Production method of nickel-based 625 and pipeline steel X65M composite board
Through asymmetric billet assembly and controlled rolling and cooling processes, the problem of partial non-composite and low shear strength of nickel-based 625 and pipeline steel X65M composite plates during the rolling process was solved, and the high mechanical properties and good shear strength of the composite plates were achieved. Corrosion resistance meets the safety requirements of oil and gas field gathering and transportation pipelines.
Patent Information
- Application Number
- CN202410909051.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing nickel-based 625 and pipeline steel X65M composite plates have problems of partial non-composite and low shear strength during the rolling process, resulting in insufficient sealing and strength of the pipeline gathering and transportation system, and prone to quality and safety accidents such as cracking, corrosion and leakage. .
The asymmetric billet assembly process is adopted, including the asymmetric combination of the rectangular X65M base material billet and the nickel-based 625 billet, heating, first-stage rolling, controlled cooling of the intermediate billet, second-stage rolling and controlled cooling treatment, controlling the heating temperature, rolling Control speed and cooling rate to ensure the composite performance and shear strength of the material.
The produced nickel-based 625 and pipeline steel X65M composite panels have excellent mechanical properties, with yield strength of 460~550Mpa, tensile strength of 550~620Mpa, -40℃ impact ≥300J, -30℃ DWTT shear area ratio ≥85%, The shear strength is ≥350MPa, and the intergranular corrosion crack rate is 0, which meets the corrosion resistance requirements of oil and gas field gathering and transportation pipelines.
Smart Images

Figure CN118788751A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rolling composite, and in particular relates to a production method of a nickel-based 625 and pipeline steel X65M composite plate. Background Art
[0002] Natural gas contains corrosive media such as hydrogen sulfide, which can cause serious corrosion to carbon steel pipes, especially process pipelines, elbows, bends, tees and other pipe fittings at stations, which are more prone to corrosion failure, seriously reducing the service life of the process pipeline network. The maintenance and replacement of pipeline fittings at stations are relatively complicated and costly. If the transportation needs to be stopped, it will seriously affect the economic benefits. Therefore, the selection of bimetallic composite pipes has become an important means of corrosion control for oil and gas field gathering and transportation pipelines. Compared with ordinary carbon steel pipes, double-layer metal composite pipes are corrosion-resistant, and compared with corrosion-resistant alloy pure materials, they are economical and have better strength and toughness. Due to the good corrosion resistance and economy of bimetallic composite pipes, their related technical development and application research have made certain progress since the 1990s. The application of bimetallic composite pipes in oil and gas gathering and transportation pipelines effectively solves the corrosion problem of highly corrosive oil and gas gathering and transportation pipes.
[0003] At present, bimetallic composite pipes are mostly made of nickel-based 625 and X65M materials that are explosively composited. This preparation method is simple, low-cost, and the composite is not affected by changes in the thickness of the substrate, so it has strong universality. However, explosive composite is greatly affected by weather and process stability, and local non-composite and low shear strength problems often occur on the bonding surface. In addition, during the process of bimetallic composite plate pipe making, welding, and construction, the bonding defects will be further magnified. Once there are problems with the sealing, strength, and corrosion resistance of the pipeline gathering and transportation system, quality and safety accidents and environmental accidents such as cracking, corrosion leakage are very likely to occur. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a production method for a nickel-based 625 and pipeline steel X65M composite plate with a relatively simple process. The obtained nickel-based 625 and pipeline steel X65M composite plate has better composite properties, better mechanical properties, and an intergranular corrosion crack rate of 0.
[0005] The technical solution adopted by the present invention to solve the technical problem is a production method of a nickel-based 625 and pipeline steel X65M composite plate, and the key production process steps include:
[0006] 1) Composite plate assembly: Asymmetric assembly is adopted, two rectangular X65M base material billets, one nickel-based 625 billet, and one sealing plate Q235B are selected to complete the processes of blanking, surface grinding, beveling, isolation agent coating, assembly, and billet welding;
[0007] 2) Heating: within 48 hours after the composite billet is welded in step 1), the composite billet is heated in a furnace, the heating temperature is controlled to be 1120-1150° C., the heating rate is ≤3 min / mm, the total time in the furnace is ≥ the thickness of the composite billet (mm)×2.0 (min / mm), and the furnace temperature is 1120-1150° C.;
[0008] 3) First stage rolling: the first three passes have a reduction of 30-55 mm, the first stage rolling end temperature is ≥1050°C, the first stage cumulative reduction rate is 60%-70%, and the rolling speed is 2.0-3.0 m / s;
[0009] The first three passes of the first stage rolling of the present invention are more suitable for the reduction amount, which can ensure the composite performance of the material. When the reduction amount is less than 30mm, the rolling composite effect becomes worse, resulting in the shear strength being difficult to reach 350Mpa; and when the reduction amount is greater than 55mm, the reduction is too large, resulting in different ductility of the two materials, reduced interface composite rate, and a significant decrease in shear strength.
[0010] In addition, the cumulative reduction rate in the first stage has a great influence on the impact and drop hammer properties of the substrate. When the cumulative reduction rate in the first stage is less than 60%, the recrystallization effect of rough rolling is weakened, resulting in poor uniformity of grain size in the thickness direction, affecting the subsequent impact and drop hammer properties of the substrate; and when the cumulative reduction rate in the first stage is greater than 70%, the space for the cumulative reduction rate in the second stage will be compressed, thereby reducing the nucleation effect of rolling in the non-recrystallized zone in the second stage, weakening the grain refinement effect, and affecting the subsequent impact and drop hammer properties of the substrate.
[0011] 4) Controlled cooling of the intermediate billet: After rough rolling, the intermediate billet is sent to the intermediate roller for laminar cooling. The cooling rate is set at 15-20℃ / s and the outlet water surface temperature is 800-830℃;
[0012] The present invention sets the cooling rate of the intermediate billet to 15-20°C / s, the purpose is to control the appropriate temperature difference between the substrate and the composite material, so as to improve the comprehensive performance of the composite plate. When the cooling rate is less than 15°C / s, it is difficult to cool the composite billet from the surface to the core. After the intermediate billet is quickly cooled, the temperature will rise again due to the internal high temperature conduction, and it will be reheated for the second stage of rolling. In this way, the temperature gradient of the intermediate billet is not enough, resulting in a large difference in ductility between the substrate X65M and the composite nickel-based 625 when the second stage of rolling begins, and the interface shear strength is difficult to ensure above 350Mpa; and when the cooling rate is greater than 20°C / s, the cooling rate is too large, the intermediate billet is cooled, resulting in insufficient temperature gradient of the intermediate billet, and when the second stage of rolling begins, it is also difficult to ensure the interface shear strength is above 350Mpa.
[0013] 5) Second stage rolling: starting rolling temperature 780-820°C, final rolling temperature 750-780°C, 7-9 rolling passes, pass reduction rate is implemented in a pass-by-pass decreasing mode, rolling speed 3.0-4.0 m / s, and the reduction rate from the last to the third last pass is ≤5.0%;
[0014] 6) Controlled cooling: After the third stage of rolling, the steel plate is subjected to controlled cooling treatment, with the initial cooling temperature of 720-760°C, the Mulpic cooling rate of 5-10°C / s, and the final cooling temperature of the composite plate of 350-450°C;
[0015] 7) Finishing: The composite panels are separated, cleaned, polished, straightened and leveled, and then cut and polished according to the final size of the order before packaging and shipment.
[0016] Further, in the step 1), the material is cut into two rectangular X65M substrate blanks, and the size requirements are as follows: the compression ratio of the lower substrate blank (the thickness of the lower substrate blank: the thickness of the finished composite plate substrate) = 6.0 ~ 8.0, the thickness of the upper substrate blank = the thickness of the lower substrate blank × 0.5; one nickel-based 625 blank, the thickness = 0.9 × (the thickness of the lower substrate blank ÷ the thickness of the finished composite plate substrate) × the thickness of the finished composite plate composite nickel-based 625; the width of the X65M substrate blank = the width of the composite nickel-based 625 blank + 400mm, the length of the X65M substrate blank = the length of the composite nickel-based 625 blank + (650 ~ 700) mm; Q235B is used as a sealing plate, which is laid around the composite nickel-based 625 for filling, and the thickness is the same as that of the composite nickel-based 625.
[0017] Furthermore, in the step 1), the substrate surface is ground: the composite surface of the substrate is ground with a grinder to ensure that there is no iron oxide scale, the substrate has a metallic luster, and there is no oil stain, debris, print stain, etc.
[0018] Furthermore, in the step 1), beveling is performed: welding bevels are performed on the four sides of the two ground substrate surfaces, with a bevel depth of 35-45 mm (preferably 40 mm) and a bevel angle of 28-32° (preferably 30°).
[0019] Furthermore, in the step 1), a release agent is applied: the contact surface of the composite nickel-based 625 and the upper substrate X65M is coated with a release agent with a thickness of 0.03 to 0.1 mm, and the entire board surface is evenly coated and then baked at a temperature of 550 to 600° C. for 30 to 40 minutes.
[0020] Furthermore, in the step 1), the blanks are assembled: the blanks are stacked in the order of upper substrate blank + separator + composite blank + lower substrate blank in thickness direction. The composite nickel-based 625 blank is located at the geometric center of the substrate blank, and is welded to the lower substrate X65M on both sides along the rolling direction, with a weld width of 20 to 30 mm. After the blank assembly machine is hydraulically pressed, ensure that there is no gap between the sealing plate and the substrate blank contact surface, and use gas shielded spot welding to firmly weld.
[0021] Further, in the step 1), the welding billet: the composite billet after positioning should be fully welded with a seal, and the width of the molten pool around it is 35 to 40 mm. After welding, two air holes are left at the joint surface of the composite plate billet for vacuum treatment, one at the head and one at the tail in the rolling direction. When the vacuum degree of the composite surface reaches below -0.1Mpa, it is maintained for more than 40 minutes. After confirming that the negative pressure of the composite billet is stable, the vacuum pipe is closed.
[0022] The nickel-based 625 and pipeline steel X65M composite plate obtained by the production method of the present invention has a material yield strength of 460-550Mpa, a tensile strength of 550-620Mpa, an impact of ≥300J at -40°C, a DWTT shear area ratio of ≥85% at -30°C, a shear strength of ≥350MPa, and an intergranular corrosion crack rate of 0.
[0023] The present invention uses an asymmetric composite method, which has a simple and easy process, covers a wide range of steel grades, and can better meet the performance requirements of nickel-based 625 and pipeline steel X65M composite plates. The biggest difficulty in composite nickel-based 625 with carbon steel is the difference in ductility of the two materials. The asynchronous deformation makes it difficult to roll and fuse. The lower the temperature, the greater the difference in ductility. The low-temperature toughness of pipeline steel X65M must be guaranteed by medium and low temperature rolling, and the two form an irreconcilable contradiction. This method adopts the control means of "low-temperature austenitization + intermediate rapid cooling + low-temperature zone excision" to solve this contradiction very well. The low-temperature + long-term heating method not only ensures that the internal heating of the composite blank is sufficient and uniform, but also avoids the abnormal growth of the original austenite grains of the substrate X65M, providing good heating conditions for subsequent composite and substrate fine grain control. A quick cooling device is set on the middle roller table, so that the surface of the intermediate billet to the 1 / 4 position of the thickness is cooled to the second stage rolling temperature in a very short time, but the temperature of the steel plate near the core (near the composite material) is still relatively high. In this way, the temperature ladder formed in the thickness direction can ensure that the rolling temperature of the base material part is in the required "low temperature zone", and on the other hand, the "high temperature zone" of the core composite material part can greatly improve its good ductility. The sealing plate Q235B is used around the composite material for large area isolation, and finally the surrounding area is cut off to solve the problem of non-composite caused by the large temperature difference between the head, tail and edge.
[0024] The present invention has the following beneficial effects: the method can produce a nickel-based 625+X65M composite plate with a thickness of 30-45 mm and a width of 1400-3800 mm through composite plate assembly + welding + controlled rolling and controlled cooling + sheeting and straightening. The nickel-based 625+X65M composite plate produced by the method has a material yield strength of 460-550 MPa, a tensile strength of 550-620 MPa, a -40°C impact of ≥300 J, a -30°C DWTT shear area ratio of ≥85%, a shear strength of ≥350 MPa, and an intergranular corrosion crack rate of 0, which can well meet the safety and corrosion resistance requirements of various pipeline engineering projects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a typical metallographic structure photo of the composite plate of Example 1;
[0026] Figure 2 This is the drop hammer morphology of the -30℃ composite plate in Example 1. DETAILED DESCRIPTION
[0027] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings.
[0028] Example 1: Production of 2+28mm nickel-based 625+X65M
[0029] The chemical composition of nickel-based 625 and pipeline steel X65M is shown in Table 1, with the remainder being Fe and unavoidable impurity elements. 2+28mm (indicates that the thickness of the finished composite plate composite nickel-based 625 is 2mm, and the thickness of the finished composite plate substrate is 28mm) The finished nickel-based 625+X65M has a width of 1400mm and a length of 15000mm. The key production process steps include:
[0030] 1) Composite plate assembly: Asymmetric assembly is adopted, two rectangular X65M base material billets, one nickel-based 625 billet, and one sealing plate Q235B are selected to complete the processes of blanking, surface grinding, beveling, isolation agent coating, assembly, and billet welding;
[0031] Cutting materials: Two rectangular X65M base material blanks, the size requirements are as follows: the thickness of the lower base material blank is 168mm, the thickness of the upper base material blank is 84mm; one nickel-based 625 blank, the thickness is 10.8mm; the width of the X65M base material blank is 1880mm, the length is 3500mm, the width of the nickel-based 625 is 1480mm, the length is 2800mm; Q235B is used as a sealing plate, which is laid around the composite nickel-based 625 for filling, and the thickness is the same as that of the composite nickel-based 625;
[0032] Surface grinding of substrate: The composite surface of the substrate is ground with a grinding machine to ensure that there is no iron oxide, the substrate has a metallic luster, and there is no oil stain, debris, print stain, etc.;
[0033] Beveling: After two polished substrate surfaces, welding bevels are made around them, with a bevel depth of 40mm and a bevel angle of 30°;
[0034] Apply isolation agent: Apply isolation agent on the contact surface of the multi-layer nickel-based 625 and the upper substrate X65M with a thickness of 0.03mm. Evenly apply it on the entire board surface and then bake it at a baking temperature of 550℃ for 30 minutes.
[0035] Assembly: The thickness direction of the assembly is stacked in the order of upper base material + separator + composite material + lower base material. The composite nickel-based 625 billet is located at the geometric center of the base material, and is welded to the lower base material X65M on both sides along the rolling direction, with a weld width of 20mm. After the assembly machine is hydraulically pressed, ensure that there is no gap between the sealing plate and the base material, and use gas shielded spot welding to secure it.
[0036] Welding billet: After positioning, the composite billet should be fully welded with seal strips. The width of the molten pool is 35mm all around. After welding, two air holes are left at the joint surface of the composite plate billet for vacuum treatment, one at the head and one at the tail in the rolling direction. When the vacuum degree of the composite surface reaches below -0.1Mpa, keep it for 40 minutes. After confirming that the negative pressure of the composite billet is stable, close the vacuum pipe.
[0037] 2) Heating: The composite billet is heated in a furnace within 48 hours after welding, the heating temperature is controlled to be 1150°C, the heating rate is 3min / mm, the total time in the furnace is 526min, and the furnace temperature is 1150°C;
[0038] 3) First stage rolling: the first three passes have a reduction of 30 mm, the first stage rolling end temperature is 1050°C, the first stage cumulative reduction rate is 60%, and the rolling speed is 3.0 m / s;
[0039] 4) Controlled cooling of the intermediate billet: After rough rolling, the intermediate billet is sent to the intermediate roller for laminar cooling. The cooling rate is set at 15°C / s and the outlet water surface temperature is 830°C.
[0040] 5) Second stage rolling: starting rolling temperature 820°C, final rolling temperature 780°C, 7 rolling passes, pass reduction rate is implemented in a pass-by-pass decreasing mode, rolling speed 4.0m / s, and the reduction rates from the last to the third last pass are 3.5%, 4.8%, and 5.0%;
[0041] 6) Controlled cooling: After the third stage of rolling, the steel plate is subjected to controlled cooling treatment, with the initial cooling temperature of 750-760°C, the Mulpic cooling rate of 10°C / s, and the final cooling temperature of the composite plate of 420-450°C;
[0042] 7) Finishing: The composite panels are separated, cleaned, polished, straightened and leveled, and then cut and polished according to the final size of the order before packaging and shipment.
[0043] Example 2: Production of 3+42mm nickel-based 625+X65M composite plate 3+42mm (indicates that the thickness of the finished composite plate composite material nickel-based 625 is 3mm, and the thickness of the finished composite plate substrate is 42mm)
[0044] The chemical composition of nickel-based 625 and pipeline steel X65M is shown in Table 2, with the remainder being Fe and unavoidable impurity elements. The finished product of 3+42mm nickel-based 625+X65M is 3800mm wide and 12000mm long. The key production process steps include:
[0045] 1) Composite plate assembly: Asymmetric assembly is adopted, two rectangular X65M base material billets, one nickel-based 625 billet, and one sealing plate Q235B are selected to complete the processes of blanking, surface grinding, beveling, isolation agent coating, assembly, and billet welding;
[0046] Cutting: Two rectangular X65M base blanks, the size requirements are as follows: the thickness of the lower base blank is 336mm, the thickness of the upper base blank is 168mm; one nickel-based 625 blank, the thickness is 21.6mm; the width of the X65M base blank is 4280mm, the length is 2340mm, the width of the nickel-based 625 is 3880mm, the length is 1690mm; Q235B is used as a sealing plate, which is laid around the composite nickel-based 625 for filling, and the thickness is the same as that of the composite nickel-based 625;
[0047] Surface grinding of substrate: The composite surface of the substrate is ground with a grinding machine to ensure that there is no iron oxide, the substrate has a metallic luster, and there is no oil stain, debris, print stain, etc.;
[0048] Breaking: Two ground substrate surfaces with welding grooves around them, groove depth 40mm, groove angle 30°;
[0049] Apply isolation agent: Apply isolation agent on the contact surface of the composite nickel-based 625 and the upper substrate X65M with a thickness of 0.1mm. Evenly apply it on the entire board surface and then bake it at a baking temperature of 600℃ for 40 minutes.
[0050] Assembly: The thickness direction of the assembly is stacked in the order of upper base material + separator + composite material + lower base material. The composite nickel-based 625 billet is located at the geometric center of the base material, and is welded to the lower base material X65M on both sides along the rolling direction, with a weld width of 30mm. After the assembly machine is hydraulically pressed, ensure that there is no gap between the sealing plate and the base material, and use gas shielded spot welding to secure it;
[0051] Welding billet: After positioning, the composite billet should be fully welded with seal strips. The width of the molten pool on all sides is 40mm. After welding, two air holes are left at the joint surface of the composite plate billet for vacuum treatment, one at the head and one at the tail in the rolling direction. When the vacuum degree of the composite surface reaches below -0.1Mpa, keep it for 45 minutes. After confirming that the negative pressure of the composite billet is stable, close the vacuum pipe.
[0052] 2) Heating: The composite billet is heated in a furnace within 48 hours after welding, the heating temperature is controlled to be 1120°C, the heating rate is 2.5min / mm, the total time in the furnace is 1052min, and the furnace temperature is 1120°C;
[0053] 3) First stage rolling: the first three passes have a reduction of 55 mm, the first stage rolling end temperature is 1060°C, the first stage cumulative reduction rate is 70%, and the rolling speed is 2.0 m / s;
[0054] 4) Controlled cooling of the intermediate billet: After rough rolling, the intermediate billet is sent to the intermediate roller for laminar cooling. The cooling rate is set at 20℃ / s and the outlet water surface temperature is 800℃;
[0055] 5) The second stage of rolling: the starting rolling temperature is 780°C, the final rolling temperature is 750-760°C, the rolling passes are 9, the pass reduction rate is implemented in a pass-by-pass decreasing mode, the rolling speed is 3.0m / s, and the reduction rates from the last to the third last pass are 3.8%, 4.5%, and 4.8% respectively;
[0056] 6) Controlled cooling: After the third stage of rolling, the steel plate is subjected to controlled cooling treatment, with the initial cooling temperature at 720-730°C, the Mulpic cooling rate at 5°C / s, and the final cooling temperature of the composite plate at 350-380°C;
[0057] 7) Finishing: The composite panels are separated, cleaned, polished, straightened and leveled, and then cut and polished according to the final size of the order before packaging and shipment.
[0058] The composite plates of the above two embodiments were subjected to tensile, impact, cold bending, shear strength and intergranular corrosion tests, and the performance test results are shown in Tables 3-4.
[0059] The detection methods of various parameters refer to standards API SPEC 5L, API SPEC 5LD, and DNVGL-ST-F101: Submarine pipeline systems.
[0060] Figure 1 This is a typical metallographic structure photo of the composite plate of Example 1;
[0061] Figure 2 This is the drop hammer morphology of the -30℃ composite plate in Example 1.
[0062] Figure 1 This is a metallographic structure picture of the composite surface. It can be seen that the composite condition is good, and no defects such as delamination and slag inclusion are found in the composite interface; Figure 2 The drop hammer fracture shows good plastic deformation and obvious necking, which proves that the material has good toughness.
[0063] Table 1 Chemical composition (weight, %) of base material pipeline steel X65M and composite material nickel-based 625 in Example 1
[0064]
[0065] Table 2 Chemical composition of base material pipeline steel X65M and composite material nickel-based 625 in Example 2 (weight, %)
[0066]
[0067] Table 3 Mechanical properties test results of the composite plate obtained in Example 1
[0068]
[0069] Table 4 Mechanical properties test results of the composite plate obtained in Example 2
[0070]
[0071] Comparative Example
[0072] Comparative Example 1
[0073] In this comparative example, except that the reduction in the first three passes in step 3) is 20 mm, other operations and parameters are the same as those in Example 1.
[0074] Comparative Example 2
[0075] In this comparative example, except that the reduction in the first three passes in step 3) is 60 mm, other operations and parameters are the same as those in Example 1.
[0076] Comparative Example 3
[0077] In this comparative example, except that the cumulative reduction rate in the first stage in step 3) is 50%, other operations and parameters are the same as those in Example 1.
[0078] Comparative Example 4
[0079] In this comparative example, except that the cumulative reduction rate in the first stage in step 3) is 80%, other operations and parameters are the same as those in Example 1.
[0080] Comparative Example 5
[0081] In this comparative example, except that the cooling rate in step 4) is set to 10°C / s, other operations and parameters are the same as those in Example 1.
[0082] Comparative Example 6
[0083] In this comparative example, except that the cooling rate in step 4) is set to 25°C / s, other operations and parameters are the same as those in Example 1.
[0084] The composite plates of the above comparative examples 1-6 were subjected to tensile, impact, cold bending, shear strength and intergranular corrosion tests, and the performance test results are shown in Table 5.
[0085] The detection methods of various parameters refer to standards API SPEC 5L, API SPEC 5LD, and DNVGL-ST-F101: Submarine pipeline systems.
[0086] Table 5 Mechanical properties test results of nickel-based 625+X65M composite plates obtained in comparative examples 1-6
[0087]
[0088]
Claims
1. A method for producing a nickel-based 625 and pipeline steel X65M composite plate, characterized in that: The composite plate with thickness specification of 30-45mm and width of 1400-3800mm is produced. The yield strength of the obtained material is 460-550Mpa, the tensile strength is 550-620Mpa, the impact at -40℃ is ≥300J, the shear area ratio of -30℃ DWTT is ≥85%, the shear strength is ≥350MPa, and the intergranular corrosion crack rate is 0. The key production process steps include: 1) Composite plate assembly: Asymmetric assembly is adopted, two rectangular X65M base material billets, one nickel-based 625 billet, and one sealing plate Q235B are selected to complete the processes of blanking, surface grinding, beveling, isolation agent coating, assembly, and billet welding; 2) Heating: within 48 hours after the composite billet is welded in step 1), the composite billet is heated in a furnace, the heating temperature is controlled to be 1120-1150° C., the heating rate is ≤3 min / mm, the total time in the furnace is ≥ the thickness of the composite billet (mm)×2.0 (min / mm), and the furnace temperature is 1120-1150° C.; 3) First stage rolling: the first three passes have a reduction of 30-55 mm, the first stage rolling end temperature is ≥1050°C, the first stage cumulative reduction rate is 60%-70%, and the rolling speed is 2.0-3.0 m / s; 4) Controlled cooling of the intermediate billet: After rough rolling, the intermediate billet is sent to the intermediate roller for laminar cooling. The cooling rate is set at 15-20℃ / s and the outlet water surface temperature is 800-830℃; 5) Second stage rolling: starting rolling temperature 780-820°C, final rolling temperature 750-780°C, 7-9 rolling passes, pass reduction rate is implemented in a pass-by-pass decreasing mode, rolling speed 3.0-4.0 m / s, and the reduction rate from the last to the third last pass is ≤5.0%; 6) Controlled cooling: After the third stage of rolling, the steel plate is subjected to controlled cooling treatment, with the initial cooling temperature of 720-760°C, the Mulpic cooling rate of 5-10°C / s, and the final cooling temperature of the composite plate of 350-450°C; 7) Finishing: The composite panels are separated, cleaned, polished, straightened and leveled, and then cut and polished according to the final size of the order before packaging and shipment.
2. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 1, characterized in that: In the step 1), two rectangular X65M substrate blanks are blanked, and the size requirements are as follows: compression ratio of the lower substrate blank (thickness of the lower substrate blank: thickness of the finished composite plate substrate) = 6.0-8.0, thickness of the upper substrate blank = thickness of the lower substrate blank × 0.5; one nickel-based 625 blank, thickness = 0.9 × (thickness of the lower substrate blank ÷ thickness of the finished composite plate substrate) × thickness of the finished composite plate composite nickel-based 625; width of the X65M substrate blank = width of the composite nickel-based 625 blank + 400 mm, length of the X65M substrate blank = length of the composite nickel-based 625 blank + (650-700) mm; Q235B is used as a sealing plate, which is laid around the composite nickel-based 625 for filling, and its thickness is the same as that of the composite nickel-based 625.
3. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 1 or 2, characterized in that: In the step 1), the substrate surface is ground: the composite surface of the substrate is ground with a grinder to ensure that there is no iron oxide scale, the substrate has a metallic luster, and there is no oil stain, debris, or print stain.
4. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 1 or 2, characterized in that: In the step 1), beveling: the two ground substrate surfaces are welded with bevels around them, with a bevel depth of 35-45 mm and a bevel angle of 28-32°.
5. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 1 or 2, characterized in that: In the step 1), a release agent is applied: the contact surface between the composite nickel-based 625 and the upper substrate X65M is coated with a release agent with a thickness of 0.03 to 0.1 mm, and the entire board surface is evenly coated and then baked at a temperature of 550 to 600° C. for 30 to 40 minutes.
6. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 1 or 2, characterized in that: In the step 1), the blanks are assembled: the blanks are stacked in the order of upper substrate blank+isolating agent+composite blank+lower substrate blank in the thickness direction.
7. The method for producing the nickel-based 625 and pipeline steel X65M composite plate according to claim 6, characterized in that: The composite nickel-based 625 billet is located at the geometric center of the base material billet and is welded to the lower base material X65M on both sides along the rolling direction, with a weld width of 20 to 30 mm.
8. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 6, characterized in that: After the assembly machine is hydraulically pressed, ensure that there is no gap between the sealing plate and the base material blank, and use gas shielded spot welding to firmly weld them.
9. The method for producing a composite plate of nickel-based 625 and pipeline steel X65M according to claim 1 or 2, characterized in that: In the step 1), the welded billet: the positioned composite billet is to be fully welded with seal strips, and the molten pool width around it is 35 to 40 mm. After welding, two air holes are left at the joint surface of the composite sheet billet for vacuum treatment, one at the head and one at the tail in the rolling direction. When the vacuum degree of the composite surface reaches below -0.1 Mpa, it is maintained for more than 40 minutes. After confirming that the negative pressure of the composite billet is stable, the vacuum pipe is closed.
Citation Information
Patent Citations
Manufacturing method for rolling titanium-steel composite plate
CN104138903A
Preparation method for asymmetrical wide hot-rolled metal composite plates
CN105458005A
Preparation method of QT-state nickel-based alloy composite plate
CN117816773A
Rolling method of Inconel 625 / X65 composite board
CN118080564A
Pipeline steel plate for alpine regions and preparation method thereof
CN118086650A
Cited By
Bimetal composite plate with X90-level composite layer made of nickel-based alloy Inconel625 and manufacturing method of bimetal composite plate with X90-level composite layer made of nickel-based alloy Inconel625
CN120697385A
Double-metal composite plate with X70-level composite layer made of nickel-based alloy Inconel 625 and manufacturing method of double-metal composite plate
CN120697386A
Preparation method of Inconel 625 nickel-based alloy and X65 pipeline steel composite plate
CN122352679A
Nickel-based corrosion-resistant alloy-steel composite plate and preparation method thereof
CN122558992A
A nickel-based corrosion-resistant alloy-steel clad plate and a preparation method thereof
CN122558992B