Detection method for decarburized layer of quenched and tempered steel
By using anti-decarburization coating in a resistance furnace and performing normalizing treatment, the steel structure is transformed into ferrite + pearlite, which solves the accuracy and applicability problems in the existing technology in detecting the depth of the decarburization layer of quenched + tempered steel. , achieving efficient and accurate detection results.
Patent Information
- Application Number
- CN202410867347.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-22
AI Technical Summary
It is difficult to efficiently and accurately detect the decarburization depth of quenched + tempered steel under the existing heating equipment conditions in the laboratory with existing technology. Especially when using ordinary resistance furnaces, the measurement accuracy and repeatability are poor, and conventional methods cannot Suitable for hypoeutectoid steel and steel types with higher hardenability.
Apply anti-decarburization paint and perform normalizing treatment in a resistance furnace. Through isothermal or medium-temperature normalizing treatment, the sample structure is transformed into ferrite + pearlite, combined with metallographic microscope measurement to ensure the accuracy of detection. degree and applicability.
It effectively avoids decarburization during normalizing treatment and improves the accuracy of test results. It is suitable for ordinary resistance furnaces and has high heating efficiency. It is suitable for daily production testing, especially for steel types with high hardenability.
Smart Images

Figure CN118817675A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of decarburization layer detection, in particular to a method for detecting a decarburization layer on the surface of a steel material after quenching and tempering treatment. Background Art
[0002] Quenching can greatly improve the hardness, wear resistance and other properties of steel. However, there are great stress and brittleness in the quenched workpiece. If tempering is not carried out in time, it is easy to deform or even crack. Therefore, quenching often needs to be used in conjunction with tempering. Tempering parts at different temperatures will not only reduce the stress and brittleness of the quenched parts, but also adjust the mechanical properties of the parts. For example, quenching + low-temperature tempering can transform its metallographic structure into tempered martensite, so that the parts can achieve good wear resistance, so it is widely used in carburized gears, tools and other wear-resistant parts; quenching + medium-temperature tempering can transform its metallographic structure into tempered troostite, so as to obtain a higher elastic limit and yield point, so it is widely used in clockwork, springs, etc.; quenching + high-temperature tempering is quenching and tempering treatment, which transforms the metallographic structure into tempered troostite, so as to obtain good comprehensive mechanical properties, so it is widely used in shafts, connecting rods, etc.
[0003] However, after quenching and tempering at different temperatures, carbon loss will occur on the surface of steel, which is called decarburization. Decarburization will cause soft spots on the surface of parts, reduce the mechanical properties of parts, and affect their service life. Therefore, the detection of decarburization layer of parts is particularly important. At present, the most widely used method for detecting the depth of decarburization layer is metallographic method.
[0004] The metallographic method is based on the change in the sample surface to the matrix as the carbon content changes. In hypoeutectoid steel, it is distinguished by the relative content change of ferrite (white structure) and other structural components. This method is mainly suitable for steel with balanced structure (ferrite + pearlite) obtained by annealing or normalizing.
[0005] However, after quenching + tempering at different temperatures, the change in the structure of the steel is relatively unobvious due to carbon loss, which increases the difficulty of measuring the decarburized layer and greatly reduces the accuracy of the decarburized layer measurement. This is mainly related to the structural changes of the steel after the above-mentioned heat treatment. As the carbon content in austenite increases, the stability of austenite increases, and the position of the C curve moves to the right. However, because the cooling rate of quenching is very fast, only when a certain degree of decarburization is formed on the surface (when the C content is lost more), can it show significantly different structural characteristics after quenching + tempering at different temperatures. Therefore, directly using the metallographic method to detect the decarburized layer of the workpiece in the quenched + tempered state will cause its measured value to be much smaller than the actual depth of the decarburized layer. In addition, since the boundary between the quenched + tempered state structures is not obvious, the position of the organizational boundary line always changes, the repeatability is poor, and the accurate measurement of the decarburized layer cannot be guaranteed.
[0006] Therefore, when measuring the depth of decarburization layer, steel that has been quenched and tempered at different temperatures often needs to be normalized. After normalizing, the quenched and tempered state structure is transformed into ferrite + pearlite. At this time, the boundary of the organizational change caused by carbon loss is obvious and easy to distinguish. However, re-normalizing will lead to an increase in the decarburization layer, which will also incorrectly guide production personnel to adjust the production process. Therefore, it is very important to improve the heat treatment conditions so that decarburization does not occur further.
[0007] In the prior art, Patent No. CN117089802A mainly provides a heating process for a controlled atmosphere heating furnace to detect the depth of the decarburization layer of bearing steel. This heat treatment process is for bearing steel. However, for hypoeutectoid steel, especially for steels with high hardenability, the conventional air cooling method cannot obtain a balanced structure (ferrite + pearlite). And the atmosphere parameters used in the above patent are not suitable for hypoeutectoid steel. Moreover, for the more commonly used ordinary resistance furnace, atmosphere protection cannot be achieved and the decarburization layer measurement requirements cannot be met.
[0008] Therefore, under the existing heating equipment conditions in the laboratory, how to efficiently and accurately detect the decarburization depth of quenched + tempered steel is an urgent problem to be solved. Summary of the invention
[0009] The technical problem to be solved by the present invention is to propose a decarburization layer detection method which is simple to operate and can be widely used in ordinary resistance furnaces based on the existing detection technology difficulties, and has the advantages of high detection efficiency, good repeatability and high measurement accuracy.
[0010] In order to solve the above technical problems, the present invention adopts the following technical scheme: a method for detecting the decarburization layer of quenched and tempered steel, comprising the following steps: (1) sampling, the workpiece in the quenched and tempered state is intercepted and cut according to the sampling requirements specified in GB / T224-2019 standard by using a band saw with cutting fluid or a metallographic cutting machine to obtain a sample; (2) applying anti-decarburization coating, the anti-decarburization coating is applied on the surface of the sample; (3) normalizing treatment, according to the characteristics of the steel, the sample coated with the anti-decarburization coating is placed in a resistance furnace for normalizing heat treatment; (4) sample preparation, the sample after heat treatment is ground, polished and etched to obtain a metallographic sample; (5) measuring the depth of the decarburization layer, the metallographic sample is placed under a metallographic microscope, and the depth of the decarburization layer on its surface is measured.
[0011] Furthermore, isothermal normalizing treatment is performed on the steel with high hardenability, and the isothermal normalizing treatment steps are as follows: put the steel into a resistance furnace at a temperature of 830℃-880℃ and keep it warm for 20min-30min; take out the kept warm sample from the furnace, transfer it to a furnace at 650℃-690℃ and keep it warm for 10min; air cool it; and transform the sample structure into a balanced structure of ferrite + pearlite.
[0012] Furthermore, for steel with low hardenability, the normalizing treatment steps are: placing in a resistance furnace at a temperature of 830°C-880°C, keeping warm for 20min-30min; air cooling; and transforming the sample structure into a balanced structure of ferrite + pearlite.
[0013] Furthermore, the steel is selected as 42CrMoA.
[0014] Furthermore, the steel is selected as 60Si2Cr.
[0015] Furthermore, the sample preparation process requires water cooling to prevent burns on the grinding surface of the sample.
[0016] Furthermore, the grinding process includes flat grinding, rough grinding, and fine grinding processes;
[0017] Furthermore, during the erosion process, the sample needs to be kept shaking to ensure uniform erosion of the sample.
[0018] The beneficial effects of the present invention are:
[0019] The present invention includes brushing anti-decarburization coating on the surface of the sample, which effectively avoids further decarburization during normalizing treatment to improve the accuracy of the detection result, and is also applicable to widely used ordinary resistance furnace heating equipment to improve its practicality.
[0020] The present invention includes an isothermal normalizing heat treatment process for steels with higher hardenability. This isothermal normalizing treatment can completely transform the structure of the steels with higher hardenability into ferrite + pearlite after heat treatment. It is easy to operate and has high heat treatment efficiency, and can meet the requirements of daily production testing. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0022] Figure 1 is a metallographic structure diagram of a 42CrMoA sample in a quenched + high-temperature tempered state coated with an anti-decarburization coating according to Example 1 of the present invention, after isothermal normalizing treatment, wherein (a) is a metallographic structure diagram of the surface decarburization layer after isothermal normalizing, and (b) is a metallographic structure diagram of the sawn surface after isothermal normalizing.
[0023] Figure 2 This is the metallographic structure diagram of the sawn surface of the 42CrMoA sample in the quenching + high temperature tempering state in Example 1 without anti-decarburization coating after isothermal normalizing treatment.
[0024] Figure 3 It is the metallographic structure diagram of the surface decarburization layer of 42CrMoA sample in quenching + high temperature tempering state without any heat treatment.
[0025] Figure 4 is a metallographic structure diagram of a 60Si2Cr sample in a quenched + medium-temperature tempered state coated with an anti-decarburization coating according to Example 2 of the present invention, after normalizing, wherein (a) is a metallographic structure diagram of the surface decarburization layer after normalizing, and (b) is a metallographic structure diagram of the sawn surface after normalizing.
[0026] Figure 5 This is the metallographic structure diagram of the sawn surface of the 60Si2Cr sample in Example 2 which is not coated with anti-decarburization coating and is in the quenched + medium-temperature tempered state after normalizing treatment.
[0027] Figure 6 This is the metallographic structure diagram of the surface decarburization layer of the 60Si2Cr sample in the quenching + medium-temperature tempering state without any heat treatment. DETAILED DESCRIPTION
[0028] The present invention will now be described in further detail with reference to the accompanying drawings.
[0029] Example 1
[0030] Detection method of decarburized layer of 42CrMoA specimen in quenching + high temperature tempering state after isothermal normalizing treatment.
[0031] In accordance with the requirements of GB / T224-2019 standard, a metallographic cutting machine is used to saw and sample 42CrMoA bars in the quenched + high-temperature tempered state. The sample height is 15mm-20mm, and the total surface detection circumference is ≥35mm. During the sampling process, cutting fluid is required for cooling to prevent burns on the cutting surface; a layer of anti-decarburization coating is applied on the surface of the cut sample, and then the sample is placed in a furnace at 850°C and kept warm for 20 minutes; then, the sample is transferred to a furnace with a temperature of 650°C, kept warm for 10 minutes, and then air-cooled.
[0032] After the heat-treated sample is ground flat on the grinder, it is first coarsely ground with 400# sandpaper, then finely ground with 800# sandpaper, and finally polished on velvet cloth. The entire sample preparation process needs to be cooled with water to prevent the sample from being burned on the grinding surface;
[0033] After the sample is polished, the polished surface is immersed in 4% nitric acid alcohol etching solution for etching. During the etching process, the sample needs to be slightly shaken to ensure uniform etching of the sample. The etching time is about 10 seconds.
[0034] The etched sample was placed on a metallographic microscope for observation, and the depth of the surface decarburization layer was measured according to the change in the ferrite (white structure) content, that is, the depth of the decarburization layer of the 42CrMoA sample in the quenching + high-temperature tempering state. It was observed that no decarburization occurred on the cut surface after isothermal normalizing treatment.
[0035] Comparative Example 1, in accordance with the requirements of GB / T224-2019 standard, a metallographic cutting machine was used to saw and sample the 42CrMoA rod in the state, the sample height was 15mm-20mm, and the total surface detection circumference was ≥35mm. During the sampling process, cutting fluid was required to cool the cutting surface to prevent burns on the cutting surface; no anti-decarburization coating was applied to it, and then it was placed in a heating furnace together with the sample of Example 1, and isothermal normalizing treatment and metallographic sample preparation were performed in the same manner.
[0036] After isothermal normalizing treatment, the sample structure is transformed into ferrite + pearlite, as shown in Figure 1(a). Compared with the 42CrMoA sample after direct grinding (the metallographic structure of the decarburized layer is shown in Figure 1(b)), the sample structure is transformed into ferrite + pearlite, as shown in Figure 1(c) and the sample structure is transformed into ferrite + pearlite, as shown in Figure 1(d) Figure 3 ), due to the change of surface carbon content to matrix carbon content, the organizational change is more obvious, easy to distinguish, and convenient to measure the depth of decarburization layer. After quenching treatment, part of the organizational difference caused by carbon deficiency will be covered up, so the result of directly using a metallographic microscope to measure the depth of decarburization layer will be low. The decarburization layer depth of 42CrMoA measured by the method of this embodiment 1 is 0.20mm, while the 42CrMoA sample directly ground without isothermal normalizing treatment has a decarburization layer depth of 0.12mm; by comparing the metallographic organization diagrams of the cut surface of the sample coated with anti-decarburization coating and the sample not coated with anti-decarburization coating after isothermal normalizing treatment, it is found that the cut surface of the sample not coated with anti-decarburization coating has obvious decarburization layer, while the cut surface of the sample coated with anti-decarburization coating has no decarburization phenomenon after the same isothermal normalizing treatment, as shown in Figures 1(b) and Figure 2 .
[0037] Example 2
[0038] Detection method of decarburized layer of 60Si2Cr spring in quenching + medium temperature tempering state after normalizing treatment.
[0039] In accordance with the requirements of GB / T224-2019 standard, a metallographic cutting machine is used to saw and sample the 60Si2Cr spring in the quenched + medium-temperature tempered state. The sample height is 15mm-20mm, and the total surface inspection circumference is ≥35mm. During the sampling process, cutting fluid is required for cooling to prevent burns on the cutting surface; a layer of anti-decarburization coating is applied on the surface of the cut sample, and then the sample is placed in a furnace at 850℃, kept warm for 20 minutes, and then taken out for air cooling.
[0040] After the heat-treated sample is ground flat on a grinder, it is coarsely ground with 400# sandpaper, then finely ground with 800# sandpaper, and finally polished on a velvet cloth. The entire sample preparation process requires cooling with water to prevent burns on the grinding surface of the sample;
[0041] After the sample is polished, the polished surface is immersed in 4% nitric acid alcohol etching solution for etching. During the etching process, the sample needs to be slightly shaken to ensure uniform etching of the sample. The etching time is about 10 seconds.
[0042] The etched sample was placed on a metallographic microscope for observation, and the depth of the surface decarburization layer was measured according to the change in the ferrite (white structure) content, that is, the decarburization layer depth of the 60Si2Cr spring in the quenching + medium-temperature tempering state. It was observed that no decarburization occurred on the cut surface after heat treatment.
[0043] Comparative Example 2, in accordance with the requirements of GB / T224-2019 standard, a metallographic cutting machine was used to saw and sample the 60Si2Cr spring in the quenched + medium-temperature tempered state. The sample height was 15mm-20mm, and the total surface detection circumference was ≥35mm. During the sampling process, cutting fluid was required for cooling to prevent burns on the cutting surface; the surface was not coated with anti-decarburization coating, and then it was placed in a heating furnace together with the sample of Example 2, and normalizing treatment and metallographic sample preparation were performed in the same manner.
[0044] After normalizing treatment, the sample structure is transformed into ferrite + pearlite, as shown in Figure 4 (a). Compared with the 60Si2Cr sample in the state of direct grinding quenching + medium temperature tempering (the metallographic structure of the decarburized layer is shown in Figure 6 ), although there is obvious white ferrite structure due to carbon loss on the surface, after quenching, it will cover up some of the organizational differences caused by carbon deficiency, so the result of directly measuring the decarburization layer depth using a metallographic microscope will be low. The decarburization layer depth of 60Si2Cr measured by the method of Example 2 is 0.40mm, while the decarburization layer depth of 60Si2Cr sample directly ground in the quenching + medium-temperature tempering state without normalizing treatment is 0.17mm; by comparing the metallographic structure diagrams of the cut surface of the sample coated with anti-decarburization coating and the sample not coated with anti-decarburization coating after normalizing treatment, it is found that the cut surface of the sample not coated with anti-decarburization coating has obvious decarburization layer, while the cut surface of the sample coated with anti-decarburization coating does not undergo decarburization after the same normalizing treatment, as shown in Figures 4(b) and Figure 5 .
[0045] In summary, the method for detecting the decarburization layer of quenched and tempered steel in the present invention involves adding anti-decarburization coating protection, which effectively avoids further decarburization during normalizing treatment to improve the accuracy of the detection results, and is also applicable to commonly used ordinary resistance furnace heating equipment, thereby improving practicality.
[0046] The heat treatment process involved in the detection method of the decarburized layer of quenched + tempered steel in the present invention is based on the C curve of the steel grade and the existing equipment conditions of the laboratory, especially for steel grades with higher hardenability, which not only ensures that they can be completely converted into ferrite + pearlite, but also facilitates the operation of heat treatment personnel. The heat treatment time is also shortened as much as possible under the premise of ensuring the heat treatment effect, so as to improve the detection efficiency.
[0047] The above is based on the ideal embodiment of the present invention. Through the above description, relevant staff can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for detecting decarburized layer of quenched and tempered steel, characterized in that: The following steps are involved: (1) Sampling: The workpiece in the quenched and tempered state is cut and cut using a band saw or metallographic cutting machine with cutting fluid to obtain a sample in accordance with the sampling requirements specified in GB / T224-2019; (2) Apply anti-decarburization paint on the surface of the sample; (3) Normalizing treatment: according to the characteristics of steel, the sample coated with anti-decarburization coating is placed in a resistance furnace for normalizing heat treatment; (4) sample preparation, grinding, polishing and etching the heat-treated sample to obtain a metallographic sample; (5) Measure the depth of the decarburized layer. Place the metallographic sample under a metallographic microscope and measure the depth of the decarburized layer on its surface.
2. The method for detecting the decarburized layer of quenched and tempered steel according to claim 1, characterized in that: Isothermal normalizing treatment is performed on steel with high hardenability. The steps of isothermal normalizing treatment are as follows: put the steel into a resistance furnace at a temperature of 830℃-880℃ and keep it warm for 20min-30min; take the kept warm sample out of the furnace and transfer it to a furnace at 650℃-690℃ and keep it warm for 10min; and air cool it.
3. The method for detecting the decarburized layer of quenched and tempered steel according to claim 1, characterized in that: For steel with low hardenability, the normalizing treatment steps are: put it into a resistance furnace with a temperature of 830℃-880℃, keep it warm for 20min-30min; air cool it.
4. The method for detecting the decarburized layer of quenched and tempered steel according to claim 2, characterized in that: The steel selected is 42CrMoA.
5. The method for detecting the decarburized layer of quenched and tempered steel according to claim 3, characterized in that: The steel selected is 60Si2Cr.
6. A method for detecting decarburized layer of quenched and tempered steel according to any one of claims 1 to 5, characterized in that: The sample preparation process requires water cooling.
7. A method for detecting decarburized layer of quenched and tempered steel according to any one of claims 1 to 5, characterized in that: The grinding process includes flat grinding, rough grinding and fine grinding.
8. A method for detecting decarburized layer of quenched and tempered steel according to any one of claims 1 to 5, characterized in that: During the erosion process, the sample needs to be kept agitated.
Citation Information
Cited By
Low-carbon steel hot-rolled wire rod and decarburized layer depth measuring method thereof
CN122038916A
Low-carbon steel hot-rolled rod and method for measuring decarburized layer depth thereof
CN122038916B