Preparation method of polymer containing sulfuryl and sulfonyl

Through a new polymer synthesis method, the reaction of aromatic monomers containing sulfide ether groups with dimethoxymethane and catalyst is solved by combining concentrated sulfuric acid sulfonation and oxidizing solution treatment, which solves the cost of raw materials in the prior art Due to the complex process, sulfone-containing and sulfonate-based polymers with rich pore structure and high stability were obtained, which are suitable for cellulose catalytic reactions.

CN118930860AActive Publication Date: 2024-11-12SHANXI YINGKUN TECH CO LTD

Patent Information

Application Number
CN202310559400.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

In the prior art, the synthetic polymers containing sulfone and sulfonic acid groups have problems such as expensive raw materials, complex processes and environmental pollution, and the specific surface area of ​​the polymer is small and the stability is poor.

Method used

By mixing the aromatic monomer containing sulfide ether groups with dimethoxymethane and a catalyst, sulfonated with concentrated sulfuric acid after reaction, followed by treatment with an oxidative solution, filtering, washing and drying, a rich pore structure and high Stable sulfone and sulfonic acid group-containing polymer.

Benefits of technology

This method reduces raw material costs, simplifies the process flow, improves the specific surface area and catalytic activity of the polymer, and has a three-dimensional network structure and high stability, which is suitable for cellulose catalytic hydrolysis and esterification reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930860A_ABST
    Figure CN118930860A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a polymer containing sulfuryl and sulfonyl, which comprises the following steps: synthesizing a polymer containing a thioether group by taking an aromatic monomer containing the thioether group as a raw material through Friedel-Crafts alkylation reaction, grinding, and sulfonating the polymer in a sulfonating agent to obtain the polymer containing the sulfuryl and the sulfonyl. And washing and drying to obtain the polymer containing the sulfonic acid group and the thioether group. And then oxidizing the polymer containing the sulfonic acid group and the thioether group by using an oxidizing agent, washing and drying to obtain the polymer containing the sulfonyl group and the sulfonic acid group, and the polymer has rich pore structures and a large number of acidic oxygen-containing functional groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the technical field of polymer preparation, in particular to a method for preparing a polymer containing sulfone groups and sulfonic acid groups. Background technology:

[0002] Traditional inorganic acids such as HCl and H2SO4 are widely used in reactions such as fine chemical synthesis and biomass conversion. However, liquid acids have a series of problems such as corrosion of equipment and difficulty in regeneration. Compared with liquid acids, solid acids have the advantages of easy product separation, reusability and no corrosion to reaction equipment. There are many types of solid acids, mainly macroporous resins, zeolites, heteropoly acids, metal oxides, carbon-based solid acids and polymer solid acids. Among them, polymer solid acids have the characteristics of easy structural adjustment, good thermal stability and high hydrophobicity, which have attracted widespread attention.

[0003] Polystyrene sulfonic acid resin with high sulfonic acid group density is a typical polymer solid acid, which shows good catalytic activity in cellulose hydrolysis, esterification and olefin hydration. However, polystyrene sulfonic acid resin has the problems of poor thermal stability of sulfonic acid group and low acid strength.

[0004] In order to solve the above problems, the introduction of a strong electron-withdrawing group sulfone group on the polymer main chain can improve the stability and acid strength of the sulfonic acid group. At present, polymers containing sulfone groups and sulfonic acid groups can be synthesized by the following methods. For example, Wang ZQ et al. proposed in the document "Sulfonated polyethersulfone directly synthesized throughsulfonic monomeras a new stable solid acid catalyst for esterification" (Catalysis Communications, 2012, 27: 164-168) that bis(4-chlorophenyl) sulfone, 4,4-dihydroxybiphenyl and 4,4-dichlorodiphenyl sulfone-3,3-disulfonic acid disodium as raw materials, and obtained polymers containing sulfone groups and sulfonic acid groups by first polymerization and then ion exchange. However, there are problems of poor pore structure and small specific surface area. On the basis of the above literature, Wang ZQ et al. used phloroglucinol as a crosslinking agent in the literature "A Cross-Linked and Swelling Polymer as an Effective Solid Acid Catalyst" (Industrial & Engineering Chemistry Research, 2015, 54: 7219-7225), and used the same raw materials and synthesis methods as the above literature to obtain polyether sulfone with sulfonic acid groups. However, there are problems of high raw material cost and complicated preparation methods. Guan R et al. dissolved linear polyether sulfone in concentrated sulfuric acid in the literature "Polyethersulfonesulfonated by chlorosulfonic acid and its membrane characteristics" (European Polymer Journal, 2005, 41, 1554-1560), and then used chlorosulfonic acid to sulfonate the polyether sulfone to obtain sulfonated polyether sulfone. However, the use of concentrated sulfuric acid and chlorosulfonic acid will cause environmental pollution. Li ZH et al. synthesized linear polyphenylene sulfide using Na2S and 1,4-dichlorobenzene in the document "Direct catalytic conversion of glucose and cellulose" (Green Chemistry, 2018, 20: 863-872). The linear polyphenylene sulfide was then sulfonated using 10% SO3 in H2SO4 to obtain a polymer containing sulfone groups and sulfonic acid groups. However, there are problems with the small specific surface area and poor stability of the polymer.

[0005] According to the above literature, the current synthesis of polymers containing sulfone groups and sulfonic acid groups has a series of problems such as expensive raw materials, complex processes and environmental pollution. In addition, there are also problems such as small specific surface area and poor stability of polymers containing sulfone groups and sulfonic acid groups. Therefore, it is necessary to develop a more environmentally friendly method to prepare polymers containing sulfone groups and sulfonic acid groups, which have rich pore structures and high stability. Summary of the invention:

[0006] The object of the present invention is to provide a method for preparing a polymer containing sulfone groups and sulfonic acid groups, which can effectively reduce costs and shorten the process flow, and the polymer has rich pore structures and surface oxygen-containing functional groups.

[0007] In order to achieve the above purpose, in-depth research was conducted, and it was found that the raw materials of the polymer containing sulfone groups and sulfonic acid groups obtained by the following method are cheap, the synthesis method is simple and the yield is high: the first step is to mix the aromatic monomer containing sulfide groups, dimethoxymethane and catalyst in a molar ratio of 1:1:1 to 1:5:5 and then add them to the organic solvent. The mixture is reacted at 45 to 80°C for 5 to 25 hours to obtain a polymer containing sulfide groups. The second step is to mix concentrated sulfuric acid and the polymer containing sulfide groups at a liquid-solid ratio of 5mL:1g to 50mL:1g, sulfonate at 40 to 150°C for 2 to 20 hours, and the solid obtained after filtering, washing and drying is the polymer containing sulfonic acid groups and sulfide groups. The third step is to mix the oxidizing solution with the polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 5mL:1g to 100mL:1g, and react at room temperature for 1 to 24 hours. Then, the solid is washed with deionized water until the filtrate is neutral. The solid obtained after drying, grinding and sieving is the polymer containing sulfone groups and sulfonic acid groups.

[0008] The present invention provides a method for preparing the above-mentioned polymer containing sulfone groups and sulfonic acid groups, characterized in that the aromatic monomer containing sulfide groups can be one of 4-methyl diphenyl sulfide, diphenyl sulfide, 4,4-diaminodiphenyl sulfide, 4,4-dihydroxydiphenyl sulfide, phenothiazine, 2-chlorophenothiazine, 9-thioxanthone, thianthrene, phenoxathiol, 4-phenylthioaniline and 4-phenylthiobenzyl chloride.

[0009] The present invention provides a method for preparing the above-mentioned polymer containing sulfone groups and sulfonic acid groups, characterized in that the organic solvent can be one of chloroform, 1,2-dichloroethane and dichloromethane.

[0010] The present invention provides a method for preparing the above-mentioned polymer containing sulfone groups and sulfonic acid groups, characterized in that the catalyst is one of AlCl3, FeCl3, SnCl4, TiCl4, ZnCl2, HF, H2SO4 and H3PO4.

[0011] The present invention provides a method for preparing the above-mentioned polymer containing sulfone groups and sulfonic acid groups, characterized in that the polymer containing sulfone groups and sulfonic acid groups can be used in one of cellulose catalytic hydrolysis reaction and esterification reaction.

[0012] The above method uses an aromatic monomer containing a thioether group as a raw material, and the polymer containing a sulfone group and a sulfonic acid group obtained by the method has a three-dimensional network structure and high stability. Compared with other polymers containing sulfone groups and sulfonic acid groups, the method also introduces a large number of phenolic hydroxyl groups and carboxyl groups, which significantly improves the catalytic activity of the polymer. Compared with other synthesis methods, this method has the characteristics of cheap raw materials and simple process.

[0013] The above preparation method uses cheap and readily available materials. The polymer containing sulfone groups and sulfonic acid groups prepared by this method has the following advantages:

[0014] 1. Compared with other polymers containing sulfone groups and sulfonic acid groups, the polymer has a rich pore structure and a larger specific surface area.

[0015] 2. Compared with other polymers containing sulfone and sulfonic acid groups, the polymer surface also contains abundant oxygen-containing functional groups, such as phenolic hydroxyl and carboxyl groups.

[0016] 3. Compared with other polymers containing sulfone and sulfonic acid groups, the polymer has higher catalytic activity.

[0017] 4. Compared with other synthesis methods of polymers containing sulfone groups and sulfonic acid groups, this synthesis method uses low-cost raw materials and has a simple process flow. Description of the drawings:

[0018] Figure 1 It is the XPS S2p narrow scan spectrum of the polymer containing thioether groups of the present invention, which shows the existence form of sulfur in the polymer.

[0019] Figure 2 It is the xPS S2p narrow scan spectrum of the polymer containing sulfone group and sulfonic acid group of the present invention, which shows the existence form of sulfur in the polymer.

[0020] Figure 3 This is the infrared spectrum of the polymer containing sulfone groups and sulfonic acid groups of the present invention, which shows the types of groups contained in the polymer. Specific implementation method:

[0021] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work should fall within the protection scope of the present invention.

[0022] Example 1

[0023] First, 4-methyldiphenyl sulfide, dimethoxymethane and AlCl3 were mixed evenly in a molar ratio of 1:1:3 and then added to 1,2-dichloroethane. The mixture was reacted at 45°C for 10 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 10mL:1g, sulfonated at 60°C for 5 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, hydrogen peroxide was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 20mL:1g and reacted at room temperature for 7 hours. Then, the solid was washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving was a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 301m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.02mmol / g and 0.62mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, and reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 71%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 62% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 63%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 51% after being used 5 times.

[0024] Example 2

[0025] First, diphenyl sulfide, dimethoxymethane and FeCl3 are mixed evenly in a molar ratio of 1:4:2 and then added to dichloromethane. The mixture is reacted at 60°C for 20 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups are mixed at a liquid-solid ratio of 30mL:1g, sulfonated at 100°C for 10 hours, and the solid obtained after filtering, washing and drying is a polymer containing sulfonic acid groups and sulfide groups. Finally, hydrogen peroxide is mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 50mL:1g and reacted at room temperature for 2 hours. Then, the solid is washed with deionized water until the filtrate is neutral. The solid obtained after drying, grinding and sieving is a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups is 259m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.23mmol / g and 0.72mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 76%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 65% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 66%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 54% after being used 5 times.

[0026] Example 3

[0027] First, 4,4-diaminodiphenyl sulfide, dimethoxymethane and SnCl4 were mixed evenly in a molar ratio of 1:2:3 and added to chloroform. The mixture was reacted at 80°C for 25 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 50mL:1g, sulfonated at 150°C for 7 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, peracetic acid was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 60mL:1g and reacted at room temperature for 7 hours. Then the solid was washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving is a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 263m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.41mmol / g and 0.47mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 69%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 58% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 59%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 52% after being used 5 times.

[0028] Example 4

[0029] First, 4.4-dihydroxydiphenyl sulfide, dimethoxymethane and TiCl4 were mixed evenly in a molar ratio of 1:3:1 and then added to 1,2-dichloroethane. The mixture was reacted at 60°C for 20 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 30mL:1g, sulfonated at 120°C for 8 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, hydrogen peroxide was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 60mL:1g and reacted at room temperature for 14 hours. Then, the solid was washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving was a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 361m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 0.99mmol / g and 0.51mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 80%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 71% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 66%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 53% after being used 5 times.

[0030] Example 5

[0031] First, thiophene, dimethoxymethane and ZnCl2 were mixed evenly in a molar ratio of 1:3:5 and then added to dichloromethane. The mixture was reacted at 80°C for 25 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 20mL:1g, sulfonated at 50°C for 10 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, peracetic acid was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 25mL:1g and reacted at room temperature for 10 hours. Then the solid was washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving is a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 306m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.11mmol / g and 0.42mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 76%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 64% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 71%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 56% after being used 5 times.

[0032] Example 6

[0033] First, thianthrene, dimethoxymethane and HF were mixed evenly in a molar ratio of 1:5:4 and added to 1,2-dichloroethane. The mixture was reacted at 60°C for 20 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 20mL:1g, sulfonated at 60°C for 15 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, peracetic acid and a polymer containing sulfonic acid groups and sulfide groups were reacted at room temperature for 10 hours at a liquid-solid ratio of 50mL:1g. The solid was then washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving is a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 369m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.44mmol / g and 0.77mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 82%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 65% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 73%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 62% after being used 5 times.

[0034] Example 7

[0035] First, 4-phenylthioaniline, dimethoxymethane and FeCl3 were mixed evenly in a molar ratio of 1:5:2 and added to dichloromethane. The mixture was reacted at 45°C for 25 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 35mL:1g, sulfonated at 65°C for 10 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, hydrogen peroxide was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 30mL:1g and reacted at room temperature for 6 hours. Then, the solid was washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving was a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 402m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.33mmol / g and 0.52mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 67%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 59% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 61%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 52% after being used 5 times.

[0036] Example 8

[0037] First, 9-thioxanthone, dimethoxymethane and AlCl3 were mixed evenly in a molar ratio of 1:1:5 and then added to chloroform. The mixture was reacted at 65°C for 25 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 15mL:1g, sulfonated at 45°C for 20 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, peracetic acid was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 10mL:1g and reacted at room temperature for 14 hours. The solid was then washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving was a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 334m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 1.31mmol / g and 0.70mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 75%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 63% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 66%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 52% after being used 5 times.

[0038] Example 9

[0039] First, phenothiazine, dimethoxymethane and FeCl3 were mixed evenly in a molar ratio of 1:2:5 and then added to chloroform. The mixture was reacted at 60°C for 20 hours to obtain a polymer containing sulfide groups. Secondly, concentrated sulfuric acid and the polymer containing sulfide groups were mixed at a liquid-solid ratio of 35mL:1g, sulfonated at 65°C for 20 hours, and the solid obtained after filtering, washing and drying was a polymer containing sulfonic acid groups and sulfide groups. Finally, peracetic acid was mixed with a polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 30mL:1g and reacted at room temperature for 12 hours. Then, the solid was washed with deionized water until the filtrate was neutral. The solid obtained after drying, grinding and sieving was a polymer containing sulfone groups and sulfonic acid groups. The specific surface area of ​​the polymer containing sulfone groups and sulfonic acid groups was 255m 2 / g. The phenolic hydroxyl and carboxyl densities of the polymer containing sulfone and sulfonic acid groups were determined by titration to be 0.89mmol / g and 0.55mmol / g, respectively. In a reactor with a condensation reflux device, the polymer containing sulfone and sulfonic acid groups, oleic acid and methanol were added to a round-bottom flask, reacted in a heating device of a constant speed magnetic stirring device, reacted at a temperature of 70°C for 2h, and the calculated oleic acid conversion rate was 65%. Under the same experimental conditions, the oleic acid conversion rate of the polymer containing sulfone and sulfonic acid groups can still reach 49% after being used 4 times. A certain amount of cellulose, a polymer containing sulfone and sulfonic acid groups, mixed and placed in a reactor, and a certain amount of distilled water was added thereto, reacted at 150°C for 4h, and the test glucose yield was 60%. Under the same experimental conditions, the glucose yield of the polymer containing sulfone and sulfonic acid groups can still reach 50% after being used 5 times.

Claims

1. A method for preparing a polymer containing sulfone groups and sulfonic acid groups, characterized in that: The preparation method is carried out according to the following steps: (1) A thioether group-containing aromatic monomer, dimethoxymethane and a catalyst are mixed uniformly in a molar ratio of 1:1:1 to 1:5:5 and then added to an organic solvent. The mixture is reacted at 45 to 80° C. for 5 to 25 hours to obtain a thioether group-containing polymer. (2) Concentrated sulfuric acid and a polymer containing sulfide groups are mixed at a liquid-to-solid ratio of 5 mL: 1 g to 50 mL: 1 g, and sulfonated at 40 to 150° C. for 2 to 20 h. The solid obtained after filtering, washing and drying is the polymer containing sulfonic acid groups and sulfide groups. (3) The oxidizing solution is mixed with the polymer containing sulfonic acid groups and sulfide groups at a liquid-solid ratio of 5 mL: 1 g to 100 mL: 1 g, and the mixture is reacted at room temperature for 1 to 24 hours. The solid is then washed with deionized water until the filtrate is neutral. The solid obtained after drying, grinding and sieving is the polymer containing sulfone groups and sulfonic acid groups.

2. The method for preparing a polymer containing sulfone groups and sulfonic acid groups according to claim 1, characterized in that: The aromatic monomer containing a thioether group may be one of 4-methyl diphenyl sulfide, diphenyl sulfide, 4,4-diaminodiphenyl sulfide, 4,4-dihydroxydiphenyl sulfide, phenothiazine, 2-chlorophenothiazine, 9-thioxanthone, thianthrene, phenoxathiol, 4-phenylthioaniline and 4-phenylthiobenzyl chloride.

3. The method for preparing a polymer containing sulfone groups and sulfonic acid groups according to claim 1, characterized in that: The organic solvent may be one of chloroform, 1,2-dichloroethane and dichloromethane.

4. The method for preparing a polymer containing sulfone groups and sulfonic acid groups according to claim 1, characterized in that: The catalyst is one of AlCl3, FeCl3, SnCl4, TiCl4, ZnCl2, HF, H2SO4 and H3PO4.

5. The method for preparing a polymer containing sulfone groups and sulfonic acid groups according to claim 1, characterized in that: The polymer containing sulfone groups and sulfonic acid groups can be used for one of cellulose catalytic hydrolysis reaction and esterification reaction.

Citation Information

Patent Citations

  • Adsorbing material for cigarette filter stick

    CN110959908A

  • Aromatic sulfonated poly thioether sulfone, preparation method and application thereof

    CN1919895A

  • Production of sulfonated polyarylene sulfide compound

    JP1995304872A

Cited By

  • 3D-triptycene based microporous polymer as electrocatalyst for hydrogen evolution reaction