Method and system for in-situ reduction of over-oxidized vanadium electrolyte

By using pipeline design and ultraviolet absorption spectrometry in all vanadium flow batteries, the vanadium ion concentration and the reduction dose are calculated, the equilibrium valence recovery of the electrolyte is achieved, the problem of capacity loss in vanadium flow batteries is solved, and the problem of capacity loss in vanadium flow batteries is extended. Battery life and simplifies the recycling process.

CN118943443AActive Publication Date: 2024-11-12TAN KAH KEE INNOVATION LAB

Patent Information

Application Number
CN202411302882.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-12
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The performance attenuation of all vanadium flow batteries in the long cycle due to the imbalance of vanadium ion concentration and valence state, especially capacity loss, hinders its commercial development.

Method used

Through appropriate pipeline design, fully mix the positive and negative electrode electrolyte, and use ultraviolet absorption spectrometry to determine the vanadium ion concentration, calculate the amount of reducing agent, perform electrolysis and charge and discharge operations to restore the equilibrium valence state of the vanadium electrolyte and achieve capacity recovery .

Benefits of technology

This method does not require replacement of the electrolyte and electrodes, simplifies the recycling process, effectively restores the battery capacity, extends the cycle life, and solves the problems of increased electrolyte valence and air oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943443A_ABST
    Figure CN118943443A_ABST
Patent Text Reader

Abstract

The invention provides a method and a system for in-situ reduction of an over-oxidized vanadium electrolyte, and relates to the technical field of all-vanadium redox flow batteries. The method comprises the following steps: (1) mixing vanadium electrolyte in a positive electrode liquid storage tank and vanadium electrolyte in a negative electrode liquid storage tank to obtain a mixed solution; (2) determining the concentration C1 of trivalent vanadium ions and the concentration C2 of tetravalent vanadium ions in the mixed solution; (3) calculating the transfer electric quantity Q required for converting vanadium ions in the vanadium electrolyte in the negative electrode liquid storage tank into trivalent vanadium ions and the electrolysis time t, and then charging for electrolysis; and (4) adding a reducing agent into the vanadium electrolyte in the positive electrode liquid storage tank, so that vanadium ions in the vanadium electrolyte in the positive electrode liquid storage tank are converted into tetravalent vanadium ions. According to the method, capacity recovery of the vanadium electrolyte is achieved, the whole recovery process is simple and efficient, and the electrolyte and the electrode do not need to be replaced or the battery does not need to be disassembled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of all-vanadium liquid flow batteries, and in particular to a method and system for in-situ reduction of over-oxidized vanadium electrolyte. Background Art

[0002] In recent years, the storage and reuse of renewable energy has become a key link in achieving carbon peak and carbon neutrality, and striving to build a clean, low-carbon, safe and efficient energy system. Under this premise, low-cost and long-life energy storage of renewable energy is a prerequisite for its incorporation into the traditional power grid system. Compared with lithium-ion batteries with high energy storage costs and limited power and energy decoupling capabilities, redox flow battery technology is one of the most promising alternatives for existing grid-scale energy storage. It has high scalability and the characteristics of energy and power decoupling control, so it can be better applied to the storage and reuse of wind power, solar energy and other renewable energy sources with large fluctuations and discontinuities.

[0003] All-vanadium liquid flow battery is one of the most promising large-scale energy storage technologies due to its power and energy decoupling characteristics, high safety, and excellent scalability. However, the inevitable performance degradation (including energy efficiency, capacity, etc.) of all-vanadium liquid flow battery in long cycles greatly reduces the life of the all-vanadium liquid flow battery system, thus hindering its commercial development. In general, the capacity loss during the operation of all-vanadium liquid flow battery is mainly caused by the unbalanced crossover of different species. During the reaction process, due to the electric field, concentration gradient, pressure difference, side reactions, etc., the four valence states of vanadium ions V 2+ 、V 3+ 、V 4+ (VO 2+ ), V 5+ (VO2 + ) have different transfer rates on the membrane, which will lead to an imbalance in the concentration and valence of vanadium ions. In addition, water molecules are also transferred along with protons and vanadium ions in the form of dragged water, resulting in a volume imbalance between the negatively charged electrolyte and the positively charged electrolyte.

[0004] In order to alleviate the capacity decay during the VRFB cycle test, several new low vanadium permeability ion exchange membranes, hydraulic pressure adjustment, osmotic pressure balance, and charge and discharge current changes have been developed to slow down the capacity decay. However, as the number of cycles increases, the capacity loss continues to accumulate, so the development of effective capacity recovery methods to extend the cycle life is a problem worthy of attention. In all-vanadium liquid flow batteries, V 3.5+ Equivalent to V 3+ and V 4+ (VO 2+ ) can be considered as a balanced electrolyte.

[0005] At present, the direct method to restore capacity after cycling operation is generally to remix the negative and positive electrolytes. Although this method successfully balances the concentration and volume of the positive and negative sides, the problem of electrolyte valence increase caused by side reactions and air oxidation caused by incomplete battery sealing still exists (C(V 3+ ) <C(V 4+ )).

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a method and system for in-situ reduction of an over-oxidized vanadium electrolyte. The method of the present invention solves the problems in the prior art of increased electrolyte valence caused by side reactions after remixing the negative and positive electrolytes, and air oxidation caused by incomplete battery sealing. The method of the present invention fully mixes the unbalanced positive and negative electrolytes through appropriate pipeline design, and can achieve capacity recovery of the vanadium electrolyte for the electrolyte with an average valence of vanadium greater than 3.5 after mixing. The entire recovery process is simple and efficient, and there is no need to replace the electrolyte and electrodes or disassemble the battery.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, the present invention provides a method for in-situ reduction of an over-oxidized vanadium electrolyte, the method comprising the following steps:

[0010] (1) mixing the vanadium electrolyte in the positive electrode storage tank and the negative electrode storage tank to obtain a mixed solution;

[0011] (2) determining the concentration C1 of trivalent vanadium ions and the concentration C2 of tetravalent vanadium ions in the mixed solution;

[0012] (3) Calculating the transfer amount Q required to convert vanadium ions in the vanadium electrolyte in the negative electrode storage tank into trivalent vanadium ions, and the electrolysis time t, and then charging for electrolysis;

[0013] (4) adding a reducing agent to the vanadium electrolyte in the positive electrode storage tank to convert the vanadium ions in the vanadium electrolyte in the positive electrode storage tank into tetravalent vanadium ions.

[0014] Preferably, in step (1), the pressure difference between the vanadium electrolyte in the positive electrode storage tank and the vanadium electrolyte in the negative electrode storage tank is 50 mV or less, indicating uniform mixing.

[0015] Preferably, in step (2), the method for determining the concentration C1 of trivalent vanadium ions and the concentration C2 of tetravalent vanadium ions in the mixed solution is:

[0016] The absorbance of the mixed solution was detected by ultraviolet-visible absorption spectroscopy, and the concentration of trivalent vanadium ions C1 and tetravalent vanadium ions C2 in the mixed solution were determined in combination with the standard curves of trivalent vanadium ion electrolyte and tetravalent vanadium ion electrolyte:

[0017] Among them, the tetravalent vanadium ion concentration C2> the trivalent vanadium ion concentration C1.

[0018] Preferably, in step (3), the transfer amount Q is calculated by the following formula:

[0019] Q=C2×V×F

[0020] Wherein, Q represents the amount of electricity transferred, C2 represents the concentration of tetravalent vanadium ions determined in step (2), V represents the volume of vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank in step (2), and F represents the Faraday constant.

[0021] Preferably, in step (3), the electrolysis time t is calculated by the following formula:

[0022]

[0023] Wherein, C2 represents the tetravalent vanadium ion concentration determined in step (2), V represents the volume of the vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank, F represents the Faraday constant, i represents the current density, S represents the effective area, and N represents the number of battery stack cells;

[0024] Preferably, in step (3), the current density i=120 mA cm -2 .

[0025] Preferably, in step (3), after the electrolysis is completed, the vanadium electrolyte in the positive electrode storage tank is composed of tetravalent vanadium ions and pentavalent vanadium ions, wherein the concentration of tetravalent vanadium ions is 2C1 and the concentration of pentavalent vanadium ions is C2-C1.

[0026] Preferably, in step (3), after the electrolysis is completed, the vanadium electrolyte in the negative electrode storage tank contains only trivalent vanadium ions, wherein the concentration of the trivalent vanadium ions is C2+C1.

[0027] Preferably, in step (4), the amount m of the reducing agent added is calculated by the following formula:

[0028]

[0029] Wherein, m represents the amount of reducing agent added, C1 represents the concentration of trivalent vanadium ions determined in step (2), C2 represents the concentration of tetravalent vanadium ions determined in step (2), V represents the volume of vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank in step (2), and M represents the molar mass of the reducing agent.

[0030] Preferably, in step (4), the reducing agent comprises any one of sodium borohydride, oxalic acid, hydrogen or formic acid, or a combination of at least two thereof, preferably oxalic acid.

[0031] Preferably, in step (4), heating and stirring are performed after adding the reducing agent.

[0032] Preferably, the heating and stirring temperature is 45-60°C, and the heating and stirring time is 2-5 hours.

[0033] Preferably, step (4) further includes step (5):

[0034] Perform charging and discharging to improve and restore the battery capacity; or, mix the vanadium electrolyte in the positive electrode storage tank and the negative electrode storage tank again to obtain a vanadium electrolyte with an average valence of 3.5;

[0035] The charging and discharging procedures are as follows:

[0036] First at 120mA·cm -2 The battery was charged at a current density of 120 mA cm -2 The battery is discharged with a cut-off voltage set to 0.9V×N, where N is the number of single battery groups contained in the battery stack.

[0037] In a second aspect, the present invention provides a system for in-situ reduction of an over-oxidized vanadium electrolyte, the system comprising: a battery stack, a positive electrode storage tank, and a negative electrode storage tank;

[0038] The positive electrode liquid storage tank and the negative electrode liquid storage tank are connected through a pipeline, and the pipeline includes a positive electrode electrolyte outlet section pipeline, a mixed liquid section pipeline and a negative electrode electrolyte outlet section pipeline;

[0039] The positive electrolyte outlet pipeline is connected to the positive electrode storage tank and is provided with a first valve; the negative electrolyte outlet pipeline is connected to the negative electrode storage tank and is provided with a fourth valve; and a fifth valve is provided in the middle of the mixed liquid pipeline.

[0040] The mixing liquid section pipeline is respectively provided with a first branch and a second branch connected to the fuel cell stack;

[0041] Wherein, the first branch is arranged between the first valve and the fifth valve, and the liquid inlet end of the first branch is connected with the mixing liquid section pipeline, and the liquid outlet end of the first branch is connected with the battery stack; and the first branch is provided with a cathode pump and a second valve;

[0042] Wherein, the second branch is arranged between the fourth valve and the fifth valve, and the liquid inlet end of the second branch is connected with the mixing liquid section pipeline, and the liquid outlet end of the second branch is connected with the fuel cell stack; and the second branch is provided with a cathode pump and a third valve;

[0043] The positive electrode liquid storage tank and the battery stack are directly connected via a first liquid return pipeline, and the negative electrode liquid storage tank and the battery stack are directly connected via a second liquid return pipeline.

[0044] Preferably, the fuel cell stack includes at least one group of fuel cell stack cells.

[0045] Preferably, the stack cell comprises end plates, electrodes and ion exchange membranes.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] (1) The present invention fully mixes the unbalanced positive and negative electrolytes through appropriate pipeline design, targeting the electrolyte in which the average valence of vanadium after mixing is greater than 3.5;

[0048] (2) The present invention determines the concentration distribution of trivalent vanadium and tetravalent vanadium in the mixed vanadium electrolyte by ultraviolet absorption spectroscopy, thereby calculating the average valence state of the vanadium electrolyte.

[0049] (3) In order to restore the capacity, the present invention first divides the mixed electrolyte into two parts to balance the concentration and volume. Then, the amount of oxalic acid, a reducing agent, required for the positive electrode electrolyte is calculated based on the average valence of vanadium calculated from the ultraviolet absorption spectrum. Considering that the reaction rate of oxalic acid with tetravalent vanadium is slow, while the reaction rate with pentavalent vanadium is fast, the method first charges the battery, and then adds oxalic acid reducing agent to the positive electrode for reduction reaction, thereby realizing the capacity recovery of the vanadium electrolyte.

[0050] (4) The entire recovery process of the method for in-situ reduction of over-oxidized vanadium electrolyte described in the present invention is simple and efficient, and there is no need to replace the electrolyte and electrodes or disassemble the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0052] Figure 1 The present invention is a flow chart of the method for in-situ reduction of over-oxidized vanadium electrolyte.

[0053] Figure 2 It is a schematic diagram of the structure of the in-situ reduction over-oxidized vanadium electrolyte system of the present invention.

[0054] Among them, 10 is a battery stack, 11 is an end plate, 12 is an electrode, 13 is an ion exchange membrane, 20 is a positive electrode liquid storage tank, 30 is a negative electrode liquid storage tank, 101 is a positive electrode electrolyte outlet section pipeline, 102 is a mixed liquid section pipeline, 103 is a negative electrode electrolyte outlet section pipeline, 104 is a first branch, 105 is a second branch, 106 is a first return liquid pipeline, 107 is a second return liquid pipeline, 1 is a first valve, 2 is a second valve, 3 is a third valve, 4 is a fourth valve, 5 is a fifth valve, 6 is a positive electrode pump, and 7 is a negative electrode pump.

[0055] Figure 3 This is a standard curve diagram of ultraviolet absorption and concentration of trivalent vanadium ions and tetravalent vanadium ions.

[0056] Figure 4 This is a charge and discharge curve diagram before and after recycling provided in Example 1. DETAILED DESCRIPTION

[0057] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0058] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0059] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] First, as Figure 1 As shown, the present invention provides a method for in-situ reduction of an over-oxidized vanadium electrolyte, the method comprising the following steps:

[0061] (1) mixing the vanadium electrolyte in the positive electrode storage tank and the negative electrode storage tank to obtain a mixed solution;

[0062] (2) determining the concentration C1 of trivalent vanadium ions and the concentration C2 of tetravalent vanadium ions in the mixed solution;

[0063] (3) Calculating the transfer amount Q required to convert vanadium ions in the vanadium electrolyte in the negative electrode storage tank into trivalent vanadium ions, and the electrolysis time t, and then charging for electrolysis;

[0064] (4) adding a reducing agent to the vanadium electrolyte in the positive electrode storage tank to convert the vanadium ions in the vanadium electrolyte in the positive electrode storage tank into tetravalent vanadium ions.

[0065] In the present invention, the method for in-situ reduction of over-oxidized vanadium electrolyte of the present invention can fully mix the unbalanced positive and negative electrolytes, for the electrolyte with an average valence of vanadium greater than 3.5 after mixing. The method determines the concentration distribution of trivalent vanadium and tetravalent vanadium in the mixed vanadium electrolyte by ultraviolet absorption spectrum, thereby calculating the average valence of the vanadium electrolyte. In order to restore the capacity, the mixed electrolyte is first divided into two parts to balance the concentration and volume. Then, according to the average valence of vanadium calculated by ultraviolet absorption spectrum, the amount of reducing agent oxalic acid required for the positive electrolyte is calculated. Considering that the reaction rate of oxalic acid with tetravalent vanadium is slow, and the reaction rate with pentavalent vanadium is fast, the method first charges the battery, and then adds oxalic acid reducing agent to the positive electrode, and reacts for a long enough time at 45, thereby realizing the capacity recovery of the vanadium electrolyte. The whole recovery process is simple and efficient, without replacing the electrolyte and electrodes or disassembling the battery.

[0066] As an optional embodiment of the present invention, in step (1), the pressure difference between the vanadium electrolyte in the positive electrode storage tank and the vanadium electrolyte in the negative electrode storage tank is 50mV or less, indicating uniform mixing, for example, it can be 50mV, 49mV, 48mV, 47mV, 46mV, 45mV, 40mV, 35mV, 30mV, 20mV, 10mV, etc.

[0067] As an optional embodiment of the present invention, in step (1), by appropriate pipeline design (such as Figure 2 As shown in the figure), the unbalanced positive and negative electrolytes are fully mixed. More specifically, the mixing includes the following steps:

[0068] (a) All valves are in a closed state, the first valve 1, the third valve 3 and the fifth valve 5 are opened, the second valve 2 and the fourth valve 4 are closed, and the negative electrode pump 7 is opened at the same time, so that the vanadium electrolyte in the positive electrode storage tank 20 is pumped into the negative electrode storage tank 30; after the vanadium electrolyte is completely pumped in, the negative electrode pump 7, the first valve 1 and the fifth valve 5 are closed first, the third valve 3 is maintained in an open state, and after the fourth valve 4 is opened, the negative electrode pump 7 is opened again, so that the electrolyte in the negative electrode storage tank 30 is circulated for the first time in the battery stack 10;

[0069] (b) Close the negative electrode pump 7 and all valves, open the second valve 2, the fourth valve 4 and the fifth valve 5, and simultaneously open the positive electrode pump 6 to pump the vanadium electrolyte in the negative electrode storage tank 30 into the positive electrode storage tank 20; after the vanadium electrolyte is completely pumped in, first close the positive electrode pump 6 and the fifth valve 5, maintain the first valve 1 and the second valve 2 in the open state, and then open the positive electrode pump 6 to allow the mixed electrolyte pumped into the positive electrode storage tank 20 to circulate a second time in the battery stack 10.

[0070] (c) repeating the operations of step (a) and step (b);

[0071] (d) Maintaining the positive electrode pump 6 and the negative electrode pump 7 in a closed state, opening the first valve 1, the second valve 2, the third valve 3, the fourth valve 4 and the fifth valve 5, so that the volume of the vanadium electrolyte in the positive electrode storage tank 20 is consistent with the volume of the vanadium electrolyte in the negative electrode storage tank 30, and the volume of the electrolyte on both sides is recorded as V.

[0072] As an optional embodiment of the present invention, in step (a), the time of the first cycle is 10 to 30 minutes, for example, it can be 10 minutes, 12 minutes, 14 minutes, 16 minutes, 18 minutes, 20 minutes, 22 minutes, 24 minutes, 26 minutes, 28 minutes, 30 minutes, etc.

[0073] As an optional embodiment of the present invention, in step (b), the time of the second cycle is 10 to 30 minutes, for example, it can be 10 minutes, 12 minutes, 14 minutes, 16 minutes, 18 minutes, 20 minutes, 22 minutes, 24 minutes, 26 minutes, 28 minutes, 30 minutes, etc.

[0074] As an optional embodiment of the present invention, in step (c), the number of repetitions is 1 to 10 times, for example, 1 time, 2 times, 3 times, 4 times, 5 times, 6 times, 7 times, 8 times, 9 times, 10 times, etc., preferably 3 to 50 times.

[0075] As an optional embodiment of the present invention, step (d) also includes the following detection steps to ensure that the electrolyte is evenly mixed: turn on the positive electrode pump 6 and the negative electrode pump 7, measure the battery voltage, and when the battery voltage is below 50mV, it indicates that the electrolyte is evenly mixed.

[0076] As an optional embodiment of the present invention, in step (2), the method for determining the concentration C1 of trivalent vanadium ions and the concentration C2 of tetravalent vanadium ions in the mixed solution is:

[0077] The absorbance of the mixed solution was detected by ultraviolet-visible absorption spectroscopy, and the concentration of trivalent vanadium ions C1 and the concentration of tetravalent vanadium ions C2 in the mixed solution were determined in combination with the standard curves of the trivalent vanadium ion electrolyte and the tetravalent vanadium ion electrolyte.

[0078] As an optional embodiment of the present invention, in step (2), the tetravalent vanadium ion concentration C2> the trivalent vanadium ion concentration C1.

[0079] As an optional implementation mode of the present invention, in step (3), the transfer amount Q is calculated by the following formula:

[0080] Q=C2×V×F

[0081] Wherein, Q represents the amount of electricity transferred, C2 represents the concentration of tetravalent vanadium ions determined in step (2), V represents the volume of vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank in step (2), and F represents the Faraday constant.

[0082] As an optional embodiment of the present invention, in step (3), the electrolysis time t is calculated by the following formula:

[0083]

[0084] Wherein, C2 represents the tetravalent vanadium ion concentration determined in step (2), V represents the volume of the vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank, F represents the Faraday constant, i represents the current density, S represents the effective area, and N represents the number of battery stack cells;

[0085] As an optional embodiment of the present invention, in step (3), the current density i=120mAcm -2 .

[0086] As an optional embodiment of the present invention, in step (3), after the electrolysis is completed, the vanadium electrolyte in the positive electrode storage tank is composed of tetravalent vanadium ions and pentavalent vanadium ions; wherein the concentration of tetravalent vanadium ions is 2C1, and the concentration of pentavalent vanadium ions is C2-C1.

[0087] As an optional embodiment of the present invention, in step (3), after the electrolysis is completed, the vanadium electrolyte in the negative electrode storage tank contains only trivalent vanadium ions; wherein the concentration of the trivalent vanadium ions is C2+C1.

[0088] As an optional embodiment of the present invention, in step (4), the amount m of the reducing agent added is calculated by the following formula:

[0089]

[0090] Wherein, m represents the amount of reducing agent added, C1 represents the concentration of trivalent vanadium ions determined in step (2), C2 represents the concentration of tetravalent vanadium ions determined in step (2), V represents the volume of vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank in step (2), and M represents the molar mass of the reducing agent.

[0091] As an optional embodiment of the present invention, in step (4), the reducing agent includes any one of sodium borohydride, oxalic acid, hydrogen or formic acid, or a combination of at least two thereof, preferably oxalic acid.

[0092] As an optional embodiment of the present invention, in step (4), heating and stirring are required after adding the reducing agent.

[0093] As an optional embodiment of the present invention, in step (4), the temperature of the heating and stirring is 45-60°C, for example, 45, 46, 48, 50, 52, 54, 56, 58, 60°C, etc.

[0094] As an optional embodiment of the present invention, in step (4), the heating and stirring time is 2 to 5 hours, for example, it can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, etc.

[0095] As an optional embodiment of the present invention, step (4) further includes step (5):

[0096] Charge and discharge to increase and restore battery capacity.

[0097] Alternatively, the vanadium electrolyte in the positive electrode storage tank and the negative electrode storage tank are mixed again to obtain a vanadium electrolyte with an average valence of 3.5.

[0098] As an optional embodiment of the present invention, the charging and discharging procedure is as follows:

[0099] First at 120mA·cm -2 The battery was charged at a current density of 120 mA cm -2 The battery is discharged with a cut-off voltage set to 0.9V×N, where N is the number of single battery groups contained in the battery stack.

[0100] In a second aspect, the present invention provides a system for in-situ reduction of an over-oxidized vanadium electrolyte, such as Figure 2 As shown, the system includes: a battery stack 10, a positive electrode liquid storage tank 20 and a negative electrode liquid storage tank 30.

[0101] The positive electrode liquid storage tank 20 and the negative electrode liquid storage tank 30 are connected through pipelines, and the pipelines include a positive electrode electrolyte outlet section pipeline 101, a mixed liquid section pipeline 102 and a negative electrode electrolyte outlet section pipeline 103.

[0102] Among them, the positive electrode electrolyte outlet section pipeline 101 is connected to the positive electrode storage tank 20 and is provided with a first valve 1; the negative electrode electrolyte outlet section pipeline 103 is connected to the negative electrode storage tank 30 and is provided with a fourth valve 4; the mixed liquid section pipeline 102 is provided with a fifth valve 5 in the middle position.

[0103] The liquid mixing section pipeline 102 is provided with a first branch 104 and a second branch 105 connected to the fuel cell stack 10 .

[0104] Among them, the first branch 104 is arranged between the first valve 1 and the fifth valve 5, and the liquid inlet end of the first branch 104 is connected to the mixed liquid section pipeline 102, and the liquid outlet end of the first branch 104 is connected to the fuel cell stack 10; and the first branch 104 is provided with a positive electrode pump 6 and a second valve 2.

[0105] Among them, the second branch 105 is arranged between the fourth valve 4 and the fifth valve 5, and the liquid inlet end of the second branch 105 is connected to the mixed liquid section pipeline 102, and the liquid outlet end of the second branch 105 is connected to the fuel cell stack 10; and the second branch 105 is provided with a cathode pump 7 and a third valve 3.

[0106] The positive electrode liquid storage tank 20 and the battery stack 10 are directly connected via a first liquid return pipeline 106 .

[0107] The negative electrode liquid storage tank 30 and the fuel cell stack 10 are directly connected via a second liquid return pipeline 107 .

[0108] As an optional embodiment of the present invention, the fuel cell stack includes at least one group of fuel cell stack cells.

[0109] As an optional embodiment of the present invention, the battery stack includes end plates, electrodes and ion exchange membranes.

[0110] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0111] Example 1

[0112] This embodiment provides a method for in-situ reduction of an over-oxidized vanadium electrolyte, the method comprising the following steps:

[0113] S1. Mixing of positive and negative electrolytes:

[0114] Open the first valve 1, the third valve 3, and the fifth valve 5, close the other valves, and start the negative electrode pump at the same time to pump the vanadium electrolyte in the positive electrode storage tank into the negative electrode storage tank; after it is completely pumped in, close the negative electrode pump and the first valve 1 and the fifth valve 5, keep the third valve 3 and the fourth valve 4 in the open state, start the negative electrode pump, and circulate the negative electrode electrolyte in the battery stack for 20 minutes;

[0115] Close the negative electrode pump, keep the second valve 2, the fourth valve 4, and the fifth valve 5 open, and the first valve 1 closed. Open the positive electrode pump to allow the electrolyte to completely enter the positive electrode storage tank. Then close the positive electrode pump and the fifth valve 5, keep the first valve 1 and the second valve 2 open, and open the positive electrode pump to allow the mixed electrolyte to circulate in the battery stack for 20 minutes.

[0116] Repeat the above operation 4 times, turn off the pump, open all valves, let it stand for 5 minutes, the volume of the positive and negative electrode solutions is consistent, close the three-way valve, turn on the positive and negative electrode pumps, the battery voltage displays 30mV, indicating that the electrolyte has been evenly mixed. At this time, the volume of the electrolyte on both sides is 19.35L.

[0117] S2. Determination of vanadium ion concentration:

[0118] The absorbance of the mixed solution was detected by ultraviolet-visible absorption spectroscopy, and the standard curves of the trivalent vanadium ion electrolyte and the tetravalent vanadium ion electrolyte (such as Figure 3 As shown), the mixed electrolyte was diluted 100 times to determine the concentration of trivalent vanadium ions C1 and tetravalent vanadium ions C2 in the mixed solution: 3+ The concentration is 0.3103mol / L, V 4+ (VO 2+ ) concentration is 1.3520mol / L.

[0119] S3, charging electrolysis:

[0120] The selected battery has an effective area of ​​15 cm × 15 cm, with 10 groups and a current density of 120 mA cm -2 According to the above calculation formula of electrolysis time t, the required electrolysis time is t = 1.3520 mol / L × 19.35 L × 96485 C·s -1 / (120mA·cm -2 ×225cm 2 ×10)=9348.8s.

[0121] S4, positive electrode electrolyte reduction:

[0122] After the charging and electrolysis, add oxalic acid m = 1.3417 mol / L / 2 × 19.35 L × 90 g / mol (molar mass of oxalic acid) = 1168.3 g to the positive electrode storage tank, stir and heat at 45 °C for 4 h to make V in the positive electrode storage tank 5+ (VO2 + ) is completely transformed into V 4+ (VO 2+ ).

[0123] S5, all-vanadium electrolyte:

[0124] Then, the positive and negative electrolytes are mixed evenly according to the step S1 to obtain an all-vanadium electrolyte with an average valence of 3.5;

[0125] Subsequently, the all-vanadium electrolyte was subjected to a charge and discharge test (wherein the charge and discharge procedure is as follows: first at 120 mA cm -2 The battery was charged at a current density of 120 mA cm -2 The battery was discharged at 120 mA cm -2 Under the current density, the capacity of the electrolyte after recycling is greatly improved compared with that before recycling (such as Figure 4 ), thus proving the feasibility of this method.

[0126] The present invention fully mixes the unbalanced positive and negative electrolytes through appropriate pipeline design. For the electrolyte with an average valence of vanadium greater than 3.5 after mixing, the method determines the concentration distribution of trivalent vanadium and tetravalent vanadium in the mixed vanadium electrolyte through ultraviolet absorption spectrum, thereby calculating the average valence of the vanadium electrolyte. In order to restore the capacity, the mixed electrolyte is first divided into two parts to balance the concentration and volume. Then, according to the average valence of vanadium calculated by ultraviolet absorption spectrum, the amount of oxalic acid, a reducing agent, required for the positive electrolyte is calculated. Considering that the reaction rate of oxalic acid with tetravalent vanadium is slow, and the reaction rate with pentavalent vanadium is fast, the method first charges the battery, and then adds oxalic acid reducing agent to the positive electrode, and reacts at 40-60°C for a sufficiently long time, thereby realizing the capacity recovery of the vanadium electrolyte. And the whole recovery process is simple and efficient, without replacing the electrolyte and electrodes or disassembling the battery.

[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for in-situ reduction of an over-oxidized vanadium electrolyte, It is characterized in that The method comprises the following steps: (1) mixing the vanadium electrolyte in the positive electrode storage tank and the negative electrode storage tank to obtain a mixed solution; (2) Determine the concentration of trivalent vanadium ions C in the mixed solution 1 and the tetravalent vanadium ion concentration C 2 ; (3) Calculating the transfer amount Q required to convert vanadium ions in the vanadium electrolyte in the negative electrode storage tank into trivalent vanadium ions, and the electrolysis time t, and then charging for electrolysis; (4) adding a reducing agent to the vanadium electrolyte in the positive electrode storage tank to convert the vanadium ions in the vanadium electrolyte in the positive electrode storage tank into tetravalent vanadium ions.

2. The method for in-situ reduction of an over-oxidized vanadium electrolyte according to claim 1, It is characterized in that In step (1), the pressure difference between the vanadium electrolyte in the positive electrode storage tank and the vanadium electrolyte in the negative electrode storage tank is 50 mV or less, indicating that the mixture is uniform.

3. The method for in-situ reduction of an over-oxidized vanadium electrolyte according to claim 1, It is characterized in that In step (2), the concentration of trivalent vanadium ions in the mixed solution is determined. 1 and the tetravalent vanadium ion concentration C 2 The method is: The absorbance of the mixed solution was detected by UV-visible absorption spectroscopy, and the concentration of trivalent vanadium ions in the mixed solution was determined by combining the standard curves of trivalent vanadium ion electrolyte and tetravalent vanadium ion electrolyte. 1 and the tetravalent vanadium ion concentration C 2 : Wherein, the tetravalent vanadium ion concentration C 2 >Trivalent vanadium ion concentration C 1 .

4. The method for in-situ reduction of an over-oxidized vanadium electrolyte according to claim 1, It is characterized in that In step (3), the transfer amount Q is calculated by the following formula: Q=C 2 ×V×F Among them, Q represents the amount of power transferred, C 2 represents the tetravalent vanadium ion concentration determined in step (2), V represents the volume of the vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank in step (2), and F represents the Faraday constant.

5. The method for in-situ reduction of over-oxidized vanadium electrolyte according to claim 1, It is characterized in that In step (3), the electrolysis time t is calculated by the following formula: Among them, C 2 represents the tetravalent vanadium ion concentration determined in step (2), V represents the volume of the vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank, F represents the Faraday constant, i represents the current density, S represents the effective area, and N represents the number of battery stack cells; And / or, the current density i=120 mA cm -2 .

6. The method for in-situ reduction of over-oxidized vanadium electrolyte according to claim 1, It is characterized in that In step (3), after the electrolysis is completed, the vanadium electrolyte in the positive electrode storage tank is composed of tetravalent vanadium ions and pentavalent vanadium ions, wherein the concentration of tetravalent vanadium ions is 2C 1 , the concentration of pentavalent vanadium ions is C 2 -C 1 ; The vanadium electrolyte in the negative electrode storage tank contains only trivalent vanadium ions, wherein the concentration of the trivalent vanadium ions is C 2 +C 1 .

7. The method for in-situ reduction of over-oxidized vanadium electrolyte according to claim 1, It is characterized in that In step (4), the amount of reducing agent added m is calculated by the following formula: Where m represents the amount of reducing agent added, C 1 represents the concentration of trivalent vanadium ions determined in step (2), C 2 represents the tetravalent vanadium ion concentration determined in step (2), V represents the volume of the vanadium electrolyte in the positive electrode storage tank or the negative electrode storage tank in step (2), and M represents the molar mass of the reducing agent; Preferably, in step (4), the reducing agent comprises any one or a combination of at least two of sodium borohydride, oxalic acid, hydrogen or formic acid, preferably oxalic acid; Preferably, in step (4), heating and stirring are performed after adding the reducing agent; Preferably, the temperature of the heating and stirring is The heating and stirring time is 2 to 5 hours.

8. The method for in-situ reduction of over-oxidized vanadium electrolyte according to claim 1, It is characterized in that The method further comprises step (5) after step (4): Charge and discharge to achieve the improvement and recovery of battery capacity; or, mix the vanadium electrolyte in the positive electrode storage tank and the negative electrode storage tank again to obtain a vanadium electrolyte with an average valence of 3.

5.

9. A system for in-situ reduction of an over-oxidized vanadium electrolyte, It is characterized in that The system comprises: a battery stack, a positive electrode liquid storage tank and a negative electrode liquid storage tank; The positive electrode liquid storage tank and the negative electrode liquid storage tank are connected through a pipeline, and the pipeline includes a positive electrode electrolyte outlet section pipeline, a mixed liquid section pipeline and a negative electrode electrolyte outlet section pipeline; The positive electrolyte outlet pipeline is connected to the positive electrode storage tank and is provided with a first valve; the negative electrolyte outlet pipeline is connected to the negative electrode storage tank and is provided with a fourth valve; and a fifth valve is provided in the middle of the mixed liquid pipeline. The mixing liquid section pipeline is respectively provided with a first branch and a second branch connected to the fuel cell stack; Wherein, the first branch is arranged between the first valve and the fifth valve, and the liquid inlet end of the first branch is connected with the mixing liquid section pipeline, and the liquid outlet end of the first branch is connected with the battery stack; and the first branch is provided with a cathode pump and a second valve; Wherein, the second branch is arranged between the fourth valve and the fifth valve, and the liquid inlet end of the second branch is connected with the mixing liquid section pipeline, and the liquid outlet end of the second branch is connected with the fuel cell stack; and the second branch is provided with a cathode pump and a third valve; The positive electrode liquid storage tank and the battery stack are directly connected via a first liquid return pipeline, and the negative electrode liquid storage tank and the battery stack are directly connected via a second liquid return pipeline.

10. The system for in-situ reduction of over-oxidized vanadium electrolyte according to claim 9, It is characterized in that The battery stack includes at least one group of battery stack cells; And / or, the battery stack includes end plates, electrodes and ion exchange membranes.

Citation Information

Patent Citations

  • Trivalent vanadium ion electrolyte and preparation method thereof, and vanadium battery

    CN103515641A

  • All-vanadium redox flow battery on-line capacity recovery method

    CN114094148A

  • Electrolyte regenerating method for vanadium redox battery

    JP2003157883A

Cited By

  • Capacity recovery method of flow battery

    CN121149297A

  • Method for detecting concentration of vanadium ions in electrolyte of all-vanadium redox flow battery

    CN121185956A