A pigment for coatings based on Pigment Red 53:1 and preparation method thereof

By coating the modified pigment red 53:1 in the acrylic resin and undergoing furan modification and diazotization treatment, the problems of poor dispersion and insufficient light resistance and stability of pigment red 53:1 are solved, and high dispersion and Stable coating applications.

CN118755298BActive Publication Date: 2024-11-15PENGLAI XINGUANG PIGMENT CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411254353.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

Pigment Red 53:1 is insoluble in water and organic solvents, has poor dispersion and poor light resistance and stability, and is prone to decomposition in an acidic or alkaline environment, resulting in a decrease in coloring power.

Method used

The modified pigment red 53:1 was coated in an acrylic resin, and the 2-naphthol modified by 2-amino-5-chloro-4-methylbenzenesulfonic acid was coupled to furan, and the aqueous barium chloride solution was added. Catalyzed to form a stable modified pigment and coated with an acrylic resin to improve dispersion and stability.

Benefits of technology

The pigment has improved its light resistance, acid and alkali resistance and dispersion resistance, enhanced hiding and tinting power, and solved the problems of poor dispersion and insufficient light resistance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a pigment for coating based on Pigment Red 53:1 and a preparation method thereof, belonging to the technical field of pigment synthesis. Modified Pigment Red 53:1 is coated in acrylic resin; the mass ratio of the modified Pigment Red 53:1 to the acrylic resin is 1:0.2-0.5; the modified Pigment Red 53:1 is diazotized with 2-amino-5-chloro-4-methylbenzenesulfonic acid, coupled with a furan-modified 2-naphthol derivative, and finally prepared by adding a barium chloride aqueous solution for color lake; the acrylic resin structure contains a sulfonic acid group, a carboxyl group and an amino group; the pigment prepared by the invention has good light resistance, acid and alkali resistance and dispersibility, and also has strong hiding power and tinting power, and has great application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pigment synthesis, and in particular is a coating pigment based on Pigment Red 53:1 and a preparation method thereof. Background Art

[0002] Pigment Red 53:1 belongs to azo pigments, with bright red color, good tinting power and hiding power. It is an important organic synthetic pigment and is widely used in coatings, plastics, inks and other fields.

[0003] However, Pigment Red 53:1 is insoluble in water and organic solvents, so it has poor dispersibility in coating applications; secondly, because it contains azo groups in its structure, it has poor light stability and is prone to photooxidation. It is easy to decompose in acidic or alkaline environments, and it is easy to change color and lose coloring power. Therefore, it is of great significance to prepare a highly dispersed and stable Pigment Red 53:1 coating pigment by modifying it. Summary of the invention

[0004] To solve the above problems, the object of the present invention is to provide a coating pigment based on Pigment Red 53:1 and a preparation method thereof.

[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A pigment for coating based on Pigment Red 53:1, wherein the modified Pigment Red 53:1 is coated in an acrylic resin; the mass ratio of the modified Pigment Red 53:1 to the acrylic resin is 1:0.2-0.5;

[0007] The modified pigment red 53:1 is prepared by diazotizing 2-amino-5-chloro-4-methylbenzenesulfonic acid, coupling with a furan-modified 2-naphthol derivative, and finally adding a barium chloride aqueous solution for color lake formation;

[0008] The acrylic resin structure contains sulfonic acid group, carboxyl group and amino group;

[0009] The furan-modified 2-naphthol derivative is prepared according to the following method:

[0010] 3-Furancarboxylic acid and 8-amino-2-naphthol are added to a polar aprotic solvent, stirred and dissolved, and then diethyl azodicarboxylate and 1-hydroxybenzotriazole are added. After reacting at 25-40° C. for 12-20 hours, the solvent is removed by vacuum distillation, and the residue is washed with petroleum ether for 2-3 times and dried to obtain a furan-modified 2-naphthol derivative.

[0011] The polar aprotic solvent is dimethyl sulfoxide or dimethylformamide.

[0012] The mass ratio of the 3-furancarboxylic acid, 8-amino-2-naphthol, polar aprotic solvent, diethyl azodicarboxylate and 1-hydroxybenzotriazole is 1:1.4-1.6:10-20:1.7-2.3:1.3-1.8.

[0013] The preparation method of the modified pigment red 53:1 comprises the following steps:

[0014] 1) In parts by weight, 1 part of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 5-6 parts of water and 0.6-0.8 parts of hydrochloric acid with a mass concentration of 30% are added to a reactor, stirred and dissolved, cooled to 5-10°C, and then 1.2-1.4 parts of a 30% aqueous sodium nitrite solution are added thereto, and diazotization reaction is carried out for 1.5-2h to obtain a diazo liquid;

[0015] 2) Add 1.2-1.5 parts of furan-modified 2-naphthol derivative to 5-8 parts of ethanol, stir to dissolve, add to the coupling reactor, add the diazo solution obtained in step 1), and carry out coupling reaction at 25-30° C. for 1-1.5 hours. After the coupling reaction is completed, adjust the pH of the system to 7.5-9 with 0.1 mol / L sodium hydroxide solution, stir to react for 20-30 minutes, and then adjust the pH of the system to 1-2 with hydrochloric acid, stir to react for 20-30 minutes to obtain a pigment suspension;

[0016] 3) Add 1-1.2 parts of 50% barium chloride aqueous solution to the pigment suspension prepared in step 2), stir for 20-30 minutes, heat to 90-95°C for reaction for 1-1.5 hours, cool to 25-30°C, filter, wash the filter cake with water for 3-5 times, and finally dry at 90-95°C for 5-8 hours to obtain modified Pigment Red 53:1.

[0017] The acrylic resin is prepared according to the following method:

[0018] In parts by weight, 1 part of acrylic acid, 0.2-0.5 parts of acrylamide and 0.3-0.8 parts of 2-acrylamide-2-methylpropanesulfonic acid are added to 1.5-2.5 parts of water, and the mixture is stirred and mixed at 50-80° C., and then 0.002-0.1 parts of ammonium persulfate are added dropwise thereto, and the reaction is continued by heat preservation for 2-3 hours. After the reaction is completed, sodium hydroxide is used to adjust the pH of the system to neutral to obtain acrylic resin.

[0019] The method for preparing the coating pigment based on Pigment Red 53:1 comprises the following steps:

[0020] In parts by weight, 1 part of modified Pigment Red 53:1 and 0.2-0.5 parts of acrylic resin are added to 3-7 parts of water, stirred and dispersed for 20-30 minutes, filtered, and the obtained filter cake is dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] The coating pigment based on Pigment Red 53:1 of the present invention is obtained by introducing conjugated structure amide and furan into Pigment Red 53:1 to obtain modified Pigment Red 53:1. The amide and furan structures can effectively absorb and disperse part of the light energy, thereby improving the light resistance of the pigment. In addition, the rigid structures of amide and furan are not prone to light-induced conformational changes, thereby further enhancing the light resistance and stability of the pigment.

[0023] The coating pigment based on Pigment Red 53:1 of the present invention comprises carboxyl groups, amino groups and sulfonic acid groups on the acrylic resin, which can form hydrogen bonds with the surface of the pigment, enhance the coating ability between the resin and the pigment, and improve the stability of the pigment in an acidic or alkaline environment; the acrylic resin forms a protective film on the surface of the pigment, protects the pigment from the influence of the external environment, and increases the stability of the pigment; it can also prevent aggregation between particles, improve the dispersibility of the pigment in the solvent, and enhance the hiding power and tinting power of the pigment.

[0024] The pigment prepared by the invention has good light resistance, acid and alkali resistance and dispersibility, and also has strong hiding power and tinting power, and has great application prospect in the field of coatings. DETAILED DESCRIPTION

[0025] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.

[0026] Example 1 Preparation of furan-modified 2-naphthol derivatives:

[0027] 0.1 kg of 3-furancarboxylic acid and 0.14 kg of 8-amino-2-naphthol were added to 1 kg of dimethyl sulfoxide, stirred and dissolved, and then 0.17 kg of diethyl azodicarboxylate and 0.13 kg of 1-hydroxybenzotriazole were added. After reacting at 25°C for 20 hours, the solvent was removed by vacuum distillation. The residue was washed twice with petroleum ether and dried to obtain a furan-modified 2-naphthol derivative. 1 H NMR (300 MHz, DMSO- d 6 , 298 K) δ 10.52 (s, 1H), 9.28(s, 1H), 8.69 (s, 1H), 7.82 (d,1H), 7.40-7.51 (m, 2H), 7.35 (m, 1H), 7.13(m, 2H), 6.93(d, 1H), 6.83 (d, 1H).

[0028] Preparation of modified pigment red 53:1:

[0029] 0.1 kg of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 0.5 kg of water and 0.06 kg of 30% hydrochloric acid were added to the reactor, stirred and dissolved, and then cooled to 5°C, and then 0.12 kg of 30% sodium nitrite aqueous solution was added thereto, and the diazotization reaction was carried out for 1.5 hours to obtain a diazo liquid;

[0030] 0.12 kg of furan-modified 2-naphthol derivative was added to 0.5 kg of ethanol, stirred and dissolved, and then added to a coupling reactor, and then a diazo solution was added thereto, and the coupling reaction was carried out at 25° C. for 1.5 hours. After the coupling reaction was completed, the pH of the system was adjusted to 7.5 with a 0.1 mol / L sodium hydroxide solution, and the reaction was stirred for 20 minutes. Then, the pH of the system was adjusted to 1 with hydrochloric acid, and the reaction was stirred for 20 minutes to obtain a pigment suspension;

[0031] To the prepared pigment suspension, 0.1 kg of 50% barium chloride aqueous solution was added, stirred for 20 min, heated to 90 ° C for reaction for 1.5 h, cooled to 25 ° C, filtered, and the filter cake was washed 3 times with water and finally dried at 90 ° C for 5 h to obtain modified pigment red 53:1.

[0032] Preparation of acrylic resin:

[0033] 0.1 kg of acrylic acid, 0.02 kg of acrylamide and 0.03 kg of 2-acrylamide-2-methylpropanesulfonic acid were added into 0.15 kg of water, and the mixture was stirred and mixed at 50° C. Then 0.0002 kg of ammonium persulfate was added dropwise thereto, and the reaction was continued for 2 hours. After the reaction was completed, sodium hydroxide was used to adjust the pH of the system to neutral to obtain acrylic resin.

[0034] Preparation of pigment for coatings based on Pigment Red 53:1:

[0035] 0.1 kg of modified Pigment Red 53:1 and 0.02 kg of acrylic resin were added into 0.3 kg of water, stirred and dispersed for 20 minutes, filtered, and the obtained filter cake was dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0036] Example 2 Preparation of furan-modified 2-naphthol derivatives:

[0037] 0.1 kg of 3-furancarboxylic acid and 0.15 kg of 8-amino-2-naphthol were added to 1.2 kg of dimethylformamide, and after stirring to dissolve, 0.18 kg of diethyl azodicarboxylate and 0.14 kg of 1-hydroxybenzotriazole were added. After reacting at 28°C for 18 hours, the solvent was removed by distillation under reduced pressure. The residue was washed three times with petroleum ether and dried to obtain a furan-modified 2-naphthol derivative.

[0038] Preparation of modified pigment red 53:1:

[0039] 0.1 kg of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 0.52 kg of water and 0.065 kg of 30% hydrochloric acid were added to the reactor, stirred and dissolved, and then cooled to 6°C, and then 0.13 kg of 30% sodium nitrite aqueous solution was added thereto, and the diazotization reaction was carried out for 1.6 hours to obtain a diazo liquid;

[0040] 0.13 kg of furan-modified 2-naphthol derivative was added to 0.55 kg of ethanol, stirred and dissolved, and then added to a coupling reactor, and then a diazo solution was added thereto, and the coupling reaction was carried out at 26°C for 1.4 hours. After the coupling reaction was completed, the pH of the system was adjusted to 7.9 with a 0.1 mol / L sodium hydroxide solution, and the reaction was stirred for 25 minutes. Then, the pH of the system was adjusted to 1.2 with hydrochloric acid, and the reaction was stirred for 24 minutes to obtain a pigment suspension;

[0041] To the prepared pigment suspension, 0.11 kg of 50% barium chloride aqueous solution was added, stirred for 23 min, heated to 91 °C for reaction for 1.4 h, cooled to 26 °C, filtered, and the filter cake was washed 4 times with water and finally dried at 91 °C for 7.5 h to obtain modified Pigment Red 53:1.

[0042] Preparation of acrylic resin:

[0043] 0.1 kg of acrylic acid, 0.025 kg of acrylamide and 0.04 kg of 2-acrylamide-2-methylpropanesulfonic acid were added to 0.18 kg of water, and the mixture was stirred and mixed at 55° C. Then 0.001 kg of ammonium persulfate was added dropwise thereto, and the reaction was continued by heat preservation for 2.2 hours. After the reaction was completed, sodium hydroxide was used to adjust the pH of the system to neutral to obtain acrylic resin.

[0044] Preparation of pigment for coatings based on Pigment Red 53:1:

[0045] 0.1 kg of modified Pigment Red 53:1 and 0.025 kg of acrylic resin were added into 0.4 kg of water, stirred and dispersed for 22 minutes, filtered, and the obtained filter cake was dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0046] Example 3 Preparation of furan-modified 2-naphthol derivatives:

[0047] 0.1 kg of 3-furancarboxylic acid and 0.15 kg of 8-amino-2-naphthol were added to 1.4 kg of dimethylformamide, and after stirring to dissolve, 0.19 kg of diethyl azodicarboxylate and 0.15 kg of 1-hydroxybenzotriazole were added. After reacting at 30° C. for 16 hours, the solvent was removed by distillation under reduced pressure. The residue was washed three times with petroleum ether and dried to obtain a furan-modified 2-naphthol derivative.

[0048] Preparation of modified pigment red 53:1:

[0049] 0.1 kg of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 0.55 kg of water and 0.07 kg of 30% hydrochloric acid were added to the reactor, stirred and dissolved, and then cooled to 8°C, and then 0.13 kg of 30% sodium nitrite aqueous solution was added thereto, and the diazotization reaction was carried out for 1.7 hours to obtain a diazo liquid;

[0050] 0.14 kg of furan-modified 2-naphthol derivative was added to 0.65 kg of ethanol, stirred and dissolved, and then added to a coupling reactor, and then a diazo solution was added thereto, and the coupling reaction was carried out at 28°C for 1.3 hours. After the coupling reaction was completed, the pH of the system was adjusted to 8 with a 0.1 mol / L sodium hydroxide solution, and the reaction was stirred for 26 minutes. Then, the pH of the system was adjusted to 1.5 with hydrochloric acid, and the reaction was stirred for 26 minutes to obtain a pigment suspension;

[0051] To the prepared pigment suspension, 0.11 kg of 50% barium chloride aqueous solution was added, stirred for 25 min, heated to 93 ° C for reaction for 1.2 h, cooled to 28 ° C, filtered, and the filter cake was washed with water 4 times and finally dried at 93 ° C for 6.5 h to obtain modified pigment red 53:1.

[0052] Preparation of acrylic resin:

[0053] 0.1 kg of acrylic acid, 0.03 kg of acrylamide and 0.05 kg of 2-acrylamide-2-methylpropanesulfonic acid were added into 0.2 kg of water, and the mixture was stirred and mixed at 65° C. Then 0.005 kg of ammonium persulfate was added dropwise thereto, and the reaction was continued by heat preservation for 2.5 hours. After the reaction was completed, sodium hydroxide was used to adjust the pH of the system to neutral to obtain acrylic resin.

[0054] Preparation of pigment for coatings based on Pigment Red 53:1:

[0055] 0.1 kg of modified Pigment Red 53:1 and 0.035 kg of acrylic resin were added into 0.55 kg of water, stirred and dispersed for 25 minutes, and then filtered. The filter cake was dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0056] Example 4 Preparation of furan-modified 2-naphthol derivatives:

[0057] 0.1 kg of 3-furancarboxylic acid and 0.16 kg of 8-amino-2-naphthol were added to 1.6 kg of dimethyl sulfoxide, stirred and dissolved, and then 0.21 kg of diethyl azodicarboxylate and 0.16 kg of 1-hydroxybenzotriazole were added. After reacting at 35° C. for 14 hours, the solvent was removed by distillation under reduced pressure. The residue was washed three times with petroleum ether and dried to obtain a furan-modified 2-naphthol derivative.

[0058] Preparation of modified pigment red 53:1:

[0059] 0.1 kg of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 0.58 kg of water and 0.075 kg of 30% hydrochloric acid were added to the reactor, stirred and dissolved, and then cooled to 9°C, and then 0.12 kg of 30% sodium nitrite aqueous solution was added thereto, and the diazotization reaction was carried out for 1.8 hours to obtain a diazo liquid;

[0060] 0.14 kg of furan-modified 2-naphthol derivative was added to 0.7 kg of ethanol, stirred and dissolved, and then added to a coupling reactor, and then a diazo solution was added thereto, and the coupling reaction was carried out at 29° C. for 1.4 hours. After the coupling reaction was completed, the pH of the system was adjusted to 8.5 with a 0.1 mol / L sodium hydroxide solution, and the reaction was stirred for 28 minutes. Then, the pH of the system was adjusted to 1.8 with hydrochloric acid, and the reaction was stirred for 28 minutes to obtain a pigment suspension;

[0061] To the prepared pigment suspension, 0.11 kg of 50% barium chloride aqueous solution was added, stirred for 28 min, heated to 94 °C for reaction for 1.1 h, cooled to 29 °C, filtered, and the filter cake was washed with water 5 times and finally dried at 94 °C for 5.5 h to obtain modified Pigment Red 53:1.

[0062] Preparation of acrylic resin:

[0063] 0.1 kg of acrylic acid, 0.04 kg of acrylamide and 0.06 kg of 2-acrylamide-2-methylpropanesulfonic acid were added into 0.22 kg of water, and the mixture was stirred and mixed at 75° C. Then 0.008 kg of ammonium persulfate was added dropwise thereto, and the reaction was continued by heat preservation for 2.8 hours. After the reaction was completed, sodium hydroxide was used to adjust the pH of the system to neutral to obtain acrylic resin.

[0064] Preparation of pigment for coatings based on Pigment Red 53:1:

[0065] 0.1 kg of modified Pigment Red 53:1 and 0.04 kg of acrylic resin were added into 0.65 kg of water, stirred and dispersed for 28 minutes, filtered, and the obtained filter cake was dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0066] Example 5 Preparation of furan-modified 2-naphthol derivatives:

[0067] 0.1 kg of 3-furancarboxylic acid and 0.16 kg of 8-amino-2-naphthol were added to 2 kg of dimethyl sulfoxide, stirred and dissolved, and then 0.23 kg of diethyl azodicarboxylate and 0.18 kg of 1-hydroxybenzotriazole were added. After reacting at 40° C. for 12 hours, the solvent was removed by vacuum distillation. The residue was washed three times with petroleum ether and dried to obtain a furan-modified 2-naphthol derivative.

[0068] Preparation of modified pigment red 53:1:

[0069] 0.1 kg of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 0.6 kg of water and 0.08 kg of 30% hydrochloric acid were added to the reactor, stirred and dissolved, cooled to 10°C, and then 0.14 kg of 30% sodium nitrite aqueous solution was added thereto, and diazotization reaction was carried out for 2 hours to obtain diazo liquid;

[0070] 0.15 kg of furan-modified 2-naphthol derivative was added to 0.8 kg of ethanol, stirred and dissolved, and then added to a coupling reactor, and then a diazo solution was added thereto, and the coupling reaction was carried out at 30° C. for 1.5 hours. After the coupling reaction was completed, the pH of the system was adjusted to 9 with a 0.1 mol / L sodium hydroxide solution, and the reaction was stirred for 30 minutes. Then, the pH of the system was adjusted to 2 with hydrochloric acid, and the reaction was stirred for 30 minutes to obtain a pigment suspension;

[0071] To the prepared pigment suspension, 0.12 kg of 50% barium chloride aqueous solution was added, stirred for 30 min, heated to 95 ° C for reaction for 1.5 h, cooled to 30 ° C, filtered, and the filter cake was washed with water 5 times, and finally dried at 95 ° C for 5 h to obtain modified pigment red 53:1.

[0072] Preparation of acrylic resin:

[0073] 0.1 kg of acrylic acid, 0.05 kg of acrylamide and 0.08 kg of 2-acrylamide-2-methylpropanesulfonic acid were added into 0.25 kg of water, and the mixture was stirred and mixed at 80° C. Then 0.01 kg of ammonium persulfate was added dropwise thereto, and the reaction was continued for 3 hours. After the reaction was completed, sodium hydroxide was used to adjust the pH of the system to neutral to obtain acrylic resin.

[0074] Preparation of pigment for coatings based on Pigment Red 53:1:

[0075] 0.1 kg of modified Pigment Red 53:1 and 0.05 kg of acrylic resin were added into 0.7 kg of water, stirred and dispersed for 30 minutes, and then filtered. The filter cake was dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0076] Example 6 Preparation of furan-modified 2-naphthol derivatives:

[0077] 0.1 kg of 3-furancarboxylic acid and 0.14 kg of 8-amino-2-naphthol were added to 1.5 kg of dimethylformamide, and after stirring to dissolve, 0.23 kg of diethyl azodicarboxylate and 0.13 kg of 1-hydroxybenzotriazole were added. After reacting at 40° C. for 20 hours, the solvent was removed by distillation under reduced pressure. The residue was washed three times with petroleum ether and dried to obtain a furan-modified 2-naphthol derivative.

[0078] Preparation of modified pigment red 53:1:

[0079] 0.1 kg of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 0.5 kg of water and 0.08 kg of 30% hydrochloric acid were added to the reactor, stirred and dissolved, and then cooled to 5°C, and then 0.14 kg of 30% sodium nitrite aqueous solution was added thereto, and diazotization reaction was carried out for 1.5 hours to obtain diazo liquid;

[0080] 0.15 kg of furan-modified 2-naphthol derivative was added to 0.5 kg of ethanol, stirred and dissolved, and then added to a coupling reactor, and then a diazo solution was added thereto, and the coupling reaction was carried out at 30° C. for 1 hour. After the coupling reaction was completed, the pH of the system was adjusted to 8.5 with a 0.1 mol / L sodium hydroxide solution, and the reaction was stirred for 25 minutes. Then, the pH of the system was adjusted to 2 with hydrochloric acid, and the reaction was stirred for 25 minutes to obtain a pigment suspension;

[0081] To the prepared pigment suspension, 0.1 kg of 50% barium chloride aqueous solution was added, stirred for 30 min, heated to 90 ° C for reaction for 1 h, cooled to 30 ° C, filtered, and the filter cake was washed with water 3 times and finally dried at 95 ° C for 8 h to obtain modified pigment red 53:1.

[0082] Preparation of acrylic resin:

[0083] 0.1 kg of acrylic acid, 0.02 kg of acrylamide and 0.08 kg of 2-acrylamide-2-methylpropanesulfonic acid were added into 0.25 kg of water, and the mixture was stirred and mixed at 80° C. Then 0.009 kg of ammonium persulfate was added dropwise thereto, and the reaction was continued for 3 hours. After the reaction was completed, sodium hydroxide was used to adjust the pH of the system to neutral to obtain acrylic resin.

[0084] Preparation of pigment for coatings based on Pigment Red 53:1:

[0085] 0.1 kg of modified Pigment Red 53:1 and 0.02 kg of acrylic resin were added into 0.7 kg of water, stirred and dispersed for 20 minutes, filtered, and the obtained filter cake was dried and crushed to obtain a coating pigment based on Pigment Red 53:1.

[0086] The pigments for coatings based on Pigment Red 53:1 prepared in Examples 1 to 6 were tested respectively, wherein the bulk density was tested according to the method in GB / T 21877-2015, 50 g of the pigment was accurately weighed, put into a measuring cylinder, sealed, and oscillated up and down 10 times, and the sample scale in the measuring cylinder was recorded; the oil absorption was tested according to GB1712-79, the light resistance was tested according to the standard GB1710-79, and the water resistance, acid resistance and alkali resistance were tested according to GB 5211.5-2008-T. The comparative example used our company's product Jinguanghong C (PR53:1), and the test results are shown in Table 1.

[0087] Table 1 Performance test results of the pigments prepared in Examples 1 to 6 and the comparative examples

[0088]

[0089] It can be seen from the results in Table 1 that the coating pigment based on Pigment Red 53:1 prepared by the present invention has higher light resistance and acid and alkali resistance than the comparative example, and has a small bulk density and is easy to disperse, and has great application prospects in the field of coatings.

[0090] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A coating pigment based on Pigment Red 53:1, characterized in that: The modified pigment red 53:1 is coated in acrylic resin; the mass ratio of the modified pigment red 53:1 to the acrylic resin is 1:0.2-0.5; The modified pigment red 53:1 is prepared by diazotizing 2-amino-5-chloro-4-methylbenzenesulfonic acid, coupling with a furan-modified 2-naphthol derivative, and finally adding a barium chloride aqueous solution for color lake formation; The acrylic resin structure contains sulfonic acid group, carboxyl group and amino group; The furan-modified 2-naphthol derivative is prepared according to the following method: 3-Furancarboxylic acid and 8-amino-2-naphthol are added to a polar aprotic solvent, stirred and dissolved, and then diethyl azodicarboxylate and 1-hydroxybenzotriazole are added. After reacting at 25-40° C. for 12-20 hours, the solvent is removed by vacuum distillation, and the residue is washed with petroleum ether for 2-3 times and dried to obtain a furan-modified 2-naphthol derivative.

2. The coating pigment based on Pigment Red 53:1 as claimed in claim 1, characterized in that: The polar aprotic solvent is dimethyl sulfoxide or dimethylformamide.

3. The coating pigment based on Pigment Red 53:1 as claimed in claim 1, characterized in that: The mass ratio of the 3-furancarboxylic acid, 8-amino-2-naphthol, polar aprotic solvent, diethyl azodicarboxylate and 1-hydroxybenzotriazole is 1:1.4-1.6:10-20:1.7-2.3:1.3-1.

8.

4. The coating pigment based on Pigment Red 53:1 as claimed in claim 1, characterized in that: The preparation method of the modified pigment red 53:1 comprises the following steps: 1) In parts by weight, 1 part of 2-amino-5-chloro-4-methylbenzenesulfonic acid, 5-6 parts of water and 0.6-0.8 parts of hydrochloric acid with a mass concentration of 30% are added to a reactor, stirred and dissolved, cooled to 5-10°C, and then 1.2-1.4 parts of a 30% aqueous sodium nitrite solution are added thereto, and diazotization reaction is carried out for 1.5-2h to obtain a diazo liquid; 2) Add 1.2-1.5 parts of furan-modified 2-naphthol derivative to 5-8 parts of ethanol, stir to dissolve, add to the coupling reactor, add the diazo solution obtained in step 1), and carry out coupling reaction at 25-30° C. for 1-1.5 hours. After the coupling reaction is completed, adjust the pH of the system to 7.5-9 with 0.1 mol / L sodium hydroxide solution, stir to react for 20-30 minutes, and then adjust the pH of the system to 1-2 with hydrochloric acid, stir to react for 20-30 minutes to obtain a pigment suspension; 3) Add 1-1.2 parts of 50% barium chloride aqueous solution to the pigment suspension prepared in step 2), stir for 20-30 minutes, heat to 90-95°C for reaction for 1-1.5 hours, cool to 25-30°C, filter, wash the filter cake with water for 3-5 times, and finally dry at 90-95°C for 5-8 hours to obtain modified Pigment Red 53:

1.

5. The coating pigment based on Pigment Red 53:1 as claimed in claim 1, characterized in that: The acrylic resin is prepared according to the following method: In parts by weight, 1 part of acrylic acid, 0.2-0.5 parts of acrylamide and 0.3-0.8 parts of 2-acrylamide-2-methylpropanesulfonic acid are added to 1.5-2.5 parts of water, and the mixture is stirred and mixed at 50-80° C., and then 0.002-0.1 parts of ammonium persulfate are added dropwise thereto, and the reaction is continued by heat preservation for 2-3 hours. After the reaction is completed, sodium hydroxide is used to adjust the pH of the system to neutral to obtain acrylic resin.

6. A method for preparing a coating pigment based on Pigment Red 53:1 according to claim 1, characterized in that: The following steps are involved: In parts by weight, 1 part of modified Pigment Red 53:1 and 0.2-0.5 parts of acrylic resin are added to 3-7 parts of water, stirred and dispersed for 20-30 minutes, filtered, and the obtained filter cake is dried and crushed to obtain a coating pigment based on Pigment Red 53:1.