, the magnitude of the surface tension when a water droplet is covered on the surface of the substrate or coating. Figure 5 The figure shows the schematic diagram of the characterization of the hydrophilicity of the substrate of the conductive porous carbon paper-based membrane (CP-0, CP-200, CP-400, CP-500, CP-600, CP-700 conductive porous carbon paper-based membrane) obtained by depositing polypyrrole at a concentration of 0.15 mol / L corresponding to different deposition layers. It can be seen from the figure that the substrate becomes more and more hydrophilic as the polypyrrole intermediate layer is deposited. This is because the polypyrrole chain contains a large number of N atoms, and the addition of the dopant sodium dodecylbenzene sulfonate (SDBS) during the deposition process increases the hydrophilicity of the substrate. A more hydrophilic substrate makes the intermediate layer conducive to the formation of a more cross-linked and more complete polyamide layer.
[0123] Zeta potential reflects the positive and negative charge and amount on the surface of the solid film. Figure 6 The Zeta potential of the conductive porous carbon paper-based membranes (CP-0, CP-200, CP-400, CP-500, CP-600, CP-700 conductive porous carbon paper-based membranes) obtained with different deposition layers at a deposited polypyrrole concentration of 0.15 mol / L is shown. It can be seen that the CP-0 base membrane exhibits a stable positive charge characteristic. With the deposition of the polypyrrole intermediate layer, the surface of the conductive porous carbon paper-based membrane exhibits a negative charge characteristic. At the same time, the introduction of the dopant sodium dodecylbenzene sulfonate (SDBS) increases the -SO3, thereby further strengthening the negative charge on the membrane surface.
[0124] The surface roughness of the base membrane not only plays a key role in the surface structure, but also has an important influence on the composition of the polyamide layer during the interfacial polymerization process, thereby affecting the separation and permeation performance of the composite membrane. Figure 7a-7f The atomic force microscope images of the conductive porous carbon paper substrates (CP-0, CP-200, CP-400, CP-500, CP-600, CP-700 conductive porous carbon paper substrates) obtained with different deposition layers of deposited polypyrrole concentration of 0.15 mol / L are shown in Table 2. The specific parameters of the surface roughness of these substrates are shown in Table 2. It can be seen that with the increase of the number of polypyrrole deposition layers, the roughness of the substrates shows a trend of first decreasing and then increasing. This is because the uniform deposition of polypyrrole covers the rough macroporous voids of the conductive porous carbon paper substrate, reducing the fluctuation of the pore size and thus reducing the roughness.
[0125] Table 2 Roughness parameters of base film surface
[0126] Basement membrane <![CDATA[R a (nm)]]> <![CDATA[R q (nm)]]> CP-0 819.2±35.2 1027.4±38.6 CP-200 570.2±29.4 717.8±31.7 CP-400 406.8±7.8 532.9±12.6 CP-500 224.1±9.6 282.3±18.1 CP-600 158.4±4.3 197.8±15.4 CP-700 207.8±2.3 291.5±17.9
[0127] Ra stands for: average surface roughness Rq stands for: root mean square roughness
[0128] like Figure 8a1-Figure 9c6 The surface schematic diagram and cross-sectional schematic diagram of the conductive forward osmosis membrane obtained after adding an intermediate layer of polypyrrole of different concentrations in different embodiments of the present application are compared for the forward osmosis membrane formed on the pure CP base membrane; Figure 8a1-Figure 8a6 and Figure 9b1-Figure 9b6 The surface images of the conductive forward osmosis membranes CPFO0, CPFO200, CPFO400, CPFO500, CPFO600 and CPFO700 of the present application formed by the base film after the deposition of polypyrrole with different concentrations and different deposition turns are shown in FIG. Figure 8a1-Figure 8a6 Schematic diagram of the surface image of the conductive forward osmosis membrane formed on the base membrane with different deposition circles at a polypyrrole deposition concentration of 0.1 mol / L; Figure 9b1-Figure 9b6The schematic diagram of the surface image of the conductive forward osmosis membrane formed on the base membrane with different deposition circles of polypyrrole deposition concentration of 0.15 mol / L. It can be seen from the figure that the forward osmosis membrane without polypyrrole intermediate layer has a smooth morphology due to the macropores and hydrophobic properties of its conductive porous substrate, and the polyamide layer formed on the CP-0 base membrane is not ridge-shaped. This is mainly because the macropores and hydrophobic properties of the conductive porous carbon paper base membrane slow down the diffusion rate of the m-phenylenediamine aqueous phase stored in the membrane pores, and the amine monomer adsorbed on the surface of the base membrane is limited. After the polypyrrole intermediate layer is deposited, a continuous, defect-free polyamide layer with a clear ridge-like structure is formed on the conductive porous carbon paper base membrane, and an increasingly larger leaf-like structure is presented. This is because the successful deposition of polypyrrole reduces the macropores of the base membrane, compensating for the macropore defects of the base membrane, making the surface morphology of the base membrane more flat and uniform, so that a perfect, defect-free polyamide layer is formed. On the other hand, the deposition of the polypyrrole intermediate layer changes the surface physical and chemical properties of the base film - the hydrophilicity of the substrate increases, allowing more amine monomers to be adsorbed, which is conducive to the interfacial polymerization reaction and forms a more obvious spine-like structure. Figure 9c1-Figure 9c6 It can be seen that the cross-sectional morphology of the conductive forward osmosis membrane provided by the present application. Figure 9c1 As shown in the figure, it can be seen that the formed polyamide layer is discontinuous and has a collapsed morphology without the deposition of polypyrrole intermediate layer. Figure 9c2-Figure 9c6 It can be seen that after depositing polypyrrole on the conductive porous carbon paper substrate, a continuous polyamide layer is formed on the CPFO200, CPFO400, CPFO500, CPFO600 and CPFO700 membranes, and the thickness increases from 260nm to 560nm. This is because the hydrophilicity of the deposited polypyrrole intermediate layer increases with the deposition time, which makes the m-phenylenediamine have a stronger adsorption force on the substrate, thereby increasing the availability of m-phenylenediamine during the interfacial polymerization process to form a thicker polyamide layer. On the other hand, as the intermediate layer is deposited, the roughness and pore size of the substrate gradually decrease, making the m-phenylenediamine more continuously and evenly distributed on the substrate, which increases the thickness of the polyamide layer.
[0129] like Figure 10a-10fShown are surface atomic force microscope images of conductive forward osmosis membranes CPFO0, CPFO200, CPFO400, CPFO500, CPFO600 and CPFO700 formed on base membranes with different deposition numbers at a polypyrrole deposition concentration of 0.15 mol / L. In the examples of the present application, an atomic force microscope was used to measure the roughness of the prepared polypyrrole conductive forward osmosis membranes with the same deposition time. It can be seen from the figure and combined with Table 3 that the average surface roughness Ra (nm) of CPFO0, CPFO200, CPFO400, CPFO500, CPFO600 and CPFO700 membranes is 380.6±16.8, 257.4±10.4, 209.5±11.3, 171.4±6.9, 107.8±7.4, 164.8±6.5nm, and the root mean square roughness Rq (nm) is 452.4±26.7, 354.8±24.6, 269.9±20.3, 269.0±16.2, 134.0±19.0, 205.8±20.3nm. The roughness of the conductive forward osmosis membrane shows a trend of decreasing first and then increasing. Because the deposited polypyrrole cannot completely cover the rough carbon fiber surface of the conductive porous carbon paper-based membrane, the surface roughness of the CPFO0 membrane is the highest, and the surface roughness of the CPFO200, CPFO400, CPFO500 membranes, CPFO600 and CPFO700 membranes after depositing different layers of conductive polypyrrole in this application are significantly lower than that of CPFO0, and the surface roughness of the membranes formed by different layers is different. With the deposition of the polypyrrole middle layer, the rough carbon fiber surface is completely covered. The roughness of the CPFO600 and CPFO700 membranes shows an increasing trend, because the formed polypyrrole middle layer has high hydrophilicity, which is sufficient to increase the reactivity of m-phenylenediamine and trimesoyl chloride, so the roughness shows an increasing trend.
[0130] Table 3 Roughness of the conductive forward osmosis membrane surface
[0131]
[0132] Ra stands for: average surface roughness Rq stands for: root mean square roughness
[0133] like Fig.11Shown is a schematic diagram of the contact angle of the forward osmosis membrane formed on a pure conductive porous carbon paper substrate, comparing the forward osmosis membrane obtained after adding a polypyrrole intermediate layer deposited at the same concentration but at different cycles in different embodiments of the present application. It can be seen that the forward osmosis membrane prepared on the base membrane exhibits increasingly hydrophilic properties as the deposited polypyrrole intermediate layer is deposited. This is because the deposition of the polypyrrole intermediate layer exhibits strong hydrophilicity, thereby adsorbing more m-phenylenediamine and reacting with trimesoyl chloride to generate more polyamide layers. The polyamide layer contains hydrophilic amino groups, so that the conductive forward osmosis membrane also exhibits an enhanced hydrophilicity effect.
[0134] The comparative forward osmosis membrane formed on the pure conductive porous carbon paper substrate and the forward osmosis membrane obtained after adding the intermediate layer of polypyrrole deposited at the same concentration but with different number of cycles in different embodiments of the present application were analyzed by X-ray spectrometer ( Fig.12 ), Table 4 shows the composition content and ratio of each element on the surface of the prepared conductive forward osmosis membrane, combined with Fig.12 It can be seen from Table 4 that the conductive forward osmosis membranes prepared under different conditions all found oxygen atom peak O1s, nitrogen atom peak N1s, and carbon atom peak C1s, which proves that the polyamide layer was successfully formed on the base membrane. The crosslinking degree of the polyamide layer formed on the base membrane without the deposition of the polypyrrole intermediate layer is 46.24%. At this time, the structure of the polyamide layer formed is loose, the crosslinking degree with the substrate is very low, and it has poor selectivity. With the increase of the deposition time of the polypyrrole, the N1s content value increases, which also indicates to a certain extent the increase in the crosslinking degree of the polyamide layer. The experimental results of the embodiments of the present application show that this is greatly related to the deposited polypyrrole intermediate layer. The increase in the amount of polypyrrole deposition causes the substrate to aggregate and adsorb more water phase-amine monomers. The results show that the concave liquid surface and the continuous smaller surface pore size provided by the high hydrophilicity of the substrate provide a larger reaction area for the interfacial polymerization reaction, thereby forming a continuous, highly selective active layer, resulting in a higher local crosslinking degree.
[0135] Table 4 Percentages of different elements and crosslinking degree of conductive forward osmosis membrane
[0136]
[0137] Electrochemical characterization is a basic and important conductive performance index of conductive composite films, including scanning the cyclic voltammetry curve of conductive composite films ( Fig.13 ) and electrochemical impedance spectroscopy (EIS) tests ( Fig.14), it can be seen from the figure that the original base film has a very stable current under the scanning voltage of -2V to +2V, the shape is narrow and thin, and there is almost no redox trend in the current range of -2V to +2V, and it has good stability in redox. The cyclic voltammetry curve of the conductive forward osmosis membrane with a deposited polypyrrole intermediate layer shows a higher current density than the CPFO0 membrane from -2V to +2V, and the current density increases with the increase in the number of deposition cycles. This is because the electron transfer rate in the conductive membrane is very high after the deposition of polypyrrole, and polypyrrole can tightly wrap the carbon fiber to form a bridging effect. This result is also consistent with the test results of electrochemical impedance, which shows that the impedance of the conductive forward osmosis membrane gradually decreases with the increase in the number of deposition cycles, further confirming the excellent conductivity of the conductive forward osmosis membrane.
[0138] The performance of the conductive forward osmosis membrane of the present application is tested as follows: Fig.15 The conductive cross-flow FO device used in the present application is shown, which is used to test the osmotic selectivity of the forward osmosis membrane. No voltage is applied during the test, the effective membrane area of the conductive forward osmosis membrane 100 in the membrane pool is 15 cm2, deionized water is placed on the stirring device 200 as the raw material liquid, and the sodium chloride solution is placed on the balance 300 as the draw liquid. Two peristaltic pumps 400 and 500 are used to circulate the raw material liquid and the draw liquid respectively. During operation, the temperature of the raw material liquid and the draw liquid is controlled at 25°C, and the rotation speed of the peristaltic pump is 9.8 cm / s.
[0139] like Figure 16a-16bThe figure shows the performance of the forward osmosis membrane formed on the pure conductive porous carbon paper substrate in the FO mode and the performance in the PRO mode after adding the intermediate layer of polypyrrole deposited at the same concentration and different cycle times in different embodiments of the present application. It can be seen from the figure that the forward osmosis membrane prepared with the original conductive porous carbon paper substrate as the base has poor forward osmosis performance, and the conductive forward osmosis membrane after depositing the polypyrrole intermediate layer shows excellent forward osmosis performance. When the deposition cycle is 600, the forward osmosis performance of the conductive forward osmosis membrane reaches the best. The water flux in the FO / PRO mode is 21.09 / 33.96L / (m2h), and the salt return flux is 4.61 / 5.48g / (m2h). When the polypyrrole deposition cycle is 700, the flux is 9.9 / 21.7L / (m2h), and the salt return is 7.71 / 3.38g / (m2h). This is because: the higher hydrophilicity of the polyamide layer will provide a larger passage for water to pass through, thereby showing a higher water flux. The increase in hydrophilicity will make the amine monomer have a stronger adsorption force on the base membrane, so that it can store more amine monomers for interfacial polymerization to generate more amide bonds, which is conducive to the increase of cross-linking degree. The higher the degree of cross-linking, the more amide bonds are generated in the polyamide layer, and the denser the polyamide layer is, thus showing a lower salt return flux. The improvement in performance is partly because the deposition of the polypyrrole intermediate layer fills the rough surface of the carbon fiber, improves the hydrophobic interface characteristics, compensates for the macropore defects and reduces the porosity. The reduction in the roughness of the intermediate layer allows the aqueous phase solution of m-phenylenediamine in the interfacial polymerization process to evenly cover the intermediate layer, making the formed polyamide layer more continuous and not easy to fall off. The improvement of macropore defects prevents the collapse of the polyamide layer, and the small pore structure allows the formation of a continuous, defect-free polyamide layer with a clear leaf-like structure. The osmosis process is performed with the active layer (polyamide) of the forward osmosis membrane facing the feed liquid and the porous support layer (base membrane) facing the draw liquid. This situation is interpreted as the AL-FS mode (also called the FO mode). The osmosis process is performed with the active layer (polyamide layer) of the forward osmosis membrane facing the draw liquid and the porous support layer (base membrane) facing the feed liquid. This situation is interpreted as the AL-DS mode (also called the PRO mode).
[0140] like Figure 17a-17b The figure shows the pure water flux A value and salt permeability coefficient B value of the forward osmosis membrane formed on the pure conductive porous carbon paper substrate, comparing the forward osmosis membrane obtained after adding the intermediate layer of polypyrrole deposited at the same concentration but different number of cycles in different embodiments of the present application ( Fig.17a ) and the schematic diagram of salt rejection rate of forward osmosis membrane ( Fig.17b). In the figure, the pure water flux (A value) and salt permeability coefficient (B value) of CPFO200, CPFO400, CPFO500, CPFO600, and CPFO700 membranes have a trend of first decreasing and then increasing. As the polyamide layer structure deposited on the CP membrane with the polypyrrole intermediate layer becomes more perfect and the cross-linking degree becomes higher, the increase in the cross-linking degree of the polyamide layer has a positive effect on the retention rate. Because a high degree of cross-linking means that the formed polyamide layer has more amide bonds, it shows a higher retention rate and salt permeability coefficient. From the above, it can be seen that the conductive forward osmosis membrane with a polypyrrole intermediate layer has better forward osmosis filtration performance.
[0141] like Figure 18a-18b The diagram shows the water flux diagram (18a) and the reverse salt flux diagram (18b) of the membrane with a polypyrrole deposition concentration at different draw solution concentrations with a cycle number of 600. In the two operating modes of the forward osmosis membrane, the water flux of the forward osmosis membrane increases with the increase of the NaCl draw solution concentration. It is also found that the reverse salt flux also increases. This is mainly because for the same salt solution, a high salt solution concentration will lead to a high osmotic pressure. When the osmotic pressure increases, the flux also increases. The higher draw solution concentration difference will cause more salt to penetrate into the raw solution, resulting in an increase in the reverse salt flux. In the figure, Draw concentration represents the draw solution concentration, Water flux represents the water flux, and Reverse salt flux represents the reverse salt flux.
[0142] In the embodiment of the present application, a conductive composite forward osmosis membrane is prepared by depositing a conductive polymer such as a polypyrrole intermediate layer on a hydrophobic, macroporous porous conductive substrate and then performing an interfacial polymerization reaction. The conductive porous base membrane has excellent conductive properties, a smooth surface structure and nano-scale filter performance, providing a good foundation for the preparation of a perfect cortex.
[0143] In the embodiments of the present application, the deposition concentration of the polypyrrole intermediate layer is preferably 0.1-0.2 mol / L, and further preferably 0.15 mol / L. The polypyrrole intermediate layer at this concentration has excellent conductivity (the minimum square resistance reaches 156.4 mΩ / sq), a smooth surface structure and nano-scale filter performance; when the intermediate layer uses pyrrole with an initial concentration of 0.15 mol / L, the number of deposition turns is preferably 600, and the prepared CPFO600 membrane has excellent performance. At this time, the water flux and salt return in the FO / PRO operating mode are 33.96 / 21.09 L / (m2h) and 5.48 / 4.61 g / (m2h), respectively, and it also has excellent electrochemical reaction activity and minimum impedance.
[0144] When the conductive intermediate layer was deposited using pyrrole at an initial concentration of 0.15 mol / L, the thickness and integrity of the cortex gradually increased with the increase in the number of deposition cycles, and the degree of cross-linking showed a trend of first increasing and then decreasing.
[0145] The conductive forward osmosis membrane of the present application has good conductivity, strong filterability and pollution resistance, and strong stability.
[0146] In the present application, the conductive porous substrate may be one of conductive carbon fiber and conductive paper.
[0147] In the present application, the conductive material of the conductive intermediate layer may also be a negatively charged, hydrophilic conductive material such as polyaniline.
[0148] The polyamide layer forms a smooth shape on the original conductive porous substrate, but it is not a spine-like shape; after the deposition of the intermediate layer, the defects of the rough large pores of the conductive porous carbon paper-based membrane are compensated, and a series of physical and chemical properties such as the hydrophilicity, roughness, pore size, and electrochemical properties of the membrane surface have changed, forming a new substrate morphology, which affects the morphology and performance of the polyamide layer. High hydrophilicity, reasonable small pore size, and uniform roughness provide greater reactivity and contact area for the interfacial polymerization reaction, thereby producing a higher degree of cross-linking and excellent forward osmosis performance.
[0149] The present application is further described in detail below through specific embodiments.
[0150] Example 1
[0151] A conductive forward osmosis membrane was prepared according to the following steps:
[0152] (1) The purchased 10×10 cm conductive porous carbon paper substrate was cut into a size of 5×10 cm and soaked in a culture dish with a 0.2 mol / L NaOH solution for 2 h to enhance the bonding ability between the polypyrrole intermediate layer and the CP membrane. After the soaking, it was rinsed with deionized water until it was neutral.
[0153] (2) 10.35 mL (0.15 mol / L) of pyrrole solution, 3.0 mL of ethylene glycol, 3.0 mL of oxalic acid, and 13.40 g of sodium dodecylbenzene sulfonate were fully dissolved in 500 mL of deionized water. 16.1 mL of concentrated sulfuric acid (98%) was measured with a measuring cylinder and completely dissolved in 500 mL of deionized water. Finally, the two solutions were mixed in a reactor and polymerized immediately using a three-electrode system. The working electrode was a pretreated conductive porous carbon paper-based membrane, the auxiliary electrodes were two titanium meshes with the same area as the CP membrane, the working electrode was placed between the two auxiliary electrodes, and the reference electrode was a saturated calomel electrode (SCE), the spacing between them was 1.5 cm, the four electrodes were completely immersed in the electrochemical polymerization solution, the reactor was placed in a stainless steel basin and placed on a magnetic stirrer, the stirring speed was 50 RPM, and the reactor was surrounded by ice bags to maintain the temperature at about 5°C. The mode of electrochemical polymerization was cyclic voltammetry (CV), in which the voltage scan range was -0.2 V to 0.9 V, the scan rate was 0.05 V / S, and the number of cycles was set to 200.
[0154] (3) Dissolve m-phenylenediamine (MPD) at 3.0 wt% in deionized water in a 50 ml brown bottle and ultrasonicate for 30 min to obtain an aqueous m-phenylenediamine solution; dissolve trimesoyl chloride (1,3,5-benzenetricarboxylic acid chloride (TMC)) at 0.15 wt% in 50 ml of n-hexane solvent and ultrasonicate for 30 min to completely dissolve it to obtain an organic phase solution of trimesoyl chloride.
[0155] (4) The prepared modified conductive porous carbon paper-based membrane is placed flat on a clean glass plate, and fixed and leak-proofed using a stainless steel plate frame and a rubber ring; the conductive porous carbon paper-based membrane after the intermediate layer is deposited is placed face up on the glass plate.
[0156] (5) Pour 50 ml of the prepared m-phenylenediamine aqueous solution into the frame to soak the conductive porous carbon paper-based membrane for 5 minutes, then pour out the excess aqueous solution and remove the stainless steel plate frame and rubber ring to obtain a pretreated membrane.
[0157] (6) Roll a rubber roller over the surface of the pretreated film.
[0158] (7) Pour 50 ml of the prepared trimesoyl chloride organic phase solution into the frame and react for 2 minutes, then pour off the excess organic solution; obtain a preliminary forward osmosis membrane with an interfacial polymerization reaction cortex.
[0159] (8) The obtained preliminary forward osmosis membrane was naturally dried in air for 60 seconds and then placed in an oven for curing for 5 minutes to obtain a conductive forward osmosis membrane having a selectively permeable polyamide layer.
[0160] (9) The prepared conductive forward osmosis membrane with a polyamide layer was stored in deionized water at 4°C until testing.
[0161] The pore diameter of the base membrane in the forward osmosis membrane prepared in the above embodiment is as follows: Figure 2f As shown in Table 1, the average pore diameter is mostly distributed in the range of 110 μm. Fig.16a , 16b As shown in Table 4, deionized water was used as the raw material liquid, and the NaCl aqueous solution was used as the draw liquid. The cross-flow rate and temperature of the raw material liquid and the draw liquid were respectively controlled at 9.8 cm / s and 25° C. After testing, the forward osmosis membrane prepared in the above embodiment had a cross-linking degree of 65.53%, a water contact angle of about 67°, a water flux of 83.4 L / m2h, a reverse salt flux of 82.7 g / m2h, a water permeability coefficient A value of 5.51 L / m2h / bar, a salt permeability coefficient B value of 2.82 L / m2h, and a salt retention rate of 68%.
[0162] The forward osmosis membrane thus produced was designated as CPFO200 membrane.
[0163] Example 2
[0164] The difference between Example 2 and Example 1 is that the number of cycles of polymerizing pyrrole when depositing polypyrrole on the conductive porous carbon paper substrate is set to 400 cycles, and other conditions are consistent with Example 1. The forward osmosis membrane thus prepared is denoted as CPFO400 membrane.
[0165] The pore diameter of the base membrane in the forward osmosis membrane prepared in the above embodiment is as follows: Figure 2g As shown in Table 1, the average pore diameter is mostly distributed at 50.6 μm. Fig.16a , 16b As shown in Table 4, deionized water was used as the raw material liquid, and the NaCl aqueous solution was used as the draw liquid. The cross-flow rate and temperature of the raw material liquid and the draw liquid were respectively controlled at 9.8 cm / s and 25° C. After testing, the forward osmosis membrane prepared in the above embodiment had a cross-linking degree of 76.05%, a water contact angle of about 63°, a water flux of 64.7 L / m2h, a reverse salt flux of 58.2 g / m2h, a water permeability coefficient A value of 4.1 L / m2h / bar, a salt permeability coefficient B value of 1.9 L / m2h, and a salt retention rate of 82.56%.
[0166] Example 3
[0167] The difference between Example 3 and Example 1 is that the number of cycles of polymerizing pyrrole when depositing polypyrrole on the conductive porous carbon paper substrate is set to 500, and other conditions are the same as those of Example 1. The forward osmosis membrane thus prepared is denoted as CPFO500 membrane.
[0168] The pore diameter of the base membrane in the forward osmosis membrane prepared in the above embodiment is as follows: Figure 2h As shown in Table 1, the average pore diameter is mostly distributed at 14.97 μm. Fig.16a , 16b As shown in Table 4, deionized water was used as the raw material liquid, and the NaCl aqueous solution was used as the draw liquid. The cross-flow rate and temperature of the raw material liquid and the draw liquid were respectively controlled at 9.8 cm / s and 25° C. After testing, the forward osmosis membrane prepared in the above embodiment had a cross-linking degree of 80.60%, a water contact angle of about 58°, a water flux of 14.21 L / m2h, a reverse salt flux of 12.07 g / m2h, a water permeability coefficient A value of 2.74 L / m2h / bar, a salt permeability coefficient B value of 0.81 L / m2h, and a salt retention rate of 88.09%.
[0169] Example 4
[0170] The difference between Example 4 and Example 1 is that the number of cycles of polymerizing pyrrole when depositing polypyrrole on the conductive porous carbon paper substrate is set to 600, and other conditions are the same as those of Example 1. The forward osmosis membrane thus prepared is denoted as CPFO600 membrane.
[0171] The pore diameter of the base membrane in the forward osmosis membrane prepared in the above embodiment is as follows: Figure 2i As shown in Table 1, the average pore diameter is mostly distributed in the range of 1.08 μm. Fig.16a , 16b As shown in Table 4, deionized water was used as the raw material liquid, and the NaCl aqueous solution was used as the draw liquid. The cross-flow rate and temperature of the raw material liquid and the draw liquid were respectively controlled at 9.8 cm / s and 25° C. After testing, the forward osmosis membrane prepared in the above embodiment had a cross-linking degree of 85.26%, a water contact angle of about 52°, a water flux of 21.09 L / m2h, a reverse salt flux of 4.61 g / m2h, a water permeability coefficient A value of 2.85 L / m2h / bar, a salt permeability coefficient B value of 0.26 L / m2h, and a salt retention rate of 98.61%.
[0172] Example 5
[0173] The difference between Example 5 and Example 1 is that the number of cycles of polymerizing pyrrole when depositing polypyrrole on the conductive porous carbon paper substrate is set to 700, and other conditions are consistent with Example 1. The forward osmosis membrane thus prepared is denoted as CPFO700 membrane.
[0174] The pore diameter of the base membrane in the forward osmosis membrane prepared in the above embodiment is as follows: Figure 2j As shown in Table 1, the average pore diameter is mostly distributed at 0.93 μm. Fig.16a , 16bAs shown in Table 4, deionized water was used as the raw material liquid, and the NaCl aqueous solution was used as the draw liquid. The cross-flow rate and temperature of the raw material liquid and the draw liquid were respectively controlled at 9.8 cm / s and 25° C. After testing, the forward osmosis membrane prepared in the above embodiment had a cross-linking degree of 85.48%, a water contact angle of about 46°, a water flux of 9.9 L / m2h, a reverse salt flux of 7.71 g / m2h, a water permeability coefficient A value of 2.23 L / m2h / bar, a salt permeability coefficient B value of 0.31 L / m2h, and a salt retention rate of 97.53%.
[0175] The present application regulates the pore size and hydrophilicity of the conductive porous carbon paper-based membrane by electrochemically depositing a polypyrrole intermediate layer, and forms a non-collapsed and continuous polyamide layer through an interfacial polymerization (IP) process, thereby preparing a conductive forward osmosis membrane, and testing its algae-water separation performance. The conductive forward osmosis membrane was characterized and analyzed by scanning electron microscopy, solid surface zeta potential instrument, and X-ray photoelectron spectrometer. The performance and structure of the conductive forward osmosis membrane provided in this application are mainly as follows: the skin thickness is 260nm-560nm; the cross-linking degree is 46.24%-85.48%; the water contact angle is 46°-74°, of which the water contact angle of the base membrane part is 29°-88°; the zeta potential is -25mv-5mv; in FO mode, the water flux of the conductive forward osmosis membrane can reach up to 92L / m2h, and the reverse salt flux is as low as 4.61g / m2h; in PRO mode, the water flux of the conductive forward osmosis membrane is as high as 135.08L / m2h, and the reverse salt flux is as low as 0.58g / m2h; the salt interception rate can reach 97%-98.6%. The results show that the polypyrrole intermediate layer with a suitable number of cycles at the optimal concentration can well regulate the conductive porous carbon paper base membrane and prepare a conductive forward osmosis membrane with excellent separation performance.
[0176] Application Example 1:
[0177] Application description of the application of conductive forward osmosis membrane in the treatment of algae liquid and algae water separation. In the application of forward osmosis membrane technology, membrane pollution has always been a challenge that is difficult to completely solve. Other researchers have also done a lot of research on anti-membrane pollution, such as modifying the surface charge of the PA layer, modifying the support layer of the composite membrane, pre-treating pollutants, etc., but these methods are relatively complicated in preparation and will introduce new sources of pollution. The present application proposes to separate algae water by applying voltage to a conductive forward osmosis membrane. The following is a description of the application of the forward osmosis algae liquid treatment method and forward osmosis algae liquid treatment system for treating algae liquid and algae water in this application, and the stability of the conductive composite FO membrane during long-term multi-cycle operation.
[0178] The forward osmosis method and system for treating algae-water separation provided in the present application include a conductive forward osmosis membrane, and a negative voltage is applied in the treatment process or system. Further, the conductive forward osmosis membrane is the forward osmosis membrane provided in the present application, and the negative voltage is -4.0V-0V (excluding 0V), further -0.5V, -1.0V, -1.5V, -2.0V, -2.5V, -3.0V, -4.0V.
[0179] like Figure 19a-19b FIG. 1 is a schematic diagram showing the change in membrane flux of a conductive forward osmosis membrane in an application example of the present application under different applied voltages, wherein Fig.19a The negative voltage applied, Fig.19b A positive voltage is applied. Fig.19a It can be seen that in the absence of an external electric field, the flux of algae-containing water decreased by 64% after continuous treatment for 8 hours. This is mainly because a large number of algae cells and extracellular polymers are deposited and adhered to the surface of the conductive forward osmosis membrane and enter the membrane pores during the treatment of algae-containing water, thereby blocking the surface pores of the conductive forward osmosis membrane and causing serious membrane pollution, resulting in a decrease in flux. When a negative voltage is applied to the conductive forward osmosis membrane, as the magnitude of the applied negative voltage increases, the membrane flux of the conductive forward osmosis membrane treating algae-containing water decreases by 56%, 46%, and 34%, respectively. When a -2V voltage is applied, the membrane flux increases by 34% compared to when no voltage is applied, because the applied negative voltage has an electrostatic repulsion effect with the negatively charged pollutants in the algae water, which alleviates the process of pollutants adhering to the surface of the conductive forward osmosis membrane, thereby reducing the membrane pollution phenomenon in the treatment of algae-containing water.
[0180] Fig.19b The figure shows the membrane flux when a positive voltage is applied to the conductive forward osmosis membrane. It can be seen from the figure that when a positive charge is applied to the CPFO, the downward trend of the membrane flux for treating algae-containing water is alleviated. When +1.0V, +1.5V, and +2.0V voltages are applied to the composite membrane, the membrane flux for treating algae-containing water decreases by 64%, 72%, and 80%, respectively. In contrast, it can be found that the flux decreases by 16% when a +2.0V voltage is applied compared to when there is no voltage. This is because the algae cells and extracellular organic matter in the algae water carry a large amount of negative charge. When a positive voltage is applied to the membrane, electrostatic attraction will occur, causing more pollutants to adhere to the membrane surface to form a thicker filter cake layer, resulting in more serious membrane pollution when a positive voltage is applied than when there is no voltage.
[0181] like Figure 20a-20gThe figure shows a schematic diagram of the thickness of the filter cake layer of the conductive forward osmosis membrane cross-section in the embodiment of the present application when different voltages are applied. The voltages applied in the figure are 0V, -1.0V, -1.5V, -2.0V, +1.0V, +1.5V and +2V. It can be seen from the figure that when a negative voltage is applied, the thickness of the filter cake layer gradually decreases from 12.56μm when no voltage is applied to 5.71μm when -2V voltage is applied. This shows that the application of a negative voltage produces an electrostatic repulsion effect on pollutants, reducing the membrane fouling phenomenon during the treatment of algae-containing water. After applying a positive voltage, the thickness of the filter cake layer becomes gradually thicker than when no voltage is applied as the applied voltage increases. This is because the application of positive electricity will produce an electrostatic attraction effect on the pollutants, causing more pollutants to adhere to the membrane surface, aggravating the membrane fouling during the treatment of algae-containing water.
[0182] like Figure 21a-Figure 21d The figure shows the effect of applying different voltages on the membrane performance of the conductive forward osmosis membrane in the application example of the present application under single and mixed algae water components, wherein 21a and 21b are flux change schematic diagrams, 21c is a flux recovery rate schematic diagram, and 21d is a membrane resistance schematic diagram. Fig.21aIn the case of the algae water component alone, when no voltage is applied, the flux of intracellular organic matter (IOM) of algae decreases more than the flux of extracellular organic matter (EOM). The final specific fluxes of intracellular organic matter and extracellular organic matter after 8 hours of operation are 0.31 and 0.36, respectively. This is related to the composition of the two substances. Because the negative potential carried by intracellular organic matter is less than that of extracellular organic matter and at the same soluble organic carbon (DOC) concentration, intracellular organic matter contains more small molecules and particles, so intracellular organic matter is more likely to adhere to the membrane surface and clog the pores, causing a more serious flux decrease. After applying a -2V electric field, due to the charge characteristics of extracellular organic matter and intracellular organic matter, the flux decrease will be slowed down. After running for 8 hours, the final specific flux of live and dead algae cells was 0.17 and 0.13. This is because the Zeta potential value of dead algae cell solution is lower than that of live algae cell solution, so dead algae cells are more likely to aggregate and precipitate in the solution and are more likely to adhere to the surface of the composite membrane. Another reason is that the broken cell structure of dead algae cells has a smaller molecular structure, so it is easy to enter the membrane pores and block the membrane pores, causing more serious membrane pollution. The reason why the flux of live and dead algae cells decays faster than that of extracellular organic matter and intracellular organic matter is that under long-term operation conditions, algae cells are compressible, and the pressure on the filter cake layer formed by algae cells gradually increases. The filter cake layer is compressed and becomes less porous, causing rapid flux decay. When a voltage of -2V is applied, it can be observed that the flux of live and dead algae cells is increased by 42% and 34% respectively compared with no voltage application. This is because the large amount of negative charges carried by live and dead algae cells themselves have an electrostatic repulsion effect with the applied negative voltage, which slows down the adhesion of algae cells on the forward osmosis membrane, reduces the accumulation of pollutants on the membrane surface, and thus alleviates the decline in membrane flux. The reason why the flux attenuation of extracellular and intracellular organic matter is not significantly improved after voltage is applied is that their own negative potential is relatively low, which slows down the effect of electrostatic repulsion (the flux is increased by 6% and 4% respectively compared with when voltage is applied).
[0183] exist Figure 21bIt can be seen from the flux change diagram of the mixed algae water components that, without applying voltage, the flux of live algae cells + extracellular organic matter decreased the fastest among the three mixed algae water components, and the final specific flux was 0.08. This is because there is a synergistic effect between live algae cells and extracellular organic matter. The compressible thick cake layer formed by algae cells and the extracellular organic matter continue to fill the gaps between algae cells to form serious complex pollution. In the presence of dead algae cells, the cake layer formed by the incompressibility of broken algae cells is thinner than that formed by live algae cells. Although the same organic matter fills the gaps in the cake layer, the final specific flux is slightly higher than that of live algae cells + extracellular organic matter. When a -2V electric field is applied, it can be seen from the figure that compared with no voltage application, the flux attenuation of the three mixed algae water components (live algae cells + extracellular organic matter, dead algae cells + extracellular organic matter + intracellular organic matter, dead algae cells + intracellular organic matter) has been alleviated, increasing by 37%, 27%, and 29% respectively. Because the live algae cells + extracellular organic matter themselves have the most negative charges, they have stronger electrostatic repulsion to reduce the attachment of pollutants, so when a negative voltage is applied, the membrane flux alleviation effect is higher than that of the other two mixed components.
[0184] Fig.21c and Fig.21dThe diagrams are flux recovery rate and membrane resistance. From the two figures, we can see the increase of flux recovery rate and the decrease of reversible and irreversible resistance after voltage is applied. In the figure, the flux recovery rates of the membranes polluted by extracellular organic matter and intracellular organic matter after hydraulic cleaning are 89.5% and 86.2% respectively, which indicates that part of the extracellular organic matter and intracellular organic matter adhere to the surface of the membrane and block the membrane pores, thus causing irreversible pollution. Due to its own characteristics, the irreversible pollution degree of intracellular organic matter is more serious than that of extracellular organic matter. The flux recovery rates of live and dead algae cells after hydraulic cleaning are 97% and 90% respectively, which indicates that organic membrane pollution is the main component of irreversible pollution in forward osmosis membrane pollution. The membrane pollution of live and dead algae cells alone can be removed under hydraulic cleaning, and the main pollution caused is reversible pollution. Among the three mixed algae water components, the maximum flux recovery rate of live algae cells + extracellular organic matter after hydraulic washing reached 92%, and the reversible resistance was the highest in algae-containing water. The flux recovery rates of dead algae cells + extracellular organic matter + intracellular organic matter and dead algae cells + intracellular organic matter after hydraulic flushing were 80.3% and 82.1%, respectively. This shows that irreversible pollution has intensified, because both dead algae cells and intracellular organic matter will lead to an increase in irreversible pollution. Therefore, when dead algae cells, intracellular organic matter and extracellular organic matter exist at the same time, irreversible pollution is the most serious. Therefore, for mixed algae components, the reversibility of pollution is worse than that observed in single algae components. Through the above application implementation instructions, the forward osmosis membrane of the present application has strong anti-fouling and stability. At the same time, it can be seen that after applying a negative voltage, the membrane pollution of each membrane is reduced, and the pollutants adhering to the membrane surface are greatly reduced.
[0185] like Fig.22a , Figure 22a1-Figure 22g1 , Figure 22a2-Figure 22g2 , Figure 22a1'-Figure 22g1' , Figure 22a2'-Figure 22g2' The figure shows a scanning electron microscope schematic diagram of the conductive forward osmosis membrane in the embodiment of the present application under different algae water components under different voltages. Fig.22a This is the scanning electron microscope image of the original film surface. Figure 22a1-22g1 The scanning electron micrographs of the membrane surface after being contaminated by extracellular organic matter, intracellular organic matter, live algae cells, dead algae cells, live algae cells + extracellular organic matter, dead algae cells + intracellular organic matter, and dead algae cells + extracellular organic matter + intracellular organic matter without applying voltage, respectively; Figure 22a2-22g2 The scanning electron micrographs of the membrane surface after being contaminated by extracellular organic matter, intracellular organic matter, live algae cells, dead algae cells, live algae cells + extracellular organic matter, dead algae cells + intracellular organic matter, and dead algae cells + extracellular organic matter + intracellular organic matter under the application of -2V voltage are shown respectively; Figure 22a1'-22g1'The scanning electron micrographs of the membrane cross-sections after being contaminated by extracellular organic matter, intracellular organic matter, live algae cells, dead algae cells, live algae cells + extracellular organic matter, dead algae cells + intracellular organic matter, and dead algae cells + extracellular organic matter + intracellular organic matter without voltage applied; Figure 22a2'-22g2' The following are the scanning electron microscope images of the membrane cross-sections after the contamination of extracellular organic matter, intracellular organic matter, live algae cells, dead algae cells, live algae cells + extracellular organic matter, dead algae cells + intracellular organic matter, and dead algae cells + extracellular organic matter + intracellular organic matter under the application of -2 V voltage. It can be seen from the figure that after the negative voltage is applied, the membrane contamination of each membrane is reduced, and the pollutants adhering to the membrane surface are greatly reduced. Among them, the thickness of the filter cake layer on the membrane surface of the three mixed algae components is reduced, which reduces the attenuation of the flux and also reduces the reversible and irreversible membrane contamination.
[0186] The following application examples illustrate the effect of coexisting substances in water on the conductive forward osmosis membrane in algae-water separation.
[0187] The composition of natural algae water is relatively complex, containing a large amount of inorganic substances, organic substances, inorganic particles and other substances. Existing research technology shows that in ultrafiltration, algae cells and soluble algae products have a synergistic effect on membrane pollution in the coexistence of natural organic matter and inorganic particles, thereby affecting membrane pollution. The following application examples of this application add Ca2+, HA and kaolin to algae water to experiment the effect of inorganic substances, organic substances and inorganic particles coexisting in algae water on the conductive forward osmosis membrane pollution and pollutant removal of this application during the separation of algae water.
[0188] Application Example 2: Effect of Algae Water with Ca2+ Coexistence on Forward Osmosis Membrane
[0189] First, Ca2+ was added to the algae-containing water to illustrate the impact of CPFO membrane fouling. After each cycle of the fouling experiment, the membrane was physically cleaned and the draw solution and feed solution were replaced. Fig.23a , 23b, 23c, 23d, and 23e. It can be seen that in the continuous multi-cycle operation, when there is no Ca2+ in the algae water, as the operation cycle increases, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 9%, 20%, and 25%, respectively. After the voltage is applied, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 2%, 7%, and 12%, respectively. This indicates that long-term multi-cycle operation under the application of negative voltage slows down the decline in flux because the electrostatic repulsion between the CPFO membrane and the algae-containing water reduces the adhesion of algae pollutants. When the coexisting substance Ca2+ is added to the algae water, as the operation cycle increases, when no voltage is applied, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 15%, 25%, and 37%, respectively. The reason is that Ca2+ promotes its combination with oxygen-containing functional groups in the algae water and the surface of the algae water membrane. Studies have shown that the average porosity of the gel cake layer formed by Ca2+ and algae will show a linear downward trend with the increase of Ca2+ concentration when the critical calcium ion concentration exceeds 6mm / L (the Ca2+ value in this experiment is 8mmol / L). Therefore, the combination of Ca2+ and algae water becomes more tightly cross-linked and denser, which is different from the floc cake layer formed in the algae water. Fig.23a , 23b It can be seen that when Ca2+ is added, the particle size in the algae water gradually increases to form a stable and dense cross-linked gel network, resulting in increased membrane fouling and irreversible fouling. When Ca2+ is added and a negative voltage is applied at the same time, the initial flux of the 2nd, 3rd, and 4th cycles on the CPFO membrane surface decreases by 5%, 10%, and 14%, respectively, indicating that membrane fouling can be effectively slowed down when a negative voltage is applied. It is found that under the same conditions, the membrane has stronger pollution resistance and stability when a negative voltage is applied than when no negative voltage is applied, and the water flux decreases less.
[0190] Next is the description of pollutant removal. When voltage is applied, the removal rate of CPFO membrane for algae toxins in four cycles is above 99.5%, because the mutual repulsion between algae toxin molecules and the surface of CPFO membrane hinders the migration of pollutants to the membrane surface, thereby increasing the removal rate. Fig.23a , 23b , 23c, 23d, and 23e, it can be seen that the removal rate of CPFO membrane for algae toxins in the four cycles is relatively low at around 95.5%. However, when Ca2+ is added to the solution, the removal rate of CPFO membrane for algae toxins is above 99.5%. This is because the adsorption kinetics and isothermal experimental studies have shown that the presence of K+ or Ca2+ in the solution will enhance the adsorption sites for microcystin adsorption, which promotes the adsorption of MC-LR in the filter cake layer to achieve a high retention rate of >99.5. The removal rates of 2-MIB and GSM are as follows: Fig.23d and 23eIt can be seen that in the first cycle, only when no voltage was applied and Ca2+ was added, the removal rate reached more than 99.5%, and the other conditions were all above 95%. In the second, third, and fourth cycles, it was found that the removal efficiency of 2-MIB and GSM reached more than 99.5%. This is because these two pollutants themselves are not charged. In the case of heavy pollution, the pore size screening of the densely cross-linked filter cake layer with smaller porosity formed by Ca2+ on the membrane surface and algae water can achieve the ideal removal effect, realizing the improvement of the removal rate from about 95% to more than 99%.
[0191] This application example shows that among the coexisting substances in water, when Ca2+ coexists in algae-containing water, without applying voltage, with long-term operation, the membrane pollution has a more serious membrane pollution than when Ca2+ is not present. This is because the combination of Ca2+ and oxygen-containing functional groups in algae water on the membrane surface forms a dense cross-linked dirt layer, which strengthens the membrane pollution. When a negative voltage is applied, the membrane pollution is reduced in the algae water after adding Ca2+, reducing the flux attenuation. When Ca2+ is added to the solution, the removal rate of MC-LR, 2-MIB and GSM reaches more than 99.5%: adsorption kinetics and isothermal experimental studies have shown that the presence of K+ or Ca2+ in the solution will enhance the adsorption sites for microcystin adsorption, which promotes the adsorption of MC-LR in the filter cake layer to achieve a high retention rate of MC-LR. The two pollutants 2-MIB and GSM themselves are electrically neutral, and the pore size screening of the dense cross-linked filter cake layer formed by Ca2+ and algae water on the membrane surface achieves an ideal removal effect. In general, under the same conditions, the membrane fouling degree is lower when negative voltage is applied.
[0192] Application Example 3: Effect of Algae Water with HA Coexistence on Conductive Forward Osmosis Membrane
[0193] Figure 24a-Figure 24e The effect of HA addition on CPFO membrane specific flux. Fig.24a is the effect of HA on membrane flux; Figure 24b is the effect of HA on the particle size in algae-containing water; Figure 24c-Figure 24eIt is a schematic diagram of pollutant removal rate; it can be seen that in the continuous multi-cycle operation, first, when HA does not exist in the algae-containing water, as the operation cycle increases, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 9%, 20%, and 25%, respectively. After the voltage is applied, the initial flux decreases of the 2nd, 3rd, and 4th cycles slow down by 6%, 11%, and 10%. The reason is that long-term multi-cycle operation with voltage applied slows down the decline in flux. The reason is that the electrostatic repulsion between the CPFO membrane and the algae-containing water reduces the adhesion of algae pollutants. When the coexisting substance HA is added to the algae-containing water, it is equivalent to increasing the concentration of organic matter in the algae water. As the operation cycle increases, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 15%, 25%, and 37%, respectively. The reason is that HA can be adsorbed on the EOM surface through hydrophobic action, enhancing the hydrophobicity of EOM, thereby increasing the irreversibility of membrane pollution. Correspondingly, from Fig.24a , 24b , 24c, 24d, and 24e, it can be seen that the particle size in the algae water gradually increases with time when HA is added. When voltage is applied to the CPFO membrane surface, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 5%, 10%, and 14%, respectively, indicating that membrane fouling can be effectively slowed down when negative voltage is applied. However, when voltage is applied to the CPFO membrane surface, Fig.24a It was found that the presence of HA reduced the flux attenuation compared to the absence of HA. This is because the addition of HA will make the algae-containing water contaminated liquid weakly acidic. Studies have shown that current density and weakly acidic pH are conducive to the rapid formation of large flocs and porous structures, effectively reducing membrane pore blockage. This is also related to Figure 24b When voltage is applied, the addition of HA causes the particle size in the algae water to gradually increase accordingly. This porous filter cake layer structure effectively alleviates membrane fouling.
[0194] In the study of pollutant removal in algae-containing water, when a voltage of -2V was applied, the removal rate of MC-LR by CPFO membrane in 4 cycles was above 99.5%, which was higher than that when no voltage was applied. This is because when a negative voltage is applied, the electrostatic repulsion between the negative charge of MC-LR molecules and the negative voltage applied to the membrane increases the removal rate of MC-LR. When no voltage is applied and HA does not coexist, the CPFO membrane shows that although it is also electronegative, it can be seen from the above application example diagram that the weak negative charge on the membrane surface cannot completely remove MC-LR in algae-containing water. However, when HA is added to the solution, it can be observed that the removal rate of MC-LR by CPFO membrane in 4 cycles also reaches above 99.5%. This is because of the background effect of HA. Some studies have shown that humus increases the negative charge on the membrane surface, thereby strengthening the electrostatic repulsion between MC-LR molecules and CPFO membrane to achieve a high removal rate. Different results are shown for the removal rates of 2-MIB and GSM. Fig.24d, 24e It can be seen that in the absence of HA, the removal rates of 2-MIB and GSM in the four cycles were all around 95%, which is a low removal rate. This may be because these two pollutants themselves are not charged and are only retained by the highly selective PA layer of the CPFO membrane. However, when HA is present in algae-containing water, it is found that the removal rates of 2-MIB and GSM in the four cycles are all above 99.5%. This is because 2-MIB and GSM are easily combined with coexisting humus in the coexisting water (the interaction between humus and 2-MIB is mainly van der Waals force and hydrogen bond, which is consistent with the fact that HA is mainly composed of proteins, amino acids and peptides), resulting in changes in the physical and chemical properties of 2-MIB and changes in its migration and removal behavior to achieve the effect of enhancing the removal rate.
[0195] The above application examples illustrate that when HA coexists in algae-containing water, the reason why the membrane pollution in the presence of HA is more serious than that in the absence of HA when no voltage is applied is that HA can be adsorbed on the EOM surface through hydrophobic action, enhancing the hydrophobicity of EOM, thereby increasing the irreversibility of membrane pollution. When voltage is applied to the surface of the CPFO membrane, the presence of HA reduces the flux attenuation (membrane flux relief is 9%) compared to when HA is not added. This is because the addition of HA will make the algae-containing water contaminated liquid weakly acidic, and the weak current density and weakly acidic pH generated by the applied voltage are conducive to the rapid generation of large flocs and porous structures, effectively reducing the blockage of membrane pores. When HA is added to the solution, the removal rate of MC-LR, 2-MIB and GSM reaches more than 99.5% because: the background effect of HA increases the negative charge on the membrane surface, thereby strengthening the electrostatic repulsion between the MC-LR molecules and the CPFO membrane to achieve a high removal rate. 2-MIB and GSM easily combine with the coexisting humus in the coexisting water (the interaction between humus and 2-MIB is mainly van der Waals force and hydrogen bond), resulting in changes in the physical and chemical properties of 2-MIB to achieve a high removal rate.
[0196] Application Example 4: Effect of Algae Water with Kaolinite on Conductive Forward Osmosis Membrane
[0197] Figure 25a-Figure 25eIt is the effect of the presence of Kaolinite coexisting substances on the specific flux of the CPFO membrane. It can be seen in the continuous multi-cycle operation that, first, when there is no Kaolinite in the algae-containing water, as the operation cycle increases, the flux decrease when the voltage is applied is alleviated by 5%, 13%, and 17% respectively compared with not applying voltage. The reason is also because the electrostatic repulsion on the surface of the CPFO membrane mentioned above reduces the adhesion of algae pollutants. When Kaolinite is present in the algae-containing water, the initial flux of the 2nd, 3rd, and 4th cycles decreases by 10%, 18%, and 27%. This is because the presence of Kaolinite inorganic particles increases the thickness of the fouling layer with the long operation of each cycle, which increases the hydraulic resistance and makes the external concentration polarization phenomenon in the FO process more serious, thereby aggravating membrane pollution and reducing water flux. When voltage is applied, from Fig.25a It was found that the flux attenuation was alleviated when kaolin was added compared to when kaolin was not present. This was because the current density generated by the applied voltage caused kaolinite to produce aluminum coagulants per unit time, thereby enhancing the aggregation of pollutants in algae-containing water and forming large-size flocs ( Fig.25b The data in can prove that) thus reducing membrane fouling.
[0198] In the study of pollutant removal in algae-containing water, Fig.25c It can be seen that when voltage is applied, the removal rate of MC-LR by CPFO membrane in 4 cycles is above 99.5%, but when no voltage is applied, it is found that the removal rate of MC-LR in algae-containing water with kaolinite particles added (>99.5%) is higher than that without kaolinite particles (<95%). This is because MC-LR can enhance the interception and filtration through particles with fine texture on the surface of high viscosity clay minerals such as kaolinite, thereby enhancing removal. The removal rate of 2-MIB and GSM is from Fig.25c , 25d It can be seen from Figures 25e that when Kaolinite was added, the removal rates of 2-MIB and GSM were all above 99.5% in the four cycles. This is because the layered structure of Kaolinite itself has strong adsorption, which enhances the retention rate of CPFO membrane for 2-MIB and GSM.
[0199] When Kaolinite coexists in algae-containing water, when no voltage is applied, the membrane fouling is heavier when Kaolinite is present than when Kaolinite is not present because the addition of Kaolinite masks the negative charge on the surface of algae cells, thereby weakening the electrostatic repulsion with the CPFO membrane surface and aggravating the membrane fouling. When a negative voltage is applied to the membrane surface, the membrane fouling is reduced when Kaolinite is present than when it is not present (membrane flux relief is 7%). This is because the current generated by the negative voltage causes kaolinite to produce aluminum coagulants per unit time, thereby enhancing the aggregation of pollutants and forming large-particle flocs that reduce membrane fouling. When Kaolinite is added to the solution, the removal rates of MC-LR, 2-MIB and GSM reach more than 99.5% because MC-LR can enhance the interception and filtration through high-viscosity clay minerals such as kaolinite with fine textures on the surface, thereby enhancing the removal rate. 2-MIB and GSM are due to the strong adsorption of organic matter by the layered structure of Kaolinite itself, thereby enhancing the removal efficiency.
[0200] The conductive forward osmosis membrane provided by the present application maintains stronger pollution resistance and strong stability during long-term multi-cycle operation.
[0201] The conductive forward osmosis membrane prepared in this application maintains strong performance in algae-water separation stability and pollutant removal capacity under long-term operation. In the examples of this application, the prepared conductive forward osmosis membrane was subjected to a long-term operation experiment for 6 consecutive cycles. In order to further verify that the prepared composite membrane has continuous and reusable value, after running for 6 cycles, the PA layer of the composite membrane was peeled off, and the PA layer was continued to be generated on the original conductive substrate by interfacial polymerization. This regenerated conductive composite base membrane was named CPFO-C, and CPFO-C continued to explore its long-term stability of algae-water separation and pollutant removal capacity. Some physical and chemical properties of CPFO and CPFO-C membranes were analyzed and characterized.
[0202] In order to better illustrate the stability of the CPFO membrane under long-term operation conditions, after the CPFO membrane has been running continuously for 6 cycles (8 hours per cycle), the PA layer on the surface is peeled off and interfacial polymerization is performed again. At this time, the conductive FO membrane is named CPFO-C membrane. Next, the flux stability and pollutant removal ability of the CPFO membrane in algae-water separation after running continuously for 6 cycles (8 hours per cycle) are explained.
[0203] from Fig.26a , Figure 26bThe figure shows the membrane flux changes of CPFO and CPFO-C membranes under long-term operation and the FT-IR spectrum of the ppy middle layer after stripping the PA layer of the CPFO membrane. It can be seen that the CPFO-C membrane after stripping, compared with the CPFO membrane before stripping, still maintains operational stability after 6 consecutive cycles of long-term operation, except for the flux drop caused by irreversible membrane fouling caused by algae-containing water in the CPFO membrane. Figure 26b It can be seen from the mid-infrared spectrum that the continuous use of the CP base film did not change the chemical composition of the ppy intermediate layer, and no new functional group peaks appeared. The stable base film properties also produced a well-shaped PA layer structure after peeling off the original PA layer by interfacial polymerization reaction (such as Figures 27a-27f , SEM images of CPFO membrane before and after peeling, where Fig.27a , 27d This is a SEM schematic diagram of the PA layer of the CPFO membrane; Figure 27b , Fig.27e This is a SEM diagram of the exposed ppy middle layer after peeling off the PA layer; Fig.27c , Figure 27f SEM schematic diagram of the PA layer of CPFO-C membrane.
[0204] Table 4-2 Pollutant removal efficiency (Remove ratio) of CPFO membrane and CPFO-C membrane
[0205]
[0206] In the case of long-term operation, it was found that the flux of the CPFO membrane before and after the PA layer was stripped off was slightly reduced, and the removal efficiency of the three pollutants remained very high. Mainly through SEM, pollutant removal efficiency, and Fourier infrared spectroscopy tests, it was found that the CP-based membrane still maintained stable chemical properties and composite FO performance with long-term operation. Therefore, long-term operation will not damage the physical and chemical properties and performance of the CPFO membrane, and it has strong chemical practicality and durability.
[0207] In addition, the conductive forward osmosis membrane provided by the present application is prepared by electrochemically depositing a polypyrrole intermediate layer on a conductive porous carbon paper substrate. The deposition of the polypyrrole intermediate layer compensates for the defects of the rough macropores of the conductive porous carbon paper substrate, so that a series of physical and chemical properties of the substrate surface, such as hydrophilicity, roughness, pore size, and electrochemical properties, have changed, and the new morphology of the intermediate layer will affect the morphology and performance of the polyamide layer. As the number of polypyrrole intermediate layer deposition turns increases, the conductive porous carbon paper substrate forms a completely new substrate morphology. The high hydrophilicity, reasonable small pore size, and uniform roughness provide greater reaction activity and contact area for the reaction of m-phenylenediamine and trimesoyl chloride, thereby producing a higher degree of crosslinking and excellent forward osmosis performance.
[0208] In addition, the forward osmosis membrane provided in the present application has a substrate surface pore size of 1.08±3.4μm, a porosity of 34.6±1.7%, and a hydrophilic contact angle of 32.4±2.31° under the conditions of a preferred pyrrole concentration of 0.15mol / L and a further preferred number of turns of 600 turns. The conductive forward osmosis membrane prepared under these conditions has the best electrochemical activity and the lowest impedance, and the forward osmosis performance also reaches the best data: the water flux and the salt return flux under the FO / PRO operating mode are 33.96 / 21.09L / (m2h) and 5.48 / 4.61g / (m2h), respectively.
[0209] In addition, the forward osmosis membrane provided in the present application has a high removal rate for undesirable metabolites in algae-containing water, such as algae toxins (MC-LR), geosmin (GSM), and dimethyl isoborneol (2-MIB). Under the influence of the electric field strength, applying a negative voltage can greatly alleviate the membrane pollution phenomenon, and the flux is increased by 34% when a -2V voltage is applied compared to when no voltage is applied. Whether or not a voltage is applied, the removal rate of the conductive forward osmosis membrane for the three pollutants reaches more than 95%, wherein the removal rate of MC-LR when a negative voltage is applied reaches more than 99.5%, and the removal of GSM and 2-MIB is more than 95%.
[0210] In addition, after voltage is applied, the forward osmosis membrane provided in the present application has the best membrane flux for the live algae cells + extracellular organic matter in the mixed algae water component, and the improvement effect is about 37%.
[0211] In addition, when the forward osmosis membrane provided by the present application is operated for a long time, even if the polyamide layer is peeled off, except for a slight decrease in flux, the removal rate of algae toxins, geosmin, and dimethyl isoborneol still maintains a very high effect, and will not cause damage to the physical and chemical properties and performance of the conductive forward osmosis membrane, and has strong chemical practicality and durability.
[0212] The conductive base membrane provided in the present application has the advantage of being reusable, saving costs for the overall filtration and separation system and reducing environmental pollution.
[0213] The above is a detailed introduction to the conductive forward osmosis membrane for algae-water separation, the preparation method, and the algae-water separation system and method thereof provided in the present application. For a person skilled in the art, according to the ideas of the embodiments of the present application, there may be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing a conductive forward osmosis membrane for algae-water separation, characterized in that: The steps include: 1) obtaining a conductive porous substrate of suitable size and performing a neutral treatment on the conductive porous substrate; 2) depositing an electrochemical polymer on the conductive porous substrate in step 1) to prepare a conductive intermediate layer and obtain a conductive base film, wherein the electrochemical polymer contains a negatively charged electrochemical material and a negatively charged dopant; 3) An interfacial polymerization reaction is performed on the conductive intermediate layer of the conductive base membrane to prepare a skin layer, thereby obtaining the conductive forward osmosis membrane for algae-water separation.
2. The conductive forward osmosis membrane method for algae-water separation according to claim 1, characterized in that: The conductive porous substrate is conductive porous carbon paper; the electrochemical polymer is a mixture of pyrrole and H2SO4; and the dopant is sodium dodecyl sulfate (SDBS).
3. The conductive forward osmosis membrane method for algae-water separation according to claim 2, characterized in that: The pyrrole concentration of the electrochemical polymer is 0.1 mol / L-0.2 mol / L.
4. The conductive forward osmosis membrane method for algae-water separation according to claim 3, characterized in that: The electrochemical polymer is obtained by the following method: a certain concentration and an appropriate amount of pyrrole solution, ethylene glycol, oxalic acid, and sodium dodecyl sulfate (SDBS) are fully dissolved in a certain amount of deionized water to obtain a first solution; a certain concentration of concentrated sulfuric acid is completely dissolved in a certain amount of deionized water to obtain a second solution, and finally the first and second solutions are mixed in a reactor for polymerization.
5. The conductive forward osmosis membrane method for algae-water separation according to claim 4, characterized in that: The electrochemical polymer is obtained by the following method: 10.35 mL of pyrrole solution, 3.0 mL of ethylene glycol, 3.0 mL of oxalic acid, and 13.40 g of sodium dodecyl sulfate (SDBS) are fully dissolved in 500 mL of deionized water to obtain a first solution; 16.1 mL of 98% concentrated sulfuric acid is completely dissolved in 500 mL of deionized water to obtain a second solution, and finally the first and second solutions are mixed in a reactor for polymerization.
6. The conductive forward osmosis membrane method for algae-water separation according to claim 5, characterized in that: When preparing the conductive intermediate layer, deposition is performed by a three-phase electrode method.
7. The conductive forward osmosis membrane method for algae-water separation as claimed in claim 6, characterized in that: 50-800 cycles of electrochemical polymer are deposited on the porous conductive substrate.
8. The conductive forward osmosis membrane method for algae-water separation as claimed in claim 7, characterized in that: The pyrrole concentration of the electrochemical polymer is 0.15 mol / L; 600 cycles of the electrochemical polymer are deposited on the porous conductive substrate.
9. The conductive forward osmosis membrane method for algae-water separation as claimed in claim 8, characterized in that: The porous conductive substrate is neutralized by: soaking the porous conductive base film in a 0.2 mol / L NaOH solution in a culture dish for 2 hours to enhance the bonding ability between the polypyrrole intermediate layer and the base film, and then soaking and rinsing with deionized water until neutralization after the soaking is completed.
10. A conductive forward osmosis membrane for algae-water separation, characterized in that: It comprises a support layer, an intermediate layer and a skin layer, wherein the support layer is a porous conductive substrate, the intermediate layer is a negatively charged conductive intermediate layer, and the conductive forward osmosis membrane for algae-water separation is prepared by the method described in any one of claims 1 to 9.
Citation Information
Cited By
Forward osmosis filtration system for removing pollutants in algal water
CN118754254A
Forward osmosis filtration system for removing contaminants from algae water
CN118754254B
Wettability switching separation membrane and preparation method thereof, and method for realizing membrane cleaning based on electric field switching wettability
CN119909551A
Conductive forward osmosis membrane
WO2025260546A1
Method for preparing electrically conductive forward osmosis membrane, and electrically conductive forward osmosis membrane thereof
WO2025260547A1