Method for preparing high-molecular water-absorbent resin concrete internal curing agent by using natural biomass guar gum as well as product and application of high-molecular water-absorbent resin concrete internal curing agent
The preparation of polymer water-absorbent resin concrete internal curing agent by modifying guar gum solves the problems of self-shrinkage and cracks of high-performance concrete, achieving efficient and environmentally friendly concrete performance improvement, reducing production costs and complexity.
Patent Information
- Application Number
- CN202411150315.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
AI Technical Summary
The existing high-performance concrete materials have problems of self-shrinkage and cracking during hardening, resulting in insufficient structural durability and crack resistance. The existing internal curing agent process is complex and costly, making it difficult to promote on a large scale.
The natural biomass guar gum is prepared by oxidation, condensation, nucleophilic substitution and graft copolymerization methods to prepare the inner curing agent of polymer water-absorbing resin concrete by modifying the molecular structure of guar gum to improve water solubility and number of active groups and enhance absorption Liquid performance and crack resistance.
Achieve green and environmentally friendly production of curing agents in polymer water-absorbing resin concrete, reduce raw material costs and production complexity, improve the liquid absorption multiple and liquid absorption speed of concrete, and significantly enhance compressive strength, volume stability and durability. , extends the service life of the structure.
Smart Images

Figure CN119060255A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomass utilization and preparation and application of concrete internal curing agent, and specifically relates to a method for preparing a high-molecular water-absorbing resin concrete internal curing agent by using natural biomass guar gum, and a product and application thereof. Background Art
[0002] Traditional concrete is an inorganic material formed by mixing cement as a cementitious material, fine aggregate and coarse aggregate as filling materials, and then solidifying and hardening after adding water. Concrete is the world's largest and most widely used civil engineering material because of its advantages such as abundant raw material sources, low cost, high compressive strength and good durability. It is widely used in the construction of roads, bridges, industry, civil and national defense projects. According to relevant data, in 2005, Italy used 330 million cubic meters of concrete; the concrete output of the European Union and other countries was 1.056 billion cubic meters; the United States used 1.43 billion cubic meters of concrete; Japan consumed 780 million cubic meters of concrete; my country's annual demand for concrete materials reached 7 billion cubic meters; and the world's annual concrete consumption reached 10 billion cubic meters. In recent decades, with the development of science and technology, civil engineering structures have developed towards heavier loads, higher heights and larger spans, which has put forward higher requirements on the performance of concrete materials. High-performance concrete with excellent working performance, high strength and high durability has attracted more and more attention from researchers in the civil engineering industry. High-performance concrete is mainly achieved by adding mineral admixtures and high-efficiency water-reducing agents to ordinary concrete to meet the requirements of high strength, low porosity and high impermeability of concrete at a low water-cement ratio. The addition of mineral admixtures can effectively improve the basic properties of concrete mixtures, optimize the pore structure of hardened concrete and enhance the performance of the interface transition zone. However, the addition of mineral admixtures blocks the internal water seepage channel of concrete, and the rate of water replenishment from the inside of the concrete to the surface is lower than the evaporation rate of water on the surface of the slurry, resulting in capillary negative pressure and plastic shrinkage of the concrete. At the same time, during the hardening process of high-performance concrete, the volume of hydration products is smaller than the volume of the initial reactants (water + cement + mineral admixtures), and high-performance concrete shrinks in volume. The amount of cementitious materials in high-performance concrete materials is large, and the heat generated inside the concrete is large. As a poor conductor of heat, the heat generated by hydration is not easy to be conducted to the outside world. The hydration heat accumulates inside the concrete, causing the temperature inside the concrete to rise and the volume to expand, while the heat dissipation on the surface of the concrete is relatively fast, which leads to uneven temperature inside and surface temperature of the concrete, and temperature shrinkage on the surface of the concrete. Although the addition of high-efficiency water reducer reduces the amount of free water in high-performance concrete, as the degree of cement hydration continues to increase, the gel water, surface adsorbed water, and capillary water inside the concrete are released to the outside, causing the capillary pores to generate capillary pressure due to water loss, resulting in concrete drying shrinkage and deformation. The secondary hydration reaction of mineral admixtures in high-performance concrete requires the participation of water. The water in the capillary pores of the cement paste is unsaturated and there is a relative humidity gradient, which generates tensile stress on the capillary wall. The presence of tensile stress exacerbates the autogenous shrinkage of hardened high-performance concrete in the later stage. As a brittle material with a non-uniform matrix, high-performance concrete has low tensile strength and impact strength, high brittleness, and poor toughness.When the local tensile stress of high-performance concrete exceeds the ultimate tensile strength of concrete, microcracks will appear on the surface of the concrete. The microcracks will continue to expand over time and eventually develop into larger cracks. At the same time, high-performance concrete materials are also susceptible to the volume shrinkage gradient of adjacent materials and connecting components, which accelerates the generation of non-load stress inside the structure and increases the risk of microcracks in concrete developing into larger cracks. Cracks in concrete exist as CO2 and Cl in the external environment. - 、SO4 2- The invasion of harmful media such as carbon dioxide provides a migration and diffusion channel, which will accelerate the corrosion of steel bars in concrete and the degradation of concrete material performance. Especially when the concrete structure is in a severely corrosive environment such as humidity, alternating dry and wet, acid rain or carbonization, the cracks on the concrete surface reduce the overall bearing capacity and durability of the concrete structure, shortening the safety factor of the structure and the service life of the structure. How to effectively reduce the shrinkage of high-performance concrete and improve its crack resistance is a common concern and research hotspot in the modern civil engineering community.
[0003] The existing methods for improving shrinkage cracking of high-performance concrete materials include adding expansion agents, shrinkage reducing agents, and internal curing agents. The expansion agent method uses the macroscopic expansion products of ettringite, calcium hydroxide, and magnesium hydroxide generated by the hydration of the expansion agent itself to fill the capillary pores of the concrete to partially offset and compensate for the internal shrinkage of the concrete. However, the addition of expansion agents has a strong dependence on the cement composition, cement hydration degree, and ambient temperature in the concrete, and it is difficult to accurately control the expansion rate; expansion agents can compensate for the early shrinkage of concrete, but it is difficult to reduce the long-term drying shrinkage cracking of concrete. At the same time, the amount of free water in the high-performance concrete slurry is small and the hardened structure is dense. It is difficult for free water to penetrate into its interior and hydrate and expand with the expansion agent, resulting in the expansion agent The shrinkage compensation effect cannot be fully exerted. External moisture will enter the concrete along the cracks and cause the delayed reaction of ettringite, which in turn aggravates the expansion cracking of the concrete. When the amount of expansion agent added is too large, its excessively high alkali content will cause an alkali-aggregate reaction in the hardened concrete. These defects limit the use of expansion agents to inhibit concrete cracking. Shrinkage reducers are composed of amphoteric surfactant molecules. When added to fresh concrete, shrinkage reducers are adsorbed on the solid-liquid interface in the cement paste, reducing the surface tension of water in the capillary pores and the capillary pore pressure, thereby reducing the concrete's autogenous shrinkage. The addition of shrinkage reducers increases the air entrainment of the cement paste and reduces the alkaline concentration in the pore solution. Shrinkage reducer molecules adsorbed on the hydration product (calcium hydroxide) limit the growth of crystals, slow down the cement hydration reaction rate and reduce the early strength of concrete. However, shrinkage reducers are not compatible with high-efficiency water reducers, and the addition of shrinkage reducers has an adverse effect on the long-term strength of hardened concrete. In addition, the high cost of shrinkage reducers is also an important reason why shrinkage reducers are difficult to promote and apply on a large scale in high-performance concrete materials. Adding internal curing agents is currently the most effective method to inhibit the shrinkage of high-performance concrete. Internal curing agents can adjust, convert, store and release free water according to external conditions. After adding the internal curing agent to the concrete, the internal curing agent and the concrete generate osmotic pressure due to the humidity gradient. The water absorbed by the internal curing agent is slowly released over time, replenishing the internal water consumption during cement hydration and delaying the decrease of relative humidity inside the concrete, ensuring that the humidity inside the concrete is at a high level and the secondary hydration of the cementitious material is carried out. This increases the compressive strength and density of the concrete, inhibits plastic shrinkage, compensates for the early drying shrinkage deformation of the concrete, reduces the restrained shrinkage and crack width in the concrete, and improves the volume stability of high-performance concrete.
[0004] The internal curing agent used in concrete materials is a polymer water-absorbing resin containing strong hydrophilic groups such as carboxyl (-COOH), hydroxyl (-OH), and amino (-NH2), and having a three-dimensional network structure with coexistence of straight chain, branched chain, and cross-linked chain. After the polymer water-absorbing resin comes into contact with water, the -COOH, -OH, and -NH2 hydrophilic groups on the water-absorbing resin are ionized into ions, allowing the network structure to stretch. There is an ion concentration gradient and osmotic pressure between the inner and outer layers of the network structure. A large amount of free water enters the inner layer of the network structure to form hydrogen bonds with the hydrophilic functional groups. The polymer water-absorbing resin can absorb liquid water dozens or even thousands of times its own weight into a gel. At the same time, the anions on the polymer chain of the water-absorbing resin are locked, and the cations are in a free ionic state. As the ionization on the strong hydrophilic groups gradually advances, the anion concentration inside the cross-linked network structure continues to increase, and the electrostatic effect between the ions gradually increases. The cross-linked network structure of the polymer water-absorbing resin continues to expand, and the polymer water-absorbing resin begins to absorb water and swell. The swelling effect can fix free water inside the polymer network and restrict the free movement of water molecules, ensuring that the polymer water-absorbing resin has good water-retaining properties. When the polymer water-absorbing resin is added to concrete, as the cement hydration reaction continues, the cations in the hydration reaction products and the pH value of the system continue to increase, and the water-absorbing resin releases the pre-absorbed water into the concrete pore solution and compensates for the amount of water required for further hydration of the cementitious material. In addition, the unreleased water inside the water-absorbing resin is combined in the form of hydrogen bonds. This part of the absorbed water forms a film on the surface of the water-absorbing resin molecules, and its evaporation consumes a lot of energy, which slows down the evaporation of water in high-performance concrete and adjusts the humidity distribution inside the concrete. The polymer water-absorbing resin internal curing agent is added to the concrete, which absorbs water and retains water in the early stage and slowly releases water in the later stage, which can promote the hydration of the cementitious material and inhibit the shrinkage and cracking of the concrete, improve the strength, volume stability, durability of the concrete, and extend the service life of the concrete structure. In the past decade, polymer water-absorbing resin concrete internal curing agent has been increasingly valued by civil engineering researchers, and the addition of polymer water-absorbing resin internal curing agent has become an important technical means to prevent concrete cracking.
[0005] The existing polymer water-absorbing resin internal curing agents mainly include synthetic polymer systems and natural polymer systems. Synthetic polymer water-absorbing resins are mainly made of acrylic acid, acrylonitrile, acrylamide, polyvinyl alcohol, and amino acids as raw materials. They are obtained by copolymerizing with hydrophilic monomers after introducing a bifunctional cross-linking agent under the action of an initiator. Synthetic polymer water-absorbing resins have the advantages of high water absorption multiples, fast water absorption speed, and not easy to mold. However, this type of polymer water-absorbing resin is very sensitive to the ionic environment. After the synthetic polymer resin is pre-absorbed with water and then mixed into the concrete, the absorbed water will be squeezed out in an alkaline environment. The gel strength of the synthetic polymer water-absorbing resin is low, and the salt resistance and repeated swelling ability are poor. The raw materials of synthetic polymer water-absorbing resins are mostly artificial chemicals and are expensive. The synthetic polymer water-absorbent resin is prepared by solution polymerization. The monomer conversion rate of the produced polymer water-absorbent resin is low, the polymerization speed is slow, and additional crushing treatment is required; the reaction system of the polymer water-absorbent resin prepared by reverse emulsion polymerization is unstable, the production efficiency is low, and the process is relatively complicated; the preparation of polymer water-absorbent resin by radiation polymerization is still in the basic experimental research stage and has not yet been industrialized. The synthesis conditions of synthetic polymer water-absorbent resin are harsh, the process is complex, the synthesis conditions have a great influence on the yield, and the production process is prone to produce highly toxic waste gas that is harmful to the surrounding environment and human health. Natural polymer water-absorbent resin is made of easily degradable biomass materials such as starch and cellulose through free radical-initiated vinyl monomer grafting polymerization. Natural polymer water-absorbent resin has the advantages of green environmental protection, low cost, stable water storage, and reusability. However, the natural polymer material is modified, and its water solubility is weak, the polymerization process is complex, the grafting reaction efficiency is low, the molecular weight is low, and the charge is insufficient. These shortcomings of existing natural polymer water-absorbing resin concrete curing agents have hindered their application in concrete materials. The development of modified natural polymer water-absorbing resin concrete curing agents with a wide range of raw material sources, low cost, simple process, good water solubility, environmental friendliness, high efficiency and broad industrialization prospects based on the alkaline environment of concrete has become a hot topic in this field of research, which is of great significance to improving the volume stability of concrete structures.
[0006] Guar gum beans are perennial legumes, grown in India, Pakistan, the southwestern United States, Australia, and arid and semi-arid regions of Africa. The total annual output of guar gum beans worldwide exceeds 320,000 tons. India and Pakistan are major guar gum bean growers, and their annual output accounts for about 90% of the world's total output. In the 1990s, Yunnan, Hunan, Hubei, Guangdong, and Guangxi in my country also began to grow guar gum beans on a large scale. Guar gum beans are mainly composed of endosperm, bean shells, and germs, and the endosperm accounts for about one-third of the weight of guar gum beans. Guar gum can be extracted by processing the endosperm part obtained after removing the bean shells and germs of guar gum beans. Guar gum is a natural polysaccharide polymer compound second only to cellulose in the world, with the advantages of low price, good film-forming properties, good biocompatibility and biodegradability, safety, non-toxicity, and natural renewability. Guar gum molecules are a non-ionic polymer with branched chains composed of a mannose main chain and a galactose side chain, and their relative molecular weight is between 200,000 and 300,000. The D-pyranose units in the main chain of guar gum molecules are connected to form polymannose by β-1,4-glycosidic bonds, and the D-galactose side chains are connected to the mannose main chain by α-1,6-glycosidic bonds. On average, there is one galactose unit connected to the main chain at the C6 position for every two mannose units. The molar ratio of galactose to mannose is 1:1.5-1:1.8 (about 1:2). The linear and branched structure of guar gum molecules determines its unique properties. There are three hydroxyl groups C1, C2, and C4 on the D-pyranose units of the guar gum molecules, and there are primary and secondary hydroxyl groups on the C2, C3, C4, and C6 of the galactose side chains. The numerous hydroxyl groups on the guar gum molecular chain form a large number of intermolecular hydrogen bonds, which have strong hydrogen bonding activity and a large hydrogen bonding area, which makes guar gum soluble in cold water and hot water, but insoluble in organic solvents such as oils, hydrocarbons, and ketones. However, the guar gum molecule contains mannose inside and galactose outside, and the spatial structure presents a curled spherical shape. The intramolecular hydrogen bonding makes the main chain and the side chain intertwined to form a supramolecular structure of intramolecular self-crosslinking. A large number of hydroxyl groups are wrapped inside the molecule, resulting in a slow dissolution rate of guar gum, a high content of water-insoluble matter, difficult viscosity control, and weak electrolyte resistance and shear resistance, which affects the performance and effect of guar gum. Guar gum needs to be modified to overcome the many shortcomings in the use of guar gum, give natural biomass guar gum materials more and better performance, thereby broadening the application field of guar gum. The enzyme method is to selectively shear the mannose and galactose in guar gum through highly selective enzymes, reduce the molecular weight of guar gum to obtain enzyme-modified guar gum with a specific molecular weight and branch density, and the enzyme-modified guar gum changes its viscosity and rheological properties. The acid method can degrade and oxidize the amorphous region of guar gum while retaining the crystal structure, thereby improving the dissolution rate of guar gum and the ability to adsorb, complex or exchange metal ions.Oxidative modification is to oxidize the C2 and C4 vicinal hydroxyl groups of the guar gum molecule into aldehyde groups under the action of a strong oxidant, and the C2-C3 chemical bond is broken into carbonyl and carboxyl groups to obtain low molecular weight oxidized guar gum products. Oxidized guar gum derivatives have the advantages of good solubility, strong temperature resistance, salt resistance, shear degradation resistance, good storage capacity, and strong moisture absorption capacity. The chemical modification method uses the fact that the mannose sugar unit on the main chain of the guar gum molecule has an average of three hydroxyl groups, which will not be spatially shielded by the galactose side chain unit and can react under certain conditions; there are four active secondary hydroxyl groups and primary hydroxyl groups on the galactose side chain, among which the C6 primary hydroxyl group has the highest chemical reaction activity. These active hydroxyl groups on the guar gum molecule can undergo etherification, esterification, cross-linking, and grafting reactions, and specific new groups are connected to the main chain and side chain of the guar gum polymer to modify the molecular structure to obtain guar gum derivatives. For example, the hydroxyl groups in guar gum react with sodium chloroacetate etherifying agent to generate carboxymethyl guar gum and hydroxypropyl guar gum substituent ethers. The etherification treatment of guar gum reduces the formation of hydrogen bonds in guar gum molecules, increases the dissolution rate of guar gum in water, ethanol and acetone, reduces the viscosity of the product, and improves the stability of the solution. Ether-modified guar gum has the characteristics of high viscosity, good transparency and compatibility, anti-biodegradation, shear resistance, and high temperature resistance. The active hydroxyl groups in guar gum can also undergo esterification reaction with inorganic acids and organic acids. Esterified guar gum can significantly improve the mechanical properties, salt resistance and acid and alkali resistance of modified guar gum. The alcohol hydroxyl groups in the molecular structure of guar gum can be chemically cross-linked with binary or multi-functional groups, and two or more guar gum molecules are "bridged" together to form a multi-dimensional spatial network structure or gel. The cross-linked guar gum has high film-forming strength, good shear resistance, viscosity resistance, and heat resistance. Guar gum polymers can undergo free radical polymerization with vinyl monomers such as acrylic acid, acrylamide, methacrylamide, and acrylonitrile. By controlling the type of polymerized monomers, reaction conditions, grafting rate, and molecular weight of the grafting reaction, grafted copolymers with unique properties can be obtained. These grafted copolymer products not only retain the properties of the guar gum itself, but also increase the properties of the polymerized monomers. Guar gum grafted copolymers exhibit excellent film-forming properties, mechanical properties, and biological stability. The modification of guar gum polymers reduces the number of hydrogen bonds in the guar gum molecules and introduces other groups, changes the spatial structure of the guar gum molecules, and expands the application field of guar gum polymer materials. Today, the use of biomass guar gum to prepare natural polymer water-absorbing resin internal curing agents has become a research focus and hotspot in the field of civil engineering materials, and its application prospects are broad. Summary of the invention
[0007] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum.
[0008] The present invention also aims to solve the technical problem of preparing a high molecular weight water-absorbing resin concrete internal curing agent according to the method.
[0009] The final technical problem to be solved by the present invention is to provide an application of a high molecular weight water-absorbing resin concrete internal curing agent in the preparation of concrete.
[0010] Technical solution: In order to solve the above technical problems, the present invention provides a method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum, comprising the following steps:
[0011] (1) Preparation of dialdehyde guar gum: weigh natural guar gum polymer and water, put them into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, and stir rapidly for 120-180 minutes. The guar gum polymer is dispersed in the water to form a uniform suspension solution. After adding a small amount of sodium bromide, the pH value of the system is adjusted to 2-3 with dilute hydrochloric acid at a temperature of 45-50° C., and the acidification is carried out for 20-30 minutes. Sodium hypochlorite and hydrogen peroxide composite oxidant are slowly added dropwise over 30-40 minutes, the temperature is raised to 55-60° C., the guar gum suspension solution is stirred rapidly, and the reaction is carried out at this temperature for 4-5 hours to obtain a dialdehyde guar gum polymer solution.
[0012] (2) Preparation of N-hydroxymethyl acrylamide monomer: Under the action of a fatty amine catalyst, an aqueous acrylamide solution and formaldehyde are subjected to a condensation reaction to obtain an N-hydroxymethyl acrylamide solution;
[0013] (3) Preparation of modified guar gum intermediate containing double bonds: under alkaline conditions, a dialdehyde guar gum polymer solution and an N-hydroxymethyl acrylamide solution undergo a nucleophilic substitution reaction to introduce double bonds into the guar gum polymer molecules, thereby obtaining a modified guar gum polymer intermediate containing double bonds and amino groups;
[0014] (4) Preparation of polymer water-absorbing resin concrete curing agent: In the presence of an initiator, a modified guar gum polymer intermediate containing double bonds and amino groups is grafted and copolymerized with styrene and butyl acrylate monomers to obtain a modified natural guar gum polymer water-absorbing resin concrete curing agent containing -OH, -NH2, and -COO(CH2)3CH3 groups.
[0015] Wherein, in step (1), the weight ratio of the guar gum polymer to water is 1:6.5-7.0, the amount of the sodium bromide is 3.5-4.0% of the weight of the guar gum polymer, the amount of the composite strong oxidant (sodium hypochlorite+hydrogen peroxide) is 7.0-7.5% of the weight of the guar gum polymer, and the weight ratio of the sodium hypochlorite to hydrogen peroxide is 2:1.
[0016] The specific steps of step (2) are as follows: placing acrylamide and water in a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, stirring with the stirrer for 30-40 minutes to allow the acrylamide to be completely dissolved in the water to form a uniform, clear solution; adjusting the pH value to 9-10 at a temperature of 30-35° C., adding triethylenediamine catalyst, slowly dropping a 37% formaldehyde aqueous solution over a period of 30-40 minutes, raising the system temperature to 55-60° C., and reacting at this temperature for 1-2 hours to obtain an N-hydroxymethyl acrylamide solution.
[0017] Wherein, the weight ratio of acrylamide, water and formaldehyde in step (2) is 1:5.5-6.0:1.25-1.30, and the fatty amine catalyst is triethylenediamine catalyst and its dosage is 2.0% of the weight of acrylamide.
[0018] The specific steps of step (3) are as follows: adding N-hydroxymethyl acrylamide solution to the dialdehyde guar gum polymer solution, stirring continuously for 1-2 hours, adjusting the pH value to 10-11 with sodium hydroxide solution, slowly adding sodium borohydride catalyst, and reacting at 60-70° C. for 2-3 hours to obtain a modified guar gum polymer intermediate containing double bonds and amino groups.
[0019] Wherein, the weight ratio of the dialdehyde guar gum polymer solution to the N-hydroxymethyl acrylamide solution in step (3) is 19.0-19.5:1, and the amount of the sodium borohydride catalyst is 0.06-0.065% of the weight of the dialdehyde guar gum polymer solution.
[0020] The specific steps of step (4) are as follows: adding an ethanol solution containing a mixed monomer of styrene and butyl acrylate to a mixed solution of a modified guar gum polymer intermediate containing double bonds and amino groups and water at a temperature of 80-85° C., adjusting the system pH value to 3-4, dropwise adding a composite initiator of potassium persulfate and sodium bisulfite, carrying out a graft copolymerization reaction at a temperature of 90-95° C. for 2-3 hours, stopping the reaction and aging for 2-3 hours, adjusting the pH value to 2-3, and obtaining a light yellow viscous modified guar gum polymer water-absorbing resin concrete curing agent solution with a solid content of 10-15%, drying, crushing, and ball milling. The modified natural guar gum polymer water-absorbing resin concrete curing agent powder is obtained; the mass ratio of the modified guar gum polymer intermediate containing double bonds and amino end-capping to water is 49.0-49.5:1, the weight ratio of the modified guar gum polymer intermediate containing double bonds and amino end-capping, styrene and butyl acrylate is 225-230:1:1.20-1.25, the amount of the potassium persulfate and sodium bisulfite composite initiator is 0.35-0.40% of the weight of the modified guar gum polymer intermediate containing double bonds and amino end-capping solution, and the weight ratio of potassium persulfate and sodium bisulfite is 2:1.
[0021] The drying condition is to perform drying at a temperature of 90-95° C. for 16-24 hours.
[0022] Among them, after the crushing and ball milling, the powder is passed through a 0.40mm round hole sieve to obtain a modified natural biomass guar gum polymer water-absorbing concrete internal curing agent powder with a particle size less than 0.40mm, and the particle size of the internal curing agent is further controlled to be 4.876-5.239μm.
[0023] The present invention also includes the polymer water-absorbing resin concrete internal curing agent obtained by the preparation method.
[0024] The present invention also includes the use of the polymer water-absorbing resin concrete internal curing agent in the preparation of concrete.
[0025] Wherein, the dosage of the polymer water-absorbing resin concrete internal curing agent is 1-3wt%.
[0026] The present invention also includes measuring the liquid absorption performance of the modified natural biomass guar gum polymer water-absorbing concrete curing agent at different dosages and its influence on the concrete performance.
[0027] The mechanism of the present invention includes: the present invention starts from the molecular structure of natural guar gum polymer and the molecular design of polymer water-absorbing resin concrete curing agent. Based on the fact that under the action of a strong oxidant, the C2-C3 chemical bond on the guar gum polymer chain is broken, resulting in a decrease in the polymerization degree of the guar gum, and the C2 and C4 adjacent hydroxyl groups on the guar gum molecule can be oxidized to dialdehyde guar gum, the oxidatively modified guar gum has a regular chemical structure, better solubility, and higher hydroxyl reaction activity. The dialdehyde guar gum polymer and the amide compound containing a double bond undergo a nucleophilic substitution reaction to obtain an amino-terminated, double-bonded modified guar gum polymer intermediate. The C6 carbon-carbon double bond on the amino-terminated modified guar gum polymer intermediate is grafted and copolymerized with an ethylene monomer to obtain a modified guar gum polymer water-absorbing resin concrete curing agent, and the grafted copolymerized modified guar gum increases the water solubility, the number of active groups, the grafting rate and the grafting density, the charge amount, and the molecular weight of the concrete curing agent product.
[0028] Beneficial effects: The present invention uses natural biomass guar gum to modify and prepare a high molecular water-absorbing resin concrete curing agent, which broadens the application field of natural guar gum polymer materials, reduces the cost of raw materials in the preparation process of the high molecular water-absorbing resin concrete curing agent, reduces the use of artificial chemicals and organic solvents such as strong acids, strong bases, toxic acrylic acid, acrylonitrile, acrylamide, polyvinyl alcohol, amino acids, etc. in production, and avoids the negative impact of the production process of the high molecular water-absorbing resin concrete curing agent on the environment. The use of this technology to prepare a natural high molecular water-absorbing resin concrete curing agent overcomes the problems of harsh synthesis conditions, complex processes, and long production time of traditional synthetic high molecular water-absorbing resins. It avoids the steps of high temperature gelatinization and acidification treatment in the preparation process of starch and cellulose natural high molecular water-absorbing resins, and directly uses water phase reactions to simplify the production process and production technology. The use of natural guar gum to modify and prepare a high molecular water-absorbing resin improves the liquid absorption multiple and liquid absorption speed of the natural high molecular water-absorbing resin concrete curing agent. The green environmental protection and high performance goals of the preparation process of the polymer water-absorbing concrete internal curing agent are achieved, which is in line with the concept of sustainable development. It can produce good economic, social and environmental benefits, and has broad application prospects. Compared with the prior art, the modified natural biomass guar gum polymer water-absorbing concrete internal curing agent prepared by the present invention also has the following advantages:
[0029] (1) Compared with the traditional starch and cellulose natural polymer water-absorbing resin concrete curing agent, the use of natural biomass guar gum to prepare the polymer water-absorbing resin concrete curing agent consumes a large amount of natural biomass guar gum materials and broadens the application field of natural guar gum polymer materials. The preparation method of this modified natural biomass guar gum polymer water-absorbing resin concrete curing agent reduces the usage of acrylic acid and acrylamide in the reaction process. According to the method of Example 1, the raw material cost of the water-absorbing resin concrete curing agent can be saved by 86.3 yuan per ton of this modified natural biomass guar gum polymer water-absorbing resin concrete curing agent. The preparation method of this polymer water-absorbing resin concrete curing agent also reduces the usage of organic solvents in production. The organic solvent usage fee of 5.42 yuan can be saved per ton of this modified natural biomass guar gum polymer water-absorbing resin concrete curing agent.
[0030] (2) The preparation method of this natural polymer water-absorbing resin concrete curing agent adopts a water phase homogeneous reaction, avoids the steps of solvent evaporation and high-temperature gelatinization in the preparation process of starch and cellulose natural polymer water-absorbing resin, and simplifies the production process and production technology. Due to the reduction of production equipment investment and equipment use costs, the production of this natural polymer water-absorbing resin concrete curing agent according to the method of Example 1 can achieve a benefit of 8.37 yuan per ton. At the same time, this natural polymer water-absorbing resin concrete curing agent preparation method can shorten the production time by 1-2 hours, and each production of one ton of this modified natural biomass guar gum polymer water-absorbing resin concrete curing agent can save 10.6 yuan in labor costs and time costs.
[0031] (3) This method for preparing the modified natural biomass guar gum polymer water-absorbing resin concrete curing agent reduces the use of strong acids, strong bases, acrylic acid, acrylonitrile, acrylamide, polyvinyl alcohol, amino acid artificial chemicals and organic solvents in production, avoids the negative impact of the production process of synthetic polymer water-absorbing resin concrete curing agent on the environment and public health, and realizes the green production of polymer water-absorbing resin concrete curing agent.
[0032] (4) The natural guar gum polymer was modified by oxidation, condensation, nucleophilic substitution and graft copolymerization, thereby increasing the water solubility, number of active groups, grafting rate and density, charge and molecular weight of the natural high molecular weight water-absorbing resin concrete curing agent.
[0033] (5) The modified natural biomass guar gum polymer water-absorbing resin concrete curing agent has active groups such as -OH, -NH2, and -COO(CH2)3CH3 on its molecules, which can significantly increase the liquid absorption multiple and liquid absorption rate of the polymer water-absorbing resin concrete curing agent. At a low dosage (0.2%), the modified natural biomass guar gum polymer water-absorbing resin concrete curing agent has a good liquid absorption capacity. Under the same liquid absorption effect, the modified natural biomass guar gum polymer water-absorbing resin concrete curing agent has a lower dosage than the traditional starch and cellulose natural polymer water-absorbing resin concrete curing agent. Due to the reduction in the use of polymer water-absorbing resin concrete curing agent, the cost of polymer water-absorbing resin concrete curing agent can be saved by 3.11 yuan per cubic meter of concrete.
[0034] (6) Adding modified natural biomass guar gum polymer water-absorbing resin concrete curing agent to concrete can promote the hydration of cementitious materials, inhibit concrete shrinkage and cracking, improve concrete strength, volume stability, durability and extend the service life of concrete structures. Each cubic meter of concrete prepared according to the method of Example 1 can generate an economic benefit of 1.56 yuan due to extending the service life of concrete structures and saving maintenance costs.
[0035] In summary, according to the method of Example 1, 5,000 tons of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent are produced annually, excluding the environmental benefits generated by reducing the emissions of strong acids, strong bases, acrylic acid, acrylonitrile, acrylamide, polyvinyl alcohol, amino acid artificial chemicals and organic solvents. Only considering reducing the raw material cost of the polymer water-absorbing resin concrete curing agent and reducing the use of acrylic acid, acrylamide reaction monomers and organic solvents can save 458,600 yuan. Saving production equipment investment, equipment use costs, simplifying processes, reducing production time and labor costs can generate 53,100 yuan in economic benefits. To produce 5,000 tons of this modified natural biomass guar gum polymer water-absorbing resin concrete curing agent, 8.45×10 5 The cost of using polymer water-absorbing resin concrete curing agent and maintaining concrete structure per cubic meter can be saved by 3.9462 million yuan. Producing 5,000 tons of this modified natural biomass guar gum polymer water-absorbing resin concrete curing agent per year can generate an economic benefit of 4.4579 million yuan. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Preparation process of modified natural biomass guar gum polymer water-absorbing resin concrete internal curing agent.
[0037] Figure 2 The liquid absorption multiples of natural biomass guar gum polymer water-absorbing resin concrete internal curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete internal curing agent.
[0038] Figure 3 The liquid absorption rate of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0039] Figure 4 The initial slump flowability and slump flowability retention of fresh concrete mixed with natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0040] Figure 5 The compressive strength of hardened concrete mixed with natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0041] Figure 6 The anti-cracking performance of hardened concrete mixed with natural biomass guar gum high molecular water-absorbent resin concrete curing agent and traditional corn starch acrylic acid graft copolymer high water-absorbent resin concrete curing agent.
[0042] Figure 7 The drying shrinkage value of hardened concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0043] Figure 8 Chloride ion diffusion coefficient of hardened concrete mixed with natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. DETAILED DESCRIPTION
[0044] According to the technical method described in the embodiment of the present invention, one ton of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent (MGG) was produced, and the liquid absorption performance of this polymer water-absorbing resin concrete curing agent and its effect on concrete performance were studied. The liquid absorption performance and the performance of concrete added with this concrete curing agent were compared with those of a traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent (CST-PAAM, industrial grade, produced by Guangdong Anxin Water Protection Agriculture Co., Ltd.).
[0045] Source of raw materials in the present invention: guar gum polymer (industrial grade, relative molecular weight 1.6×10 5 ) was provided by Beijing Guarrun Biotechnology Co., Ltd.; sodium bromide (industrial grade) was produced by Henan Yuhai Fine Chemical Co., Ltd.; sodium hydroxide (industrial grade) was produced by Hebei Cangzhou Xincheng Chemical Products Co., Ltd.; sodium hypochlorite (industrial grade) was produced by Shandong Zibo Nano Industry and Trade Co., Ltd.; hydrogen peroxide (industrial grade, concentration 30%) was produced by Zhejiang Hangzhou Jingxin Chemical Co., Ltd.; acrylamide (industrial grade, crystal) was produced by Henan Xinxiang Xinchang Chemical Co., Ltd.; triethylenediamine (industrial grade, crystal) was produced by Shanghai Xindian Chemical Materials Co., Ltd.; formaldehyde (industrial grade, 37% concentration) was produced by Shandong Aldehyde Chemical Co., Ltd. The products are produced by Jiangsu Yongzheng Chemical Co., Ltd.; sodium borohydride (industrial grade, solid) is produced by Jiangsu Yongzheng Chemical Co., Ltd.; dilute hydrochloric acid (industrial grade, 37% concentration) is produced by Jiangsu Yangzhou Huafu Chemical Co., Ltd.; styrene (industrial grade) is produced by Shandong Xinhongyunguang Chemical Co., Ltd.; butyl acrylate (industrial grade, purity 99%) is produced by Shandong Xinhongyunguang Chemical Co., Ltd.; ethanol (industrial grade, purity 99%) is provided by Shandong Xinhongyunguang Chemical Co., Ltd.; potassium persulfate (industrial grade, purity ≥90.0%) is provided by Fujian Hongguan Chemical Co., Ltd.; sodium bisulfite (industrial grade) is produced by Tianjin Jinyaoxiangcheng Technology Co., Ltd.
[0046] Example 1 Preparation and performance test of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent 1. Preparation of dialdehyde guar gum
[0047] Weigh 970kg guar gum polymer and 6652.8kg water and put them into a reactor equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, and stir rapidly for 120 minutes. The guar gum polymer is dispersed in the water to form a uniform suspension solution. Add 34.65kg sodium bromide, and use 37% hydrochloric acid (weight percentage concentration) to adjust the system pH value to 2.75 at a temperature of 50°C, and acidify for 25 minutes. Then, slowly drip 69.3kg sodium hypochlorite and hydrogen peroxide composite oxidant (sodium hypochlorite: hydrogen peroxide=2:1, weight ratio) in 40 minutes, raise the temperature to 60°C, accelerate the stirring of the guar gum suspension solution, and react at this temperature for 5 hours to obtain 7599.02kg dialdehyde guar gum polymer solution.
[0048] 2. Preparation of N-hydroxymethyl acrylamide
[0049] 51.20 kg of acrylamide and 269.5 kg of water were placed in a reactor equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser. The stirrer was turned on and stirred for 40 minutes to completely dissolve the acrylamide in the water to form a uniform, clear solution. The system was kept at 35°C, and the pH value was adjusted to 9.57 using a sodium hydroxide solution. 1.0241 kg of triethylenediamine catalyst was added to the acrylamide solution, and 64.295 kg of 37% formaldehyde solution was slowly added dropwise over 30 minutes. The system temperature was raised to 60°C, and acrylamide and formaldehyde were condensed for 2 hours to obtain 378.61 kg of N-hydroxymethyl acrylamide solution.
[0050] 3. Preparation of modified guar gum polymer intermediates containing double bonds and amino groups
[0051] 7326.55 kg of dialdehyde guar gum polymer solution was placed in a reactor equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, and 377.04 kg of N-hydroxymethyl acrylamide solution was added to the dialdehyde guar gum polymer solution, and stirring was continued for 2 hours. Sodium hydroxide was used to adjust the pH value of the system to 10.25. After adding 4.528 kg of sodium borohydride catalyst, at a temperature of 70°C, the dialdehyde guar gum polymer solution and the N-hydroxymethyl acrylamide solution were subjected to nucleophilic substitution reaction for 3 hours to introduce double bonds into the guar gum polymer molecules to obtain 7656.61 kg of modified guar gum polymer intermediates containing double bonds and amino end-capping.
[0052] 4. Preparation of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent
[0053] In a reactor equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, add 7590kg of a modified guar gum polymer intermediate containing double bonds and amino-terminated and 154kg of water, and stir to completely mix the modified guar gum polymer intermediate containing double bonds and amino-terminated and water into a uniform solution. Keep the temperature at 80°C, add 3.34kg of styrene and 4.10kg of butyl acrylate (styrene and butyl acrylate are dissolved in 8.327kg of ethanol solvent) to the modified guar gum polymer intermediate solution containing double bonds and amino-terminated to form a mixed solution. Adjust the pH value of the system to 3.25 with 37% dilute hydrochloric acid, slowly drop 28.05kg of potassium persulfate and sodium bisulfite composite initiator (potassium persulfate: sodium bisulfite = 2:1, weight ratio) in 40 minutes, and graft copolymerize at 95°C for 3 hours. Stop the reaction and cool naturally to ambient temperature, and mature in the reactor for 2 hours. Add dilute hydrochloric acid to adjust the pH value to 2.49, and obtain a light yellow, viscous modified natural biomass guar gum polymer water-absorbing resin concrete curing agent solution with a solid content of 12.89%. Place the modified natural biomass guar gum polymer water-absorbing resin concrete curing agent solution in an oven and dry it at 90-95°C for 18 hours. After the dried solid is crushed, it passes through a 5mm square hole sieve and is placed in a vibrating ball mill and ground at 500 rpm for 10 minutes. The ball-milled modified natural biomass guar gum polymer water-absorbing resin concrete curing agent powder passes through a 0.40mm round hole sieve to obtain 998.25kg of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent powder with a particle size less than 0.40mm. The average particle size of the modified natural biomass guar gum polymer water-absorbing resin concrete curing agent powder measured by a laser particle size analyzer is 5.211μm.
[0054] 5. Liquid absorption performance test of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent
[0055] 5.1. Liquid absorption test
[0056] In this test, the nylon tea bag method is used to measure the liquid absorption multiple of the polymer water-absorbing resin concrete curing agent. A 200-mesh nylon tea bag is soaked in water, and the surface liquid is dripped and weighed as m0. The polymer water-absorbing resin concrete curing agent with a weight of m3 (0.1g, 0.2g, 0.3g) prepared in step 4 is placed in the pre-wetted nylon tea bag. Nylon tea bags with different weights of polymer water-absorbing resin concrete curing agent are placed in a 2000L beaker containing 1000mL simulated concrete pore solution (0.6mol / LKOH+0.2mol / L NaOH+0.01mol / L Ca(OH)2, NaHCO3 solution adjusts the solution pH to 12.5) to fully swell and soak for 2 hours. After the soaking is completed, the nylon tea bag is taken out of the beaker and hung for 30 minutes, and the excess liquid on the surface of the nylon tea bag is dripped, and the total weight of the nylon tea bag and the polymer water-absorbing resin concrete curing agent is weighed as M. The liquid absorption multiple of the polymer water-absorbing resin concrete curing agent is calculated according to formula (1). The liquid absorption multiple of the traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent is tested in the same way as a control.
[0057]
[0058] In the formula: Q-absorption multiples of polymer water-absorbent resin concrete curing agent (%); M-total weight of polymer water-absorbent resin concrete curing agent and nylon tea bag after 24 hours of absorption (g); m0-weight of pre-wet nylon tea bag (g); m3-weight of polymer water-absorbent resin concrete curing agent before absorption (g).
[0059] Figure 2 The figure shows the liquid absorption multiples of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent at different dosages. Figure 2 It can be seen that with the increase of the dosage, the liquid absorption multiples of the two polymer water-absorbing resin concrete curing agents continue to increase. At the same dosage of polymer water-absorbing resin concrete curing agent, the natural biomass guar gum polymer water-absorbing resin concrete curing agent has a greater liquid absorption multiple than the traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0060] 5.2. Liquid absorption rate test
[0061] Weigh 0.1g, 0.2g, and 0.3g of polymer water-absorbing resin concrete curing agent respectively in a pre-wetted nylon tea bag, soak it in a beaker containing 1000mL simulated concrete pore solution, and cover the beaker with plastic wrap to reduce the evaporation of the polymer water-absorbing resin concrete curing agent. Measure the liquid absorption multiples of the polymer water-absorbing resin concrete curing agent at different dosages and the simulated concrete pore solution at the corresponding time points of 5, 20, 40, 80, 120, 160, 200, and 240 minutes. The liquid absorption rate curve can be drawn based on the relationship between the liquid absorption multiple and the liquid absorption time. The liquid absorption rate of the traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent was tested in the same way as a control.
[0062] Figure 3 The figure shows the liquid absorption rate of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent at different dosages. Figure 3 It can be seen that with the increase of the absorption time, the absorption multiples of the two polymer water-absorbing resin concrete curing agents continue to increase. Under the same polymer water-absorbing resin concrete curing agent dosage (0.1%, 0.2%, 0.3%) and the same absorption time (240 minutes), the natural biomass guar gum polymer water-absorbing resin concrete curing agent (465-785%) has a faster absorption rate than the traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent (435-654%).
[0063] Example 2 Preparation and performance test of concrete containing modified natural biomass guar gum polymer water-absorbing resin concrete curing agent
[0064] 1. Concrete mix ratio
[0065] The concrete used was of C60 strength grade, and the cement was P.O42.5 ordinary Portland cement produced by Jiangnan Onoda Cement Co., Ltd. with a density of 3.05 g / cm 3 , with a specific surface area of 3850cm 2 / g, 28d compressive strength is 55.9MPa. The fly ash is Class F secondary fly ash produced by Nanjing Huaneng International Power Co., Ltd., with a density of 2.25g / cm 3 , water requirement ratio is 95%, loss on ignition is 2.11%. Fine aggregate is medium sand from Jiangxi Ganjiang II area, with fineness modulus of 2.50, mud content of 0.5%, water content of 0.65%, and apparent density of 2630kg / m 3 , bulk density is 1510kg / m 3The coarse aggregate is 5-25mm continuously graded Zhenjiang Chuanshan crushed stone, with a mud content of 0.5%, a water content of 0.70%, and an apparent density of 2725kg / m 3 , bulk density is 1680kg / m 3 . The high-efficiency water reducer is a polycarboxylic acid high-efficiency water reducer (water agent) produced by Jiangsu Bote New Materials Co., Ltd., with a solid content of 20%. The mixing water is drinking water. In the concrete mix ratio of this experiment, the cementitious material (cement + fly ash): coarse aggregate: fine aggregate: water = 1:2.18:1.27:0.35 (weight percentage). The total amount of cementitious material in one cubic meter of concrete is 545kg / m 3 , the fly ash replacement cement ratio is 30.3%, the amount of polycarboxylic acid high-efficiency water reducing agent is 1.2% of the weight of the cementitious material (weight percentage of water agent), and the experimental C60 concrete mix ratio is shown in Table 1. The concrete properties of the concrete with the addition of 1% (1%-MGG, 5.45kg), 2% (2%-MGG, 10.9kg), 3% (3%-MGG, 16.35kg) of modified natural biomass guar gum polymer water-absorbing resin concrete curing agent and the addition of 1% (1%-CST-PAAM, 5.45kg), 2% (2%-CST-PAAM, 10.9kg), 3% (3%-CST-PAAM, 16.35kg) of traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent were determined, and the amount of the two polymer water-absorbing resin concrete curing agents was the weight percentage of the cementitious material.
[0066] Table 1 Concrete experimental mix ratio
[0067]
[0068]
[0069] 2. Preparation and maintenance of concrete
[0070] 380kg of cement, 165kg of fly ash and modified natural biomass guar gum (MGG) polymer water-absorbing resin concrete curing agent (5.45-16.35kg, see the values 5.45, 10.9, 16.35kg in Table 1 for details) were put into a mixer and mixed at a stirring speed of 30 rpm for 2 minutes. Then, 690kg of river sand fine aggregate and 1187kg of crushed stone coarse aggregate were added to the mixture and stirred at a speed of 30 rpm for 1 minute. 3.27kg of polycarboxylate superplasticizer was dissolved in 95.5kg of mixing water and added to the mixer and stirred at a speed of 60 rpm for 2 minutes. Subsequently, the remaining 3.27kg of polycarboxylate superplasticizer was dissolved in 95.5kg of mixing water and added to the mixture and stirred at a speed of 60 rpm for 2 minutes. To avoid stratification of the mixture at the bottom of the container, the slurry was manually stirred twice with a shovel and continued to be mixed at 60 rpm for 2 minutes to remove bubbles in the fresh concrete slurry. Next, the initial slump flow and slump flow retention (2 hours) of the fresh MGG concrete were tested to evaluate the fluidity of the fresh concrete. Finally, the fresh concrete mixed with MGG polymer water-absorbing resin concrete curing agent was vibrated and compacted for 30 seconds. The vibrated and compacted MGG fresh concrete was poured into a 100mm×100mm×100mm mold to prepare 12 specimens, and the compressive strength of the hardened concrete was tested at 3, 7, 28, and 90d. Part of the MGG fresh concrete slurry was poured into three 75mm×75mm×285mm test molds to test the drying shrinkage value of the concrete. The other part of MGG fresh concrete was poured into three 30mm×250mm×250mm thin plate molds to test the crack resistance of concrete with high molecular water-absorbing resin concrete curing agent. Three rods were used on each side of the mold. The screw rods are used as constraints. 12 constraint screw rods are used on the four sides to provide constraints. The plastic film is covered with concrete test molds and placed in an environment with a temperature and humidity of RH (60±5%) and a temperature (20±2℃) for 2 hours. The surface of the specimen is blown dry by an electric fan. The wind direction is 100mm above the center of the specimen surface. The fan wind speed is 4±0.5m / s. The cracking of the concrete specimen is observed for 24 hours. Other MGG fresh concrete is poured to Six specimens were prepared in the test mold to measure the chloride ion diffusion coefficient of 28d and 90d hardened concrete. All concrete test molds filled with MGG polymer water-absorbing resin concrete curing agent were covered with wet sacks and placed in a room at a temperature of 20-23℃ for 24 hours. The specimens were removed from the test molds and placed in a standard curing room at a temperature of 25℃ and a humidity of 90±5% to cure to the specified age. Under the same conditions, the same number of specimens added with traditional corn starch acrylic acid grafted copolymer polymer water-absorbing resin concrete curing agent (CST-PAAM) were prepared for comparative experiments.
[0071] 3. Test methods for concrete performance
[0072] 3.1. Initial slump flow and slump flow retention of fresh concrete
[0073] Before the experiment, wipe the conical slump test cylinder with a wet cloth and place it on a horizontal steel plate. After the fresh concrete mixed with the polymer water-absorbing resin concrete curing agent is fully mixed, it is loaded into the circular slump test cylinder in three layers. The amount of concrete sample added each time is one-third of the height of the conical slump test cylinder. Use a vibrator to evenly insert and tamp the concrete from the edge to the center 25 times. After the concrete is filled and tamped, the concrete surface is smoothed. The slump cylinder is lifted vertically and steadily in 5-10 seconds. After the fresh concrete stops flowing, the average value of the fresh concrete mixture in two perpendicular directions is measured as the initial slump flow of the fresh concrete. After the initial slump flow test of the concrete is completed, the fresh concrete sample is placed in an iron bucket and sealed and left to stand for 30, 60, 90, and 120 minutes, and the slump flow of the concrete is repeatedly measured within the specified time. The retention of the slump flow of the fresh concrete is the change in the slump flow of the fresh concrete in two hours. Before each concrete slump flow test, the concrete sample must be re-stirred to ensure uniformity.
[0074] Figure 4 The figure shows the initial slump flow and slump flow retention of fresh concrete with different dosages of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. Figure 4It can be seen that with the increase of dosage, the initial collapse fluidity of concrete added with two polymer water-absorbing resin concrete curing agents continues to decrease. At the same dosage of polymer water-absorbing resin concrete curing agent, the concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent has lower initial collapse fluidity than the concrete added with traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. With the increase of placement time, the collapse fluidity of concrete added with two polymer water-absorbing resin concrete curing agents decreases. At the same dosage of polymer water-absorbing resin concrete curing agent (1%, 2%, 3%), the concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent (49.65%, 53.20%, 61.78%) has a higher slump fluidity loss rate than the concrete added with traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent (47.87%, 49.49%, 51.72%). The concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent has lower initial slump fluidity and slump fluidity retention than the concrete added with traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0075] 3.2 Compressive strength of hardened concrete
[0076] After 3, 7, 28, and 90 days of standard curing of concrete with high molecular weight water-absorbing resin concrete curing agent, the concrete specimens were removed from the standard curing environment. According to the national standard "Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T50081-2002), the compressive strength of hardened concrete was tested. The maximum load borne by the concrete specimen was measured at a loading rate of 1.3 MPa / s using the YAW-3000 electro-hydraulic servo loading system. The maximum load value per unit area of concrete is the compressive strength of hardened concrete.
[0077] Figure 5 The figure shows the change of compressive strength of hardened concrete with curing time under different dosages of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. Figure 5It can be seen that with the increase of curing age, the compressive strength of concrete added with two kinds of high molecular water-absorbing resin concrete curing agents increases. In the same curing age, with the increase of dosage, the early compressive strength of hardened concrete added with two kinds of high molecular water-absorbing resin concrete curing agents continues to decrease. In the late curing period, increasing the dosage of high molecular water-absorbing resin concrete curing agent can significantly improve the compressive strength of hardened concrete. At the same dosage of high molecular water-absorbing resin concrete curing agent (1%, 2%, 3%) and in the late curing period (90 days), the concrete added with natural biomass guar gum high molecular water-absorbing resin concrete curing agent (75.6MPa, 77.8MPa, 79.4MPa) has higher compressive strength than the concrete added with traditional corn starch acrylic acid graft copolymer high molecular water-absorbing resin concrete curing agent (74.6MPa, 75.9MPa, 77.3MPa).
[0078] 3.3 Concrete cracking
[0079] The crack resistance of concrete with modified natural biomass guar gum polymer water-absorbing resin concrete curing agent was tested according to the flat plate method specified in GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". The test time starts from the pouring of concrete into the test mold. After pouring to the test mold for 24 hours, the initial crack start time, number of cracks, total length and total width of the fresh concrete in the plastic stage are observed. The total crack area per unit area of concrete is used to evaluate the ability of concrete to resist cracking. Initially, observations were made every 5 minutes to determine the time when the first crack of the concrete appeared, and observations were made every 30 minutes after the initial cracks appeared. When the cracks penetrated the concrete surface, observations were made every 1 hour, and the total number of cracks on the concrete surface after 24 hours was recorded. The length of the cracks on the concrete surface was measured with a ruler. The total length of the cracks was the distance between the two ends of the crack. When a crack had multiple branches, the distance between the main cracks was taken first, and then the distance between the two ends of the branch cracks was measured. The crack width is measured using a DJCK-2 crack reading microscope (40 times). The reading drum of the rotating reading microscope is marked with scales to read the scale value. The crack width is the average of two readings. The total crack area per unit area of concrete is calculated according to formula (4).
[0080]
[0081]
[0082] c=a×b(4)
[0083] Where: W i - Maximum width of the i-th crack (mm); L i- length of the i-th crack (mm); N- total number of cracks (cracks); a- average crack area of each crack (mm 2 / strip); A-the area of the sheet metal mold (m 2 ); b-Number of cracks per unit area of concrete (cracks / m 2 ); c-total crack area per unit area of concrete (mm 2 / m 2 ).
[0084] Figure 6 The figure shows the anti-cracking performance of hardened concrete with different dosages of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. Figure 6 It can be seen that with the increase in dosage, the initial crack start time of the hardened concrete added with the two polymer water-absorbing resin concrete curing agents increases, and the number of cracks, crack length, crack width and total crack area per unit area all decrease. At the same dosage of polymer water-absorbing resin concrete curing agent, the concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent has a longer initial crack start time, fewer cracks, crack length, crack width and total crack area per unit area than the concrete added with traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent.
[0085] 3.4 Concrete drying shrinkage
[0086] The drying shrinkage of concrete with modified polymer water-absorbing resin concrete curing agent was tested according to the "Testing Procedure for Hydraulic Concrete" (DL / T 5150-2001). After three 75mm×75mm×285mm test molds were placed in a room with a temperature of 20-23℃ for 24 hours, the reference length of concrete with polymer water-absorbing resin concrete curing agent was measured, and the concrete specimens were placed in a shrinkage test box (temperature of 20-25℃, humidity of 50-55%). The concrete specimens were taken out of the shrinkage test box at 1, 4, 7, 28, 56, 90, and 112 days, and the length of concrete specimens at different ages was tested. The drying shrinkage value of concrete is the ratio of the change in specimen length to the reference length at the specified test age.
[0087] Figure 7 The figure shows the change of concrete drying shrinkage over time with different dosages of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. Figure 7It can be seen that as the drying time increases, the drying shrinkage of the concrete added with the two polymer water-absorbing resin concrete curing agents increases. At the same drying time, as the dosage of the two polymer water-absorbing resin concrete curing agents increases, the drying shrinkage of the concrete decreases. At the same dosage of polymer water-absorbing resin concrete curing agent (1%, 2%, 3%) and the same drying age (56 days), the concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent (0.0493%, 0.0431%, 0.376%) has a lower drying shrinkage value than the concrete added with the traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent (0.0644%, 0.0587%, 0.0512%).
[0088] 3.5 Chloride ion diffusion coefficient of hardened concrete
[0089] The chloride ion permeability coefficient of hardened concrete was tested according to the method of "Guidelines for Durability Design and Construction of Concrete Structures" (CCES 01-2004). After standard curing for 28 and 90 days, the hardened concrete mixed with modified polymer water-absorbing resin concrete curing agent was vacuum saturated for 16 hours. The vacuum saturated hardened concrete was moved into a test box filled with chloride ion solution. In the test box, the top surface of the hardened concrete was filled with 3% sodium chloride solution, and the other surfaces were in contact with 0.3N sodium hydroxide solution. A 30V DC voltage was applied to both ends of the specimen for 24 hours or 48 hours, and the parallel voltage, series current, and initial and final electrolyte temperatures were recorded. After the test was completed, the specimen was removed from the test box, split into two halves, and 0.1 mol / L AgNO3 solution was sprayed on the surface of the split specimen to measure the chloride ion penetration depth. The chloride ion diffusion coefficient of hardened concrete was calculated according to the following formula (5).
[0090]
[0091] Where: D RCM0 -Concrete chloride ion diffusion coefficient (m 2 / s); T-average value of initial and final temperature of anolyte (K); h-height of specimen (m); X d -Chloride ion diffusion depth (m); t-power-on test time (s); ɑ-auxiliary variable.
[0092] Figure 8 The figure shows the chloride ion diffusion coefficient of hardened concrete with different dosages of natural biomass guar gum polymer water-absorbing resin concrete curing agent and traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent. Figure 8It can be seen that with the increase of curing age, the chloride ion diffusion coefficient of hardened concrete added with two kinds of polymer water-absorbing resin concrete curing agents decreases. At the same curing age, with the increase of the dosage of polymer water-absorbing resin concrete curing agent, the chloride ion diffusion coefficient of hardened concrete decreases. At the same dosage of polymer water-absorbing resin concrete curing agent (1%, 2%, 3%) and curing age (90 days), the chloride ion diffusion coefficient of hardened concrete added with natural biomass guar gum polymer water-absorbing resin concrete curing agent (1.89×10 -12 m 2 / s, 1.81×10 -12 m 2 / s, 1.76×10 -12 m 2 / s) has a higher curing effect than that of concrete added with traditional corn starch acrylic acid graft copolymer polymer water-absorbing resin concrete curing agent (2.23×10 -12 m 2 / s, 2.05×10 -12 m 2 / s, 1.92×10 -12 m 2 / s) smaller chloride ion diffusion coefficient.
Claims
1. A method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum, characterized in that: The following steps are involved: (1) Preparation of dialdehyde guar gum: guar gum polymer and water are fully mixed to form a suspension, sodium bromide is added, and the pH value of the system is adjusted to 2-3 with dilute hydrochloric acid at a temperature of 45-50° C., acidification treatment is performed for 20-30 minutes, and a composite strong oxidant is slowly added dropwise over 30-40 minutes, the temperature is raised to 55-60° C., the guar gum suspension solution is stirred at an accelerated rate, and the reaction is performed at this temperature for 4-5 hours to obtain a dialdehyde guar gum polymer solution; (2) Preparation of N-hydroxymethyl acrylamide monomer: Under the action of a fatty amine catalyst, an aqueous acrylamide solution and formaldehyde are condensed to obtain an N-hydroxymethyl acrylamide solution; (3) Preparation of modified guar gum intermediate containing double bonds: under alkaline conditions, a dialdehyde guar gum polymer solution and an N-hydroxymethyl acrylamide solution undergo a nucleophilic substitution reaction to introduce double bonds into the guar gum polymer molecules, thereby obtaining a modified guar gum polymer intermediate containing double bonds and amino groups; (4) Preparation of polymer water-absorbing resin concrete curing agent: In the presence of an initiator, a modified guar gum polymer intermediate containing double bonds and amino groups is grafted and copolymerized with styrene and butyl acrylate monomers to obtain a modified natural guar gum polymer water-absorbing resin concrete curing agent containing -OH, -NH2, and -COO(CH2)3CH3 groups.
2. The method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum according to claim 1, characterized in that: In step (1), the weight ratio of the guar gum polymer to water is 1:6.5-7.0, the amount of sodium bromide is 3.5-4.0% of the weight of the guar gum polymer, the composite strong oxidant is a composite strong oxidant of sodium hypochlorite and hydrogen peroxide, the amount of which is 7.0-7.5% of the weight of the guar gum polymer, and the weight ratio of the sodium hypochlorite to hydrogen peroxide is 2:
1.
3. The method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum according to claim 1, characterized in that: The specific steps of step (2) are as follows: dissolving acrylamide in water to form a clear solution, adjusting the pH value to 9-10 at a temperature of 30-35° C., adding triethylenediamine catalyst, slowly adding 37% formaldehyde aqueous solution dropwise over 30-40 minutes, raising the system temperature to 55-60° C., reacting at this temperature for 1-2 hours to obtain N-hydroxymethyl acrylamide solution.
4. The method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum according to claim 1, characterized in that: In step (2), the weight ratio of acrylamide, water and formaldehyde is 1:5.5-6.0:1.25-1.30, and the fatty amine catalyst is triethylenediamine catalyst, and its dosage is 2.0% of the weight of acrylamide.
5. According to the method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum as claimed in claim 1, the specific steps of step (3) are: adding N-hydroxymethyl acrylamide solution to the dialdehyde guar gum polymer solution, continuously stirring for 1-2 hours, adjusting the pH value to 10-11 with sodium hydroxide solution, slowly adding sodium borohydride catalyst, and reacting at a temperature of 60-70° C. for 2-3 hours to obtain a modified guar gum polymer intermediate containing double bonds and amino end-capping.
6. The method for preparing a high molecular weight water-absorbing resin concrete internal curing agent using natural biomass guar gum according to claim 5, wherein the weight ratio of the dialdehyde guar gum polymer solution to the N-hydroxymethyl acrylamide solution in step (3) is 19.0-19.5:1, and the amount of the sodium borohydride catalyst is 0.06-0.065% of the weight of the dialdehyde guar gum polymer solution.
7. The method for preparing a high molecular weight water-absorbing resin concrete curing agent using natural biomass guar gum according to claim 1, wherein the specific steps of step (4) are as follows: adding an ethanol solution containing a mixed monomer of styrene and butyl acrylate to a mixed solution of a modified guar gum polymer intermediate containing double bonds and amino groups and water at a temperature of 80-85° C., adjusting the system pH value to 3-4, dropwise adding a composite initiator of potassium persulfate and sodium bisulfite, carrying out a graft copolymerization reaction at a temperature of 90-95° C. for 2-3 hours, stopping the reaction and aging for 2-3 hours, adjusting the pH value to 2-3, and obtaining a light yellow viscous modified guar gum high molecular weight water-absorbing resin with a solid content of 10-15%. The modified natural guar gum polymer water-absorbing resin concrete curing agent solution is dried, crushed and ball-milled to obtain a modified natural guar gum polymer water-absorbing resin concrete curing agent powder, wherein the mass ratio of the modified guar gum polymer intermediate containing double bonds and amino end-capping to water is 49.0-49.5:1, the weight ratio of the modified guar gum polymer intermediate containing double bonds and amino end-capping to styrene and butyl acrylate is 225-230:1:1.20-1.25, the amount of the potassium persulfate and sodium bisulfite composite initiator is 0.35-0.40% of the weight of the modified guar gum polymer intermediate containing double bonds and amino end-capping, and the weight ratio of the potassium persulfate and sodium bisulfite is 2:1; Preferably, the drying condition is to perform drying treatment at a temperature of 90-95° C. for 16-24 hours; Preferably, the powder is sieved through a 0.40 mm round hole after the crushing and ball milling to obtain a modified natural biomass guar gum polymer water-absorbing concrete internal curing agent powder with a particle size less than 0.40 mm, and the particle size of the internal curing agent is controlled to be 4.876-5.239 μm.
8. The polymer water-absorbing resin concrete internal curing agent obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the polymer water-absorbing resin concrete internal curing agent according to claim 8 in the preparation of concrete.
10. The use according to claim 9, characterized in that: The dosage of the polymer water-absorbing resin concrete internal curing agent is 1-3wt%.
Citation Information
Cited By
Material applied to preparation of biodegradable wrapping film and preparation method of wrapping film
CN120648182A