Ship lock U-shaped side wall pouring cooling system and construction method

By adopting a reverse vertical and vertical cooling water pipe system in the construction of the U-shaped side wall of the ship lock, combined with efficient crack-resistant composite materials, the crack problem caused by temperature deformation in large-volume concrete is solved, and the internal temperature of the concrete is achieved. Accurate control significantly reduces crack generation.

CN118880840APending Publication Date: 2024-11-01CCCC SHEC FOURTH ENG +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410654929.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Large volume concrete is prone to cracks during construction, mainly due to temperature deformation and shrinkage deformation, and it is difficult for the prior art to effectively control the generation of cracks.

Method used

A U-shaped side wall casting cooling system was designed, using two layers of reverse vertical cooling water pipes and two vertical cooling water pipes, combining efficient crack-resistant composite materials and an optimized cooling water circulation system to monitor the internal temperature of the concrete in real time. Reduce cracks through scientific temperature control measures.

Benefits of technology

It effectively reduces the occurrence of concrete cracks, improves construction quality and structural stability, and achieves precise control of the internal temperature of large volume concrete by optimizing the coordination between cooling system and crack-resistant materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880840A_ABST
    Figure CN118880840A_ABST
Patent Text Reader

Abstract

The invention discloses a ship lock U-shaped side wall pouring cooling system and an arrangement method.The cooling system comprises a lock chamber and two layers of cooling water pipes arranged on a lock head bottom plate, the two layers of cooling water pipes are oppositely and perpendicularly arranged, a layer of cooling water pipe is arranged at the chamfer position of a lock chamber wall and arranged to be a single loop, and the lock chamber wall is provided with two layers of vertical cooling water pipes; the cooling water pipe on the soil facing side does not need to be disconnected at the position of the floating bollard and is arranged to be a single loop, the cooling water pipe on the water facing side is disconnected at the position of the floating bollard and is arranged to be a double loop, and both inlets and outlets of the cooling water pipes adopt two-way water stop valves. The construction method comprises the steps of concrete pouring, concrete vibrating and cooling water pipe arrangement. By optimizing the mix proportion design of the mass concrete and adding the efficient anti-crack composite material, a scientific basis is provided for adjusting internal temperature control measures of the concrete, the internal temperature of the mass concrete can be dynamically monitored in real time, a cooling water circulation system is adjusted, and concrete cracks can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mass concrete construction, and in particular to a ship lock U-shaped side wall casting cooling system and an installation method. Background Art

[0002] With the development of my country's water transport industry and the increase in navigation demand, the scale of ship lock construction has gradually developed towards large-scale, and large-volume concrete has become more and more common. Cracks in large-volume concrete are mainly caused by temperature deformation and shrinkage deformation. The types of cracks and their main causes are analyzed as follows: (1) Surface cracks. In the early stage of pouring large-volume concrete, a large amount of cement hydration heat is generated, causing the temperature of the concrete to rise rapidly. However, due to the good heat dissipation conditions on the surface of the concrete, the heat can be dissipated into the atmosphere, and its temperature rise is small; while due to the poor heat dissipation conditions inside the concrete, the heat is not easy to dissipate, and its temperature rise is large. The high temperature inside the concrete and the low surface temperature form a temperature gradient, which causes compressive stress inside the concrete and tensile stress on the surface. When the tensile stress exceeds the ultimate tensile strength of the concrete, cracks will appear on the concrete surface. (2) Through cracks. In the early stage of pouring large-volume concrete, the concrete is in a heating stage and plastic state, with a very small elastic modulus, and the stress caused by deformation changes is very small, and the temperature stress can generally be ignored. (3) Deep cracks. The concrete within the foundation constraint range is in a state of large-area tensile stress. If surface cracks occur in this area, they are very likely to develop into deep cracks or even through cracks. How to control the occurrence of large-volume concrete cracks has become one of the urgent problems to be solved in the construction field. Summary of the invention

[0003] The object of the present invention is to provide a cooling system and installation method for casting a U-shaped side wall of a ship lock, which can control the generation of cracks in large-volume concrete.

[0004] In one aspect of the present invention, the present invention proposes a cooling system for casting the U-shaped side wall of a ship lock. According to an embodiment of the present invention, the lock chamber and the lock head bottom plate are provided with two layers of cooling water pipes, and the two layers of cooling water pipes are arranged vertically in opposite directions, a layer of cooling water pipes is provided at the chamfer of the lock chamber wall, and is provided as a single circuit, and two layers of vertical cooling water pipes are provided on the lock chamber wall, the cooling water pipe on the soil side does not need to be disconnected at the position of the floating mooring column, and is provided as a single circuit, the cooling water pipe on the water side is disconnected at the position of the floating mooring column, and is provided as a double circuit, and two-way water stop valves are used at the inlet and outlet of the cooling water pipe.

[0005] In another aspect of the present invention, the present invention provides a method for casting a U-shaped side wall of a ship lock. According to an embodiment of the present invention, the method comprises the following steps:

[0006] S1. Concrete pouring

[0007] S101, Concrete pouring of upper and lower gate bottom slabs

[0008] The bottom plates of the upper and lower gates are cast in layers. The first casting is for the side slope section of the gate chamber, the second casting is for the 3.5m high solid section, and the third casting is for the bottom of the side pier.

[0009] S102, Lock Chamber Concrete Pouring

[0010] a. Casting of the chamber bottom slab

[0011] The standard section of the lock chamber bottom plate is cast in one step, and the lock chamber and gate head connection section is cast in two steps. The lock chamber bottom plate concrete is cast on both sides at the same time. After the left and right bottom plates are cast, the middle plate is cast.

[0012] b. Casting of chamber wall

[0013] After the chamber bottom plate is poured, the chamfered part is poured to 0.15m above the chamber wall. The single-segment chamber wall is symmetrically cast on both sides at one time using a mobile mold machine;

[0014] S2. Concrete Vibration

[0015] S3. Cooling water pipe layout

[0016] Two layers of cooling water pipes are set on the lock chamber and the bottom plate of the gate head, and the two layers of cooling water pipes are arranged vertically in opposite directions. A layer of cooling water pipes is set at the chamfer of the lock chamber wall and is set as a single circuit. Two vertical layers of cooling water pipes are set on the lock chamber wall. The cooling water pipe on the soil side does not need to be disconnected at the floating mooring column position and is set as a single circuit. The cooling water pipe on the water side is disconnected at the floating mooring column position and is set as a double circuit. Two-way water stop valves are used at the inlet and outlet of the cooling water pipe to cool the concrete by passing water through the cooling water pipe.

[0017] In addition, the method for casting the U-shaped side wall of a ship lock according to the above embodiment of the present invention may also have the following additional technical features:

[0018] In some embodiments of the present invention, in step S1, the concrete includes the following components in parts by weight: 176 parts of cement, 64 parts of fly ash, 80 parts of slag powder, 696 parts of sand, 1227 parts of crushed stone, 138 parts of water, 2.84 parts of admixture, and 26 parts of anti-cracking expansion agent.

[0019] In some embodiments of the present invention, the admixture is a polycarboxylic acid high-performance water reducer, and the anti-cracking expansion agent is a HEA anti-cracking agent.

[0020] In some embodiments of the present invention, in step S3, the cooling water pipes of each layer are arranged in an S shape, the cooling water pipes are made of PE hoses, and hot-melt joints are used.

[0021] In some embodiments of the present invention, in step S3, a layer of cooling water pipes is provided at the chamfer of the lock chamber wall, which is set as a single circuit; two vertical layers of cooling water pipes are provided on the lock chamber wall, and the cooling water pipes on the soil-facing side do not need to be disconnected at the floating mooring column position and are set as a single circuit, while the cooling water pipes on the water-facing side need to be disconnected at the floating mooring column position and are set as a double circuit.

[0022] In some embodiments of the present invention, temperature measurement is also included, and the measurement points are arranged as follows:

[0023] The location and number of measuring points at the gate head: According to the needs of temperature control and crack prevention during the construction period, 5 measuring positions and 20 measuring points are set on the left, middle and right bottom plates of the gate head;

[0024] Location and number of measuring points in the lock chamber: According to the needs of temperature control and crack prevention during the construction period, 15 measuring points are set up, with one layer arranged every 10-15m along the mileage direction.

[0025] In some embodiments of the present invention, after the bottom slab concrete is finished, hot water from the cooling water pipe outlet is immediately used to sprinkle water on the surface to replenish surface moisture and prevent water loss and shrinkage. Thereafter, the surface is immediately covered with a layer of plastic film, and then covered with a 20 mm thick straw bag. A layer of rainproof plastic film or a one-cloth-one-film geomembrane or a 20 mm rubber-plastic sponge is added on the straw bag. The insulation time should be determined according to the construction environment temperature.

[0026] In some embodiments of the present invention, the chamber wall insulation method comprises the following steps:

[0027] 1) Cover the top of the chamber wall with a quilt, and cover the back ribs of the formwork on the water-facing and soil-facing sides with insulation cotton. Mainly maintain the formwork with the formwork removed, and extend the formwork removal time to 5-7 days;

[0028] 2) Take windproof measures outside the formwork to prevent the concrete surface from cooling too quickly and causing a large temperature difference between the inside and outside. If the formwork needs to be removed, do it when the temperature is highest on that day;

[0029] 3) If the on-site formwork needs to be removed in advance, insulation and moisture retention measures should be taken on the side facades after the formwork is removed, and 20mm rubber-plastic sponge should be used for wrapping after the formwork is removed;

[0030] 4) When encountering adverse weather conditions such as strong winds and dryness, close attention should be paid to the moisture retention of concrete during the demolding process. After demolding, the concrete surface should be covered in time and watered for maintenance;

[0031] 5) After the concrete water cooling work is completed, with the consent of the owner and the supervisor, the cooling water pipe can be sealed with mortar, and then the exposed part of the serpentine pipe can be cut off and processed to meet the aesthetic requirements of the concrete surface.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention optimizes the conventional cooling system by optimizing the mix design of large-volume concrete and adding high-efficiency anti-cracking composite materials, thereby improving the rationality of the internal cooling water pipe layout, the flexibility of the cooling water circulation system, the frequency, accuracy and timeliness of temperature data collection, and providing a scientific basis for adjusting the internal temperature control measures of concrete. The present invention can dynamically monitor the internal temperature of large-volume concrete in real time and adjust the cooling water circulation system, thereby effectively reducing the occurrence of concrete cracks. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of layered push-type casting in an embodiment of the present invention;

[0035] Figure 2 This is a schematic diagram of the first pouring of the upper gate head in an embodiment of the present invention;

[0036] Figure 3 This is a schematic diagram of the first pouring of the lower gate head in an embodiment of the present invention;

[0037] Figure 4 is a schematic diagram of the bottom plate layering in an embodiment of the present invention;

[0038] Figure 5 1. It is a schematic diagram of the casting layers of the gate chamber and gate head connection section in an embodiment of the present invention;

[0039] Figure 6 Schematic diagram of the casting layers of the standard section of the gate chamber in the embodiment of the present invention;

[0040] Figure 7 This is a cross-sectional view of the cooling water pipe arrangement of the gate head bottom plate in an embodiment of the present invention;

[0041] Figure 8 This is a first-layer plan view of the cooling water pipe arrangement on the bottom plate of the gate head according to an embodiment of the present invention;

[0042] Fig. 9 This is a second-layer plan view of the cooling water pipes on the bottom plate of the gate in an embodiment of the present invention;

[0043] Fig.10 2. It is a cross-sectional view of the arrangement of cooling water pipes of the lock chamber bottom plate in an embodiment of the present invention;

[0044] Fig.11 2. It is a cross-sectional view of the arrangement of cooling water pipes for the lock chamber wall in an embodiment of the present invention;

[0045] Fig.12 This is a plan view of the cooling water pipe arrangement at the chamfer of the lock chamber wall in an embodiment of the present invention;

[0046] Fig.13 This is a vertical layout diagram of cooling water pipes on the soil-facing side of the lock chamber wall in an embodiment of the present invention;

[0047] Fig.14This is a vertical layout diagram of cooling water pipes on the water-facing side of the lock chamber wall in an embodiment of the present invention;

[0048] Fig.14 In the figure, the left figure is a diagram showing the arrangement of temperature measuring points on the left bottom plate in an embodiment of the present invention, and the right figure is a diagram showing the arrangement of temperature measuring points on the middle bottom plate;

[0049] Fig.15 It is a cross-sectional view of the arrangement of the temperature measuring points on the bottom plate in an embodiment of the present invention;

[0050] Fig.16 : is a layout diagram of temperature measurement points in the lock chamber in an embodiment of the present invention;

[0051] Fig.17 1 is a layout diagram of temperature measurement points in the lock chamber in an embodiment of the present invention.

[0052] In the figure, 1, the bottom plate of the gate head, 101, the bottom plate of the left side of the gate head, 102, the middle bottom plate of the gate head, 103, the bottom plate of the right side of the gate head, 2, cooling water pipe, 3, lock chamber wall, 4, floating mooring column, DETAILED DESCRIPTION

[0053] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0054] A ship lock U-shaped side wall casting cooling system and installation method, comprising the following steps:

[0055] 1. Determination of concrete mix ratio

[0056] 1.1 Determine the test strength (Mpa)

[0057] fcu,o≥32.4(Mpa).

[0058] 1.2 Calculation of water-cement ratio

[0059] Selected benchmark water-cement ratio: W / B=0.47.

[0060] 1.3 Determine the amount of water and admixtures

[0061] According to the designed slump (100-140) mm, the water consumption of concrete with a slump of 90 mm in Table 5.2.1-2 of (JGJ 55-2011) is used as the basis to calculate the water consumption of concrete without admixtures. wo =215kg, m is determined based on tests and experience wo =220kg.

[0062] The water reduction rate of admixture is calculated as 27%.

[0063] The dosage is 1.2% of the gel material.

[0064] Water consumption for admixture m wO =220×(1-27%)=160kg / m 3 .

[0065] 1.4 Determine the amount of gel material per cubic meter of concrete

[0066] m bO =m wO / (W / B)=160 / 0.47=340(kg / m 3 ),

[0067] According to experience, the amount of fly ash is determined to be 31%, m f o=340×31%=105kg / m 3

[0068] The cement consumption is m co =m b0 -m f0 =340-105=235kg / m 3 .

[0069] 1.5 Determine the sand ratio (βs)

[0070] The sand ratio βs is determined to be 38%.

[0071] 1.6 Calculate the amount of various materials in the theoretical mix ratio by weight

[0072] Assume that the weight of concrete mixture per cubic meter is m cp =2400kg

[0073] mcp=(m wO +m cO +m sO+ m gO )

[0074] β S =m sO / (m sO+ m gO )

[0075] 1.7 Determine the initial matching ratio as follows:

[0076] Cement: sand: crushed stone: fly ash: water reducing agent: anti-cracking agent: water = 235: 722: 1178: 105: 4.08: 27.2: 160 (kg / m 3 ).

[0077] The design mix ratio is shown in the following table:

[0078] Table 1 Theoretical mix proportion of mass concrete

[0079]

[0080] 1.8 Trial preparation, adjustment and determination of concrete mix ratio

[0081] The trial mixing is carried out on the basis of the calculated theoretical mix ratio. The performance of the concrete mixture is adjusted to meet the design and construction requirements. The slump, cohesiveness and water retention of the mixture with a water-cement ratio of W / B=0.47 meet the design requirements of the trial mix, and the amount of various materials in the design mix ratio is determined as follows:

[0082] Cement: sand: crushed stone: fly ash: water reducing agent: anti-cracking agent: water = 235: 722: 1178: 105: 4.08: 27.2: 160 (kg / m 3 ).

[0083] Among them, cement comes from Huainan Conch Cement Co., Ltd., variety: P.O42.5 grade; all technical indicators are qualified. Crushed stone is produced from Liuxing Mining in Jinzhai, Lu'an, Anhui Province; the maximum particle size is 31.5mm, using synthetic grading, (16-31.5) mm: (10-20) mm: (5-10) mm = 10%: 55%: 35% (mass ratio) to form a continuous grading, and all technical indicators are qualified. Natural sand is produced from: Lu'an Huoshan Yingjia Sand Field; fineness modulus: Mx = 2.5, all technical indicators are qualified. Admixtures are produced from Anhui Hengtong Admixture Co., Ltd., CH polycarboxylic acid high-performance water reducer (standard type), and all technical indicators are qualified. Anti-cracking agent is produced from Anhui Hengtong Admixture Co., Ltd., HEA anti-cracking agent, and all technical indicators are qualified. Fly ash is produced from Huainan Fengtai Power Plant, Class I fly ash, and all technical indicators are qualified. Water is domestic water, and all technical indicators are qualified.

[0084] 2. Concrete pouring

[0085] Before pouring concrete, sprinkle water on the foundation or construction joints to moisten them. Because the warehouse surface is large, pouring is carried out from far to near, layer by layer, with each section length of 5 to 8m and layer thickness of 300 to 500mm. When pouring, pour the previous layer of concrete before the next layer of concrete begins to set to avoid cold joints.

[0086] 2.1 Concrete pouring of upper and lower gate bottom plates

[0087] The upper and lower gate bottom plates are poured in layers. The first pouring is for the side slope section of the gate chamber, the second pouring is for the 3.5m high solid section (except for the middle bottom plate which is poured twice), and the third pouring is to the bottom of the side pier. The concrete volume of the upper gate bottom plate is about 14926.55m 3The first phase of the sluice gate has a concrete volume of approximately 14585.4m 3 The base plate concrete is poured on site using a belt conveyor + long-arm excavator.

[0088] (1) Figure 1 As shown in the figure, the gate head bottom plate is cast by the layered push-casting method of "one slope, thin layer casting, gradual advancement, and reaching the top at one time". The bottom plate casting is carried out in a period of time with lower temperature.

[0089] (2) The maximum single pouring volume of the gate head bottom plate is 1980m 3 Consider arranging 1 conveyor belt + 1 long-arm excavator for pouring, and pouring within the upstream or downstream navigation wall. Considering the need to reduce the pouring environment temperature of concrete, the concrete pouring is chosen to start at around 18:00, at a rate of 50m per hour. 3 Calculation of pouring speed: a total of 40 hours are needed, that is, the pouring time is from 18:00 to 10:00 on the third day. The order of concrete pouring is from far to near, from low to high.

[0090] (3) Overall pouring sequence: The upper and lower gates are constructed first at 15.9m on the gate chamber side, and then at 28.5m on the other side after the construction reaches the same elevation. Figure 2-3 shown.

[0091] After the first pouring is completed, the upper and lower gate bottom plates are poured in three times. Figure 4 As shown. The first floor is 3.5m, the second floor is 2.3m, and the third floor is 3.0m.

[0092] 2.2 Lock chamber concrete pouring

[0093] (1) Casting of the chamber bottom plate

[0094] The standard section thickness of the chamber bottom plate is 4m and is cast in one go. Figure 5 As shown, the thickness of the bottom plate of the connection section between the gate chamber and the gate head is 8.8m, which is cast in two times, the first casting is 4.4m, and the second casting is 4.4m; the concrete of the gate chamber bottom plate is cast on both sides at the same time. After the left and right bottom plates are cast, the middle plate is cast. The bottom plate concrete is plastic concrete, and it is cast on site using a belt conveyor + long-arm excavator;

[0095] The concrete of the lock chamber bottom slab is poured in the same way as the lock head bottom slab, with a maximum single pouring volume of 2080m 3 Considering the arrangement of 1 belt conveyor + 1 long-arm excavator for pouring, in order to reduce the pouring environment temperature of concrete, the concrete pouring is chosen to start at around 18:00, at a rate of 50m per hour. 3Calculation of pouring speed shows that a total of 41 hours are needed, that is, the pouring time is from 18:00 to 11:00 on the third day. The order of concrete pouring is from far to near, from low to high.

[0096] (2) Casting of chamber wall

[0097] After the chamber bottom plate is poured, the chamfered part is poured to 0.15m above the chamber wall (thickness 1.5m+0.15m), and a single segment chamber wall (wall height about 15.6m) is cast symmetrically on both sides at one time using a mobile mold machine. During the pouring, a pump truck is used to support the chamber bottom plate and alternately place the material on both sides.

[0098] The concrete is evenly distributed and poured in layers with a layer thickness of 30cm. During pouring, the pump pipe is extended with a hose (or a channeling tube is used), and the bottom of the hose is extended into the formwork to control the free fall height of the concrete to be no more than 2m. In order to avoid concentrated distribution of materials, which may cause the vibrator to drive the materials and cause aggregate separation, 5 distribution points are set on each side with a spacing of 4m. The position of the floating bollard is affected by the main beam of the mobile formwork and can be slightly biased to the side.

[0099] The pouring sequence of the standard section of the gate chamber is as follows: Figure 6 As shown, the pouring is divided into three times, the first pouring is 4m, the second pouring is 1.65m, and the third pouring is 15.6m.

[0100] 3. Concrete vibration

[0101] In order to increase the workability of concrete and ensure the quality of concrete construction, the vibration method is strictly controlled during concrete construction: three vibrating rods are arranged at each discharge port, and N70 is used with N100 insert vibrators for vibrating. The vibrators are inserted quickly and pulled out slowly, and the insertion points are evenly arranged and moved point by point with a moving spacing of 30 to 40 cm. When vibrating the upper layer, the lower layer should be inserted about 5 cm. The vibration duration of each vibration point should ensure that the concrete is sufficiently compacted, and no vibration is missed or over-vibrated. Start from the near mold, first outside and then inside, insert quickly and pull out slowly, and twitch up and down. The moving spacing is not greater than 1.5D of the vibration action radius. The vibrating rod should avoid steel bars, embedded parts, and templates as much as possible.

[0102] The bottom slab surface concrete should be vibrated twice to make it dense before initial setting. The elevation of the poured concrete surface should be measured before initial setting to ensure that the designed elevation is reached. After initial setting, the surface layer should be smoothed with a polisher and then manually polished for at least two times, and maintenance should be carried out in a timely manner.

[0103] 4. Cooling water pipe setting and temperature measurement

[0104] 4.1 Temperature control requirements and scope

[0105] During the curing period of large-volume concrete, the temperature difference between inside and outside must be strictly controlled to ensure that no harmful cracks appear. To ensure the quality of concrete, temperature control and curing are very critical processes. Temperature control measures should be taken according to climatic conditions, and the surface and internal temperature of the poured concrete should be measured as needed; at the same time, the following requirements should be met.

[0106] ① The concrete pouring temperature shall not be higher than 30℃ and not lower than 5℃;

[0107] ②The temperature difference between the inner and outer surfaces of concrete shall not exceed 25℃;

[0108] ③The maximum temperature inside the concrete is not higher than 70℃;

[0109] ④The cooling rate of concrete block shall not exceed 2℃ / d.

[0110] In order to ensure that no temperature cracks occur in the concrete, temperature control and maintenance measures are implemented on the large volume concrete of the lock.

[0111] 4.2 Cooling water pipe setting

[0112] According to the relevant specifications for mass concrete pouring and previous successful cases, when thermal insulation and moisture retention measures are taken during concrete maintenance, the use of cooling pipe circulating water in combination with the specific conditions of the project construction is the most effective measure for heat dissipation inside the concrete, and it is also the most fundamental method.

[0113] The solid structure thickness of the gate head bottom plate is 3.5m, the thickness of the standard section of the gate chamber bottom plate is 4m, and the thickness of the gate chamber wall is between 1.14m and 4.9m. They are all large-volume concrete structures. Conventional thermal insulation and moisture retention measures cannot better control the temperature of the concrete, so the temperature is controlled by adding cooling water pipes.

[0114] 4.2.1 Layout location

[0115] (1) Layout of bottom plate cooling water pipes

[0116] The cooling water pipes are all φ32mm high-density polyethylene cooling water pipes, arranged in an S shape. Figure 7 As shown, the cooling water pipes of the lock chamber and the bottom plate of the gate are arranged in two layers, with the horizontal spacing between the cooling pipes being 1.2 to 1.5 meters, the cooling pipes being 1 to 1.25 meters away from the bottom and top of the concrete, and 0.75 to 1.15 meters away from the edge of the concrete. The spacing between each layer is 1.5 meters, and the inlet and outlet are respectively arranged in the middle. The upper and lower layers are arranged in reverse vertical direction. Specifically, Figure 8 This is the first-level plan layout of the cooling water pipes on the bottom plate of the gate head. The left picture is the layout of the cooling water pipes in and out of the bottom plate on the left side of the gate head, with three groups of cooling water pipes arranged; the middle picture is the layout of the cooling water pipes in and out of the middle bottom plate of the gate head, with four groups of cooling water pipes arranged; the right picture is the layout of the cooling water pipes in and out of the bottom plate on the right side of the gate head, with three groups of cooling water pipes arranged. Fig. 9The second-layer plan layout of the cooling water pipes on the bottom plate of the gate head is shown in the left picture. The layout of the cooling water pipes in and out of the bottom plate on the left side of the gate head is arranged with four groups of cooling water pipes; the middle picture is the layout of the cooling water pipes in and out of the middle bottom plate of the gate head, with five groups of cooling water pipes; the right picture is the layout of the cooling water pipes in and out of the bottom plate on the right side of the gate head, with four groups of cooling water pipes. Fig.10 As shown, the cross-sectional view of the cooling water pipe arrangement on the bottom plate of the lock chamber is two layers, the rectangular frame is the bottom plate, and the two lines in the middle represent the cooling water pipes.

[0117] (2) Arrangement of cooling water pipes on the lock chamber wall

[0118] The thickness of the lock chamber wall is 1.2 to 4.9 meters. According to the requirements of cooling pipes in the Technical Code for Temperature Crack Control of Mass Concrete in Water Transport Engineering JTS202-1-2010, φ32mm high-density polyethylene cooling water pipes are used within the range of 10.74 to 25.93 meters in elevation, and arranged in an S shape;

[0119] like Fig.12 As shown, a layer of cooling water pipes is set at the chamfer of the lock chamber wall, which is set as a single loop and arranged according to the principle of 1.4m pipe spacing and 0.75m away from the concrete edge;

[0120] like Fig.11 As shown in Figure 1, two layers of vertical cooling water pipes are set on the lock chamber wall. Fig.13 As shown in the figure, the cooling water pipe on the earthward side does not need to be disconnected at the floating bollard position and is set as a single circuit. Fig.14 As shown, the cooling water pipe on the waterfront side needs to be disconnected at the floating bollard position and set up as a double circuit, arranged according to the principle of a pipe spacing of 1.4m and a distance of 0.75m from the concrete edge.

[0121] 4.2.2 Connection of cooling water pipe

[0122] (1) The pipeline is connected and fixed at the same time, and the pipeline is fixed to the steel support ribs with iron wire; each circuit is provided with an inlet and outlet.

[0123] (2) The inlet and outlet of the condensate pipe are controlled by a two-way water stop valve, which can realize the conversion of water outlet and water inlet, ensure the uniform water flow of the cooling water pipe, and timely control of hot and cold water. Hot melt welding is used at the joints. Compared with steel pipes, the linear layout is more flexible, reducing straight and bent joints, with better sealing and easy installation. After the pipeline is installed and fixed, the pipeline is subjected to a water pressure test to ensure that the pipeline does not leak during the water flow process.

[0124] 4.2.3 Water cooling

[0125] During the concrete cooling stage, water from a water tank is used to supply circulating water. The volume of the water tank is not less than 10m 3The water in the water tank is blended by underground well water and water stored in the gate chamber through a water pump to ensure that the water temperature in the water tank is within 20°C of the temperature of the concrete core. The water inlet of the water tank is provided by the water pump in the water collection well. A water distribution bag is set on the side of the water tank. The water distribution bag is equipped with an automatic control valve and connected to the cooling water pipe through a hose to realize the cooling water circulation. The actual location of the water tank on site and the amount of water tank used can be adjusted appropriately according to construction needs.

[0126] (1) The water temperature at the cooling water pipe inlet is controlled, and the cooling water flow rate is not less than 0.6m / s (can be adjusted according to actual conditions), and the water flow direction is changed every 24 hours. Maintain a water flow rate of 3.7m 3 / h for 3 days, then the flow rate is halved for 2 days, then the flow rate is halved again for 2 days. The total water flow time is about 7 days. It will be adjusted according to the actual temperature of the concrete. The water flow time shall not exceed 15 days.

[0127] (2) The difference between the cooling water inlet temperature and the maximum concrete temperature shall not exceed 25°C.

[0128] (3) Cooling water supply end control standard: The water supply time is about 7 days, and the water flow rate is adjusted according to the actual internal temperature conditions.

[0129] (4) The main purpose of water cooling is to reduce the initial temperature rise of the casting layer, control the concrete not to exceed the maximum allowable temperature, and at the same time reduce the temperature difference between the inside and outside of the concrete and reduce temperature stress.

[0130] (5) Before pouring concrete, check the laid cooling water pipes. If leakage or blockage is found, it should be dealt with immediately. If it is not dealt with properly, pouring shall not be allowed.

[0131] (6) On the premise of ensuring that the water pipes are not leaking, water cooling can be started when the concrete is poured.

[0132] (7) During the concrete pouring process, care should be taken to prevent water pipes from being damaged, broken, hit or blocked.

[0133] (8) After cooling is completed, all cooling water pipes required for subsequent cooling should be properly protected to prevent damage and blockage.

[0134] 3.3 The significance of temperature measurement

[0135] In the temperature control construction of large-volume concrete, the pouring temperature of concrete should be tracked and monitored during the pouring process of concrete. During the curing process, the temperature rise and fall of the concrete pouring block, the temperature difference between the inside and outside, the cooling rate and the ambient temperature should be monitored to provide a scientific basis for timely and accurate temperature control measures during the construction process. Through temperature measurement, the internal temperature of large-volume concrete can be understood, and according to the temperature measurement results, the insulation and moisture retention of the external concrete can be known to reduce the temperature difference between the inside and outside of the concrete, which is of great significance to ensuring the later quality of concrete and controlling concrete cracks.

[0136] 4.3.1 Implementation of temperature measurement

[0137] (1) Arrangement of temperature measurement points

[0138] Measuring point arrangement principles: convenient for observation, not interfering with the construction of other projects, selecting representative locations, and being able to fully and truly reflect the temperature distribution inside the block; according to Section 8.3.2 of the "Specifications for Hydraulic Concrete Construction", each pouring layer shall have no less than 3 measuring points, and every 100m 3 The warehouse surface area shall have no less than one measuring point; refer to Section 6.0.2 of "Standards for Large Volume Concrete Construction", along the thickness direction of concrete casting, at least surface, bottom and center temperature measuring points shall be arranged, and the distance between measuring points shall not be greater than 500mm. The surface temperature of concrete shall be 50mm within the surface of concrete casting body, and the bottom temperature of concrete shall be 50-100mm above the bottom surface of concrete casting body.

[0139] The location and number of measuring points at the gate head: According to the needs of temperature control and crack prevention during the construction period, 5 side positions and 20 measuring points are set on the left, middle and right bottom plates of the gate head (the measuring points on the upper surface of the concrete can be monitored by a temperature measuring gun without burying temperature measuring elements). Fig.15 As shown in the figure, 5 measuring points are set on the left bottom plate and 5 measuring points are also set on the middle bottom plate. Fig.16 As shown, the bottom plate temperature measurement points are set between the two layers of cooling water pipes, above and below the cooling water pipes. Considering the field loss, it is recommended that the number of buried temperature probes is about 24. The bottom plate of the lock chamber is arranged in reference.

[0140] The location and number of measuring points in the lock chamber: According to the needs of temperature control and crack prevention during the construction period, 15 side positions are set, one layer is arranged every 10-15m along the mileage direction, and the total number of temperature measuring points in each part is 45 (considered as 3 layers). Considering the on-site loss, it is recommended to bury about 50 temperature probes. Fig.17 As shown, Fig.17 The medium grey points are the measuring points.

[0141] (2) Temperature measuring element installation

[0142] The internal temperature measuring instrument uses an inserted electronic thermometer, the specific model is NT59-WG59-LE-B multi-channel remote GPS transmission wireless temperature sensor, WG59 wireless temperature collector; the sensing end of the thermometer is fixed on the support bar, fixed with insulating tape and the sensing end and the steel bar are insulated. A thermometer and hygrometer are used for environmental temperature monitoring.

[0143] (3) Temperature measurement method

[0144] When measuring temperature, just connect the temperature probe to the thermometer to measure the temperature. When reading, wait until the temperature display on the thermometer is stable. When the measured temperature rises or falls continuously, the frequency of temperature measurement should be appropriately increased, and the temperature monitoring duration should be no less than 30 days. In order to control the outlet temperature, a thermometer is added there to measure the outlet temperature. The temperature measurement points should be numbered on the plan and numbered signs should be hung on site. The temperature measurement should be recorded in detail and the temperature curve should be drawn. The temperature changes should be fed back to the person in charge of the sub-project, the technical person in charge and the supervision office in a timely manner.

[0145] 4.4 Temperature alarm:

[0146] When the temperature difference reaches 15℃, a warning should be given, and when it reaches 20℃, an alarm should be given; when the maximum temperature inside the concrete reaches 55℃, a warning should be given, and when it exceeds 60℃, an alarm should be given; when a warning or alarm occurs, the external water storage curing temperature and the cooling pipe temperature should be adjusted immediately to ensure that the difference between the internal temperature and the surface temperature of the concrete, the difference between the outer surface of the concrete and the ambient temperature, and the internal temperature of the concrete are all within the range.

[0147] Temperature control monitoring records:

[0148] Monitoring content: environmental information (air temperature, sunshine, wind speed, etc.), concrete measuring point temperature and cooling water temperature.

[0149] Monitoring duration: Temperature monitoring should last at least 30 days. If the temperature difference between the concrete measuring point and the ambient temperature exceeds 5°C after 30 days, continuous measurement should be continued.

[0150] Monitoring frequency: The temperature monitoring frequency is shown in the table below. During monitoring, a temperature curve should be drawn in a timely manner. When it is found that the temperature difference between the inside and outside, the cooling rate, etc. exceed the values ​​specified in the construction plan, and an abnormality occurs, it must be reported immediately to the technical person in charge and the supervisor of the construction project, prompting analysis of the cause and taking measures.

[0151] Table 2 Temperature monitoring and recording frequency

[0152] Temperature measurement period Temperature measurement times 10 consecutive days Every 2 hours Next 10 days Every 4 hours Next 10 days Every 8 hours

[0153] 5. Concrete maintenance

[0154] Concrete maintenance includes two aspects: humidity and temperature. When the temperature is low, construction is mainly based on thermal insulation maintenance, and when the temperature is high, construction is mainly based on moisture retention maintenance.

[0155] 5.1 Insulation and maintenance

[0156] When the construction environment temperature is lower than 5℃, the concrete should be kept warm and maintained moisturizing; when the environment temperature is higher than 5℃, the insulation and maintenance can be postponed depending on the temperature rise inside the concrete.

[0157] The temperature of large-volume concrete will continue to rise due to hydration heat release. During the period of temperature rise, internal heat dissipation should be strengthened, such as increasing the water flow rate and reducing the water temperature. When the concrete is in the cooling stage, the surface should be covered with insulation to reduce the cooling rate. If the temperature is low during the cooling stage, the temperature difference between the inner and outer surfaces is greater than 25°C or the temperature is more than 20°C lower than the concrete surface temperature, the large-volume concrete must also be insulated and maintained.

[0158] Here’s how to do it:

[0159] (1) Bottom plate insulation

[0160] After the bottom slab concrete is finished, immediately use the hot water from the cooling water pipe outlet to sprinkle water on the surface to replenish the surface moisture and prevent water loss and shrinkage. Then immediately cover the surface with a layer of plastic film, then cover it with a 20mm thick straw bag, and then add a layer of rainproof plastic film or "one cloth and one film" geomembrane on the straw bag. Alternatively, use a 20mm rubber-plastic sponge, and the insulation time should be determined according to the construction environment temperature.

[0161] If the surface insulation material must be removed due to construction needs, the geomembrane must be removed first when the temperature is high on the day, and the straw bag must be removed when the temperature is high at noon the next day, and the bottom plastic film must be removed after 2 to 3 hours. If steel formwork is used around the bottom plate, the formwork should also be removed after 2 weeks when the temperature is high on the day, and the surface of the concrete should be covered in time.

[0162] (2) Lock chamber wall insulation scheme

[0163] 1) Cover the top of the chamber wall with a quilt, and cover the back ribs of the templates facing the water and soil with insulation cotton. Mainly maintain with the template, and the demolding time is extended to 5-7 days.

[0164] 2) Take windproof measures outside the formwork to prevent the side concrete surface from cooling down too quickly and causing a large temperature difference between the inside and outside. If the formwork needs to be removed, do it when the temperature is highest that day.

[0165] 3) If the on-site formwork needs to be removed in advance, insulation and moisture retention measures must be taken on the side facades after removal of the formwork, and 20mm rubber-plastic sponge should be used for wrapping after removal of the formwork.

[0166] 4) When encountering adverse weather conditions such as strong winds and dryness, pay close attention to the moisture retention of the concrete during the demolding process. After demolding, cover the surface of the concrete in time and carry out watering maintenance.

[0167] 5) After the concrete water cooling work is completed, with the consent of the owner and the supervisor, the cooling water pipe can be sealed with mortar, and then the exposed part of the serpentine pipe can be cut off and processed to meet the aesthetic requirements of the concrete surface.

[0168] 5.2 Moisturizing and maintenance

[0169] When the temperature is high in summer, moisturizing and maintenance should be carried out in time after the concrete is poured.

[0170] Table 3 Thermal insulation and moisture maintenance measures

[0171]

[0172] In accordance with the above requirements, after the concrete is demolded, the sides are covered with moist geotextile to keep them moist and covered with 2mm rainproof colored strips for windproof maintenance, and water is replenished by sprinkling; water is discharged from the critical surface of the upper warehouse through water pipes, and water storage is maintained for maintenance around the clock as much as possible. If water storage is not possible due to construction conditions, water is applied every two hours. When the temperature is too high, the watering frequency should be increased to ensure that the concrete surface is moist.

[0173] Water for maintenance is obtained nearby. The project department assigns special personnel to carry out concrete maintenance. The project quality inspection department implements daily inspections, and the maintenance period is no less than 14 days.

[0174] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A cooling system for casting a U-shaped side wall of a ship lock, characterized in that: Two layers of cooling water pipes are set on the lock chamber and the bottom plate of the gate head, and the two layers of cooling water pipes are arranged vertically in opposite directions. A layer of cooling water pipes is set at the chamfer of the lock chamber wall and is set as a single circuit. Two vertical layers of cooling water pipes are set on the lock chamber wall. The cooling water pipes on the earthward side do not need to be disconnected at the floating mooring column position and are set as a single circuit. The cooling water pipes on the waterward side are disconnected at the floating mooring column position and are set as a double circuit. Two-way water stop valves are used at the inlet and outlet of the cooling water pipe.

2. A method for casting a U-shaped side wall of a ship lock, characterized in that: The following steps are involved: S1. Concrete pouring S101, Concrete pouring of upper and lower gate bottom slabs The bottom plates of the upper and lower gates are cast in layers. The first casting is for the side slope section of the gate chamber, the second casting is for the 3.5m high solid section, and the third casting is for the bottom of the side pier. S102, Lock Chamber Concrete Pouring a. Casting of the chamber bottom slab The standard section of the lock chamber bottom plate is cast in one step, and the lock chamber and gate head connection section is cast in two steps. The lock chamber bottom plate concrete is cast on both sides at the same time. After the left and right bottom plates are cast, the middle plate is cast. b. Casting of chamber wall After the chamber bottom plate is poured, the chamfered part is poured to 0.15m above the chamber wall. The single-segment chamber wall is symmetrically cast on both sides at one time using a mobile mold machine; S2. Concrete Vibration S3. Cooling water pipe layout Two layers of cooling water pipes are set on the lock chamber and the bottom plate of the gate head, and the two layers of cooling water pipes are arranged vertically in opposite directions. A layer of cooling water pipes is set at the chamfer of the lock chamber wall and is set as a single circuit. Two vertical layers of cooling water pipes are set on the lock chamber wall. The cooling water pipe on the soil side does not need to be disconnected at the floating mooring column position and is set as a single circuit. The cooling water pipe on the water side is disconnected at the floating mooring column position and is set as a double circuit. Two-way water stop valves are used at the inlet and outlet of the cooling water pipe to cool the concrete by passing water through the cooling water pipe.

3. A method for casting a U-shaped side wall of a ship lock according to claim 2, characterized in that: In step S1, the concrete includes the following components in parts by weight: 176 parts of cement, 64 parts of fly ash, 80 parts of slag powder, 696 parts of sand, 1227 parts of crushed stone, 138 parts of water, 2.84 parts of admixture, and 26 parts of anti-cracking expansion agent.

4. A method for casting a U-shaped side wall of a ship lock according to claim 3, characterized in that: The admixture is a polycarboxylic acid high-performance water reducer, and the anti-cracking expansion agent is a HEA anti-cracking agent.

5. The method for casting a U-shaped side wall of a ship lock according to claim 2, characterized in that: In step S3, the cooling water pipes of each layer are arranged in an S shape, the cooling water pipes are made of PE hoses, and hot-melt joints are used.

6. A method for casting a U-shaped side wall of a ship lock according to claim 2, characterized in that: In step S3, a layer of cooling water pipes is arranged at the chamfer of the lock chamber wall, which is set as a single circuit; two vertical layers of cooling water pipes are arranged on the lock chamber wall, and the cooling water pipes on the soil-facing side do not need to be disconnected at the floating mooring column position and are set as a single circuit, while the cooling water pipes on the water-facing side need to be disconnected at the floating mooring column position and are set as a double circuit.

7. A method for casting a U-shaped side wall of a ship lock according to claim 2, characterized in that: It also includes temperature measurement, and the measurement points are arranged as follows: The location and number of measuring points at the gate head: According to the needs of temperature control and crack prevention during the construction period, 5 measuring positions and 20 measuring points are set on the left, middle and right bottom plates of the gate head; Location and number of measuring points in the lock chamber: According to the needs of temperature control and crack prevention during the construction period, 15 measuring points are set up, with one layer arranged every 10-15m along the mileage direction.

8. The method for casting a U-shaped side wall of a ship lock according to claim 2, characterized in that: After the base slab concrete is finished, immediately use hot water from the cooling water pipe outlet to sprinkle water on the surface to replenish surface moisture and prevent water loss and shrinkage. Then immediately cover the surface with a layer of plastic film, then cover it with a 20mm thick straw bag, and add a layer of rainproof plastic film or a one-cloth-one-film geomembrane or a 20mm rubber-plastic sponge on the straw bag. The insulation time should be determined according to the construction environment temperature.

9. A method for casting a U-shaped side wall of a ship lock according to claim 2, characterized in that: The chamber wall insulation method includes the following steps: 1) Cover the top of the chamber wall with a quilt, and cover the back ribs of the formwork on the water-facing and soil-facing sides with insulation cotton. Mainly maintain the formwork with the formwork removed, and extend the formwork removal time to 5-7 days; 2) Take windproof measures outside the formwork to prevent the concrete surface from cooling too quickly and causing a large temperature difference between the inside and outside. If the formwork needs to be removed, do it when the temperature is highest on that day; 3) If the on-site formwork needs to be removed in advance, insulation and moisture retention measures should be taken on the side facades after the formwork is removed, and 20mm rubber-plastic sponge should be used for wrapping after the formwork is removed; 4) When encountering adverse weather conditions such as strong winds and dryness, close attention should be paid to the moisture retention of concrete during the demolding process. After demolding, the concrete surface should be covered in time and watered for maintenance; 5) After the concrete water cooling work is completed, with the consent of the owner and the supervisor, the cooling water pipe can be sealed with mortar, and then the exposed part of the serpentine pipe can be cut off and processed to meet the aesthetic requirements of the concrete surface.

Citation Information

Cited By

  • Ship lock floating bollard guide groove embedded part structure and pouring equipment

    CN120666716A