Iron monatomic catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating and application of iron monatomic catalyst
By preparing a high-loading iron single-atom catalyst coordinated by sulfur atoms, and using the Fe electron-rich region/S electron-deficient region to regulate the electron transfer process, the problem of degradation and defluorination of fluoroquinolone antibiotics has been solved, and efficient degradation and defluorination have been achieved. , protecting the environment and human health.
Patent Information
- Application Number
- CN202410828814.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-25
Smart Images

Figure HDA0004911246130000011 
Figure HDA0004911246130000021 
Figure HDA0004911246130000022
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material engineering and environmental engineering, and specifically relates to an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating and an application thereof. Background Art
[0002] my country produces a large amount of antibiotics every year and has a huge demand for antibiotics. Fluoroquinolone antibiotics such as norfloxacin and ciprofloxacin are widely used in the pharmaceutical and aquaculture industries because of their broad antibacterial spectrum and strong antibacterial activity due to the antibiotics with valence groups (such as -F, piperazine ring, cyclopropyl, hydroxyl, etc.) in their molecular structure. Due to the lack of green, economical and efficient fluoroquinolone antibiotic wastewater treatment technology, it is easy to cause the production of drug-resistant bacteria and the spread of resistance genes, threatening human health and ecological environmental safety. Therefore, it is urgent to develop efficient degradation and defluorination technology for fluoroquinolone antibiotic wastewater.
[0003] In traditional advanced oxidation technology, the utilization rate of target active species is low and the electron transfer process (ET) is difficult to regulate. Therefore, the treatment effect on fluoroquinolone antibiotics and their high bond energy carbon-fluorine bonds is poor. Iron single atom catalysts (Fe SACs) can efficiently remove antibiotics in advanced oxidation technology. However, the structure-activity relationship between the metal atom loading and the activity and selectivity of single atom catalysts (SACs) is unclear. Through the synergistic effect of single metal atoms and coordinating atoms, the atomic utilization rate can be improved to achieve high activity; highly uniform active sites and geometric configurations enable energy level structure matching to achieve the purpose of highly selective generation of active species (such as ET). By precisely designing the electron-rich / deficient regions within the SAC, the sp 2 The carbon content is optimized, the disadvantage of poor conductivity of the carrier is optimized, and the electron transfer process between persulfate (PMS, PDS) and organic pollutants is directionally regulated, thereby achieving efficient degradation and defluorination process.
[0004] The high-loaded iron single-atom catalyst coordinated by sulfur (S) atoms can be precisely prepared through hydrogen bond self-assembly coupled with hydrothermal strategy. S coordination activates PMS to generate singlet oxygen ( 1 O2) and PDS for ET and other processes. The Fe electron-rich region / S electron-deficient region not only serves as a catalytic site to improve the utilization rate of PDS, but also accelerates the electron transfer rate in the carrier, which is conducive to the breaking of high-energy carbon-fluorine bonds. 2 Carbon-supported iron single-atom catalysts to activate persulfate-enhanced ET are key technologies for achieving defluorination of fluoroquinolone antibiotics. Summary of the invention
[0005] The purpose of the present invention is to address the deficiencies of the prior art and provide an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating and its application.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] In a first aspect, the present invention provides an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating. The iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating is prepared by the following steps:
[0008] (1) dissolving 0.25-0.35 g of oxalic acid and 0.25-0.35 g of ferric nitrate nonahydrate in 30-40 mL of deionized water to obtain solution A; dissolving 0.8-0.9 g of cyanuric acid in 90-100 mL of deionized water under magnetic stirring at 85-90° C. to obtain a cyanuric acid solution, then slowly adding solution A to the cyanuric acid solution and mixing thoroughly to obtain solution B; dissolving 0.9-1.0 g of melamine in 100-110 mL of deionized water under magnetic stirring at 85-90° C. to obtain a melamine solution, then slowly adding the melamine solution to solution B and continuing magnetic stirring for 4-5 hours to obtain solution C; then filtering solution C to obtain a supramolecular precursor;
[0009] (2) The supramolecular precursor is washed several times with deionized water, and then dried at 55-65°C for 12-16 hours; the dried supramolecular precursor is then placed in a tube furnace, heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon, reacted for 4-5 hours, and taken out after natural cooling to obtain Fe1 / CN;
[0010] (3) The Fe1 / CN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is recorded as Fe1 / NC.
[0011] In a second aspect, the present invention provides an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating. The iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating is prepared by the following steps:
[0012] (1) dissolving 0.05-0.1 g of ferric citrate and 0.07-0.13 g of N-allylthiourea in 30-40 mL of deionized water to obtain solution A; dissolving 0.8-0.9 g of cyanuric acid in 90-100 mL of deionized water under magnetic stirring at 85-90° C. to obtain a cyanuric acid solution, then slowly adding solution A to the cyanuric acid solution and mixing thoroughly to obtain solution B; dissolving 0.9-1.0 g of melamine in 100-110 mL of deionized water under magnetic stirring at 85-90° C. to obtain a melamine solution, then slowly adding the melamine solution to solution B and continuing magnetic stirring for 4-5 hours to obtain solution C; then filtering solution C to obtain a supramolecular precursor;
[0013] (2) The supramolecular precursor is washed several times with deionized water, and then dried at 55-65°C for 12-16 hours; the dried supramolecular precursor is then placed in a tube furnace, heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon, reacted for 4-5 hours, and taken out after natural cooling to obtain Fe1S / CN;
[0014] (3) The Fe1S / CN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h, and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon gas for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is recorded as Fe1S / NC.
[0015] In a third aspect, the present invention provides an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating. The iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating is prepared by the following steps:
[0016] (1) dissolving 0.6-0.7 g of ferric citrate and 0.15-0.25 g of thiocyanate in 30-40 mL of deionized water to obtain solution A; dissolving 0.8-0.9 g of cyanuric acid in 90-100 mL of deionized water under magnetic stirring at 85-90° C. to obtain a cyanuric acid solution, then slowly adding solution A to the cyanuric acid solution and mixing thoroughly to obtain solution B; dissolving 0.9-1.0 g of melamine in 100-110 mL of deionized water under magnetic stirring at 85-90° C. to obtain a melamine solution, then slowly adding the melamine solution to solution B and continuing magnetic stirring for 4-5 hours to obtain solution C; then filtering solution C to obtain a supramolecular precursor;
[0017] (2) The supramolecular precursor is washed several times with deionized water, and then dried at 55-65°C for 12-16 hours; the dried supramolecular precursor is then placed in a tube furnace, heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon, reacted for 4-5 hours, and taken out after natural cooling to obtain Fe1 / SCN;
[0018] (3) The Fe1 / SCN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is recorded as Fe1 / SNC.
[0019] In a fourth aspect, the present invention provides an application of an iron single-atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates in removing degraded fluoroquinolone antibiotics in water, comprising the following steps: adding an iron single-atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates to water containing fluoroquinolone antibiotics, magnetically stirring to obtain a mixed solution, adding persulfate (PMS, PDS) after adsorption equilibrium for 25 to 35 minutes, activating and degrading for 4 to 5 hours, and completing the removal of degraded fluoroquinolone antibiotics in the water; the dosage of the fluoroquinolone antibiotics is 0.1 to 0.3 g / L; the dosage of the iron single-atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates is 0.02 to 0.08 mM; and the dosage of the persulfate is 1 to 3 mM.
[0020] Furthermore, the fluoroquinolone antibiotic is ciprofloxacin, norfloxacin, moxifloxacin, pazufloxacin or gatifloxacin.
[0021] Furthermore, the persulfate is peroxymonosulfate or peroxydisulfate.
[0022] The beneficial effects of the present invention are:
[0023] 1) By regulating the added ligands, the controllable preparation of different S coordination was achieved, and then the generation of high-load Fe site activated PMS was precisely controlled 1 O2 and PDS undergo electron transfer (ET);
[0024] 2) Utilize the existence of Fe-rich electron region / S-deficient electron region to regulate the PDS activation pathway, improve the PDS utilization rate, and sp 2The carbon carrier has good conductivity, and a huge potential difference is formed between the Fe and S sites. Fe1S / NC and Fe1 / SNC activate PDS to generate ET, which is beneficial to the breaking of carbon-fluorine bonds. By removing high-energy carbon-fluorine bonds and their valence groups, the efficient degradation of fluoroquinolone antibiotics is promoted. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscope images and Fe, S, C, and N element distribution spectra of the iron single-atom catalysts prepared in Example 1, Example 2, and Example 3, wherein: Figure 1 (a) is a spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the iron single-atom catalyst prepared in Example 1 and a distribution spectrum of Fe, S, C, and N elements. Figure 1 (b) is a spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscopy image and a Fe, S, C, and N element distribution spectrum of the iron single-atom catalyst prepared in Example 2. Figure 1 (c) is a spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph and a Fe, S, C, and N element distribution spectrum of the iron single-atom catalyst prepared in Example 3;
[0026] Figure 2 The X-ray diffraction patterns of the iron single atom catalysts and NC prepared in Example 1, Example 2 and Example 3;
[0027] Figure 3 Fe K-edge X-ray absorption near-edge structure spectra of the iron single-atom catalysts, FeO, Fe2O3 and Fe3O4 prepared in Example 1, Example 2 and Example 3;
[0028] Figure 4 Fourier transform Fe K-edge R-space X-ray extended edge absorption fine structure spectra of the iron single atom catalyst, FeS, Fe3N, Fe4N and iron foil prepared in Example 1, Example 2 and Example 3;
[0029] Figure 5 The concentration change curve of CIP during the process of activating PMS or PDS with different concentrations by the iron single atom catalyst prepared in Example 3 to degrade CIP is shown in FIG. Figure 5 (a) is a graph showing the concentration variation of CIP during the degradation of CIP by using the iron single atom catalyst prepared in Example 3 to activate PMS with different concentrations. Figure 5 (b) is a graph showing the concentration variation of CIP during the process of activating different concentrations of PDS to degrade CIP using the iron single atom catalyst prepared in Example 3;
[0030] Figure 6This is a graph showing the degradation rate during the degradation of CIP by activating PMS or PDS of different concentrations with the iron single atom catalyst prepared in Example 3;
[0031] Figure 7 The graph of CIP concentration variation over time during the activation of PDS or the degradation of CIP by PDS alone during the activation of PDS by the iron single atom catalyst, NC and SNC prepared in Example 1, Example 2 and Example 3;
[0032] Figure 8 The graph of the defluorination rate variation over time during the process of activating PDS or degrading CIP with only PDS obtained by the iron single atom catalyst, NC and SNC prepared in Example 1, Example 2 and Example 3;
[0033] Fig. 9 The degradation rate and final defluorination rate of the iron single atom catalyst, NC and SNC activated PDS in the process of degrading CIP prepared in Example 1, Example 2 and Example 3;
[0034] Fig.10 The degradation rate and final defluorination rate of the iron single atom catalyst, NC and SNC activated PMS in the process of degrading CIP prepared in Example 1, Example 2 and Example 3;
[0035] Fig.11 The contribution rate of various active species to CIP degradation generated during the CIP degradation process of PMS activated by the iron single atom catalysts, NC and SNC prepared in Example 1, Example 2 and Example 3;
[0036] Fig.12 The graphs of NOX concentration and defluorination rate over time during NOX degradation by the iron single atom catalyst and NC activated PDS prepared in Example 1, Example 2 and Example 3, wherein: Fig.12 (a) is a graph showing the change of NOx concentration over time during the NOx degradation process of the iron single atom catalyst and NC activated PDS prepared in Example 1, Example 2 and Example 3, Fig.12 (b) is a graph showing the change of defluorination rate over time during NOx degradation by the iron single atom catalysts prepared in Examples 1, 2 and 3 and NC activated PDS;
[0037] Fig.13 The graphs of the MOX concentration and defluorination rate over time during the MOX degradation process of the iron single atom catalyst prepared in Example 1, Example 2 and Example 3 and NC activated PDS are shown, wherein: Fig.13 (a) is a graph showing the change of MOX concentration over time during the MOX degradation process of the iron single atom catalysts prepared in Examples 1, 2 and 3 and NC activated PDS, Fig.13 (b) is a graph showing the change of defluorination rate over time during the degradation of MOX by the iron single atom catalyst prepared in Example 1, Example 2 and Example 3 and NC activated PDS;
[0038] Fig.14 The graphs of the PAZ concentration and defluorination rate over time during the PAZ degradation process of the iron single-atom catalysts prepared in Examples 1, 2 and 3 and NC activated PDS are shown, wherein: Fig.14 (a) is a graph showing the change of PAZ concentration over time during the process of PAZ degradation by NC activated PDS and the iron single atom catalysts prepared in Examples 1, 2 and 3, Fig.14 (b) is a graph showing the change of defluorination rate over time during the degradation of PAZ by the iron single atom catalyst prepared in Example 1, Example 2 and Example 3 and NC activated PDS;
[0039] Fig.15 The graphs of the GAT concentration and defluorination rate over time during the GAT degradation process of the iron single atom catalyst prepared in Example 1, Example 2 and Example 3 and NC activated PDS are shown, wherein: Fig.15 (a) is a graph showing the change of GAT concentration over time during the GAT degradation process of the iron single atom catalysts prepared in Examples 1, 2 and 3 and NC activated PDS, Fig.15 (b) is a graph showing the change of defluorination rate over time during the degradation of GAT by the iron single atom catalysts prepared in Examples 1, 2 and 3 and NC activated PDS;
[0040] Fig.16 The degradation rate diagram of the iron single atom catalyst and NC activated PDS in the process of degrading various fluoroquinolone antibiotics prepared in Example 1, Example 2 and Example 3;
[0041] Fig.17 The dechlorination rate diagram of the iron single atom catalyst prepared in Example 1, Example 2 and Example 3 and the NC-activated PDS in the process of degrading various fluoroquinolone antibiotics. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0043] The present invention provides a method for preparing an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating the catalyst, comprising the following steps:
[0044] (1) 0.25-0.35 g of oxalic acid and 0.25-0.35 g of ferric nitrate nonahydrate are dissolved in 30-40 mL of deionized water to obtain solution A; 0.8-0.9 g of cyanuric acid is dissolved in 90-100 mL of deionized water under magnetic stirring at 85-90° C. to obtain a cyanuric acid solution, and then solution A is slowly added to the cyanuric acid solution and fully mixed to obtain solution B; 0.9-1.0 g of melamine is dissolved in 100-110 mL of deionized water under magnetic stirring at 85-90° C. to obtain a melamine solution, and then the melamine solution is slowly added to solution B and magnetic stirring is continued for 4-5 hours to obtain solution C, so that the iron atoms are fixed on the carrier along with the organic ligands; and then solution C is filtered to obtain a supramolecular precursor.
[0045] (2) The supramolecular precursor is washed several times with deionized water and then dried at 55-65°C for 12-16 hours. The dried supramolecular precursor is then placed in a tubular furnace and heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon for 4-5 hours. After natural cooling, the precursor is taken out to obtain Fe1 / CN, where the carrier is graphite phase carbon nitride.
[0046] (3) The Fe1 / CN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of the reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is denoted as Fe1 / NC. At this time, the carrier is nitrogen (N)-doped carbon (C).
[0047] The present invention also provides a second method for preparing an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating the catalyst, comprising the following steps:
[0048] (1) 0.05-0.1 g of ferric citrate and 0.07-0.13 g of N-allylthiourea are dissolved in 30-40 mL of deionized water to obtain solution A; while magnetically stirring at 85-90° C., 0.8-0.9 g of cyanuric acid is dissolved in 90-100 mL of deionized water to obtain a cyanuric acid solution, and then solution A is slowly added to the cyanuric acid solution and fully mixed to obtain solution B; while magnetically stirring at 85-90° C., 0.9-1.0 g of melamine is dissolved in 100-110 mL of deionized water to obtain a melamine solution, and then the melamine solution is slowly added to solution B and magnetically stirred for 4-5 hours to obtain solution C, so that the iron atoms are fixed on the carrier along with the organic ligands; and then solution C is filtered to obtain a supramolecular precursor.
[0049] (2) The supramolecular precursor is washed several times with deionized water and then dried at 55-65°C for 12-16 hours. The dried supramolecular precursor is then placed in a tubular furnace and heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon for 4-5 hours. After naturally cooling, the precursor is taken out to obtain Fe1S / CN, in which the carrier is graphite phase carbon nitride.
[0050] (3) The Fe1S / CN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of the reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating, which is denoted as Fe1S / NC, and the carrier is N-doped C.
[0051] The present invention also provides a third method for preparing an iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating the same, comprising the following steps:
[0052] (1) 0.6-0.7 g of ferric citrate and 0.15-0.25 g of thiocyanate are dissolved in 30-40 mL of deionized water to obtain solution A; while magnetically stirring at 85-90° C., 0.8-0.9 g of cyanuric acid is dissolved in 90-100 mL of deionized water to obtain a cyanuric acid solution, and then solution A is slowly added to the cyanuric acid solution and fully mixed to obtain solution B; while magnetically stirring at 85-90° C., 0.9-1.0 g of melamine is dissolved in 100-110 mL of deionized water to obtain a melamine solution, and then the melamine solution is slowly added to solution B and magnetically stirred for 4-5 hours to obtain solution C, so that the iron atoms are fixed on the carrier along with the organic ligands; and then solution C is filtered to obtain a supramolecular precursor.
[0053] (2) The supramolecular precursor is washed several times with deionized water and then dried at 55-65°C for 12-16 hours. The dried supramolecular precursor is then placed in a tubular furnace and heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon for 4-5 hours. After natural cooling, the precursor is taken out to obtain Fe1 / SCN, in which the carrier is graphite phase carbon nitride.
[0054] (3) The Fe1 / SCN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating, which is denoted as Fe1 / SNC, and the carrier is N-doped C.
[0055] The present invention also provides an application of an iron single-atom catalyst capable of efficiently degrading fluoroquinolone antibiotics and defluorinating in removing degraded fluoroquinolone antibiotics in water, comprising the following steps: adding the iron single-atom catalyst capable of efficiently degrading fluoroquinolone antibiotics and defluorinating in water containing fluoroquinolone antibiotics, magnetically stirring to obtain a mixed solution, adding persulfate after adsorption equilibrium for 25 to 35 minutes, activating and degrading for 4 to 5 hours, and completing the removal of degraded fluoroquinolone antibiotics in the water; the dosage of the fluoroquinolone antibiotics is 0.1 to 0.3 g / L; the dosage of the iron single-atom catalyst capable of efficiently degrading fluoroquinolone antibiotics and defluorinating is 0.02 to 0.08 mM; and the dosage of the persulfate is 1 to 3 mM.
[0056] The fluoroquinolone antibiotic is ciprofloxacin (CIP), norfloxacin (NOX), moxifloxacin (MOX), pazufloxacin (PAZ) or gatifloxacin (GAT).
[0057] The persulfate is peroxymonosulfate (PMS) or peroxydisulfate (PDS).
[0058] Example 1 An iron single-atom catalyst (Fe1 / NC) for efficient degradation and defluorination of fluoroquinolone antibiotics was prepared by the following steps:
[0059] (1) 0.29 g of oxalic acid and 0.32 g of ferric nitrate nonahydrate were dissolved in 30 mL of deionized water to obtain solution A; 0.83 g of cyanuric acid was dissolved in 90 mL of deionized water under magnetic stirring at 85° C. to obtain a cyanuric acid solution, and then solution A was slowly added to the cyanuric acid solution and mixed thoroughly to obtain solution B; 1.0 g of melamine was dissolved in 100 mL of deionized water under magnetic stirring at 85° C. to obtain a melamine solution, and then the melamine solution was slowly added to solution B and magnetic stirring was continued for 4 hours to obtain solution C; solution C was then filtered to obtain a supramolecular precursor.
[0060] (2) The supramolecular precursor was washed several times with deionized water and then dried at 60°C for 14 h. The dried supramolecular precursor was then placed in a tubular furnace and heated to 600°C at a heating rate of 5°C / min under flowing argon for 4 h. After naturally cooling, the precursor was taken out to obtain Fe1 / CN.
[0061] (3) Fe1 / CN prepared in step (2), 4.32 g glucose and 35 mL ultrapure water were added to the inner tank of the reactor, and the reactor was assembled and placed in an oven, heated at 180°C for 10 h for filtration; the filtered solid was dried at 60°C for 14 h. The mixture was placed in a tube furnace, heated to 900°C at a heating rate of 5°C / min under flowing argon for 4 h, and cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which was recorded as Fe1 / NC.
[0062] Example 2 An iron single-atom catalyst (Fe1S / NC) for efficient degradation of fluoroquinolone antibiotics and defluorination was prepared by the following steps:
[0063] (1) 0.07 g of ferric citrate and 0.1 g of N-allylthiourea were dissolved in 30 mL of deionized water to obtain solution A; 0.83 g of cyanuric acid was dissolved in 90 mL of deionized water under magnetic stirring at 85° C. to obtain a cyanuric acid solution, and then solution A was slowly added to the cyanuric acid solution and mixed thoroughly to obtain solution B; 1.0 g of melamine was dissolved in 100 mL of deionized water under magnetic stirring at 85° C. to obtain a melamine solution, and then the melamine solution was slowly added to solution B and magnetic stirring was continued for 4 hours to obtain solution C; and then solution C was filtered to obtain a supramolecular precursor.
[0064] (2) The supramolecular precursor was washed several times with deionized water and then dried at 60°C for 14 h. The dried supramolecular precursor was then placed in a tube furnace and heated to 600°C at a heating rate of 5°C / min under flowing argon for 4 h. After naturally cooling, the precursor was taken out to obtain Fe1S / CN.
[0065] (3) Fe1S / CN prepared in step (2), 4.32g glucose and 35mL ultrapure water were added to the inner tank of the reactor, and the reactor was assembled and placed in an oven, heated at 180°C for 10h for filtration; the filtered solid was dried at 60°C for 14h. Placed in a tube furnace, heated to 900°C at a heating rate of 5°C / min under flowing argon for 4h, and cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, recorded as Fe1S / NC.
[0066] Example 3 The iron single atom catalyst (Fe1 / SNC) for efficient degradation of fluoroquinolone antibiotics and defluorination was prepared by the following steps:
[0067] (1) 0.62 g of ferric citrate and 0.2 g of thiocyanic acid were dissolved in 30 mL of deionized water to obtain solution A; 0.83 g of cyanuric acid was dissolved in 90 mL of deionized water under magnetic stirring at 85° C. to obtain a cyanuric acid solution, and then solution A was slowly added to the cyanuric acid solution and mixed thoroughly to obtain solution B; 1.0 g of melamine was dissolved in 100 mL of deionized water under magnetic stirring at 85° C. to obtain a melamine solution, and then the melamine solution was slowly added to solution B and magnetic stirring was continued for 4 hours to obtain solution C; and then solution C was filtered to obtain a supramolecular precursor.
[0068] (2) The supramolecular precursor was washed several times with deionized water and then dried at 60°C for 14 h. The dried supramolecular precursor was then placed in a tube furnace and heated to 600°C at a heating rate of 5°C / min under flowing argon for 4 h. After naturally cooling, the precursor was taken out to obtain Fe1 / SCN.
[0069] (3) The Fe1 / SCN prepared in step (2), 0.43 g glucose and 35 mL ultrapure water were added to the inner tank of the reactor, and the reactor was assembled and placed in an oven, heated at 180°C for 10 h for filtration; the filtered solid was dried at 60°C for 14 h. The mixture was placed in a tube furnace, heated to 900°C at a heating rate of 5°C / min under flowing argon for 4 h, and cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which was recorded as Fe1 / SNC.
[0070] Figure 1 The spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscope images and Fe, S, C, and N element distribution spectra of the iron single-atom catalysts prepared in Example 1, Example 2, and Example 3, wherein: Figure 1 (a) is a spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the iron single-atom catalyst prepared in Example 1 and a distribution spectrum of Fe, S, C, and N elements. Figure 1 (b) is a spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscopy image and a Fe, S, C, and N element distribution spectrum of the iron single-atom catalyst prepared in Example 2. Figure 1 (c) is a spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the iron single-atom catalyst prepared in Example 3 and a distribution spectrum of Fe, S, C, and N elements. Figure 1 As shown in (a), on the left is a spherical aberration-corrected high-angle annular dark field scanning transmission electron microscopy image of the iron single atom catalyst prepared in Example 1 at a scale of 5nm, the upper middle is a spherical aberration-corrected high-angle annular dark field scanning transmission electron microscopy image of the iron single atom catalyst prepared in Example 1 at a scale of 50nm, the lower middle is the original distribution spectrum of N and Fe of the iron single atom catalyst prepared in Example 1, the upper right is the original distribution spectrum of C and Fe of the iron single atom catalyst prepared in Example 1, and the lower right is the original distribution spectrum of S and Fe of the iron single atom catalyst prepared in Example 1. Figure 1 (a) Figure 1 (b) and Figure 1 (c) shows that the evenly distributed single iron atoms in the iron single atom catalysts prepared in Example 1, Example 2 and Example 3 exist in CN; in the element distribution spectrum of Fe1 / NC, only the uniform existence of iron element can be observed; in the element distribution spectrum of Fe1 / SNC, Fe and S elements are not completely distributed in the same area; in the element distribution spectrum of Fe1S / NC, Fe and S elements are distributed in the same area.
[0071] Figure 2The X-ray diffraction patterns of the iron single atom catalyst and NC prepared in Example 1, Example 2 and Example 3 are shown. Figure 2 As shown, Fe1 / NC, Fe1S / NC and Fe1 / SNC are all consistent with the structure of NC, and the characteristic diffraction peaks of iron nanoparticles do not appear, indicating that the iron in each iron single atom catalyst exists in the form of small-sized atoms, which is consistent with the test results of spherical aberration electron microscopy.
[0072] Figure 3 The Fe K-edge X-ray absorption near-edge structure spectra of the iron single-atom catalysts, FeO, Fe2O3 and Fe3O4 prepared in Examples 1, 2 and 3 are shown. Figure 3 As shown, it was found that the absorption edges and transition energies of Fe1 / NC, Fe1S / NC and Fe1 / SNC were all located between the FeO and Fe2O3 benchmarks, and Fe1S / NC and Fe1 / SNC were closer to Fe3O4, confirming that the valence state of iron atoms in Fe1S / NC and Fe1 / SNC was lower than that in Fe1 / NC.
[0073] Figure 4 The Fourier transform Fe K-edge R-space X-ray extended edge absorption fine structure spectra of the catalysts, FeS, Fe3N, Fe4N and iron foil (Fefoil) prepared in Examples 1, 2 and 3 are shown. Figure 4 As shown in Figure 2, the coordination configurations of iron atoms in Fe1 / NC, Fe1S / NC and Fe1 / SNC were studied based on extended X-ray absorption fine measurement. At the same time, standard samples such as FeS, Fe3N, Fe4N and iron foil (Fe foil) were studied. It was found that Fe1 / NC and Fe1 / SNC There is a characteristic peak corresponding to Fe-N coordination scattering at This corresponds to the Fe-S coordination bond of the FeS standard sample, indicating that there is a Fe-S coordination configuration inside it.
[0074] Application Example 1 Degradation experiment of ciprofloxacin (CIP) by Fe1 / SNC at different PMS and PDS concentrations
[0075] (1) A saturated aqueous solution of CIP was added to a 100 mL beaker containing 50 mL of deionized water, so that the initial concentration of the CIP solution was 0.05 mM. 0.2 g / L of the iron single atom catalyst prepared in Example 3 was added, ultrasonically dispersed, and placed on a magnetic stirrer for stirring until the adsorption reaction equilibrium between the solid and the liquid was reached, and then an activator was added, and the concentrations of the activators PMS and PDS were controlled to be 0.25 mM, 0.5 mM, 1.0 mM, and 2.0 mM, respectively.
[0076] (2) After adding the activator, start timing and use a syringe to take samples at 0, 10, 30, 60, 120, 180 and 240 minutes respectively. After solid-liquid separation with a 0.22 micron filter membrane, add the samples to an ampoule containing 10% by volume methanol solution.
[0077] (3) The concentration of CIP in the solution was determined using high performance liquid chromatography.
[0078] Figure 5 The concentration change curve of CIP during the process of activating PMS or PDS with different concentrations by the iron single atom catalyst prepared in Example 3 to degrade CIP is shown in FIG. Figure 5 (a) is a graph showing the concentration variation of CIP during the degradation of CIP by using the iron single atom catalyst prepared in Example 3 to activate PMS with different concentrations. Figure 5 (b) is a graph showing the concentration variation of CIP during the process of activating PDS with different concentrations using the iron single atom catalyst prepared in Example 3 to degrade CIP. Figure 5 (a) and Figure 5 The degradation curves in (b) were fitted with their first-order kinetics to obtain the degradation rate diagram of Fe1 / SNC during the degradation of CIP at different PMS or PDS concentrations ( Figure 6 ).like Figure 6 As shown in the figure, in the case of low concentration of activator (≤1.0mM), the degradation rate of activated PDS is higher than that of activated PMS; in the case of high concentration of activator (>1.0mM), the degradation rate of activated PMS is higher than that of activated PDS. The consumption rate of PMS is positively correlated with its addition amount, while the relationship between the consumption rate of PDS and its addition amount is not obvious.
[0079] Application Example 2 Experiment on the degradation of CIP by PDS activated by different catalysts (Fe1 / NC, Fe1S / NC and Fe1 / SNC)
[0080] (1) A saturated aqueous solution of CIP was added to a 100 mL beaker containing 50 mL of deionized water, so that the initial concentration of the CIP solution was 0.05 mM. 0.2 g / L of the iron single atom catalyst (Fe1 / NC) prepared in Example 1, the iron single atom catalyst (Fe1S / NC) prepared in Example 2, the iron single atom catalyst (Fe1 / SNC) prepared in Example 3, NC or SNC were added respectively, ultrasonically dispersed, placed on a magnetic stirrer and stirred until the adsorption reaction equilibrium between the solid and the liquid was reached, and then an activator was added to control the activator PDS concentration to be 2.0 mM.
[0081] (2) After adding the activator, start timing and use a syringe to take samples at 0, 10, 30, 60, 120, 180 and 240 minutes respectively. After solid-liquid separation with a 0.22 micron filter membrane, add the samples to an ampoule bottle and a centrifuge tube filled with a 10% by volume methanol solution.
[0082] (3) The concentration of CIP and the concentration of fluoride ions in the solution were determined by high performance liquid chromatography and fluoride ion electrode, respectively.
[0083] Figure 7 The graph shows the change of CIP concentration over time during the activation of PDS by Fe1 / NC, Fe1S / NC, Fe1 / SNC, NC and SNC, or the degradation of CIP by PDS alone. Figure 8 The graph shows the change of defluorination rate over time during the process of Fe1 / NC, Fe1S / NC, Fe1 / SNC, NC and SNC activating PDS or only PDS degrading CIP. Fig. 9 This is a graph showing the degradation rate and final defluorination rate during the degradation of CIP by Fe1 / NC, Fe1S / NC, Fe1 / SNC, NC and SNC activated PDS.
[0084] Figure 7 , Fig. 9 It shows that the rate of PDS degradation by Fe1 / SNC is significantly faster than that by Fe1S / NC and Fe1 / NC. Figure 8 It shows that the defluorination rate of CIP by Fe1 / SNC activated PDS is also greater than that of Fe1S / NC and Fe1 / NC, and there is a positive correlation between the reaction rate constant and the defluorination rate.
[0085] Application Example 3 Degradation experiment of CIP by PMS activated by different catalysts (Fe1 / NC, Fe1S / NC and Fe1 / SNC)
[0086] (1) A saturated aqueous solution of CIP was added to a 100 mL beaker containing 50 mL of deionized water, so that the initial concentration of the CIP solution was 0.05 mM. 0.2 g / L of the iron single atom catalyst (Fe1 / NC) prepared in Example 1, the iron single atom catalyst (Fe1S / NC) prepared in Example 2, the iron single atom catalyst (Fe1 / SNC) prepared in Example 3, NC or SNC were added respectively, ultrasonically dispersed, placed on a magnetic stirrer and stirred until the adsorption reaction equilibrium between the solid and the liquid was reached, and then an activator was added to control the concentration of the activator PMS to be 2.0 mM.
[0087] (2) After adding the activator, start timing and use a syringe to take samples at 0, 10, 30, 60, 120, 180 and 240 minutes respectively. After solid-liquid separation with a 0.22 micron filter membrane, add the samples to an ampoule bottle and a centrifuge tube filled with a 10% by volume methanol solution.
[0088] (3) The concentration of CIP and the concentration of fluoride ions in the solution were determined by high performance liquid chromatography and fluoride ion electrode, respectively.
[0089] Fig.10 This is a graph showing the degradation rate and final defluorination rate during the degradation of CIP by Fe1 / NC, Fe1S / NC, Fe1 / SNC, NC and SNC activated PMS. Fig.10 It shows that the degradation rate and defluorination rate of CIP by Fe1 / SNC activated PMS are slightly different from those of Fe1S / NC and Fe1 / NC, and there is no obvious relationship between the reaction rate constant and the defluorination rate.
[0090] Application Example 4: Exploring the contribution of various active species to CIP degradation
[0091] (1) Add a saturated aqueous solution of CIP to several 100 mL beakers containing 50 mL of deionized water, so that the initial concentration of the CIP solution is 0.05 mM. Weigh various quenchers and add them to each CIP solution, so that the concentrations of methanol and tert-butyl alcohol are 500 mM, the concentration of nitroblue tetrazolium is 5 mM, the concentration of methylphenyl sulfoxide is 5 mM, and the concentration of sodium azide is 5 mM. Add 0.2 g / L of the iron single atom catalyst (Fe1 / NC) prepared in Example 1, the iron single atom catalyst (Fe1S / NC) prepared in Example 2, the iron single atom catalyst (Fe1 / SNC) prepared in Example 3, NC or SNC to each beaker, perform ultrasonic dispersion, place on a magnetic stirrer and stir until the adsorption reaction equilibrium is reached between the solid and the liquid, then add an activator, and control the concentration of the activator PDS to 2.0 mM.
[0092] (2) After adding the activator, start timing and use a syringe to take samples at 0, 10, 30, 60, 120, 180 and 240 minutes respectively. After solid-liquid separation with a 0.22 micron filter membrane, add the samples to an ampoule containing 10% by volume methanol solution.
[0093] (3) The concentration of CIP in the solution was determined using high performance liquid chromatography.
[0094] Fig.11 The various active species (free radicals (such as ·OH, ·SO4 - 、O2 - etc.), singlet oxygen ( 1 O2) and high-valent iron (Fe VI =O)) to CIP degradation. According to the addition of methanol (quenching ·OH and ·SO4 - ), tert-butyl alcohol (quenching ·OH), nitro blue tetrazolium (quenching ·O2 - ), sodium azide (quenching 1 O2) and methyl phenyl sulfoxide (quenching Fe VI =O) to different single-atom catalysts, the degradation rate of CIP, and the contribution rate of various active species to CIP degradation are obtained, such as Fig.11 As shown, Fe1 / SNC activated PMS to generate 1 O2 is the main source, while Fe1 / SNC activates PDS to generate electron transfer (ET). The generation mechanism is that the Fe atom in Fe1 / SNC combines with the terminal O site in the PMS molecule to break the OO bond and generate 1 O2; the Fe atoms in Fe1 / SNC form an inner complex (PDS*) with the PDS molecules, using the carrier NC as a platform for transferring electrons. Fe1 / SNC captures the electrons from the antibiotic molecules, and the activation process is mainly ET.
[0095] Application Example 5 Degradation and defluorination effect of fluoroquinolone antibiotics
[0096] (1) Saturated aqueous solutions of norfloxacin (NOX), moxifloxacin (MOX), pazufloxacin (PAZ), and gatifloxacin (GAT) were added to several 100 mL beakers containing 50 mL of deionized water, respectively, so that the initial concentration of each antibiotic solution was 0.05 mM. 0.2 g / L of the iron single atom catalyst (Fe1 / NC) prepared in Example 1, the iron single atom catalyst (Fe1S / NC) prepared in Example 2, the iron single atom catalyst (Fe1 / SNC) prepared in Example 3 or NC was added, ultrasonically dispersed, placed on a magnetic stirrer and stirred until the adsorption reaction equilibrium was reached between the solid and the liquid, and then an activator was added to control the activator PDS concentration to be 1.0 mM.
[0097] (2) After adding the activator, start timing and use a syringe to take samples at 0, 10, 30, 60, 120, 180 and 240 minutes respectively. After solid-liquid separation with a 0.22 micron filter membrane, add the samples to an ampoule bottle and a centrifuge tube filled with a 10% by volume methanol solution.
[0098] (3) The concentrations of NOX, MOX, PAZ and GAT and the fluoride ion concentration in the solution were determined by high performance liquid chromatography and fluoride ion electrode, respectively.
[0099] Fig.12 The graph of NOX concentration and defluorination rate over time during the NOX degradation process of Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS, where: Fig.12 (a) is the graph showing the change of NOX concentration over time during the NOX degradation process of Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.12 (b) The defluorination rate changes with time during the degradation of NOX by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.13 The graph of MOX concentration and defluorination rate over time during the degradation of MOX by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS, where: Fig.13 (a) is the graph showing the change of MOX concentration over time during the degradation of MOX by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.13 (b) The defluorination rate changes with time during the degradation of MOX by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.14 The graph of PAZ concentration and defluorination rate over time during the degradation of PAZ by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS, where: Fig.14 (a) is the change of PAZ concentration over time during the degradation of PAZ by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.14 (b) The defluorination rate changes with time during the degradation of PAZ by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.15 The graph of GAT concentration and defluorination rate over time during the degradation of GAT by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS, where: Fig.15 (a) is the graph showing the change of GAT concentration over time during the degradation of GAT by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS. Fig.15 (b) The defluorination rate changes with time during the degradation of GAT by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS.
[0100] Fig.12 , Fig.13 , Fig.14 and Fig.15 It shows that Fe1 / SNC, Fe1S / NC and Fe1 / NC activated PDS can completely degrade MOX, PAZ, GAT within 1 hour, and completely degrade NOX within 2 hours, and the defluorination rate can reach 10%-30%.
[0101] Fig.16 The degradation rate diagram of Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS during the degradation of fluoroquinolone antibiotics. Fig.17 The dechlorination rate diagram during the degradation of fluoroquinolone antibiotics by Fe1 / NC, Fe1S / NC, Fe1 / SNC and NC activated PDS.
[0102] Fig.16 and Fig.17 It shows that different catalysts have different degradation effects and defluorination rates for fluoroquinolone antibiotics, which may be related to the different effects of ET on the valence groups (-F, piperazine ring, cyclopropyl, hydroxyl, etc.) of fluoroquinolone antibiotics. For example, Fe1S / NC has the best effect on the degradation of NOX, Fe1 / SNC has the best effect on the degradation of MOX and PAZ, and the best effect on the defluorination of CIP.
[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An iron single-atom catalyst for efficient degradation and defluorination of fluoroquinolone antibiotics, characterized in that: The iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating is prepared by the following steps: (1) dissolving 0.25-0.35 g of oxalic acid and 0.25-0.35 g of ferric nitrate nonahydrate in 30-40 mL of deionized water to obtain solution A; dissolving 0.8-0.9 g of cyanuric acid in 90-100 mL of deionized water under magnetic stirring at 85-90° C. to obtain a cyanuric acid solution, then slowly adding solution A to the cyanuric acid solution and mixing thoroughly to obtain solution B; dissolving 0.9-1.0 g of melamine in 100-110 mL of deionized water under magnetic stirring at 85-90° C. to obtain a melamine solution, then slowly adding the melamine solution to solution B and continuing magnetic stirring for 4-5 hours to obtain solution C; Then, solution C is filtered to obtain a supramolecular precursor; (2) The supramolecular precursor is washed several times with deionized water, and then dried at 55-65°C for 12-16 hours; the dried supramolecular precursor is then placed in a tube furnace, heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon, reacted for 4-5 hours, and taken out after natural cooling to obtain Fe1 / CN; (3) The Fe1 / CN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is recorded as Fe1 / NC.
2. An iron single-atom catalyst for efficient degradation and defluorination of fluoroquinolone antibiotics, characterized in that: The iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating is prepared by the following steps: (1) 0.05-0.1 g of ferric citrate and 0.07-0.13 g of N-allylthiourea are dissolved in 30-40 mL of deionized water to obtain a solution A; while magnetically stirring at 85-90° C., 0.8-0.9 g of cyanuric acid is dissolved in 90-100 mL of deionized water to obtain a cyanuric acid solution, and then the solution A is slowly added to the cyanuric acid solution and mixed thoroughly to obtain a solution B; while magnetically stirring at 85-90° C., 0.9-1.0 g of melamine is dissolved in 100-110 mL of deionized water to obtain a melamine solution, and then the melamine solution is slowly added to the solution B and the magnetic stirring is continued for 4-5 hours to obtain a solution C; Then, solution C is filtered to obtain a supramolecular precursor; (2) The supramolecular precursor is washed several times with deionized water, and then dried at 55-65°C for 12-16 hours; the dried supramolecular precursor is then placed in a tube furnace, heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon, reacted for 4-5 hours, and taken out after natural cooling to obtain Fe1S / CN; (3) The Fe1S / CN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h, and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon gas for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is recorded as Fe1S / NC.
3. An iron single-atom catalyst for efficient degradation and defluorination of fluoroquinolone antibiotics, characterized in that: The iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating is prepared by the following steps: (1) dissolving 0.6-0.7 g of ferric citrate and 0.15-0.25 g of thiocyanate in 30-40 mL of deionized water to obtain solution A; dissolving 0.8-0.9 g of cyanuric acid in 90-100 mL of deionized water under magnetic stirring at 85-90° C. to obtain a cyanuric acid solution, then slowly adding solution A to the cyanuric acid solution and mixing thoroughly to obtain solution B; dissolving 0.9-1.0 g of melamine in 100-110 mL of deionized water under magnetic stirring at 85-90° C. to obtain a melamine solution, then slowly adding the melamine solution to solution B and continuing magnetic stirring for 4-5 hours to obtain solution C; Then, solution C is filtered to obtain a supramolecular precursor; (2) The supramolecular precursor is washed several times with deionized water, and then dried at 55-65°C for 12-16 hours; the dried supramolecular precursor is then placed in a tube furnace, heated to 550-650°C at a heating rate of 4-6°C / min under flowing argon, reacted for 4-5 hours, and taken out after natural cooling to obtain Fe1 / SCN; (3) The Fe1 / SCN prepared in step (2), 4.3-4.4 g of glucose and 30-40 mL of ultrapure water are added to the inner tank of a reactor. After assembling the reactor, the reactor is placed in an oven and heated at 170-190° C. for 10-11 h and then filtered; the filtered solid is dried at 55-65° C. for 12-16 h; the solid is placed in a tubular furnace and heated to 800-1000° C. at a heating rate of 4-6° C. / min under flowing argon for 4-5 h, and then cooled naturally to obtain an iron single atom catalyst that efficiently degrades fluoroquinolone antibiotics and defluorinates, which is recorded as Fe1 / SNC.
4. Use of the iron single-atom catalyst for efficiently degrading fluoroquinolone antibiotics and defluorinating according to claim 1, 2 or 3 for removing degraded fluoroquinolone antibiotics in water, characterized in that: The following steps are involved: In water containing fluoroquinolone antibiotics, an iron single atom catalyst that can efficiently degrade fluoroquinolone antibiotics and defluorinate is added, a mixed solution is obtained by magnetic stirring, and after adsorption equilibrium for 25 to 35 minutes, persulfate is added to activate and degrade for 4 to 5 hours to complete the removal of degraded fluoroquinolone antibiotics in the water body; the dosage of the fluoroquinolone antibiotics is 0.1 to 0.3 g / L; the dosage of the iron single atom catalyst that can efficiently degrade fluoroquinolone antibiotics and defluorinate is 0.02 to 0.08 mM; and the dosage of the persulfate is 1 to 3 mM.
5. The use according to claim 4, characterized in that: The fluoroquinolone antibiotic is ciprofloxacin, norfloxacin, moxifloxacin, pazufloxacin or gatifloxacin.
6. The use according to claim 4, characterized in that: The persulfate is peroxymonosulfate or peroxydisulfate.
Citation Information
Patent Citations
Controllable synthesis method of monoatomic catalyst with low cost and high loading capacity
CN111939961A
Preparation method and application of nitrogen-doped porous carbon catalyst
CN114984996A
Method and device for treating fluoroquinolone antibiotics in wastewater solution
CN116443982A
Method for preparing monatomic catalyst by loading monatomic through cascade fixation strategy and application of monatomic catalyst
CN116851020A
Single-atom catalyst for activation of persulfate to generate pure singlet oxygen as well as preparation method and application thereof
US20220315425A1
Cited By
Kilogram-level high-loading iron monatomic catalyst as well as preparation method and application of kilogram-level high-loading iron monatomic catalyst
CN119215895A
Method for synthesizing monatomic cobalt catalyst through ligand-assisted supramolecular strategy pyrolysis, obtained catalyst and application
CN119771411A
Iron monatomic catalyst with controllable doping of elements in p region and application of iron monatomic catalyst
CN119838622A
Iron monatomic catalyst for efficiently and directionally converting rifamycin B to O and application of iron monatomic catalyst
CN120079435A
Highly efficient and directional conversion of rifamycin B to O using an iron single-atom catalyst and its application