Gamma '-phase reinforced high-entropy alloy with high heat-resistant stability and preparation of gamma'-phase reinforced high-entropy alloy

By generating γ' nanoprecipitate phase in high-entropy alloys, the problem of poor thermal stability in high-temperature environments is solved, and high-temperature performance and mechanical properties are improved, making it suitable for high-temperature structural materials.

CN118792564APending Publication Date: 2024-10-18UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410838678.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-18

Smart Images

  • Figure CN118792564A_ABST
    Figure CN118792564A_ABST
Patent Text Reader

Abstract

The invention relates to the field of high-entropy alloy high temperature, in particular to a gamma'phase reinforced high-entropy alloy with high heat-resistant stability and a preparation method thereof.The preparation method comprises the following steps that S1, multiple kinds of metal are selected as raw materials, the metal comprises Ni, Co, Cr, Fe, Al, Ti and Nb, S2, the raw materials are weighed according to the components and the atomic percent and then vacuumized, protective gas is introduced, heating is conducted till the raw materials are molten, molten metal is obtained, and the gamma 'phase reinforced high-entropy alloy with the high heat-resistant stability is obtained; stirring and cooling to obtain a cast ingot; and S3, regular-shape casting, high-temperature solution treatment and rolling deformation treatment are sequentially conducted on the cast ingot, a rolled piece is obtained, recrystallization annealing treatment, aging treatment and cooling are conducted on the rolled piece, and then the gamma'phase strengthened high-entropy alloy with the high heat-resistant stability is obtained. Compared with the prior art, the alloy prepared by the invention has the advantages of high heat-resistant stability, stable grain size and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the high-temperature field of high-entropy alloys, and in particular to a γ′ phase-reinforced high-entropy alloy with high heat resistance stability and a preparation method thereof. Background Art

[0002] Traditional alloys usually use one or two elements as the main elements, and adding a small amount of other elements can adjust the required properties. High entropy alloys break the design concept of traditional alloys. They use four or more elements as the main elements and design the alloy composition according to the equiatomic ratio or near-equiatomic ratio, which brings a large number of alloy systems that have never been developed. High entropy alloys combine high entropy effect, lattice distortion effect, hysteresis diffusion effect, high hardness, high strength, strong plasticity adaptation, high corrosion resistance and other advantages.

[0003] At present, a lot of research has been done on traditional high-temperature structural materials, such as strengthening mechanism, microstructure, creep performance, etc., but there are few reports on the application of high-entropy alloys in high-temperature structural materials. The high-temperature performance of ordinary high-entropy alloys is insufficient. In order to develop new high-temperature structural materials, we can start with the composition design of high-entropy alloys, regulate the element composition, and generate coherent nano-precipitation phases in high-entropy alloys through the alloying effect of elements. The mechanical properties of the alloy are greatly enhanced by nano-precipitation strengthening. However, in a high-temperature environment, due to the poor thermal stability of the unmodified high-entropy alloy, the matrix grains and nano-precipitation phases begin to grow rapidly, resulting in deterioration of the organization, and even the generation of new harmful phases, which rapidly deteriorates the mechanical properties of the alloy and even leads to failure. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a γ′ phase-reinforced high entropy alloy with high heat resistance and stability and its preparation. Through recrystallization and aging treatment, a γ′ nano-precipitate phase is cast on the basis of the γ matrix phase, so that the alloy has excellent high temperature performance.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing a γ′ phase strengthened high entropy alloy with high heat resistance stability comprises the following steps:

[0007] S1: Select a plurality of metals as raw materials, the metals including Ni, Co, Cr, Fe, Al, Ti and Nb,

[0008] S2: Weigh the raw materials according to their components and atomic percentages, evacuate the materials, fill them with protective gas, heat them until they melt, obtain molten metal, stir them, and cool them to obtain an ingot;

[0009] S3: The ingot is sequentially subjected to regular shape casting, high temperature solution treatment, and rolling deformation treatment to obtain a rolled piece, and the rolled piece is subjected to recrystallization annealing treatment, aging treatment, and cooling to obtain the γ′ phase strengthened high entropy alloy with high heat resistance stability.

[0010] Further, in step S1, the components in atomic percentage are:

[0011] Ni: 10-25%, Co: 10-25%, Cr: 10-25%, Fe: 10-25%, Al: 0-6%, Ti: 0-6%, Nb: 0-6%.

[0012] Furthermore, in step S1, the system pressure is not greater than 10 -3 Pa.

[0013] Furthermore, in step S2, the heating temperature is 2500-2800°C.

[0014] Furthermore, in step S2, the cooling method is furnace cooling.

[0015] Furthermore, in step S3, the temperature of the high temperature solution treatment is 1000-1250° C., and the time is 0.5-2 h.

[0016] Furthermore, in step S3, the deformation amount of the rolling deformation treatment is 1-90%.

[0017] Furthermore, in step S3, the temperature of the recrystallization annealing treatment is 1000-1200° C., and the time is 1-10 min.

[0018] Furthermore, in step S3, the aging treatment is performed at a temperature of 600-900°C and for a time of 2-1000 hours.

[0019] A γ′ phase strengthened high entropy alloy with high heat resistance and stability is prepared by the above-mentioned preparation method.

[0020] In order to solve the problem of insufficient thermal stability of high entropy alloys, the present invention proposes to add alloying elements, regulate the alloy composition, reduce the stacking fault energy, and form a coherent nano-precipitation phase in the original matrix of the alloy, and greatly improve the comprehensive performance of the alloy by precipitating the coherent phase. The effect of nano-precipitation phase strengthening depends on the morphology and size of the nano-phase. Therefore, it is very important to improve the thermal stability of the phase. The high entropy effect and lattice distortion effect of the high entropy alloy are enhanced by the solid solution of elements; the energy barrier of diffusion is increased through the synergistic effect between elements, the mutual diffusion between elements is hindered, and the hysteresis diffusion effect is enhanced. The two improve the stability, structural stability, and organizational stability of the phase, reduce the growth rate of matrix grains and nano-phases, and achieve high-temperature strengthening of high entropy alloys. For example, by adding and regulating the refractory element Nb in a high-entropy alloy, a coherent two-phase structure of a nano-precipitate phase γ′ that is coherent with the matrix γ phase is generated, so that the elements are segregated in γ′, which hinders the diffusion between atoms and achieves nano-precipitation strengthening. At the same time, it inhibits phase transformation and the formation of harmful phases, stabilizes the structure and organization, improves the thermal stability of the high-entropy alloy, and enhances the high-temperature performance.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0022] (1) The high entropy alloy in the present invention has a small lattice mismatch, and the interface between the matrix phase and the nano-precipitated phase is a coherent interface. Due to the high entropy effect of the high entropy alloy itself and the interaction between atoms, the element diffusion at high temperature is reduced, and the coarsening rate of the nano-precipitated phase is significantly reduced, which inhibits the growth of the nano-precipitated phase. The mechanical properties are increased while the organizational stability and structural stability are improved. It is a series of high entropy alloys with excellent high-temperature properties, which has a significant impact on the application of high-temperature structural materials.

[0023] (2) In the present invention, the microstructure of the alloy can be controlled by the heat treatment system. The recrystallized alloy is isothermally aged at 600-900°C for 2-1000h at different temperatures. The alloying elements enhance the hysteresis diffusion and lattice distortion effects, hinder atomic diffusion, and significantly reduce the growth rate of the strengthening phase in the alloy compared with the traditional high-temperature alloy. At the same time, due to the pinning effect of the strengthening phase generated after adding the alloying elements on the grain boundaries of the matrix grains, the grains do not grow significantly and the grain size remains stable.

[0024] (3) Compared with traditional high-temperature alloys, the high-entropy alloy with high heat resistance and stability developed in the present invention has a stable grain size during long-term high-temperature heat exposure; the growth rate of the nano-precipitation phase of the high-entropy alloy developed is significantly reduced. The alloy exhibits excellent strengthening structural stability and microstructural heat resistance stability at high temperatures, which also helps to achieve excellent strengthening effects of the alloy at high temperatures, and has engineering value and scientific significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 XRD pattern of the product prepared in Example 1;

[0026] Figure 2 XRD pattern of the product prepared in Example 2;

[0027] Figure 3 This is a SEM image of the product prepared in Example 1;

[0028] Figure 4 This is the SEM image of the product prepared in Example 2;

[0029] Figure 5 This is a statistical diagram of the nano-precipitated phase size of the product prepared in Example 1;

[0030] Figure 6 This is a statistical diagram of the nano-precipitated phase size of the product prepared in Example 2;

[0031] Figure 7 A comparison chart of the growth rate of nano-precipitated phases of the product prepared in Example 1 and other Ni-based high-temperature alloys;

[0032] Figure 8 This is the SEM image of the product prepared in Comparative Example 1 after recrystallization annealing without aging treatment. DETAILED DESCRIPTION

[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0035] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained.

[0036] Example 1-2

[0037] This embodiment provides a γ′ phase strengthened high entropy alloy with high heat resistance stability and a preparation method thereof.

[0038] The following are the selected atoms and their atomic proportions: Ni = 23.5%; Co = 23.5%; Cr = 23.5%; Fe = 23.5%; Al = 1%; Ti = 5%, the expression is (NiCoCrFe) 94 Al1Ti5, the raw materials used are high-purity metals (>99.99%).

[0039] The production steps include:

[0040] (1) Weigh the required elements according to the atomic ratio and expression, and place the metal elements in the vacuum arc melting furnace in the order of the alloy melting point from small to large, and evacuate to 4×10 -4 Pa, high-purity Ar gas is introduced for protection, and then arc is struck to increase the temperature for melting, the heating rate is 500℃ / min, the termination temperature is 2600℃, electromagnetic stirring is turned on during the melting process, the melting time is 15min, and the furnace is cooled after the melting is completed. This step is repeated at least five times to improve the uniformity of the alloy elements. The regular ingot with a size of 5×12×50mm is obtained by suction casting in the last melting.

[0041] (2) placing the regularly sized ingot in a heating furnace and heating it to 1200°C for high temperature solution treatment for 2 hours, followed by cooling by water cooling;

[0042] The ingot after solution treatment is cold rolled to obtain a plate with a deformation of 70%, and then placed in a heating furnace and heated to 1100°C for recrystallization annealing for 3 minutes, followed by cooling by water cooling.

[0043] (3) The recrystallization annealed plates were divided into two groups, placed in a heating furnace and heated to 800°C for aging treatment. The heat treatment time was 24 hours (Example 1) and 480 hours (Example 2), respectively. The cooling method was water cooling to form a γ′ nano-precipitate phase coherent with the matrix, and an alloy plate with a γ / γ′ coherent dual-phase structure was obtained. Experiments have shown that the alloy obtained at different heat treatment times is both γ and γ′ phases, without phase transformation and new phase generation. Figure 1 , 2 It can be seen that at this heat treatment temperature, the growth rate of the resulting γ′ nano-precipitate phase is low. Figure 5 , 6 It can be seen that the board has good thermal stability and excellent high temperature performance.

[0044] The sheet metal is mechanically cut using a high-speed wire EDM machine to obtain components of the desired shape.

[0045] like Figure 1 , 2 As shown, it is the XRD diagram of the products prepared in Example 1 and Example 2, proving that they are composed of two phases, γ phase and γ′ phase, and the phases are stable;

[0046] like Figure 3 , 4 As shown, it is the SEM picture of the products prepared in Example 1 and Example 2, and the nano-precipitated phase has a good morphology.

[0047] like Figure 5 , 6As shown, it is a statistical diagram of the nano-precipitated phase size of the products prepared in Example 1 and Example 2, and the nano-precipitated phases all have small sizes.

[0048] like Figure 7 As shown, the coarsening rate of the nano-precipitation phase of the high entropy alloy obtained by the method of Example 1 is compared with that of other Ni-based high-temperature alloys. The coarsening rate of the nano-precipitation phase of Example 1 is significantly reduced, and the grain size of the alloy remains stable.

[0049] Example 3

[0050] This embodiment provides a γ′ phase strengthened high entropy alloy with high heat resistance stability and a preparation method thereof.

[0051] The following are the selected atoms and their atomic proportions: Ni = 23.5%; Co = 23.5%; Cr = 23.5%; Fe = 23.5%; Al = 2%; Ti = 4%, the expression is (NiCoCrFe) 94 Al2Ti4, the raw materials used are high-purity metals (>99.99%).

[0052] The production steps include:

[0053] (1) Weigh the required elements according to the atomic ratio and expression, and place the metal elements in a certain order in a vacuum arc melting furnace, and evacuate to 4×10 -4 Pa, high-purity Ar gas was introduced for protection, and then arc was ignited to increase the temperature for melting, the heating rate was 500℃ / min, the end temperature was 2600℃, electromagnetic stirring was turned on during the melting process, the melting time was 15min, and the furnace was cooled after the melting was completed.

[0054] This step was repeated at least five times to improve the uniformity of alloy elements, and a regular ingot with a size of 5×12×50 mm was obtained by suction casting in the last smelting.

[0055] (2) placing the regularly sized ingot in a heating furnace and heating it to 1200°C for high temperature solution treatment for 2 hours, followed by cooling by water cooling;

[0056] The ingot after solution treatment is cold rolled to obtain a plate with a deformation of 70%, and then placed in a heating furnace and heated to 1100°C for recrystallization annealing for 3 minutes, followed by cooling by water cooling.

[0057] (3) The recrystallization annealed plates were divided into two groups, placed in a heating furnace and heated to 700°C for aging treatment. The heat treatment time was 240 hours respectively, and the cooling method was water cooling to form a γ′ nano-precipitate phase coherent with the matrix, and an alloy plate with a γ / γ′ coherent dual-phase structure was obtained. Experiments have shown that the alloys obtained after heat treatment are all γ and γ′ phases, without phase transformation and new phase generation, and the growth rate of the obtained γ′ nano-precipitate phase is low. Experiments have shown that the alloys obtained under different heat treatment times are all γ and γ′ phases, without phase transformation and new phase generation, and the growth rate of the obtained γ′ nano-precipitate phase is low. The plate has good thermal stability and excellent high-temperature performance.

[0058] The sheet metal is mechanically cut using a high-speed wire EDM machine to obtain components of the desired shape.

[0059] Example 4

[0060] This embodiment provides a γ′ phase strengthened high entropy alloy with high heat resistance stability and a preparation method thereof.

[0061] The following are the selected atoms and their atomic proportions: Ni = 23.5%; Co = 23.5%; Cr = 23.5%; Fe = 23.5%; Al = 3%; Ti = 3%, the expression is (NiCoCrFe) 94 Al3Ti3, the raw materials used are high-purity metals (>99.99%).

[0062] The production steps include:

[0063] (1) Weigh the required elements according to the atomic ratio and expression, and place the metal elements in a certain order in a vacuum arc melting furnace, and evacuate to 4×10 -4 Pa, high-purity Ar gas was introduced for protection, and then arc was ignited to increase the temperature for melting, the heating rate was 500℃ / min, the end temperature was 2600℃, electromagnetic stirring was turned on during the melting process, the melting time was 15min, and the furnace was cooled after the melting was completed.

[0064] This step was repeated at least five times to improve the uniformity of alloy elements, and a regular ingot with a size of 5×12×50 mm was obtained by suction casting in the last smelting.

[0065] (2) placing the regularly sized ingot in a heating furnace and heating it to 1200°C for high temperature solution treatment for 2 hours, followed by cooling by water cooling;

[0066] The ingot after solution treatment is cold rolled to obtain a plate with a deformation of 70%, and then placed in a heating furnace and heated to 1100°C for recrystallization annealing for 3 minutes, followed by cooling by water cooling.

[0067] (3) The recrystallization annealed plates were divided into two groups and placed in a heating furnace and heated to 700°C for aging treatment. The heat treatment time was 240 h and the cooling method was water cooling to form a γ′ nano-precipitate phase coherent with the matrix, thereby obtaining an alloy plate with a γ / γ′ coherent dual-phase structure. Experiments have shown that the alloys obtained at different heat treatment times are both γ and γ′ phases, without phase transformation and new phase generation, and the growth rate of the obtained γ′ nano-precipitate phase is low. The plate has good thermal stability and excellent high-temperature performance.

[0068] The sheet metal is mechanically cut using a high-speed wire EDM machine to obtain components of the desired shape.

[0069] Comparative Example 1

[0070] This comparative example provides a γ′ phase strengthened high entropy alloy with high heat resistance stability and a preparation method thereof. The difference from the process of Example 1 is that step (3) is omitted and only recrystallization treatment is performed. Figure 8 As shown, this is the SEM image of the product prepared in this embodiment after recrystallization annealing without aging treatment. Figure 8 It can be seen that the high entropy alloy without heat treatment after recrystallization annealing is in a recrystallized state, the grains grow again, the structure becomes a homogeneous structure, and no nano-precipitate phase or other new phases can be produced.

[0071] Comparative Example 1, as Figure 3 As shown, the recrystallized annealed high entropy alloy forms a nano-precipitation phase after heat treatment, which makes the alloy nano-precipitation strengthened and improves the performance of the material.

[0072] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability, characterized in that: The following steps are involved: S1: Select a plurality of metals as raw materials, the metals including Ni, Co, Cr, Fe, Al, Ti and Nb, S2: Weigh the raw materials according to their components and atomic percentages, evacuate the materials, fill them with protective gas, heat them until they melt, obtain molten metal, stir them, and cool them to obtain an ingot; S3: The ingot is sequentially subjected to regular shape casting, high temperature solution treatment, and rolling deformation treatment to obtain a rolled piece, and the rolled piece is subjected to recrystallization annealing treatment, aging treatment, and cooling to obtain the γ' phase strengthened high entropy alloy with high heat resistance stability.

2. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S1, the components in atomic percentage are: Ni: 10-25%, Co: 10-25%, Cr: 10-25%, Fe: 10-25%, Al: 0-6%, Ti: 0-6%, Nb: 0-6%.

3. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S1, the system pressure is not greater than 10 -3 Pa.

4. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S2, the heating temperature is 2500-2800°C.

5. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S2, the cooling method is furnace cooling.

6. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S3, the temperature of the high temperature solution treatment is 1000-1250°C and the time is 0.5-2h.

7. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S3, the deformation amount of the rolling deformation treatment is 1-90%.

8. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S3, the temperature of the recrystallization annealing treatment is 1000-1200° C., and the time is 1-10 min.

9. The method for preparing a γ' phase strengthened high entropy alloy with high heat resistance stability according to claim 1, characterized in that: In step S3, the aging treatment is performed at a temperature of 600-900°C and for a time of 2-1000 hours.

10. A γ' phase strengthened high entropy alloy with high heat resistance and stability, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Necklace-shaped heterostructure high-entropy alloy and preparation method thereof

    CN119776711A

  • Kovar alloy with high tensile ductility and tensile strength and preparation method

    CN120330604A

  • High tensile ductility and tensile strength can alloy and method of making

    CN120330604B