Sulfide solid electrolyte precursor, sulfide solid electrolyte preparation method and battery

By forming a silica coating layer outside the sulfide electrolyte and doping silica, the problems of hydrolysis and interface side reactions of the sulfide solid electrolyte in humid air are solved, and the cycle stability of the battery is improved.

CN118763271APending Publication Date: 2024-10-11HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202410955672.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Sulfide solid electrolytes are easily hydrolyzed in humid air, resulting in a decrease in ionic conductivity, and interfacial side reactions occur when in contact with lithium metal, affecting battery performance.

Method used

By forming a silica coating layer outside the sulfide electrolyte and doping silica in the electrolyte bulk phase, the air stability of the electrolyte and the stability of the lithium metal interface are improved. It is prepared by siloxane coating and sintering methods. Sulfide solid electrolyte.

Benefits of technology

Significantly improve the air stability of the sulfide solid electrolyte and the stability of the lithium metal interface, achieving high cycle stability of all-solid-state lithium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763271A_ABST
    Figure CN118763271A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfide solid electrolyte precursor, a sulfide solid electrolyte preparation method and a battery, and relates to the technical field of batteries, and the preparation method comprises the following steps: preparing electrolyte raw materials according to a stoichiometric ratio in a chemical formula of the sulfide solid electrolyte, adding a first solvent, and carrying out ball milling to form the electrolyte precursor; placing the electrolyte precursor in a second solvent containing siloxane, heating and stirring to coat the electrolyte precursor with siloxane, and forming an electrolyte precursor with siloxane; and sintering the electrolyte precursor with siloxane to obtain the doped and coated sulfide electrolyte. According to the invention, the coating layer is formed outside the sulfide electrolyte, so that the air stability of the sulfide solid electrolyte is greatly improved, and the stability of the sulfide electrolyte to a lithium metal interface is improved, so that the high cycle stability of the all-solid-state lithium metal battery is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of batteries, and in particular to a sulfide solid electrolyte precursor, a method for preparing a sulfide solid electrolyte, and a battery. Background Art

[0002] Lithium batteries are energy storage devices that are mainly used in mobile devices, electric vehicles, and household appliances. In modern society, lithium batteries have been widely used and have become an essential component of many devices and products.

[0003] In some related technologies, research has found that using solid electrolytes to replace the original liquid electrolytes in lithium-ion batteries can greatly solve the safety problems of batteries, and solid electrolytes have a wide electrochemical window, which is conducive to the uniform deposition of lithium. Among them, sulfide solid electrolytes are considered to be solid electrolyte materials with broad application prospects due to their excellent mechanical properties and high ionic conductivity, and their ionic conductivity can reach a level comparable to that of liquid electrolytes.

[0004] However, there are still some problems in the actual use of sulfide electrolytes. For example, sulfide solid electrolytes are very easy to hydrolyze in humid air, which will lead to a decrease in the ionic conductivity of the electrolyte, greatly limiting the application and production of sulfide solid electrolytes; and when the sulfide solid electrolyte comes into contact with lithium metal, serious interfacial side reactions will occur, causing the battery interface impedance to increase, affecting the performance of the all-solid-state battery. Summary of the invention

[0005] In order to solve at least one of the problems mentioned in the above background technology, the present application provides a sulfide solid electrolyte precursor, a sulfide solid electrolyte preparation method and a battery. By forming a coating layer on the outside of the sulfide electrolyte, the air stability of the sulfide solid electrolyte is greatly improved, and the stability of the sulfide electrolyte to the lithium metal interface is improved, so as to achieve high cycle stability of an all-solid-state lithium metal battery.

[0006] The specific technical solutions provided by the embodiments of this application are as follows:

[0007] In a first aspect, a sulfide solid electrolyte precursor is provided, wherein the sulfide solid electrolyte precursor has a chemical formula of Li 6-m PS 5-m X 1+m ; Wherein, 0<m<2.5; Wherein, the element X includes one or more of fluorine, chlorine, bromine and iodine.

[0008] The sulfide solid electrolyte precursor formed according to the ratio of elements in the above chemical formula has a surface structure that is more suitable for subsequent surface coating due to the interaction between the sulfide solid electrolyte precursor particles and other particles, and can ensure that siloxane is subsequently doped into the electrolyte phase, so that the doped and coated sulfide solid electrolyte has higher stability.

[0009] In a specific embodiment, in the chemical formula of the sulfide solid electrolyte precursor, 0<m<1; further, 0.2≤m≤0.7.

[0010] By controlling the ratio between the various elements in the sulfide solid electrolyte precursor within a reasonable range, sufficient reaction between the particles in the solid is ensured, which is beneficial for doping and coating.

[0011] In a second aspect, a method for preparing a sulfide solid electrolyte using the sulfide solid electrolyte precursor as described above is provided, the method comprising: configuring electrolyte raw materials according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, adding a first solvent and ball milling to form a new electrolyte precursor; placing the new electrolyte precursor in a second solvent containing siloxane, heating and stirring to coat the new electrolyte precursor with siloxane to form an electrolyte precursor having siloxane; and sintering the electrolyte precursor having siloxane to obtain a doped and coated sulfide electrolyte.

[0012] Through the above scheme, the electrolyte raw materials are configured according to the stoichiometric ratio of the chemical formula in the precursor, and then the first solvent is added for dispersion and ball milling to prepare a dispersed new precursor solution. The new precursor solution is placed in a second solvent containing siloxane, heated and stirred to coat the siloxane on the new electrolyte precursor, and then sintered to decompose the siloxane to form a silica coating layer, which is coated on the surface of the new electrolyte precursor, and at the same time, silica is doped in the electrolyte phase. At the same time, the thickness of the coating layer is controlled by controlling the concentration of the siloxane solution in this process, thereby obtaining a silica-coated and doped sulfide electrolyte, wherein the silica coating on the electrolyte surface greatly improves the air stability of the electrolyte and improves the stability of the electrolyte to the lithium metal interface, and the silica generated by decomposition is doped in the electrolyte to further improve the intrinsic air stability of the prepared electrolyte, thereby achieving high cycle stability of all-solid-state lithium metal batteries.

[0013] In a specific embodiment, the method further includes: configuring the electrolyte raw materials according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, adding a first solvent, and ball milling to form a precursor solution; heating and drying the precursor solution to obtain the new electrolyte precursor.

[0014] By dispersing the electrolyte precursor in the first solvent to form a precursor solution, it can be ensured that the electrolyte precursor is evenly dispersed. By heating and drying, on the one hand, impurities on the surface of the new electrolyte precursor particles can be removed, and on the other hand, the new electrolyte precursor that is aggregated in clusters can be evenly dispersed to obtain dispersed particles of the new electrolyte precursor.

[0015] In a specific embodiment, the first solvent is an alkane solvent; further, the first solvent includes one or more of n-heptane, hexane or octane;

[0016] The ball milling speed is 200 rpm to 800 rpm; further, the ball milling speed is 400 rpm to 600 rpm;

[0017] The ball milling time is 10h to 60h; further, the ball milling time is 20h to 48h;

[0018] The drying temperature of the precursor solution is 60°C to 140°C; further, the drying temperature of the precursor solution is 80°C to 120°C;

[0019] The drying time of the precursor solution is 8 hours to 50 hours; further, the drying time of the precursor solution is 10 hours to 40 hours.

[0020] By controlling the type of the first solvent, as well as the rotation speed and time parameters during the ball milling process, it is ensured that the solid electrolyte precursor can be dispersed to form a uniform precursor solution, which is beneficial for the subsequent coating of siloxane on the surface of the new electrolyte precursor.

[0021] In a specific embodiment, the chemical formula of the siloxane is Si n O n-1 H 2n+2 or (H2SiO) n , wherein n is an integer greater than or equal to 2; the mass concentration of siloxane in the second solvent is 1% to 9%; further, the mass concentration of siloxane in the second solvent is 2% to 6%;

[0022] The second solvent is an aromatic hydrocarbon solvent; further, the second solvent includes one or more of benzene, toluene or chlorobenzene.

[0023] By controlling the type and mass concentration of the siloxane contained in the second solvent, the thickness of the coating layer formed on the sulfide solid electrolyte can be controlled. By controlling the thickness of the coating layer on the surface of the sulfide solid electrolyte within a reasonable range, it is ensured that the finally prepared sulfide solid electrolyte has both good interface stability and good ionic conductivity.

[0024] In a specific embodiment, the method further comprises: coating the new electrolyte precursor with siloxane and drying the new electrolyte precursor to form an electrolyte precursor having siloxane;

[0025] The drying temperature is 60°C to 140°C; further, the drying temperature is 70°C to 130°C; the drying time is 10h to 50h; further, the drying time is 12h to 48h.

[0026] The electrolyte precursor with siloxane and stable surface properties is obtained by coating the new electrolyte precursor with siloxane and then drying it while controlling the temperature and time in the drying process within a reasonable range.

[0027] In a specific embodiment, the method further comprises: placing the electrolyte precursor having siloxane in a tubular furnace with an inert gas atmosphere for sintering to form a silicon dioxide coating layer on the surface of the electrolyte, and doping silicon dioxide in the electrolyte bulk phase to form the doped and coated sulfide electrolyte;

[0028] Wherein, the thickness of the silicon dioxide coating layer is 1nm to 500nm; further, the thickness of the silicon dioxide coating layer is 10nm to 50nm;

[0029] The inert gas includes one or more of nitrogen, helium, neon, argon, krypton, xenon or radon.

[0030] By sintering an electrolyte precursor containing siloxane in a tubular furnace in an inert atmosphere, siloxane undergoes a thermal decomposition reaction to form a silicon dioxide coating layer on the surface of the electrolyte, and at the same time, part of the silicon dioxide is doped into the bulk phase of the electrolyte, thereby forming a doped and coated sulfide electrolyte. By controlling the thickness of the silicon dioxide coating layer within a reasonable range, it is ensured that the finally prepared sulfide solid electrolyte has both good interface stability and good ionic conductivity.

[0031] In a specific embodiment, the sintering temperature is 300°C to 800°C; further, the sintering temperature is 400°C to 600°C.

[0032] The temperature during the sintering process is controlled to ensure that siloxane undergoes a smooth thermal decomposition reaction on the surface of the electrolyte precursor to form a silicon dioxide coating layer.

[0033] In a third aspect, a battery is provided, comprising a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is prepared by the method as described above.

[0034] The embodiments of the present application have the following beneficial effects:

[0035] 1. The embodiments of the present application provide a method for improving the air stability of the sulfide solid electrolyte and improving the stability of the sulfide electrolyte to the lithium metal interface by forming a silicon dioxide coating layer on the outside of the sulfide electrolyte and doping silicon dioxide in the bulk phase of the electrolyte, so as to achieve high cycle stability of the all-solid-state lithium metal battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0037] Figure 1 A schematic diagram of a method for preparing a sulfide solid electrolyte according to the present application is shown;

[0038] Figure 2 The SEM image of the sulfide solid electrolyte prepared in Example 1 of the present application is shown;

[0039] Figure 3 The TEM image of the sulfide solid electrolyte prepared in Example 1 of the present application is shown. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0042] This embodiment provides a sulfide solid electrolyte precursor, the sulfide solid electrolyte chemical formula is Li 6-m PS 5-m X 1+m ; Wherein, 0<m<2.5; Wherein, the element X includes but is not limited to one or more of fluorine, chlorine, bromine and iodine.

[0043] For example, when the element X is selected as chlorine and bromine, and the electrolyte raw materials are selected as Li2S, P2S5, LiCl and LiBr, when m is configured to be 2.4, the chemical formula of the sulfide solid electrolyte is Li 3.7 PS 2.6 X 3.4 The configuration ratio of electrolyte raw materials Li2S, P2S5, LiCl and LiBr is Li2S:P2S5:LiCl:LiBr is 0.3:0.98:3:3.8.

[0044] For example, when the element X is selected as chlorine and bromine, and the electrolyte raw materials are selected as Li2S, P2S5, LiCl and LiBr, when m is configured to be 0.1, the chemical formula of the sulfide solid electrolyte is Li 5.9 PS 4.9 X 1.1 The configuration ratio of electrolyte raw materials Li2S, P2S5, LiCl and LiBr is Li2S:P2S5:LiCl:LiBr is 4.8:1:1:1.2.

[0045] In a specific embodiment, in the chemical formula of the sulfide solid electrolyte precursor, 0<m<1; further, 0.2≤m≤0.7.

[0046] For example, when the element X is selected as chlorine and bromine, and the electrolyte raw materials selected are Li2S, P2S5, LiCl and LiBr, when m is configured to be 0.5, the chemical formula of the sulfide solid electrolyte is Li 5.5 PS 4.5 X 1.5 , that is, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr are configured in a ratio of Li2S:P2S5:LiCl:LiBr of 4:1:1.6:1.4.

[0047] When m is configured to 0.7, the chemical formula of the sulfide solid electrolyte is Li 5.3 PS 4.3 X 1.7 At this time, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr are configured in a ratio of Li2S:P2S5:LiCl:LiBr of 3.6:1:1.6:1.8.

[0048] When m is set to 0.2, the chemical formula of the sulfide solid electrolyte is Li 5.8 PS 4.8 X 1.2At this time, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr are configured in a ratio of Li2S:P2S5:LiCl:LiBr of 4.6:1:1.2:1.2.

[0049] Through research, it was found that the sulfide solid electrolyte precursor formed according to the ratio of elements in the above chemical formula has a surface structure that is more suitable for subsequent surface coating due to the interaction between the sulfide solid electrolyte precursor particles and other particles, and can ensure the subsequent doping of siloxane into the electrolyte phase, so that the doped and coated sulfide solid electrolyte has higher stability.

[0050] In one embodiment, a method for preparing a sulfide solid electrolyte using the sulfide solid electrolyte precursor as described above is provided, the method comprising:

[0051] Step 1: preparing electrolyte raw materials according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, adding a first solvent and performing ball milling to form a new electrolyte precursor;

[0052] Specifically, the electrolyte raw materials are configured according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, and a first solvent is added to perform ball milling to form a precursor solution; and the precursor solution is heated and dried to obtain the new electrolyte precursor.

[0053] The electrolyte raw materials include but are not limited to one or more of Li2S, P2S5, LiCl, LiBr, LiF or LiI.

[0054] The first solvent is an alkane solvent, and the specific first solvent includes but is not limited to one or more of ethane, propane, butane, pentane, 2-methylbutane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane, 2,3-dimethylbutane, n-heptane, heptane isomers, octane, 2,2,4-trimethylpentane, 2,3,4-trimethylpentane, 2,2,3-trimethylpentane, nonane, 2,2,5-trimethylhexane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, heptadecane, and octadecane.

[0055] For example, when the element X is selected as chlorine and bromine, and the electrolyte raw materials selected are Li2S, P2S5, LiCl and LiBr, when m is configured to be 0.5, the chemical formula of the sulfide solid electrolyte is Li 5.5 PS 4.5 X 1.5 , that is, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr are configured in a ratio of Li2S:P2S5:LiCl:LiBr of 4:1:1.6:1.4.

[0056] When m is configured to 0.7, the chemical formula of the sulfide solid electrolyte is Li 5.3 PS 4.3 X 1.7 At this time, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr are configured in a ratio of Li2S:P2S5:LiCl:LiBr of 3.6:1:1.6:1.8.

[0057] When m is set to 0.2, the chemical formula of the sulfide solid electrolyte is Li 5.8 PS 4.8 X 1.2 At this time, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr are configured in a ratio of Li2S:P2S5:LiCl:LiBr of 4.6:1:1.2:1.2.

[0058] Furthermore, after the electrolyte raw materials are configured according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, they are dispersed by ball milling, and the ball milling speed is specifically set to 200rpm~800rpm; specifically, the ball milling speed is 400rpm~600rpm; the ball milling time is 10h~60h; specifically, the ball milling time is 20h~48h.

[0059] In order to ensure that the solid electrolyte precursor can be dispersed to form a uniform precursor solution, the drying temperature of the precursor solution is set to 60°C ~ 140°C; specifically, the drying temperature of the precursor solution is 80°C ~ 120°C; the drying time of the precursor solution is 8h ~ 50h; specifically, the drying time of the precursor solution is 10h ~ 40h.

[0060] Step 2: placing the new electrolyte precursor in a second solvent containing siloxane, heating and stirring, so that the siloxane is coated on the new electrolyte precursor to form an electrolyte precursor containing siloxane.

[0061] The siloxane includes chain siloxane and cyclic siloxane, and the chemical formula of the chain siloxane is Si n O n-1 H 2n+2 , the cyclic siloxane chemical formula is (H2SiO) n , wherein n is an integer greater than or equal to 2; specifically, the siloxane includes but is not limited to one or more of disiloxane, trisiloxane, cyclotetrasiloxane or organosiloxane.

[0062] The type and mass concentration of siloxane contained in the second solvent are controlled to achieve control of the thickness of the coating layer formed on the sulfide solid electrolyte. Specifically, the mass concentration of siloxane in the second solvent is 1% to 9%; specifically, the mass concentration of siloxane in the second solvent is 2% to 6%.

[0063] The second solvent is an aromatic hydrocarbon solvent. Specifically, the second solvent includes one or more of benzene, toluene, naphthalene, styrene, dimethylacetamide, dimethylformamide, ethylbenzene, isopropylbenzene, or chlorobenzene.

[0064] In a specific embodiment, the process includes coating siloxane on a new electrolyte precursor and drying the resulting electrolyte precursor to form an electrolyte precursor having siloxane; wherein the drying temperature is 60°C to 140°C; specifically, the drying temperature is 70°C to 130°C; the drying time is 10h to 50h; specifically, the drying time is 12h to 48h.

[0065] Step 3: sintering the electrolyte precursor containing siloxane to obtain a doped and coated sulfide electrolyte.

[0066] Specifically, the electrolyte precursor containing siloxane is placed in a tubular furnace with an inert gas atmosphere for sintering, a silicon dioxide coating layer is formed on the electrolyte surface, and silicon dioxide is doped in the electrolyte bulk phase to form the sulfide solid electrolyte.

[0067] Wherein, the thickness of the silicon dioxide coating layer is controlled to be 1nm to 500nm; specifically, the thickness of the silicon dioxide coating layer is 10nm to 50nm; wherein, the inert gas includes one or more of nitrogen, helium, neon, argon, krypton, xenon or radon.

[0068] In this embodiment, the sintering temperature is 300°C to 800°C; specifically, the sintering temperature is 400°C to 600°C.

[0069] Through the above scheme, the electrolyte raw materials are configured according to the stoichiometric ratio of the chemical formula in the precursor, and then the first solvent is added for dispersion and ball milling to prepare a dispersed new precursor solution. The new precursor solution is placed in a second solvent containing siloxane, heated and stirred to coat the siloxane on the new electrolyte precursor, and then sintered to decompose the siloxane to form a silica coating layer, which is coated on the surface of the new electrolyte precursor, and at the same time, silica is doped in the electrolyte phase. At the same time, the thickness of the coating layer is controlled by controlling the concentration of the siloxane solution in this process, thereby obtaining a silica-coated and doped sulfide electrolyte, wherein the silica coating on the electrolyte surface greatly improves the air stability of the electrolyte and improves the stability of the electrolyte to the lithium metal interface, and the silica generated by decomposition is doped in the electrolyte to further improve the intrinsic air stability of the prepared electrolyte, thereby achieving high cycle stability of all-solid-state lithium metal batteries.

[0070] Embodiment 1

[0071] When m is set to 0.5, the chemical formula of the sulfide solid electrolyte is Li 5.5 PS 4.5 X 1.5 , namely, the electrolyte raw materials Li2S, P2S5, LiCl and LiBr, with a configuration ratio of 4:1:1.6:1.4; weigh the electrolyte raw materials Li2S:P2S5:LiCl:LiBr according to the stoichiometric ratio of 4:1:1.6:1.4, put them into a ball mill, add the organic solvent n-heptane and seal it, ball mill for 24 hours at a speed of 500rpm to obtain a uniformly mixed precursor solution, and dry the precursor solution at 100°C for 12 hours to obtain an electrolyte precursor. Add the electrolyte precursor to a xylene solution with a siloxane concentration of 2%, stir it at 80°C for 12 hours, obtain an electrolyte precursor solution uniformly coated with siloxane, heat it to 100°C and dry it for 24 hours to obtain a dry siloxane-coated electrolyte precursor, and sinter the siloxane-coated electrolyte precursor at 450°C for 12 hours under an argon atmosphere to obtain a silica-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 Sulfide solid electrolyte. The prepared silicon dioxide-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 The sulfide solid electrolyte was tested by SEM and coating thickness, and the test results were as follows: Figure 1 and Figure 2 shown.

[0072] pass Figure 1The SEM image in FIG. 1 shows that the solution in this embodiment can obtain SiO2-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 Sulfide solid electrolyte; Figure 2 As can be seen from the TEM image in the example, the SiO2-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 The thickness of the silicon dioxide coating on the sulfide solid electrolyte meets the requirements.

[0073] Embodiment 2

[0074] The difference from Example 1 is that the concentration of siloxane in the xylene solution is controlled to be 3%, and the other conditions are the same as those in Example 1. The specific preparation process is as follows:

[0075] The electrolyte raw materials Li2S:P2S5:LiCl:LiBr were weighed according to the stoichiometric ratio of 4:1:1.6:1.4, put into a ball mill, added with organic solvent n-heptane and sealed, and ball milled at a speed of 500rpm for 24h to obtain a uniformly mixed precursor solution, and the precursor solution was dried at 100°C for 12h to obtain an electrolyte precursor. The electrolyte precursor was added to a xylene solution with a siloxane concentration of 3%, stirred at 80°C for 12h, and a siloxane-uniformly coated electrolyte precursor solution was obtained, which was heated to 100°C and dried for 24h to obtain a dry siloxane-coated electrolyte precursor, and the siloxane-coated electrolyte precursor was sintered at 450°C for 12h under an argon atmosphere to obtain a silica-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 Sulfide solid electrolyte.

[0076] Embodiment 3

[0077] The difference from Example 1 is that the concentration of siloxane in the xylene solution is controlled to be 4%, and the other conditions are the same as those in Example 1. The specific preparation process is as follows:

[0078] The electrolyte raw materials Li2S:P2S5:LiCl:LiBr were weighed according to the stoichiometric ratio of 4:1:1.6:1.4, put into a ball mill, added with organic solvent n-heptane and sealed, and ball milled at a speed of 500rpm for 24 hours to obtain a uniformly mixed precursor solution, and the precursor solution was dried at 100°C for 12 hours to obtain an electrolyte precursor. The electrolyte precursor was added to a xylene solution with a siloxane concentration of 4%, stirred at 80°C for 12 hours to obtain an electrolyte precursor solution uniformly coated with siloxane, heated to 100°C and dried for 24 hours to obtain a dry siloxane-coated electrolyte precursor, and the siloxane-coated electrolyte precursor was sintered at 450°C for 12 hours under an argon atmosphere to obtain a silica-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 Sulfide solid electrolyte.

[0079] Comparative Example 1

[0080] Corresponding to the above-mentioned embodiment, the difference between comparative example 1 and implementation example 1 is that the concentration of siloxane in the xylene solution is controlled to be 0, and the other conditions are the same as those in implementation example 1. The specific preparation process is as follows:

[0081] The electrolyte raw materials Li2S:P2S5:LiCl:LiBr were weighed according to the stoichiometric ratio of 4:1:1.6:1.4, put into a ball mill, added with organic solvent n-heptane and sealed, and ball milled at a speed of 500rpm for 24h to obtain a uniformly mixed precursor solution, and the precursor solution was dried at 100℃ for 12h to obtain an electrolyte precursor. The electrolyte precursor was added to a pure xylene solution, stirred at 80℃ for 12h, heated to 100℃ and dried for 24h to obtain an electrolyte precursor without any coating, and the electrolyte precursor was sintered at 450℃ for 12h under an argon atmosphere to obtain Li 5.5 PS 4.5 Cl 0.8 Br 0.7 Sulfide solid electrolyte.

[0082] Comparative Example 2

[0083] The difference from Example 1 is that no sintering is performed, and other conditions are the same as those in Example 1. The specific preparation process is as follows:

[0084] The electrolyte raw materials Li2S:P2S5:LiCl:LiBr were weighed according to the stoichiometric ratio of 4:1:1.6:1.4, put into a ball mill, added with organic solvent n-heptane and sealed, ball milled at 500rpm for 24h to obtain a uniformly mixed precursor solution, and the precursor solution was dried at 100℃ for 12h to obtain an electrolyte precursor. The electrolyte precursor was added to a xylene solution with a siloxane concentration of 2%, stirred at 80℃ for 12h, and an electrolyte precursor solution uniformly coated with siloxane was obtained, which was heated to 100℃ and dried for 24h to obtain a dry siloxane-coated sulfide solid electrolyte.

[0085] Comparative Example 3

[0086] The difference from Example 1 is that the concentration of siloxane in the xylene solution is 10%, and the other conditions are the same as those in Example 1. The specific preparation process is as follows:

[0087] The electrolyte raw materials Li2S:P2S5:LiCl:LiBr were weighed according to the stoichiometric ratio of 4:1:1.6:1.4, put into a ball mill, added with organic solvent n-heptane and sealed, and ball milled at a speed of 500rpm for 24h to obtain a uniformly mixed precursor solution, and the precursor solution was dried at 100°C for 12h to obtain an electrolyte precursor. The electrolyte precursor was added to a xylene solution with a siloxane concentration of 10%, stirred at 80°C for 12h, and a siloxane-uniformly coated electrolyte precursor solution was obtained, which was heated to 100°C and dried for 24h to obtain a dry siloxane-coated electrolyte precursor, and the siloxane-coated electrolyte precursor was sintered at 450°C for 12h under an argon atmosphere to obtain a silica-coated and doped Li 5.5 PS 4.5 Cl 0.8 Br 0.7 Sulfide solid electrolyte.

[0088] The EIS impedance was measured for a blocked battery with carbon-coated aluminum foil on both sides of the electrolytes obtained in the above embodiments and comparative examples. The test method was as follows: the assembled blocked battery was placed in a constant temperature box at 25°C for 1 hour to make the temperature of the electrolyte inside the battery reach 25°C. The battery was connected to a Su Liqiang electrochemical workstation to measure the constant voltage AC impedance at a frequency range of 1 MHz to 1 Hz. The ionic conductivity of the prepared electrolyte was obtained after conversion. The results are shown in Table 1.

[0089] Among them, the assembly process of the all-solid-state lithium metal battery is as follows: the high-nickel ternary NCM811, the sulfide electrolyte prepared above, the conductive agent VGCF and the adhesive SBS are weighed in a certain mass ratio and added to isobutyl isobutyrate, and then placed in a slurry machine and set to mix at a speed. After the slurry is mixed, the slurry is scraped to obtain a positive electrode sheet, and then punched to obtain a positive electrode sheet with a diameter of 10 mm. Weigh 150 mg of the above-prepared electrolyte powder and put it into a PEEK mold with a diameter of 10 mm, and press it at a pressure of 100 MPa for 1 min through a tablet press; then put the prepared 10 mm positive electrode sheet on one side, and press it again at a pressure of 500 MPa for 10 minutes through a tablet press; finally, place the metal lithium negative electrode on the other side of the obtained thin sheet, and press it at a pressure of 20 MPa for 1 minute to make an all-solid-state lithium metal battery. The cycle stability of the all-solid-state lithium metal battery was verified by constant current charge and discharge cycle test.

[0090] The test conditions are as follows: 300 mg of the prepared electrolyte powder is placed in a 10L drying dish with controlled humidity at 20%. After being placed for 24 hours, its ionic conductivity is measured, and the ionic conductivity retention rate of the electrolyte after exposure to air is calculated. The results are shown in Table 1.

[0091] Table 1 Comparison results of the first cycle lithium insertion and extraction specific capacity and first efficiency of half-cell in the examples and comparative examples

[0092]

[0093] It can be seen from the data in Table 1 that when the concentration of siloxane is 2% siloxane during the coating process, the thickness of the silicon dioxide coating layer is only about 10nm, which has basically no effect on the ionic conductivity of the electrolyte, and can significantly improve the air stability and lithium stability of the electrolyte, and improve the cycle stability of the all-solid-state lithium metal battery; By comparing Example 1 and Comparative Example 2, it can be found that after siloxane is decomposed at high temperature to generate silicon dioxide, the lithium stability of the electrolyte can be improved, thereby improving the cycle stability of the whole battery. By comparing Examples 1, 2, 3 and Comparative Example 3, it can be found that with the increase of siloxane concentration, the electrolyte has better air stability and higher ionic conductivity retention rate after exposure to air, but a large amount of siloxane coating will significantly reduce the ionic conductivity of the electrolyte itself. An appropriate amount of silicon dioxide coating will not only not reduce the ionic conductivity of the electrolyte, but can improve the air stability and lithium stability of the electrolyte, thereby reducing production costs and improving the cycle stability of all-solid-state lithium metal batteries.

[0094] In one embodiment, a battery is provided, comprising a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is prepared by the method as described above.

[0095] The preparation method of the sulfide solid electrolyte comprises: preparing electrolyte raw materials according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, adding a first solvent and performing ball milling to form a new electrolyte precursor; placing the new electrolyte precursor in a second solvent containing siloxane, heating and stirring to coat the new electrolyte precursor with siloxane to form an electrolyte precursor containing siloxane; and sintering the electrolyte precursor containing siloxane to obtain a doped and coated sulfide electrolyte.

[0096] In a specific embodiment, the method further includes: configuring the electrolyte raw materials according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, adding a first solvent, and ball milling to form a precursor solution; heating and drying the precursor solution to obtain the new electrolyte precursor.

[0097] Regarding the specific limitations on the method for preparing a sulfide solid electrolyte using a sulfide solid electrolyte as the electrolyte in the battery, please refer to the above limitations on the method for preparing a sulfide solid electrolyte using the sulfide solid electrolyte precursor as described above, which will not be repeated here.

[0098] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications falling within the scope of the embodiments of the present application.

[0099] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A sulfide solid electrolyte precursor, characterized in that: The chemical formula of the sulfide solid electrolyte precursor is Li 6-m PS 5-m X 1+m ; Among them, 0<m<2.5; The element X includes one or more of fluorine, chlorine, bromine and iodine.

2. The sulfide solid electrolyte precursor according to claim 1, characterized in that: In the chemical formula of the sulfide solid electrolyte precursor, 0<m<1.

3. A method for preparing a sulfide solid electrolyte using the sulfide solid electrolyte precursor according to claim 1 or 2, characterized in that: The method comprises: The electrolyte raw materials are prepared according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, and the first solvent is added and ball milled to form a new electrolyte precursor; placing the new electrolyte precursor in a second solvent containing siloxane, heating and stirring, so that the siloxane is coated on the new electrolyte precursor to form an electrolyte precursor containing siloxane; The electrolyte precursor containing siloxane is sintered to obtain a sulfide solid electrolyte.

4. The method for preparing a sulfide solid electrolyte according to claim 3, characterized in that: The method further comprises: The electrolyte raw materials are prepared according to the stoichiometric ratio in the chemical formula of the sulfide solid electrolyte precursor, and a first solvent is added thereto for ball milling to form a precursor solution; The precursor solution is heated and dried to obtain the new electrolyte precursor.

5. The method for preparing a sulfide solid electrolyte according to claim 4, characterized in that: The electrolyte raw material includes one or more of Li2S, P2S5, LiCl, LiBr, LiF or LiI; The first solvent is an alkane solvent; The ball milling speed is 200 rpm to 800 rpm; The ball milling time is 10h to 60h; The drying temperature of the precursor solution is 60°C to 140°C; The drying time of the precursor solution is 8 hours to 50 hours.

6. The method for preparing a sulfide solid electrolyte according to claim 3, characterized in that: The chemical formula of the siloxane is Si n O n-1 H 2n+2 or (H2SiO) n , where n is an integer greater than or equal to 2; The mass concentration of siloxane in the second solvent is 1% to 9%; The second solvent is an aromatic hydrocarbon solvent.

7. The method for preparing a sulfide solid electrolyte according to claim 3, characterized in that: The method further comprises: coating the new electrolyte precursor with siloxane and drying the new electrolyte precursor to form an electrolyte precursor having siloxane; The drying temperature is 60°C to 140°C; The drying time is 10 hours to 50 hours.

8. The method for preparing a sulfide solid electrolyte according to claim 3, characterized in that: The method further comprises: The electrolyte precursor containing siloxane is placed in a tubular furnace with an inert gas atmosphere for sintering to form a silicon dioxide coating layer on the surface of the electrolyte, and silicon dioxide is doped in the electrolyte bulk phase to form the sulfide solid electrolyte; Wherein, the thickness of the silicon dioxide coating layer is 1nm to 500nm; The inert gas includes one or more of nitrogen, helium, neon, argon, krypton, xenon or radon.

9. The method for preparing a sulfide solid electrolyte according to claim 8, characterized in that: The sintering temperature is 300°C to 800°C.

10. A battery comprising a positive electrode, a negative electrode and an electrolyte, characterized in that: The electrolyte is prepared by the method according to any one of claims 3 to 9.

Citation Information

Patent Citations

  • Preparation method of all-solid-state sulfide electrolyte for lithium ion battery

    CN112421119A

  • Method for modifying sulfide electrolyte by doping and coating synergistically and application of sulfide electrolyte

    CN115954536A

  • Sulfide electrolyte material and preparation method and application thereof

    CN116487687A

  • Modified sulfide solid electrolyte, preparation method thereof and all-solid-state battery

    CN116505059A

  • Surface coating modified sulfide solid electrolyte and preparation method and application thereof

    CN118299650A

Cited By

  • Preparation method of pure-phase sulfide solid-state electrolyte, solid-state electrolyte and solid-state battery

    CN119370812A

  • Sulfide solid electrolyte for in-situ construction of gradient interface layer based on grain boundary engineering and molecular bridging and preparation method thereof

    CN122177920A

  • A sulfide solid electrolyte based on in-situ construction of gradient interface layers using grain boundary engineering and molecular bridging, and its preparation method.

    CN122177920B

  • Sulfide solid-state electrolyte precursor, electrolyte precursor having siloxane, preparation method for sulfide solid-state electrolyte, and battery