Ultrahigh-performance repairing grouting material for underwater construction as well as preparation method and application thereof

By using fast-condensing, fast-hard, high-belitt sulfaluminate cement and calcium aluminate amorphous materials, high-performance underwater repair grouting materials were prepared, which solved the problem of insufficient performance of underwater repair materials in the prior art. , achieving volume stability, strong adhesion and high durability, reducing repair costs.

CN118955064AActive Publication Date: 2024-11-15CNBM ZHONGYAN TECH

Patent Information

Application Number
CN202411167117.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing underwater repair grouting material technology is relatively lacking, especially the application of high-performance repair materials in underwater construction. The existing epoxy grouting material is expensive and the elastic modulus does not match ordinary concrete, which affects its application.

Method used

Fast-condensing, fast-hard, high-Belite sulfa aluminate cement as the main cementitious material, combined with calcium aluminate amorphous phase, ultra-fine fly ash, ultra-fine ore powder and silicon fume, combined with compound admixtures, to prepare Ultra-high performance repair grouting material that resists cracking, high bonding, ultra-high strength, underwater dispersion, and high durability.

Benefits of technology

It achieves volume stability, strong adhesion, ultra-high strength and high durability, reduces the risk of shrinkage and cracking, improves the underwater repair effect, and is relatively economical.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of cement-based building materials, in particular to an ultrahigh-performance repairing grouting material for underwater construction and a preparation method and application of the ultrahigh-performance repairing grouting material for underwater construction. Fast-setting and fast-hardening high-belite sulphoaluminate cement is adopted as a main cementing material, and a calcium aluminate amorphous phase is added to promote hydration; the ultra-fine fly ash, the ultra-fine mineral powder and the silica fume are added as auxiliary cementing materials to ensure the later strength of the repairing grouting material, and the repairing grouting material with ultra-high performance, which has the advantages of cracking resistance, high adhesion, ultra-high strength, underwater dispersion resistance and high durability, is prepared by matching with a compound additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-based building materials, and in particular to an ultra-high performance repair grouting material for underwater construction, and a preparation method and application thereof. Background Art

[0002] With the rapid development of road traffic construction, more and more cross-sea and cross-river bridges have been put into use. As the service life of ordinary concrete increases, problems such as steel bar corrosion and concrete spalling occur, which seriously affect the safety of bridge structures.

[0003] The existing technology often adopts the reinforcement measure of glass fiber sleeve wrapped underwater epoxy grouting material, but the high price of epoxy grouting material and the mismatch of elastic modulus with ordinary concrete limit its application.

[0004] Cement-based grouting materials have the advantages of low cost and service synergy, and have received increasing attention. However, there is little research on the existing technology of repair grouting materials for underwater structures. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides an ultra-high performance repair grouting material for underwater construction and a preparation method and application thereof. Specifically, fast-setting and fast-hardening high-belite sulphoaluminate cement is used as the main cementitious material, calcium aluminate amorphous phase is added to promote hydration, ultra-fine fly ash, ultra-fine mineral powder and silica fume are added as auxiliary cementitious materials to ensure the later strength of the repair grouting material, and a compound admixture is used to prepare an ultra-high performance repair grouting material with resistance to cracking, high adhesion, ultra-high strength, underwater anti-dispersion and high durability.

[0006] Specifically, the ultra-high performance repair grouting material for underwater construction of the present invention is composed of the following raw materials in parts by weight: 23-30 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 0.5-4.5 parts of calcium aluminate amorphous phase, 0.01-0.03 parts of retarder, 3-8 parts of ultrafine fly ash, 5-10 parts of ultrafine mineral powder, 2-6 parts of silica fume, 43-55 parts of fine aggregate, 0.01-0.15 parts of sodium nitrite, 0.3-0.6 parts of high-performance polycarboxylic acid water reducer, 0.03-0.06 parts of defoaming agent, 0.02-0.5 parts of expansion agent, 0.6-1.1 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, 0.5-1 parts of anti-dispersant, and 2-6 parts of copper-plated steel fiber.

[0007] The anti-dispersion agent is prepared by compounding a viscosity adjuster, disodium ethylenediaminetetraacetate, sodium sulfoaluminate, glycerol polyoxyethylene ether, sodium phosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1: (0.1-0.2): (0.8-1): (0.5-0.8): (0.3-0.6): (0.2-0.3). The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in a sodium hydroxide alkaline solution, stirred at 90°C until the solution is uniformly dissolved, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause a polymerization reaction.

[0008] Preferably, the fast-setting and fast-hardening high-belite sulphoaluminate cement is composed of fast-setting and fast-hardening high-belite sulphoaluminate clinker, anhydrite, and mixed materials, and the fast-setting and fast-hardening high-belite sulphoaluminate cement clinker contains 0.5-4.6% f-CaO and 14-26.3% CaSO4.

[0009] The invention adopts fast-setting and fast-hardening high-belite sulphoaluminate cement as the main cementitious material. The high free gypsum content of the cement can ensure that all C4A3$ minerals are hydrated to form AFt, thereby ensuring good volume stability. Compared with ordinary calcium aluminate minerals, amorphous calcium aluminate has higher hydration activity and can be used in combination with fast-setting and fast-hardening high-belite sulphoaluminate cement for hydration, and promotes the hydration of ultrafine mineral admixtures, thereby providing high early strength and stable late strength. The addition of sodium nitrite also promotes cement hydration, improves the pore structure of cement stone, and improves the structural density. Sodium nitrite has the effects of lowering the freezing point and inhibiting steel corrosion.

[0010] Preferably, the retarder consists of sodium citrate, citric acid, tartaric acid and boric acid in a mass ratio of 1:1:1:1 or 2:1:1:2.

[0011] Preferably, the high-performance polycarboxylate water-reducing agent is a powder, and the water-reducing rate is ≥32%.

[0012] Preferably, the defoaming agent is a polyether defoaming agent.

[0013] Preferably, the expansion agent is at least one of a plastic expansion agent and a CaO-C4A3$-type mineral expansion agent. More preferably, the expansion agent is a composite of a plastic expansion agent and a CaO-C4A3$-type mineral expansion agent in a mass ratio of 0.5:(8-12). More preferably, the mineral expansion agent is ZY-II type.

[0014] Preferably, the fine aggregate is calcined corundum, which is continuously graded within four particle size ranges of 70-120 mesh, 40-70 mesh, 20-40 mesh, and 10-20 mesh.

[0015] Preferably, the copper-plated steel fiber is a wavy copper-plated steel fiber with a length of 3 mm and a diameter of 0.2 mm.

[0016] The present invention also relates to a method for preparing the above-mentioned ultra-high performance repair grouting material for underwater construction, which specifically comprises the following steps: 1) Weigh each raw material by weight, 2) Evenly mix fast-setting and fast-hardening high-belite sulphoaluminate cement, calcium aluminate amorphous phase, retarder, ultrafine fly ash, ultrafine mineral powder, silica fume, fine aggregate, sodium nitrite, high-performance polycarboxylic acid water reducer, defoamer, expander, ethylene / vinyl laurate / vinyl chloride terpolymer rubber powder, anti-dispersant and copper-plated steel fiber to obtain powder, and package it.

[0017] The present invention also relates to the application of the above-mentioned underwater construction ultra-high performance repair grouting material in underwater engineering repair.

[0018] Preferably, the above application comprises the following steps: a) Weigh the mixing water according to the water-to-material ratio of 0.08-0.1, b) Add the powder into the mixer, add mixing water and mix evenly to obtain slurry.

[0019] The present invention draws on the design concept of UHPC ultra-high performance concrete and adopts an ultra-low water-to-cement ratio and high-density mix design; at the same time, with the help of rapid hydration of fast-hardening cementitious materials and regulation of hydration minerals, the generation of AFt is promoted and the interfacial bonding performance is improved; with the help of the modification of anti-dispersants, the influence of the addition of traditional thickeners and flocculants on the flowability and working performance in the prior art is solved, so that the repair grouting material of the present invention has good working performance.

[0020] The present invention has the following technical advantages: 1. Good volume stability: The present invention adopts fast-setting and fast-hardening high-belite sulphoaluminate cement as the main cementitious material. Its high free gypsum content can ensure that the C4A3$ mineral is fully hydrated to form AFt, ensuring good volume stability; the addition of expansion agent further compensates for the volume shrinkage caused by the hydration of the cementitious material; and by adding short copper-plated steel fibers, compared with traditional steel fibers longer than 10 mm, the flow properties are not affected, and at the same time, the cement paste is restrained, which greatly reduces the risk of shrinkage cracking. 2. Strong bonding strength: The present invention adopts ethylene / vinyl laurate / vinyl chloride terpolymer powder to achieve the characteristics of strong soap resistance and excellent hydrophobicity. The calcium aluminate amorphous phase is hydrated in the early stage to produce a large amount of needle-shaped calcium aluminate at the interface between the new and old marine structures to produce the mortise and tenon structure, which can significantly improve the bonding mechanical properties. 3. Ultra-high strength: The present invention adopts fast-setting and fast-hardening high-belite sulphoaluminate cement and calcium aluminate amorphous phase composite, combined with ultra-fine admixtures, the cementitious material has a large specific surface area and high activity; ultra-high strength fine aggregate is used to assist in achieving better mechanical properties compared to traditional quartz sand and basalt sand; the present invention uses ultra-low water consumption with the help of UHPC configuration experience, reduces the fine defects inside the slurry, and adds an appropriate amount of steel fiber, which can have a great restraining effect on the matrix at the macro scale, greatly improving the final strength performance. 4. High durability: The present invention uses low water consumption, reduces internal defects, reduces the diffusion of harmful components such as chloride ions, and greatly reduces the damage of freeze-thaw environment. The application of ethylene / vinyl laurate / vinyl chloride ternary copolymer rubber powder realizes the hydrophobic effect inside the hardened slurry, reducing the damage of external harmful substances to the hardened slurry. 5. Good underwater repair effect: The present invention prepares a specific anti-dispersant for cementitious materials, which has good compatibility with high-performance polycarboxylic acid water-reducing agent, can ensure that the repair grouting material does not disperse during the underwater repair construction process and has good fluidity. DETAILED DESCRIPTION

[0021] To prove the technical effect of the present invention, a repair grouting material was prepared and its performance was tested. During the test, the retarder was composed of sodium citrate, citric acid, tartaric acid, and boric acid in a mass ratio of 1:1:1:1, the high-performance polycarboxylic acid water reducer was a powder with a water reduction rate of 34%, the expansion agent was a mixture of a plastic expansion agent and a ZY-II type CaO mineral expansion agent in a mass ratio of 0.5:10, the fine aggregate was calcined corundum, and it was continuously graded within four particle size ranges of 70-120 mesh, 40-70 mesh, 20-40 mesh, and 10-20 mesh, and the copper-plated steel fiber was a wavy copper-plated steel fiber with a length of 3 mm and a diameter of 0.2 mm.

[0022] During the test, the water-to-material ratio was 0.085, the mortar fluidity test was carried out in an underwater environment at a depth of 0.3m, the expansion of the slurry was tested underwater, and the compressive strength specimens were cured using standard conditions.

[0023] Example 1: Repair grouting material, composed of the following raw materials in parts by weight: 25 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 4 parts of calcium aluminate amorphous phase, 0.01 parts of retarder, 5 parts of ultrafine fly ash, 9 parts of ultrafine mineral powder, 3 parts of silica fume, 50 parts of fine aggregate, 0.1 parts of sodium nitrite, 0.4 parts of high-performance polycarboxylate water reducer, 0.04 parts of defoamer, 0.3 parts of expansion agent, 0.8 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, 0.7 parts of anti-dispersion agent, copper plating 3 parts of steel fiber, the anti-dispersion agent is compounded by viscosity adjuster, disodium ethylenediaminetetraacetate, sodium sulfoaluminate, glycerol polyoxyethylene ether, sodium phosphate, and sodium dodecylbenzene sulfonate in a mass ratio of 1:0.2:0.9:0.6:0.5:0.3. The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in sodium hydroxide alkaline solution, stirred at 90°C until uniformly dissolved, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause polymerization reaction.

[0024] After testing, the initial fluidity of the slurry is 305mm, the fluidity at 30min is 265mm, the underwater cohesion is good, the slurry does not disperse, the flexural strength at 28d is 25.5MPa, the compressive strength at 1d is 80.6MPa, the compressive strength at 3d is 103.2MPa, the compressive strength at 28d is 131.3MPa, the vertical expansion rate at 3h is 0.08%, the difference between the expansion values ​​at 24h and 3h is 0.06%, the tensile bonding strength at 28d is 2.9MPa, the static elastic modulus at 28d is 52.8GPa, and the self-drying shrinkage at 28d is 0.029%.

[0025] Example 2: Repair grouting material, composed of the following raw materials in parts by weight: 30 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 3.5 parts of calcium aluminate amorphous phase, 0.03 parts of retarder, 8 parts of ultrafine fly ash, 6 parts of ultrafine mineral powder, 5 parts of silica fume, 50 parts of fine aggregate, 0.11 parts of sodium nitrite, 0.6 parts of high-performance polycarboxylate water reducer, 0.04 parts of defoamer, 0.4 parts of expansion agent, 0.7 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, and 0.9 parts of anti-dispersant , 4 parts of copper-plated steel fiber, the anti-dispersion agent is compounded by viscosity adjuster, disodium ethylenediaminetetraacetate, sodium sulfoaluminate, glycerol polyoxyethylene ether, sodium phosphate, and sodium dodecylbenzene sulfonate in a mass ratio of 1:0.1:1:0.6:0.4:0.3. The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in sodium hydroxide alkaline solution, stirred at 90°C until uniformly dissolved, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause polymerization reaction.

[0026] After testing, the initial fluidity of the slurry is 330mm, the fluidity at 30 minutes is 310mm, the underwater cohesion is good, the slurry does not disperse, the flexural strength at 28 days is 27.6MPa, the compressive strength at 1 day is 86.5MPa, the compressive strength at 3 days is 112.3MPa, the compressive strength at 28 days is 144.1MPa, the vertical expansion rate at 3 hours is 0.09%, the difference between the expansion values ​​at 24 hours and 3 hours is 0.08%, the tensile bonding strength at 28 days is 3.1MPa, the static elastic modulus at 28 days is 52.2GPa, and the self-drying shrinkage at 28 days is 0.026%.

[0027] Comparative Example 1: Repair grouting material, composed of the following raw materials by weight: 25 parts of 52.5 grade sulphoaluminate cement, C 12 4 parts of A7 mineral, 0.01 parts of retarder, 5 parts of ultrafine fly ash, 9 parts of ultrafine mineral powder, 3 parts of silica fume, 50 parts of fine aggregate, 0.4 parts of high-performance polycarboxylic acid water reducer, 0.04 parts of defoamer, 0.3 parts of expander, 0.8 parts of ethylene / vinyl laurate / vinyl chloride terpolymer rubber powder, 0.7 parts of anti-dispersant, 3 parts of copper-plated steel fiber. The anti-dispersant is compounded by viscosity adjuster, disodium ethylenediaminetetraacetate, sodium sulfoaluminate, glycerol polyoxyethylene ether, sodium phosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1:0.2:0.9:0.6:0.5:0.3. The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in sodium hydroxide alkaline solution, stirred at 90°C until dissolved evenly, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause polymerization reaction.

[0028] After testing, the initial fluidity of the slurry is 310mm, the fluidity at 30 minutes is 268mm, the underwater cohesion is good, the slurry does not disperse, the flexural strength at 28 days is 19.3MPa, the compressive strength at 1 day is 56.4MPa, the compressive strength at 3 days is 87.3MPa, the compressive strength at 28 days is 91.2MPa, the vertical expansion rate at 3 hours is 0.05%, the difference between the expansion values ​​at 24 hours and 3 hours is 0.04%, the tensile bonding strength at 28 days is 1.8MPa, the static elastic modulus at 28 days is 41.9GPa, and the self-drying shrinkage at 28 days is 0.038%.

[0029] Comparative Example 2: Repair grouting material, composed of the following raw materials in parts by weight: 25 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 4 parts of calcium aluminate amorphous phase, 0.01 parts of retarder, 5 parts of ultrafine fly ash, 9 parts of ultrafine mineral powder, 3 parts of silica fume, 50 parts of fine aggregate, 0.1 parts of sodium nitrite, 0.4 parts of high-performance polycarboxylate water reducer, 0.04 parts of defoamer, 0.3 parts of expansion agent, 0.8 parts of ethylene / vinyl acetate copolymer powder, 0.7 parts of anti-dispersant, and 0.1 parts of anti- The dispersant is prepared by compounding a viscosity adjuster, disodium ethylenediaminetetraacetate, sodium sulfoaluminate, glycerol polyoxyethylene ether, sodium phosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1:0.2:0.9:0.6:0.5:0.3. The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in a sodium hydroxide alkaline solution, stirred at 90°C until uniformly dissolved, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause a polymerization reaction.

[0030] After testing, the initial fluidity of the slurry is 320mm, the fluidity at 30 minutes is 260mm, the underwater cohesion is good, the slurry does not disperse, the flexural strength at 28 days is 13.4MPa, the compressive strength at 1 day is 59.0MPa, the compressive strength at 3 days is 87.1MPa, the compressive strength at 28 days is 96.6MPa, the vertical expansion rate at 3 hours is 0.07%, the difference between the expansion values ​​at 24 hours and 3 hours is 0.04%, the tensile bonding strength at 28 days is 2.5MPa, the static elastic modulus at 28 days is 43.5GPa, and the self-drying shrinkage at 28 days is 0.042%.

[0031] Comparative Example 3: Repair grouting material is composed of the following raw materials in parts by weight: 25 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 4 parts of calcium aluminate amorphous phase, 0.01 parts of retarder, 5 parts of ultrafine fly ash, 9 parts of ultrafine mineral powder, 3 parts of silica fume, 50 parts of fine aggregate, 0.1 parts of sodium nitrite, 0.4 parts of high-performance polycarboxylic acid water reducer, 0.04 parts of defoaming agent, 0.3 parts of expansion agent, 0.8 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, 0.7 parts of hydroxypropyl methylcellulose ether, and 3 parts of copper-plated steel fiber.

[0032] After testing, the initial fluidity of the slurry was 300mm, the fluidity after 30 minutes was 250mm, the underwater cohesion was general, the slurry was partially dispersed, the flexural strength at 28 days was 23.4MPa, the compressive strength at 1 day was 42.5MPa, the compressive strength at 3 days was 79.0MPa, the compressive strength at 28 days was 114.1MPa, the vertical expansion rate at 3 hours was 0.07%, the difference between the expansion values ​​at 24 hours and 3 hours was 0.03%, the tensile bonding strength at 28 days was 2.5MPa, the static elastic modulus at 28 days was 38.2GPa, and the self-drying shrinkage at 28 days was 0.036%.

[0033] Comparative Example 4: Repair grouting material, composed of the following raw materials in parts by weight: 25 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 4 parts of calcium aluminate amorphous phase, 0.01 parts of retarder, 5 parts of ultrafine fly ash, 9 parts of ultrafine mineral powder, 3 parts of silica fume, 50 parts of fine aggregate, 0.1 parts of sodium nitrite, 0.4 parts of high-performance polycarboxylate water reducer, 0.04 parts of defoamer, 0.3 parts of expansion agent, 0.8 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, 0.7 parts of anti-dispersant and 3 parts of copper-plated steel fiber. The anti-dispersant is compounded by viscosity adjuster, glycerol polyoxyethylene ether, sodium phosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1:0.6:0.5:0.3. The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in a sodium hydroxide alkaline solution, stirred at 90°C until uniformly dissolved, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause polymerization reaction.

[0034] After testing, the initial fluidity of the slurry was 322mm, the fluidity at 30 minutes was 280mm, the underwater cohesion was good, the slurry was slightly dispersed, the flexural strength at 28 days was 20.7MPa, the compressive strength at 1 day was 69.8MPa, the compressive strength at 3 days was 84.5MPa, the compressive strength at 28 days was 117.2MPa, the vertical expansion rate at 3 hours was 0.07%, the difference between the expansion values ​​at 24 hours and 3 hours was 0.04%, the tensile bonding strength at 28 days was 2.2MPa, the static elastic modulus at 28 days was 38.8GPa, and the self-drying shrinkage at 28 days was 0.038%.

[0035] Comparative Example 5: Repair grouting material is composed of the following raw materials in parts by weight: 25 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 4 parts of calcium aluminate amorphous phase, 0.01 parts of retarder, 5 parts of ultrafine fly ash, 9 parts of ultrafine mineral powder, 3 parts of silica fume, 50 parts of fine aggregate, 0.1 parts of sodium nitrite, 0.4 parts of high-performance polycarboxylic acid water reducer, 0.04 parts of defoaming agent, 0.3 parts of expansion agent, 0.8 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, 0.7 parts of anti-dispersant, 3 parts of copper-plated steel fiber, and the anti-dispersant is compounded by polyacrylamide, disodium ethylenediaminetetraacetate, and sodium sulphoaluminate in a mass ratio of 1:0.2:0.9.

[0036] After testing, the initial fluidity of the slurry is 310mm, the fluidity at 30 minutes is 280mm, the underwater cohesion is general, the slurry is partially dispersed, the flexural strength at 28 days is 20.2MPa, the compressive strength at 1 day is 41.7MPa, the compressive strength at 3 days is 60.3MPa, the compressive strength at 28 days is 89.4MPa, the vertical expansion rate at 3 hours is 0.04%, the difference between the expansion values ​​at 24 hours and 3 hours is 0.07%, the tensile bonding strength at 28 days is 2.3MPa, the static elastic modulus at 28 days is 36.5GPa, and the self-drying shrinkage at 28 days is 0.039%.

[0037] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An ultra-high performance repair grouting material for underwater construction, characterized in that: The invention is composed of the following raw materials in parts by weight: 23-30 parts of fast-setting and fast-hardening high-belite sulphoaluminate cement, 0.5-4.5 parts of calcium aluminate amorphous phase, 0.01-0.03 parts of retarder, 3-8 parts of ultrafine fly ash, 5-10 parts of ultrafine mineral powder, 2-6 parts of silica fume, 43-55 parts of fine aggregate, 0.01-0.15 parts of sodium nitrite, 0.3-0.6 parts of high-performance polycarboxylate water reducer, 0.03-0.06 parts of defoamer, 0.02-0.5 parts of expansion agent, 0.6-1.1 parts of ethylene / vinyl laurate / vinyl chloride terpolymer powder, 0.5-1 parts of anti-dispersant, 2-6 parts of copper-plated steel fiber, The anti-dispersion agent is prepared by compounding a viscosity adjuster, disodium ethylenediaminetetraacetate, sodium sulfoaluminate, glycerol polyoxyethylene ether, sodium phosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1: (0.1-0.2): (0.8-1): (0.5-0.8): (0.3-0.6): (0.2-0.3). The preparation process of the viscosity adjuster is as follows: 85 parts of water-soluble acrylic acid and 15 parts of ethyleneimine are dissolved in a sodium hydroxide alkaline solution, stirred at 90°C until the solution is uniformly dissolved, and then 0.02 parts of sodium thiosulfate solution are added dropwise to the solution to cause a polymerization reaction.

2. The ultra-high performance repair grouting material for underwater construction according to claim 1, characterized in that: The fast-setting and fast-hardening high-belite sulphoaluminate cement is composed of fast-setting and fast-hardening high-belite sulphoaluminate clinker, anhydrite and mixed materials. The fast-setting and fast-hardening high-belite sulphoaluminate cement clinker contains 0.5-4.6% f-CaO and 14-26.3% CaSO4.

3. The ultra-high performance repair grouting material for underwater construction according to claim 1, characterized in that: The retarder is composed of sodium citrate, citric acid, tartaric acid and boric acid in a mass ratio of 1:1:1:1 or 2:1:1:

2.

4. The ultra-high performance repair grouting material for underwater construction according to claim 1, characterized in that: The high-performance polycarboxylate water reducer is a powder with a water reduction rate of ≥32%.

5. The ultra-high performance repair grouting material for underwater construction according to claim 1, characterized in that: The defoaming agent is a polyether defoaming agent, and the expansion agent is at least one of a plastic expansion agent and a CaO-C4A3$ mineral expansion agent.

6. The ultra-high performance repair grouting material for underwater construction according to claim 1, characterized in that: The fine aggregate is calcined corundum, which is continuously graded within four particle size ranges of 70-120 mesh, 40-70 mesh, 20-40 mesh, and 10-20 mesh.

7. The ultra-high performance repair grouting material for underwater construction according to claim 1, characterized in that: The copper-plated steel fiber is a wavy copper-plated steel fiber with a length of 3 mm and a diameter of 0.2 mm.

8. The method for preparing the ultra-high performance repair grouting material for underwater construction according to any one of claims 1 to 7, characterized in that: The steps include: 1) Weigh each raw material by weight, 2) Evenly mix fast-setting and fast-hardening high-belite sulphoaluminate cement, calcium aluminate amorphous phase, retarder, ultrafine fly ash, ultrafine mineral powder, silica fume, fine aggregate, sodium nitrite, high-performance polycarboxylic acid water reducer, defoamer, expander, ethylene / vinyl laurate / vinyl chloride terpolymer rubber powder, anti-dispersant and copper-plated steel fiber to obtain powder, and package it.

9. Use of the underwater construction ultra-high performance repair grouting material according to any one of claims 1 to 7 in underwater engineering repair.

10. The use according to claim 9, characterized in that: The steps include: a) Weigh the mixing water according to the water-to-material ratio of 0.08-0.1, b) Add the powder into the mixer, add mixing water and mix evenly to obtain slurry.

Citation Information

Patent Citations

  • Activated powdered concrete for bridge engineering

    CN107500659A

  • Underwater concrete anti-dispersing agent and preparation method thereof

    CN111635497A

  • Dry milling of clay minerals, milled clay minerals and their use in building materials

    CN116724012A

  • High functional cement mortar composition for repairing and reinforcing concrete structure and repairing and reinforcing method for concrete structure using the same

    KR102546492B1

Cited By

  • A high-performance cement-based composite material for repair and reinforcement engineering and preparation method thereof

    CN119774960A

  • Ultrahigh-performance grouting material for offshore wind power jacket in low-temperature environment and application of grouting material

    CN120504528A

  • Ultrahigh performance grouting material for offshore wind power jacket under low temperature environment and application thereof

    CN120504528B

  • High-free-calcium belite sulphoaluminate clinker, preparation method thereof, high-strength water-resistant anti-freezing inorganic self-leveling material and application of high-strength water-resistant anti-freezing inorganic self-leveling material

    CN120717759A

  • High free calcium belite sulphoaluminate clinker and method of preparation, high strength water resistant frost resistant inorganic self-leveling material and applications

    CN120717759B