Resin composition

By using resin compositions with specific structural units and solvent combinations, the problems of insufficient filtration and transparency in the manufacturing process of polyimide resins were solved, enabling the formation of highly efficient polyimide films suitable for display processes.

CN118852618APending Publication Date: 2024-10-29ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410506189.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-25
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the prior art, the solvent of polyimide resin does not have sufficient filterability and low YI (transparency) properties during the manufacturing process, which cannot meet the requirements of display manufacturing.

Method used

A resin composition containing specific structural units is used, along with a combination of a primary solvent and a secondary solvent. The Hansen solubility parameter of the secondary solvent is within a specific range, and the proportion of the secondary solvent is controlled within a certain range. A silicon-containing compound is added as a monomer to form a polyimide film suitable for display processes.

Benefits of technology

It improves the filterability and low YI properties of the resin composition, making it suitable for LTPS and LTPO display processes, and forms a polyimide film with good transparency and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852618A_ABST
    Figure CN118852618A_ABST
Patent Text Reader

Abstract

Provided is a resin composition containing a resin containing a structural unit represented by general formula (1) and / or general formula (2) and a structure derived from a silicon-containing compound represented by general formula (3), and a solvent containing a main solvent and an auxiliary solvent, the main solvent containing at least one type selected from the group consisting of NMP, DMF, DMAc, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, 1, 3-propylene glycol, and 1, 3-propylene glycol. The auxiliary solvent comprises 2, 3-dimethyl imidazolidone, tetramethylurea, 3-methoxy-N, N-dimethyl propionamide, 3-butoxy-N, N-dimethyl propionamide, gamma-butyrolactone, gamma-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, methylpyridine and pyridine, and Hansen solubility parameters of the auxiliary solvent meet the following conditions: delta D is equal to 16.5 to 18.9, delta P is equal to 0.1 to 8.2, delta H is equal to 1.1 to 5.5, and delta D is equal to 0.1 to 8.2. # imgabs0 # wherein the total amount of the solvent is 100 mass% and the auxiliary solvent is less than 50 mass%
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a display using the resin composition, a method for producing the resin composition, a polyimide resin film, a display, and a method for producing a laminate. Background Art

[0002] Polyimide resin is an insoluble, infusible, super heat-resistant resin having excellent properties such as thermal oxidation resistance, heat resistance, radiation resistance, low temperature resistance, and chemical resistance. Therefore, polyimide resin is used in a wide range of fields including electronic materials.

[0003] Examples of applications of polyimide resins in the field of electronic materials include insulating coating materials, insulating films, semiconductors, and electrode protective films for thin film transistor liquid crystal displays (TFT-LCDs).

[0004] Recently, studies have been conducted on using polyimide films as flexible substrates, taking advantage of their lightness and flexibility, to replace glass substrates that have been conventionally used in the field of display materials.

[0005] In particular, in recent years, materials such as LTPS (Low-temperature polysilicon) and LTPO (Low-temperature polycrystalline oxide) that can withstand high-temperature processes above 400°C have been sought.

[0006] One form of polyimide for display use is to ship to display manufacturers in a varnish state, where it is formed into a film. The production process of the varnish includes a filtration step for removing impurities, etc., but good filterability is required from the perspective of productivity.

[0007] For example, Document 1 discloses a polyimide composition containing butyl benzoate as an aromatic solvent and γ-butyrolactone (hereinafter also referred to as GBL) as a polar solvent.

[0008] For example, Document 2 discloses an insulating coating material in which N-methylpyrrolidone (hereinafter also referred to as NMP) is used as a main solvent and butylbenzene is used as a subsolvent as a solvent of a polyamide-imide varnish.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2010-155895

[0012] Patent Document 2: Chinese Patent Application Publication No. 102559040 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] However, the solvents used in the above-mentioned patent documents do not have sufficient filterability (filtration rate) required when producing polyimide.

[0015] Furthermore, the varnish of the above-mentioned patent document is not sufficient from the viewpoint of achieving both the properties required for display applications (low YI (transparency) and filterability, etc.).

[0016] Therefore, an object of the present invention is to provide a resin composition for forming a polyimide film applicable to a display process, which uses a silicon-containing compound as a monomer and has both filterability and low YI (transparency) applicable to a resin manufacturing process.

[0017] Another object of the present invention is to provide a display obtained by using the resin composition, and methods for producing the resin composition, the polyimide resin film, the display, and the laminate.

[0018] Solutions for solving problems

[0019] That is, the above-mentioned problems can be solved by the following technical means.

[0020] [Item 1]

[0021] A resin composition comprising a resin and a solvent, wherein the resin comprises a structural unit represented by the following general formula (1) and / or general formula (2), and comprises a structure derived from a silicon-containing compound represented by the following general formula (3),

[0022]

[0023] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.}

[0024]

[0025] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.}

[0026]

[0027] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.}

[0028] The aforementioned solvent includes a main solvent and an auxiliary solvent.

[0029] The main solvent comprises at least one selected from the group consisting of the following solvents:

[0030] N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, methylpyridine and pyridine,

[0031] The Hansen solubility parameters of the aforementioned co-solvents satisfy the following:

[0032] δD=16.5~18.9、

[0033] δP=0.1~8.2、

[0034] δH=1.1~5.5,

[0035] When the total amount of the solvent is 100% by mass, the auxiliary solvent is less than 50% by mass.

[0036] [Item 2]

[0037] The resin composition according to item 1, wherein the Hansen solubility parameter of the auxiliary solvent satisfies the following:

[0038] δD=16.5~18.4、

[0039] δP=0.1~5.6、

[0040] δH=1.1~4.7.

[0041] [Item 3]

[0042] The resin composition according to item 1 or 2, wherein the auxiliary solvent comprises a solvent selected from the group consisting of n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4- At least one of the group consisting of eucalyptol, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenyl acetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate and benzyl benzoate.

[0043] [Item 4]

[0044] The resin composition according to item 1 or 2, wherein the auxiliary solvent comprises a solvent selected from the group consisting of n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexyl At least one of the group consisting of benzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, tolan, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, α-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-tert-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene and 2-propylstyrene.

[0045] [Item 5]

[0046] The resin composition according to item 1 or 2, wherein the auxiliary solvent has a boiling point lower than 250°C.

[0047] [Item 6]

[0048] The resin composition according to item 1 or 2, wherein the auxiliary solvent comprises at least one selected from the group consisting of n-butylbenzene and ethoxybenzene.

[0049] [Item 7]

[0050] The resin composition according to any one of items 1 to 6, wherein P1 and / or P3 contains a structural unit derived from the following general formula (4).

[0051]

[0052] [Item 8]

[0053] The resin composition according to any one of items 1 to 7, wherein P2 and / or P4 contains a structural unit derived from the following general formula (5).

[0054]

[0055] [Item 9]

[0056] The resin composition according to any one of items 1 to 8, wherein P1 and / or P3 contains a structural unit derived from the following general formula (6).

[0057]

[0058] [Item 10]

[0059] The resin composition according to any one of items 1 to 9, wherein the auxiliary solvent is 5% by mass or more and 40% by mass or less, when the total amount of the solvent is 100% by mass.

[0060] [Item 11]

[0061] The resin composition according to any one of items 1 to 9, wherein the auxiliary solvent is 5% by mass or more and 30% by mass or less, when the total amount of the solvent is 100% by mass.

[0062] [Item 12]

[0063] The resin composition according to any one of items 1 to 11, which is used for a substrate of a flexible display.

[0064] [Item 13]

[0065] A display comprising a thin film transistor (TFT) substrate and / or a color filter substrate obtained using the resin composition according to any one of items 1 to 12.

[0066] [Item 14]

[0067] A method for producing a resin composition, wherein the resin composition contains a resin and a solvent, wherein the resin contains a structural unit represented by the following general formula (1) and / or general formula (2), and contains a structure derived from a silicon-containing compound represented by the following general formula (3),

[0068]

[0069] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.}

[0070]

[0071] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.}

[0072]

[0073] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.}

[0074] The method for preparing the resin composition comprises:

[0075] A step of synthesizing the resin using at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, picoline and pyridine as a main solvent; and

[0076] A process for preparing a resin composition by adding a co-solvent satisfying the following Hansen solubility parameters after synthesizing the aforementioned resin and before filtering.

[0077] δD=16.5~18.9、

[0078] δP=0.1~8.2、

[0079] δH=1.1~5.5.

[0080] [Item 15]

[0081] A method for producing a polyimide resin film, comprising:

[0082] a coating step of coating the resin composition described in any one of items 1 to 12 or the resin composition obtained by the method described in item 14 on the surface of the support,

[0083] a film forming step of heating the resin composition to form a polyimide resin film;

[0084] a peeling step of peeling the polyimide resin film from the support; and

[0085] The irradiation treatment is performed by irradiating the polyimide resin film with laser light from the support side before the peeling step.

[0086] [Item 16]

[0087] A method for manufacturing a display, comprising:

[0088] a coating step of coating the resin composition described in any one of items 1 to 12 or the resin composition obtained by the method described in item 14 on the surface of the support;

[0089] a film forming step of heating the resin composition to form a polyimide resin film;

[0090] an element forming step of forming an element on the polyimide resin film; and

[0091] The peeling step is to peel the polyimide resin film on which the element is formed from the support.

[0092] [Item 17]

[0093] A method for manufacturing a laminate, comprising:

[0094] a coating step of coating the resin composition described in any one of items 1 to 12 or the resin composition obtained by the method described in item 14 on the surface of the support;

[0095] a film forming step of heating the resin composition to form a polyimide resin film; and

[0096] The device forming step is to form a device on the polyimide resin film.

[0097] [Item 18]

[0098] A method for manufacturing a laminate, comprising:

[0099] a coating step of coating the resin composition described in any one of items 1 to 12 or the resin composition obtained by the method described in item 14 on the surface of the support;

[0100] a film forming step of heating the resin composition to form a polyimide resin film;

[0101] an element forming step of forming an element on the polyimide resin film; and

[0102] A peeling step of peeling the polyimide resin film on which the element is formed from the support.

[0103] [Item 19]

[0104] A resin composition comprising a resin and a solvent, wherein the resin comprises a structural unit represented by the following general formula (1) and / or general formula (2), and comprises a structure derived from a silicon-containing compound represented by the following general formula (3),

[0105]

[0106] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.}

[0107]

[0108] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.}

[0109]

[0110] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.}

[0111] The aforementioned solvent comprises one or more mixed solvents,

[0112] The Hansen solubility parameters of the aforementioned mixed solvents satisfy the following:

[0113] δD=16.8~18.8、

[0114] δP=6.8~9.8、

[0115] δH=4.5~6.8.

[0116] Effects of the Invention

[0117] According to the present invention, a polyimide-containing resin composition can be provided which uses a silicon-containing compound as a monomer and has both filterability and low YI (transparency) properties applicable to a resin production process.

[0118] Specifically, it is possible to provide a resin composition for forming a polyimide film that has both filterability and low YI (transparency) and can be applied to display processes such as LTPS (low temperature polycrystalline silicon) and LTPO (low temperature polycrystalline oxide).

[0119] The present invention can also provide a display using the resin composition, and methods for producing the resin composition, the polyimide resin film, the display, and the laminate.

[0120] It should be noted that the above description cannot be regarded as disclosing all embodiments of the present invention and all advantages related to the present invention. Other embodiments of the present invention and their advantages will be clarified by referring to the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0121] Figure 1 This is a schematic diagram showing the structure of a top emission type flexible organic EL display as an example of the display according to the present embodiment, above the polyimide substrate.

[0122] Description of Reference Numerals

[0123] 2a lower base plate

[0124] 2b Sealing substrate

[0125] 25Organic EL structure

[0126] 250a Organic EL element emitting red light

[0127] 250b Organic EL element emitting green light

[0128] 250c Organic EL element that emits blue light

[0129] 251 partition wall (embankment)

[0130] 252 lower electrode (anode)

[0131] 253 Hole transport layer

[0132] 254 luminous layer

[0133] 255 upper electrode (cathode)

[0134] 256TFT

[0135] 257 contact holes

[0136] 258 interlayer insulation film

[0137] 259 Lower electrode

[0138] 261 Hollow DETAILED DESCRIPTION

[0139] Hereinafter, an exemplary embodiment of the present invention (hereinafter referred to as "the present embodiment") is described in detail. The present invention is not limited to the present embodiment, and various modifications can be made within the scope of the present invention. In the present specification, the upper limit and lower limit of each numerical range can be arbitrarily combined.

[0140] 《Resin composition》

[0141] In one embodiment, the resin composition of the present embodiment is a resin composition comprising a resin and a solvent described later, wherein the resin comprises a structural unit represented by the following general formula (1) and / or general formula (2).

[0142]

[0143] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.}

[0144] The number p of repeating units in the general formula (1) is not particularly limited and may be an integer of 2 to 150.

[0145]

[0146] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.}

[0147] The number q of repeating units in the general formula (2) is not particularly limited and may be an integer of 2 to 150.

[0148] In one embodiment, the resin composition of the present embodiment is a resin composition comprising a resin and a solvent, wherein the resin comprises a structural unit represented by the following general formula (1) and / or general formula (2), and comprises a structure derived from a silicon-containing compound described later and represented by the following general formula (3).

[0149]

[0150] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.}

[0151] The number p of repeating units in the general formula (1) is not particularly limited and may be an integer of 2 to 150.

[0152]

[0153] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.}

[0154] The number q of repeating units in the general formula (2) is not particularly limited and may be an integer of 2 to 150.

[0155]

[0156] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.}

[0157] The solvent includes a main solvent and an auxiliary solvent.

[0158] The main solvent comprises at least one selected from the group consisting of the following solvents:

[0159] N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, methylpyridine and pyridine,

[0160] The Hansen solubility parameters of the co-solvents are described as follows:

[0161] δD=16.5~18.9、

[0162] δP=0.1~8.2、

[0163] δH=1.1~5.5,

[0164] When the total amount of the solvent is 100% by mass, the auxiliary solvent is less than 50% by mass.

[0165] 〈Polyimide precursor / polyimide〉

[0166] As long as the resin contained in the resin composition of the present embodiment contains the structural unit represented by the general formula (1) and / or (2), its structure can be used without particular limitation. Hereinafter, the resin containing the structural unit represented by the general formula (1) is referred to as a polyimide precursor, and the resin containing the structural unit represented by the general formula (2) is referred to as a polyimide, and the components constituting the resin and the components constituting the resin composition are described.

[0167] The polyimide is obtained by thermal imidization of a polyimide precursor (including a polyimide precursor partially imidized), or by chemical imidization. From the viewpoint of transparency of the obtained polyimide film, thermal imidization is preferred. In addition, the resin composition may contain an imidization accelerator.

[0168] In the resin having the structures of the general formula (1) and the general formula (2), when the structure derived from the general formula (1) (amide unit) is set to L (mol) and the structure derived from the general formula (2) (imide unit) is set to M (mol), the ratio of L to M, i.e., L / M, is (5 mol% / 95 mol%) to (95 mol% / 5 mol%), and preferably (10 mol% / 90 mol%) to (90 mol% / 10 mol%).

[0169] From the viewpoint of storage stability of the resin composition, the molar fraction of the imide unit M is preferably 5 mol % or more, more preferably 10 mol % or more, further preferably 15 mol % or more, particularly preferably 20 mol % or more.

[0170] From the viewpoint of suppressing turbidity / whitening of the resin composition, the molar fraction of the amide unit L is preferably 95 mol % or less, more preferably 90 mol % or less, further preferably 85 mol % or less, particularly preferably 80 mol % or less.

[0171] The ratio L / M of L to M can be calculated not only from the charge amounts of the monomers and the synthesis conditions, but also by the following method.

[0172] The obtained resin composition (for example, a polyimide precursor partially imidized) was measured. 13C-NMR. In addition, all the polyimide precursors and all the polyimide resins were synthesized using the same monomers as the monomers constituting the resin in the same ratio (mol%), and the respective resins were measured in the same manner. 13 C-NMR: L / M can be calculated by comparing the integrated values ​​of the obtained spectra (for example, the integrated value of the peak of C of the carbonyl group of the amide / imide bond).

[0173] (Diamine)

[0174] In the general formulae (1) and (2), P1 and P3 are each independently preferably a structure derived from the following diamine.

[0175] For example, examples of diamines include 9,9-bis(4-aminophenyl)fluorene (BAFL), p-phenylenediamine (pPD), m-phenylenediamine (mPD), 3,3'-diaminodiphenyl sulfone (3,3-DAS), 4,4'-diaminodiphenyl sulfone (4,4-DAS), 3,5-diaminobenzoic acid, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether, 4-aminophenyl-4'-aminobenzoate (APAB), 4,4'-diaminobenzanilide ... 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10 -Bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl)hexafluoropropane and 1,4-bis(3-aminopropyldimethylsilyl)benzene, 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene (BiSAM), 1,4-cyclohexanediamine (CHDA) and 4,4-diaminodiphenyl ether (ODA), etc.

[0176] These diamines may be used alone or in combination of two or more.

[0177] Among these, from the viewpoint of being applicable to LTPS (low temperature polycrystalline silicon) and LTPO (low temperature polycrystalline oxide) processes and achieving both low YI (transparency) and low Rth of the resulting polyimide film, preferably at least one selected from the group consisting of 9,9-bis(4-aminophenyl)fluorene (BAFL), p-phenylenediamine (pPD), m-phenylenediamine (mPD), 3,3'-diaminodiphenyl sulfone (3,3-DAS), 4,4'-diaminodiphenyl sulfone (4,4-DAS), 3,5-diaminobenzoic acid and 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether is used, and more preferably 9,9-bis(4-aminophenyl)fluorene (BAFL), 3,3'-diaminodiphenyl sulfone (3,3-DAS) and 4,4'-diaminodiphenyl sulfone (4,4-DAS).

[0178] In the present application, YI (yellowness index) refers to the depth of yellow of the color of the polyimide resin film, and the lower the value, the higher the transparency of the polyimide resin film.

[0179] From the viewpoint of transparency, the polyimide film obtained from the resin composition of the present embodiment has a YI value of preferably 16 or less, more preferably 13 or less, further preferably 10 or less, particularly preferably 5 or less, and most preferably 3 or less when the film thickness is 10 μm.

[0180] In addition, the YI of the resin composition was measured by the method described in the Examples.

[0181] It should be noted that in the present application, Rth refers to the thickness-direction delay when the resin composition is made into a film. In the case of a display (specifically, a bottom-emitting OLED, liquid crystal, transmissive display, under-screen imaging camera, etc.) in which an image is observed and recognized or a photographed object is photographed through a polyimide resin film (with the human eye or a camera, etc.), the closer the Rth value is to 0, the lower the value is, which is preferred.

[0182] The Rth (converted to a film thickness of 10 μm) was determined by measuring five locations of each sample using a phase difference birefringence measuring device (manufactured by Oji Scientific Instruments Co., Ltd., product name: KOBRA-WR) (wavelength of measuring light: 589 nm).

[0183] In addition, in the above resin, P1 and / or P3 preferably includes a structural unit derived from the following general formula (4).

[0184]

[0185] When the resin includes a structural unit derived from the formula (4), it is preferred because low YI, high heat resistance, and low Rth can be achieved while maintaining the solvent solubility of the resin.

[0186] On the other hand, if the proportion of the general formula (4) in the resin in the resin composition of the present embodiment is high, there is a tendency for poor chemical resistance. The reason is still uncertain, but it can be considered that this is because the compound of the general formula (4) has an alicyclic part, and the chemical resistance of this part is poor. Similarly, there is also a tendency for poor chemical resistance in resins using alicyclic monomers (such as CpODA, etc.).

[0187] In the resin, P1 and / or P3 preferably includes a structural unit derived from the following general formula (6).

[0188]

[0189] Such a resin is preferred from the viewpoint of transparency (low yellowness: low YI in one embodiment) and low Rth of the obtained resin.

[0190] (Acid dianhydride)

[0191] In the above general formulae (1) and (2), P2 and P4 are each independently preferably a structure derived from the following acid dianhydride.

[0192] For example, examples of the acid dianhydride include 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), pyromellitic anhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic anhydride (BPDA), 4,4'-oxydiphthalic anhydride (ODPA), norbornane 2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic anhydride (CpODA), 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2-dicarboxylic anhydride, 1,2,3,4-benzenetetracarboxylic anhydride, 3,3 ',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethylidene-4,4'-diphthalic dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, p-phenylene diphthalic dianhydride (trimellitic anhydride), thio-4,4'-diphthalic anhydride, sulfonyl-4,4'-diphthalic anhydride, 1,3-bis(3,4-dicarboxyphenyl)phthalic anhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic anhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic anhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy) 1,2,7,8-phenanthrenetetracarboxylic dianhydride; 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA); and 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA);

[0193] The compound shown in the following structure (BzDA):

[0194]

[0195] The compound represented by the following structure (BNBDA), etc.

[0196]

[0197] Among these acid dianhydrides, from the viewpoint of being applicable to LTPS (low-temperature polycrystalline silicon) and LTPO (low-temperature polycrystalline oxide) processes and achieving both low YI and low Rth of the resulting polyimide film, preferred are 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF) represented by the following general formula (5), pyromellitic anhydride (PMDA) and 3,3',4,4'-biphenyltetracarboxylic anhydride (BPDA), and more preferred is BPAF.

[0198] In one embodiment, a polyimide resin composition containing 4,4'-oxydiphthalic dianhydride (ODPA) can be cured at a low temperature of about 260° C. to form a polyimide resin film. Therefore, 4,4'-oxydiphthalic dianhydride (ODPA) is preferred as the acid dianhydride.

[0199] These acid dianhydrides may be used alone or in combination of two or more.

[0200] In the resin composition of the present embodiment, P2 and / or P4 may include a structural unit derived from the general formula (5).

[0201]

[0202] Furthermore, in the resin composition of the present embodiment, P2 and / or P4 may include a structural unit derived from the following general formula (7).

[0203]

[0204] In one embodiment, in the resin composition of the present embodiment, P1 and / or P3 include at least a structural unit derived from the general formula (4), and P2 and / or P4 may include a structural unit derived from the general formula (5).

[0205] In one embodiment, in the resin composition of the present embodiment, the structural unit derived from the general formula (4) may be 80 mol% or less of all diamine monomers, or the structural unit derived from the general formula (5) may be 15 mol% or more of all acid dianhydride monomers.

[0206] By setting the structural units derived from the general formula (4) to less than 80 mol % of all diamine monomers, the resulting polyimide film can achieve low YI, and by setting the structural units derived from the general formula (5) to more than 15 mol % of all acid dianhydride monomers, the resulting polyimide film can achieve high heat resistance and high Young's modulus.

[0207] In the resin composition of the present embodiment, P1 and / or P3 include at least a structural unit derived from the general formula (3) described below, and P2 and / or P4 may include a structural unit derived from the general formula (7).

[0208] In one embodiment, in the resin composition of the present embodiment, P1 and / or P3 contain at least one structural unit derived from the general formula (3) and the general formula (4), and P2 and / or P4 contain a structural unit derived from the general formula (5). The structural unit derived from the general formula (3) can be set to 20 mol% or more of all diamine monomers.

[0209] By setting the structural unit derived from the general formula (3) to 20 mol % or more in all diamine monomers, the resulting polyimide film can have low YI and low Rth.

[0210] In one embodiment, in the resin composition of the present embodiment, P1 and / or P3 may contain at least one structural unit derived from general formula (3) and general formula (4), and P2 and / or P4 may contain at least one structural unit derived from general formula (5) and general formula (7).

[0211] 〈Silicon-containing compounds〉

[0212] The resin in the present embodiment, in particular, the structural unit of the general formula (2) may include a structure derived from a silicon-containing compound represented by the following general formula (3).

[0213]

[0214] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.}

[0215] Therefore, the silicon-containing compound used for the synthesis of the polyimide precursor in the present embodiment may be a compound having a reactive group capable of co-condensing with at least one of tetracarboxylic dianhydride and diamine.

[0216] Examples of the silicon-containing compound in the present embodiment include compounds represented by the following formula (17) (hereinafter also simply referred to as (17)).

[0217]

[0218] {where,

[0219] R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms;

[0220] R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R2 and R3 is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms;

[0221] R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R4 and R5 is a monovalent aromatic group having 6 to 10 carbon atoms;

[0222] R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R6 and R7 is an organic group having 2 to 10 carbon atoms and containing an unsaturated aliphatic hydrocarbon group;

[0223] L1 and L2 are each independently a monovalent organic group containing an acid anhydride structure, an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group or a mercapto group;

[0224] i is an integer from 1 to 200;

[0225] j and k are each independently an integer from 0 to 200, j is an integer from 1 to 200; and

[0226] 0≤j / (i+j+k)≤0.50, which satisfies the relationship 0.05≤j / (i+j+k)≤0.50.}

[0227] R1 in formula (17) is independently a single bond or a divalent organic group having 1 to 10 carbon atoms. The divalent organic group having 1 to 10 carbon atoms may be linear, cyclic or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group).

[0228] When R1 is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, examples thereof include straight-chain or branched alkylene groups such as methylene (in one embodiment, trimethylene), ethylene, propylene (in one embodiment, n-propylene and isopropylene), butylene (in one embodiment, n-butylene, sec-butylene and tert-butylene), pentylene (in one embodiment, n-pentylene and neopentylene), n-hexylene, n-heptylene, n-octylene, n-nonylene and n-decylene;

[0229] Cycloalkylene groups such as cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, cycloheptylene and cyclooctylene.

[0230] When R1 is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, it is preferably at least one selected from the group consisting of a trimethylene group, an ethylene group, a n-propylene group, and an isopropylene group.

[0231] When R1 is an unsaturated aliphatic hydrocarbon group, specifically, it may be an alkenyl group or an allyl group.

[0232] In the formula (17), R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R2 and R3 is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms.

[0233] The monovalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group).

[0234] For example, when R2 and R3 are monovalent organic groups having 1 to 10 carbon atoms, examples thereof include straight-chain or branched-chain alkyl groups such as methyl, ethyl, propyl (in one embodiment, n-propyl or isopropyl), butyl (in one embodiment, n-butyl, sec-butyl or tert-butyl), pentyl (in one embodiment, n-pentyl or neopentyl), n-hexyl, n-heptyl, n-octyl, n-nonyl or n-decyl.

[0235] Cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl;

[0236] Aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl and β-naphthyl, etc.

[0237] The monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group).

[0238] For example, when R2 and R3 are monovalent aliphatic hydrocarbon groups having 1 to 5 carbon atoms, examples thereof include straight-chain or branched-chain alkyl groups such as methyl, ethyl, propyl (in one embodiment, n-propyl or isopropyl), butyl (in one embodiment, n-butyl, sec-butyl or tert-butyl), and pentyl (in one embodiment, n-pentyl or neopentyl);

[0239] Cycloalkyl groups such as cyclopropyl, cyclobutyl and cyclopentyl, etc.

[0240] When R2 and R3 are monovalent aliphatic hydrocarbon groups having 1 to 5 carbon atoms, they are preferably at least one selected from the group consisting of a methyl group, an ethyl group, and an n-propyl group.

[0241] In the formula (17), R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R4 and R5 is a monovalent aromatic group having 6 to 10 carbon atoms.

[0242] The monovalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group).

[0243] For example, when R4 and R5 are monovalent organic groups having 1 to 10 carbon atoms, examples thereof include straight-chain or branched-chain alkyl groups such as methyl, ethyl, propyl (in one embodiment, n-propyl or isopropyl), butyl (in one embodiment, n-butyl, sec-butyl or tert-butyl), pentyl (in one embodiment, n-pentyl or neopentyl), n-hexyl, n-heptyl, n-octyl, n-nonyl and n-decyl.

[0244] Cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl;

[0245] Aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl and β-naphthyl, etc.

[0246] When R4 and R5 are monovalent aromatic groups having 6 to 10 carbon atoms, examples thereof include phenyl, tolyl, xylyl, α-naphthyl and β-naphthyl, and preferably at least one selected from the group consisting of phenyl, tolyl and xylyl.

[0247] In formula (17), R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R6 and R7 is preferably an organic group having 2 to 10 carbon atoms and having an unsaturated aliphatic hydrocarbon group.

[0248] The monovalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group).

[0249] When R6 and R7 are monovalent organic groups having 1 to 10 carbon atoms, examples thereof include straight-chain or branched-chain alkyl groups such as methyl, ethyl, propyl (in one embodiment, n-propyl or isopropyl), butyl (in one embodiment, n-butyl, sec-butyl or tert-butyl), pentyl (in one embodiment, n-pentyl or neopentyl), n-hexyl, n-heptyl, n-octyl, n-nonyl or n-decyl;

[0250] Cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl;

[0251] Aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl and β-naphthyl, etc.

[0252] When R6 and R7 are monovalent organic groups having 1 to 10 carbon atoms, they are preferably at least one selected from the group consisting of a methyl group, an ethyl group, and a phenyl group.

[0253] The organic group having an unsaturated aliphatic hydrocarbon group may be an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, and may be linear, cyclic, or branched.

[0254] When R6 and R7 are unsaturated aliphatic hydrocarbon groups having 2 to 10 carbon atoms, examples thereof include alkenyl groups such as vinyl, allyl, 1-propenyl, butenyl (in one embodiment, 3-butenyl and 2-butenyl), pentenyl, hexenyl, heptenyl, octenyl, nonenyl and decenyl;

[0255] Alkynyl groups such as ethynyl, propynyl, butynyl, pentynyl and hexynyl;

[0256] Cycloalkenyl groups such as cyclopentenyl and cyclohexenyl.

[0257] When R6 and R7 are unsaturated aliphatic hydrocarbon groups having 2 to 10 carbon atoms, they are preferably at least one selected from the group consisting of vinyl, allyl and 3-butenyl.

[0258] Some or all of the hydrogen atoms in R1 to R7 in the formula (17) may be substituted with a substituent such as a halogen atom such as F, Cl, or Br, or may be unsubstituted.

[0259] L1 and L2 in formula (17) are each independently a monovalent organic group containing an acid anhydride structure (also referred to as an acid anhydride group), an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group or a mercapto group.

[0260] Examples of the monovalent organic group including an acid anhydride structure include a 2,5-dioxotetrahydrofuran-3-yl group represented by the following formula.

[0261]

[0262] {Wherein, “*” represents a connecting bond.}

[0263] Among these, an amino group and an acid anhydride group are preferred, and an amino group is more preferred from the viewpoint of viscosity stability of the resin composition.

[0264] The alkoxy group in the alkoxycarbonyl group may be an alkoxy group having 1 to 6 carbon atoms, and examples thereof include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, and tert-butoxy.

[0265] The halogen atom in the halocarbonyl group is preferably a halogen atom other than a fluorine atom, and more preferably a chlorine atom or an iodine atom.

[0266] i in formula (17) is an integer of 1-200, preferably an integer of 2-100, more preferably an integer of 4-80, and further preferably an integer of 8-40.

[0267] In formula (17), j and k are each independently an integer of 0 to 200, j is preferably an integer of 1 to 200, j and k are more preferably integers of 0 to 50, and even more preferably integers of 0 to 20.

[0268] In the formula (17), 0≤j / (i+j+k)≤0.50, preferably 0.05≤j / (i+j+k)≤0.50 is satisfied.

[0269] From the viewpoint of filterability of the resin composition of the present application, the functional group equivalent of the silicon-containing compound represented by formula (17) is preferably 800 or more, more preferably 1000 or more, and even more preferably 1500 or more.

[0270] On the other hand, when the functional group equivalent is 500 or less, the filterability tends to be poor.

[0271] Here, the functional group equivalent mentioned in the present application refers to the molecular weight of the silicon-containing compound per 1 mol of the functional group (unit: g / mol). The functional group equivalent can be measured by a known method according to existing standards or the like.

[0272] In addition, it is preferred that the functional group equivalent of the silicon-containing compound is 800 or more because the residual stress of the polyimide film in a nitrogen atmosphere is small. This is believed to be because when the functional group equivalent is a specific value or more, the organic silicon region increases and the stress is relaxed.

[0273] In addition, the filterability (filtration rate) of the resin composition of the present application was measured by the method described in the Examples.

[0274] If the resin in the resin composition of the present application has a structure derived from formula (17), the residual stress of the polyimide film measured in a nitrogen atmosphere becomes small, and the performance is good, so it is preferred. The reason for measuring in a nitrogen atmosphere is that: in the manufacturing process of a display, when an inorganic film such as SiO and SiN is formed on the polyimide film, it is sometimes exposed to a nitrogen atmosphere, and the residual stress in a nitrogen atmosphere is required to be small.

[0275] From the viewpoint of monomer type and cost and the viewpoint of increasing the molecular weight of the obtained polyimide precursor, the silicon-containing compound having a structure represented by the general formula (17) is preferably a silicon-containing diamine.

[0276] As the silicon-containing diamine, for example, diamino (poly)siloxane represented by the following formula (18) is preferred.

[0277]

[0278] {In the formula, P5 each independently represents a divalent hydrocarbon group having 1 to 10 carbon atoms, and may be the same or different, P3 and P4 are the same as R2 and R3 defined in the general formula (17), and l represents an integer of 1 to 200.}

[0279] Preferred structures of P3 and P4 in the general formula (18) include methyl, ethyl, propyl, butyl and phenyl groups, among which methyl is preferred.

[0280] In addition, P5 in the general formula (18) may be a trimethylene group (-CH2CH2CH2-).

[0281] In the general formula (18), l is an integer of 1 to 200, and is preferably an integer of 3 to 200 from the viewpoint of heat resistance of a polyimide obtained by using the silicon-containing diamine represented by the general formula (18).

[0282] The preferred range of the functional group equivalent of the compound represented by the general formula (18) is the same as that of the silicon-containing compound represented by the general formula (17).

[0283] The copolymerization ratio of the silicon-containing diamine is preferably 0.5 to 30% by mass, more preferably 1.0 to 25% by mass, and further preferably 1.5 to 20% by mass, based on the total mass of the polyimide precursor / polyimide.

[0284] When the content of the silicon-containing diamine is 0.5% by mass or more, the residual stress generated between the silicon-containing diamine and the support described below can be effectively reduced.

[0285] When the silicon-containing diamine content is 30% by mass or less, it is preferred because the transparency of the obtained polyimide film is good from the viewpoint of achieving low haze, high total light transmittance and high glass transition temperature (hereinafter referred to as Tg).

[0286] The silicon-containing compound as a monomer used for the polyimide precursor / polyimide may be synthesized using the common technical knowledge at the time of filing the application as described above, or a commercially available product may be used.

[0287] Examples of commercially available products include: methylphenyl silicone oil modified with amines at both ends: X22-1660B-3 (functional group equivalent: 2200), X22-9409 (functional group equivalent: 670) (both manufactured by Shin-Etsu Chemical Co., Ltd.);

[0288] Methylphenyl silicone oil modified with anhydride at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-168-P5-B (functional group equivalent: 2100));

[0289] Both-end epoxy-modified methylphenyl silicone oil (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-2000 (functional group equivalent: 620));

[0290] Dimethyl silicone modified with amino groups at both ends: PAM-E (functional group equivalent weight 130), X22-161A (functional group equivalent weight 800), X22-161B (functional group equivalent weight 1500), KF8012 (functional group equivalent weight 2200) (all manufactured by Shin-Etsu Chemical Co., Ltd.);

[0291] Made by Toray Dow Corning: BY16-853U (functional group equivalent weight 450);

[0292] Made by JNC: Silaplane FM3311 (number average molecular weight: 1000);

[0293] Both-end epoxy-modified dimethyl silicone (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-163A (functional group equivalent weight: 1750);

[0294] Both-end alicyclic epoxy-modified dimethyl silicone (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-169B (functional group equivalent weight: 1700));

[0295] Dimethyl silicone modified with hydroxyl groups at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: KF-6000);

[0296] Dimethyl silicone modified with mercapto groups at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-167B (functional group equivalent: 1700));

[0297] Dimethyl silicone modified with anhydride at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-168A (functional group equivalent: 1000)) and the like.

[0298] Among these, dimethyl silicone oils modified with amines at both ends are preferred from the viewpoints of price, improvement of chemical resistance, and improvement of Tg.

[0299] 〈Solvent〉

[0300] The resin composition of the present embodiment includes a solvent. In one embodiment, the solvent includes a main solvent and a sub-solvent.

[0301] Main solvent

[0302] In the present application, the main solvent refers to the component with the largest mass relative to the total amount of solvents including the main solvent and the auxiliary solvent, and the auxiliary solvent refers to the component with the smallest mass relative to the total amount of solvents including the main solvent and the auxiliary solvent.

[0303] When the total amount of the solvent is 100% by mass, the content of the main solvent is 50% by mass or more, preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0304] As the main solvent of the present application, a solvent which has good solubility of the polyimide / polyimide precursor and can appropriately control the solution viscosity of the resin composition of the present application is preferably used.

[0305] In the present application, for example, the main solvent includes at least one selected from the group consisting of amides such as N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide and hexamethylphosphoramide; lactones such as 1,3-dimethylimidazolidinone, tetramethylurea, γ-butyrolactone and γ-valerolactone; dimethyl sulfoxide, cyclopentane, methylpyridine and pyridine.

[0306] These main solvents may be used alone or in combination of two or more. Among them, it is preferred that the main solvent contains at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), hexamethylphosphoramide, and N,N-dimethylacetamide.

[0307] Specific examples of the composition of the main solvent include N-methyl-2-pyrrolidone (NMP) when one type is used alone, or combinations of N-methyl-2-pyrrolidone (NMP) and γ-butyrolactone (GBL), GBL and dimethyl sulfoxide, and GBL and 3-methoxy-N,N-dimethylpropionamide when two types are used in combination (e.g., main solvent 1 and main solvent 2). The mass ratio when two types of main solvents are used in combination is preferably main solvent 1:main solvent 2 = 10:90 to 90:10.

[0308] The mass ratio of NMP to GBL may be, for example, NMP:GBL=10:90 to 90:10, and is preferably 50:50.

[0309] The numerical range of the Hansen solubility parameter (hereinafter also referred to as SP value) of the main solvent is not particularly limited as long as the monomer as a raw material of the polyimide and the polymer as a product can be dissolved.

[0310] In one embodiment, as the main solvent, the Hansen solubility parameters may be in the range of δD=16.5 to 19.0, δP=8.0 to 17.5, and δH=5.7 to 12.3.

[0311] When the SP value of the main solvent is within the above range, the solubility of the polyimide / polyimide precursor is good. In addition, when the main solvent is used as a synthesis solvent used in synthesizing the resin of the present application, the molecular weight of the polyimide / polyimide precursor can be increased, which is preferred.

[0312] ·Co-solvent

[0313] As the auxiliary solvent, the following solvent is preferred: Hansen solubility parameters are in the range of δD=16.5-18.9, δP=0.1-8.2, δH=1.1-5.5, when mixed with the main solvent, the solubility of the polyimide / polyimide precursor is good, and the solution viscosity of the resin composition of the present application can be appropriately controlled. When the SP value of the auxiliary solvent is within the above range, the filterability of the resin composition can be improved.

[0314] It should be noted that two or more solvents may be mixed and used as a co-solvent. The Hansen solubility parameter in this case is calculated by multiplying the Hansen solubility parameter of each solvent by the volume fraction (vol %) of each solvent.

[0315] When the Hansen solubility parameter of the auxiliary solvent is in the following range, filterability is better and therefore it is preferred.

[0316] δD=16.5~18.4

[0317] δP=0.1~5.6

[0318] δH=1.1~4.7

[0319] In the present application, a mixed solvent refers to a solvent containing one or more main solvents and one or more auxiliary solvents. The resin composition of the present embodiment may contain a solvent containing one or more mixed solvents.

[0320] Furthermore, when the Hansen solubility parameters of the mixed solvent containing the main solvent and the auxiliary solvent are in the following ranges: δD = 16.8 to 18.8, δP = 6.8 to 9.8, and δH = 4.5 to 6.8, the resin composition has good filterability, which is preferred. It is believed that good filterability is related to the Hansen solubility parameters of the polymer constituting the resin.

[0321] Hansen Solubility Parameters are parameters developed by Charles M. Hansen as a method of predicting whether a substance will dissolve in other substances to form a solution. They are based on the idea that similar substances dissolve when they are bound in the same way as a molecule defined as "similar" to other molecules. Specifically, each molecule is assigned the following three Hansen Solubility Parameters, each in MPa 0.5 .

[0322] δD: Energy from the dispersion force between molecules

[0323] δP: Energy derived from the dipole intermolecular forces between molecules

[0324] δH: Energy derived from hydrogen bonds between molecules.

[0325] These three parameters can be treated as coordinates of three-dimensional points also known as Hansen space. The closer two molecules are in this three-dimensional space, the more likely they are to dissolve in each other.

[0326] It should be noted that the SP values ​​of the main solvent and the auxiliary solvent were measured by the method described in the Examples.

[0327] When the main solvent or auxiliary solvent is a combination of two or more solvents, the solubility parameter is a value calculated based on the respective solvents and their charging ratio.

[0328] The present inventors have found that a polyimide precursor obtained by using a specific main solvent and an auxiliary solvent that fully satisfies a specific Hansen solubility parameter, in particular, has excellent properties required for display applications, such as filterability and low YI (transparency).

[0329] In addition, by using a specific auxiliary solvent in a specific ratio, a polyimide-containing resin composition applicable to displays (especially displays using LTPS (low temperature polycrystalline silicon) and LTPO (low temperature polycrystalline oxide)) can be provided.

[0330] Specific examples of the auxiliary solvent include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, benzyl Ethyl phthalate, propyl benzoate, diphenyl acetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, toluene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-tert-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene and 2-propylstyrene, n-butyl benzoate and dibutyl sebacate, etc.

[0331] These auxiliary solvents may be used alone or in combination.

[0332] Examples of the auxiliary solvent having a more preferred SP value include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, toluene, diphenyl acetylene, dibutyl sebacate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, and 4-tert-butylstyrene.

[0333] By using these solvents as auxiliary solvents, the filterability of the resin composition of the present embodiment is improved, which is preferred.

[0334] In one embodiment, from the viewpoint that the filtration speed is not easily reduced as the filtration time passes, the auxiliary solvent of the present application preferably includes a solvent selected from the group consisting of n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate , tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenyl acetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate and benzyl benzoate. At least one of the group consisting of.

[0335] In one embodiment, the auxiliary solvent of the present invention is selected from n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate The polyimide obtained by using at least one of the group consisting of propyl benzoate, diphenyl acetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, α-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-tert-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene and 2-propylstyrene is preferred from the viewpoint of low YI.

[0336] When the boiling point of the auxiliary solvent of the present application is above 250°C, it can also be suitably used as the auxiliary solvent of the present embodiment. However, when a resin is added to the auxiliary solvent to prepare a polyimide resin composition and the composition is heated to form a polyimide resin film, the YI value can be reduced. Therefore, the boiling point of the auxiliary solvent of the present application is preferably lower than 250°C.

[0337] Examples of the auxiliary solvent having a boiling point of 250° C. or higher include tolan, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, butyl benzoate, and butyl sebacate.

[0338] Examples of auxiliary solvents having a boiling point lower than 250° C. include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, Esters, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-tert-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene and 2-propylstyrene, etc.

[0339] Among the auxiliary solvents, at least one selected from the group consisting of n-butylbenzene and ethoxybenzene is particularly preferred from the viewpoint of being able to achieve both filterability and a low YI value.

[0340] From the viewpoint of both the filterability of the resin composition and the low YI of the polyimide resin film, when the total amount of the solvent is set to 100% by mass, the content of the auxiliary solvent is less than 50% by mass, preferably less than 40% by mass, and particularly preferably less than 30% by mass. From the viewpoint of the filterability of the resin composition, when the total amount of the solvent is set to 100% by mass, the content of the auxiliary solvent is preferably more than 5% by mass.

[0341] When the total amount of the solvent is 100% by mass, the content of the auxiliary solvent is preferably 5% by mass or more and 40% by mass or less, and more preferably 5% by mass or more and 30% by mass or less.

[0342] As a specific example of the composition mixed with a co-solvent, in the case of combining two kinds (for example, co-solvent 1 and co-solvent 2), a combination of n-butylbenzene and ethoxybenzene, and a combination of n-butylbenzene and n-butyl benzoate, etc. The mass ratio of the co-solvent when it is the above combination is preferably co-solvent 1:co-solvent 2 = 10:90 to 90:10.

[0343] The mass ratio of n-butylbenzene to ethoxybenzene may be, for example, n-butylbenzene:ethoxybenzene=10:90 to 90:10, and is preferably 50:50.

[0344] Specific examples of the solvent composition of the present application include a mixed solvent of N-methyl-2-pyrrolidone (NMP) as a main solvent and n-butylbenzene as an auxiliary solvent, etc. The mass ratio of the main solvent to the auxiliary solvent can be, for example, main solvent:auxiliary solvent=95:5 to 51:49.

[0345] 〈Additional ingredients〉

[0346] The resin composition of the present embodiment may further contain an additional component in addition to the polyimide / polyimide precursor and the solvent. Examples of the additional component include a surfactant and an alkoxysilane compound.

[0347] (Surfactant)

[0348] By adding a surfactant to the resin composition of the present embodiment, the coating properties of the resin composition can be improved. Specifically, the generation of streaks in the coating film can be prevented.

[0349] Examples of the surfactant include silicone-based surfactants, fluorine-based surfactants, and other nonionic surfactants.

[0350] Examples of the silicone-based surfactant include organosiloxane polymers KF-640, 642, 643, KP341, X-70-092, and X-70-093 (all manufactured by Shin-Etsu Chemical Co., Ltd.);

[0351] SH-28PA, SH-190, SH-193, SZ-6032, SF-8428, DC-57, DC-190 (all manufactured by Toray Dow Corning Silicone Co., Ltd.); SILWET L-77, L-7001, FZ-2105, FZ-2120, FZ-2154, FZ-2164, FZ-2166, L-7604 (all manufactured by Unicharm Co., Ltd., Japan);

[0352] DBE-814, DBE-224, DBE-621, CMS-626, CMS-222, KF-352A, KF-354L, KF-355A, KF-6020, DBE-821, DBE-712 (Gelest), BYK-307, BYK-310, BYK-378, BYK-333 (all manufactured by BYK-Chemie Japan);

[0353] GLANOL (manufactured by Kyoeisha Chemical Co., Ltd.), etc.

[0354] Examples of the fluorine-based surfactant include Megafac F171, F173, and R-08 (manufactured by Dainippon Ink & Chemicals Co., Ltd.);

[0355] Fluorad FC4430, FC4432 (Sumitomo 3M Co.), etc.

[0356] Examples of other nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, and polyoxyethylene octylphenol ether.

[0357] Among these surfactants, from the viewpoint of the coating properties of the resin composition (suppression of streaks), silicone-based surfactants and fluorine-based surfactants are preferred, and from the viewpoint of reducing the effect of oxygen concentration during the curing process on the YI value and total light transmittance, silicone-based surfactants are preferred.

[0358] When a surfactant is used, the content thereof is preferably 0.001 to 5 parts by mass, more preferably 0.01 to 3 parts by mass, based on 100 parts by mass of the polyimide precursor in the resin composition.

[0359] (Alkoxysilane compound)

[0360] When the polyimide film obtained from the resin composition of this embodiment is used for a flexible substrate, etc., from the viewpoint of obtaining good adhesion between the support and the polyimide film in the manufacturing process, the resin composition of the present application may contain 0.01 to 20 parts by mass of an alkoxysilane compound relative to 100 parts by mass of the polyimide precursor.

[0361] By setting the content of the alkoxysilane compound to 0.01 parts by mass or more relative to 100 parts by mass of the polyimide precursor, good adhesion between the support and the polyimide film can be obtained. In addition, from the viewpoint of storage stability of the resin composition of the present application, the content of the alkoxysilane compound is preferably 20 parts by mass or less.

[0362] The content of the alkoxysilane compound is preferably 0.02 to 15 parts by mass, more preferably 0.05 to 10 parts by mass, and further preferably 0.1 to 8 parts by mass relative to 100 parts by mass of the polyimide precursor. By using the alkoxysilane compound, the coating property of the resin composition of the present application is improved (suppressing uneven streaks) on the basis of improving the adhesion, and the influence of the oxygen concentration during curing on the YI value of the polyimide film can also be reduced.

[0363] Examples of the alkoxysilane compound include 3-ureidopropyltriethoxysilane, bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltripropoxysilane, γ-aminopropyltributoxysilane, γ-aminoethyltriethoxysilane, γ-aminoethyltripropoxysilane, γ-aminoethyltributoxysilane, γ-aminobutyltriethoxysilane, γ-aminobutyltrimethoxysilane, γ-aminobutyltripropoxysilane, γ-aminobutyltributoxysilane, phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, and alkoxysilane compounds each having the following structure.

[0364]

[0365] The alkoxysilane compounds may be used alone or in combination of two or more.

[0366] 《Method for producing resin composition》

[0367] One aspect of the present embodiment provides a method for producing a resin composition, including a step of synthesizing a resin, using one selected from the group consisting of the following solvents as a main solvent:

[0368] N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, methylpyridine and pyridine.

[0369] In one embodiment, a method for producing a resin composition includes a step of preparing a solvent including a main solvent and a co-solvent.

[0370] In one embodiment, the method for producing a resin composition comprises: after synthesizing the resin and before filtering, adding the following auxiliary solvent to prepare the resin composition,

[0371] Co-solvents with Hansen Solubility Parameters of:

[0372] δD=16.5~18.9、

[0373] δP=0.1~8.2、

[0374] δH=1.1~5.5.

[0375] The method for producing the resin composition in the present embodiment is not particularly limited, and can be based on, for example, the following steps.

[0376] · Synthetic resin process

[0377] This process is a process for synthesizing a resin (in one embodiment, a polyimide / polyimide precursor) using one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, cyclopentane, picoline and pyridine as a main solvent.

[0378] 〈Synthesis of polyimide / polyimide precursor〉

[0379] The polyimide / polyimide precursor of the present embodiment can be synthesized by causing a polycondensation reaction of a polycondensation component containing an acid dianhydride and a diamine. In addition, a silicon-containing compound can be added as a polycondensation component to synthesize the polyimide / polyimide precursor of the present application. The silicon-containing compound is preferably a compound purified by the method described below.

[0380] In a preferred embodiment, the polycondensation component comprises an acid dianhydride, a diamine and a silicon-containing compound. The polycondensation reaction is preferably carried out in a suitable solvent.

[0381] Specifically, for example, a method of dissolving a predetermined amount of a diamine component and a silicon-containing compound in a solvent, adding a predetermined amount of an acid dianhydride to the obtained diamine solution, and stirring the solution. The imidization during the synthesis of the polyimide may be thermal imidization or chemical imidization using an imidization catalyst.

[0382] It should be noted that the acid dianhydride, diamine and silicon-containing compound are the same as above.

[0383] From the viewpoint of the high molecular weight of the resin composition as a polyimide precursor and the slit coating characteristics of the resin composition, the molar ratio of the acid dianhydride to the diamine when synthesizing the polyimide / polyimide precursor is preferably in the range of acid dianhydride: diamine = 100:90 to 100:110 (0.90 to 1.10 mol parts of diamine relative to 1 mol part of acid dianhydride), and more preferably in the range of 100:92 to 100:101 (0.92 to 1.01 mol parts of diamine relative to 1 mol part of acid dianhydride).

[0384] The weight average molecular weight of the polyimide / polyimide precursor can be controlled by adjusting the types of acid dianhydride, diamine and silicon-containing compound, the molar ratio of acid dianhydride to diamine, adding a capping agent, adjusting the reaction conditions, etc. The closer the molar ratio of the acid dianhydride component to the diamine component is to 1:1 and the smaller the amount of the capping agent used, the higher the molecular weight of the polyimide precursor can be achieved.

[0385] It is recommended to use high-purity products as the acid dianhydride component and the diamine component. As the purity, it is preferably 98% by mass or more, more preferably 99% by mass or more, and further preferably 99.5% by mass or more. By reducing the water content in the acid dianhydride component and the diamine component, high purity can also be achieved.

[0386] When a plurality of acid dianhydride components and / or a plurality of diamine components are used, the acid dianhydride components as a whole and the diamine components as a whole preferably have the above purity, and all the acid dianhydride components and diamine components used more preferably each have the above purity.

[0387] 〈Synthesis solvent for polyimide / polyimide precursor〉

[0388] The synthesis solvent of the polyimide / polyimide precursor is not particularly limited as long as it is a solvent that can dissolve the acid dianhydride component and the diamine component and the generated polyimide / polyimide precursor and can obtain a high molecular weight polymer.

[0389] In one embodiment, as the synthesis solvent of polyimide / polyimide precursor, the main solvent and / or auxiliary solvent of the present application can be used. In other words, as the synthesis solvent, the main solvent of the present application or the auxiliary solvent of the present application can be used alone, or the main solvent and auxiliary solvent of the present application can also be used in combination and used in the form of a mixed solvent.

[0390] As the main solvent that can be used as the synthesis solvent, it is preferred to contain, for example, at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, cyclopentane, methylpyridine and pyridine.

[0391] Examples of the auxiliary solvent that can be used as the synthesis solvent include n-butylbenzene, n-butyl benzoate, and ethoxybenzene.

[0392] The main solvent and auxiliary solvent that can be used as the synthetic solvent are the same as described above.

[0393] When a mixed solvent of a main solvent and an auxiliary solvent is used as the synthesis solvent, the mass ratio of main solvent:auxiliary solvent is preferably 10:90 to 90:10.

[0394] In order to facilitate the polycondensation reaction, the water content in the synthesis solvent is preferably 3,000 mass ppm or less, for example.

[0395] In the resin composition of the present application, the content of molecules with a weight average molecular weight of less than 1,000 is preferably less than 5% by mass. It can be considered that the reason why the molecules with a molecular weight of less than 1,000 exist in the resin composition of the present application is related to the moisture content of the solvent and raw materials (acid dianhydride and diamine) used during synthesis. That is, it can be considered that this is because the anhydride gene of a part of the acid dianhydride monomer is hydrolyzed by moisture and forms a carboxyl group, which remains in a low molecular state without high molecular weight. Therefore, the less moisture content of the solvent used in the polycondensation reaction, the more preferred.

[0396] The amount of water in the synthesis solvent is preferably 3,000 mass ppm or less, more preferably 1,000 mass ppm or less. Similarly, the amount of water contained in the raw material is also preferably 3,000 mass ppm or less, more preferably 1,000 mass ppm or less.

[0397] The amount of water in the synthesis solvent is considered to be related to the grade of the solvent used (dehydrated grade, general grade, etc.), the solvent container (bottle, 18L can, small can, etc.), the storage state of the synthesis solvent (whether a rare gas is sealed, etc.), the time from opening to use (use immediately after opening or use after a certain period of time after opening, etc.). It is also considered to be related to the rare gas replacement of the reactor before synthesis, whether a rare gas is circulated during synthesis, etc.

[0398] Therefore, when synthesizing a polyimide precursor, it is recommended to use a high-purity product as a raw material, use a solvent with a small amount of water, and take measures to prevent water from the environment from mixing into the system before and during the reaction.

[0399] When each polycondensation component is dissolved in the synthesis solvent, heating may be performed as needed. From the viewpoint of obtaining a polyimide precursor with a high degree of polymerization, the reaction temperature when synthesizing the polyimide precursor may preferably be 0° C. to 120° C., 40° C. to 100° C., or 60° C. to 100° C. The polymerization time when synthesizing the polyimide precursor may preferably be 1 to 100 hours or 2 to 10 hours.

[0400] The reaction temperature when synthesizing the polyimide is preferably 130° C. to 200° C., 150° C. to 190° C., or 160° C. to 180° C. The polymerization time when synthesizing the polyimide is preferably 1 to 100 hours, or 2 to 10 hours.

[0401] By setting the polymerization time to 1 hour or more, a polyimide precursor / polyimide having a uniform degree of polymerization can be formed, and by setting the polymerization time to 100 hours or less, a polyimide precursor / polyimide having a high degree of polymerization can be obtained.

[0402] In addition to the polyimide / polyimide precursor in the present embodiment, the resin composition of the present embodiment may also include other arbitrary polyimide precursors. However, from the viewpoint of reducing the oxygen dependence of the YI value and the total light transmittance of the polyimide film, the mass ratio of the arbitrary polyimide / polyimide precursor is preferably less than 30% by mass, more preferably less than 10% by mass relative to the total amount of the polyimide / polyimide precursor in the resin composition of the present application.

[0403] The polyimide precursor in the present embodiment may be partially imidized (partially imidized). By partially imidizing the polyimide precursor, the viscosity stability of the resin composition of the present application during storage can be improved.

[0404] From the viewpoint of balancing the solubility of the polyimide precursor in the resin composition of the present application and the storage stability of the solution, the imidization rate when the polyimide precursor is partially imidized is preferably 5% or more, more preferably 8% or more, and preferably 90% or less, more preferably 80% or less, and further preferably 70% or less. The partial imidization is obtained by heating the polyimide precursor and performing dehydration ring closure.

[0405] The heating for partial imidization is preferably performed at a temperature of 120 to 200° C., more preferably 150 to 185° C., and even more preferably 150 to 180° C. for preferably 15 minutes to 20 hours, and more preferably 30 minutes to 10 hours.

[0406] The material obtained by adding N,N-dimethylformamide dimethyl acetal or N,N-dimethylformamide diethyl acetal to the polyimide / polyimide precursor obtained by the above reaction and heating to esterify a part or all of the carboxylic acids can be used as the polyimide precursor of the present embodiment. By esterification, the viscosity stability during storage can be improved. These ester-modified polyamic acids can also be obtained by reacting the above-mentioned acid dianhydride component with a monohydric alcohol having 1 equivalent relative to the acid anhydride group, and a dehydration condensation agent such as thionyl chloride and dicyclohexylcarbodiimide, and then reacting with a diamine component to obtain the condensation reaction.

[0407] 〈Synthesis of polyimide〉

[0408] The synthesis of the polyimide of the present embodiment may include a thermal imidization step. During the thermal imidization, an azeotropic solvent such as toluene may be used as a co-solvent of the present embodiment, and the azeotropic solvent is usually distilled off (under reduced pressure) at the end of the thermal imidization step.

[0409] As a more preferred mode for the synthesis of polyimide, it is possible to dissolve acid dianhydride component and diamine component in the above-mentioned synthetic solvent, add azeotropic solvents such as toluene, remove the water produced during imidization to outside the system, thereby manufacture in the form of a polyimide solution (also referred to as polyimide varnish) containing polyimide and solvent. By using auxiliary solvent as azeotropic solvent and implementing (decompression) to evaporate, thus usually the content of auxiliary solvent becomes less than 5% by mass relative to resin combination 100% by mass, give play to the effect of the present embodiment (improvement of filterability, etc.), so preferably.

[0410] Here, the reaction conditions are not particularly limited, and for example, the reaction temperature is 0° C. to 190° C., and the reaction time is 3 to 72 hours.

[0411] In one embodiment, when the diamine component contains a sulfonic group, it is preferably heated at 180° C. for about 12 hours to fully react. During the reaction, an inert atmosphere such as argon or nitrogen is preferably used.

[0412] 〈Purification of Silicon-Containing Compounds〉

[0413] The resin composition of the present embodiment can be produced by subjecting a polycondensation component including an acid dianhydride, a diamine, and a silicon-containing compound to a polycondensation reaction.

[0414] As a method for reducing the total amount of the cyclic silicon-containing compound contained in the resin composition of the present embodiment, for example, the total amount of the cyclic silicon-containing compound can be reduced by purifying the silicon-containing compound before the polycondensation reaction. Alternatively, after the polycondensation reaction of the present application, the resin composition can be purified to reduce the total amount of the cyclic silicon-containing compound.

[0415] As a method for purifying the silicon-containing compound, for example, stripping the silicon-containing compound in any container while blowing an inert gas such as nitrogen. The stripping temperature is preferably 200° C. to 300° C., more preferably 220° C. to 300° C., and further preferably 240° C. to 300° C.

[0416] The steam pressure of the gas stripping is preferably as low as possible, and is 1000 Pa or less, more preferably 300 Pa or less, further preferably 200 Pa or less, and further preferably 133.32 Pa (1 mmHg) Pa or less.

[0417] The gas stripping time is preferably 4 hours to 12 hours, more preferably 6 hours to 10 hours.

[0418] By adjusting to the above conditions, the cyclic silicon-containing compound can be effectively removed, and the total amount of the cyclic silicon-containing compound can be controlled to a preferred range (in one embodiment, 1000 ppm or less based on the total of the silicon-containing compound and the cyclic silicon-containing compound).

[0419] ·Process for preparing resin composition

[0420] This step is a step of preparing a resin composition by adding a solvent having a Hansen solubility parameter of the following value after the step of synthesizing the above-mentioned resin and before filtration.

[0421] δD=16.5~18.9

[0422] δP=0.1~8.2

[0423] δH=1.1~5.5

[0424] One embodiment of the resin composition of the present application is for use in displays. From the viewpoint of productivity, filtration is performed to remove impurities, and therefore, the resin composition of the present application is required to have good filterability.

[0425] By adding a solvent (in one embodiment, a co-solvent) that satisfies the above-mentioned specific Hansen solubility parameters before filtration, a solution (in one embodiment, a polyimide / polyimide precursor solution or varnish) containing the resin of the present application and a solvent (in one embodiment, a main solvent and / or a co-solvent) is diluted, thereby improving the filterability of the resin composition of the present application.

[0426] The solvent added to the polyimide / polyimide precursor solution for dilution is not particularly limited as long as it satisfies the above-mentioned specific Hansen solubility parameter.

[0427] In one embodiment, the auxiliary solvent of the present application can be used as a diluting solvent for the polyimide / polyimide precursor solution, and the description related to the auxiliary solvent is the same as above.

[0428] These auxiliary solvents may be used alone or in combination of two or more.

[0429] Specific examples of the composition mixed with the auxiliary solvent include a mixed solvent of n-butylbenzene and ethoxybenzene, etc. The mass ratio of n-butylbenzene to ethoxybenzene may be, for example, n-butylbenzene:ethoxybenzene=10:90 to 90:10, preferably 50:50.

[0430] In one embodiment, the co-solvent of the present application can be used as a synthesis solvent or a dilution solvent.

[0431] As auxiliary solvents that can be used as diluent solvents, for example, n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate , ethyl benzoate, propyl benzoate, diphenyl acetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, toluene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-tert-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene, 2-propylstyrene, n-butyl benzoate and dibutyl sebacate, etc.

[0432] <Preparation of resin composition>

[0433] When the synthesis solvent (in one embodiment, the main solvent and / or the auxiliary solvent) used in synthesizing the polyimide precursor is the same as the solvent contained when diluting the polyimide / polyimide precursor solution (in one embodiment, the auxiliary solvent), the synthesized polyimide / polyimide precursor solution can be directly used as a resin composition.

[0434] As required, by adding one or more of the optional solvent and additional components to the polyimide precursor within a temperature range of room temperature (in one embodiment, 25°C) to 80°C, and stirring and mixing, a resin composition can be prepared. The stirring and mixing can be carried out using a Three-One Motor (manufactured by Shinto Chemical Co., Ltd.) equipped with a stirring blade, a rotation and revolution stirrer, and other appropriate devices. As required, the resin composition can be heated to 40°C to 100°C.

[0435] On the other hand, when the synthesis solvent (in one embodiment, the main solvent and / or the auxiliary solvent) used in the synthesis of the polyimide / polyimide precursor is different from the solvent (in one embodiment, the auxiliary solvent) contained in the dilution of the polyimide / polyimide precursor solution, the solvent in the synthesized polyimide precursor solution can be removed by appropriate methods such as reprecipitation and solvent distillation to separate the polyimide / polyimide precursor. Then, the desired solvent and the additional components as needed are added to the separated polyimide precursor within the temperature range of room temperature (25°C) to 80°C, and stirred and mixed, thereby preparing a resin composition.

[0436] After the resin composition is prepared as described above, the resin composition can be heated at, for example, 130 to 200° C. for 5 minutes to 2 hours to dehydrate and imidize a portion of the polyimide precursor to such an extent that the polymer does not precipitate (partial imidization). The imidization rate can be controlled by controlling the heating temperature and the heating time. By partially imidizing the polyimide precursor, the viscosity stability of the resin composition during storage can be improved.

[0437] From the viewpoint of slit coating performance, the solution viscosity of the resin composition is preferably 500 to 100,000 mPa·s, more preferably 1,000 to 50,000 mPa·s, and even more preferably 3,000 to 20,000 mPa·s.

[0438] Specifically, from the viewpoint of preventing the liquid from leaking from the slit nozzle, it is preferably 500 mPa·s or more, more preferably 1,000 mPa·s or more, and even more preferably 3,000 mPa·s or more. From the viewpoint of preventing the slit nozzle from being clogged, it is preferably 100,000 mPa·s or less, more preferably 50,000 mPa·s or less, and even more preferably 20,000 mPa·s or less.

[0439] Regarding the solution viscosity of the resin composition when synthesizing polyimide / polyimide precursor, if the value is higher than the above range, there is a tendency that it is difficult to stir during synthesis. Among them, even if the solution reaches a high viscosity (in this application, 1000mPa·s or more) during synthesis, a resin composition with a viscosity that is easy to handle can be obtained by adding a solvent and stirring after the reaction is completed.

[0440] The solution viscosity of the resin composition in the present embodiment is a value measured at 23° C. using an E-type viscometer (for example, VISCONICE HD, manufactured by Toki Sangyo Co., Ltd.).

[0441] From the viewpoint of viscosity stability of the resin composition during storage, the water content of the resin composition of the present embodiment is preferably 3,000 mass ppm or less, more preferably 2,500 mass ppm or less, further preferably 2,000 mass ppm or less, further preferably 1,500 mass ppm or less, particularly preferably 1,000 mass ppm or less, particularly preferably 500 mass ppm or less, particularly preferably 300 mass ppm or less, and particularly preferably 100 mass ppm or less.

[0442] The polyimide / polyimide precursor may be synthesized in a main solvent and an auxiliary solvent may be added before filtration to obtain the resin composition. Alternatively, the polyimide / polyimide precursor may be synthesized in a mixed solvent of the main solvent and the auxiliary solvent to obtain the resin composition.

[0443] · Process for preparing a solvent comprising a main solvent and a co-solvent

[0444] This step is a step of preparing a solvent including a main solvent and a co-solvent.

[0445] The preparation conditions and the like of the solvent are the same as those described above with respect to the main solvent and the auxiliary solvent.

[0446] The solvent may be used for the synthesis of the polyimide / polyimide precursor, or may be used for diluting the polyimide / polyimide precursor solution before filtration.

[0447] The resin composition was filtered by placing a membrane filter (pore size: 0.5 μm) in a stainless steel holder with a tank, pouring the varnish, sealing the tank, and filtering under pressure with air (about 0.3 MPa).

[0448] "Polyimide film and method for producing the same"

[0449] Using the resin composition of the present embodiment, a polyimide film (hereinafter also referred to as a polyimide resin film) can be provided.

[0450] A method for producing a polyimide resin film provided in one aspect of the present embodiment includes a coating step of coating the resin composition of the present embodiment on a surface of a support.

[0451] In one embodiment, a method for producing a polyimide resin film includes a film forming step of heating a resin composition to form a polyimide resin film.

[0452] In one embodiment, the method for producing a polyimide resin film includes a peeling step of peeling the polyimide resin film from a support.

[0453] In one embodiment, the method for producing a polyimide resin film includes an irradiation treatment of irradiating the polyimide resin film with laser light from a support side before the peeling step.

[0454] 〈Coating process〉

[0455] The coating step is a step of coating the resin composition of the present embodiment on the surface of the support.

[0456] The support is not particularly limited as long as it is heat-resistant to the heating temperature in the film forming step after the coating step and has good peeling properties in the peeling step. Examples of the support include glass substrates (e.g., alkali-free glass substrates); silicon wafers; resin substrates such as PET (polyethylene terephthalate), OPP (oriented polypropylene), polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, polyamide-imide, polyetherimide, polyetheretherketone, polyethersulfone, polyphenylsulfone, and polyphenylene sulfide; and metal substrates such as stainless steel, alumina, copper, and nickel.

[0457] When forming a thin film of polyimide molding, for example, a glass substrate, a silicon wafer, etc. is preferred, and when forming a thick film or sheet of polyimide molding, for example, a support formed of PET (polyethylene terephthalate), OPP (oriented polypropylene), etc. is preferred.

[0458] As the coating method, generally, coating methods such as a blade coater, an air knife coater, a roll coater, a spin coater, a flow coater, a die coater, and a rod coater can be cited;

[0459] Coating methods such as slit coating, spin coating, spray coating, dip coating, etc.

[0460] Printing technologies represented by screen printing and gravure printing, etc.

[0461] The resin composition of the present embodiment is preferably applied by slit coating.

[0462] The thickness of the coating film obtained by coating (referred to as film thickness) should be appropriately adjusted depending on the desired thickness of the polyimide film and the content of the polyimide precursor in the resin composition, and is preferably about 1 to 1,000 μm.

[0463] The temperature in the coating step may be room temperature, but the resin composition may be heated to, for example, 40° C. to 80° C. in order to reduce the viscosity and improve workability.

[0464] <Optional drying process>

[0465] After the coating step, a drying step may be performed, or the drying step may be omitted and the process may directly proceed to the subsequent film forming step (heating step).

[0466] The drying step is performed for the purpose of removing the organic solvent in the resin composition. When performing the drying step, for example, an appropriate device such as a hot plate, a box dryer, a conveyor dryer, or a reduced pressure dryer can be used.

[0467] The temperature in the drying step is preferably 80°C to 200°C, more preferably 100°C to 150°C.

[0468] The pressure in the drying step is preferably 40 Pa to 140 Pa, more preferably 60 Pa to 120 Pa.

[0469] The drying step is preferably performed for 1 minute to 10 hours, more preferably 3 minutes to 1 hour. As described above, a coating film containing a polyimide precursor is formed on the surface of the support.

[0470] <Film formation process>

[0471] Next, a film forming step (hereinafter also referred to as a heating step) is performed.

[0472] The film forming step is a step of removing the organic solvent contained in the coating film obtained in the coating step by heating, and performing an imidization reaction of the polyimide precursor in the coating film to form a polyimide resin film.

[0473] As the heating method, hot air drying, infrared heater, hot air drying and infrared heater, etc. can be used. Infrared rays can also use far infrared rays. The heating process can be carried out using devices such as an inert gas oven, a hot plate, a box-type dryer, and a conveyor belt type dryer. The heating process can be carried out at the same time as the drying process, or the two processes can be carried out in sequence.

[0474] The heating step can be carried out in an air atmosphere, but is preferably carried out in an inert gas atmosphere from the viewpoint of obtaining safety, good transparency of the obtained polyimide film, low thickness direction retardation (Rth) and low YI value. Examples of the inert gas include nitrogen and argon.

[0475] The heating temperature is appropriately set according to the type of polyimide precursor and the type of solvent in the resin composition, and is preferably 250° C. to 550° C., and more preferably 300° C. to 450° C. If it is 250° C. or higher, imidization proceeds well, and if it is 550° C. or lower, disadvantages such as decreased transparency and decreased heat resistance of the obtained polyimide film can be avoided.

[0476] The heating time is preferably about 0.1 hour to 10 hours.

[0477] In the present embodiment, from the viewpoint of low YI value and transmittance of the obtained polyimide film, the oxygen concentration of the surrounding atmosphere in the heating step is preferably 2,000 mass ppm or less, more preferably 300 mass ppm or less, and further preferably 10 mass ppm or less.

[0478] By heating in an atmosphere having an oxygen concentration of 2,000 mass ppm or less, the YI value of the obtained polyimide film can be set to 16 or less.

[0479] 〈Peeling process〉

[0480] In the peeling step, the polyimide resin film on the support is peeled off after being cooled to, for example, about 25° C. (room temperature) to 50° C. As the peeling step, for example, the following treatments (1) to (4) may be mentioned.

[0481] (1) After a structure including a polyimide resin film / support is prepared by the above method, a laser is irradiated from the support side of the structure to ablate the interface between the support and the polyimide resin film, thereby peeling off the polyimide resin (in one embodiment, irradiation treatment).

[0482] Examples of the type of laser include solid (YAG) lasers, gas (UV excimer) lasers, etc. It is preferable to use a spectrum having a wavelength of 308 nm or the like (see JP-A-2007-512568 and JP-A-2012-511173, etc.).

[0483] The irradiation treatment is a treatment of irradiating the polyimide resin film with laser light from the support side.

[0484] From the viewpoint of the difference in refractive index between the front and back sides of the obtained polyimide resin film, it is preferred to perform irradiation treatment before the peeling step.

[0485] (2) A treatment in which a release layer is formed on a support before applying the resin composition to the support, and then a structure including a polyimide resin film / release layer / support is obtained, and the polyimide resin film is released.

[0486] Examples of the release layer include PARYLENE (registered trademark, manufactured by Nippon PARYLENE Co., Ltd.) and tungsten oxide. Vegetable oil-based, silicone-based, fluorine-based, alkyd-based release agents can be used (see JP-A Nos. 2010-067957 and 2013-179306).

[0487] The laser irradiation of the process (2) and the process (1) may be used in combination.

[0488] (3) A process in which an etchable metal substrate is used as a support to obtain a structure including a polyimide resin film / support, and then the metal is etched with an etchant to obtain a polyimide resin film.

[0489] As the metal, for example, copper (as a specific example, electrolytic copper foil "DFF" manufactured by Mitsui Mining & Smelting Co., Ltd.), aluminum, etc. can be used. As the etchant, ferric chloride, etc. can be used for copper, and diluted hydrochloric acid, etc. can be used for aluminum.

[0490] (4) After obtaining a structure including a polyimide resin film / support by the above method, an adhesive film is attached to the surface of the polyimide resin film, the adhesive film / polyimide resin film is separated from the support, and then the polyimide resin film is separated from the adhesive film.

[0491] Among these peeling treatments, treatment (1) or (2) is preferred, and treatment (1) is more preferred, from the viewpoint of the difference in refractive index between the front and back sides of the obtained polyimide resin film, a low YI value, and elongation of the resin film.

[0492] In addition, when copper was used as a support in the treatment (3), the YI value of the obtained polyimide resin film increased and the elongation of the resin film tended to decrease. This is considered to be the influence of copper ions.

[0493] The thickness of the polyimide film obtained after the peeling step is not limited, but is preferably 1 to 200 μm, more preferably 5 to 100 μm.

[0494] 《Polyimide resin film (resin film after curing of resin composition)》

[0495] The structure of the polyimide contained in the polyimide resin film formed from the polyimide precursor of the present embodiment is represented by the following general formula (20):

[0496]

[0497] {In the general formula (20), P1 and P2 are the same as P1 and P2 in the general formula (1) or the general formula (2) or P3 and P4 in the general formula (2), and m is a positive integer.}

[0498] For the same reasons as in the general formula (1) or (2), preferred P1 and P2 in the general formula (20) are also preferred in the polyimide of the general formula (20).

[0499] The number m of repeating units in the general formula (20) is not particularly limited and may be an integer of 2 to 150.

[0500] The structure of the polyimide contained in the polyimide resin film formed from the polyimide precursor composition of the present embodiment is represented by the following general formula (21):

[0501]

[0502] {In the general formula (21), P3 and P4 are the same as P1 and P2 in the general formula (1), and in the general formula (21), P5 and P6 are the same as P3 and P4 in the general formula (2), and m and n are positive integers.}

[0503] For the same reasons as P1 and P2 in the general formula (1) and preferred P3 and P4 in the general formula (2), preferred P3 and P4 and P5 and P6 in the general formula (21) are also preferred in the polyimide of the general formula (21).

[0504] The number of repeating units m and n in the general formula (21) is not particularly limited and may be an integer of 2 to 150.

[0505] The polyimide resin film of this embodiment preferably satisfies the following properties;

[0506] ·YI (yellowness index) is 16 or less (converted to a film thickness of 10 μm):

[0507] · Degassing start temperature (TDS) is above 420℃

[0508] The residual stress is 35 MPa or less (under nitrogen atmosphere) or the Rth (retardation in the thickness direction) is 100 nm or less (converted to a film thickness of 10 μm).

[0509] Therefore, the polyimide resin film of the present embodiment can be suitably applied to displays (particularly displays using LTPS (low temperature polycrystalline silicon) and LTPO (low temperature polycrystalline oxide)).

[0510] 《Application of polyimide film》

[0511] The polyimide film obtained from the resin composition of this embodiment can be used as, for example, a semiconductor insulating film, a thin film transistor liquid crystal display (TFT-LCD) insulating film, an electrode protective film, and can also be used as a transparent substrate for display devices such as flexible displays, liquid crystal displays, organic electroluminescent displays, field emission displays, and electronic paper.

[0512] The polyimide film obtained from the resin composition of the present embodiment can be suitably used as a display including a thin film transistor (TFT) substrate and / or a color filter substrate.

[0513] In particular, the polyimide film obtained from the resin composition of the present embodiment can be suitably used as a thin film transistor (TFT) substrate, a color filter substrate, a touch panel substrate, and a substrate of a transparent conductive film (ITO, Indium Thin Oxide) in the production of flexible devices.

[0514] Flexible devices to which the polyimide film in this embodiment can be applied include, for example, TFT devices for flexible displays, flexible solar cells, flexible touch panels, flexible lighting, flexible batteries, flexible printed circuit boards, flexible color filters, and surface cover lenses for smartphones.

[0515] Typically, the process of forming a TFT on a flexible substrate using a polyimide film is performed at a wide temperature range of 150° C. to 650° C. Specifically, when amorphous silicon is used to make a TFT device, a process temperature of 250° C. to 350° C. is generally required, and the polyimide film of this embodiment needs to be able to withstand this temperature. Therefore, specifically, it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition start temperature above the process temperature.

[0516] When using metal oxide semiconductors (IGZO, etc.) to manufacture TFT devices, a process temperature of 320°C to 400°C is generally required. The polyimide film of this embodiment needs to be able to withstand this temperature. Therefore, it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition start temperature that are higher than the highest temperature of the TFT manufacturing process.

[0517] When LTPS (low-temperature polycrystalline silicon) or LTPO (low-temperature polycrystalline oxide) is used to manufacture TFT devices, a process temperature of 380°C to 520°C is generally required. The polyimide film of this embodiment needs to be able to withstand this temperature. Therefore, it is necessary to appropriately select a glass transition temperature and a thermal decomposition start temperature that are above the highest temperature of the TFT manufacturing process.

[0518] On the other hand, due to these thermal histories, there is a tendency for the optical properties (particularly transmittance, retardation properties, and YI value) of the polyimide film to decrease to the extent of being exposed to a high temperature process.

[0519] However, the polyimide obtained from the polyimide precursor of the present embodiment has good optical properties even after undergoing a thermal history.

[0520] Hereinafter, as application examples of the polyimide film of the present embodiment, a method for producing a display and a laminate will be described.

[0521] "Manufacturing method of display device"

[0522] A method for producing a display provided in one aspect of the present embodiment includes a coating step of coating the resin composition of the present embodiment on a surface of a support.

[0523] In one embodiment, a method for producing a display includes a film forming step of heating a resin composition to form a polyimide resin film.

[0524] In one embodiment, a method for manufacturing a display includes an element forming step of forming an element on a polyimide resin film.

[0525] In one embodiment, a method for manufacturing a display includes a peeling step of peeling a polyimide resin film having an element formed thereon from a support.

[0526] The display of the present application is obtained by forming elements on the polyimide resin film of the present application.

[0527] In the method for producing a display of the present application, preferred specific procedures of the coating step and the film forming step are the same as those described in the method for producing the polyimide film.

[0528] In the method for manufacturing a display of the present application, the element forming step is a step of forming an element on a polyimide resin film.

[0529] Examples of the element in the display of the present application include an organic EL element, a liquid crystal element, and a micro LED element.

[0530] The element forming step can be carried out using known manufacturing conditions, and can be carried out, for example, by the organic EL substrate manufacturing step, the sealing substrate manufacturing step, and the assembling step described later.

[0531] In the method for manufacturing a display of the present application, the peeling step is a step of peeling the polyimide resin film and the element from the support.

[0532] In the method for producing a display of the present application, preferred specific procedures of the peeling step are the same as those described in the method for producing the polyimide film.

[0533] ·Production example of flexible organic EL display

[0534] Figure 1 This is a schematic diagram showing the structure of a top emission type flexible organic EL display as an example of the display according to the present embodiment, above the polyimide substrate.

[0535] against Figure 1The organic EL structure 25 of the embodiment is described. For example, an organic EL element 250a emitting red light, an organic EL element 250b emitting green light, and an organic EL element 250c emitting blue light are arranged as one unit in a matrix, and a partition wall (bank) 251 is used to divide the light-emitting area of ​​each organic EL element. Each organic EL element is composed of a lower electrode (anode) 252, a hole transport layer 253, a light-emitting layer 254, and an upper electrode (cathode) 255. On the lower layer 2a representing a CVD multilayer film (multi-barrier layer) formed of silicon nitride (SiN) and silicon oxide (SiO), a plurality of TFTs 256 (selected from low-temperature polycrystalline silicon (LTPS), metal oxide semiconductor (IGZO, etc.)) for driving the organic EL element, an interlayer insulating film 258 having a contact hole 257, and a lower electrode 259 are provided. The organic EL element is sealed by a sealing substrate 2b, and a hollow portion 261 is formed between each organic EL element and the sealing substrate 2b.

[0536] The manufacturing process of the flexible organic EL display includes: a process of making a polyimide film on a glass substrate support; Figure 1 The process of manufacturing the organic EL substrate shown in the figure; the process of manufacturing the sealing substrate; the assembly process of bonding the two substrates; and the peeling process of peeling the organic EL display made on the polyimide film from the glass substrate support. The organic EL substrate manufacturing process, the sealing substrate manufacturing process and the assembly process can apply known manufacturing processes. An example thereof is listed below, but it is not limited to this. The process of manufacturing the polyimide film and the peeling process are the same as the coating process, film forming process and peeling process of the above-mentioned polyimide film.

[0537] For example, if you refer to Figure 1 First, a polyimide film is prepared on a glass substrate support by the above method, and a multi-barrier layer (SiN) formed by a multilayer structure of silicon nitride (SiN) and silicon oxide (SiO) is prepared on the upper portion thereof by a CVD method or a sputtering method. Figure 1 The lower substrate 2a in the middle is used to make a metal wiring layer for driving TFT on its upper part using photoresist or the like. An active buffer layer such as SiO is made on its upper part using CVD method, and a TFT device such as metal oxide semiconductor (IGZO) or low temperature polycrystalline silicon (LTPS) is made on its upper part ( Figure 1 After the TFT substrate for the flexible display is manufactured, an interlayer insulating film 258 having a contact hole 257 is formed by using a photosensitive acrylic resin or the like. An ITO film is formed by a sputtering method or the like to form a lower electrode 259 in a manner matching the TFT.

[0538] Next, after forming a partition wall (bank) 251 using photosensitive polyimide or the like, a hole transport layer 253 and a light-emitting layer 254 are formed in each space divided by the partition wall. An upper electrode (cathode) 255 is formed so as to cover the light-emitting layer 254 and the partition wall (bank) 251. Thereafter, an organic EL material (which is the same as the red light) emitting red light is evaporated by a known method using a fine metal mask or the like as a mask. Figure 1 The organic EL element 250a emitting red light in the embodiment corresponds to the organic EL element 250a emitting red light), the organic EL material emitting green light (corresponding to the organic EL element 250a emitting red light in the embodiment Figure 1 The organic EL element 250b emitting green light in the embodiment corresponds to the organic EL element 250b emitting green light and the organic EL material emitting blue light (corresponding to Figure 1 The organic EL substrate is manufactured by sealing the organic EL substrate with a sealing film or the like ( Figure 1 The device above the polyimide substrate is separated from the glass substrate support by a known separation method such as laser separation, thereby making a top-emitting flexible organic EL display. When the polyimide of this embodiment is used, a bottom-seeing flexible organic EL display can be made. A bottom-emitting flexible organic EL display can be made by a known method.

[0539] ·Production example of flexible liquid crystal display

[0540] The polyimide film of this embodiment can be used to make a flexible liquid crystal display. As a specific production method, a polyimide film is produced on a glass substrate support using the above method, and a TFT substrate formed of, for example, amorphous silicon, a metal oxide semiconductor (IGZO, etc.) and low-temperature polycrystalline silicon is produced using the above method. Separately, a polyimide film is produced on a glass substrate support according to the coating process and film formation process of this embodiment, and a color filter glass substrate (CF substrate) having a polyimide film is produced according to a known method and using a color resist, etc. For one of the TFT substrate and the CF substrate, a sealing material including a thermosetting epoxy resin or the like is applied by screen printing into a frame-shaped pattern lacking a liquid crystal injection port, and spherical spacers are scattered on the other substrate, wherein the spherical spacers have a diameter equivalent to the thickness of the liquid crystal layer and are formed of plastic or silicon dioxide.

[0541] Next, the TFT substrate and the CF substrate are attached to solidify the sealing material. In addition, a liquid crystal material is injected into the space surrounded by the TFT substrate, the CF substrate and the sealing material by a decompression method, a thermosetting resin is applied to the liquid crystal injection port, and the liquid crystal material is sealed by heating to form a liquid crystal layer. Finally, the glass substrate on the CF side and the glass substrate on the TFT side are peeled off at the interface between the polyimide film and the glass substrate by laser irradiation or the like, thereby making it possible to produce a flexible liquid crystal display.

[0542] In particular, in the present embodiment, by including a process of heating a laminate comprising a polyimide resin film / inorganic film having a YI (yellowness index) of 16 or less (converted to a film thickness of 10 μm) at 260° C. or above or 430° C. or above, it is possible to manufacture a display having sufficient characteristics required for a display (taking into account characteristics such as the glass transition temperature when cured at 260° C. or above or 430° C., low YI, Young's modulus, chemical resistance, and heat resistance of the laminate, etc.).

[0543] Furthermore, in the present embodiment, the polyimide film satisfies the following properties, thereby making it possible to manufacture a display having properties sufficient for the properties required for the above-mentioned display.

[0544] · Degassing start temperature (TDS) is above 420℃

[0545] · Residual stress is 35MPa or less (under nitrogen atmosphere) or Rth (thickness direction retardation) is 100nm or less (converted to 10μm film thickness)

[0546] Therefore, the resin composition of the present embodiment can be suitably used for producing a display substrate, preferably for producing a flexible display substrate.

[0547] 《Method for producing laminated body》

[0548] A method for producing a laminated body provided by one aspect of the present embodiment includes a coating step of coating the resin composition of the present embodiment on the surface of a support.

[0549] In one embodiment, a method for producing a laminate includes a film forming step of heating a resin composition to form a polyimide resin film.

[0550] In one embodiment, a method for producing a laminate includes an element forming step of forming an element on a polyimide resin film.

[0551] In one embodiment, a method for producing a laminate includes the step of peeling a polyimide resin film having an element formed thereon from a support.

[0552] The laminate of the present application is formed by forming an element on the polyimide resin film of the present application. In one embodiment, the laminate comprises a polyimide resin film and an inorganic film. Examples of the inorganic film include SiO2 film, SiN X Membranes and SiON X Membrane, etc.

[0553] In the method for producing a laminate of the present application, preferred specific procedures of the coating step, the film forming step, the element forming step, and the peeling step are the same as those described above for the method for producing a polyimide film and the method for producing a display.

[0554] Examples of the element in the laminate of the present application include an organic EL element, a liquid crystal element, and a micro LED element.

[0555] In the method for producing a laminate of the present application, a peeling step may be optionally performed.

[0556] Example

[0557] Hereinafter, although embodiment of this invention is demonstrated concretely by an Example and a comparative example, this invention is not limited to these Examples and comparative examples.

[0558] 《Measurement and evaluation methods of physical properties》

[0559] 〈Boiling point (℃) of auxiliary solvent〉

[0560] With reference to the official website of the reagent manufacturer, the boiling point of the auxiliary solvent is recorded in Table 1. For the solvents recorded in the official website of Tokyo Chemical Industry Co., Ltd. (hereinafter also referred to as TCI), the boiling point recorded in TCI is used as the boiling point of the auxiliary solvent of the present application. When the auxiliary solvent is a combination of more than two kinds, the temperature with the higher boiling point among the solvents is used as the boiling point and recorded in Table 1.

[0561] ·SP value calculation method

[0562] The values ​​obtained by the following method are set as the Hansen Solubility Parameters (HSPiP) of the main solvent and auxiliary solvent of the present application;

[0563] 1) Use the application that can be downloaded from the following website;

[0564] https: / / www.hansen-solubility.com / buy-HSPiP-software.php

[0565] 2) Applications using HSPiP 5th Edition and later;

[0566] 3) For solvents listed in this application (listed in Solvent Optimizer), the solubility parameters (δD, δP, δH values) listed there are used;

[0567] 4) For solvents not included in the application, calculate the SMILES (simplified molecular input line entry system) notation based on the structure of the solvent, input the SMILES in the "DIY" of the aforementioned application, and use the solubility parameters (δD, δP, and δH values) calculated from it.

[0568] 〈Yellowness (YI)〉

[0569] On an alkali-free glass substrate (hereinafter also referred to as "glass substrate" or simply "substrate") of 100 mm in length × 100 mm in width × 0.5 mm in thickness, the resin composition of the embodiment and the comparative example was applied in an area 5 mm inside from the end of the glass substrate so that the film thickness after curing became 10 μm. A slit coater (LC-R300G, manufactured by SCREENFINETEC SOLUTIONS) was used for coating. A reduced pressure dryer (manufactured by Tokyo Ohka Kogyo Co., Ltd.) was used to remove the solvent from the obtained glass substrate with a coating film under the conditions of 80°C, 100 Pa, and 30 minutes to obtain a glass substrate with a resin composition coating film.

[0570] The obtained glass substrate having a resin composition coating film was heated in an oven (INH-9N1, manufactured by KOYO THERMOSYSTEMS Co., Ltd.) at 430° C. for 30 minutes under a nitrogen atmosphere (oxygen concentration of 300 ppm or less) for Examples using substances other than ODPA as acid anhydride 1, i.e., Examples 1 to 115, even-numbered examples among Examples 151 to 162, even-numbered examples among Examples 171 to 184, Examples 191, 193, odd-numbered examples among Examples 210 to 223, Example 228, and even-numbered examples among Examples 229 to 234, and Comparative Examples using substances other than ODPA as acid anhydride 1, i.e., Comparative Examples 2 to 4, to prepare samples.

[0571] The obtained sample was used as a test piece, and the yellowness (YI) value was measured using a spectrocolorimeter (manufactured by Nippon Denshoku Industries, Ltd., model name "SE600") with the light source being D65.

[0572] The results obtained are calculated as a film thickness of 10 μm, and the even-numbered examples in Examples 1 to 115, Examples 151 to 162, the even-numbered examples in Examples 171 to 184, Examples 191, 193, the odd-numbered examples in Examples 210 to 223, Example 228, the even-numbered examples in Examples 229 to 234, and Comparative Examples 2 to 4 are evaluated according to the following criteria.

[0573] A: YI is below 10, "Excellent"

[0574] B: YI is more than 10 and less than 13 "Excellent"

[0575] C: YI is more than 13 and less than 16 "good"

[0576] D: YI over 16 "bad"

[0577] If the evaluation is A, B or C, it can be suitably used as a resin composition for forming a display.

[0578] In the examples using ODPA as the acid anhydride 1, namely, the odd-numbered examples among Examples 116 to 151, Examples 153 to 162, Examples 163 to 171, Examples 173 to 184, Examples 185 to 190, Example 192, Examples 194 to 210, Examples 212 to 223, the even-numbered examples among Examples 224 to 227 and Examples 229 to 234, and Comparative Example 1 using ODPA as the acid anhydride 1, samples of polyimide resin films were formed on glass substrates by heating at 260° C. for 30 minutes in an air atmosphere using an oven (INH-9N1, manufactured by KOYO THERMOSYSTEMS Co., Ltd.).

[0579] The obtained sample was used as a test piece, and the yellowness (YI) value was measured using a spectrocolorimeter (manufactured by Nippon Denshoku Industries, Ltd., model name "SE600") with the light source being D65.

[0580] The results obtained are calculated as a film thickness of 10 μm, and the odd-numbered examples in Examples 116 to 151 and Examples 153 to 162, the odd-numbered examples in Examples 163 to 171 and Examples 173 to 184, the even-numbered examples in Examples 185 to 190, Example 192, Examples 194 to 210 and Examples 212 to 223, the odd-numbered examples in Examples 224 to 227 and Examples 229 to 234, and Comparative Example 1 are evaluated according to the following criteria.

[0581] A: YI is 3 or less, "Excellent"

[0582] B: YI is more than 3 and less than 5 "Excellent"

[0583] C: YI is more than 5 and less than 10 "good"

[0584] D: YI more than 10 "bad"

[0585] If the evaluation is A, B, or C, it can be suitably used as a resin composition for forming a color filter substrate.

[0586] 〈Filterability〉

[0587] A membrane filter (pore size: 0.5 μm) manufactured by ADVANTEC was placed on a stainless steel holder with a pot manufactured by ADVANTEC (model: KST-47), a varnish prepared as described below was poured into it, and the container was sealed and pressure filtered at a pressure of 0.3 MPa using air.

[0588] The filtrate was placed in a container, and the filtration amount per hour after 30 minutes from the start of filtration was measured to calculate the filtration rate.

[0589] "5": Filtration rate is above 10g / Hr "Excellent"

[0590] "4": Filtration rate is above 5g / Hr and less than 10g / Hr "Excellent"

[0591] "3": Filtration rate is above 3g / Hr and less than 5g / Hr "good"

[0592] "2": Filtration rate is above 1g / Hr and less than 3g / Hr "qualified"

[0593] "1": Filtration rate is less than 1g / Hr, "unqualified"

[0594] When the evaluation is "2" or more, the resin composition can be suitably used as a resin composition for forming a display.

[0595] 〈Filtration speed〉

[0596] Pressure filtration was performed in the same manner as described in <Filterability>, and the filtration amount after 5 hours from the start of filtration was measured to calculate the filtration rate after 5 hours from the start of filtration.

[0597] "a": Filtration rate is above 5g / Hr "excellent"

[0598] "b": Filtration rate is above 3g / Hr and less than 5g / Hr "excellent"

[0599] "c": Filtration rate is above 1g / Hr and less than 3g / Hr "good"

[0600] "d": Filtration rate is less than 1g / Hr "poor"

[0601] If the evaluation is a, b or c, the resin composition can be suitably used as a resin composition for forming a display.

[0602] 《Example 1》

[0603] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (200 g) as a main solvent, toluene (150 g), BAFL (13.52 g; 38.8 mmol) as a diamine, and SiDA (7 g) as a silicon-containing monomer were added while stirring, and then PMDA (3.27 g; 15 mmol), BPDA (4.41 g; 15 mmol), and BPAF (9.2 g; 20 mmol) as acid dianhydrides were added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0604] Then, the mixture was cooled to room temperature, and pPD (6.29 g; 58.2 mmol) as a diamine was added while stirring. Then, BPAF (22.9 g; 50.0 mmol) as an acid dianhydride was added. The mixture was stirred at room temperature for 24 hours, and the toluene was distilled off under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized (L / M = 60 / 40 mol%) polyimide precursor (hereinafter also referred to as PAI).

[0605] The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and n-butylbenzene was added as an auxiliary solvent to give 30 wt% of the total solvent and 15 wt% of the solid content.

[0606] 《Examples 2 to 5》

[0607] Except having changed the content ratio of the auxiliary solvent as shown in Table 1, it carried out similarly to Example 1, and obtained the varnish.

[0608] 《Examples 6 to 18 and 24》

[0609] A varnish was obtained in the same manner as in Example 1 except that the main solvent described in Table 1 was used instead of NMP as the main solvent.

[0610] 《Example 19》

[0611] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (200 g) as a main solvent, toluene (150 g), APAB (4.6 g; 20 mmol) and SiDA (7 g) as a diamine were added while stirring, and then CpODA (38.44 g; 100 mmol) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 180° C., and the mixture was heated under reflux at 180° C. for 3 hours to carry out imidization.

[0612] Then, the mixture was cooled to room temperature, and APAB (17.43 g; 76.5 mmol) as a diamine was added while stirring. The mixture was stirred at room temperature for 24 hours, and toluene was distilled off under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized (L / M = 20 / 80 mol%) polyimide precursor (PAI).

[0613] The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and n-butylbenzene was added as an auxiliary solvent to give 30 wt% of the total solvent and 15 wt% of the solid content.

[0614] 《Example 20》

[0615] Except having changed the diamine as shown in Table 1, it carried out similarly to Example 19, and obtained the varnish.

[0616] 《Example 21》

[0617] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (200 g) as a main solvent, toluene (150 g), BAFL (13.52 g; 38.8 mmol) and pPD (6.29 g; 58.2 mmol) and SiDA (7 g) as diamines were added while stirring, and then PMDA (3.27 g; 15 mmol), BPDA (4.41 g; 15 mmol), and BPAF (32.09 g; 70 mmol) as dianhydrides were added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0618] Then, the mixture was cooled to room temperature, stirred at room temperature for 24 hours, and toluene was distilled off under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of polyimide (hereinafter also referred to as PI). The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and n-butylbenzene was added as a cosolvent in a manner of 30 wt% of the total solvent, and was added and used in a manner of 15 wt% of the solid content.

[0619] 《Example 22》

[0620] The amount of the above-mentioned PMDA was changed to 3.71 g. After adding the same components as in Example 21 at room temperature, the mixture was stirred at room temperature for 24 hours, heated to 180° C. and toluene was distilled off under reduced pressure. The same operations were performed as in Example 1 to obtain an NMP solution (hereinafter also referred to as varnish) of a polyimide precursor (hereinafter also referred to as PAA).

[0621] 《Example 23》

[0622] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (200 g) as a main solvent, toluene (80 g), BAFL (13.52 g; 38.8 mmol) and SiDA (7 g) as a diamine were added while stirring, and then PMDA (3.27 g; 15 mmol), BPDA (4.41 g; 15 mmol), and BPAF (9.2 g; 20 mmol) as dianhydrides were added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0623] Then, the mixture was cooled to room temperature, and n-butylbenzene (70 g) was added as a synthetic solvent as an auxiliary solvent. pPD (6.29 g; 58.2 mmol) as a diamine was added while stirring. Next, BPAF (22.9 g; 50.0 mmol) as an acid dianhydride was added. The mixture was stirred at room temperature for 24 hours, and toluene was distilled off under reduced pressure to obtain a solution (hereinafter also referred to as varnish) in which a part of the imidized (L / M=60 / 40 mol%) polyimide precursor (PAI) was dissolved in NMP.

[0624] The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and n-butylbenzene was added as an auxiliary solvent to give 30 wt% of the total solvent and 15 wt% of the solid content.

[0625] 《Examples 25-38, 40, 42, 44, 46, 48, 50-59, 61, 63, 65, 67, 69, 71, 73-77, 79, 81-97, 99, 101, 103, 105, 107, 109 and 111-114》

[0626] A varnish was obtained in the same manner as in Example 1 except that the co-solvent described in Table 1 was used instead of n-butylbenzene as the co-solvent.

[0627] 《Example 39》

[0628] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (400 g) as a main solvent, toluene (250 g), TFMB (12.81 g; 40 mmol) as a diamine, and SiDA (7.7 g) as a silicon-containing monomer were added while stirring, and then PMDA (3.27 g; 15 mmol) and 6FDA (6.66 g; 15 mmol) as an acid dianhydride were added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0629] Then, the mixture was cooled to room temperature, and TFMB (18.25 g; 57 mmol) as a diamine was added while stirring. Then, PMDA (15.27 g; 70.0 mmol) as an acid dianhydride was added, and the mixture was stirred at room temperature for 24 hours. The toluene was distilled off under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized (L / M=70 / 30 mol%) polyimide precursor (hereinafter also referred to as PAI).

[0630] The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and n-butylbenzene was added as an auxiliary solvent to give 30 wt% of the total solvent and to give 10 wt% of the solid content.

[0631] 《Examples 41, 43, 45, 47, 49, 60, 62, 64, 66, 68, 70, 72, 78, 80, 98, 100, 102, 104, 106, 108, 110, 115, 152, 154, 156, 158, 160, 162, 172, 174, 176, 178, 180, 182, 184, 191, 193, 211, 213, 215, 217, 219, 221, 223, 228, 230, 232 and 234》

[0632] A varnish was obtained in the same manner as in Example 39 except that the co-solvent described in Table 1 was used instead of n-butylbenzene as the co-solvent.

[0633] 《Example 116》

[0634] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (200 g) as a main solvent, toluene (150 g), 4,4-DAS (12.4 g; 50 mmol) and 3,3-DAS (7.4 g; 30 mmol) as diamines, and SiDA (7 g) were added while stirring, and then ODPA (31.0 g; 100 mmol) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0635] Then, the mixture was cooled to room temperature, 4,4-DAS (14.42 g; 58.1 mmol) and 3,3-DAS (9.61 g; 38.7 mmol) as diamines were added with stirring, and the mixture was stirred at room temperature for 24 hours. The toluene was distilled off under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized (L / M=80 / 20 mol%) polyimide precursor (PAI).

[0636] The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and ethoxybenzene was added as an auxiliary solvent so as to be 30 wt% of the total solvent and so as to be 15 wt% of the solid content.

[0637] 《Examples 117 to 123, 128 to 133 and 137》

[0638] A varnish was obtained in the same manner as in Example 116 except that the main solvent described in Table 1 was used instead of NMP as the main solvent.

[0639] 《Examples 124 to 127》

[0640] A varnish was obtained in the same manner as in Example 116 except that the content ratio of the auxiliary solvent was changed as shown in Table 1.

[0641] 《Example 134》

[0642] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and GBL (200 g) as a main solvent, toluene (150 g), 4,4-DAS (14.42 g; 58.1 mmol) and 3,3-DAS (9.61 g; 38.7 mmol) as diamines, and SiDA (7 g) were added while stirring, and then ODPA (31.02 g; 100 mmol) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0643] Then, the mixture was cooled to room temperature, stirred at room temperature for 24 hours, and toluene was distilled off under reduced pressure to obtain a GBL solution (hereinafter also referred to as varnish) of polyimide (hereinafter also referred to as PI). The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and ethoxybenzene was added as a cosolvent in such a manner as to be 30 wt% of the total solvent, and was added and used in such a manner as to be 15 wt% of the solid content.

[0644] 《Example 135》

[0645] After adding the same components as in the above-mentioned Example 134 at room temperature, the mixture was stirred at room temperature for 24 hours, heated at 180°C and toluene was distilled off under reduced pressure. The same operations were performed as in Example 116 to obtain a GBL solution (hereinafter also referred to as varnish) of a polyimide precursor (hereinafter also referred to as PAA).

[0646] 《Example 136》

[0647] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and GBL (200 g) as a main solvent, toluene (80 g), 4,4-DAS (12.4 g; 50 mmol) and 3,3-DAS (7.4 g; 30 mmol) as diamines, and SiDA (7 g) were added while stirring, and then ODPA (31.02 g; 100 mmol) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 180°C, and the mixture was heated under reflux at 180°C for 3 hours to carry out imidization.

[0648] Then, the mixture was cooled to room temperature, ethoxybenzene (70 g) was added as a synthetic solvent as an auxiliary solvent, 4,4-DAS (2.01 g; 8.1 mmol) and 3,3-DAS (2.16 g; 8.7 mmol) as diamines were added while stirring, and the mixture was stirred at room temperature for 24 hours. The toluene was distilled off under reduced pressure to obtain a solution (hereinafter also referred to as varnish) in which a part of the imidized (L / M=80 / 20 mol%) polyimide precursor (PAI) was dissolved in GBL.

[0649] The obtained varnish was stored in a freezer (set temperature: -20°C), thawed during performance evaluation, and ethoxybenzene was added as an auxiliary solvent so as to be 30 wt% of the total solvent and so as to be 15 wt% of the solid content.

[0650] 《Examples 138-151, 153, 155, 157, 159, 161, 163-171, 173, 175, 177, 179, 181, 183, 185-190, 192, 194-210, 212, 214, 216, 218, 220, 222 and 224-227》

[0651] A varnish was obtained in the same manner as in Example 116, except that GBL was used as the main solvent instead of NMP, and the auxiliary solvent described in Table 1 was used as the auxiliary solvent instead of ethoxybenzene.

[0652] Comparative Example 1

[0653] A beaded condenser equipped with a moisture separation trap was attached to a 2-liter separable three-necked flask equipped with a stainless steel anchor-type stirrer.

[0654] Add 67.96 g (360 mmol) of bis(3,4-dicarboxyphenyl)ether acid dianhydride (manufactured by MANAC) (hereinafter referred to as ODPA), 165.24 g (180 mmol) of diaminosiloxane compound BY16-853U (manufactured by Toray Dow Corning) (amino equivalent of 459, hereinafter referred to as BY16), 4.33 g (43 mmol) of γ-valerolactone, 6.83 g (86 mmol) of pyridine, 235.2 g of n-butyl benzoate, and 100.8 g of γ-butyrolactone. Stir at room temperature and nitrogen atmosphere at 180 rpm for 30 minutes, then heat to 180°C and stir for 1 hour. Remove water during the reaction.

[0655] Then, the mixture was cooled, and ODPA 22.34 g (72 mmol), 1,3-bis(3-aminophenoxy)benzene (Mitsui Chemicals, Inc.) (hereinafter referred to as APB) 63.15 g (216 mmol), 1,3-bis(4-aminophenoxy)benzene (Wakayama Seika Industries, Ltd.) (hereinafter referred to as TPE-R) 10.52 g (36 mmol), a mixed solvent of 140 g of n-butyl benzoate as a synthetic solvent and 60 g of γ-butyrolactone as a main solvent were added for the second time, and the mixture was stirred at 180° C. and 180 rpm for 5 hours. During the reaction, refluxed materials such as water were removed from the system to obtain a polyimide solution containing an organic silicon group having a concentration of 41% by mass.

[0656] 325 g of n-butyl benzoate was added to 900 g of the synthesized polyimide solution containing an organic silicon group to obtain a composition. The composition contained 77.9 wt % of n-butyl benzoate.

[0657] In addition, the resin composition of Comparative Example 1 corresponds to the composition described in Patent Document 1.

[0658] Comparative Example 2

[0659] A varnish was obtained in the same manner as in Example 1 except that sulfolane was used as a co-solvent.

[0660] 《Comparative Example 3》

[0661] A varnish was obtained in the same manner as in Example 1 except that n-butylbenzene was not used as a co-solvent.

[0662] 《Comparative Example 4》

[0663] A varnish was obtained in the same manner as in Example 1 except that cyclohexanone was used as the main solvent instead of NMP.

[0664] 《Comparative Example 5》

[0665] A varnish was obtained in the same manner as in Example 1 except that the amounts of the main solvent and the auxiliary solvent were changed to the content ratios described in Table 1.

[0666] It should be noted that note *1 in Table 1 indicates that the mixing ratio of the main solvents in Examples 24 and 137 is 50 wt% / 50 wt%, and *2 indicates that the mixing ratio of the auxiliary solvents in Examples 25 and 138 is 50 wt% / 50 wt%.

[0667] (Components used in Examples and Comparative Examples)

[0668] 〈Acid dianhydride〉

[0669] BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride

[0670] PMDA: Pyromellitic anhydride

[0671] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0672] ODPA: 4,4'-oxydiphthalic dianhydride (bis-(3,4-dicarboxyphenyl) ether acid dianhydride)

[0673] CpODA: Norbornane 2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride

[0674] 6FDA: 4,4'-(hexafluoroisopropylidene) diphthalic anhydride

[0675] 〈Diamine〉

[0676] BAFL: 9,9-bis(4-aminophenyl)fluorene

[0677] pPD: p-phenylenediamine

[0678] mPD: meta-phenylenediamine

[0679] 3,3-DAS: 3,3-diaminodiphenyl sulfone

[0680] 4,4-DAS: 4,4-diaminodiphenyl sulfone

[0681] APAB: 4-aminophenyl-4-aminobenzoate

[0682] TFMB: 2,2'-bis(trifluoromethyl)benzidine

[0683] APB: 1,3-bis(3-aminophenoxy)benzene

[0684] TPE-R: 1,3-bis(4-aminophenoxy)benzene

[0685] 〈Monomers containing silicon element〉

[0686] SiDA: (a compound in which, in the general formula (17), L1 and L2 are amino groups (-NH2), R1 is trimethylene (-CH2CH2CH2-), R2 and R3 are methyl groups, i is a positive integer, j and k are 0, and the functional group equivalent is 2200)

[0687] General formula (17):

[0688]

[0689] 〈Main solvent〉

[0690] NMP: N-methyl-2-pyrrolidone

[0691] DMF: N,N-dimethylformamide

[0692] DMAc: N,N-dimethylacetamide

[0693] 1,3-Dimethylimidazolidinone

[0694] Tetramethylurea

[0695] 3-Methoxy-N,N-dimethylpropionamide

[0696] 3-Butoxy-N,N-dimethylpropionamide

[0697] γ-Butyrolactone

[0698] γ-Valerolactone

[0699] Hexamethylphosphoramide

[0700] Dimethyl sulfoxide

[0701] Sulfolane

[0702] Pyridine

[0703] Pyridine

[0704] 〈Co-solvent〉

[0705] n-Butylbenzene

[0706] Cyclopropene

[0707] Cyclopentene

[0708] Ethylbenzyl sulfide

[0709] Cyclohexene

[0710] Diethyl sulfide

[0711] Cycloheptane

[0712] Ethylbenzene

[0713] 1,8-Cineole

[0714] Dipentene

[0715] Tributyl borate

[0716] Benzyl methacrylate

[0717] Furan

[0718] Phenylacetylene

[0719] Ethoxybenzene

[0720] Dihexyl phthalate

[0721] Methyl benzoate

[0722] 1-Menthone

[0723] Dioctyl adipate

[0724] 1-Menthyl acetate

[0725] Diisononyl adipate

[0726] Tert-Butylbenzene

[0727] 1,4-Cineole

[0728] Benzyl methyl ether

[0729] Isopropoxybenzene

[0730] tert-Butyloxybenzene

[0731] Propoxybenzene

[0732] Benzaldehyde dimethyl acetal

[0733] Amylbenzene

[0734] Butoxybenzene

[0735] Benzyl isobutyl ether

[0736] Tert-Butyl Benzoate

[0737] Benzyl butyl ether

[0738] Benzaldehyde diethyl acetal

[0739] Hexylbenzene

[0740] Cyclohexylbenzene

[0741] Isobutyl benzoate

[0742] Ethyl benzoate

[0743] Propyl benzoate

[0744] Tolan

[0745] Ethyl cinnamate

[0746] Diethylhexyl phthalate

[0747] Diisoheptyl phthalate

[0748] Diisononyl phthalate

[0749] Benzyl benzoate

[0750] 2-Methyltetrahydrofuran

[0751] Cyclopentyl methyl ether

[0752] p-Xylene

[0753] Cumene

[0754] d-Limonene

[0755] Toluene

[0756] Styrene

[0757] a-Methylstyrene

[0758] 2-Methylcyclohexanone

[0759] 3-Methylcyclohexanone

[0760] 2-Vinyltoluene

[0761] Isophorone

[0762] Diisodecyl phthalate

[0763] Propylbenzene

[0764] Isobutylbenzene

[0765] 4-Methylstyrene

[0766] 2-Ethylstyrene

[0767] 2-Isopropylstyrene

[0768] Isopropyl benzoate

[0769] 4-tert-Butylstyrene

[0770] Cycloheptanone

[0771] 4-Ethylstyrene

[0772] 4-Isopropylstyrene

[0773] 2-Propylstyrene

[0774] Butyl benzoate

[0775] Dibutyl Sebacate

[0776] 〈Name of polymer type〉

[0777] PAA: Polyimide Precursor

[0778] PI: Polyimide

[0779] PAI: partially imidized polyimide precursor

[0780] [Table 1-1]

[0781]

[0782] [Table 1-2]

[0783]

[0784] [Table 1-3]

[0785]

[0786] [Table 1-4]

[0787]

[0788] [Table 1-5]

[0789]

[0790] [Table 1-6]

[0791]

[0792] [Table 1-7]

[0793]

[0794] [Table 1-8]

[0795]

[0796] [Table 1-9]

[0797]

[0798] [Table 1-10]

[0799]

[0800] [Table 1-11]

[0801]

[0802] [Table 1-12]

[0803]

[0804] [Table 1-13]

[0805]

[0806] [Table 1-14]

[0807]

[0808] [Table 1-15]

[0809]

[0810] [Table 1-16]

[0811]

[0812] [Table 1-17]

[0813]

[0814] [Table 1-18]

[0815]

[0816] *1 Mixing ratio 50wt% / 50wt% *2 Mixing ratio 50wt% / 50wt%

[0817] [Table 1-19]

[0818]

[0819] [Table 1-20]

[0820]

[0821] [Table 1-21]

[0822]

[0823] [Table 1-22]

[0824]

[0825] [Table 1-23]

[0826]

[0827] [Table 1-24]

[0828]

[0829] As shown in Table 1, the polyimide obtained from the resin composition of the example has both low YI (transparency) and filterability as compared with the comparative example, and is excellent in the properties required for display applications.

[0830] The resin composition of Comparative Example 1 corresponds to the composition described in Patent Document 1, and has low YI (transparency), filterability, and filtration rate of D, "1", and "d", and cannot achieve all the properties.

[0831] The resin composition of Comparative Example 2 is a resin composition using an auxiliary solvent whose Hansen solubility parameter does not meet the specific range. In terms of low YI (transparency) and filterability, the YI value is A, but the filterability and filtration speed are "1" and "d", and all characteristics cannot be taken into account.

[0832] The resin composition of Comparative Example 3 is a resin composition when a co-solvent is not used, and in terms of low YI (transparency) and filterability, the YI value is A, but the filterability and filtration speed are "1" and "d", and each characteristic cannot be taken into account. Comparative Example 3 without a co-solvent can not exert the effect (filterability, etc.) of the present embodiment.

[0833] The resin composition of Comparative Example 4 is a resin composition in which a solvent other than a specific solvent selected from the group consisting of N-methyl-2-pyrrolidone (NMP) and the like is used as a main solvent, and the low YI (transparency) is D.

[0834] In addition, the resin composition of Comparative Example 4 had precipitation of the polyimide polymer and had poor filterability of "1", so that various properties could not be achieved at the same time.

[0835] In Comparative Example 5, the content of n-butylbenzene as the auxiliary solvent was 55 wt % or more of the total solvent, and the YI value was A, but the filterability was as poor as "1" and the filtration speed was as poor as "d", and both properties could not be achieved.

[0836] The reason for the deterioration of filterability in Comparative Examples 3 and 4 is not clear, but it is believed that the cause is the presence of a trace amount of ultrahigh molecular weight polymer. From the perspective of Hansen solubility parameters, it is known that if the solubility of the polymer is sought, the SP value used for the main solvent is close, and the polymer has the property of being easily soluble in the main solvent.

[0837] However, although the co-solvents of Comparative Examples 3 and 4 have high solubility in the polymer, the filterability still deteriorates. It is generally known that the solubility of a polymer decreases as it becomes a high molecular weight body. Therefore, it can be seen that even if it is a good solvent, the ultra-high molecular weight polymer will present a fine gel state, which fills the pores inside the filter paper and deteriorates the filterability.

[0838] As a solution, there is the addition of the auxiliary solvent shown in the examples. From the viewpoint of Hansen solubility parameters, the auxiliary solvent in the examples is a poor solvent for the polymer, and the solubility of the polymer can be maintained by adjusting the addition ratio of the auxiliary solvent to the main solvent which is a good solvent.

[0839] It was found that the gel-like ultrahigh molecular weight polymer, which is believed to cause deterioration of filterability, was liquefied by the influence of the auxiliary solvent as a poor solvent. The liquefied ultrahigh molecular weight polymer did not stay on the surface of the filter paper and clog the pores, thereby improving the filterability.

[0840] In the present application, a resin composition is obtained by using a specific main solvent and an auxiliary solvent having a Hansen solubility parameter within a specific range. The resin composition can take into account both filterability and low YI (transparency) properties and can be suitably used as a polyimide film that can be applied to display processes such as LTPS (low-temperature polycrystalline silicon) and LTPO (low-temperature polycrystalline oxide).

Claims

1. A resin composition comprising a resin and a solvent, wherein the resin comprises a structural unit represented by the following general formula (1) and / or general formula (2), and comprises a structure derived from a silicon-containing compound represented by the following general formula (3), In formula (1), P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer. In formula (2), P3 represents a divalent organic group, P4 represents a tetravalent organic group, q represents a positive integer, In formula (3), R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200. The solvent comprises a main solvent and a co-solvent, The main solvent comprises at least one selected from the group consisting of the following solvents: N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, methylpyridine and pyridine, The Hansen solubility parameters of the co-solvent satisfy the following: δD=16.5~18.9、 δP=0.1~8.2、 δH=1.1~5.5, When the total amount of the solvent is set to 100% by mass, the auxiliary solvent is less than 50% by mass.

2. The resin composition according to claim 1, wherein The Hansen solubility parameters of the co-solvent satisfy the following: δD=16.5~18.4、 δP=0.1~5.6、 δH=1.1~4.

7.

3. The resin composition according to claim 1 or 2, wherein The auxiliary solvent comprises a solvent selected from the group consisting of n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether , isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenyl acetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate and benzyl benzoate. At least one of the group consisting of.

4. The resin composition according to claim 1 or 2, wherein The auxiliary solvent comprises a solvent selected from the group consisting of n-butylbenzene, cyclopropene, cyclopentene, ethylbenzyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, tert-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, pentylbenzene, butoxybenzene, benzyl isobutyl ether, tert-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, At least one member selected from the group consisting of ethyl benzoate, propyl benzoate, tolan, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, α-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-tert-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene and 2-propylstyrene.

5. The resin composition according to claim 1 or 2, wherein The boiling point of the auxiliary solvent is lower than 250°C.

6. The resin composition according to claim 1 or 2, wherein The auxiliary solvent includes at least one selected from the group consisting of n-butylbenzene and ethoxybenzene.

7. The resin composition according to claim 1 or 2, wherein The P1 and / or P3 comprise a structural unit derived from the following general formula (4), 8. The resin composition according to claim 1 or 2, wherein The P2 and / or P4 comprise a structural unit derived from the following general formula (5), 9. The resin composition according to claim 1 or 2, wherein The P1 and / or P3 comprise a structural unit derived from the following general formula (6), 10. The resin composition according to claim 1 or 2, wherein When the total amount of the solvent is 100% by mass, the auxiliary solvent is 5% by mass or more and 40% by mass or less.

11. The resin composition according to claim 1 or 2, wherein When the total amount of the solvent is 100% by mass, the auxiliary solvent is 5% by mass or more and 30% by mass or less. 12 . The resin composition according to claim 1 , which is used for a substrate of a flexible display. 13 . A display comprising a thin film transistor (TFT) substrate and / or a color filter substrate obtained using the resin composition according to claim 1 or 2 .

14. A method for producing a resin composition, wherein: The resin composition contains a resin and a solvent, wherein the resin contains a structural unit represented by the following general formula (1) and / or general formula (2), and contains a structure derived from a silicon-containing compound represented by the following general formula (3), In formula (1), P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer. In formula (2), P3 represents a divalent organic group, P4 represents a tetravalent organic group, q represents a positive integer, In formula (3), R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200. The method for preparing the resin composition comprises: A step of synthesizing the resin using at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoramide, dimethyl sulfoxide, sulfolane, picoline and pyridine as a main solvent; and After the resin is synthesized and before filtering, a co-solvent satisfying the following Hansen solubility parameters is added to prepare a resin composition, δD=16.5~18.9、 δP=0.1~8.2、 δH=1.1~5.

5.

15. A method for producing a polyimide resin film, comprising: A coating step of coating the resin composition according to claim 1 or 2, or the resin composition obtained by the method according to claim 14, on the surface of the support; a film forming step of heating the resin composition to form a polyimide resin film; a peeling step of peeling the polyimide resin film from the support; and an irradiation treatment of irradiating the polyimide resin film with a laser beam from the support body side before the peeling step.

16. A method for manufacturing a display, comprising: A coating step of coating the resin composition according to claim 1 or 2, or the resin composition obtained by the method according to claim 14, on the surface of the support; a film forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; and The peeling step is to peel the polyimide resin film on which the element is formed from the support.

17. A method for manufacturing a laminate, comprising: A coating step of coating the resin composition according to claim 1 or 2, or the resin composition obtained by the method according to claim 14, on the surface of the support; a film forming step of heating the resin composition to form a polyimide resin film; and The device forming step is to form a device on the polyimide resin film.

18. A method for manufacturing a laminate, comprising: A coating step of coating the resin composition according to claim 1 or 2, or the resin composition obtained by the method according to claim 14, on the surface of the support; a film forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; and A peeling step of peeling the polyimide resin film on which the element is formed from the support.

19. A resin composition comprising a resin and a solvent, wherein the resin comprises a structural unit represented by the following general formula (1) and / or general formula (2), and comprises a structure derived from a silicon-containing compound represented by the following general formula (3), In formula (1), P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer. In formula (2), P3 represents a divalent organic group, P4 represents a tetravalent organic group, q represents a positive integer, In formula (3), R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200. The solvent comprises one or more mixed solvents, The Hansen solubility parameters of the mixed solvent satisfy the following: δD=16.8~18.8、 δP=6.8~9.8、 δH=4.5~6.8.